Method for producing oxidized cellulose nanofiber dispersion
The method of stirring and standing oxidized cellulose nanofiber dispersions with optional dilution and dispersant addition addresses the viscosity loss issue, ensuring stable thickening performance.
Patent Information
- Application Number
- PCT/JP2024/008258
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Cellulose nanofibers used as thickeners experience significant viscosity decrease when stirred with other materials, compromising their thickening function.
A method involving a stirring step at 2000-6000 rpm for 1-90 minutes followed by a standing step at 4-35°C for 12 hours or more, and optional dilution and dispersant addition, to produce an oxidized cellulose nanofiber dispersion that maintains viscosity retention.
The method effectively suppresses viscosity decrease during and after stirring, enhancing the thickening properties of the dispersion.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Method for producing oxidized cellulose nanofiber dispersion
[0001] The present invention relates to a method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention.
[0002] Nanotechnology, a technique for freely controlling matter at the nanometer scale, or the atomic and molecular scale, is expected to lead to the creation of a variety of convenient new materials and devices. One example is cellulose nanofiber, obtained by finely disintegrating plant fibers. These cellulose nanofibers are highly crystalline, characterized by a low coefficient of thermal expansion and a high modulus of elasticity. Furthermore, because they have a high aspect ratio, they are expected to be effective in strengthening and stabilizing shapes when combined with rubbers and resins. Furthermore, when in a dispersed state, these cellulose nanofibers possess viscosity properties such as pseudoplasticity and thixotropy, making them suitable for use as thickeners and other additives.
[0003] Various developments and research have been conducted on cellulose nanofibers. For example, Patent Document 1 discloses fine cellulose fibers (cellulose nanofibers) in which some of the hydroxyl groups of cellulose have been carboxylated and have a number-average fiber diameter of 2 to 150 nm. These cellulose nanofibers have the properties of high viscosity at low shear rates and low viscosity at high shear rates. Because of these viscosity characteristics, cellulose nanofibers are used as thickeners in various fields, such as cosmetics, food, civil engineering, building materials, inks, and paints.
[0004] Japanese Patent Application Laid-Open No. 2008-1728
[0005] However, when the cellulose nanofibers described in Patent Document 1 are used as a thickener, there is a problem in that the viscosity drops significantly when the cellulose nanofibers are mixed with the other substance to which the thickening function is to be imparted and agitated.
[0006] Therefore, the present invention aims to provide a method for producing an oxidized cellulose nanofiber dispersion that can suppress the decrease in viscosity before and after stirring when stirring is performed when mixing with a component that imparts a thickening function.
[0007] The present invention provides the following (1) to (5): (1) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention, comprising: a stirring step of stirring an oxidized cellulose nanofiber dispersion with a solid content concentration of 0.1 to 5.0% by mass at a rotation speed of 2000 to 6000 rpm for 1 to 90 minutes; and a standing step of standing the oxidized cellulose nanofiber dispersion at a temperature of 4 to 35°C for 12 hours or more after the stirring step. (2) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to (1), further comprising a dilution step of diluting the oxidized cellulose nanofiber dispersion to a solid content concentration of 0.1 to 0.8% by mass after the standing step. (3) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to (1) or (2), wherein the oxidized cellulose nanofibers have a carboxyl content of 0.2 to 2.0 mmol / g relative to the bone dry mass of the oxidized cellulose nanofibers. (4) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to (2), characterized in that in the dilution step, 5 to 100 parts by mass of a dispersant is further added per 100 parts by mass of the oxidized cellulose nanofiber solids content. (5) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to (2), further comprising, after the dilution step, a step of adding 5 to 100 parts by mass of a dispersant per 100 parts by mass of the oxidized cellulose nanofiber solids content in the oxidized cellulose nanofiber dispersion, and mixing.
[0008] According to the present invention, a method for producing an oxidized cellulose nanofiber dispersion can be provided that, when a stirring process is carried out when mixing with a component that imparts a thickening function, can suppress a decrease in viscosity before and after stirring.
[0009] The method for producing an oxidized cellulose nanofiber (oxidized CNF) dispersion with improved viscosity retention of the present invention comprises a stirring step in which an oxidized cellulose nanofiber dispersion having a solids concentration of 0.1 to 5.0 mass% is stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which, after the stirring step, the oxidized cellulose nanofiber dispersion is allowed to stand at a temperature of 4 to 35°C for 12 hours or more.
[0010] (Oxidized Cellulose Nanofiber (Oxidized CNF)) The oxidized CNF used in the present invention can be obtained by defibrating oxidized cellulose obtained by introducing carboxyl groups into a cellulose raw material.
[0011] (Raw Material) Examples of cellulose raw materials include plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (e.g., unbleached softwood kraft pulp (NUKP), bleached softwood kraft pulp (NBKP), unbleached hardwood kraft pulp (LUKP), bleached hardwood kraft pulp (LBKP), unbleached softwood sulfite pulp (NUSP), bleached softwood sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), and materials derived from microbial products, and any of these can be used. Preferably, the cellulose raw material is derived from a plant or a microorganism, and more preferably from a plant.
[0012] (Introduction of Carboxyl Group) Carboxyl groups can be introduced into the cellulose raw material by oxidizing (carboxylating) the cellulose raw material using a known method.
[0013] One example of oxidation is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound, a bromide, an iodide, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the pyranose ring on the cellulose surface. As a result, oxidized cellulose having aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO-) on the surface can be obtained. The cellulose concentration during the reaction is not particularly limited, but is preferably 5% by mass or less.
[0014] An N-oxyl compound refers to a compound capable of generating a nitroxy radical. Any compound can be used as the N-oxyl compound as long as it promotes the target oxidation reaction. Examples include 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO).
[0015] The amount of N-oxyl compound used is not particularly limited, as long as it is a catalytic amount capable of oxidizing the raw material cellulose. The amount is preferably 0.01 mmol to 10 mmol, more preferably 0.01 mmol to 1 mmol, and even more preferably 0.05 mmol to 0.5 mmol, per 1 g of bone-dry cellulose. The concentration of the N-oxyl compound in the reaction system is preferably about 0.1 mmol / L to 4 mmol / L.
[0016] Bromides are compounds containing bromine, including alkali metal bromides that can dissociate and ionize in water, while iodides are compounds containing iodine, including alkali metal iodides.
[0017] The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is preferably 0.1 mmol to 100 mmol, more preferably 0.1 mmol to 10 mmol, and even more preferably 0.5 mmol to 5 mmol, per 1 g of bone-dry cellulose.
[0018] Any known oxidizing agent can be used, such as halogen, hypohalous acid, halous acid, perhalogen acid or salts thereof, halogen oxide, peroxide, etc. Among these, sodium hypochlorite is preferred because it is inexpensive and has a low environmental impact.
[0019] The amount of the oxidizing agent used is preferably 0.5 mmol to 500 mmol, more preferably 0.5 mmol to 50 mmol, and even more preferably 1 mmol to 25 mmol, per 1 g of bone-dry cellulose, and is preferably 1 mol to 40 mol per 1 mol of the N-oxyl compound, for example.
[0020] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4°C to 40°C, and may be room temperature, approximately 15°C to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, causing the pH of the reaction solution to decrease. To efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution during the reaction to maintain the pH of the reaction solution at 8 to 12, preferably about 10 to 11. Water is preferred as the reaction medium because of its ease of handling and the fact that side reactions are unlikely to occur.
[0021] The reaction time in the oxidation reaction can be appropriately set depending on the degree of progress of the oxidation, and is usually 0.5 to 6 hours, preferably 0.5 to 4 hours.
[0022] Alternatively, the oxidation reaction may be carried out in two stages. For example, the oxidized cellulose obtained by filtration after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing for efficient oxidation without reaction inhibition by sodium chloride produced as a by-product in the first-stage reaction.
[0023] Another example is a method of oxidizing cellulose raw materials by contacting them with an ozone-containing gas, which oxidizes at least the hydroxyl groups at positions 2 and 6 of the pyranose ring and decomposes the cellulose chain.
[0024] The ozone concentration in the ozone-containing gas is 50 g / m 3 ~250g / m3 It is preferable that the thickness is 50 g / m 3 ~220g / m 3 The amount of ozone added to the cellulose raw material is preferably 0.1 parts by mass to 30 parts by mass, and more preferably 5 parts by mass to 30 parts by mass, when the solid content of the cellulose raw material is taken as 100 parts by mass.
[0025] The ozone treatment temperature is preferably 0°C to 50°C, and more preferably 20°C to 50°C. The ozone treatment time is not particularly limited, but is about 1 minute to 360 minutes, and preferably about 30 minutes to 360 minutes. When the ozone treatment conditions are within these ranges, excessive oxidation and decomposition of cellulose can be prevented, and a good yield of oxidized cellulose can be achieved.
[0026] After the ozone treatment, a further oxidation treatment may be carried out using an oxidizing agent. The oxidizing agent used in the further oxidation treatment is not particularly limited, but examples include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, the further oxidation treatment can be carried out by dissolving these oxidizing agents in water or a polar organic solvent such as alcohol to prepare an oxidizing agent solution, and then immersing the cellulose raw material in the solution.
[0027] The amount of carboxyl groups, which indicates the degree of modification of oxidized cellulose, can be adjusted by controlling reaction conditions such as the amount of oxidizing agent added and reaction time, as described above. The amount of carboxyl groups is preferably approximately 0.2 to 2.0 mmol / g, and more preferably 0.5 to 1.6 mmol / g, relative to the bone-dry mass of oxidized cellulose. If the amount is less than 0.2 mmol / g, a large amount of energy is required to defibrate it into oxidized CNF. Furthermore, if more than 2.0 mmol of oxidized cellulose is used as a raw material, the resulting oxidized CNF will not have a fibrous form. The amount of carboxyl groups in oxidized cellulose is usually the same as the amount of carboxyl groups when made into cellulose nanofibers.
[0028] (Defibrillation) The device used for defibration is not particularly limited, but examples include devices of high-speed rotation type, colloid mill type, high-pressure type, roll mill type, and ultrasonic type. A high-pressure or ultra-high-pressure homogenizer is preferred, and a wet high-pressure or ultra-high-pressure homogenizer is more preferred. The device is preferably capable of applying a strong shear force to the cellulose raw material or oxidized cellulose (usually a dispersion). The pressure that the device can apply is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 140 MPa or more. The device is preferably a wet high-pressure or ultra-high-pressure homogenizer that can apply the above pressure and strong shear force to the cellulose raw material or oxidized cellulose (usually a dispersion). This allows for efficient defibration. The number of treatments (passes) in the defibration device may be one or two or more, with two or more being preferred.
[0029] In the dispersion treatment, oxidized cellulose is usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse oxidized cellulose, but examples include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Because the cellulose raw material is hydrophilic, water is preferably used as the solvent.
[0030] The solids concentration of oxidized cellulose in the dispersion is usually 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. This ensures that the amount of liquid relative to the amount of cellulose fiber raw material is appropriate and efficient. The upper limit is usually 10% by mass or less, and preferably 6% by mass or less. This allows fluidity to be maintained.
[0031] The order of the defibration treatment and dispersion treatment is not particularly limited, and either may be performed first, or they may be performed simultaneously, but it is preferable to perform the defibration treatment after the dispersion treatment. Each combination of treatments needs to be performed at least once, and may be repeated two or more times.
[0032] Prior to the defibration treatment or dispersion treatment, a pretreatment may be carried out as necessary. The pretreatment may be carried out using a mixing, stirring, emulsifying, or dispersing device such as a high-speed shear mixer.
[0033] The average fiber diameter and average fiber length of the cellulose nanofibers can be measured, for example, by preparing a 0.001% by mass aqueous dispersion of oxidized CNF, spreading this diluted dispersion thinly on a mica sample stage, and heating and drying it at 50°C to prepare an observation sample, and measuring the cross-sectional height of the shape image observed with an atomic force microscope (AFM) to calculate the number-average fiber diameter or fiber length.
[0034] The average aspect ratio of oxidized CNF is usually 50 or more. There is no particular upper limit, but it is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter
[0035] (Stirring Process) In the stirring process of the present invention, an oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0% by mass is stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm. The solid content concentration of the oxidized CNF dispersion used in the stirring process is 0.1 to 5.0% by mass, preferably 0.1 to 3.0% by mass. If the concentration is too high, stirring becomes difficult, while if the concentration is too low, the amount of CNF added when added to other materials becomes low, making it difficult to use as a thickener. As long as the solid content concentration of the oxidized CNF dispersion used in the stirring process is within the above range, the oxidized CNF dispersion after the dispersion and defibration process can be used directly in the stirring process. The solid content concentration can be adjusted by appropriate dilution, dehydration, etc. The rotation speed in the stirring process is 2000 to 6000 rpm, preferably 2000 to 3000 rpm, from the viewpoint of thoroughly stirring the entire CNF dispersion. The stirring time is 1 to 90 minutes, preferably 5 to 60 minutes, and more preferably 10 to 60 minutes, from the viewpoint of imparting a shearing effect by stirring to the entire CNF dispersion.
[0036] The agitator used in the agitation process is not particularly limited as long as it can agitate an oxidized CNF dispersion liquid having a solid content concentration of 0.1 to 5.0 mass% at the above rotation speed, and examples thereof include high-speed agitators and high-speed emulsifying dispersers. As a high-speed agitator, for example, a Homo Disper manufactured by Primix Corporation can be used.
[0037] (Standing Step) In the standing step of the present invention, the oxidized CNF dispersion after the stirring step is left standing at a temperature of 4 to 35°C, preferably 6 to 25°C, for 12 hours or more, preferably 24 hours or more. There is no particular upper limit to the standing time, but from the viewpoint of long-term storage, it is, for example, 10 days or less. If the standing time is too short, there is a risk that the temporary viscosity decrease immediately after stirring will not recover. In the standing step, it is preferable to place the oxidized CNF dispersion in a container and leave it standing to prevent evaporation of water in the CNF dispersion. The material of the container is not particularly limited, and may be a glass bottle or plastic. It is preferable that the container be one that can be closed with a lid.
[0038] (Dilution Step) The production method of the present invention may include a dilution step after the standing step. When the dilution step is included, the oxidized CNF is diluted until the solids concentration is preferably 0.1 to 0.8% by mass, more preferably 0.1 to 0.6% by mass. The solvent used for dilution may be the same as or different from the solvent used in the dispersion before dilution, and examples thereof include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixed solvents thereof. Since the cellulose raw material is hydrophilic, the solvent is preferably water. In the dilution step, the stirring and mixing conditions are not particularly limited as long as uniform dilution is achieved; for example, dilution is achieved by stirring at a rotation speed of 1000 rpm for 10 minutes.
[0039] (Dispersant) The oxidized CNF dispersion produced by the production method of the present invention may contain a dispersant. When a dispersant is added, the amount added is preferably 5 to 100 parts by mass, more preferably 10 to 50 parts by mass, per 100 parts by mass of the oxidized CNF solids, from the perspective of the solid content of the CNF. The type of dispersant may be used without particular limitation as long as it achieves the effects of the present invention, and examples thereof include polyacrylic acid, carboxymethyl cellulose, and polyurethane dispersants.
[0040] When a dispersant is contained, the step of adding the dispersant is not particularly limited as long as the effects of the present invention are achieved. However, the dispersant may be added in the stirring step, the dispersant may be added in the dilution step, or a step of adding the dispersant and mixing may be provided after the dilution step. If a dilution step is not provided, a step of adding the dispersant and mixing may be provided after the standing step. When a dispersant is added and mixed at a step other than the stirring step and the dilution step, the device used for stirring and mixing is not particularly limited, and a commonly used stirring device may be used. The stirring time is also not particularly limited, and stirring may be performed within a range of about 1 minute to 1 hour.
[0041] (Viscosity Retention Rate) The viscosity retention rate of an oxidized cellulose nanofiber dispersion can be calculated from the viscosity before and after stirring determined by the stability test described below using the following formula: Viscosity retention rate (%) = (viscosity after stirring / viscosity before stirring) × 100
[0042] (Stability test) The Brookfield viscosity of the oxidized cellulose nanofiber dispersion immediately after the dilution step is measured using a Brookfield viscometer at 6 rpm, 23°C, and for 1 minute (viscosity before stirring). If the dilution step is not required, the viscosity before stirring can be measured under the same conditions for the dispersion to which shear force has been applied by stirring (1000 rpm, 10 minutes) after the standing step. If the dilution step includes a step of adding and mixing a dispersant, the viscosity before stirring can be measured under the same conditions for the dispersion after that step.
[0043] After measuring the B-type viscosity, the oxidized cellulose nanofiber dispersion is stirred for 30 minutes (1000 rpm, 23°C) using a high-speed stirrer. Immediately after 30 minutes of stirring, the B-type viscosity is measured using a B-type viscometer at 6 rpm, 23°C, and for 1 minute (viscosity after stirring). As the high-speed stirrer, for example, a Homo Disper manufactured by Primix Corporation can be used.
[0044] According to the production method of the present invention, it is possible to produce an oxidized cellulose nanofiber dispersion with improved viscosity retention.
[0045] The reason why the production method of the present invention can produce an oxidized cellulose nanofiber dispersion with improved viscosity retention is believed to be as follows: Cellulose nanofibers can be obtained by defibrating oxidized cellulose. The cellulose nanofibers obtained here are in a state where each fiber is swollen (defibrated) to the nano-level, but the physical entanglements of the cellulose fibers that existed before defibration remain. When such an oxidized cellulose nanofiber dispersion is stirred under the stability test conditions (1000 rpm, 23°C), the entangled nanofibers become loose, changing the dispersion state. The loosened nanofibers become oriented in a certain direction, resulting in the development of pseudoplasticity and a decrease in viscosity. In the production method of the present invention, a stirring step is performed before the stability test, and this step can dissolve the physical entanglements of the cellulose fibers remaining after defibration. Therefore, the decrease in viscosity before and after the stability test is suppressed, and as a result, an oxidized cellulose nanofiber dispersion with improved viscosity retention can be produced.
[0046] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0047] (Method for measuring the amount of carboxyl groups) 60 mL of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. After that, a 0.05 N aqueous sodium hydroxide solution was added dropwise, and the electrical conductivity was measured until the pH reached 11. The amount of carboxyl groups was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of a weak acid, where the change in electrical conductivity is gradual: Amount of carboxyl groups [mmol / g oxidized cellulose] = a [mL] × 0.05 / mass of oxidized cellulose [g]
[0048] (Stability Test) For the oxidized cellulose nanofiber aqueous dispersions of the Examples and Comparative Examples, the Brookfield viscosity was measured immediately after the dilution step using a Brookfield viscometer at 6 rpm, 23°C, and for 1 minute (viscosity before stirring).
[0049] After measuring the B-type viscosity, the oxidized cellulose nanofiber aqueous dispersion was stirred for 30 minutes (1000 rpm, 23°C) using a high-speed stirrer (Homodisper, manufactured by Primix Corporation). Immediately after 30 minutes of stirring, the B-type viscosity was measured using a B-type viscometer at 6 rpm, 23°C, and for 1 minute (viscosity after stirring).
[0050] (Viscosity Retention Rate) The viscosity retention rate was calculated using the viscosity before stirring and the viscosity after stirring measured in the stability test according to the following formula: Viscosity retention rate (%) = (viscosity after stirring / viscosity before stirring) x 100
[0051] (Production Example A) (Production of Oxidized Cellulose Nanofiber Aqueous Dispersion A) 5.00 g (bone dry) of bleached, unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma-Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.1 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 90%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as "degree of modification") was 1.46 mmol / g. This was adjusted to 1.0 mass% with water and subjected to defibration treatment three times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion A. The average fiber diameter was 4 nm and the aspect ratio was 270.
[0052] (Production Example B) (Production of Oxidized Cellulose Nanofiber Aqueous Dispersion B) 5.00 g (bone dry) of bleached, unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma-Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 3.4 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 92%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as "degree of modification") was 1.1 mmol / g. This was adjusted to 1.0 mass% with water and subjected to defibration treatment three times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion B. The average fiber diameter was 4 nm and the aspect ratio was 273.
[0053] (Production Example C) (Production of Oxidized Cellulose Nanofiber Aqueous Dispersion C) 5.00 g (bone dry) of bleached, unbeaten kraft pulp (brightness 85%) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma-Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 1.0 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, which was then thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 93%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as "degree of modification") was 0.58 mmol / g. This was adjusted to 1.0% by mass with water and defibrated five times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion C. The average fiber diameter was 4 nm and the aspect ratio was 290.
[0054] (Production Example D) (Production of Oxidized Cellulose Nanofiber Aqueous Dispersion D) 5.00 g (bone dry) of bleached, unbeaten kraft pulp derived from coniferous trees (brightness 85%) was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone dry cellulose) of TEMPO (Sigma-Aldrich) and 514 mg (1.0 mmol per 1 g of bone dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 2.2 mmol / g, initiating the oxidation reaction. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was gradually added to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The reaction mixture was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 93%, the time required for the oxidation reaction was 60 minutes, and the carboxyl group content was 0.76 mmol / g. This was adjusted to 1.0% by mass with water and defibrated five times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion D. The average fiber diameter was 4 nm and the aspect ratio was 280.
[0055] (Example 1) (Stirring step) The oxidized cellulose nanofiber aqueous dispersion A having a solid content concentration of 1.0 mass% obtained in Production Example A was subjected to a stirring treatment for 5 minutes using a high-speed stirrer (Homodisper, manufactured by Primix Corporation) at a rotation speed of 3000 rpm.
[0056] (Standing Step) The oxidized cellulose nanofiber aqueous dispersion A that had been stirred in the stirring step above was placed in a plastic container and left to stand at 23°C for 7 days.
[0057] (Dilution step) The oxidized cellulose nanofiber aqueous dispersion A that had been subjected to the standing step was placed in a plastic container, deionized water was added, and the mixture was stirred (1000 rpm, 10 minutes) to obtain oxidized cellulose nanofiber aqueous dispersion A diluted to a solids concentration of 0.5 mass %.
[0058] A stability test was conducted on this diluted oxidized cellulose nanofiber aqueous dispersion A, and the Brookfield viscosity values before and after stirring were obtained. The results are shown in Table 1.
[0059] (Examples 2 to 4) Stability tests were conducted in the same order as in Example 1, with the exception that the stirring time in the stirring step was changed to 15 minutes (Example 2), 30 minutes (Example 3), and 60 minutes (Example 4), respectively. The results are shown in Table 1.
[0060] (Example 5) A stability test was conducted by carrying out the stirring step, standing step, and dilution step in this order in the same manner as in Example 1, except that oxidized cellulose nanofiber aqueous dispersion B obtained in Production Example B was used. The results are shown in Table 1.
[0061] (Examples 6 to 8) Stability tests were conducted in the same order as in Example 5, with the exception that the stirring time in the stirring step was changed to 15 minutes (Example 6), 30 minutes (Example 7), and 60 minutes (Example 8). The results are shown in Table 1.
[0062] (Example 9) A stability test was carried out by carrying out the stirring step, standing step, and dilution step in this order in the same manner as in Example 1, except that oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C was used. The results are shown in Table 1.
[0063] (Examples 10 to 12) Stability tests were carried out in the same order as in Example 9, with the exception that the stirring time in the stirring step was changed to 15 minutes (Example 10), 30 minutes (Example 11), and 60 minutes (Example 12), respectively. The results are shown in Table 1.
[0064] Comparative Example 1 The standing and dilution steps were carried out in the same manner as in Example 1, except that oxidized cellulose nanofiber aqueous dispersion A, which had not been subjected to the stirring step and had been stirred in the standing step, was replaced with oxidized cellulose nanofiber aqueous dispersion A which had not been subjected to the stirring step, to obtain an oxidized cellulose nanofiber aqueous dispersion with a solids concentration of 0.5% by mass. A stability test was conducted on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.
[0065] Comparative Example 2 The standing and dilution steps were carried out in the same manner as in Example 5, except that oxidized cellulose nanofiber aqueous dispersion B, which had not been subjected to the stirring step and had been stirred in the standing step, was replaced with oxidized cellulose nanofiber aqueous dispersion B, which had not been subjected to the stirring step, and an oxidized cellulose nanofiber aqueous dispersion with a solids concentration of 0.5% by mass was obtained. A stability test was carried out on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.
[0066] (Comparative Example 3) The standing and dilution steps were carried out in the same manner as in Example 9, except that oxidized cellulose nanofiber aqueous dispersion C, which had not been subjected to the stirring step and had been stirred in the standing step, was replaced with oxidized cellulose nanofiber aqueous dispersion C which had not been subjected to the stirring step, to obtain an oxidized cellulose nanofiber aqueous dispersion with a solids concentration of 0.5% by mass. A stability test was conducted on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.
[0067]
[0068] As can be seen from Table 1, when the methods of Examples 1 to 12 were used, which included a stirring step in which a 0.1 to 5.0 mass% oxidized cellulose nanofiber dispersion was stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which the oxidized cellulose nanofiber dispersion was allowed to stand at a temperature of 4 to 35°C for 12 hours or more after the stirring step, the obtained oxidized cellulose nanofiber dispersions had improved viscosity retention when compared with Comparative Examples 1 to 3 in which the stirring step was not performed, which had the same degree of modification.
[0069] (Example 13) Using the oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D, the stirring step and the standing step were carried out in this order in the same manner as in Example 1, except that the stirring treatment time was changed to 15 minutes.
[0070] (Dilution Step) Oxidized cellulose nanofiber aqueous dispersion D that had been subjected to the standing step was placed in a plastic container, and polyacrylic acid (Aron A-7100, manufactured by Toagosei Co., Ltd., hereinafter sometimes abbreviated as "PAA") was further added as a dispersant in an amount of 20 parts by mass per 100 parts by mass of the oxidized cellulose nanofiber solids content. Deionized water was then added to this plastic container and stirred (1000 rpm, 10 minutes), yielding a dispersion with an oxidized cellulose nanofiber solids concentration of 0.5% by mass and a dispersant concentration of 0.1% by mass, relative to the total volume of the dispersion.
[0071] The resulting dispersion was subjected to a stability test to obtain Brookfield viscosity values before and after stirring. The results are shown in Table 2.
[0072] Example 14 A dispersion with an oxidized cellulose nanofiber solids concentration of 0.5% by mass and a dispersant concentration of 0.1% by mass was obtained in the same manner as in Example 13, except that the dispersant was changed to carboxymethyl cellulose (Sunrose A04SH, manufactured by Nippon Paper Industries Co., Ltd., hereinafter sometimes abbreviated as "CMC"). A stability test was conducted on the obtained dispersion. The results are shown in Table 2.
[0073] Example 15 A dispersion with an oxidized cellulose nanofiber solids concentration of 0.5 mass% and a dispersant concentration of 0.1 mass% was obtained in the same manner as in Example 13, except that oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C was used instead of oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D. A stability test was conducted on the obtained dispersion. The results are shown in Table 2.
[0074] Example 16 A dispersion with an oxidized cellulose nanofiber solids concentration of 0.5 mass% and a dispersant concentration of 0.1 mass% was obtained in the same manner as in Example 14, except that oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C was used instead of oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D. A stability test was conducted on the obtained dispersion. The results are shown in Table 2.
[0075] (Comparative Examples 4 to 5) The standing and dilution steps were carried out in the same manner as in Examples 13 and 14, except that oxidized cellulose nanofiber aqueous dispersion D, which had not been subjected to the stirring step and had been stirred in the standing step, was replaced with an aqueous dispersion that had not been subjected to the stirring step, thereby obtaining dispersions of Comparative Examples 4 and 5, respectively, with oxidized cellulose nanofiber solids concentrations of 0.5% by mass and dispersant concentrations of 0.1% by mass. Stability tests were conducted on the resulting dispersions. The results are shown in Table 2.
[0076]
[0077] As can be seen from Table 2, when the methods of Examples 13 to 16 were used, which included a stirring step in which a 0.1 to 5.0 mass% oxidized cellulose nanofiber dispersion was stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which the oxidized cellulose nanofiber dispersion was allowed to stand at a temperature of 4 to 35°C for 12 hours or more after the stirring step, the viscosity retention of the resulting oxidized cellulose nanofiber dispersion was improved, even when a dispersant was added, compared to Comparative Examples 4 and 5, in which the stirring step was not performed.
Claims
1. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention, comprising: a stirring step of stirring an oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0% by mass at a rotation speed of 2000 to 6000 rpm for 1 to 90 minutes; and a standing step of standing the oxidized cellulose nanofiber dispersion at a temperature of 4 to 35°C for 12 hours or more after the stirring step.
2. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention as described in claim 1, further comprising a dilution step of diluting the oxidized cellulose nanofiber dispersion to a solids concentration of 0.1 to 0.8 mass % after the standing step.
3. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to claim 1 or 2, wherein the oxidized cellulose nanofiber has a carboxyl amount of 0.2 to 2.0 mmol / g relative to the bone dry mass of the oxidized cellulose nanofiber.
4. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention, as described in claim 2, characterized in that in the dilution process, 5 to 100 parts by mass of a dispersant is further added per 100 parts by mass of the oxidized cellulose nanofiber solids content.
5. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention as described in claim 2, further comprising the step of adding 5 to 100 parts by mass of a dispersant per 100 parts by mass of the solid content of oxidized cellulose nanofibers in the oxidized cellulose nanofiber dispersion after the dilution step, and mixing.
Citation Information
Patent Citations
Concentrate of anion-modified cellulose nanofiber, method for the production thereof and dispersion liquid thereof
JP2016186018A
Cellulose nano-fiber dry solid material and production method therefor, and dry solid material re-dispersion
JP2017002135A
Viscous water base composition and method for producing the same
JP2017110085A
Cellulose nanofiber composition and production method therefor
JP2022102007A
Oxidized cellulose, nanocellulose and their dispersions
JP2022165987A