Laminate and laminate production method
The laminate, composed of a vinyl chloride resin and foamed polyurethane with specific additives, addresses the issue of discoloration under high temperatures by using aliphatic dicarboxylic acid salts and plasticizers, enhancing its thermal stability and performance for automotive applications.
Patent Information
- Application Number
- PCT/JP2024/008347
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-05
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional laminates of vinyl chloride resin and foamed polyurethane molded bodies undergo discoloration when exposed to high temperature conditions, limiting their durability and performance in applications like automobile interior parts.
A laminate comprising a vinyl chloride resin molded body formed from a composition containing a vinyl chloride resin, an aliphatic dicarboxylic acid salt, and a plasticizer, with specific mass ratios and types of aliphatic dicarboxylate and plasticizer, such as disodium maleate and polyester, which suppresses discoloration and improves powder fluidity and surface smoothness.
The laminate effectively prevents discoloration under high temperature conditions, enhances the flexibility and light resistance of the vinyl chloride resin, and improves the meltability and surface smoothness, making it suitable for use in automobile interior materials like instrument panels.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Laminate and method for manufacturing laminate
[0001] The present invention relates to a laminate and a method for manufacturing the laminate.
[0002] Vinyl chloride resins are generally used in a variety of applications due to their excellent properties, such as cold resistance, heat resistance, and oil resistance. For example, laminates in which a vinyl chloride resin molded product and a polyurethane foam molded product are laminated adjacent to each other are used to form automobile interior parts such as automobile instrument panels and door trims. Techniques for producing such laminates have been investigated.
[0003] For example, in Patent Document 1, a vinyl chloride resin composition containing vinyl chloride resin, a plasticizer, and additives such as a hydrotalcite-based stabilizer, a zeolite-based stabilizer, and β-diketones is powder-molded to prepare a vinyl chloride resin molded body, and a foamed polyurethane molded body is laminated onto this vinyl chloride resin molded body to produce a laminate.
[0004] International Publication No. 2020 / 090556
[0005] Here, conventional laminates of vinyl chloride resin molded articles and polyurethane foam molded articles, including the one disclosed in Patent Document 1, have had the problem that the vinyl chloride resin molded article discolors (particularly yellows) when exposed to high temperature conditions. In other words, conventional laminates have room for improvement in terms of suppressing discoloration of the vinyl chloride resin molded article under high temperature conditions.
[0006] Therefore, an object of the present invention is to provide a laminate of a vinyl chloride resin molded article and a polyurethane foam molded article, in which discoloration of the vinyl chloride resin molded article under high-temperature conditions is suppressed, and a method for producing the laminate.
[0007] The present inventors have conducted extensive research to solve the above-mentioned problems, and have found that discoloration of vinyl chloride resin molded articles under high temperature conditions can be suppressed by using a vinyl chloride resin composition containing an aliphatic dicarboxylate in addition to vinyl chloride resin and a plasticizer in the production of vinyl chloride resin molded articles that constitute a laminate, and have completed the present invention based on this finding.
[0008] That is, the present invention aims to advantageously solve the above problems, and provides laminates [1] to [6] and methods for manufacturing laminates [7] to
[12] .
[0009] [1] A laminate having a vinyl chloride resin molded article and a foamed polyurethane molded article laminated adjacent to the vinyl chloride resin molded article, wherein the vinyl chloride resin molded article is a molded article obtained by molding a vinyl chloride resin composition containing vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer. In a laminate of the vinyl chloride resin molded article, which is a molded article of a vinyl chloride resin composition containing vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer, and the foamed polyurethane molded article, the vinyl chloride resin molded article is resistant to discoloration when exposed to high temperature conditions.
[0010] [2] The laminate according to [1] above, wherein the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is 0.30 parts by mass or more and 8.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin. When the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is within the above range, discoloration of the vinyl chloride resin molded article constituting the laminate under high-temperature conditions can be further suppressed. Furthermore, when a vinyl chloride resin molded article is produced from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved.
[0011] [3] The laminate according to [1] or [2] above, wherein the aliphatic dicarboxylate comprises at least one selected from the group consisting of disodium maleate, disodium malonate, disodium succinate, disodium adipate, and disodium sebacate. Using any of the above aliphatic dicarboxylates as the aliphatic dicarboxylate further suppresses discoloration of a vinyl chloride resin molded article constituting the laminate under high-temperature conditions. Furthermore, when a vinyl chloride resin molded article is produced from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved.
[0012] [4] The laminate according to any one of [1] to [3] above, wherein the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin. By controlling the content of the plasticizer in the vinyl chloride resin composition within the above range, the flexibility and light resistance of the vinyl chloride resin molded article constituting the laminate can be improved. Furthermore, when producing a vinyl chloride resin molded article from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved. In addition, the meltability of the vinyl chloride resin composition can be improved, while the surface smoothness of the vinyl chloride resin molded article can be improved.
[0013] [5] The laminate according to any one of [1] to [4] above, wherein the plasticizer comprises a polyester containing a structural unit derived from adipic acid and a structural unit derived from a polyhydric alcohol. Using the polyester as a plasticizer can improve the light resistance and heat shrinkage resistance of the vinyl chloride resin molded article constituting the laminate. Furthermore, when producing a vinyl chloride resin molded article from the vinyl chloride resin composition, the powder fluidity of the vinyl chloride resin composition can be improved. Additionally, the meltability of the vinyl chloride resin composition can be increased while improving the surface smoothness of the vinyl chloride resin molded article.
[0014] [6] The laminate according to any one of [1] to [5] above, which is used for an automobile instrument panel.
[0015] [7] A method for producing a laminate, comprising the steps of: molding a vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer to obtain a vinyl chloride resin molded body; and laminating a foamed polyurethane molded body on the surface of the vinyl chloride resin molded body to obtain a laminate in which the vinyl chloride resin molded body and the foamed polyurethane molded body are adjacently laminated. In the laminate of the foamed polyurethane molded body and the vinyl chloride resin molded body obtained by molding the vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer, the vinyl chloride resin molded body is resistant to discoloration when exposed to high-temperature conditions.
[0016] [8] The method for producing a laminate according to [7], wherein the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is 0.30 parts by mass or more and 8.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin. When the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is within the above range, discoloration of a vinyl chloride resin molded article constituting the laminate under high-temperature conditions can be further suppressed. Furthermore, when a vinyl chloride resin molded article is produced from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved.
[0017] [9] The method for producing a laminate according to [7] or [8], wherein the aliphatic dicarboxylate comprises at least one selected from the group consisting of disodium maleate, disodium malonate, disodium succinate, disodium adipate, and disodium sebacate. Using any of the above aliphatic dicarboxylates as the aliphatic dicarboxylate further suppresses discoloration of a vinyl chloride resin molded article constituting the laminate under high-temperature conditions. Furthermore, when a vinyl chloride resin molded article is produced from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved.
[0018]
[10] The method for producing a laminate according to any one of [7] to [9], wherein the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin. By controlling the content of the plasticizer in the vinyl chloride resin composition within the above range, the flexibility and light resistance of the vinyl chloride resin molded article constituting the laminate can be improved. Furthermore, when producing a vinyl chloride resin molded article from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved. In addition, the meltability of the vinyl chloride resin composition can be improved, while the surface smoothness of the vinyl chloride resin molded article can be improved.
[0019]
[11] The method for producing a laminate according to any one of [7] to
[10] above, wherein the plasticizer comprises a polyester containing a structural unit derived from adipic acid and a structural unit derived from a polyhydric alcohol. Using the polyester as a plasticizer can improve the light resistance and heat shrinkage resistance of the vinyl chloride resin molded article constituting the laminate. Furthermore, when producing a vinyl chloride resin molded article from the vinyl chloride resin composition, the powder flowability of the vinyl chloride resin composition can be improved. Additionally, the meltability of the vinyl chloride resin composition can be increased while improving the surface smoothness of the vinyl chloride resin molded article.
[0020]
[12] The method for producing a laminate according to any one of [7] to
[11] above, wherein the vinyl chloride resin composition is powder slush molded to obtain the vinyl chloride resin molded article. By powder slush molding the vinyl chloride resin composition to produce a vinyl chloride resin molded article, it is possible to easily obtain a vinyl chloride resin molded article that can be favorably used as an automotive interior material, for example, a skin for an automotive instrument panel.
[0021] According to the present invention, it is possible to provide a laminate of a vinyl chloride resin molded article and a polyurethane foam molded article, in which discoloration of the vinyl chloride resin molded article under high-temperature conditions is suppressed, and a method for producing the laminate.
[0022] Hereinafter, embodiments of the present invention will be described in detail. The laminate of the present invention can be suitably used as an automobile interior material used in producing automobile interior parts such as automobile instrument panels and door trims. The method for producing the laminate of the present invention can be used in producing the laminate of the present invention.
[0023] (Laminate) The laminate of the present invention is formed by stacking a vinyl chloride resin molded article and a polyurethane foam molded article adjacent to each other. The vinyl chloride resin molded article usually constitutes one surface of the laminate. The laminate may have any component other than the vinyl chloride resin molded article and the polyurethane foam molded article depending on its application.
[0024] Furthermore, in the laminate of the present invention, the vinyl chloride resin molded article is formed from a vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer, and therefore the vinyl chloride resin molded article is less likely to discolor when exposed to high-temperature conditions. The reason why molding a vinyl chloride resin molded article using the vinyl chloride resin composition as described above can suppress discoloration of the vinyl chloride resin molded article when the laminate is exposed to high-temperature conditions is not clear, but is presumed to be as follows.
[0025] First, polyurethane foam moldings may contain residual amine components used as polymerization catalysts. In laminates of vinyl chloride resin moldings and foamed polyurethane moldings, these amine components may migrate from the foamed polyurethane molding to the vinyl chloride resin molding, especially under high-temperature conditions. The inventors' investigations have revealed that hydrogen chloride is released from the vinyl chloride resin through reaction with the amine components, causing discoloration of the vinyl chloride resin molding. In contrast, in the laminates of the present invention, the vinyl chloride resin moldings contain aliphatic dicarboxylates derived from the vinyl chloride resin composition, which can deactivate the amine components. In particular, the aliphatic dicarboxylates contain two carboxylic acid groups, rather than one, and therefore can strongly capture the amine components through the crosslinked structure between the carboxylic acid groups. This is believed to suppress hydrogen chloride release from the vinyl chloride resin due to the amine components, thereby preventing discoloration of the vinyl chloride resin moldings.
[0026] <Vinyl chloride resin molded article> A vinyl chloride resin molded article is a molded article of a vinyl chloride resin composition. Here, the vinyl chloride resin composition contains a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer, and may optionally contain additives other than the vinyl chloride resin, the aliphatic dicarboxylate, and the plasticizer. Note that, since the vinyl chloride resin molded article is obtained by molding the vinyl chloride resin composition, the mass ratio of each blended component in the vinyl chloride resin molded article is usually the same as the mass ratio of each blended component in the vinyl chloride resin composition.
[0027] <<Vinyl Chloride Resin>> As the vinyl chloride resin, a particulate vinyl chloride resin is usually used. The vinyl chloride resin may contain, for example, one or more types of vinyl chloride resin particles, and may optionally further contain one or more types of vinyl chloride resin microparticles. Among these, the vinyl chloride resin preferably contains at least vinyl chloride resin particles, and more preferably contains vinyl chloride resin particles and vinyl chloride resin microparticles. The vinyl chloride resin may be produced by any conventionally known production method, such as suspension polymerization, emulsion polymerization, solution polymerization, or bulk polymerization. In this specification, "resin particles" refers to particles having a particle diameter of 30 μm or more, and "resin microparticles" refers to particles having a particle diameter of less than 30 μm.
[0028] Examples of vinyl chloride resins include homopolymers composed of vinyl chloride monomer units, as well as vinyl chloride copolymers containing preferably 50% by mass or more, more preferably 70% by mass or more, of vinyl chloride monomer units. Specific examples of monomers (comonomers) copolymerizable with vinyl chloride monomers that can constitute vinyl chloride copolymers include those described in International Publication No. WO 2016 / 098344. These components may be used alone or in combination of two or more in any ratio.
[0029] [Vinyl chloride resin particles] In the vinyl chloride resin composition, the vinyl chloride resin particles usually function as a matrix resin (substrate). The vinyl chloride resin particles are preferably produced by a suspension polymerization method.
[0030] -Average Degree of Polymerization- The average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is preferably 800 or more, more preferably 1000 or more, and preferably 5000 or less, more preferably 3000 or less, and even more preferably 2800 or less. When the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is 800 or more, the physical strength of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be sufficiently high, while, for example, tensile properties, particularly tensile elongation, can be improved. Furthermore, a vinyl chloride resin molded article with good tensile elongation can be suitably used as an automotive interior material, such as the surface of an automobile instrument panel, which has excellent ductility and breaks as designed without scattering fragments when an airbag is inflated and deployed. On the other hand, when the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles is 5000 or less, the meltability of the vinyl chloride resin composition can be improved, and the surface smoothness of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be enhanced. The average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin particles may be 1400 or more, 1500 or more, or 1600 or more, or may be 1600 or less, 1500 or less, or 1400 or less. In this specification, the "average degree of polymerization" can be measured in accordance with JIS K6720-2.
[0031] -Average Particle Diameter- The average particle diameter of the vinyl chloride resin particles is typically 30 μm or more, preferably 50 μm or more, more preferably 100 μm or more, and preferably 500 μm or less, and more preferably 200 μm or less. When the average particle diameter of the vinyl chloride resin particles is 30 μm or more, the powder fluidity of the vinyl chloride resin composition can be improved. On the other hand, when the average particle diameter of the vinyl chloride resin particles is 500 μm or less, the meltability of the vinyl chloride resin composition can be improved, thereby increasing the surface smoothness of a vinyl chloride resin molded article formed using the vinyl chloride resin composition. In this specification, the "average particle diameter" can be measured as the volume average particle diameter by laser diffraction in accordance with JIS Z8825.
[0032] -Content- The content of vinyl chloride resin particles in the vinyl chloride resin is preferably 70% by mass or more, more preferably 80% by mass or more, and can be 100% by mass, and is preferably 95% by mass or less, and more preferably 90% by mass or less. When the content of vinyl chloride resin particles in the vinyl chloride resin is 70% by mass or more, the tensile elongation of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be improved while ensuring a sufficiently high physical strength. On the other hand, when the content of vinyl chloride resin particles in the vinyl chloride resin is 95% by mass or less, the powder flowability of the vinyl chloride resin composition can be improved.
[0033] [Vinyl chloride resin fine particles] In the vinyl chloride resin composition, the vinyl chloride resin fine particles usually function as a dusting agent (powder flow improver). The vinyl chloride resin fine particles are preferably produced by emulsion polymerization.
[0034] -Average Degree of Polymerization- The average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is preferably 500 or more, more preferably 700 or more, and preferably 2600 or less, and more preferably 2400 or less. If the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles as a dusting agent is 500 or more, the powder fluidity of the vinyl chloride resin composition can be improved and the tensile elongation of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be improved. On the other hand, if the average degree of polymerization of the vinyl chloride resin constituting the vinyl chloride resin microparticles is 2600 or less, the meltability of the vinyl chloride resin composition can be improved, and the surface smoothness of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be increased.
[0035] -Average particle size- Furthermore, the average particle size of the vinyl chloride resin fine particles is usually less than 30 μm, preferably 10 μm or less, more preferably 5 μm or less, preferably 0.1 μm or more, and more preferably 1 μm or more. If the average particle size of the vinyl chloride resin fine particles is 0.1 μm or more, the powder fluidity of the vinyl chloride resin composition can be improved, for example, without excessively reducing the size as a dusting agent. On the other hand, if the average particle size of the vinyl chloride resin fine particles is less than 30 μm, the meltability of the vinyl chloride resin composition can be improved, and the surface smoothness of the vinyl chloride resin molded article formed can be increased.
[0036] [Content] The content of vinyl chloride resin microparticles in the vinyl chloride resin may be 0% by mass, but is preferably 5% by mass or more, more preferably 10% by mass or more, and preferably 30% by mass or less, and more preferably 20% by mass or less. If the content of vinyl chloride resin microparticles in the vinyl chloride resin is 5% by mass or more, the powder fluidity of the vinyl chloride resin composition can be improved. On the other hand, if the content of vinyl chloride resin microparticles in the vinyl chloride resin is 30% by mass or less, the physical strength of a vinyl chloride resin molded article formed using the vinyl chloride resin composition can be increased.
[0037] <Aliphatic dicarboxylate> In the laminate of the present invention, the aliphatic dicarboxylate is a component that can suppress discoloration of a vinyl chloride resin molded article under high-temperature conditions, as described above. The aliphatic dicarboxylate is also a component that can function as a powder flowability improver for a vinyl chloride resin composition when producing a vinyl chloride resin molded article from the vinyl chloride resin composition. The aliphatic dicarboxylate may be used alone or in combination of two or more at any ratio.
[0038] Here, the aliphatic dicarboxylic acid salt is not particularly limited as long as the aliphatic dicarboxylic acid is in the form of a salt. Preferred salt forms include sodium salts, potassium salts, and calcium salts, and among these, sodium salts are particularly preferred from the viewpoint of further suppressing discoloration of vinyl chloride resin molded articles under high-temperature conditions. It should be noted that the aliphatic dicarboxylic acid must be used in the form of a salt, i.e., as an aliphatic dicarboxylic acid salt. If an aliphatic dicarboxylic acid is used instead of an aliphatic dicarboxylic acid salt, discoloration of the vinyl chloride resin molded article constituting the laminate under high-temperature conditions cannot be sufficiently suppressed.
[0039] The aliphatic dicarboxylic acid constituting the aliphatic dicarboxylate is not particularly limited as long as it is an aliphatic compound having two carboxylic acid groups, but from the viewpoint of enhancing the fluidity of the vinyl chloride resin composition and further suppressing discoloration of vinyl chloride resin molded articles under high-temperature conditions, preferred examples include maleic acid, malonic acid, succinic acid, adipic acid, and sebacic acid. Of these, maleic acid is particularly preferred from the viewpoint of further suppressing discoloration of vinyl chloride resin molded articles under high-temperature conditions.
[0040] In the laminate of the present invention, from the viewpoint of further suppressing discoloration of vinyl chloride resin molded articles under high-temperature conditions while increasing the fluidity of the vinyl chloride resin composition, the aliphatic dicarboxylate is preferably a compound represented by the formula: NaOOC-R-COONa (wherein R is an aliphatic group having from 1 to 8 carbon atoms), and more preferably disodium maleate, disodium malonate, disodium succinate, disodium adipate, or disodium sebacate. Of these, disodium maleate is particularly preferred from the viewpoint of further suppressing discoloration of vinyl chloride resin molded articles under high-temperature conditions.
[0041] Here, from the viewpoint of further suppressing discoloration of a vinyl chloride resin molded article under high-temperature conditions while increasing the fluidity of the vinyl chloride resin composition, the content of the aliphatic dicarboxylate salt in the vinyl chloride resin composition is preferably 0.30 parts by mass or more, more preferably 0.40 parts by mass or more, and even more preferably 2.00 parts by mass or more, and is preferably 8.00 parts by mass or less, and more preferably 7.00 parts by mass or less, per 100 parts by mass of vinyl chloride resin. When disodium maleate is used as the aliphatic dicarboxylate, the content of disodium maleate in the vinyl chloride resin composition is, from the viewpoint of further suppressing discoloration of a vinyl chloride resin molded article under high-temperature conditions, preferably 0.30 parts by mass or more, more preferably 0.40 parts by mass or more, even more preferably 1.00 parts by mass or more, still more preferably 2.00 parts by mass or more, and preferably 8.00 parts by mass or less, more preferably 7.00 parts by mass or less, even more preferably 5.00 parts by mass or less, still more preferably 4.00 parts by mass or less, and particularly preferably 3.00 parts by mass or less, per 100 parts by mass of vinyl chloride resin.
[0042] <Plasticizer> A plasticizer is a component that can impart flexibility to a vinyl chloride resin molded article formed using a vinyl chloride resin composition. Furthermore, by using a plasticizer in a vinyl chloride resin composition, the meltability of the vinyl chloride resin composition is increased, which facilitates molding (particularly powder molding) into a vinyl chloride resin molded article and increases the surface smoothness of the vinyl chloride resin molded article formed. One type of plasticizer may be used alone, or two or more types may be used in combination at any ratio.
[0043] Here, the content of the plasticizer in the vinyl chloride resin composition is preferably 50 parts by mass or more, more preferably 75 parts by mass or more, even more preferably 80 parts by mass or more, even more preferably 85 parts by mass or more, particularly preferably 90 parts by mass or more, and preferably 200 parts by mass or less, more preferably 185 parts by mass or less, and even more preferably 150 parts by mass or less, per 100 parts by mass of vinyl chloride resin. If the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more per 100 parts by mass of vinyl chloride resin, the meltability of the vinyl chloride resin composition can be sufficiently improved and sufficient flexibility can be imparted to the vinyl chloride resin molded article formed. Furthermore, if the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more per 100 parts by mass of vinyl chloride resin, the powder flowability of the vinyl chloride resin composition can be improved. On the other hand, if the content of the plasticizer in the vinyl chloride resin composition is 200 parts by mass or less per 100 parts by mass of vinyl chloride resin, the light resistance of the vinyl chloride resin molded article formed can be improved.
[0044] Here, the vinyl chloride resin composition preferably contains, as a plasticizer, at least a polyester containing a structural unit derived from adipic acid and a structural unit derived from a polyhydric alcohol, and more preferably contains both the polyester and a plasticizer other than the polyester (hereinafter referred to as "other plasticizer").
[0045] <<Polyester>> As described above, the polyester contains a structural unit derived from adipic acid and a structural unit derived from a polyhydric alcohol. By including the polyester as a plasticizer, the vinyl chloride resin composition can exhibit excellent melting properties. Furthermore, the polyester improves the powder fluidity of the vinyl chloride resin composition and can also enhance the light resistance and heat shrinkage resistance of the vinyl chloride resin molded article formed therefrom.
[0046] [Composition] The polyester preferably contains a structural unit derived from 2-methyl-1,3-propanediol as the polyhydric alcohol-derived structural unit. The polyester may also contain a structural unit derived from a polyhydric alcohol other than 2-methyl-1,3-propanediol (hereinafter, sometimes referred to as "other polyhydric alcohols").
[0047] The content of 2-methyl-1,3-propanediol-derived structural units among the polyhydric alcohol-derived structural units is preferably greater than 70 mol%, more preferably 80 mol% or greater, even more preferably 90 mol% or greater, and even more preferably 95 mol% or greater, when the total amount of polyhydric alcohol-derived structural units contained in the polyester is taken as 100 mol%. When the content of 2-methyl-1,3-propanediol-derived structural units among the total amount of polyhydric alcohol-derived structural units contained in the polyester is greater than 70%, the meltability and powder flowability of the vinyl chloride resin composition can be sufficiently improved, and the light resistance of the vinyl chloride resin molded article formed can be sufficiently enhanced. Furthermore, from the viewpoint of improving the meltability and powder flowability of the vinyl chloride resin composition and the light resistance of the vinyl chloride resin molded article formed, the content of 2-methyl-1,3-propanediol-derived structural units among the polyhydric alcohol-derived structural units is particularly preferably 100 mol%, when the total amount of polyhydric alcohol-derived structural units contained in the polyester is taken as 100 mol%. That is, it is particularly preferable that the polyester contains only structural units derived from 2-methyl-1,3-propanediol as structural units derived from polyhydric alcohols.
[0048] Examples of polyhydric alcohols other than 2-methyl-1,3-propanediol that can form structural units derived from other polyhydric alcohols in polyesters include 1,2-propylene glycol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,2-dimethyl-1,3-propanediol, and 3-methyl-1,5-pentanediol.
[0049] The content of structural units derived from other polyhydric alcohols in the structural units derived from polyhydric alcohols is preferably less than 30 mol%, more preferably 20 mol% or less, even more preferably 10 mol% or less, and even more preferably 5 mol% or less, when the total amount of structural units derived from polyhydric alcohols contained in the polyester is taken as 100 mol%. If the content of structural units derived from other polyhydric alcohols in the total amount of structural units derived from polyhydric alcohols contained in the polyester is less than 30 mol%, the meltability and powder flowability of the vinyl chloride resin composition can be further improved, and the light resistance of the vinyl chloride resin molded article formed can be further increased. From the viewpoint of improving the meltability and powder flowability of the vinyl chloride resin composition and the light resistance of the vinyl chloride resin molded article formed, the content of structural units derived from other polyhydric alcohols in the structural units derived from polyhydric alcohols is particularly preferably 0 mol%, when the total amount of structural units derived from polyhydric alcohols contained in the polyester is taken as 100 mol%. That is, it is particularly preferable that the polyester does not contain, as the structural units derived from polyhydric alcohols, structural units derived from polyhydric alcohols other than 2-methyl-1,3-propanediol.
[0050] Although the polyester may contain structural units derived from polycarboxylic acids other than adipic acid as structural units derived from polycarboxylic acids, the content of structural units derived from adipic acid in the total amount of structural units derived from polycarboxylic acids in the polyester is preferably 50 mol % or more, more preferably 80 mol % or more, and particularly preferably 100 mol %. That is, it is particularly preferable that the polyester contains only structural units derived from adipic acid as structural units derived from polycarboxylic acids.
[0051] [Production Method] The polyester can be obtained by condensation polymerization of adipic acid and a polyhydric alcohol, without any particular limitation. The condensation polymerization can be carried out in the presence of a catalyst. The condensation polymerization can be carried out using an alcohol and / or a monobasic acid as a terminal-terminating component. The condensation polymerization of adipic acid and a polyhydric alcohol and the termination reaction of the resulting condensation polymer with the terminal-terminating component can be carried out simultaneously or separately. The product obtained through the condensation polymerization and termination reaction can be subjected to post-treatment such as distillation. The reaction conditions for the condensation polymerization, such as the amounts of adipic acid and polyhydric alcohol as the monomers, catalyst, and terminal-terminating component, can be any known conditions. The polyester can also be a commercially available product.
[0052] The catalyst used in the condensation polymerization reaction is not particularly limited, and examples thereof include dibutyltin oxide and tetraalkyl titanate.
[0053] Examples of alcohols that can be used as end-stopping components include methanol, ethanol, propanol, isopropanol, butanol, isobutanol, pentanol, hexanol, isohexanol, heptanol, isoheptanol, octanol, isooctanol, 2-ethylhexanol, nonanol, isononanol, decanol, isodecanol, undecanol, isoundecanol, dodecanol, tridecanol, isotridecanol, tetradecanol, pentadecanol, hexadecanol, heptadecanol, octadecanol, cellosolve, carbitol, phenol, nonylphenol, benzyl alcohol, and mixtures thereof. Furthermore, examples of monobasic acids that can be used as end-stopping components include acetic acid, propionic acid, butyric acid, isobutyric acid, valeric acid, pivalic acid, caproic acid, heptanoic acid, caprylic acid, 2-ethylhexylic acid, pelargonic acid, capric acid, undecanoic acid, lauric acid, tridecanoic acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, stearic acid, benzoic acid, and mixtures thereof. Among these, 2-ethylhexanol is preferred as the end-stopping component.
[0054] [Physical Properties, etc.] The weight average molecular weight of the polyester is preferably 1,000 or more, more preferably 2,000 or more, and even more preferably 3,000 or more, and is preferably 10,000 or less, and more preferably 7,000 or less. In this specification, the "weight average molecular weight" of the polyester can be determined as a polystyrene-equivalent value by gel permeation chromatography (GPC) using tetrahydrofuran as a solvent.
[0055] The acid value of the polyester is preferably 0.5 mgKOH / g or more and 2 mgKOH / g or less. Furthermore, the hydroxyl value of the polyester is preferably 30 mgKOH / g or less, more preferably 10 mgKOH / g or less, and even more preferably 7 mgKOH / g or less. In this specification, the "acid value" and "hydroxyl value" of the polyester can be measured using a method in accordance with JIS K0070.
[0056] The viscosity of the polyester is preferably 500 mPa·s or more, more preferably 1000 mPa·s or more, and is preferably 8000 mPa·s or less, more preferably 5000 mPa·s or less, and even more preferably 3000 mPa·s or less. In this specification, the "viscosity" of the polyester can be measured in accordance with JIS Z8803 at a temperature of 23°C.
[0057] [Content, etc.] The content of the polyester in the vinyl chloride resin composition is preferably more than 30 parts by mass per 100 parts by mass of vinyl chloride resin, more preferably 50 parts by mass or more, even more preferably 70 parts by mass or more, even more preferably 80 parts by mass or more, particularly preferably 85 parts by mass or more, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 140 parts by mass or less. If the content of the polyester in the vinyl chloride resin composition is more than 30 parts by mass per 100 parts by mass of vinyl chloride resin, the meltability and powder flowability of the vinyl chloride resin composition, as well as the light resistance and heat shrinkage resistance of the vinyl chloride resin molded article formed can be improved. On the other hand, if the content of the polyester in the vinyl chloride resin composition is 200 parts by mass or less per 100 parts by mass of vinyl chloride resin, the light resistance of the vinyl chloride resin molded article formed can be improved.
[0058] The content of polyester in the plasticizer is preferably 50% by mass or more, more preferably 65% by mass or more, even more preferably 90% by mass or more, even more preferably 93% by mass or more, and particularly preferably 95% by mass or more, based on the total mass of the plasticizer being 100% by mass. It can be 100% by mass or less, preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less. When the content of polyester in the plasticizer is 50% by mass or more, the meltability and powder flowability of the vinyl chloride resin composition, as well as the light resistance and heat shrinkage resistance of the vinyl chloride resin molded article formed can be improved. On the other hand, when the content of polyester in the plasticizer is 99% by mass or less, the light resistance of the vinyl chloride resin molded article formed can be improved.
[0059] <<Other Plasticizers>> The content of the other plasticizer in the vinyl chloride resin composition can be 0 parts by mass or more, preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, still more preferably 2 parts by mass or more, and preferably 40 parts by mass or less, more preferably 35 parts by mass or less, even more preferably 20 parts by mass or less, still more preferably 10 parts by mass or less, and particularly preferably 7 parts by mass or less, per 100 parts by mass of the vinyl chloride resin. If the content of the other plasticizer in the vinyl chloride resin composition is 0.5 parts by mass or more per 100 parts by mass of the vinyl chloride resin, the flexibility of the formed vinyl chloride resin molded article can be increased. On the other hand, if the content of the other plasticizer in the vinyl chloride resin composition is 40 parts by mass or less, the powder fluidity of the vinyl chloride resin composition can be improved.
[0060] Furthermore, the content of the other plasticizer in the plasticizer can be 0% by mass or more, preferably 1% by mass or more, more preferably 2% by mass or more, even more preferably 3% by mass or more, even more preferably 4.2% by mass or more, and preferably 50% by mass or less, more preferably 35% by mass or less, even more preferably 10% by mass or less, even more preferably 7% by mass or less, and particularly preferably 5% by mass or less, where the total mass of the plasticizer is 100% by mass. If the content of the other plasticizer in the plasticizer is 1% by mass or more, the flexibility of the vinyl chloride resin molded article formed can be further enhanced. On the other hand, if the content of the other plasticizer in the plasticizer is 50% by mass or less, the powder fluidity of the vinyl chloride resin composition can be improved.
[0061] Examples of the other plasticizer include plasticizers other than the polyesters described above among the plasticizers described in International Publication No. 2016 / 098344. More specifically, trimellitic acid esters and epoxidized vegetable oils can be used as the other plasticizer, and epoxidized vegetable oils are preferably used.
[0062] [Epoxidized Vegetable Oil] Examples of the epoxidized vegetable oil that can be used include epoxidized soybean oil, epoxidized linseed oil, etc. Among these, it is preferable to use epoxidized soybean oil as the epoxidized vegetable oil from the viewpoint of improving the tensile properties of the vinyl chloride resin molded article to be formed at low temperatures.
[0063] The content of the epoxidized vegetable oil in the vinyl chloride resin composition is preferably 2 to 7 parts by mass per 100 parts by mass of the vinyl chloride resin. When the content of the epoxidized vegetable oil in the vinyl chloride resin composition is within the above range, the tensile properties of the resulting vinyl chloride resin molded article at low temperatures can be improved.
[0064] The content of the epoxidized vegetable oil in the plasticizer is preferably 1% by mass or less, more preferably 2% by mass or more, even more preferably 3% by mass or more, still more preferably 3.5% by mass or more, and preferably 10% by mass or less, more preferably 7% by mass or less, and even more preferably 5% by mass or less. If the content of the epoxidized vegetable oil in the plasticizer is within the above range, the tensile properties of the resulting vinyl chloride resin molded article at low temperatures can be improved.
[0065] <Additives> In addition to the components described above, the vinyl chloride resin composition of the present invention may further contain various additives. Examples of additives include, but are not limited to, lubricants; stabilizers such as perchloric acid-treated hydrotalcite, zeolite, β-diketone, fatty acid metal salt, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butylmalonate (light stabilizer), and 6-amino-1,3-dimethyluracil; release agents; dusting agents other than the above-mentioned vinyl chloride resin fine particles; impact modifiers; perchlorate compounds other than perchloric acid-treated hydrotalcite (sodium perchlorate, potassium perchlorate, etc.); antioxidants; mildew inhibitors; flame retardants; antistatic agents; fillers; foaming agents; pigments; and the like. As the additives that can be contained in the vinyl chloride resin composition of the present invention, for example, those described in WO 2016 / 098344 can be used, and the preferred contents thereof can also be the same.
[0066] <Method for Preparing Vinyl Chloride Resin Composition> The vinyl chloride resin composition used to produce a vinyl chloride resin molded article can be prepared by mixing the above-mentioned components. The method for mixing the vinyl chloride resin, aliphatic dicarboxylate, plasticizer, and various additives further blended as needed is not particularly limited, and examples thereof include a method in which the components excluding the dusting agent (including vinyl chloride resin fine particles) are mixed by dry blending, and then the dusting agent is added and mixed. A Henschel mixer is preferably used for dry blending. The temperature during dry blending is not particularly limited, and is preferably 50°C or higher, more preferably 70°C or higher, and preferably 200°C or lower.
[0067] <Polyurethane foam molded body> The polyurethane foam molded body is not particularly limited, and a known polyurethane foam molded body obtained by reacting isocyanates with polyols or the like to polymerize and foam the polyurethane can be used. The isocyanates and polyols are not particularly limited, and known ones can be used. The polymerization and foaming methods are also not particularly limited, and known methods can be used. The polymerization catalyst used for the reaction of isocyanates with polyols is not particularly limited, and examples thereof include amine components such as triethylenediamine, triethanolamine, and triethylamine.
[0068] (Method for Producing Laminate) The laminate of the present invention described above can be produced using the method for producing a laminate of the present invention, although it is not particularly limited thereto. The method for producing a laminate of the present invention includes a step of molding a vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer to obtain a vinyl chloride resin molded body (molded body forming step), and a step of laminating a foamed polyurethane molded body on the surface of the vinyl chloride resin molded body obtained in the molded body forming step to obtain a laminate in which the vinyl chloride resin molded body and the foamed polyurethane molded body are laminated adjacent to each other (laminate forming step). The method for producing a laminate of the present invention may optionally include steps other than the molded body forming step and the laminate forming step. Furthermore, according to the method for producing a laminate of the present invention, a laminate in which discoloration of the vinyl chloride resin molded body under high-temperature conditions is suppressed can be efficiently produced.
[0069] <Molded Body Forming Step> In the molded body forming step, a vinyl chloride resin composition containing at least a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer, and optionally containing additives, is molded to obtain a vinyl chloride resin molded body. Here, the “vinyl chloride resin,” “aliphatic dicarboxylate,” “plasticizer,” and “additives” are the same as those described above in the “Laminate” section, and preferred examples and preferred contents thereof are also the same as those described above in the “Laminate” section.
[0070] The molding method for molding the vinyl chloride resin composition into a vinyl chloride resin molded article is not particularly limited, and any known molding method can be used. As the molding method, powder slush molding is preferred from the viewpoint of easily obtaining a vinyl chloride resin molded article that can be favorably used as an automobile interior material, such as a skin for an automobile instrument panel.
[0071] When a vinyl chloride resin molded article is formed by powder slush molding, the mold temperature during powder slush molding is not particularly limited, but is preferably 200°C or higher, more preferably 220°C or higher, and is preferably 300°C or lower, more preferably 280°C or lower.
[0072] The vinyl chloride resin molded article can be produced by any method, including, but not limited to, the following method. Specifically, the vinyl chloride resin composition of the present invention is sprinkled onto a mold at a temperature within the above range, and the mold is left standing for 5 to 30 seconds. The excess vinyl chloride resin composition is then shaken off, and the mold is then left standing at a given temperature for 30 seconds to 3 minutes. The mold is then cooled to 10 to 60°C, and the resulting vinyl chloride resin molded article is released from the mold. A sheet-like molded article conforming to the shape of the mold is then obtained.
[0073] <Laminate Forming Step> In the laminate forming step, a polyurethane foam molded body is laminated (backed) on the surface of the vinyl chloride resin molded body obtained in the molded body forming step to obtain a laminate of the vinyl chloride resin molded body and the polyurethane foam molded body.
[0074] The method for laminating a vinyl chloride resin molded body and a polyurethane foam molded body is not particularly limited, and the following methods can be used, for example. That is, (1) a method in which a vinyl chloride resin molded body and a polyurethane foam molded body are separately prepared and then bonded together by heat fusion, heat adhesion, or using a known adhesive, etc.; (2) a method in which isocyanates and polyols, which are raw materials for the polyurethane foam molded body, are reacted on the vinyl chloride resin molded body to polymerize and foam the polyurethane, thereby directly forming a polyurethane foam molded body on the vinyl chloride resin molded body; etc. Among these, the latter method (2) is preferred because of its simple process and the ease with which the vinyl chloride resin molded body and the polyurethane foam molded body can be firmly bonded together even when laminates of various shapes are obtained.
[0075] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples. In the following description, "%" and "parts" representing amounts are based on mass unless otherwise specified. The powder flowability of the vinyl chloride resin composition and the discoloration suppression under high temperature conditions of the vinyl chloride resin molded article constituting the laminate were evaluated by the following methods.
[0076] <Powder fluidity> The vinyl chloride resin compositions obtained in the Examples and Comparative Examples were poured from the funnel of a powder property tester (manufactured by Nippon Oil Testing Instruments Co., Ltd., model "TESTERTYPE 6721") into a 100 cc brass cylinder, thereby filling the cylinder with the vinyl chloride resin composition. Thereafter, the vinyl chloride resin composition was again poured from the cylinder into the funnel and dropped onto a flat plate. The time (seconds) until all of the vinyl chloride resin composition had dropped was measured, and this was recorded as the number of seconds until the drop. A shorter number of seconds until the drop indicates that the vinyl chloride resin composition has better powder fluidity. <Suppression of discoloration> The color tone of the surface (embossed surface) of the laminate obtained in the Examples and Comparative Examples facing the vinyl chloride resin molded product was measured using a spectrophotometer (manufactured by Konica Minolta, model "CM-700d"). More specifically, the entire grained surface was divided into nine sections, and a total of nine points, each at the center of each section, were measured. The nine E values obtained were * The average value of E 0 * The laminate was then subjected to a high-temperature treatment at 120°C for 400 hours in a gear oven. The laminate after the high-temperature treatment was subjected to color measurement in the same manner as above, and the resulting E * The average value of E 1 * Then, the formula: ΔE * = E 1 * -E 0 * From ΔE * was calculated. * The smaller the value, the more the discoloration of the vinyl chloride resin molded article under high temperature conditions is suppressed.
[0077] (Preparation of Polyester A Containing Structural Units Derived from Adipic Acid and Structural Units Derived from Polyhydric Alcohols) Adipic acid as the polycarboxylic acid, 2-methyl-1,3-propanediol as the polyhydric alcohol, and 2-ethylhexanol as the stopper (terminal termination component) were charged into a reaction vessel, tetraisopropyl titanate was added as a catalyst, a solvent was added as appropriate, and the temperature was raised with stirring. The by-product water was removed under normal pressure and reduced pressure, and the temperature was finally raised to 220-230°C to complete the dehydration condensation reaction, yielding Polyester A (viscosity: 2800 mPa s, weight average molecular weight: 4200, acid value: 1.0 mgKOH / g, hydroxyl value: 5.5 mgKOH / g) consisting of 2-ethylhexoxy groups at the ends.
[0078] Example 1 Preparation of Vinyl Chloride Resin Composition The ingredients shown in Table 1, excluding the plasticizer (Polyester A and epoxidized soybean oil) and the vinyl chloride resin fine particles serving as a dusting agent, were mixed in a Henschel mixer. When the temperature of the mixture reached 80°C, all of the plasticizer was added, and the mixture was allowed to dry up (referring to the state in which the plasticizer was absorbed into the vinyl chloride resin particles, making the mixture smooth). When the dried mixture was cooled to 70°C or below, the vinyl chloride resin fine particles serving as a dusting agent were added to prepare a vinyl chloride resin composition. The powder flowability of the resulting vinyl chloride resin composition was evaluated. The results are shown in Table 3. Molded Body Formation Process The vinyl chloride resin composition obtained above was sprinkled onto a textured mold heated to 250°C, left to melt for a desired period of time, and then the excess vinyl chloride resin composition was shaken off. Thereafter, the textured mold onto which the vinyl chloride resin composition had been sprinkled was placed in an oven set at 200°C, and 60 seconds after being placed, the textured mold was cooled with cooling water. When the mold temperature had cooled to 40°C, a vinyl chloride resin molded article (vinyl chloride resin molded sheet) measuring 150 mm x 200 mm x 1 mm was removed from the mold. <Laminate Forming Step> Two vinyl chloride resin molded articles obtained above were placed in a 200 mm x 300 mm x 10 mm mold with the textured side facing down so that the two sheets did not overlap. Separately, a polyol mixture was obtained by mixing 50 parts of a PO (propylene oxide)-EO (ethylene oxide) block adduct of propylene glycol (hydroxyl value: 28 mg KOH / g, terminal EO unit content: 10%, internal EO unit content: 4%), 50 parts of a PO-EO block adduct of glycerin (hydroxyl value: 21 mg KOH / g, terminal EO unit content: 14%), 2.5 parts of water, 0.2 parts of an ethylene glycol solution of triethylenediamine (manufactured by Tosoh Corporation, trade name "TEDA-L33"), 1.2 parts of triethanolamine, 0.5 parts of triethylamine, and 0.5 parts of a foam stabilizer (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "F-122").A mixed solution was prepared by mixing the obtained polyol mixture with polymethylene polyphenylene polyisocyanate (polymeric MDI) in a ratio such that the index was 98. The prepared mixed solution was then poured onto two vinyl chloride resin molded sheets placed in a mold. The mold was then covered with an aluminum plate measuring 200 mm x 300 mm x 10 mm to seal the mold. After sealing the mold, the mold was left for 5 minutes, and a foamed polyurethane molded body (thickness: 9 mm, density: 0.18 g / cm) was formed on a vinyl chloride resin molded body (thickness: 1 mm) as a skin. 3 A laminate backed with the vinyl chloride resin film was formed in the mold. The formed laminate was removed from the mold, and the laminate was evaluated for its ability to inhibit discoloration of vinyl chloride resin molded articles under high-temperature conditions. The results are shown in Table 3.
[0079] (Examples 2 to 16, Comparative Example 1) Vinyl chloride resin compositions, vinyl chloride resin molded articles, and laminates were produced in the same manner as in Example 1, except that the types and / or amounts of the blending components used in preparing the vinyl chloride resin compositions were changed as shown in Tables 1 and 2. Evaluations were then carried out in the same manner as in Example 1. The results are shown in Tables 3 and 4.
[0080]
[0081]
[0082]
[0083]
[0084] 1) Shin-Dai-Ichi Vinyl Corporation, product name "ZEST (registered trademark) 1700ZI" (prepared by suspension polymerization, average degree of polymerization: 1700, average particle size: 129 μm) 2) Shin-Dai-Ichi Vinyl Corporation, product name "ZEST PQLTX" (prepared by emulsion polymerization, average degree of polymerization: 800, average particle size: 1.8 μm) 3) ADEKA Corporation, product name "ADEKA Cizer (registered trademark) O-130S" 4) Kyowa Chemical Industry Co., Ltd., product name "Alkamizer (registered trademark) 5" 5) Mizusawa Industrial Chemicals, Ltd., product name "MIZUKALIZER (registered trademark) DS" 6) Resonac Corporation, product name "Karends (registered trademark) DK-1" 7) BASF Corporation, product name "Tinuvin (registered trademark)" 144", bis(1,2,2,6,6-pentamethyl-4-piperidinyl)-[[3,5-bis(1,1-dimethylethyl)-4-hydroxyphenyl]methyl]butyl malonate 8) Sakai Chemical Industry Co., Ltd., product name "SAKAI SZ2000" 9) Fujifilm Wako Pure Chemical Industries, Ltd. 10) ADEKA Corporation, product name "ADEKA STAB (registered trademark) LS-12" 11) Dainichiseika Color & Chemicals Co., Ltd., product name "DA P-1050 White" 12) Dainichiseika Color & Chemicals Co., Ltd., product name "DA P-4720 Black" 13) Dainichiseika Color & Chemicals Co., Ltd., product name "DA P-4446 Yellow" 14) Tokyo Chemical Industry Co., Ltd. 15) Tokyo Chemical Industry Co., Ltd. 16) Tokyo Chemical Industry Co., Ltd. 17) Tokyo Chemical Industry Co., Ltd. 18) Tokyo Chemical Industry Co., Ltd.
[0085] Tables 1 to 4 show that the laminates of Examples 1 to 16 obtained by laminating a vinyl chloride resin molded body, which was obtained by molding a vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylic acid salt, and a plasticizer, with a foamed polyurethane molded body, were able to suppress discoloration of the vinyl chloride resin molded body under high temperature conditions compared to Comparative Example 1.
[0086] According to the present invention, it is possible to provide a laminate of a vinyl chloride resin molded article and a polyurethane foam molded article, in which discoloration of the vinyl chloride resin molded article under high-temperature conditions is suppressed, and a method for producing the laminate.
Claims
1. A laminate having a vinyl chloride resin molded product and a polyurethane foam molded product laminated adjacent to the vinyl chloride resin molded product, wherein the vinyl chloride resin molded product is a molded product obtained by molding a vinyl chloride resin composition containing vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer.
2. The laminate according to claim 1, wherein the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is 0.30 parts by mass or more and 8.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin.
3. The laminate according to claim 1, wherein the salt of an aliphatic dicarboxylate comprises at least one selected from the group consisting of disodium maleate, disodium malonate, disodium succinate, disodium adipate, and disodium sebacate.
4. The laminate according to claim 1, wherein the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin.
5. The laminate of claim 1, wherein the plasticizer comprises a polyester containing structural units derived from adipic acid and structural units derived from a polyhydric alcohol.
6. The laminate according to any one of claims 1 to 5, which is used for an automobile instrument panel.
7. A method for producing a laminate, comprising: a step of molding a vinyl chloride resin composition containing a vinyl chloride resin, an aliphatic dicarboxylate, and a plasticizer to obtain a vinyl chloride resin molded body; and a step of laminating a foamed polyurethane molded body on a surface of the vinyl chloride resin molded body to obtain a laminate in which the vinyl chloride resin molded body and the foamed polyurethane molded body are laminated adjacent to each other.
8. The method for producing a laminate described in claim 7, wherein the content of the aliphatic dicarboxylate in the vinyl chloride resin composition is 0.30 parts by mass or more and 8.00 parts by mass or less per 100 parts by mass of the vinyl chloride resin.
9. The method for producing a laminate according to claim 7, wherein the salt of an aliphatic dicarboxylate includes at least one selected from the group consisting of disodium maleate, disodium malonate, disodium succinate, disodium adipate, and disodium sebacate.
10. The method for producing a laminate described in claim 7, wherein the content of the plasticizer in the vinyl chloride resin composition is 50 parts by mass or more and 200 parts by mass or less per 100 parts by mass of the vinyl chloride resin.
11. The method for producing a laminate according to claim 7, wherein the plasticizer comprises a polyester containing structural units derived from adipic acid and structural units derived from a polyhydric alcohol.
12. The method for producing a laminate according to any one of claims 7 to 11, wherein the vinyl chloride resin composition is powder slush molded to obtain the vinyl chloride resin molded article.
Citation Information
Patent Citations
Composition comprising alkali metal carboxylates for stabilizing halogen-containing polymers
EP2363431A1
Stabilized halogenated polymer composition
JP1992304255A
Vinyl chloride-based resin composition
JP1995118478A
Polyvinyl chloride resin composition