Electrolytic capacitor

By minimizing defects in the dielectric layer of electrolytic capacitors through targeted cleaning and processing of sintered valve metal particles, the reliability and capacity of electrolytic capacitors are enhanced, addressing the limitations of existing technologies in handling hazardous materials and reducing leakage current.

WO2024203050A1PCT designated stage expired Publication Date: 2024-10-03PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008415
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing electrolytic capacitors with sintered bodies of valve metal particles face challenges in reducing defects in the dielectric layer, leading to increased leakage current, which hampers reliability, capacity, and lifespan due to the susceptibility of high-purity niobium foils and the hazardous handling of hydrofluoric acid in manufacturing processes.

Method used

The electrolytic capacitor design incorporates a sintered body of valve metal particles with a dielectric layer and a solid electrolyte layer, where six arbitrary regions on the anode body are cleaned and processed to minimize defects, using a cleaning solution and specific processing techniques to form a dielectric layer with fewer than four defects per field of view, thereby reducing leakage current and enhancing reliability.

Benefits of technology

This approach significantly suppresses leakage current, improves the reliability of the electrolytic capacitor, allows for increased capacity, and extends its lifespan by ensuring a low defect count in the dielectric layer, making it suitable for electronic circuits and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008415_03102024_PF_FP_ABST
    Figure JP2024008415_03102024_PF_FP_ABST
Patent Text Reader

Abstract

This electrolytic capacitor comprises: a positive electrode body; a dielectric layer that covers at least a part of the positive electrode body; and a solid electrolyte layer that covers at least a part of the dielectric layer. The positive electrode body is a sintered body of valve-acting metal particles. If six regions are arbitrarily selected in the surface of the positive electrode body, and the six regions are each observed in a field of view of 100 μm2, the total number of defects found in the dielectric layer is 4 or less.
Need to check novelty before this filing date? Find Prior Art

Description

electrolytic capacitor

[0001] The present disclosure relates to electrolytic capacitors.

[0002] Patent Document 1 proposes "a method for producing a porous niobium material having a porous oxide coating on the surface of a niobium substrate, the method comprising anodizing the surface of the substrate with an electrolyte containing hydrofluoric acid." Patent Document 1 also proposes "a porous niobium material having a porous layer with a pore size of 10 to 20 nm on a barrier layer, the porous layer being free of pores or petal-shaped defects with a pore size of 0.2 to 1 μm or larger than this range."

[0003] Japanese Patent Application Laid-Open No. 2006-83425

[0004] One aspect of the present disclosure relates to an electrolytic capacitor. The electrolytic capacitor includes an anode body, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer. The anode body is a sintered body of valve action metal particles. Six regions are arbitrarily set on the surface of the anode body, and each of the six regions is sintered to a diameter of 100 μm. 2 When observed in a field of view, the total number of defects found in the dielectric layer is four or less.

[0005] When a sintered body of valve-action metal particles is used as the anode body, defects in a dielectric layer covering at least a portion of the anode body are reduced.

[0006] 1 is a diagram showing an example of how to set six arbitrary regions in an anode body of an electrolytic capacitor according to an embodiment of the present disclosure; FIG. 2 is a schematic cross-sectional view of an electrolytic capacitor according to an embodiment of the present disclosure; FIG. 3 is a scanning electron microscope (SEM) image showing defects formed in a dielectric layer;

[0007] Patent Document 1 proposes the use of an electrolyte containing hydrofluoric acid, but hydrofluoric acid is difficult to handle due to its significant effects on the human body. Patent Document 1 also uses high-purity niobium foil, but the sintered body of valve-action metal particles is porous and has a very large surface area, making it difficult to eliminate defects, just as with high-purity niobium foil.

[0008] Hereinafter, embodiments of the present disclosure will be described using examples, but the present disclosure is not limited to the examples described below. In the following description, specific numerical values, materials, etc. may be exemplified, but other numerical values, materials, etc. may be applied as long as the effects of the present disclosure are obtained. Note that components other than those characteristic of the present disclosure may be components of known capacitors. In this specification, when a "range from numerical value A to numerical value B" is mentioned, the range includes numerical value A and numerical value B. When multiple materials are exemplified, one may be selected from the materials and used alone, or two or more may be used in combination.

[0009] An electrolytic capacitor according to one embodiment of the present disclosure (hereinafter also referred to as "capacitor (C)") includes an anode body, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer.

[0010] The smallest unit of an electrolytic capacitor, including an anode body, a dielectric layer, and a solid electrolyte layer, is sometimes referred to as a “capacitor element.” Therefore, the term “capacitor (C)” is a concept that encompasses both electrolytic capacitors and capacitor elements.

[0011] In the capacitor (C), the anode body is a sintered body of valve metal particles. In the capacitor (C), six regions are arbitrarily set on the surface of the anode body, and each of the six regions is 100 μm 2 When observed in this field of view, the total number of defects in the dielectric layer (total of six locations) found is limited to four or less.

[0012] When a sintered body of valve-action metal particles is used as an anode body of an electrolytic capacitor, if there are many defects in the dielectric layer covering at least a part of the anode body, leakage current increases. If the leakage current increases, the reliability of the electrolytic capacitor cannot be improved, and it is difficult to increase the capacitance and extend the life of the electrolytic capacitor.

[0013] On the other hand, six arbitrary regions on the surface of the anode body were each cut to 100 μm 2When the total number of defects found in the dielectric layer is limited to four or less when observed from a wide field of view, leakage current is significantly reduced, thereby improving the reliability of the electrolytic capacitor and enabling it to have a larger capacitance and a longer life.

[0014] Here, defects refer to petal-shaped cracks that form in the dielectric layer, which can reduce long-term reliability. The dielectric layer is required to have an amorphous structure in order to improve insulation. However, the areas where defects form usually have crystallinity. The defects may also be called crystalline defects. The size of the defects varies somewhat, and larger defects result in larger petal-shaped cracks.

[0015] The areas where defects are formed have a crystalline structure and therefore have a different appearance from areas with an amorphous structure. Therefore, by performing processing such as binarization on images in which defects are observed, it is possible to distinguish between defects and areas other than defects.

[0016] Six arbitrary areas on the surface of the anode body were each cut to 100 μm 2 The method for observing the anode body in a field of view is not particularly limited. For example, a scanning electron microscope (SEM) is used to observe the anode body in a field of view of 100 μm. 2 It is sufficient to photograph six areas.

[0017] Six arbitrary areas on the surface of the anode body were each cut to 100 μm 2 When observed in a field of view of 100 μm, the total number of defects in the dielectric layer found in six regions is preferably as small as possible, and is preferably one or less. 2 It is most preferable that no defects in the dielectric layer be found when observed in this field of view.

[0018] The anode body has a shape of, for example, a rectangular parallelepiped. An anode wire is implanted from a first main surface of the rectangular parallelepiped anode body. The six arbitrary regions are set so as to include the centers of six regions obtained by dividing a second main surface (one of the four second main surfaces) that intersects with the first main surface of the rectangular parallelepiped into six equal parts. The second main surface is equally divided into a matrix of two rows and three columns. The direction in which the three columns are arranged is the longitudinal direction.

[0019] FIG. 1 shows an example of how to set six arbitrary regions. The anode unit 111 shown in FIG. 1 includes an anode wire 112 and a rectangular anode body 113. A dielectric layer is formed on the surface of the anode body 113. If the main surface on which the anode wire 112 is implanted is defined as the first main surface, six arbitrary regions (observation regions) 109 can be selected on one second main surface as shown in the example shown. The six arbitrary regions (observation regions) 109 are set so as to include the centers of six equally divided rectangular regions in a 2-row by 3-column matrix. The shape of each observation region 109 may be rectangular, circular, or some other shape.

[0020] A dielectric layer with fewer defects is formed, for example, by cleaning the anode body with a cleaning solution before forming the dielectric layer. The anode body is a sintered body of valve metal particles. The sintered body of valve metal particles is formed by sintering a porous compact obtained by molding valve metal-containing particles. The valve metal-containing particles and their compacts typically contain impurities such as foreign metals and carbon residues. Until now, it was not believed that there was a correlation between the amount of such impurities and the number of defects in the dielectric layer, but a correlation has actually been observed. In other words, a dielectric layer with fewer defects can be formed by thoroughly cleaning the sintered body with a cleaning solution. The anode body after cleaning is typically dried. Drying is performed, for example, at a temperature of 60°C to 150°C for 5 to 60 minutes.

[0021] The cleaning liquid may be an acidic solution, an organic solvent, or the like. A mixture of an acidic solution and an organic solvent may also be used. Examples of organic solvents include alcohols (such as ethanol), ketones (such as acetone and ethyl methyl ketone), nitriles (such as acetonitrile), esters (such as ethyl acetate), ethers (such as diethyl ether and tetrahydrofuran), amides (such as dimethylformamide and N-methylpyrrolidone), and sulfoxides (such as dimethyl sulfoxide). The cleaning liquid may contain one organic solvent or a combination of two or more organic solvents. Examples of acidic solutions include aqueous sulfuric acid solutions, aqueous hydrochloric acid solutions, aqueous nitric acid solutions, and aqueous phosphoric acid solutions. One acid may be used alone, or two or more acids may be used in combination. The concentration of the acid in the cleaning liquid may be 1% by mass or more and 30% by mass or less.

[0022] The components of the capacitor (C) will be described in more detail below. The capacitor (C) includes at least one capacitor element. The capacitor element includes an anode portion and a cathode portion. The cathode portion includes a solid electrolyte layer. The anode portion includes an anode body, and a dielectric layer is formed on the surface of the anode body.

[0023] (Anode Body) The anode body is, for example, a sintered body of valve metal particles. The sintered body of valve metal particles is entirely porous. A porous anode body has a large surface area, and therefore can achieve a high capacity.

[0024] The valve action metal particles are particles of a valve action metal, an alloy containing a valve action metal, a metal compound containing a valve action metal, or the like. The valve action metal particles may be used alone or in combination of two or more. Examples of the valve action metal include aluminum, tantalum, niobium, and titanium. Among these, tantalum is preferred as the valve action metal for forming the sintered body.

[0025] The anode body has a cathode-forming portion. A cathode portion including a solid electrolyte is formed on the surface of the cathode-forming portion of the anode body. An anode wire is connected to the anode body, for example, to electrically connect the anode body to an external electrode on the anode side. The anode body has a shape of, for example, a rectangular parallelepiped. The anode wire extends from a first main surface of the rectangular parallelepiped anode body. A portion of the anode wire is embedded in the anode body, and the remainder of the anode wire protrudes outward from the first main surface. The remainder of the anode wire is connected to, for example, an anode lead terminal that is continuous with an external terminal.

[0026] (Dielectric Layer) The dielectric layer is an insulating layer that functions as a dielectric. The dielectric layer may be formed by anodizing the valve metal on the surface of the anode body. For example, when tantalum particles are used as the valve metal particles, the dielectric layer formed by anodization is Ta. 2 O 5 This results in an anode element composed of an anode body and a dielectric layer. Because the anode body is porous, the anode element is also porous. The porosity of the anode element is, for example, 45% to 75%, or may be 55% to 65%. The porosity of the anode element can be calculated, for example, from the amount of pure water displaced when the anode element is immersed in pure water and the apparent volume calculated from the external dimensions of the anode element (Archimedes' method).

[0027] (Capacitor Element) The capacitor element includes an anode body, a dielectric layer, and a cathode portion covering at least a portion of the dielectric layer. The cathode portion includes at least a solid electrolyte layer and may include a cathode extraction layer. The cathode portion typically includes the solid electrolyte layer covering at least a portion of the dielectric layer and the cathode extraction layer covering at least a portion of the solid electrolyte layer.

[0028] (Solid electrolyte layer) The solid electrolyte layer is formed on the cathode forming portion of the anode body via a dielectric layer. The solid electrolyte layer may cover the dielectric layer in a layered manner. The solid electrolyte layer may also be a laminate of two or more layers of different solid electrolytes.

[0029] The solid electrolyte constituting the solid electrolyte layer is not particularly limited, and a solid electrolyte used in a known electrolytic capacitor may be used. The solid electrolyte is disposed so as to cover at least a portion of the dielectric layer. The solid electrolyte may be formed using, for example, at least one of a manganese compound and a conductive polymer. The conductive polymer may include, for example, a conjugated polymer and a dopant. The conductive polymer may include a self-doping conductive polymer.

[0030] Examples of conjugated polymers include polypyrrole, polythiophene, polyaniline, and derivatives thereof. These may be used alone or in combination. The conjugated polymer may also be a copolymer of two or more types of monomers. Note that a derivative of a conjugated polymer refers to a polymer having a conjugated polymer as its basic skeleton. An example of a polythiophene derivative is poly(3,4-ethylenedioxythiophene).

[0031] The dopant can be selected depending on the conjugated polymer, and known dopants may be used. Examples of dopants include compounds capable of generating anions (e.g., aromatic sulfonic acids (e.g., naphthalenesulfonic acid, p-toluenesulfonic acid, etc.) or salts thereof), polyanions (e.g., polymer-type polyanions (e.g., polystyrenesulfonic acid)), etc. Examples of solid electrolytes include polypyrrole doped with aromatic sulfonic acids and poly(3,4-ethylenedioxythiophene) (PEDOT) doped with polystyrenesulfonic acid (PSS).

[0032] The solid electrolyte layer may be formed, for example, by polymerizing a precursor of a conjugated polymer (such as a raw material monomer) on a dielectric layer in the presence of a dopant as needed. The solid electrolyte layer may be formed by applying a liquid composition containing the conjugated polymer (and a dopant as needed) to the dielectric layer and then drying the applied composition.

[0033] (Cathode Extraction Layer) The cathode extraction layer is a conductive layer. The cathode extraction layer is disposed so as to cover at least a portion of the solid electrolyte layer. The configuration of the cathode extraction layer is not particularly limited, and a known cathode extraction layer may be employed. The cathode extraction layer may include, for example, a carbon layer formed on the solid electrolyte layer and a metal particle-containing layer formed on the carbon layer. The carbon layer may include a conductive carbon material such as graphite and a resin. The metal particle-containing layer may include metal particles (e.g., silver particles) and a resin. The metal particle-containing layer may be a silver particle-containing layer formed from a silver paste containing silver particles or silver alloy particles.

[0034] The cathode extraction layer may include a metal foil. The metal foil may be a valve metal (such as aluminum, tantalum, or niobium) or an alloy containing a valve metal. If necessary, the surface of the metal foil may be roughened. The surface of the metal foil may be provided with a chemical conversion coating, or may be provided with a coating of a metal (dissimilar metal) or a nonmetal different from the metal constituting the metal foil. Examples of dissimilar metals and nonmetals include metals such as titanium and nonmetals such as carbon (e.g., conductive carbon).

[0035] The cathode extraction layer may be electrically connected to one end of a cathode lead terminal that is continuous with the external terminal. The cathode lead terminal is bonded to the cathode extraction layer via a conductive adhesive applied to the cathode extraction layer. An anode wire protruding from the anode body may be electrically connected to one end of the anode lead terminal.

[0036] The other end of the anode lead terminal and the other end of the cathode lead terminal are each drawn out from the resin exterior body or the case. The other end of each of the anode lead terminal and the cathode lead terminal exposed from the resin exterior body or the case is used for, for example, soldering to a substrate on which the solid electrolytic capacitor is to be mounted. Alternatively, at least one end face of the anode portion and the cathode portion may be exposed from the outer surface of the sealing body and electrically connected to an external electrode without drawing out a portion of the anode lead terminal and the cathode lead terminal.

[0037] The capacitor element is sealed in a resin outer casing or case. For example, the capacitor element may be placed in a mold and sealed in the resin outer casing by transfer molding, compression molding, or the like using a resin material for the outer casing (e.g., an uncured thermosetting resin and a filler). At this time, the other ends of the anode lead terminal and the cathode lead terminal connected to the anode wire drawn from the capacitor element are exposed from the mold.

[0038] FIG. 2 is a cross-sectional view schematically illustrating an example of a solid electrolytic capacitor according to the present disclosure. The solid electrolytic capacitor 100 shown in FIG. 2 includes a capacitor element 110, an anode lead terminal 120, a cathode lead terminal 130, an outer casing 101, and a conductive layer 141. The capacitor element 110 includes an anode portion 111, a dielectric layer 114, and a cathode portion 115. The anode portion 111 includes an anode body 113 and an anode wire 112. The anode body 113 is a sintered body of valve metal particles and has a rectangular parallelepiped shape. A dielectric layer 114 is formed on the surface of the anode body 113. A portion of the anode wire 112 protrudes from a first end face of the anode body 113 toward a front surface 100f of the solid electrolytic capacitor 100. The other portion of the anode wire 112 is embedded in the anode body 113.

[0039] Cathode section 115 includes solid electrolyte layer 116 disposed so as to cover at least a portion of dielectric layer 114, and cathode extraction layer 117 formed on solid electrolyte layer 116. Cathode extraction layer 117 includes, for example, a carbon layer formed on solid electrolyte layer 116, and a metal particle-containing layer formed on the carbon layer. The metal particle-containing layer is formed using, for example, a metal paste (such as a silver paste).

[0040] The anode lead terminal 120 includes an anode terminal portion 121 and a lead connection portion 122. The anode terminal portion 121 is exposed on the bottom surface 100b of the solid electrolytic capacitor 100. The lead connection portion 122 is connected to the anode wire 112. The cathode lead terminal 130 includes a cathode terminal portion 131 and a connection portion 132. The cathode terminal portion 131 is exposed on the bottom surface 100b of the solid electrolytic capacitor 100. The connection portion 132 is electrically connected to the cathode extraction layer 117 by a conductive layer 141.

[0041] EXAMPLES The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0042] Example 1 (1) Fabrication of Capacitor Element (i) Preparation of Anode Body Tantalum (Ta) particles (Ta powder) were used as valve metal particles. The Ta powder was molded into a rectangular parallelepiped so that one end of an anode wire made of Ta was embedded in the Ta powder, and the molded body was then sintered in a vacuum. This resulted in an anode part including a sintered body (anode body) of a porous Ta particle molded body and an anode wire that was partially embedded in the sintered body (anode body) and the remainder protruding from the first main surface of the anode body.

[0043] The anode part, which was composed of the sintered body (anode body) and the anode wire, was washed using isopropanol (IPA) as a cleaning liquid, and then dried at 150° C. for 30 minutes.

[0044] (ii) Formation of Dielectric Layer (Anode Element) 106 cleaned anode parts were lined up at regular intervals, and the anode wire was welded to a long, thin, plate-shaped first electrode. The anode body and a portion of the anode wire were immersed in an anodizing solution in a glass anodizing tank, and a Ta second electrode was immersed in the anodizing solution. A DC voltage was applied between the first and second electrodes to oxidize the surface of the anode body and form a dielectric layer. A 0.06 mass % aqueous solution of nitric acid was used as the anodizing solution. The temperature of the anodizing solution was 60°C. A DC voltage of 15 V was applied for 10 hours. After anodization, the anode body was dried at 100°C for 10 minutes. In this way, a dielectric layer of tantalum oxide (TaO) was formed on the surface of the anode body and on the surface of a portion of the anode wire. 2 O 5 ) to form a uniform chemical conversion coating (thickness: about 30 nm).

[0045] (iii) Formation of a Solid Electrolyte Layer 3,4-ethylenedioxythiophene and polystyrene sulfonic acid were dissolved in ion-exchanged water to prepare a mixed solution. Iron (III) sulfate (oxidant) dissolved in ion-exchanged water was added to the mixed solution while stirring, and a polymerization reaction was carried out. After the reaction, the resulting reaction solution was dialyzed to remove unreacted monomers and excess oxidant. A predetermined amount of water was removed from the resulting mixture, and isopropanol (IPA) was added to obtain a liquid dispersion containing polyethylenedioxythiophene doped with polystyrene sulfonic acid (PEDOT / PSS). The liquid dispersion was impregnated into the anode element with the dielectric layer formed thereon for 5 minutes, followed by drying at 150°C for 30 minutes, forming a solid electrolyte layer on the dielectric layer.

[0046] (iv) Formation of Carbon Layer A dispersion liquid (carbon paste) in which carbon particles were dispersed in water was applied to the solid electrolyte layer, and then heated at 200°C to form a carbon layer on the surface of the solid electrolyte layer.

[0047] (v) Formation of Metal Particle-Containing Layer A silver paste containing silver particles, a binder resin, and a solvent was applied to the surface of the carbon layer, and then heated at 200°C to form a metal particle-containing layer, thereby obtaining a capacitor element.

[0048] (2) Fabrication of Electrolytic Capacitor A conductive adhesive was applied to the metal particle-containing layer of the capacitor element, and the cathode lead terminal and the metal particle-containing layer were bonded. The anode lead and the anode lead terminal were bonded by resistance welding. Next, the capacitor element with each bonded lead terminal was placed in a mold and sealed with an exterior material (thermosetting resin composition) by transfer molding. In this way, an electrolytic capacitor A1 with a rated voltage Rv of 35 V was fabricated.

[0049] Example 2 An electrolytic capacitor A2 was produced in the same manner as in Example 1, except that the anode part including the sintered body (anode body) and the anode wire was cleaned using a mixed solvent of isopropanol (IPA) and distilled water in a mass ratio of 60:40 as the cleaning liquid.

[0050] Example 3 An electrolytic capacitor A3 was produced in the same manner as in Example 1, except that the anode part including the sintered body (anode body) and the anode wire was cleaned with a solution obtained by mixing isopropanol (IPA) and an aqueous sulfuric acid solution (sulfuric acid concentration: 1 mass %) in a mass ratio of 60:40 as the cleaning liquid.

[0051] Comparative Example 1 An electrolytic capacitor B1 was produced in the same manner as in Example 1, except that the anode part composed of the sintered body (anode body) and the anode wire was washed using distilled water as a cleaning solution.

[0052] Comparative Example 2 An electrolytic capacitor B2 was produced in the same manner as in Example 1, except that the anode portion was not washed.

[0053] <Evaluation> The electrolytic capacitors obtained in the examples and comparative examples were dried at 170° C. for 3 hours and then cooled in a drying chamber to 20° C.±5° C. The solid electrolytic capacitors in this state were used to carry out the following evaluations.

[0054] The initial capacitance C0 (mΩ) of the electrolytic capacitor at a frequency of 120 kHz was measured using a four-terminal LCR meter at 20°C. Next, a rated voltage (35 V) was applied to the electrolytic capacitor for 2000 hours at 125°C (reliability test). The capacitance C1 (mΩ) was then measured using the same method as above. The ratio (%) of the difference (ΔC) between C0 and C1 to C0 was calculated as the capacity degradation rate. The evaluation results are shown in Table 1.

[0055]

[0056] 3 shows one of the SEM images of the dielectric layer of the solid electrolytic capacitor B1 of Comparative Example 1. In the SEM image, petal-shaped cracks are seen in the circled area.

[0057] The electrolytic capacitor of the present disclosure has low leakage current and high reliability. Therefore, the solid electrolytic capacitor is suitable for use in connection with electronic circuits, and can suppress malfunctions of the electronic circuits in such applications. However, the applications of the electrolytic capacitor are not limited to these.

[0058] 100: Electrolytic capacitor 109: Observation area 110: Capacitor element 111: Anode portion 112: Anode wire 113: Anode body 114: Dielectric layer 115: Cathode portion 116: Solid electrolyte layer 117: Cathode extraction layer 120: Anode lead terminal 121: Anode terminal portion 122: Lead connection portion 130: Cathode lead terminal 131: Cathode terminal portion 132: Connection portion 141: Conductive layer

Claims

1. An anode body, a dielectric layer covering at least a portion of the anode body, and a solid electrolyte layer covering at least a portion of the dielectric layer, the anode body being a sintered body of valve metal particles, six regions being arbitrarily set on the surface of the anode body, and each of the six regions is 100 μm 2 13. An electrolytic capacitor, wherein the total number of defects found in the dielectric layer is 4 or less when observed in a field of view of 100 mm.

2. Each of the six areas is cut by 100 μm. 2 2. The electrolytic capacitor according to claim 1, wherein the total number of defects found in the dielectric layer is one or less when observed in a field of view.

3. The six areas are each cut by 100 μm. 2 2. The electrolytic capacitor according to claim 1, wherein no defects are found in the dielectric layer when observed in a visual field of 100 .mu.m.

4. The electrolytic capacitor according to any one of claims 1 to 3, wherein the anode body is shaped like a rectangular parallelepiped, an anode wire is implanted from a first main surface of the anode body, and the six regions are set so as to include the centers of six regions obtained by equally dividing a second main surface of the rectangular parallelepiped that intersects with the first main surface into six parts.

Citation Information

Patent Citations

  • Method for reducing leakage current of high-voltage large-capacity tantalum electrolytic capacitor

    CN103500658A

  • Electrolytic capacitor

    JP1974119151A

  • Method of producing solid electrolyte capacitor

    JP1979082067A

  • Manufacture of porous anode in solid electrolytic capacitor

    JP1999111575A

  • Manufacture of solid electrolytic capacitor

    JP1999288851A