Multilayer body and virtual reality display device

The laminate configuration with controlled crosslinking and protective layers addresses the issues of image sharpness and heat resistance in virtual reality display devices, enhancing the performance of pancake lens type VR devices by improving heat resistance and image quality.

WO2024203067A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/008509
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-06
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Virtual reality display devices with pancake lens configurations face challenges in achieving high image sharpness and heat resistance due to the deterioration of absorption polarizer surface properties when molded into curved shapes, leading to suboptimal performance in recent years.

Method used

A laminate configuration comprising a stretched resin film absorption polarizer with a crosslinked resin and protective layers made of acrylic or methacrylic resins, where the crosslinking agent amount is controlled to prevent surface deterioration, and the protective layers' thickness is optimized to suppress dichroic substance diffusion, enhancing both heat resistance and image sharpness.

Benefits of technology

The proposed laminate configuration significantly improves heat resistance and image sharpness in pancake lens type virtual reality display devices, ensuring better performance and durability under high temperature and humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024008509_03102024_PF_FP_ABST
    Figure JP2024008509_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention provides: a multilayer body which has excellent heat resistance and exhibits excellent image sharpness when applied to a pancake lens-type virtual reality display device; and a virtual reality display device. The multilayer body according to the present invention is provided with: an absorptive polarizer that is a stretched resin film; a first protective layer that is disposed on one surface side of the absorptive polarizer; and a second protective layer that is disposed on the other surface side of the absorptive polarizer. The multilayer body has a curved surface part. The absorptive polarizer contains a resin that has a crosslinked part, and the amount of a crosslinking agent derived from the crosslinked part is 0.050 × 10-6 g / m3 or less. The thickness of the first protective layer and the thickness of the second protective layer are both 0.10 to 10 µm, and the first protective layer and the second protective layer both contain a resin that is selected from the group consisting of an acrylic resin and a methacrylic resin.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate, virtual reality display device

[0001] The present invention relates to a laminate and a virtual reality display device.

[0002] A virtual reality display device is a display device that allows a user to feel as if they are immersed in a virtual world by wearing a dedicated headset on their head and viewing images displayed through lenses. Virtual reality display devices generally include an image display panel and a Fresnel lens, but the distance from the image display panel to the Fresnel lens is large, which makes the headset thick and makes it difficult to wear. To address this issue, as described in Patent Literature 1, a lens configuration called a pancake lens has been proposed, which includes an image display panel, a reflective polarizer, and a half mirror, and reduces the overall thickness of the headset by directing light emitted from the image display panel back and forth between the reflective polarizer and the half mirror.

[0003] Special Publication No. 2020-519964

[0004] Pancake lens-type virtual reality display devices require further improvements in image sharpness. Virtual reality display devices such as those described in Patent Document 1 use an absorptive polarizer. This absorptive polarizer needs to be curved to match the shape of the lens or the like. The present inventors applied a conventional absorptive polarizer to a virtual reality display device and evaluated its properties, finding that the image sharpness did not meet the current higher level of demand and that further improvement was necessary. Furthermore, the absorptive polarizer used is required to have high heat resistance. Heat resistance means that the transmittance, an optical property, is suppressed from changing even after the absorptive polarizer is left standing in a high-temperature, high-humidity environment.

[0005] In view of the above circumstances, an object of the present invention is to provide a laminate that has excellent heat resistance and, when applied to a pancake lens-type virtual reality display device, has excellent image sharpness.An object of the present invention is also to provide a virtual reality display device.

[0006] The present inventors have conducted extensive research into the above-mentioned problems and have found that the above-mentioned problems can be solved by the following configuration.

[0007] (1) A laminate having an absorptive polarizer that is a stretched resin film, a first protective layer disposed on one surface side of the absorptive polarizer, and a second protective layer disposed on the other surface side of the absorptive polarizer, the laminate having a curved surface portion, the absorptive polarizer containing a resin having a crosslinked portion, and the amount of crosslinking agent derived from the crosslinked portion is 0.050 × 10 -6 g / m 3 (2) A laminate having an absorptive polarizer that is a stretched resin film, a first protective layer disposed on one surface side of the absorptive polarizer, and a second protective layer disposed on the other surface side of the absorptive polarizer, the laminate having a curved surface portion, the absorptive polarizer containing a resin having boric acid crosslinking moieties, and the amount of boric acid derived from the boric acid crosslinking moieties is 0.050 × 10 or less, the thickness of each of the first protective layer and the second protective layer is 0.10 to 10 μm, and the first protective layer and the second protective layer each contain a resin selected from the group consisting of an acrylic resin and a methacrylic resin. -6 g / m 3 (3) The laminate according to (1) or (2), wherein the thickness of each of the first protective layer and the second protective layer is 0.10 to 10 μm, and each of the first protective layer and the second protective layer contains a resin selected from the group consisting of an acrylic resin and a methacrylic resin. (4) A virtual reality display device comprising, in this order, an image display panel, an absorptive polarizer, a first retardation layer, a half mirror, a second retardation layer, a reflective polarizer, and the laminate according to any of (1) to (3). (5) A virtual reality display device comprising, in this order, an image display panel, an absorptive polarizer, a retardation layer, a half mirror, a reflective circular polarizer, and the laminate according to any of (1) to (3).

[0008] According to the present invention, it is possible to provide a laminate that has excellent heat resistance and, when applied to a pancake lens type virtual reality display device, has excellent image sharpness. According to the present invention, it is possible to provide a virtual reality display device.

[0009] Fig. 1 is a top view of an example of a laminate of the present invention. Fig. 2 is a cross-sectional view taken along line A-A in Fig. 1. Fig. 3 is a diagram showing an example of a first embodiment of a virtual reality display device of the present invention. Fig. 4 is a diagram showing an example of a second embodiment of a virtual reality display device of the present invention.

[0010] The present invention will be described in detail below. The following description of the constituent elements may be based on representative embodiments and specific examples, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits.

[0011] In this specification, "absorption axis" refers to the polarization direction in which absorbance is maximized in a plane when linearly polarized light is incident. "Reflection axis" refers to the polarization direction in which reflectance is maximized in a plane when linearly polarized light is incident. "Transmission axis" refers to the direction perpendicular to the absorption axis or reflection axis in a plane. "Slow axis" refers to the direction in which refractive index is maximized in a plane.

[0012] In this specification, Re(λ) and Rth(λ) represent the in-plane retardation and the thickness retardation, respectively, at a wavelength λ. Unless otherwise specified, the wavelength λ is 550 nm. In the present invention, Re(λ) and Rth(λ) are values ​​measured at a wavelength λ using an AxoScan (manufactured by Axometrics). By inputting the average refractive index ((nx + ny + nz) / 3) and film thickness (d) into AxoScan, the following slow axis direction (°) is calculated: Re(λ) = R0(λ) Rth(λ) = ((nx + ny) / 2 - nz) × d. Note that R0(λ) is displayed as a numerical value calculated by AxoScan, but it means Re(λ).

[0013] In this specification, the refractive indices nx, ny, and nz are measured using an Abbe refractometer (NAR-4T, manufactured by Atago Co., Ltd.) with a sodium lamp (λ = 589 nm) as a light source. When measuring wavelength dependency, measurements can be made using a multi-wavelength Abbe refractometer DR-M2 (manufactured by Atago Co., Ltd.) in combination with an interference filter. Values ​​from the Polymer Handbook (John Wiley & Sons, Inc.) and catalogs of various optical films can also be used. Examples of average refractive index values ​​for major optical films are listed below: cellulose acylate (1.48), cycloolefin polymer (1.52), polycarbonate (1.59), polymethyl methacrylate (1.49), and polystyrene (1.59).

[0014] The laminate of the present invention is characterized by the amount of crosslinking agent derived from the crosslinking moieties (preferably, the amount of boric acid derived from the boric acid crosslinking moieties, as described below) being equal to or less than a predetermined value, and by the use of a protective layer containing a predetermined resin and having a thickness within a predetermined range. The present inventors investigated the reason why the desired effect was not obtained when a conventional absorptive polarizer, which is a stretched resin film, was applied to a pancake lens-type virtual reality display device. They found that when the absorptive polarizer was molded into a curved shape, the surface properties of the absorptive polarizer deteriorated, resulting in poor image sharpness. After extensive research, the present inventors found that the deterioration of surface properties could be prevented by reducing the amount of crosslinking agent derived from the crosslinking moieties. Reducing the amount of crosslinking agent derived from the crosslinking moieties means a decrease in crosslink density. As a result, the absorptive polarizer is more easily stretched when molded into a curved shape, suppressing distortion during stretching and preventing deterioration of surface properties. Furthermore, the laminate of the present invention has improved heat resistance by using a protective layer containing a predetermined resin and having a thickness within a predetermined range. The present inventors have discovered that the mechanism by which heat resistance deteriorates is that the transmittance changes due to the diffusion of a dichroic material contained in an absorptive polarizer into an adjacent layer. Therefore, it is presumed that by disposing a protective layer containing a predetermined resin and having a thickness within a predetermined range as a layer adjacent to the absorptive polarizer, the dichroic material diffuses into the protective layer, but the thin thickness of the protective layer makes it easy for the concentration of the dichroic material to increase, resulting in a small concentration gradient between the absorptive polarizer and the protective layer, which suppresses the diffusion of the dichroic material and the change in transmittance.

[0015] <Laminate> The laminate of the present invention has an absorptive polarizer that is a stretched resin film, a first protective layer arranged on one surface side of the absorptive polarizer, and a second protective layer arranged on the other surface side of the absorptive polarizer. The laminate of the present invention has a curved surface portion. The laminate of the present invention may have a curved surface portion as a whole, or a portion of the laminate may have a curved surface portion. When a portion of the laminate is a curved surface portion, the other portion may be a flat portion. The curved surface portion means a portion with a curved shape.

[0016] The above-mentioned curved surface shape refers to a shape having a curvature greater than zero, and includes developable curved surface shapes and three-dimensional curved surface shapes. A developable surface is a surface that can be developed into a plane without expanding or contracting any part of the surface. Examples of developable curved surface shapes include surfaces corresponding to cylindrical surfaces, elliptical cylindrical surfaces, conical surfaces, and elliptical conical surfaces, and may be convex or concave curved surfaces. A three-dimensional curved surface refers to a curved surface that cannot be formed by deformation of a plane, i.e., a curved surface that is not developable. Examples of three-dimensional curved surfaces include surfaces corresponding to spherical surfaces and spheroidal surfaces, and surfaces corresponding to curved surfaces whose cross sections form parabolas or hyperbolas (e.g., paraboloids of revolution), and may be convex or concave curved surfaces.

[0017] The curved surface shape is preferably a lens shape. Examples of the lens shape include a spherical shape and a shape of a body of revolution such as a spheroid, and the shape may be a convex lens shape or a concave lens shape.

[0018] The shape of the curved surface portion of the laminate is preferably a spherical shape, a spheroid shape, or a paraboloid of revolution. That is, the curved surface portion is preferably a spherical shape, a spheroid shape, or a radial surface of revolution. As described above, the shape of the curved surface portion of the laminate is preferably a solid of revolution.

[0019] The radius of curvature of the curved surface of the laminate is not particularly limited, but is preferably 20 to 80 mm, more preferably 30 to 80 mm.

[0020] FIG. 1 shows an example of a laminate of the present invention. FIG. 1 is a top view of the laminate, and FIG. 2 is a cross-sectional view taken along line A-A in FIG. 1 . Note that line A-A is a line passing through the center C of the laminate 10, which is circular when viewed in plan. As shown in FIGS. 1 and 2 , the laminate 10 includes an absorbing polarizer 12, a first protective layer 14 disposed on one surface of the absorbing polarizer 12, and a second protective layer 16 disposed on the other surface of the absorbing polarizer 12. Also, as shown in FIGS. 1 and 2 , the laminate 10 has a curved shape. More specifically, as shown in FIG. 2 , the laminate 10 has a shape (convex shape) that is curved convexly toward the upper side of the paper. In other words, the laminate 10 has a convex shape that protrudes toward one surface. Note that the laminate 10 can also be said to have a concave shape in which the other surface is concave. In the laminate 10, the entire laminate 10 corresponds to the curved portion. 2, the laminate 10 has two opposing surfaces, a first surface 10A and a second surface 10B, where the first surface 10A is a curved surface that is convex toward the top of the page, and the second surface 10B is a curved surface that is convex toward the top of the page. Note that the curved surface of the laminate 10 shown in FIGS. 1 and 2 is a paraboloid of revolution, but may also be a spherical or spheroidal shape.

[0021] 1 , when the laminate 10 is observed from the normal direction of the tangent plane to the center C of the laminate 10 (corresponding to the apex of the convex portion) (when the laminate 10 is viewed from above), the shape of the laminate 10 is circular. Note that the center C of the laminate 10 is the intersection point between the axis of the spheroid shape and the laminate 10, and corresponds to the position where the center C intersects with the normal to the center of the exit surface of the image display device when the laminate 10 is incorporated into the virtual reality display device described below. When the laminate 10 is incorporated into the virtual reality display device described below, the laminate 10 is positioned so that it is convex toward the image display panel side.

[0022] In Figure 1, an embodiment has been described in which the shape of the curved surface portion of the laminate is circular when viewed in a plane (when observed from the direction of the rotation axis of the laminate), but the present invention is not limited to this embodiment, and the shape of the curved surface portion of the laminate when viewed in a plane may be elliptical or another shape.

[0023] Each member included in the laminate will be described in detail below.

[0024] <Absorptive Polarizer> The laminate of the present invention includes an absorptive polarizer (absorptive linear polarizer) that is a stretched resin film. A stretched resin film is a film obtained by stretching a resin film. The degree of polarization of the absorptive polarizer is not particularly limited, but is preferably 99.0% or more, more preferably 99.5% or more, and even more preferably 99.9% or more, from the viewpoint of achieving better performance of a virtual reality display device to which the laminate is applied. The upper limit is not particularly limited, and can be 100%. The method for measuring the degree of polarization of the absorptive polarizer is as follows. First, a portion of the absorptive polarizer (particularly the central portion) is cut into a 2 cm square and bonded to a Fujitac TD80UL (manufactured by Fujifilm Corporation) with a pressure-sensitive adhesive sheet "NCF-D692(5)" manufactured by Lintec Corporation. The luminous efficiency-corrected degree of polarization is then calculated using an automatic polarizing film measuring device VAP-7070 manufactured by JASCO Corporation. Here, the term "luminosity-corrected polarization degree" refers to the average value obtained by measuring the transmittance in the wavelength range of 380 to 780 nm for light incident from the Fujitac TD80UL side by placing a light source, a linear polarizer, and an absorptive polarizer in that order, calculating the polarization degree for each wavelength using the following formula, and multiplying the calculated values ​​by the luminosity correction coefficient: Polarization degree P (%) = {((Ty - Tx) / (Ty + Tx)) 1/2 × 100} Tx: transmittance when the incident polarized light emitted through the linear polarizer and the transmission axis of the absorptive polarizer 1 are arranged so that they are in a crossed Nicol state (incident polarized light is 100%) Ty: transmittance when the incident polarized light emitted through the linear polarizer and the transmission axis of the absorptive polarizer 1 are arranged so that they are in a paranic Nicol state (incident polarized light is 100%)

[0025] The absorptive polarizer contains a resin. The type of resin is not particularly limited, and known resins can be used. Examples of the resin include polyvinyl alcohol resins, (meth)acrylic resins, styrene resins, and cellulose resins. Among these, polyvinyl alcohol resins are preferred, and examples of polyvinyl alcohol and its derivatives include polyvinyl alcohol. Examples of polyvinyl alcohol derivatives include polyvinyl formal; polyvinyl acetal; and derivatives of polyvinyl alcohol, polyvinyl formal, and polyvinyl acetal modified with olefins such as ethylene and propylene, or unsaturated carboxylic acids such as acrylic acid, methacrylic acid, and crotonic acid.

[0026] The average degree of polymerization of the polyvinyl alcohol resin is preferably 100 to 10,000, more preferably 1,000 to 10,000. The degree of saponification of the polyvinyl alcohol resin is preferably 80 to 100 mol%, more preferably 95 to 99.95 mol. The average degree of polymerization and the degree of saponification can be determined in accordance with JIS K 6726.

[0027] The resin in the absorptive polarizer has a crosslinked moiety. The crosslinked moiety is a linking moiety formed using a known crosslinking agent. The type of crosslinking agent is not particularly limited, but when the above-mentioned polyvinyl alcohol resin is used as the resin, the crosslinking agent is preferably boric acid. In other words, the absorptive polarizer may contain a resin having a boric acid crosslinked moiety. The boric acid crosslinked moiety is a crosslinked moiety that is generated when boric acid is used as a crosslinking agent, and is formed by boric acid and a hydroxyl group in the resin.

[0028] The amount of the crosslinking agent derived from the crosslinked portion is 0.050 × 10 -6 g / m 3 and when the laminate of the present invention is applied to a pancake lens type virtual reality display device, the image sharpness is more excellent, so that the -6 g / m 3 In addition, in terms of the superior heat resistance of the laminate, it is preferable that the -6 g / m 3 More than 0.020 × 10 is preferable. -6g / m 3 More preferably, 0.030 × 10 -6 g / m 3 The above is even more preferable. When the crosslinked moiety is a boric acid crosslinked moiety, the amount of the crosslinking agent corresponds to the amount of boric acid. The method for calculating the amount of crosslinking agent derived from the crosslinked moiety is not particularly limited, and known methods can be used. For example, a method can be used in which bonds in the crosslinked moiety are cleaved, the crosslinking agent constituting the crosslinked moiety is extracted, and its content is measured. More specifically, when the crosslinked moiety is a boric acid crosslinked moiety, the amount of boric acid can be calculated by the following procedure. First, an absorptive polarizer is cut into a 1 cm x 1 cm piece, 3 cc of nitric acid is added, and the resulting product is incinerated at a maximum temperature of 230°C using microwaves. Water is added to the resulting product to make a total volume of 50 g, and the boron emission intensity is measured using an ICP-OES (Optima 7300DV) manufactured by PerkimElmer. Next, multiple aqueous solutions with known boric acid concentrations are prepared, and a calibration curve showing the relationship between the amount of boric acid and emission intensity is prepared from the ICP emission intensity data of boron measured using each aqueous solution. Using this calibration curve, the amount of boric acid (g) is calculated from the boron emission intensity data measured using a sample of an absorptive polarizer. Next, the calculated amount of boric acid (g) is divided by the volume of the sample (1 cm × 1 cm × thickness) to obtain the amount of boric acid (g / m 3 ) is calculated.

[0029] The content of the resin in the absorptive polarizer is not particularly limited, but is preferably from 50 to 99% by mass, and more preferably from 75 to 99% by mass, based on the total mass of the absorptive polarizer.

[0030] The absorptive polarizer preferably contains a dichroic material. A dichroic material refers to a material whose absorbance varies depending on the direction. The dichroic material is not particularly limited, and examples thereof include visible light absorbing materials (dichroic dyes), luminescent materials (fluorescent materials, phosphorescent materials), ultraviolet absorbing materials, infrared absorbing materials, nonlinear optical materials, carbon nanotubes, and inorganic materials (e.g., quantum rods). Conventionally known dichroic materials (preferably dichroic dyes) can be used. Among these, iodine is preferable as the dichroic material. Iodine may exist in an ionic state. When the absorptive polarizer contains iodine and polyvinyl alcohol resin (PVA), the iodine in the absorptive polarizer is expressed as I. - , I 2 , I 3 - , I 3 - -PVA complex, and I 5 - It may be present in the form of a -PVA complex.

[0031] The content of the dichroic material in the absorptive polarizer is not particularly limited, but is preferably 0.1 to 1.5 g / m 2 is preferably 0.1 to 1.0 g / m 2 It is more preferable that the above g / m 2 is the unit area of ​​the absorptive polarizer (m 2 The values ​​represent the content (g) of dichroic substance per 1000g of the sample.

[0032] The absorptive polarizer may contain components other than the resin and dichroic material described above, such as a plasticizer.

[0033] <First Protective Layer and Second Protective Layer> The laminate of the present invention includes a first protective layer and a second protective layer. The first protective layer and the second protective layer are disposed on both sides of the absorptive polarizer and prevent diffusion of the dichroic material. Both the first protective layer and the second protective layer may function as pressure-sensitive adhesive layers. Both the first protective layer and the second protective layer are in contact with the absorptive polarizer. The thickness of each of the first protective layer and the second protective layer is 0.10 to 10 μm. In particular, a thickness of 0.10 to 8.0 μm is preferred, and 0.10 to 6.0 μm is more preferred, in terms of superior heat resistance of the laminate. When the thickness is 0.1 μm or more, the protection of the absorptive polarizer is improved, and when the first protective layer or the second protective layer functions as a pressure-sensitive adhesive layer, superior adhesiveness is achieved. When the thickness is 10 μm or less, the heat resistance of the laminate is excellent. The above thickness is an average thickness, and is determined as follows. First, the cross section of the laminate is exposed, and the thickness of the first protective layer (or the second protective layer) is measured at 20 or more locations. These values ​​are then arithmetically averaged to determine the average thickness, which is defined as the thickness of the first protective layer (or the second protective layer).

[0034] Both the first protective layer and the second protective layer contain a resin selected from the group consisting of acrylic resins and methacrylic resins (hereinafter simply referred to as "(meth)acrylic resin"). The (meth)acrylic resin is a polymer whose main component is a monomer having a (meth)acryloyl group among the monomers that make up the (meth)acrylic resin. Here, the term "main component" refers to the monomer with the largest content (mass%) among the monomer components that make up the (meth)acrylic resin. The term "(meth)acryloyl group" refers to a group selected from the group consisting of an acryloyl group and a methacryloyl group.

[0035] The number of (meth)acryloyl groups contained in the (meth)acryloyl group-containing monomer is not particularly limited, but 1 to 3 is preferred. Examples of (meth)acryloyl group-containing monomers include alkyl (meth)acrylates. Examples of alkyl (meth)acrylates include those having an alkyl group with 1 to 20 carbon atoms, and the alkyl group may be linear or branched. Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-propyl (meth)acrylate, n-butyl (meth)methacrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, undecyl (meth)acrylate, and dodecyl (meth)acrylate. The alkyl (meth)acrylates may be used alone or in combination of two or more.

[0036] The content of the repeating unit derived from alkyl (meth)acrylate in the (meth)acrylic resin is not particularly limited, but is preferably 70 to 100% by mass, more preferably 80 to 100% by mass, in terms of better heat resistance of the laminate.

[0037] Examples of other monomers besides alkyl(meth)acrylates include monomers having a reactive group (e.g., a hydroxyl group, a carboxyl group, an amino group, an epoxy group, etc.) and monomers having an aromatic ring. The other monomers are preferably monomers having a (meth)acryloyl group.

[0038] The content of the (meth)acrylic resin in the first protective layer is not particularly limited, but is preferably 50 to 100% by mass, more preferably 75 to 99% by mass, relative to the total mass of the first protective layer. The content of the (meth)acrylic resin in the second protective layer is not particularly limited, but is preferably 50 to 100% by mass, more preferably 75 to 99% by mass, relative to the total mass of the second protective layer.

[0039] <Method for manufacturing laminate> The method for manufacturing the laminate is not particularly limited, and a known method can be used. For example, a preferred method is to obtain an absorptive polarizer that is a stretched resin film, then form a first protective layer and a second protective layer on both sides of the obtained absorptive polarizer, and then form a curved surface portion. The steps of the method are described in detail below.

[0040] The method for obtaining an absorptive polarizer is not particularly limited, and known methods can be used. When the absorptive polarizer contains iodine and a polyvinyl alcohol-based resin and the crosslinked moieties are boric acid crosslinked moieties, it is preferable to perform the following steps 1 to 6. As will be described later, boric acid is used in steps 3 and 5, and boric acid is also used in step 6 as needed. By adjusting the amount of boric acid used in these steps, the amount of boric acid derived from the above-mentioned boric acid crosslinked moieties can be adjusted. Step 1: A step of applying a composition containing a polyvinyl alcohol-based resin onto a substrate to form a resin layer on the substrate to obtain a pre-stretched film. Step 2: A step of stretching the pre-stretched film obtained in Step 1 (air-assisted stretching treatment step). Step 3: A step of contacting the stretched film with boric acid (insolubilization treatment step). Step 4: A step of dyeing the film obtained in Step 3 with iodine (dyeing treatment step). Step 5: A step of contacting the film obtained in Step 4 with boric acid (crosslinking treatment step). Step 6: A step of stretching the film obtained in Step 5 in an aqueous solution (underwater stretching treatment step). The procedures for each step are described in detail below.

[0041] Step 1 is a step of applying a composition containing a polyvinyl alcohol-based resin onto a substrate to form a resin layer on the substrate and obtain a pre-stretched film. The polyvinyl alcohol-based resin contained in the composition containing a polyvinyl alcohol-based resin is as described above. The composition may contain a solvent. Examples of the solvent include water and organic solvents. The composition may contain a halide to improve the orientation of polyvinyl alcohol molecules by stretching. Examples of the halide include iodide and sodium chloride. Examples of the iodide include potassium iodide, sodium iodide, and lithium iodide.

[0042] The substrate used in step 1 is not particularly limited, and a thermoplastic resin substrate is preferred. Examples of materials constituting the thermoplastic resin substrate include ester resins such as polyethylene terephthalate resins, cycloolefin resins such as norbornene resins, olefin resins such as polypropylene, polyamide resins, polycarbonate resins, and copolymer resins thereof. Examples of methods for applying the composition include roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, and knife coating (such as comma coating).

[0043] Step 2 is a step of stretching the pre-stretched film obtained in Step 1. Stretching methods in this step include fixed-end stretching (e.g., stretching using a tenter stretching machine) and free-end stretching (e.g., uniaxial stretching by passing the film between rolls with different peripheral speeds). The stretching ratio is preferably 2.0 to 3.5 times. Stretching may be performed in one stage or multiple stages. The stretching temperature is preferably, for example, equal to or higher than the glass transition temperature (Tg) of the thermoplastic resin substrate, and more preferably equal to or higher than the glass transition temperature (Tg) + 10°C.

[0044] Step 3 is a step of contacting the stretched film with boric acid. The procedure of this step is not particularly limited, but an example is a method of immersing the film in an aqueous boric acid solution. The content of boric acid in the aqueous boric acid solution is preferably 1 to 10 parts by mass per 100 parts by mass of water. The liquid temperature of the aqueous boric acid solution is preferably 20 to 50°C.

[0045] Step 4 is a step of dyeing the film obtained in Step 3 with iodine. The procedure for this step is not particularly limited, but examples include a method of immersing the film in a dye solution containing iodine, a method of coating the film with the dye solution, and a method of spraying the dye solution onto the film. The iodine content in the dye solution is preferably 0.05 to 0.5 parts by mass per 100 parts by mass of water. In order to increase the solubility of iodine in water, the dye solution preferably contains iodide. The iodide content in the dye solution is preferably 0.1 to 10 parts by mass, more preferably 0.3 to 5 parts by mass, per 100 parts by mass of water. The temperature of the dye solution is preferably 20 to 50°C. The contact time between the film and iodine is preferably 5 seconds to 5 minutes, more preferably 30 to 90 seconds. The ratio of the contents of iodine and iodide in the dye solution (iodine / iodide) is preferably 1 / 5 to 1 / 20, more preferably 1 / 5 to 1 / 10.

[0046] Step 5 is a step of contacting the film obtained in step 4 with boric acid. The procedure of this step is not particularly limited, but an example is a method of immersing the film in an aqueous boric acid solution. The content of boric acid in the aqueous boric acid solution is preferably 1 to 10 parts by mass per 100 parts by mass of water. The liquid temperature of the aqueous boric acid solution is preferably 20 to 50°C.

[0047] Step 6 is a step of stretching the film obtained in step 5 in an aqueous solution. The aqueous solution used in this step is preferably a boric acid aqueous solution. The content of boric acid in the boric acid aqueous solution is preferably 1 to 10 parts by mass, more preferably 2.5 to 6 parts by mass, per 100 parts by mass of water. The boric acid aqueous solution may also contain iodide. The temperature of the aqueous solution is preferably 40 to 85°C, more preferably 60 to 75°C. The immersion time of the film in the aqueous solution is preferably 15 seconds to 5 minutes.

[0048] The stretching method in this step includes fixed-end stretching (for example, a method of stretching using a tenter stretching machine) and free-end stretching (for example, a method of uniaxially stretching the laminate by passing it between rolls with different peripheral speeds). The stretching ratio is preferably 1.5 times or more, and more preferably 3 times or more.

[0049] The film obtained in step 6 may be further subjected to washing and drying treatments.

[0050] The method for forming the first protective layer and the second protective layer on both sides of the obtained absorptive polarizer is not particularly limited. For example, a method of forming the first protective layer (or the second protective layer) by applying a composition containing a (meth)acrylic resin to the surface of the absorptive polarizer is exemplified. The (meth)acrylic resin contained in the composition is as described above. The composition may contain a solvent. Examples of the solvent include water and an organic solvent. Examples of methods for applying the composition include roll coating, spin coating, wire bar coating, dip coating, die coating, curtain coating, spray coating, and knife coating (such as comma coating). Another method includes a method of separately applying the composition to a temporary support to form a first protective layer (or a second protective layer), and then transferring the layer to the absorptive polarizer. The method for forming the curved surface is not particularly limited, and known methods can be used. For example, a method of molding a laminate including the first protective layer, the absorptive polarizer, and the second protective layer using a molding die having a concave or convex molding surface is exemplified.

[0051] <Virtual reality display device> A first embodiment of the virtual reality display device of the present invention includes a virtual reality display device having, in this order, an image display panel, an absorptive polarizer, a first retardation layer, a half mirror, a second retardation layer, a reflective polarizer, and the laminate. A second embodiment of the virtual reality display device of the present invention includes a virtual reality display device having, in this order, an image display panel, an absorptive polarizer, a retardation layer, a half mirror, a reflective circular polarizer, and the laminate. Each embodiment will be described below with reference to the drawings.

[0052] 3 includes, in this order, an image display panel 20, a λ / 4 retardation layer 22, an absorptive polarizer 24, a λ / 4 retardation layer 26, an antireflection layer 28, a half mirror 30, a lens substrate 32, a λ / 4 retardation layer 34, a reflective polarizer 36, and a laminate 38. The laminate 38 includes the above-described first protective layer, absorptive polarizer, and a second protective layer.

[0053] In the example shown in FIG. 3, the λ / 4 retardation layer 22, the absorbing polarizer 24, the λ / 4 retardation layer 26, and the anti-reflection layer 28 are laminated in this order on the display surface side of the image display panel 20.

[0054] The lens substrate 32 is disposed at a predetermined distance from the image display panel 20 (anti-reflection layer 28), and the surface facing the image display panel 20 is convex, while the opposite surface is concave.

[0055] The half mirror 30 is laminated on the convex side of the lens substrate 32, and is curved to follow the curved shape of the convex surface of the lens substrate 32. On the concave side of the lens substrate 32, a λ / 4 retardation layer 34, a reflective polarizer 36, and a laminate 38 are laminated in this order, and are each curved to follow the curved shape of the concave surface of the lens substrate 32.

[0056] In this virtual reality display device 100A, when unpolarized light (image light) is irradiated from the image display panel 20, it passes through the λ / 4 retardation layer 22 as unpolarized light and is converted into linearly polarized light by the absorptive polarizer 24, and then converted into circularly polarized light by the λ / 4 retardation layer 26. In other words, the transmission axis of the absorptive polarizer 24 and the slow axis of the λ / 4 retardation layer 26 are arranged so that they form an angle of 45°.

[0057] As an example, assuming that light is converted into left-handed circularly polarized light by the λ / 4 retardation layer 26, the left-handed circularly polarized light is incident on the half mirror 30. Approximately half of the left-handed circularly polarized light that has entered the half mirror 30 passes through the half mirror 30, passes through the lens substrate 32, and enters the λ / 4 retardation layer 34 where it is converted into linearly polarized light, and the linearly polarized light then enters the reflective polarizer 36. The reflective polarizer 36 is disposed so as to reflect the linearly polarized light that has entered it, and therefore the linearly polarized light that has entered it is reflected by the reflective polarizer 36 toward the half mirror 30. The linearly polarized light reflected by the reflective polarizer 36 is converted into left-handed circularly polarized light by the λ / 4 retardation layer 34. Approximately half of the left-handed circularly polarized light that has entered the half mirror 30 is reflected by the half mirror 30. At this time, the left-handed circularly polarized light is converted into right-handed circularly polarized light.

[0058] The right-handed circularly polarized light reflected by the half mirror 30 passes through the lens substrate 32, enters the λ / 4 retardation layer 34, and is converted into linearly polarized light. The linearly polarized light then enters the reflective polarizer 36. Because the reflective polarizer 36 is configured to transmit the incident linearly polarized light, the incident linearly polarized light passes through the reflective polarizer 36 and enters the laminate 38. Because the absorptive polarizer included in the laminate 38 is configured to transmit the linearly polarized light, the linearly polarized light also passes through the laminate 38 and is emitted toward the user U. When viewed from the user U side, the half mirror 30 is formed in a concave shape, and the concave mirror action of the half mirror 30 causes the light to be more concentrated than immediately after being emitted from the image display panel 20 and emitted toward the viewing side. As a result, the light appears to be emitted from a position farther away from the image display panel 20. Therefore, when the user U sees this light, it appears as if the light is being emitted from the rear of the image display panel 20 (the side opposite the user U side). As a result, the video (image) displayed on the image display panel 20 is visually recognized by the user U as a virtual image on the rear side of the image display panel 20 .

[0059] Furthermore, approximately half of the left-handed circularly polarized light reflected by the reflective polarizer 36 and incident on the half mirror 30 is transmitted through the half mirror 30. The transmitted left-handed circularly polarized light passes through the antireflection layer 28, enters the λ / 4 retardation layer 26, and is converted into linearly polarized light. This linearly polarized light passes through the absorbing polarizer 24, enters the λ / 4 retardation layer 22, and is converted into circularly polarized light. This circularly polarized light is reflected by the surface of the image display panel 20, etc., and again enters the λ / 4 retardation layer 22. Upon reflection, the rotation direction of the circularly polarized light is reversed, so that the λ / 4 retardation layer 22 converts the circularly polarized light into linearly polarized light in a direction perpendicular to the transmission axis of the absorbing polarizer 26. This linearly polarized light is absorbed by the absorbing polarizer 26.

[0060] The virtual reality display device 100B shown in Figure 4 includes, in this order, an image display panel 20, a λ / 4 retardation layer 22, an absorptive polarizer 24, a λ / 4 retardation layer 26, an antireflection layer 28, a half mirror 30, a lens substrate 32, a reflective circular polarizer 40, a λ / 4 retardation layer 42, and a laminate 38. The laminate 38 includes the first protective layer, the absorptive polarizer, and a second protective layer described above. The virtual reality display device 100B shown in Figure 4 has a similar configuration to the virtual reality display device 100A shown in Figure 3, except that it includes a reflective circular polarizer 40 and a λ / 4 retardation layer 42 instead of the λ / 4 retardation layer 34 and the reflective polarizer 36 in the virtual reality display device 100A shown in Figure 3.

[0061] In the virtual reality display device 100B shown in FIG. 4 , left-handed circularly polarized light is incident on the half mirror 30, similar to the virtual reality display device 100A shown in FIG. 3 described above. Approximately half of the left-handed circularly polarized light that is incident on the half mirror 30 is transmitted through the half mirror 30, transmitted through the lens substrate 32, and incident on the reflective circular polarizer 40. In this case, since the reflective circular polarizer 40 is a circular polarizing plate that reflects left-handed circularly polarized light and transmits right-handed circularly polarized light, the incident left-handed circularly polarized light is reflected by the reflective circular polarizer 40 toward the half mirror 30. Approximately half of the left-handed circularly polarized light that is reflected by the reflective circular polarizer 40 and incident on the half mirror 30 is reflected by the half mirror 30. At this time, the left-handed circularly polarized light is converted to right-handed circularly polarized light.

[0062] The right-handed circularly polarized light reflected by the half mirror 30 passes through the lens substrate 32 and enters the reflective circular polarizer 40. However, because the reflective circular polarizer 40 is a circular polarizer that transmits right-handed circularly polarized light, the incident right-handed circularly polarized light passes through the reflective circular polarizer 40 and enters the λ / 4 retardation layer 42. The right-handed circularly polarized light that has entered the λ / 4 retardation layer 42 is converted into linearly polarized light and enters the laminate 38. Because the absorptive polarizer in the laminate 38 is arranged to transmit this linearly polarized light, this linearly polarized light passes through the laminate 38 and is emitted toward the user U.

[0063] In the first and second embodiments, the λ / 4 retardation layer is used as the retardation layer, but the type of the retardation layer is not limited to this.

[0064] Hereinafter, the members other than the laminate included in the above-described virtual reality display device (first embodiment and second embodiment) will be described in detail.

[0065] (Image Display Panel) The image display panel is, for example, a known image display panel (display panel) such as an organic electroluminescence (EL) display panel.

[0066] (λ / 4 Retardation Layer) The λ / 4 retardation layer is a layer having a λ / 4 function, specifically, a layer having a function of converting linearly polarized light of a certain wavelength (preferably visible light) into circularly polarized light (or circularly polarized light into linearly polarized light). The in-plane retardation of the λ / 4 retardation layer at a wavelength of 550 nm is not particularly limited, but is preferably 120 to 150 nm, more preferably 125 to 150 nm, and even more preferably 135 to 150 nm. In addition to the λ / 4 retardation layer, a retardation layer whose in-plane retardation at a wavelength of 550 nm is 3 / 4 or 5 / 4 of the wavelength of any light of visible light is also preferred.

[0067] (Absorptive Polarizer) The absorptive polarizer is a member that absorbs polarized light in a specific direction (linearly polarized light). As the absorptive polarizer, a known absorptive polarizer can be used.

[0068] (Anti-Reflection Layer) The type of anti-reflection layer is not particularly limited, but from the viewpoint of further reducing the reflectance, a moth-eye film and an AR (Anti-Reflection) film are preferred.

[0069] (Half Mirror) A half mirror is a component that transmits approximately half of incident light and reflects the remaining half. Conventionally known half mirrors can be used as the half mirror. The transmittance of the half mirror is preferably 50±30%, more preferably 50±10%. The type of half mirror is not particularly limited, but examples include a reflective layer made of a metal. Examples of metals include silver and aluminum. The thickness of the half mirror is preferably 1 to 20 nm, more preferably 2 to 10 nm, and even more preferably 3 to 6 nm.

[0070] (Lens substrate) Known lens substrates can be used as the lens substrate, and examples thereof include convex lenses and concave lenses. Convex lenses include biconvex lenses, plano-convex lenses, and convex meniscus lenses. Concave lenses include biconcave lenses, plano-concave lenses, and concave meniscus lenses. As lenses used in virtual reality display devices, convex meniscus lenses or concave meniscus lenses are preferred in terms of widening the viewing angle, and concave meniscus lenses are more preferred in terms of minimizing chromatic aberration. As materials for the lens substrate, materials transparent to visible light, such as glass, crystal, and plastic, can be used.

[0071] (Reflective Polarizer (Reflective Linear Polarizer)) A reflective polarizer is a polarizer that has the function of reflecting one of mutually orthogonal linearly polarized light beams and transmitting the other linearly polarized light beam. Examples of reflective polarizers include a film obtained by stretching a dielectric multilayer film and a wire grid polarizer. Commercially available products include a reflective polarizer (product name: APF) manufactured by 3M and a wire grid polarizer (product name: WGF) manufactured by Asahi Kasei Corporation.

[0072] (Reflective Circular Polarizer) A reflective circular polarizer is a polarizer that reflects one of right-handed and left-handed circularly polarized light and transmits the other. Examples of reflective circular polarizers include a cholesteric liquid crystal layer.

[0073] In addition to the above-mentioned components, the virtual reality display device may include other components, such as a retardation layer such as a positive C plate, a support, and an adhesive layer.

[0074] The features of the present invention will be explained in more detail below with reference to examples. Note that the materials, amounts used, ratios, processing details, and processing procedures shown below can be changed as appropriate without departing from the spirit of the present invention. Furthermore, configurations other than those shown below can also be used without departing from the spirit of the present invention.

[0075] <Preparation of Absorptive Polarizer> A long, amorphous, isophthalic-copolymerized polyethylene terephthalate film (thickness: 100 μm) with a water absorption of 0.75% and a glass transition temperature (Tg) of approximately 75°C was used as the resin substrate. One side of the resin substrate was subjected to a corona treatment. A PVA-based resin was prepared by mixing polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Nippon Synthetic Chemical Industry Co., Ltd., trade name "GOHSEFIRMER Z410") in a 9:1 ratio. 13 parts by mass of potassium iodide was added to 100 parts by mass of the resulting mixture, and the resulting mixture was dissolved in water to prepare an aqueous PVA solution (coating solution). The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60°C to form a 13 μm-thick PVA-based resin layer, producing a laminate. The obtained laminate was free-end uniaxially stretched 2.4 times in the longitudinal direction (machine direction) between rolls with different peripheral speeds in an oven at 130°C (in-air auxiliary stretching treatment). The laminate was then immersed in an insolubilizing bath (a boric acid aqueous solution obtained by blending 3.0 mass% of boric acid with respect to the total mass of the boric acid aqueous solution) at a liquid temperature of 40°C for 30 seconds (insolubilization treatment). The laminate was then immersed in a dyeing bath (an iodine aqueous solution obtained by blending iodine and potassium iodide in a mass ratio of 1:7 with 100 parts by mass of water) at a liquid temperature of 30°C for 60 seconds while adjusting the concentration so that the single transmittance (Ts) of the final polarizer was 43.0% or more (dyeing treatment). The laminate was then immersed in a crosslinking bath (a boric acid aqueous solution obtained by blending 3 parts by mass of potassium iodide and 3.0 parts by mass of boric acid with 100 parts by mass of water) at a liquid temperature of 40°C for 30 seconds (crosslinking treatment). The laminate was then immersed in a boric acid aqueous solution (boric acid concentration 3.0% by mass, potassium iodide concentration 5% by mass) at a liquid temperature of 70°C, and uniaxially stretched in the longitudinal direction (longitudinal direction) between rolls with different peripheral speeds to a total stretch ratio of 5.5 times (underwater stretching treatment). The laminate was then immersed in a cleaning bath (aqueous solution obtained by blending 4 parts by mass of potassium iodide with 100 parts by mass of water) at a liquid temperature of 20°C (washing treatment). The resulting laminate was then dried in an oven maintained at 90°C, and brought into contact with a SUS heated roll maintained at a surface temperature of 75°C for about 2 seconds (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%.In this manner, an absorptive polarizer 1 having a thickness of 5 μm was formed on the resin substrate. At this time, the content of the dichroic material in the absorptive polarizer was 0.5 g / m. 2 It was.

[0076] Absorbent polarizers 2 to 5 were produced according to the same procedure as for absorbent polarizer 1, except that the boric acid concentration (% by mass) in the insolubilization bath in the insolubilization treatment, the amount of boric acid (parts by mass) in the crosslinking bath in the crosslinking treatment, and the boric acid concentration (% by mass) in the aqueous boric acid solution in the underwater stretching treatment were changed as shown in Table 1. In Table 1, the "boric acid concentration" column indicates the boric acid concentration (% by mass) in the insolubilization bath in the insolubilization treatment and the boric acid concentration (% by mass) in the aqueous boric acid solution in the underwater stretching treatment, expressed in "% by mass," and the amount of boric acid (parts by mass) in the crosslinking bath in the crosslinking treatment, expressed in "parts by mass." For example, in absorbent polarizer 2, the boric acid concentration (% by mass) in the insolubilization bath in the insolubilization treatment and the boric acid concentration (% by mass) in the aqueous boric acid solution in the underwater stretching treatment were 2% by mass, and the amount of boric acid (parts by mass) in the crosslinking bath in the crosslinking treatment was 2 parts by mass.

[0077]

[0078] <Production of Polymer P1> In a reaction vessel equipped with a stirrer, thermometer, reflux condenser, and nitrogen gas inlet tube, a mixture containing butyl acrylate (65 parts by mass), methyl acrylate (23 parts by mass), 2-phenoxyethyl acrylate (6 parts by mass), 2,2'-azobisisobutyronitrile (AIBN) (0.1 parts by mass), and ethyl acetate and toluene as solvents (solids concentration 50% by mass, toluene content in the solvent 5% by mass) was stirred at 55°C for 6 hours under a nitrogen atmosphere (polymerization reaction). This yielded a solution containing an acrylic polymer (Polymer P1). Ethyl acetate was then added to this solution to adjust the polymer concentration of the solution to 30% by mass. This yielded a polymer solution containing an acrylic polymer (Polymer P1). The weight-average molecular weight of the acrylic polymer in the polymer solution was 1.15 million.

[0079] <Preparation of Protective Layer-Containing Member> The above polymer solution was applied to the corona-treated surface of a 38 μm-thick transparent polyethylene terephthalate (PET) film, one side of which (first side) had been corona-treated, and then heated at 130 ° C. for 2 minutes to dry, thereby forming a 5 μm-thick adhesive layer. The release-treated surface of a 25 μm-thick PET film (peelable film), one side of which had been subjected to a release treatment with a silicone-based release agent, was bonded to this adhesive layer to prepare a protective layer-containing member 1, which included a corona-treated PET film, a protective layer 1 (an adhesive layer), and a peelable film. Protective layer-containing member 2 was prepared according to the same procedure as the protective layer-containing member 1, except that the thickness of the protective layer was changed from 5 μm to 10 μm. Protective layer-containing member 3 was prepared according to the same procedure as the protective layer-containing member 1, except that the thickness of the protective layer was changed from 5 μm to 15 μm.

[0080] <Preparation of Laminate> A PET film (release film) having one surface subjected to a release treatment with a silicone-based release agent was removed from the protective layer-containing member 1, the exposed protective layer 1 was attached to the absorbing polarizer 1, and the resin substrate adjacent to the absorbing polarizer 1 was peeled off. The PET film (release film) having one surface subjected to a release treatment with a silicone-based release agent was removed from the protective layer-containing member 1, and a protective layer 1 was attached to the surface of the absorbing polarizer 1 opposite to the surface to which the protective layer 1 was attached, thereby preparing a laminate 1 including the absorbing polarizer 1 having the protective layer 1 on both sides. Note that a laminate 2 was prepared in the same manner as the preparation of the laminate 1 described above, except that a protective layer-containing member 2 was used instead of the protective layer-containing member 1. Furthermore, a laminate 3 was prepared in the same manner as the preparation of the laminate 1 described above, except that an absorbing polarizer 2 was used instead of the absorbing polarizer 1. Furthermore, a laminate 4 was prepared in the same manner as the preparation of the laminate 1 described above, except that an absorbing polarizer 3 was used instead of the absorbing polarizer 1. Furthermore, laminate 5 was produced in the same manner as the production procedure for laminate 1, except that absorbing polarizer 4 was used instead of absorbing polarizer 1. Furthermore, laminate 6 was produced in the same manner as the production procedure for laminate 1, except that protective layer-containing member 3 was used instead of protective layer-containing member 1. Furthermore, laminate 7 was produced in the same manner as the production procedure for laminate 1, except that absorbing polarizer 5 was used instead of absorbing polarizer 1.

[0081] <Preparation of Positive C Plate 1> The film thickness was adjusted with reference to the method described in paragraphs 0132 to 0134 of JP 2016-053709 A to prepare a positive C plate 1. The positive C plate 1 had Re=0.2 nm and Rth=−70 nm.

[0082] <Preparation of Retardation Layer 1> A reverse dispersion retardation layer 1 was prepared with reference to the method described in paragraphs 0151 to 0163 of JP 2020-084070 A. The retardation layer 1 had Re=146 nm and Rth=73 nm.

[0083] <Preparation of Optical Member> The corona-treated PET films were peeled from both sides of the laminate 1 to obtain an absorptive polarizer 1 having protective layers 1 on both sides. Next, the retardation layer 1, the reflective polarizer, the absorptive polarizer 1 having protective layers 1 on both sides, and the retardation layer 1 were bonded together in this order to prepare an optical member 1. The retardation layer 1 and the reflective polarizer were bonded together using a pressure-sensitive adhesive sheet "NCF-D692(5)" manufactured by Lintec Corporation. The optical member 2 was prepared according to the same procedure as the preparation of the optical member 1 described above, except that the laminate 2 was used instead of the laminate 1. The optical member 3 was prepared according to the same procedure as the preparation of the optical member 1 described above, except that the laminate 3 was used instead of the laminate 1. The optical member 4 was prepared according to the same procedure as the preparation of the optical member 1 described above, except that the laminate 4 was used instead of the laminate 1. The optical member 5 was prepared according to the same procedure as the preparation of the optical member 1 described above, except that the laminate 5 was used instead of the laminate 1. Optical member 6 was produced in the same manner as the above-described optical member 1, except that laminate 6 was used instead of laminate 1. Optical member 7 was produced in the same manner as the above-described optical member 1, except that laminate 7 was used instead of laminate 1.

[0084] <Preparation of Virtual Reality Display Device> An "Oculus Quest" virtual reality display device manufactured by Facebook was disassembled, and an image display panel was removed. This image display panel was an organic EL display panel, and the λ / 4 retardation layer and absorbing polarizer bonded to the surface were peeled off. Next, the prepared retardation layer 1, absorbing polarizer 5, retardation layer 1, and positive C plate 1 were bonded to the surface of the image display panel in this order using an adhesive sheet "NCF-D692(5)" manufactured by Lintec Corporation. Note that when bonding the retardation layer 1, absorbing polarizer 5, and positive C plate 1, their respective temporary supports were peeled off and removed. The image display panel 1 obtained in this manner emitted right-handed circularly polarized light. Next, a concave meniscus lens (made of optical glass) with a diameter of 50 mm and a curvature radius of the curved surface of 65 mm, half-mirror coated on one side, was prepared, and the prepared optical member 1 was molded onto the curved surface of the concave meniscus lens. That is, a laminate 1 having a curved surface was molded. The laminate 1 (optical element 1) was molded onto the curved surface of the concave meniscus lens by attaching a Lintec Corporation pressure-sensitive adhesive sheet "NCF-D692(5)" to the surface of the retardation layer 1 in the optical element 1, and then vacuum molding was performed using the method described in JP 2012-116094 A in a state where the separator film of the pressure-sensitive adhesive sheet was peeled off. The molding temperature was 120°C. In this manner, a half-mirror-coated concave meniscus lens 1 was produced in which the optical element 1 was attached to the curved surface. The optical element 1 was attached to the concave meniscus lens 1 so that the reflective polarizer was positioned closer to the half-mirror coat than the absorptive polarizer. The concave meniscus lens 1 was positioned so that the concave surface was on the viewing side, and the distance between the concave meniscus lens and the concave meniscus lens was adjusted so that the virtual reality display image was appropriately displayed, thereby producing the virtual reality display device 1. Virtual reality display device 2 was fabricated according to the same procedure as that for virtual reality display device 1, except that optical element 2 was used instead of optical element 1. Virtual reality display device 3 was fabricated according to the same procedure as that for virtual reality display device 1, except that optical element 3 was used instead of optical element 1. Virtual reality display device 4 was fabricated according to the same procedure as that for virtual reality display device 1, except that optical element 4 was used instead of optical element 1.Furthermore, virtual reality display device 5 was fabricated according to the same procedure as that for fabricating virtual reality display device 1 described above, except that optical element 5 was used instead of optical element 1. Furthermore, virtual reality display device 6 was fabricated according to the same procedure as that for fabricating virtual reality display device 1 described above, except that optical element 6 was used instead of optical element 1. Furthermore, virtual reality display device 7 was fabricated according to the same procedure as that for fabricating virtual reality display device 1 described above, except that optical element 7 was used instead of optical element 1.

[0085] <Evaluation> (Quantitative Evaluation of Boric Acid) Absorptive polarizer 1 was cut into a 1 cm x 1 cm piece, and after adding 3 cc of nitric acid, the piece was subjected to ashing treatment using a microwave at a maximum temperature of 230°C. Water was added to the resulting product to make the total amount 50 g, and the boron emission intensity was measured using an ICP-OES (Optima 7300DV) manufactured by PerkimElmer. Next, multiple aqueous solutions with known boric acid concentrations were prepared, and a calibration curve showing the relationship between the amount of boric acid and the emission intensity was prepared from the ICP emission intensity data of boron measured using each aqueous solution. Using this calibration curve, the amount of boric acid (g) was calculated from the boron emission intensity data measured using a sample of absorptive polarizer 1. Next, the calculated amount of boric acid (g) was divided by the volume of the sample (1 cm x 1 cm x thickness) to obtain the amount of boric acid (g / m 3 The amount of boric acid was calculated for absorptive polarizers 2 to 5 according to the same procedure.

[0086] (Polarization Degree Evaluation) Absorptive polarizer 1 was curved according to the same procedure as described above in <Fabrication of Virtual Reality Display Device>. The polarization performance of the obtained curved-formed absorptive polarizer 1 was evaluated by cutting a 2 cm square piece from the center of the absorptive polarizer 1 and bonding it to a Fujitac TD80UL (manufactured by Fujifilm Corporation) using a Lintec adhesive sheet "NCF-D692(5)." The luminosity-corrected degree of polarization was calculated using an automatic polarization film measuring device VAP-7070 manufactured by JASCO Corporation. The results are shown in Table 2 below. Here, the "luminosity-corrected degree of polarization" refers to the average value obtained by placing a light source, a linear polarizer, and the absorptive polarizer 1 in this order, measuring the transmittance in the wavelength range of 380 to 780 nm for light incident from the Fujitac TD80UL side, calculating the degree of polarization for each wavelength using the following formula, and multiplying the calculated values ​​by the luminosity correction coefficient: Polarization degree P (%) = {((Ty-Tx) / (Ty+Tx)) 1/2 × 100} Tx: transmittance when the incident polarized light emitted through the linear polarizer and the transmission axis of the absorptive polarizer 1 are arranged so that they are in a crossed Nicol state (incident polarized light is 100%) Ty: transmittance when the incident polarized light emitted through the linear polarizer and the transmission axis of the absorptive polarizer 1 are arranged so that they are in a paranic Nicol state (incident polarized light is 100%) The polarization degrees of absorptive polarizers 2 to 5 were also calculated according to the same procedure.

[0087] (Heat Resistance Test) The laminate 1 was curved according to the same procedure as described above in <Preparation of Virtual Reality Display Device>. A 2 cm x 2 cm central section was cut out of the curved laminate 1, the PET film was peeled off from one side, and the section was attached to a Fujitac TD80UL (manufactured by Fujifilm Corporation). The remaining PET film was then peeled off and attached to the Fujitac TD80UL to prepare a sample. The single-plate transmittance of the prepared sample was measured using the following method. The sample was then placed in a thermo-hygrostat and stored at 85°C dry for 500 hours to conduct a heat resistance test. The single-plate transmittance of the sample after the heat resistance test was measured using the following method. The single-plate transmittance change ΔT (single-plate transmittance after heat resistance test - single-plate transmittance before heat resistance test) was calculated from the single-plate transmittance values ​​measured before and after the heat resistance test using the above method. The closer the value of the transmittance change ΔT is to 0, the better the heat resistance. A to C are at a level that presents no practical problems. Heat resistance was also evaluated for Laminates 2 to 7 according to the same procedure. A: Transmittance change ΔT is 0.0% or more and less than 1.0% B: Transmittance change ΔT is 1.0% or more and less than 3.0% C: Transmittance change ΔT is 3.0% or more and less than 5.0% D: Transmittance change ΔT is 5.0% or more -Single Plate Transmittance- Transmittance refers to the average value obtained by multiplying the transmittance measured at wavelengths of 380 to 780 nm using an automatic polarizing film measuring device VAP-7070 manufactured by JASCO Corporation by a luminosity correction coefficient, and the single plate transmittance is defined as (Tx+Ty) / 2 shown in the following formula. Tx: transmittance when the incident polarized light and the transmission axis of the absorptive polarizer in the sample are arranged in crossed Nicols (incident polarized light is 100%). Ty: transmittance when the incident polarized light and the transmission axis of the absorptive polarizer in the sample are arranged in parallel Nicols (incident polarized light is 100%).

[0088] <Evaluation of image sharpness> In the produced virtual reality display devices 1 to 7, a black and white checkered pattern was displayed on the image display device, and the degree of image sharpness was visually evaluated using the following three-point scale. If the image sharpness is poor, part or all of the checkered pattern appears distorted. A or B is preferable. A: Distortion of the checkered pattern is barely noticeable. B: Distortion of the checkered pattern is slightly noticeable, but not bothersome. C: Distortion of the checkered pattern is clearly noticeable.

[0089]

[0090] As shown in Table 2, the laminate of the present invention exhibited the desired effects. A comparison of Examples 1 and 2 confirmed that when the thickness of the protective layer was 8.0 μm or less, the heat resistance was superior. A comparison of Examples 1 and 3 to 4 confirmed that when the amount of crosslinking agent was 0.020×10 -6 g / m 3 In the above cases, the heat resistance is excellent, and -6 g / m 3 In the above cases, it was confirmed that the heat resistance was even better.

[0091] 10, 38 Laminate 12, 26 Absorptive polarizer 14 First protective layer 16 Second protective layer 20 Image display panel 22, 26, 34, 42 λ / 4 retardation layer 28 Antireflection layer 30 Half mirror 32 Lens substrate 36 Reflective polarizer 38 Laminate 40 Reflective circular polarizer

Claims

1. A laminate comprising an absorptive polarizer which is a stretched resin film, a first protective layer disposed on one surface side of the absorptive polarizer, and a second protective layer disposed on the other surface side of the absorptive polarizer, the laminate having a curved surface portion, the absorptive polarizer containing a resin having a crosslinked portion, and an amount of a crosslinking agent derived from the crosslinked portion being 0.050×10 -6 g / m 3 or less, the first protective layer and the second protective layer each have a thickness of 0.10 to 10 μm, and the first protective layer and the second protective layer each contain a resin selected from the group consisting of an acrylic resin and a methacrylic resin.

2. A laminate comprising an absorptive polarizer which is a stretched resin film, a first protective layer disposed on one surface side of the absorptive polarizer, and a second protective layer disposed on the other surface side of the absorptive polarizer, the laminate having a curved surface portion, the absorptive polarizer containing a resin having a boric acid crosslinking portion, and an amount of boric acid derived from the boric acid crosslinking portion being 0.050×10 -6 g / m 3 or less, the first protective layer and the second protective layer each have a thickness of 0.10 to 10 μm, and the first protective layer and the second protective layer each contain a resin selected from the group consisting of an acrylic resin and a methacrylic resin.

3. The laminate according to claim 1 or 2, wherein the absorptive polarizer contains iodine and a polyvinyl alcohol-based resin.

4. A virtual reality display device having, in this order, an image display panel, an absorptive polarizer, a first retardation layer, a half mirror, a second retardation layer, a reflective polarizer, and the laminate according to claim 1 or 2.

5. A virtual reality display device comprising an image display panel, an absorptive polarizer, a retardation layer, a half mirror, a reflective circular polarizer, and the laminate according to claim 1 or 2, in this order.

Citation Information

Patent Citations

  • Preparation method and application of multifunctional modified starch-based hydrogel material

    CN115368638A

  • Multilayer structure and production method thereof

    JP2021192978A