Primer composition and laminate
The primer composition, featuring polyoxyalkylene polymers and an amine compound with hydrolyzable silyl groups, addresses the challenge of adhesion to concrete and mortar by improving adhesion and water-resistant properties, as shown in testing.
Patent Information
- Application Number
- PCT/JP2024/009469
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-03
AI Technical Summary
Curable compositions containing polyoxyalkylene polymers with hydrolyzable silyl groups face difficulties in adhering to concrete and mortar, especially in providing water-resistant adhesion.
A primer composition comprising a polyoxyalkylene polymer with hydrolyzable silyl groups and an amine compound having two hydrolyzable silyl groups, formulated to improve adhesion and water-resistant adhesion to concrete and mortar, with specific molecular weight ranges and structural characteristics for the polymers and amine compound.
The primer composition enhances the adhesion and water-resistant adhesion between the curable composition and concrete or mortar, as demonstrated by improved tensile strength and elongation at break, and cohesive fracture rates in testing.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Primer composition and laminate
[0001] The present invention relates to a primer composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group and an amine compound having two hydrolyzable silyl groups, and a laminate comprising the primer composition.
[0002] Organic polymers having hydrolyzable silyl groups have the property of crosslinking through the formation of siloxane bonds accompanied by the hydrolysis reaction of the hydrolyzable silyl groups due to moisture or the like, even at room temperature, to form a cured product.
[0003] Among these polymers having hydrolyzable silyl groups, polymers having a polyoxyalkylene main chain skeleton have already been industrially produced and are widely used for applications such as sealants and adhesives. Although these sealants and adhesives generally adhere to a variety of substrates, they have had the problem of poor adhesion to concrete, mortar, and other substrates that are subject to water immersion.
[0004] Therefore, when the sealants and adhesives are used on substrates to which they have difficulty adhering, a primer has generally been used to enhance adhesion. Examples of the primer include silane-based primers containing a silane coupling agent, acrylic-based primers containing a silyl group-containing acrylic polymer, and urethane-based primers containing a polyisocyanate and an isocyanate group-containing urethane prepolymer (see, for example, Patent Document 1).
[0005] Sealing materials containing polymers having hydrolyzable silyl groups, and primers containing polyoxyalkylene polymers having hydrolyzable silyl groups for use in adhesives, etc. have also been developed (e.g., Patent Documents 2 and 3).
[0006] Japanese Unexamined Patent Publication No. 2012-077143 Japanese Unexamined Patent Publication No. 07-011222 Unexamined Japanese Patent Application No. 07-011223
[0007] Curable compositions containing polyoxyalkylene polymers having hydrolyzable silyl groups sometimes have poor adhesion to concrete, mortar, and the like. Therefore, it has been common to apply a primer to concrete or mortar before applying the curable composition. However, even when a primer is used, there is still room for improvement in adhesion to concrete, mortar, and the like, particularly in water-resistant adhesion.
[0008] As a result of extensive research into solving the above problems, the present inventors have completed the following invention.
[0009] That is, the present invention provides: (A) a polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (1): —SiR 1 3 - a X a (1) (In formula (1), R 1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each X independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2. (B) A polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (2), having 3 or more terminal structures, and having a number average molecular weight of 1,000 to 10,000: -SiY 3 (2) A primer composition comprising: (in formula (2), each Y is independently a hydroxyl group or a hydrolyzable group); and (C) an amine compound having two hydrolyzable silyl groups, wherein the amount of the amine compound (C) is 12 to 50 parts by weight when the total amount of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) is 100 parts by weight.
[0010] An object of the present invention is to provide a primer composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group, which provides good adhesion, particularly water-resistant adhesion, between a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group and concrete, mortar, etc.
[0011] The present invention will be described in detail below.
[0012] The primer composition of the present invention comprises: (A) a polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (1) (sometimes simply referred to as "polyoxyalkylene polymer (A)" or "polymer (A)"); -SiR 1 3 - a X a (1) (In formula (1), R 1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2. (B) A polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (2), having 3 or more terminal structures, and having a number average molecular weight of 1,000 or more and 10,000 or less (sometimes simply referred to as "polyoxyalkylene polymer (B)" or "polymer (B)"); -SiY 3 (2) A primer composition comprising: (in formula (2), each Y is independently a hydroxyl group or a hydrolyzable group); and (C) an amine compound having two hydrolyzable silyl groups (sometimes simply referred to as "amine compound (C)"), wherein the amount of the amine compound (C) is 12 to 50 parts by weight when the total amount of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) is 100 parts by weight.
[0013] <<Polyoxyalkylene Polymer (A)>> A primer composition according to one embodiment of the present invention contains a polyoxyalkylene polymer (A) having a hydrolyzable silyl group represented by the following general formula (1).
[0014] -SiR 1 3 - a X a (1) (In formula (1), R 1each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each X independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2.
[0015] Use of a primer composition containing the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) described below can improve the adhesion and water-resistant adhesion between a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group and concrete, mortar, etc.
[0016] <Hydrolyzable Silyl Group> The polyoxyalkylene polymer (A) has a hydrolyzable silyl group represented by the following general formula (1).
[0017] -SiR 1 3 - a X a (1) (In formula (1), R 1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each X independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2.
[0018] R 1 are each independently a hydrocarbon group having 1 to 10 carbon atoms, which may have a substituent comprising a heteroatom-containing group or a halogen atom. The number of carbon atoms is preferably 1 to 6, more preferably 1 to 4, and particularly preferably 1 or 2. The hydrocarbon group may be an unsubstituted hydrocarbon group, or may be a hydrocarbon group having a substituent comprising a heteroatom-containing group or a halogen atom.
[0019] R 1Heteroatoms in the heteroatom-containing group included in include N, O, S, P, and Si. Suitable examples of the heteroatom-containing group include a mercapto group, a nitro group, a cyano group, alkoxy groups such as a methoxy group and an ethoxy group, alkylthio groups such as a methylthio group and an ethylthio group, acyl groups such as an acetyl group, acyloxy groups such as an acetyloxy group, and substituted or unsubstituted amino groups such as an amino group, a methylamino group, an ethylamino group, a dimethylamino group, and a diethylamino group.
[0020] R 1 The halogen atoms contained in include Cl, Br, I, and F.
[0021] R 1 Specific examples of the alkyl group include alkyl groups such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl; alkenyl groups such as vinyl and 2-propenyl; cycloalkyl groups such as cyclopropyl, cyclohexyl, and cyclooctyl; aryl groups such as phenyl, naphthalen-1-yl, and naphthalen-2-yl; aralkyl groups such as benzyl; halogenated methyl groups such as chloromethyl and bromomethyl; alkoxymethyl groups such as methoxymethyl, and aminomethyl groups such as diethylaminomethyl.
[0022] R 1 Suitable examples of R include alkyl groups such as a methyl group and an ethyl group; halogenated methyl groups such as a chloromethyl group; alkoxymethyl groups such as a methoxymethyl group; cycloalkyl groups such as a cyclohexyl group; aryl groups such as a phenyl group; and aralkyl groups such as a benzyl group. 1 As the alkyl group, a methyl group, a methoxymethyl group, and a chloromethyl group are preferred, a methyl group and a methoxymethyl group are more preferred, and a methyl group is even more preferred.
[0023] Examples of X include hydroxyl groups, halogens, alkoxy groups such as methoxy, ethoxy, propoxy, isopropoxy, butoxy, and tert-butoxy groups, acyloxy groups such as acetoxy groups, ketoximate groups, amino groups, amide groups, acid amide groups, aminooxy groups, mercapto groups, and alkenyloxy groups. Among these, alkoxy groups such as methoxy and ethoxy groups are more preferred, methoxy and ethoxy groups are even more preferred, and methoxy groups are particularly preferred, because of their mild hydrolysis and ease of handling.
[0024] a is 1 or 2. a is preferably 2.
[0025] Specific examples of hydrolyzable silyl groups include, but are not limited to, dimethoxymethylsilyl, diethoxymethylsilyl, dimethoxyethylsilyl, (chloromethyl)dimethoxysilyl, (chloromethyl)diethoxysilyl, (methoxymethyl)dimethoxysilyl, (methoxymethyl)diethoxysilyl, (N,N-diethylaminomethyl)dimethoxysilyl, and (N,N-diethylaminomethyl)diethoxysilyl groups. Among these, dimethoxymethylsilyl and diethoxymethylsilyl groups are preferred because of their mild hydrolysis and ease of handling.
[0026] The number of hydrolyzable silyl groups contained in one molecule of the polyoxyalkylene polymer (A) is preferably 0.5 or more, more preferably 1.0 or more, and even more preferably 1.2 or more, on average. The upper limit of the average number of hydrolyzable silyl groups is preferably 4.0 or less, and more preferably 3.0 or less. The range of the number of hydrolyzable silyl groups contained in one molecule is preferably 0.5 to 4.0, more preferably 1.0 to 3.0, and even more preferably 1.2 to 3.0.
[0027] <Main Chain Structure> The main chain structure of the polyoxyalkylene polymer (A) may be linear or branched, but is preferably linear in order to improve the flexibility of the cured primer composition.
[0028] The main chain of the polyoxyalkylene polymer (A) is -R 2 -O- (wherein, R 2 is a linear or branched alkylene group having 1 to 14 carbon atoms), and R 2 is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. 2 Specific examples of the repeating unit represented by —O— include —CH 2 O-, -CH 2 CH 2 O-, -CH 2 CH (CH 3 ) O—, —CH 2 C(CH 3 ) (CH 3 ) O—, —CH 2 CH 2 CH 2 CH 2 O-, etc., but -CH 2 CH 2 O-, -CH 2 CH (CH 3 )O— is preferred, and —CH 2 CH (CH 3 ) O- is more preferred.
[0029] The main chain structure of the polyoxyalkylene polymer (A) may contain a urethane bond, a urea bond, an ester bond, etc., but it is preferable that it does not contain such a bond.
[0030] The number average molecular weight of the polyoxyalkylene polymer (A), as measured by GPC in terms of polystyrene, is preferably 5,000 to 50,000, more preferably 7,000 to 40,000, particularly preferably 10,000 to 30,000, and most preferably 12,000 to 20,000. When the number average molecular weight is within the above range, a primer composition having a low viscosity and being easy to apply can be obtained.
[0031] The molecular weight of the polyoxyalkylene polymer (A) can also be expressed as an end-group-converted molecular weight obtained by directly measuring the end-group concentration of a polymer precursor before the introduction of hydrolyzable silyl groups by titration analysis based on the principles of the hydroxyl value measurement method specified in JIS K 1557 and the iodine value measurement method specified in JIS K 0070, and taking into consideration the polymer structure (the degree of branching determined by the polymerization initiator used). The number-average molecular weight of the polyoxyalkylene polymer (A) measured by GPC can also be obtained by preparing a calibration curve of the number-average molecular weight measured by GPC and the end-group-converted molecular weight, and converting the end-group-converted molecular weight of the polymer precursor into the number-average molecular weight measured by GPC of the hydrolyzable silyl group-containing polymer.
[0032] The molecular weight distribution (Mw / Mn) of the polyoxyalkylene polymer (A) is not particularly limited, but is preferably small. Specifically, it is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less.
[0033] The molecular weight distribution of the polyoxyalkylene polymer (A) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.
[0034] <Method for producing polyoxyalkylene polymer (A)> Preferred methods for producing the polyoxyalkylene polymer (A) include: (i) using a composite metal cyanide complex catalyst to polymerize an epoxy compound with a hydroxyl group-containing initiator to obtain a hydroxyl-terminated polyoxyalkylene polymer, converting the hydroxyl groups of the resulting hydroxyl-terminated polyoxyalkylene polymer to carbon-carbon unsaturated groups, and then adding a silane compound by a hydrosilylation reaction; (ii) using a composite metal cyanide complex catalyst to polymerize an epoxy compound with a hydroxyl group-containing initiator to obtain a hydroxyl-terminated polyoxyalkylene polymer, and then reacting the resulting hydroxyl-terminated polyoxyalkylene polymer with a compound having both a group reactive with a hydroxyl group and a hydrolyzable silyl group; and (iii) reacting a hydroxyl-terminated polyoxyalkylene polymer with an excess polyisocyanate compound to obtain a polymer having isocyanate groups at its terminals, and then reacting the resulting polymer with a compound having both a group reactive with an isocyanate group and a hydrolyzable silyl group.
[0035] Examples of initiators having a hydroxyl group that can be used in methods (i) and (ii) include those having one or more hydroxyl groups, such as ethylene glycol, propylene glycol, glycerin, pentaerythritol, low-molecular-weight polypropylene glycol, low-molecular-weight polyoxypropylene triol, allyl alcohol, methanol, ethanol, propanol, butanol, pentanol, hexanol, polypropylene monoallyl ether, and polypropylene monoalkyl ether.
[0036] When a polymer having a linear main chain structure is to be obtained, it is preferable to use an initiator having one or two hydroxyl groups, and it is more preferable to use an initiator having two hydroxyl groups.
[0037] Examples of epoxy compounds used in methods (i) and (ii) include alkylene oxides such as ethylene oxide and propylene oxide; and glycidyl ethers such as methyl glycidyl ether and allyl glycidyl ether. Of these, propylene oxide is preferred.
[0038] Examples of the carbon-carbon unsaturated group used in method (i) include a vinyl group, an allyl group, a methallyl group, and a propargyl group, with the allyl group being preferred.
[0039] As a method for converting the hydroxyl groups in (i) into carbon-carbon unsaturated groups, it is preferable to use a method in which an alkali metal salt is reacted with a hydroxyl-terminated polymer, and then a halogenated hydrocarbon compound having a carbon-carbon unsaturated bond is reacted therewith.
[0040] Examples of the halogenated hydrocarbon compound used in method (i) include vinyl chloride, allyl chloride, methallyl chloride, propargyl chloride, vinyl bromide, allyl bromide, methallyl bromide, propargyl bromide, vinyl iodide, allyl iodide, methallyl iodide, and propargyl iodide.
[0041] Examples of the hydrosilane compound that can be used in method (i) include dimethoxymethylsilane, diethoxymethylsilane, dimethoxyethylsilane, (chloromethyl)dimethoxysilane, (chloromethyl)diethoxysilane, (methoxymethyl)dimethoxysilane, (methoxymethyl)diethoxysilane, (N,N-diethylaminomethyl)dimethoxysilane, and (N,N-diethylaminomethyl)diethoxysilane.
[0042] The hydrosilylation reaction used in method (i) is accelerated by various catalysts. Known catalysts may be used as the hydrosilylation catalyst. Examples include chloroplatinic acid; chloroplatinic acid complexes composed of chloroplatinic acid and alcohols, aldehydes, or ketones; platinum-olefin complexes [e.g., Pt(CH 2 =CH 2 ) 2 (PPh 3 ), Pt(CH 2 =CH 2 ) 2 Cl 2 ]; platinum-vinylsiloxane complex [Pt{(vinyl)Me 2 SiOSiMe 2 (vinyl)}, Pt{Me(vinyl)SiO} 4 ] etc. can be used.
[0043] Examples of compounds having both a group reactive with a hydroxyl group and a hydrolyzable silyl group that can be used in method (ii) include isocyanate silanes such as 3-isocyanatepropyldimethoxymethylsilane and isocyanatemethyldimethoxymethylsilane; mercaptosilanes such as 3-mercaptopropyldimethoxymethylsilane; and epoxysilanes such as 3-glycidoxypropyldimethoxymethylsilane.
[0044] Examples of polyisocyanate compounds that can be used in method (iii) include aromatic polyisocyanates such as toluene (tolylene) diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate; and aliphatic polyisocyanates such as isophorone diisocyanate and hexamethylene diisocyanate.
[0045] Examples of compounds having both a group reactive with an isocyanate group and a hydrolyzable silyl group that can be used in method (iii) include amino group-containing silanes such as γ-aminopropyldimethoxymethylsilane, N-(β-aminoethyl)-γ-aminopropyldimethoxymethylsilane, γ-(N-phenyl)aminopropyldimethoxymethylsilane, N-ethylaminoisobutyldimethoxymethylsilane, and N-cyclohexylaminomethyldimethoxymethylsilane; hydroxy group-containing silanes such as γ-hydroxypropyldimethoxymethylsilane; and mercapto group-containing silanes such as γ-mercaptopropyldimethoxymethylsilane.
[0046] Furthermore, polyoxyalkylene polymers having multiple hydrolyzable silyl groups at one terminal can also be used as the polyoxyalkylene polymer (A). A method for producing a polyoxyalkylene polymer having multiple hydrolyzable silyl groups at one terminal involves first polymerizing an epoxy compound with a hydroxyl-containing initiator in the presence of a double metal cyanide complex catalyst to obtain a hydroxyl-terminated polyoxyalkylene polymer. An alkali metal salt is then reacted with the hydroxyl groups of the resulting polyoxyalkylene polymer, followed by reaction with allyl glycidyl ether. The resulting hydroxyl terminal is then again reacted with an alkali metal salt, followed by reaction with a halogenated hydrocarbon compound having a carbon-carbon unsaturated bond, to obtain a polyoxyalkylene polymer having multiple carbon-carbon unsaturated groups at one terminal. A silane compound is then added to the resulting polyoxyalkylene polymer having a carbon-carbon unsaturated group via a hydrosilylation reaction, thereby obtaining a polyoxyalkylene polymer having multiple hydrolyzable silyl groups at one terminal.
[0047] <<Polyoxyalkylene Polymer (B)>> A primer composition according to one embodiment of the present invention contains a polyoxyalkylene polymer (B) having a hydrolyzable silyl group represented by the following general formula (2), having three or more terminal structures, and having a number average molecular weight of 1,000 or more and 10,000 or less:
[0048] -SiY 3 (2) (In formula (2), each Y is independently a hydroxyl group or a hydrolyzable group.)
[0049] By preparing a primer composition containing the polyoxyalkylene polymer (B) and the polyoxyalkylene polymer (A), it is possible to improve the adhesion and water-resistant adhesion between a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group and concrete, mortar, etc.
[0050] <Hydrolyzable Silyl Group> The polyoxyalkylene polymer (B) has a hydrolyzable silyl group represented by the following general formula (2).
[0051] -SiY3 (2) (In formula (2), each Y is independently a hydroxyl group or a hydrolyzable group.) Examples of Y include a hydroxyl group; a halogen; an alkoxy group such as a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, and a tert-butoxy group; an acyloxy group such as an acetoxy group; a ketoximate group, an amino group, an amide group, an acid amide group, an aminooxy group, a mercapto group, and an alkenyloxy group. Among these, alkoxy groups such as a methoxy group and an ethoxy group are more preferred, a methoxy group and an ethoxy group are even more preferred, and a methoxy group is particularly preferred, because they are mildly hydrolyzable and easy to handle.
[0052] Specific examples of the hydrolyzable silyl group include a trimethoxysilyl group, a triethoxysilyl group, a tris(2-propenyloxy)silyl group, a triacetoxysilyl group, etc. Among these, the trimethoxysilyl group and the triethoxysilyl group are preferred, and the trimethoxysilyl group is more preferred, because they have high activity and provide good curability.
[0053] The number of hydrolyzable silyl groups contained in one molecule of the polyoxyalkylene polymer (B) is preferably 1.0 or more, more preferably 1.2 or more, and even more preferably 1.5 or more. The upper limit of the average is preferably 6.0 or less, more preferably 5.0 or less, and even more preferably 4.0 or less. The range of the number of hydrolyzable silyl groups contained in one molecule is preferably 1.0 or more and 6.0 or less, more preferably 1.2 or more and 5.0 or less, and even more preferably 1.5 or more and 4.0 or less.
[0054] <Main Chain Structure> The polyoxyalkylene polymer (B) has three or more terminal structures in one molecule.
[0055] The term "terminal structure" refers to a moiety located at the terminal of a polyoxyalkylene polymer. In the case of a polyoxyalkylene polymer obtained by polymerizing an alkylene oxide with an initiator having a hydroxyl group, the number of terminal structures is the same as the number of hydroxyl groups in the initiator.
[0056] The number of terminal structures in one molecule is three or more, preferably three to six, more preferably three to four, and even more preferably three.
[0057] The main chain of the polyoxyalkylene polymer (B) is -R 2 -O- (wherein, R 2 is a linear or branched alkylene group having 1 to 14 carbon atoms), and R2 is more preferably a linear or branched alkylene group having 2 to 4 carbon atoms. 2 Specific examples of the repeating unit represented by —O— include —CH 2 O-, -CH 2 CH 2 O-, -CH 2 CH (CH 3 ) O—, —CH 2 C(CH 3 ) (CH 3 ) O—, —CH 2 CH 2 CH 2 CH 2 O-, etc., but -CH 2 CH 2 O-, -CH 2 CH (CH 3 )O— is preferred, and —CH 2 CH (CH 3 ) O- is more preferred.
[0058] The main chain structure of the polyoxyalkylene polymer (B) may contain a urethane bond, a urea bond, an ester bond, or the like, but it is preferable that it does not contain such a bond.
[0059] The number average molecular weight of the polyoxyalkylene polymer (B), as calculated as polystyrene by GPC, is 1,000 to 10,000, preferably 2,000 to 8,000, more preferably 2,000 to 7,000, and even more preferably 2,000 to 6,000. When the number average molecular weight is within the above range, a primer composition having a low viscosity and being easy to apply can be obtained.
[0060] The molecular weight distribution (Mw / Mn) of the polyoxyalkylene polymer (B) is not particularly limited, but a small value is preferred. Specifically, it is preferably 1.6 or less, more preferably 1.4 or less, even more preferably 1.3 or less, and particularly preferably 1.2 or less. The molecular weight distribution of the polyoxyalkylene polymer (B) can be determined from the number average molecular weight and weight average molecular weight obtained by GPC measurement.
[0061] It is believed that the polyoxyalkylene polymer (B) has a main chain number-average molecular weight of 2,000 to 6,000, has three terminal structures per molecule, and has a trimethoxysilyl group as the hydrolyzable silyl group, which enables the production of a primer composition having low viscosity and improved adhesion.
[0062] <Method for Producing Polyoxyalkylene Polymer (B)> As a method for producing the polyoxyalkylene polymer (B), the same methods as the above-described methods (i) to (iii) for producing the polyoxyalkylene polymer (A) can be used.
[0063] Examples of initiators having hydroxyl groups that can be used in methods (i) and (ii) include those having three or more hydroxyl groups, such as glycerin, pentaerythritol, and low-molecular-weight polyoxypropylenetriol.
[0064] As the epoxy compound used in the methods (i) and (ii), the epoxy compounds described above in <<Polyoxyalkylene polymer (A)>> can be used.
[0065] As the carbon-carbon unsaturated group used in method (i), the carbon-carbon unsaturated groups described above in <<Polyoxyalkylene polymer (A)>> can be used.
[0066] As a method for converting the hydroxyl group of (i) into a carbon-carbon unsaturated group, the method described above in <<Polyoxyalkylene polymer (A)>> can be used.
[0067] As the halogenated hydrocarbon compound used in the method (i), the halogenated hydrocarbon compounds described above in <<Polyoxyalkylene polymer (A)>> can be used.
[0068] As the hydrosilane compound used in method (i), trimethoxysilane, triethoxysilane, tris(2-propenyloxy)silane, triacetoxysilane, etc. can be used.
[0069] The hydrosilylation reaction used in method (i) is accelerated by various catalysts. As the hydrosilylation catalyst, the known catalysts described above in <<Polyoxyalkylene Polymer (A)>> can be used.
[0070] Examples of compounds having both a group reactive with a hydroxyl group and a hydrolyzable silyl group that can be used in method (ii) include isocyanate silanes such as 3-isocyanatepropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, isocyanatemethyltrimethoxysilane, and isocyanatemethyltriethoxysilane; mercaptosilanes such as 3-mercaptopropyltrimethoxysilane and 3-mercaptopropyltriethoxysilane; and epoxy silanes such as 3-glycidoxypropyltrimethoxysilane and 3-glycidoxypropyltriethoxysilane.
[0071] As the polyisocyanate compound that can be used in the method (iii), the isocyanates described in the above-mentioned <<Polyoxyalkylene polymer (A)>> can be used.
[0072] Examples of compounds having both a group reactive with an isocyanate group and a hydrolyzable silyl group that can be used in the method (iii) include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, N-(β-aminoethyl)-γ-aminopropyltriethoxysilane, γ-(N-phenyl)aminopropyltrimethoxysilane, N-ethylaminoisobutyltrimethoxysilane, and N-cyclohexylaminomethyltrimethoxysilane; hydroxy group-containing silanes such as γ-hydroxypropyltrimethoxysilane; and mercapto group-containing silanes such as γ-mercaptopropyltrimethoxysilane.
[0073] Furthermore, a polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one end can also be used as the polyoxyalkylene polymer (B). The polyoxyalkylene polymer having a plurality of hydrolyzable silyl groups at one end can be produced by the method described above in <<Polyoxyalkylene polymer (A)>>.
[0074] <<Addition Amounts of Polyoxyalkylene Polymer (A) and Polyoxyalkylene Polymer (B)>> The ratio (A) / (B) of the addition amounts of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) is preferably 25 / 75 to 95 / 5, more preferably 40 / 60 to 90 / 10, and even more preferably 50 / 50 to 85 / 15. By setting the ratio within this range, a primer composition having low viscosity and improved adhesion can be obtained.
[0075] <<Amine Compound (C)>> The primer composition according to one embodiment of the present invention contains an amine compound having two hydrolyzable silyl groups. By including the amine compound (C), it is possible to improve the adhesion between a curable composition containing a polyoxyalkylene polymer having hydrolyzable silyl groups and concrete, mortar, or the like.
[0076] The amine compound (C) has two hydrolyzable silyl groups. The hydrolyzable silyl groups may be any of the silyl groups described above as the hydrolyzable silyl groups of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B). Preferred are dimethoxymethylsilyl, diethoxymethylsilyl, trimethoxysilyl, and triethoxysilyl groups, more preferred are dimethoxymethylsilyl, trimethoxysilyl, and triethoxysilyl groups, and even more preferred are dimethoxymethylsilyl and trimethoxysilyl groups.
[0077] The amine compound (C) preferably does not contain a siloxane bond (Si—O—Si).
[0078] The amine compound (C) has one or more amino groups, and preferably has one amino group in order to further improve adhesion to concrete, mortar, and the like.
[0079] Specific examples of the amino compound (C) include bis(3-triethoxysilylpropyl)amine and bis(3-trimethoxysilylpropyl)amine, which are available from Evonik as Dynasylan 1122 and Dynasylan 1124.
[0080] The amount of the amine compound (C) added is 12 to 50 parts by weight, preferably 12 to 40 parts by weight, more preferably 17 to 40 parts by weight, even more preferably 25 to 40 parts by weight, and most preferably 25 to 35 parts by weight, relative to 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B). By adjusting the amount within this range, the water-resistant adhesion between the curable composition containing the polyoxyalkylene polymer having a hydrolyzable silyl group and concrete, mortar, etc. is improved.
[0081] <<Primer Composition>> In addition to the polyoxyalkylene polymer (A), the polyoxyalkylene polymer (B), and the amine compound (C), the primer composition according to one embodiment of the present invention may contain additives such as a silanol condensation catalyst, an adhesion promoter other than the amine compound (C), a dehydrating agent, a plasticizer, a solvent, a diluent, an antioxidant, a light stabilizer, an ultraviolet absorber, and a filler.
[0082] <Silanol Condensation Catalyst> The primer composition according to one embodiment of the present invention may contain a silanol condensation catalyst that condenses the hydrolyzable silyl groups of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0083] Examples of silanol condensation catalysts include organotin compounds, metal carboxylates, amine compounds, carboxylic acids, and alkoxy metals.
[0084] Specific examples of organotin compounds include dibutyltin dilaurate, dibutyltin dioctanoate, dibutyltin bis(butyl maleate), dibutyltin diacetate, dibutyltin oxide, dibutyltin bis(acetylacetonate), dioctyltin bis(acetylacetonate), dioctyltin dilaurate, dioctyltin distearate, dioctyltin diacetate, dioctyltin oxide, reaction products of dibutyltin compounds with silicate compounds, reaction products of dioctyltin compounds with silicate compounds such as reaction products of bis(acetyloxy)dioctyltin with tetraethyl silicate ester, and reaction products of dibutyltin compounds with phthalate esters.
[0085] Specific examples of metal carboxylates include tin carboxylate, bismuth carboxylate, titanium carboxylate, zirconium carboxylate, iron carboxylate, potassium carboxylate, and calcium carboxylate. Specific examples include iron 2-ethylhexanoate (divalent), iron 2-ethylhexanoate (trivalent), titanium 2-ethylhexanoate, vanadium 2-ethylhexanoate, calcium 2-ethylhexanoate, potassium 2-ethylhexanoate, barium 2-ethylhexanoate, manganese 2-ethylhexanoate, nickel 2-ethylhexanoate, cobalt 2-ethylhexanoate, zirconium 2-ethylhexanoate, iron neodecanoate (divalent), iron neodecanoate (trivalent), titanium neodecanoate, Examples of the oleate include vanadium neodecanoate, calcium neodecanoate, potassium neodecanoate, barium neodecanoate, zirconium neodecanoate, iron oleate (divalent), iron oleate (trivalent), titanium oleate, calcium oleate, potassium oleate, cobalt oleate, zirconium oleate, iron naphthenate, iron naphthenate, titanium naphthenate, calcium naphthenate, potassium naphthenate, cobalt naphthenate, and zirconium naphthenate.
[0086] Specific examples of the amine compound include amines such as octylamine, 2-ethylhexylamine, laurylamine, and stearylamine; nitrogen-containing heterocyclic compounds such as pyridine, 1,8-diazabicyclo[5,4,0]undecene-7 (DBU), and 1,5-diazabicyclo[4,3,0]nonene-5 (DBN); guanidines such as guanidine, phenylguanidine, and diphenylguanidine; biguanides such as butylbiguanide, 1-o-tolylbiguanide, and 1-phenylbiguanide; amino group-containing silane coupling agents; and ketimine compounds.
[0087] Specific examples of carboxylic acids include acetic acid, propionic acid, butyric acid, 2-ethylhexanoic acid, lauric acid, stearic acid, oleic acid, linoleic acid, neodecanoic acid, and versatic acid.
[0088] Specific examples of alkoxy metals include titanium compounds such as tetrabutyl titanate titanium tetrakis(acetylacetonate) and diisopropoxytitanium bis(ethylacetoacetate), aluminum compounds such as aluminum tris(acetylacetonate) and diisopropoxyaluminum ethylacetoacetate, and zirconium compounds such as zirconium tetrakis(acetylacetonate).
[0089] Two or more different silanol condensation catalysts may be used in combination.
[0090] The amount of the silanol condensation catalyst used is preferably 0.001 to 20 parts by weight, more preferably 0.01 to 10 parts by weight, still more preferably 0.01 to 5 parts by weight, and most preferably 0.01 to 3 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0091] <Adhesion Imparting Agent Other Than Amine Compound (C)> The primer composition according to one embodiment of the present invention contains the amine compound (C) as an adhesion imparting agent, but may also contain an adhesion imparting agent other than the amine compound (C).
[0092] As the adhesion promoter, a silane coupling agent or a reaction product of a silane coupling agent can be added.
[0093] Specific examples of the silane coupling agent include amino group-containing silanes such as γ-aminopropyltrimethoxysilane, γ-aminopropylmethyldimethoxysilane, N-β-aminoethyl-γ-aminopropyltrimethoxysilane, N-β-aminoethyl-γ-aminopropylmethyldimethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, and (2-aminoethyl)aminomethyltrimethoxysilane; γ-isocyanatepropyltrimethoxysilane, γ-isocyanatepropyltriethoxy ... isocyanate group-containing silanes such as propylmethyldimethoxysilane, α-isocyanatomethyltrimethoxysilane, and α-isocyanatomethyldimethoxymethylsilane; mercapto group-containing silanes such as γ-mercaptopropyltrimethoxysilane, γ-mercaptopropyltriethoxysilane, and γ-mercaptopropylmethyldimethoxysilane; and epoxy group-containing silanes such as γ-glycidoxypropyltrimethoxysilane and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0094] Further, as the adhesion promoter, condensates of various silane coupling agents such as condensates of aminosilane and condensates of aminosilane and other alkoxysilanes, and reaction products of various silane coupling agents such as reaction products of aminosilane and epoxysilane, and reaction products of aminosilane and (meth)acrylic group-containing silane can also be used. Specific examples of commercially available adhesion promoters include Dynasylan 1146.
[0095] The adhesion promoters may be used alone or in combination of two or more.
[0096] The amount of the adhesion promoter other than the amine compound (C) used is preferably 0.1 to 40 parts by weight, more preferably 1.0 to 30 parts by weight, and still more preferably 3.0 to 20 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0097] <Dehydrating Agent> The primer composition according to one embodiment of the present invention may contain a dehydrating agent from the viewpoint of improving storage stability. The dehydrating agent is preferably an alkoxysilane compound capable of reacting with water. Specific examples of the dehydrating agent include n-propyltrimethoxysilane, vinyltrimethoxysilane, vinylmethyldimethoxysilane, γ-mercaptopropylmethyldimethoxysilane, γ-mercaptopropylmethyldiethoxysilane, and γ-glycidoxypropyltrimethoxysilane. Condensates obtained by partially condensing the above alkoxysilanes can also be used as dehydrating agents.
[0098] The amount of the dehydrating agent used is preferably 0.1 to 20 parts by weight, more preferably 1.0 to 10 parts by weight, and even more preferably 1.0 to 5.0 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0099] <Plasticizer> The primer composition according to one embodiment of the present invention may contain a plasticizer. Specific examples of the plasticizer include phthalate ester compounds such as dibutyl phthalate, diisononyl phthalate (DINP), diheptyl phthalate, di(2-ethylhexyl) phthalate, diisodecyl phthalate (DIDP), and butyl benzyl phthalate; terephthalate ester compounds such as bis(2-ethylhexyl)-1,4-benzenedicarboxylate; 1,2-cyclohexanedicarboxylic acid diisononyl ester (specifically, Hexamoll®, a product under the trade name of Hexamoll®); aliphatic polycarboxylic acid ester compounds such as dioctyl adipate, dioctyl sebacate, dibutyl sebacate, diisodecyl succinate, and acetyl tributyl citrate; unsaturated fatty acid ester compounds such as butyl oleate and methyl acetylricinoleate; alkylsulfonic acid phenyl esters (specifically, trade name: Mesamoll (manufactured by LANXESS)); phosphate ester compounds; trimellitic acid ester compounds; chlorinated paraffins; hydrocarbon oils such as alkyl diphenyls and partially hydrogenated terphenyls; process oils; and epoxy plasticizers such as epoxidized soybean oil and epoxy benzyl stearate.
[0100] Furthermore, polymer plasticizers can be used. Specific examples of polymer plasticizers include vinyl polymers, polyester plasticizers, polyether polyols such as polyethylene glycol and polypropylene glycol having a number average molecular weight of 500 or more, and polyethers such as derivatives in which the hydroxy groups of these polyether polyols are converted into ester groups, ether groups, etc., polystyrenes, and hydrocarbon polymers such as polybutadiene, polybutene, polyisobutylene, butadiene-acrylonitrile, and polychloroprene.
[0101] The amount of plasticizer used is preferably 5 to 150 parts by weight, more preferably 10 to 120 parts by weight, and even more preferably 20 to 100 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B). If the amount is less than 5 parts by weight, the effect of the plasticizer will not be exhibited, and if the amount exceeds 150 parts by weight, the mechanical strength of the cured product will be insufficient. The plasticizer may be used alone or in combination of two or more types.
[0102] <Solvent, Diluent> The primer composition according to one embodiment of the present invention may contain a solvent or diluent. The solvent and diluent are not particularly limited, but examples thereof include aliphatic hydrocarbons, aromatic hydrocarbons, alicyclic hydrocarbons, halogenated hydrocarbons, alcohols, esters, ketones, and ethers.
[0103] The amount of the solvent or diluent used is preferably 5 to 50 parts by weight, more preferably 5 to 20 parts by weight, and even more preferably 5 to 10 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0104] <Antioxidant> The primer composition according to one embodiment of the present invention may contain an antioxidant (antiaging agent). Examples of antioxidants include hindered phenol-based, monophenol-based, bisphenol-based, and polyphenol-based antioxidants.
[0105] Examples of antioxidants include BHT, Irganox 245, Irganox 1010, Irganox 1035, Irganox 1076, Irganox 1135, Irganox 1330, Irganox 1520, and SONGNOX 1076. Similarly, hindered amine light stabilizers such as TINUVIN 622LD, TINUVIN 144, and TINUVIN 292; CHIMASSORB 944LD and CHIMASSORB 119FL (all manufactured by BASF); ADK STAB LA-57, ADK STAB LA-62, ADK STAB LA-67, ADK STAB LA-63, and ADK STAB LA-68 (all manufactured by ADEKA Corporation); SANOL LS-2626, SANOL LS-1114, and SANOL LS-744 (all manufactured by Sankyo Lifetech Co., Ltd.); and NOCRAC CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) can also be used. Other antioxidants that can be used include SONGNOX 4120, NAUGUARD 445, and OKABEST CLX050.
[0106] Specific examples of antioxidants are also described in Japanese Patent Application Laid-Open Nos. 4-283259 and 9-194731.
[0107] The amount of the antioxidant used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0108] <Light Stabilizer> The primer composition according to one embodiment of the present invention may contain a light stabilizer. Use of a light stabilizer can prevent photooxidative degradation of the cured product. Examples of light stabilizers include benzotriazole-based, hindered amine-based, and benzoate-based compounds, with hindered amine-based compounds being particularly preferred.
[0109] Examples of hindered amine light stabilizers include TINUVIN 123, TINUVIN 144, TINUVIN 249, TINUVIN 292, TINUVIN 312, TINUVIN 622LD, TINUVIN 765, TINUVIN 770, TINUVIN 880, TINUVIN 5866, and TINUVIN B97; CHIMASSORB 119FL and CHIMASSORB 944LD (all manufactured by BASF); ADK STAB LA-57, LA-62, LA-63, LA-67, and LA-68 (all manufactured by ADEKA Corporation); SANOL LS-292, LS-2626, LS-765, LS-744, and LS-1114 (all manufactured by Sankyo Lifetech Co., Ltd.); SABOSTAB UV91 and SABOSTAB Examples of light stabilizers include UV119, SONGSORB CS5100, SONGSORB CS622, SONGSORB CS944 (all manufactured by SONGWON), and NOCRAC CD (manufactured by Ouchi Shinko Chemical Industry Co., Ltd.).
[0110] The amount of the light stabilizer used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0111] <UV Absorber> The primer composition according to one embodiment of the present invention may contain an UV absorber. The use of a UV absorber can improve the surface weather resistance of the cured product. Examples of UV absorbers include benzophenone-based, benzotriazole-based, salicylate-based, triazine-based, substituted acrylonitrile-based, and metal chelate-based compounds, with benzotriazole-based compounds being particularly preferred. Examples include Tinuvin 234, Tinuvin 326, Tinuvin 327, Tinuvin 328, Tinuvin 329, Tinuvin 350, Tinuvin 571, Tinuvin 900, Tinuvin 928, Tinuvin 1130, and Tinuvin 1600 (all manufactured by BASF); and SONGSORB 3290 (manufactured by SONGWON). Examples of triazine compounds include TINUVIN 400, TINUVIN 405, TINUVIN 477, and TINUVIN 1577ED (all manufactured by BASF), SONGSORB CS400, and SONGSORB 1577 (manufactured by SONGWON), etc. Examples of benzophenone compounds include SONGSORB 8100 (manufactured by SONGWON).
[0112] The amount of the ultraviolet absorber used is preferably 0.1 to 10 parts by weight, more preferably 0.2 to 5 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0113] <Filler> The primer composition according to one embodiment of the present invention may contain various fillers, such as heavy calcium carbonate, colloidal calcium carbonate, magnesium carbonate, diatomaceous earth, clay, talc, titanium oxide, fumed silica, precipitated silica, crystalline silica, fused silica, silicic acid anhydride, hydrated silicic acid, carbon black, ferric oxide, fine aluminum powder, zinc oxide, activated zinc white, PVC powder, PMMA powder, glass fiber, and filament.
[0114] The amount of the filler used is preferably 1 to 100 parts by weight, more preferably 5 to 50 parts by weight, per 100 parts by weight of the total of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B).
[0115] <<Preparation of Primer Composition>> The primer composition according to one embodiment of the present invention can be prepared as a one-component composition in which all ingredients are blended in advance and stored in a sealed container, and which cures with moisture in the air after application. Alternatively, the primer composition can be prepared as a two-component composition in which ingredients such as a curing catalyst, filler, plasticizer, and water are blended separately as a curing agent, and the curing agent and polymer composition are mixed before use. From the viewpoint of workability, a one-component primer composition is preferred.
[0116] <<Laminate Containing Primer Composition>> The primer composition according to one embodiment of the present invention is preferably used for bonding a substrate layer to various curable compositions.
[0117] The substrate layer is not particularly limited, but examples thereof include inorganic materials such as concrete, mortar, ceramic, and glass, various metals such as iron, stainless steel, aluminum, nickel, zinc, and copper, synthetic resin materials such as acrylic resin, phenolic resin, epoxy resin, polycarbonate resin, polybutylene terephthalate resin, acrylic electrodeposition paint, and fluororesin paint, and stone materials such as marble and granite, etc. Among these, the substrate layer is preferably made of concrete, mortar, glass, iron, stainless steel, aluminum, acrylic resin, epoxy resin, or polycarbonate resin, and more preferably made of concrete or mortar.
[0118] The curable composition is not particularly limited, and examples thereof include polymers having a hydrolyzable silyl group, such as polyoxyalkylene polymers having a hydrolyzable silyl group, (meth)acrylic acid ester polymers having a hydrolyzable silyl group, and hydrocarbon polymers having a hydrolyzable silyl group; urethane polymers; acrylic polymers; polysulfides; and epoxy resins. Among these, polymers having a hydrolyzable silyl group are preferred, and polyoxyalkylene polymers having a hydrolyzable silyl group are more preferred.
[0119] In particular, it is preferably used for bonding concrete or mortar to a composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group.
[0120] The laminate containing the primer composition according to one embodiment of the present invention is preferably a laminate comprising (X) a substrate layer, (Y) a cured layer obtained by curing the primer composition according to one embodiment of the present invention, and (Z) a cured layer obtained by curing a curable composition, wherein the (X) layer and the (Y) layer are in contact with each other and the (Y) layer is in contact with each other; and more preferably a laminate comprising (X) a substrate layer which is concrete or mortar, (Y) a cured layer obtained by curing the primer composition of the present invention, and (Z) a cured layer obtained by curing a composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group, wherein the (X) layer and the (Y) layer are in contact with each other and the (Y) layer is in contact with each other.
[0121] A preferred method for producing the laminate is to apply the primer composition according to one embodiment of the present invention to a substrate such as concrete or mortar, cure the applied primer composition, and then apply a composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group.
[0122] The method for applying the primer composition according to one embodiment of the present invention is not particularly limited, and a wide variety of conventionally known application means, such as application by brush, application by roll, or application by spray, can be used. 2 The amount of the coating is usually about 50 to 300 g, preferably about 50 to 150 g, per coating. To form a coating film on a substrate, after coating, the coating may be dried at room temperature or heated at a temperature of about 50 to 120°C.
[0123] <Curable Composition Containing Polyoxyalkylene Polymer Having Hydrolyzable Silyl Group> Examples of the curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group include sealing materials, adhesives, and coating materials containing a polyoxyalkylene polymer having a hydrolyzable silyl group.
[0124] As the hydrolyzable silyl group of the polyoxyalkylene polymer having a hydrolyzable silyl group, the hydrolyzable silyl groups described above in <<Polyoxyalkylene Polymer (A)>> and <<Polyoxyalkylene Polymer (B)>> can be used.
[0125] A polyoxyalkylene polymer having a hydrolyzable silyl group can be obtained by polymerizing an epoxy compound with an initiator having a hydroxyl group to obtain a hydroxyl-terminated polyoxyalkylene polymer, and then converting the hydroxyl terminal to a hydrolyzable silyl group.
[0126] The curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group may contain, in addition to the polyoxyalkylene polymer having a hydrolyzable silyl group, additives such as a silanol condensation catalyst, an adhesion promoter, a dehydrating agent, a plasticizer, a solvent, a diluent, an antioxidant, a light stabilizer, an ultraviolet absorber, a filler, a physical property adjuster, a tackifier resin, a compound containing an epoxy group, a photocurable substance, an oxygen-curable substance, or an epoxy resin.
[0127] <<Uses>> The primer composition according to one embodiment of the present invention is preferably used as a primer for various sealants, adhesives and coating materials, and more preferably used as a primer for sealants and adhesives.
[0128] Applications for using the primer composition according to one embodiment of the present invention include sealing applications such as sealants for joints of exterior materials such as sizing boards, sealants for direct glazing, sealants for double-glazing, and sealants for working joints; adhesive applications such as tile adhesives, adhesives for exterior panels, adhesives for interior panels, adhesives for stone veneer, adhesives for floor finishing, adhesives for waterproof sheets, adhesives for vehicle panels, and adhesives for assembling electrical, electronic, and precision equipment; and coating applications such as waterproof coating materials, materials to prevent concrete spalling, and air barrier coatings.
[0129] The primer composition according to one embodiment of the present invention has particularly good adhesion to concrete or mortar, and is therefore useful as a primer that improves adhesion between concrete or mortar and sealant, adhesion between a concrete or mortar base and floor adhesive, adhesion between concrete or mortar and tile adhesive, adhesion between concrete or mortar and crack repair material, adhesion between concrete or mortar and coating material, etc.
[0130] The present invention is not limited to the above-described embodiments, and various modifications are possible within the scope of the claims. Embodiments obtained by appropriately combining the technical means disclosed in different embodiments are also included in the technical scope of the present invention.
[0131] One aspect of the present invention includes the following configuration.
[0132] <1> (A) a polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (1): —SiR 1 3 - a X a (1) (In formula (1), R 1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each X independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2. (B) A polyoxyalkylene polymer having a hydrolyzable silyl group represented by the following general formula (2), having 3 or more terminal structures, and having a number average molecular weight of 1,000 to 10,000: -SiY 3 (2) A primer composition comprising: (in formula (2), each Y is independently a hydroxyl group or a hydrolyzable group); and (C) an amine compound having two hydrolyzable silyl groups, wherein the amount of the amine compound (C) is 12 to 50 parts by weight when the total amount of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) is 100 parts by weight.
[0133] <2> The primer composition according to <1>, wherein the polyoxyalkylene polymer (B) has a number average molecular weight of 1,000 to 6,000.
[0134] <3> The primer composition according to <1> or <2>, wherein the amine compound (C) has one amino group.
[0135] <4> The primer composition according to any one of <1> to <3>, wherein the polyoxyalkylene polymer (A) has a linear main chain structure.
[0136] <5> The primer composition according to any one of <1> to <4>, which is used for bonding concrete or mortar to a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group.
[0137] <6> A laminate comprising: (X) a substrate layer which is concrete or mortar; (Y) a cured layer obtained by curing the primer composition according to any one of <1> to <4>; and (Z) a cured layer obtained by curing a composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group, wherein the (X) layer and the (Y) layer are in contact with each other, and the (Y) layer and the (Z) layer are in contact with each other.
[0138] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples.
[0139] (Number Average Molecular Weight) The number average molecular weight in the examples is a GPC molecular weight measured under the following conditions.
[0140] Pumping system: Tosoh HLC-8220GPC Column: Tosoh TSKgel Super H series Solvent: THF (tetrahydroxyfuran) Molecular weight: polystyrene equivalent Measurement temperature: 40°C
[0141] The average number of silyl groups introduced per terminal or per molecule of the polymers shown in the examples was calculated from the results of NMR measurement and the structure of the polymer.
[0142] Synthesis Example 1 Polymer (A-1) Using polyoxypropylene glycol having a number-average molecular weight of approximately 4,500 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain polyoxypropylene (P-1) having hydroxyl groups at both ends and a number-average molecular weight of 14,300 and a molecular weight distribution Mw / Mn = 1.21. To the hydroxyl groups of the obtained hydroxyl-terminated polyoxypropylene (P-1), 1.2 molar equivalents of sodium methoxide were added as a 28% methanol solution. After distilling off the methanol by vacuum devolatilization, an additional 1.5 molar equivalents of allyl chloride was added relative to the hydroxyl groups of the polymer (P-1) to convert the terminal hydroxyl groups to allyl groups. After conversion, unreacted allyl chloride remaining in the reaction system was removed by vacuum devolatilization. The obtained unpurified polyoxypropylene was mixed and stirred with n-hexane and water, and the water was then removed by centrifugation to obtain a hexane solution. The metal salts in the polymer were removed by devolatilizing the hexane from the resulting hexane solution under reduced pressure. This yielded polyoxypropylene (Q-1) having allyl groups at its termini. 50 μL of a platinum divinyldisiloxane complex solution (a 3 wt % isopropanol solution calculated as platinum) was added to 500 g of this polymer (Q-1), and 8.6 g of dimethoxymethylsilane was slowly added dropwise while stirring. After reacting at 100°C for 2 hours, unreacted dimethoxymethylsilane was distilled off under reduced pressure to yield polyoxypropylene (A-1) having dimethoxymethylsilyl groups at its termini and a number-average molecular weight of 14,600. It was found that polymer (A-1) contained an average of 0.8 dimethoxymethylsilyl groups at each terminus and an average of 1.5 dimethoxymethylsilyl groups per molecule.
[0143] Synthesis Example 2 Polymer (A'-1) To 500 g of polymer (Q-1) obtained in Synthesis Example 1, 50 μL of a platinum divinyldisiloxane complex solution (a 3 wt % isopropanol solution calculated as platinum) was added, and 8.6 g of trimethoxysilane was slowly added dropwise while stirring. After reacting at 100°C for 2 hours, unreacted trimethoxysilane was distilled off under reduced pressure to obtain polyoxypropylene (A'-1) having terminal trimethoxysilyl groups and a number-average molecular weight of 14,600. It was found that polymer (A'-1) had an average of 0.8 trimethoxysilyl groups at each terminal and an average of 1.5 trimethoxysilyl groups per molecule.
[0144] Synthesis Example 3 Polymer (B-1) To a polyoxypropylene triol having a number-average molecular weight of approximately 4,500, 1.2 molar equivalents of sodium methoxide were added as a 28% methanol solution relative to the hydroxyl groups. After distilling off the methanol by vacuum devolatilization, 1.5 molar equivalents of allyl chloride relative to the hydroxyl groups of the polyoxypropylene triol were added to convert the terminal hydroxyl groups to allyl groups. After conversion, unreacted allyl chloride remaining in the reaction system was removed by vacuum devolatilization. The resulting crude polyoxypropylene, n-hexane, and water were mixed and stirred, and the water was removed by centrifugation to obtain a hexane solution. The hexane was then devolatilized under reduced pressure from the resulting hexane solution to remove metal salts from the polymer. As a result, a polyoxypropylene (Q-2) having terminal allyl groups was obtained. To 500 g of this polymer (Q-2), 50 μL of a platinum divinyldisiloxane complex solution (a 3 wt % isopropanol solution calculated as platinum) was added, and 40.7 g of trimethoxysilane was slowly added dropwise while stirring. After reacting at 100°C for 2 hours, unreacted trimethoxysilane was distilled off under reduced pressure to obtain polyoxypropylene (B-1) having a number average molecular weight of 5,200 and containing trimethoxysilyl groups at its terminals. It was found that polymer (B-1) contained an average of 0.7 trimethoxysilyl groups at each terminal and an average of 1.9 trimethoxysilyl groups per molecule.
[0145] Synthesis Example 4 Polymer (B'-1) 500 g of polymer (Q-2) obtained in Synthesis Example 3 was added with 50 μL of a platinum divinyldisiloxane complex solution (a 3 wt % isopropanol solution calculated as platinum), and 8.6 g of dimethoxymethylsilane was slowly added dropwise with stirring. After reacting at 100°C for 2 hours, unreacted dimethoxymethylsilane was distilled off under reduced pressure to obtain polyoxypropylene (B'-1) having terminal dimethoxymethylsilyl groups and a number-average molecular weight of 5,000. It was found that polymer (B'-1) contained an average of 0.7 dimethoxymethylsilyl groups at each terminal and an average of 2.0 dimethoxymethylsilyl groups per molecule.
[0146] Synthesis Example 5 Polymer (H-1) Using polyoxypropylene glycol having a number average molecular weight of approximately 2,000 as an initiator, propylene oxide was polymerized in the presence of a zinc hexacyanocobaltate glyme complex catalyst to obtain polyoxypropylene (P-2) having hydroxyl groups at both ends and a number average molecular weight of 28,500. Subsequently, 1.2 molar equivalents of sodium methoxide relative to the hydroxyl groups of this hydroxyl-terminated polyoxypropylene (P-2) were added as a 28% methanol solution. After distilling off the methanol by vacuum devolatilization, 1.5 molar equivalents of allyl chloride relative to the hydroxyl groups of polymer (P-2) were added to convert the terminal hydroxyl groups to allyl groups. After conversion, unreacted allyl chloride contained in the reaction system was removed by vacuum devolatilization. The obtained unpurified polyoxypropylene was mixed and stirred with n-hexane and water, and the water was removed by centrifugation to obtain a hexane solution. The hexane was devolatilized under reduced pressure from the obtained hexane solution to remove metal salts from the polymer. As a result, polyoxypropylene (Q-3) having allyl groups at its terminals was obtained. 50 μL of platinum divinyldisiloxane complex solution (3 wt % isopropanol solution calculated as platinum) was added to 500 g of this polymer (Q-3), and 4.5 g of trimethoxysilane was slowly added dropwise while stirring. After reacting at 100°C for 2 hours, unreacted trimethoxysilane was distilled off under reduced pressure to obtain polyoxypropylene (H-1) having trimethoxysilyl groups at its terminals and a number-average molecular weight of 29,100. It was found that polymer (H-1) had an average of 0.6 trimethoxysilyl groups at each terminal and an average of 1.2 trimethoxysilyl groups per molecule.
[0147] Synthesis Example 6 Polymer (H-2) To 500 g of polymer (Q-3) obtained in Synthesis Example 1, 50 μL of a platinum divinyldisiloxane complex solution (a 3 wt % isopropanol solution calculated as platinum) was added, and 5.4 g of trimethoxysilane was slowly added dropwise while stirring. After reacting at 100°C for 2 hours, unreacted trimethoxysilane was distilled off under reduced pressure to obtain polyoxypropylene (H-2) having terminal trimethoxysilyl groups and a number average molecular weight of 28,900. It was found that polymer (H-2) had an average of 0.7 trimethoxysilyl groups at each terminal and an average of 1.5 trimethoxysilyl groups per molecule.
[0148] (Preparation of Curable Composition) A mixture of 65 parts by weight of polymer (H-1) and 35 parts by weight of polymer (H-2), 100 parts by weight of diisononyl phthalate (manufactured by BASF, hereinafter referred to as DINP), 100 parts by weight of Hakuenka CCR (manufactured by Shiraishi Calcium Co., Ltd.: heavy calcium carbonate), 142.4 parts by weight of Omyacarb 2T-AV (manufactured by OMYA: colloidal calcium carbonate), 12.5 parts by weight of Ti-Pure 902 (manufactured by DuPont: titanium oxide), 26.4 parts by weight of Clevalac SLT (manufactured by Clevaly Co., Ltd.: amide wax), and Addworks IBC was used. 1 part by weight of 760 (manufactured by CLARIANT: a mixture of an ultraviolet absorber, a light stabilizer, and an antioxidant) and 1 part by weight of Irganox 245 (manufactured by BASF: ethylene bis(oxyethylene) bis-(3-(5-tert-butyl-4-hydroxy-m-tolyl) propionate) were mixed and uniformly dispersed using a three-roll mill. Thereafter, 9.75 parts by weight of VP700 (manufactured by WERNER HOLLBECK: a silane coupling agent), 5 parts by weight of Dynasylan VTMO (manufactured by Evonik: vinyltrimethoxysilane), and 0.5 parts by weight of TIB KAT423 (manufactured by TIB CHEMICALS: a dioctyltin-silane mixture) were added and thoroughly mixed with a spatula. The mixture was then uniformly mixed and degassed using a planetary centrifugal mixer to obtain curable composition (D).
[0149] Example 1 To 75 parts by weight of the polymer (A-1) described in Synthesis Example 1, 25 parts by weight of the polymer (B-1) described in Synthesis Example 3, 15 parts by weight of Dynasylan 1124 (manufactured by Evonik: bis(trimethoxysilylpropyl)amine), 15 parts by weight of Dynasylan 1146 (manufactured by Evonik: aminoalkyl group-modified alkylpolysiloxane), 3 parts by weight of Dynasylan AMMO (manufactured by Evonik: 3-aminopropyltrimethoxysilane), 2 parts by weight of Dynasylan VTMO, and 1.2 parts by weight of Neostan S-1 (manufactured by Nitto Kasei Kogyo Co., Ltd.: reaction product of silicate tetraethyl ester and bis(acetyloxy)dioctyltin) were added, and the mixture was thoroughly mixed with a spatula, and then uniformly mixed and degassed using a planetary centrifugal mixer to obtain a primer composition (E-1).
[0150] The obtained primer composition (E-1) was subjected to the following ISO 8340 test and ISO 10590 test.
[0151] (ISO 8340 Test): Test of Adhesion to Concrete Substrate Primer composition (E-1) was applied with a brush to a concrete substrate (manufactured by ROCHOLL: conforming to ISO 13640 Method 1, 71 x 12 x 25 mm) and cured for 1 hour at 23 ° C. and 50% relative humidity. Subsequently, H-type test specimens were prepared using the curable composition (D) according to a method conforming to ISO 8340 and aged for 28 days at 23 ° C. and 50% relative humidity. After aging, a tensile test was performed at a test speed of 6 mm / min, and the state of adhesion retention (presence or absence of peeled portions) at 100% elongation was confirmed and evaluated as follows. The tensile test was performed twice, and the numerical values of the tensile properties were taken as the average of the two tests. The results are shown in Table 1. A: Two H-type test specimens were evaluated, and there was no peeling in either of the cured specimens at 100% elongation. B: Two H-type test pieces were evaluated, and one showed no peeling when the cured product was elongated to 100%, while the other showed peeling. C: Two H-type test pieces were evaluated, and both showed peeling when the cured product was elongated to 100%. Furthermore, the strength at break (TB) and elongation at break (EB) were measured. Furthermore, the proportion of cohesive failure among the fracture states of the curable composition (D) after fracture was calculated as the cohesive failure rate. The results are shown in Table 1.
[0152] (ISO 10590 test): Test of waterproof adhesion to concrete substrate Primer composition (E-1) was applied with a brush to a concrete substrate (manufactured by ROCHOLL: conforming to ISO 13640 Method 1, 71 x 12 x 25 mm), and cured for 1 hour at 23 ° C. and 50% relative humidity. Then, using the curable composition (D), an H-type test specimen was prepared according to a method conforming to ISO 10590 and aged for 28 days at 23 ° C. and 50% relative humidity. After aging, the H-type test specimen was immersed in water for 4 days at 23 ° C., removed, and then dried for 1 day at 23 ° C. and 50% relative humidity. A tensile test was performed at a test speed of 6 mm / min, and the state of adhesion retention at 100% elongation (presence or absence of peeled portions) was confirmed and evaluated as follows. The results are shown in Table 1. A: Two H-type test specimens were evaluated, and there was no peeling in either of the cured specimens at 100% elongation. B: Two H-type test pieces were evaluated, and one showed no peeling when the cured product was elongated to 100%, while the other showed peeling. C: Two H-type test pieces were evaluated, and both showed peeling when the cured product was elongated to 100%. Furthermore, the strength at break (TB) and elongation at break (EB) were measured. Furthermore, the proportion of cohesive failure among the fracture states of the curable composition (D) after fracture was calculated as the cohesive failure rate. The tensile test was performed twice, and the numerical values of the tensile properties were calculated as the average of the two tests. The results are shown in Table 1.
[0153] Comparative Example 1 A primer composition (E-2) was obtained in the same manner as in Example 1, except that 25 parts by weight of polymer (B'-1) was used instead of 25 parts by weight of polymer (B-1). The obtained primer composition (E-2) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 1.
[0154] Comparative Example 2 A primer composition (E-3) was obtained in the same manner as in Example 1, except that 75 parts by weight of polymer (A'-1) was used instead of 75 parts by weight of polymer (A-1) and 0.3 parts by weight of Neostan S-1. The obtained primer composition (E-3) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 1.
[0155] Comparative Example 3 A primer composition (E-4) was obtained in the same manner as in Example 1, except that 75 parts by weight of polymer (A'-1) was used instead of 75 parts by weight of polymer (A-1), 25 parts by weight of polymer (B'-1) was used instead of 25 parts by weight of polymer (B-1), and 0.3 parts by weight of Neostan S-1. The obtained primer composition (E-4) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 1.
[0156] Comparative Example 4 A primer composition (E-5) was obtained in the same manner as in Example 1, except that the amount of Dynasylan 1146 added was 10 parts by weight and the amount of Dynasylan 1124 added was 10 parts by weight. The obtained primer composition (E-5) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 1.
[0157] Comparative Example 5 A primer composition (E-6) was obtained in the same manner as in Example 1, except that the amount of Dynasylan 1146 added was 5 parts by weight and the amount of Dynasylan 1124 added was 5 parts by weight. The obtained primer composition (E-6) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 1.
[0158]
[0159] As can be seen from Table 1, Example 1 containing polyoxyalkylene polymer (A) and polyoxyalkylene polymer (B) has good adhesion to concrete and water-resistant adhesion, whereas Comparative Example 1 containing a polyoxyalkylene polymer having a dimethoxymethylsilyl group instead of polyoxyalkylene polymer (B), Comparative Example 2 containing a polyoxyalkylene polymer having a trimethoxysilyl group instead of polyoxyalkylene polymer (A), and Comparative Example 3 containing a polyoxyalkylene polymer having a trimethoxysilyl group instead of polyoxyalkylene polymer (A) and a polyoxyalkylene polymer having a dimethoxymethylsilyl group instead of polyoxyalkylene polymer (B) have poor adhesion to concrete and water-resistant adhesion.
[0160] Furthermore, Comparative Examples 4 and 5, in which the content of amine compound (C) was less than 12 parts by weight when the total of polyoxyalkylene polymers (A) and (B) was 100 parts by weight, were inferior in water-resistant adhesion.
[0161] Example 2 A primer composition (E-7) was obtained in the same manner as in Example 1, except that the adhesion promoter Dynasylan 1146 was not added. The obtained primer composition (E-7) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 2.
[0162] Comparative Example 6 A primer composition (E-8) was obtained in the same manner as in Example 1, except that Dynasylan 1124, the amine compound (C), was not added. The obtained primer composition (E-8) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 2.
[0163]
[0164] For reference, the results of Example 1 are also shown in Table 2. As can be seen from Table 2, Examples 1 and 2, which contain the amine compound (C), have good adhesion to concrete and good water-resistant adhesion, whereas Comparative Example 6, which does not contain the amine compound (C), has poor adhesion to concrete and good water-resistant adhesion.
[0165] Example 3 A primer composition (E-9) was obtained in the same manner as in Example 1, except that the adhesion promoter Dynasylan 1146 was not added and the amount of Dynasylan 1124 added as the amine compound (C) was changed to 20 parts by weight. The obtained primer composition (E-9) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 3.
[0166] Example 4 A primer composition (E-10) was obtained in the same manner as in Example 1, except that the adhesion promoter Dynasylan 1146 was not added and the amount of Dynasylan 1124 added as the amine compound (C) was changed to 30 parts by weight. The obtained primer composition (E-10) was subjected to the same ISO 8340 test and ISO 10590 test as in Example 1. The results are shown in Table 3.
[0167]
[0168] For reference, the results of Example 2 are also shown in Table 3. From Table 3, it can be seen that Examples 2 to 4, in which the amount of amine compound (C) added was 15 to 30 parts by weight, had good adhesion to concrete and water-resistant adhesion.
Claims
1. (A) a polyoxyalkylene polymer having a hydrolyzable silyl group represented by the general formula (1), -SiR 1 3 - a X a (1) (In formula (1), R 1 each independently represents a hydrocarbon group having 1 to 10 carbon atoms which may have a substituent consisting of a heteroatom-containing group or a halogen atom; each independently represents a hydroxyl group or a hydrolyzable group; and a represents 1 or 2. (B) A polyoxyalkylene polymer having a hydrolyzable silyl group represented by general formula (2), having 3 or more terminal structures, and having a number average molecular weight of 1,000 to 10,000, and 3 (2) In formula (2), each Y is independently a hydroxyl group or a hydrolyzable group; and (C) an amine compound having two hydrolyzable silyl groups, wherein the amount of the amine compound (C) is 12 to 50 parts by weight when the total amount of the polyoxyalkylene polymer (A) and the polyoxyalkylene polymer (B) is 100 parts by weight.
2. The primer composition according to claim 1, wherein the polyoxyalkylene polymer (B) has a number average molecular weight of 1,000 to 6,000.
3. The primer composition according to claim 1 or 2, wherein the amine compound (C) has one amino group.
4. The primer composition according to claim 1 or 2, wherein the main chain structure of the polyoxyalkylene polymer (A) is a straight chain.
5. The primer composition according to claim 1 or 2, which is used for bonding concrete or mortar to a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group.
6. A laminate comprising: (X) a substrate layer which is concrete or mortar; (Y) a cured layer obtained by curing the primer composition according to claim 1 or 2; and (Z) a cured layer obtained by curing a curable composition containing a polyoxyalkylene polymer having a hydrolyzable silyl group, wherein the (X) layer and the (Y) layer are in contact with each other, and the (Y) layer and the (Z) layer are in contact with each other.
Citation Information
Patent Citations
Curable composition
JP1992283259A
Primer composition
JP1995011222A
Primer composition
JP1995011223A
Curable composition
JP1997194731A
Primer composition
JP2012077143A