Optical film
The optical film addresses visibility issues in VR goggles by controlling foreign matter content and manufacturing processes, resulting in improved image quality by reducing recognizable defects.
Patent Information
- Application Number
- PCT/JP2024/009615
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-12
- Publication Date
- 2024-10-03
AI Technical Summary
Image display devices, particularly VR goggles, face issues with visibility due to minute foreign objects within the optical film, which are easily recognized and affect image quality.
An optical film with controlled foreign matter content, specifically designed to minimize particles greater than 50 μm in diameter per unit length, and optimized manufacturing processes such as cutting and surface treatment to reduce fluff and improve visibility.
The optical film enhances the visibility of image display devices by reducing the presence of foreign particles and fluff, thereby minimizing defects and improving overall image quality in VR goggles.
Smart Images

Figure JP2024009615_03102024_PF_FP_ABST
Abstract
Description
Optical Film
[0001] The present invention relates to an optical film.
[0002] Image display devices, such as liquid crystal display devices and electroluminescence (EL) display devices (e.g., organic EL display devices), are rapidly becoming popular. In image display devices, optical components such as polarizing components and phase difference components are generally used to realize image display and improve image display performance (see, for example, Patent Document 1).
[0003] In recent years, new applications of image display devices have been developed. For example, goggles with displays (VR goggles) for realizing virtual reality (VR) have begun to be commercialized. The use of VR goggles in various situations is being considered, and improvements in visibility, such as higher definition, are desired.
[0004] Japanese Patent Application Laid-Open No. 2021-103286
[0005] In VR goggles, images are viewed through lenses, so minute foreign objects present inside the VR goggles tend to be easily visible.
[0006] In view of the above, the present invention provides an optical film that can contribute to improving the visibility of an image display device.
[0007] 1. An optical film according to an embodiment of the present invention is an optical film including at least one of a polarizing member or a retardation member, and the number of foreign particles having a major axis of more than 50 μm and not more than 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 10 or less. 2. In the optical film described in 1 above, the number of foreign particles having a major axis of more than 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face may be 3 or less. 3. In the optical film described in 1 or 2 above, the number of foreign particles having a major axis of more than 100 μm and not more than 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face may be 3 or less. 4. In the optical film described in any one of 1 to 3 above, the number of foreign particles having a major axis of more than 15 μm and not more than 50 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face may be 80 or less. 5. In the optical film described in any one of 1 to 4 above, the amount of foreign matter particles having a major axis of more than 5 μm and not more than 15 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face may be 30 or less. 6. In the optical film described in any one of 1 to 5 above, the foreign matter may include a component derived from a member contained in the optical film.
[0008] According to the embodiment of the present invention, the visibility of the image display device can be improved.
[0009] 1 is a perspective view schematically illustrating an optical film according to an embodiment of the present invention; FIG. 2 is a schematic perspective view for explaining an example of cutting processing; FIG. 3 is a schematic view showing a general configuration of an example of a display system for VR goggles; and FIG. 4 is a schematic cross-sectional view showing an example of the details of an optical film.
[0010] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to these embodiments. In addition, in order to clarify the description, the drawings may show the width, thickness, shape, etc. of each part more schematically than in the embodiment, but these are merely examples and do not limit the interpretation of the present invention.
[0011] (Definition of Terms and Symbols) The definitions of terms and symbols used in this specification are as follows. (1) Refractive Index (nx, ny, nz) "nx" is the refractive index in the direction in which the in-plane refractive index is maximum (i.e., the slow axis direction), "ny" is the refractive index in the in-plane direction perpendicular to the slow axis (i.e., the fast axis direction), and "nz" is the refractive index in the thickness direction. (2) In-Plane Retardation (Re) "Re(λ)" is the in-plane retardation measured with light having a wavelength of λ nm at 23°C. For example, "Re(550)" is the in-plane retardation measured with light having a wavelength of 550 nm at 23°C. Re(λ) is calculated by the formula: Re(λ) = (nx - ny) × d, where d (nm) is the thickness of the layer (film). (3) Thickness Direction Retardation (Rth) "Rth(λ)" is the retardation in the thickness direction measured with light having a wavelength of λ nm at 23°C. For example, "Rth(550)" is the retardation in the thickness direction measured with light having a wavelength of 550 nm at 23°C. Rth(λ) is calculated by the formula: Rth(λ) = (nx - nz) x d, where d (nm) is the thickness of the layer (film). (4) Nz coefficient The Nz coefficient is calculated by Nz = Rth / Re. (5) Angle When an angle is mentioned in this specification, the angle includes both clockwise and counterclockwise angles relative to the reference direction. Therefore, for example, "45°" means ±45°.
[0012] FIG. 1 is a perspective view schematically illustrating an optical film according to one embodiment of the present invention, showing a state in which multiple optical films are stacked. The optical film 2 can typically be obtained by cutting the outer peripheral surface of the optical film body so as to obtain a desired planar shape. The end surface 2a of the optical film 2 is a machined surface that has been subjected to cutting. For example, from the viewpoint of manufacturing efficiency, cutting can be performed simultaneously on multiple optical film bodies. Specifically, multiple optical film bodies are stacked to form an assembly (also referred to as a workpiece), and cutting can be performed on the multiple optical film bodies in the stacked state. Note that FIG. 1 shows the state after cutting has been performed on the workpiece.
[0013] The cutting process is typically performed using a cutting blade. FIG. 2 is a schematic perspective view illustrating an example of cutting process. A plurality of optical film bodies 3 are stacked to form a workpiece 4. When forming the workpiece 4, each optical film body 3 is cut in advance into any appropriate shape depending on the purpose. In the example shown in FIG. 2, the optical film body 3 is cut into a rectangular shape, but it may also be cut into other shapes (e.g., a circle). The number of optical film bodies 3 forming the workpiece 4 is not particularly limited, and may be, for example, 10 to 200 sheets, or may be 10 to 100 sheets. The thickness of the workpiece 4 is, for example, 5 mm to 50 mm.
[0014] In the example shown in FIG. 2 , the outer peripheral surface 4 a of the workpiece 4 is cut by the cutting portion 6 of a cutting tool. Specifically, a cutting blade 8 provided on the cutting portion 6 is brought into contact with the outer peripheral surface 4 a of the workpiece 4 to cut the outer peripheral surface 4 a of the workpiece 4. In the example shown in FIG. 2 , the cutting portion 6 of an end mill, which is a cutting tool, is rotated while the end mill is moved along the outer peripheral surface 4 a of the workpiece 4 to perform cutting. The rotation speed of the cutting portion 6 is, for example, 1,000 rpm to 60,000 rpm. The feed rate of the cutting portion 6 is, for example, 500 mm / min to 10,000 mm / min. The cutting process may be performed over the entire outer peripheral surface 4 a of the workpiece 4, or may be performed selectively at predetermined locations. During cutting, the workpiece 4 may be fixed by a fixture (not shown).
[0015] It is preferable that fuzz produced by cutting be removed from the end surface 2a, which is the processed surface of the optical film 2. Specific examples of fuzz include poor cutting or uncut areas. For example, the fuzz may be whisker-like protrusions, some of which are connected to the end surface of the optical film. The fuzz may contain components derived from the components contained in the optical film.
[0016] The number of foreign particles having a major axis exceeding 150 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face 2 a of the optical film 2 is preferably 3 or less, more preferably 2 or less, even more preferably 1 or less, and particularly preferably 0. The number of foreign particles having a major axis exceeding 50 μm and 150 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face 2 a of the optical film 2 is preferably 10 or less, more preferably 5 or less, even more preferably 3 or less, and particularly preferably 1 or less. The number of foreign particles having a major axis exceeding 100 μm and 150 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face 2 a of the optical film 2 is preferably 3 or less, more preferably 2 or less, even more preferably 1 or less, and particularly preferably 0 or less. The number of foreign particles having a major axis exceeding 50 μm and not exceeding 100 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face 2 a of the optical film 2 is preferably not more than 10, more preferably not more than 5, even more preferably not more than 3, and particularly preferably not more than 1. Here, the major axis refers to the longest linear distance between any two points on the cross-sectional shape.
[0017] The optical film can be typically applied to an image display device. In an image display device, foreign matter generated from the optical film may affect visibility. Specifically, foreign matter generated from the optical film may be visually recognized as a defect. Removing fuzz generated by cutting can contribute to improving the visibility of the image display device. Specifically, removing fuzz generated by cutting can reduce foreign matter generated from the optical film during the manufacturing process of an image display device or an image display panel, thereby suppressing the occurrence of defects. In VR goggles, foreign matter may be magnified and tend to be visually recognized as a defect. Therefore, removing fuzz generated by cutting can greatly contribute to improving visibility.
[0018] The amount (number) of foreign matter particles per 10 mm unit length in a direction perpendicular to the thickness direction of the end face of an optical film can be determined using an adhesive film. Specifically, the amount of foreign matter particles per unit length can be determined by attaching an adhesive film to the end face of the optical film, peeling it off, and counting the number of foreign matter particles adhering to the adhesive surface of the adhesive film. In one embodiment, as shown in FIG. 1 , multiple optical films are stacked so that their end faces are flush with each other, and an adhesive film F of a predetermined size is attached to the resulting flush surface and peeled off. The number of foreign matter particles adhering to the adhesive surface of the adhesive film F within a predetermined range is counted, and the counted number is divided by the number of optical films present within the predetermined range. When multiple optical film bodies are cut while stacked, the flush surface can be formed without aligning the optical films after cutting. The counting can be performed, for example, using PartSens manufactured by Intechnos Japan Co., Ltd.
[0019] The peeling force of the PSA film F used when counting the amount of the foreign matter (for example, peeling force from a glass plate) may be about 3.5 N / 25 mm.
[0020] The number of foreign particles having a major axis of more than 15 μm and not more than 50 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face of the optical film is preferably not more than 80, more preferably not more than 60, and even more preferably not more than 40. The number of foreign particles having a major axis of more than 15 μm and not more than 50 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face of the optical film may be, for example, not less than 20, or not less than 30.
[0021] The number of foreign particles having a major axis of more than 5 μm and not more than 15 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face of the optical film is preferably not more than 30, more preferably not more than 20, and even more preferably not more than 10. The number of foreign particles having a major axis of more than 5 μm and not more than 15 μm per unit length of 10 mm in the direction perpendicular to the thickness direction of the end face of the optical film may be, for example, not less than 1, or not less than 10.
[0022] Any appropriate method capable of achieving the above amount of foreign matter can be adopted as the method for removing the fuzz. In one embodiment, the fuzz is removed using tape. By using tape, the fuzz can be removed efficiently. It is preferable to remove the fuzz using tape multiple times. Specifically, it is preferable to remove the fuzz by applying tape to the machined surface and peeling it off multiple times.
[0023] The peeling strength of the tape used for removal is preferably 2 N / 25 mm or more, more preferably 3 N / 25 mm or more. With such a peeling strength, fuzz can be removed well. On the other hand, the peeling strength of the tape is preferably 10 N / 25 mm or less, more preferably 5 N / 25 mm or less. With such a peeling strength, defects such as delamination and lifting can be suppressed in the optical film.
[0024] In another embodiment, the burrs are removed by blowing gas (e.g., air) onto the machined surface, preferably pressurized gas.
[0025] The optical film according to the embodiment of the present invention typically includes an optical member such as a polarizing member or a retardation member. The optical film can be used in any appropriate image display device. For example, the optical film can be suitably used in VR goggles.
[0026] FIG. 3 is a schematic diagram showing the overall configuration of an example of a display system for VR goggles, illustrating the arrangement and shape of each component of the display system. The display system 10 includes a display element 12, a reflective polarizing element 14, a first lens unit 16, a half mirror 18, a first λ / 4 element 20, a second λ / 4 element 22, and a second lens unit 24. The reflective polarizing element 14 is disposed in front of the display surface 12a of the display element 12 and can reflect light emitted from the display element 12. The first lens unit 16 is disposed on the optical path between the display element 12 and the reflective polarizing element 14, and the half mirror 18 is disposed between the display element 12 and the first lens unit 16. The first λ / 4 element 20 is disposed on the optical path between the display element 12 and the half mirror 18, and the second λ / 4 element 22 is disposed on the optical path between the half mirror 18 and the reflective polarizing element 14.
[0027] The display element 12 is, for example, a liquid crystal display or an organic EL display, and has a display surface 12 a for displaying an image. The light emitted from the display surface 12 a passes through, for example, a polarizing member that may be included in the display element 12, and is converted into first linearly polarized light.
[0028] The first λ / 4 member 20 can convert the first linearly polarized light incident on the first λ / 4 member 20 into the first circularly polarized light. The first λ / 4 member 20 may be provided integrally with the display element 12.
[0029] The half mirror 18 transmits the light emitted from the display element 12 and reflects the light reflected by the reflective polarizing member 14 back toward the reflective polarizing member 14. The half mirror 18 is provided integrally with the first lens portion 16.
[0030] The second λ / 4 member 22 can transmit the light reflected by the reflective polarizing member 14 and the half mirror 18 through the reflective polarizing member 14. The second λ / 4 member 22 may be provided integrally with the first lens portion 16.
[0031] The first circularly polarized light output from the first λ / 4 member 20 passes through the half mirror 18 and the first lens portion 16, and is converted into the second linearly polarized light by the second λ / 4 member 22. The second linearly polarized light output from the second λ / 4 member 22 is reflected toward the half mirror 18 without passing through the reflective polarizing member 14. At this time, the polarization direction of the second linearly polarized light incident on the reflective polarizing member 14 is the same as the reflection axis of the reflective polarizing member 14. Therefore, the second linearly polarized light incident on the reflective polarizing member 14 is reflected by the reflective polarizing member 14.
[0032] The second linearly polarized light reflected by the reflective polarizing element 14 is converted into second circularly polarized light by the second λ / 4 element 22, and the second circularly polarized light emitted from the second λ / 4 element 22 passes through the first lens unit 16 and is reflected by the half mirror 18. The second circularly polarized light reflected by the half mirror 18 passes through the first lens unit 16 and is converted into third linearly polarized light by the second λ / 4 element 22. The third linearly polarized light is transmitted through the reflective polarizing element 14. At this time, the polarization direction of the third linearly polarized light incident on the reflective polarizing element 14 is the same direction as the transmission axis of the reflective polarizing element 14. Therefore, the third linearly polarized light incident on the reflective polarizing element 14 is transmitted through the reflective polarizing element 14.
[0033] The light transmitted through the reflective polarizing member 14 passes through the second lens portion 24 and enters the user's eye 26 .
[0034] The absorption axis of the polarizing member included in the display element 12 and the reflection axis of the reflective polarizing member 14 may be disposed approximately parallel to each other or approximately perpendicular to each other. The angle between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the first λ / 4 member 20 is, for example, 40° to 50°, or may be 42° to 48°, or may be approximately 45°. The angle between the absorption axis of the polarizing member included in the display element 12 and the slow axis of the second λ / 4 member 22 is, for example, 40° to 50°, or may be 42° to 48°, or may be approximately 45°.
[0035] The in-plane retardation Re(550) of the first λ / 4 member 20 is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The first λ / 4 member 20 preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The Re(450) / Re(550) of the first λ / 4 member 20 may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.
[0036] The in-plane retardation Re(550) of the second λ / 4 member 22 is, for example, 100 nm to 190 nm, or may be 110 nm to 180 nm, 130 nm to 160 nm, or 135 nm to 155 nm. The second λ / 4 member 22 preferably exhibits an inverse dispersion wavelength characteristic in which the retardation value increases according to the wavelength of the measurement light. The Re(450) / Re(550) of the second λ / 4 member 22 may be, for example, 0.75 or more and less than 1, or 0.8 or more and 0.95 or less.
[0037] Although not shown, display system 10 may also include an absorptive polarizer disposed in front of reflective polarizer 14. The reflective axis of the reflective polarizer and the absorption axis of the absorptive polarizer may be disposed approximately parallel to each other.
[0038] The optical film according to the embodiment of the present invention may include, for example, components included in the display system. Specifically, the optical film may include a polarizing component such as a reflective polarizing component or an absorptive polarizing component. The optical film may also include a retardation component such as a λ / 4 component. Furthermore, the optical film may include other components such as a protective component, an adhesive layer for integrating adjacent components, a surface protective film, and a release liner. The thickness of the optical film may vary depending on, for example, the type and number of components included, but is, for example, 200 μm to 400 μm.
[0039] FIG. 4 is a schematic cross-sectional view showing an example of the details of an optical film. FIG. 4 may also be a schematic cross-sectional view showing an example of the details of an optical film body before cutting. The optical film 2 includes a first λ / 4 member 20, a polarizing member 12b disposed on one side of the first λ / 4 member 20, and a protective member 30 disposed on the other side of the first λ / 4 member 20. The polarizing member 12b may correspond to the polarizing member that may be included in the display element (display element 12). An adhesive layer (e.g., a pressure-sensitive adhesive layer) 40 is provided on the polarizing member 12b side, and a release liner 50 is bonded to its surface. Furthermore, a surface protective film 60 is bonded to the surface of the protective member 30.
[0040] The first λ / 4 member 20 preferably has a refractive index characteristic that satisfies the relationship nx>ny≧nz. Here, "ny=nz" does not only mean that ny and nz are completely equal, but also includes cases where they are substantially equal. Therefore, there may be cases where ny<nz. The Nz coefficient of the first λ / 4 member 20 is preferably 0.9 to 3, more preferably 0.9 to 2.5, even more preferably 0.9 to 1.5, and particularly preferably 0.9 to 1.3.
[0041] The first λ / 4 member 20 may be made of any suitable material that satisfies the above characteristics, and may be, for example, a stretched resin film or an oriented and solidified layer of a liquid crystal compound.
[0042] Examples of resins contained in the resin film include polycarbonate-based resins, polyester carbonate-based resins, polyester-based resins, polyvinyl acetal-based resins, polyarylate-based resins, cyclic olefin-based resins, cellulose-based resins, polyvinyl alcohol-based resins, polyamide-based resins, polyimide-based resins, polyether-based resins, polystyrene-based resins, and acrylic-based resins. These resins may be used alone or in combination. Examples of methods for combining include blending and copolymerization. When the first λ / 4 member 20 exhibits reverse dispersion wavelength characteristics, a resin film containing a polycarbonate-based resin or a polyester carbonate-based resin (hereinafter sometimes simply referred to as a polycarbonate-based resin) can be suitably used.
[0043] Any suitable polycarbonate resin can be used as the polycarbonate resin. For example, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from at least one dihydroxy compound selected from the group consisting of alicyclic diols, alicyclic dimethanols, di-, tri-, or polyethylene glycols, and alkylene glycols or spiroglycols. Preferably, the polycarbonate resin contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, structural units derived from an alicyclic dimethanol and / or structural units derived from di-, tri-, or polyethylene glycol; more preferably, it contains structural units derived from a fluorene-based dihydroxy compound, structural units derived from an isosorbide-based dihydroxy compound, and structural units derived from di-, tri-, or polyethylene glycol. The polycarbonate resin may contain structural units derived from other dihydroxy compounds as needed. Details of polycarbonate-based resins that can be suitably used for the first λ / 4 member 20 and methods for forming the first λ / 4 member 20 are described, for example, in JP 2014-10291 A, JP 2014-26266 A, JP 2015-212816 A, JP 2015-212817 A, and JP 2015-212818 A, and the descriptions in these publications are incorporated herein by reference.
[0044] The thickness of the first λ / 4 member 20 made of a stretched resin film is, for example, 10 μm to 100 μm, preferably 10 μm to 70 μm, and more preferably 20 μm to 60 μm.
[0045] The above-mentioned liquid crystal compound alignment solidified layer is a layer in which the liquid crystal compound is aligned in a predetermined direction within the layer and the alignment state is fixed. The term "alignment solidified layer" encompasses an alignment solidified layer obtained by curing a liquid crystal monomer, as described below. In the first λ / 4 member 20, rod-shaped liquid crystal compounds are typically aligned in the slow axis direction of the first λ / 4 member 20 (homogeneous alignment). Examples of rod-shaped liquid crystal compounds include liquid crystal polymers and liquid crystal monomers. The liquid crystal compound is preferably polymerizable. If the liquid crystal compound is polymerizable, the alignment state of the liquid crystal compound can be fixed by aligning the liquid crystal compound and then polymerizing it.
[0046] The alignment and solidification layer of the liquid crystal compound (liquid crystal alignment and solidification layer) can be formed by performing an alignment treatment on the surface of a predetermined substrate, applying a coating liquid containing a liquid crystal compound to the surface to align the liquid crystal compound in a direction corresponding to the alignment treatment, and fixing the alignment state. Any appropriate alignment treatment can be used as the alignment treatment. Specific examples include mechanical alignment treatment, physical alignment treatment, and chemical alignment treatment. Specific examples of mechanical alignment treatment include rubbing treatment and stretching treatment. Specific examples of physical alignment treatment include magnetic field alignment treatment and electric field alignment treatment. Specific examples of chemical alignment treatment include oblique vapor deposition and photoalignment treatment. Any appropriate treatment conditions can be used for the various alignment treatments depending on the purpose.
[0047] The alignment of liquid crystal compounds is achieved by treating them at a temperature at which they exhibit a liquid crystal phase depending on the type of liquid crystal compound. By performing such temperature treatment, the liquid crystal compounds assume a liquid crystal state and are aligned in accordance with the alignment treatment direction of the substrate surface.
[0048] In one embodiment, the alignment state is fixed by cooling the liquid crystal compound aligned as described above. When the liquid crystal compound is polymerizable or crosslinkable, the alignment state is fixed by subjecting the liquid crystal compound aligned as described above to a polymerization treatment or a crosslinking treatment.
[0049] Any suitable liquid crystal polymer and / or liquid crystal monomer can be used as the liquid crystal compound. The liquid crystal polymer and the liquid crystal monomer can be used alone or in combination. Specific examples of liquid crystal compounds and methods for producing a liquid crystal alignment solidified layer are described in, for example, JP 2006-163343 A, JP 2006-178389 A, and WO 2018 / 123551 A. The descriptions in these publications are incorporated herein by reference.
[0050] The thickness of the first λ / 4 member 20 formed of the liquid crystal alignment solidified layer is, for example, 1 μm to 10 μm, preferably 1 μm to 8 μm, more preferably 1 μm to 6 μm, and even more preferably 1 μm to 4 μm.
[0051] The polarizing member 12b may include, for example, a resin film containing a dichroic material (sometimes referred to as an absorptive polarizing film). The thickness of the absorptive polarizing film is, for example, 1 μm to 20 μm, or may be 2 μm to 15 μm, or may be 12 μm or less, 10 μm or less, 8 μm or less, or may be 5 μm or less.
[0052] The absorptive polarizing film may be made from a single layer of resin film or may be made from a laminate of two or more layers.
[0053] When the absorptive polarizing film is produced from a single-layer resin film, for example, an absorptive polarizing film can be obtained by subjecting a hydrophilic polymer film such as a polyvinyl alcohol (PVA)-based film, a partially formalized PVA-based film, or a partially saponified ethylene-vinyl acetate copolymer-based film to a dyeing treatment with iodine or a dichroic substance such as a dichroic dye, a stretching treatment, etc. Among these, an absorptive polarizing film obtained by dyeing a PVA-based film with iodine and uniaxially stretching it is preferred.
[0054] The dyeing with iodine is carried out, for example, by immersing the PVA-based film in an aqueous iodine solution. The stretching ratio of the uniaxial stretching is preferably 3 to 7 times. The stretching may be carried out after the dyeing treatment or while dyeing. Alternatively, the PVA-based film may be dyed after stretching. If necessary, the PVA-based film may be subjected to a swelling treatment, a crosslinking treatment, a washing treatment, a drying treatment, or the like.
[0055] Examples of laminates produced using the two or more layer laminate include a laminate of a resin substrate and a PVA-based resin layer (PVA-based resin film) laminated on the resin substrate, and a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate. An absorptive polarizing film obtained using a laminate of a resin substrate and a PVA-based resin layer formed by coating on the resin substrate can be produced, for example, by applying a PVA-based resin solution to the resin substrate and drying the solution to form a PVA-based resin layer on the resin substrate, thereby obtaining a laminate of the resin substrate and the PVA-based resin layer, and then stretching and dyeing the laminate to convert the PVA-based resin layer into an absorptive polarizing film. In this embodiment, a polyvinyl alcohol-based resin layer containing a halide and a polyvinyl alcohol-based resin is preferably formed on one side of the resin substrate. The stretching typically involves immersing the laminate in an aqueous boric acid solution to stretch it. Furthermore, the stretching may optionally include in-air stretching of the laminate at a high temperature (e.g., 95°C or higher) before stretching in the boric acid aqueous solution. In addition, in this embodiment, the laminate is preferably subjected to a drying shrinkage treatment in which the laminate is heated while being transported in the longitudinal direction, thereby shrinking the laminate by 2% or more in the width direction. Typically, the manufacturing method of this embodiment includes subjecting the laminate to an auxiliary in-air stretching treatment, a dyeing treatment, an underwater stretching treatment, and a drying shrinkage treatment, in this order. By introducing auxiliary stretching, it is possible to increase the crystallinity of the PVA, even when the PVA is coated on a thermoplastic resin substrate, thereby achieving high optical properties. Furthermore, by simultaneously increasing the orientation of the PVA in advance, problems such as a decrease in orientation or dissolution of the PVA when immersed in water in the subsequent dyeing or stretching steps can be prevented, thereby achieving high optical properties. Furthermore, when the PVA-based resin layer is immersed in a liquid, the disordering of the polyvinyl alcohol molecules and the decrease in orientation can be suppressed compared to when the PVA-based resin layer does not contain a halide. This can improve the optical properties of the absorptive polarizing film obtained through treatment steps in which the laminate is immersed in a liquid, such as a dyeing treatment and an underwater stretching treatment.Furthermore, the optical properties can be improved by shrinking the laminate in the width direction through a drying shrinkage treatment.The obtained resin substrate / absorptive polarizing film laminate may be used as is (i.e., the resin substrate may be used as a protective layer for the absorptive polarizing film), or any suitable protective layer may be laminated depending on the purpose on the surface obtained by peeling the resin substrate from the resin substrate / absorptive polarizing film laminate or on the surface opposite to the peeled surface. Details of such methods for producing an absorptive polarizing film are described in, for example, JP-A-2012-73580 and Japanese Patent No. 6,470,455. The entire disclosures of these publications are incorporated herein by reference.
[0056] The polarizing member (absorptive polarizing film) preferably has a crossed transmittance (Tc) of 0.5% or less, more preferably 0.1% or less, and even more preferably 0.05% or less. The polarizing member (absorptive polarizing film) has a single transmittance (Ts) of, for example, 41.0% to 45.0%, and preferably 42.0% or more. The polarizing member (absorptive polarizing film) has a degree of polarization (P) of, for example, 99.0% to 99.997%, and preferably 99.9% or more.
[0057] The crossed transmittance, single transmittance, and degree of polarization can be measured, for example, using an ultraviolet-visible spectrophotometer. The degree of polarization P can be calculated from the obtained Tp and Tc by measuring the single transmittance Ts, parallel transmittance Tp, and crossed transmittance Tc using an ultraviolet-visible spectrophotometer, using the following formula: Ts, Tp, and Tc are Y values measured using a 2-degree visual field (C light source) according to JIS Z 8701 and corrected for visibility. Degree of polarization P (%) = {(Tp - Tc) / (Tp + Tc)} 1/2 ×100
[0058] The protective member 30 typically includes a substrate. The substrate may be composed of any appropriate film. Examples of materials that form the main component of the film constituting the substrate include cellulose-based resins such as triacetyl cellulose (TAC), polyester-based, polyvinyl alcohol-based, polycarbonate-based, polyamide-based, polyimide-based, polyethersulfone-based, polysulfone-based, polystyrene-based, cycloolefin-based resins such as polynorbornene, polyolefin-based, (meth)acrylic, and acetate-based resins. The thickness of the substrate is preferably 5 μm to 80 μm, more preferably 10 μm to 40 μm, and even more preferably 15 μm to 35 μm.
[0059] The protective member 30 may preferably have a substrate and a surface treatment layer formed on the substrate. A protective member having a surface treatment layer can be disposed so that the substrate is located on the first λ / 4 member 20 side. The surface treatment layer can have any appropriate function. For example, the surface treatment layer preferably has an anti-reflection function. The thickness of the surface treatment layer is preferably 1 μm to 20 μm, more preferably 2 μm to 15 μm, and even more preferably 3 μm to 10 μm.
[0060] Although not shown, a member (so-called positive C plate) whose refractive index characteristics can exhibit the relationship nz > nx = ny may be provided in the optical film 2 (for example, between the first λ / 4 member 20 and the protective member 30). The thickness direction retardation Rth(550) of the positive C plate is preferably −50 nm to −300 nm, more preferably −70 nm to −250 nm, even more preferably −90 nm to −200 nm, and particularly preferably −100 nm to −180 nm. Here, "nx = ny" encompasses not only the case where nx and ny are strictly equal, but also the case where nx and ny are substantially equal. The in-plane retardation Re(550) of the positive C plate is, for example, less than 10 nm.
[0061] The positive C plate can be formed from any suitable material, but is preferably composed of a film containing a liquid crystal material fixed in homeotropic alignment. The liquid crystal material (liquid crystal compound) that can be homeotropically aligned may be a liquid crystal monomer or a liquid crystal polymer. Specific examples of such liquid crystal compounds and methods for forming a positive C plate include the liquid crystal compounds and methods for forming the retardation layer described in paragraphs
[0020] to
[0028] of JP 2002-333642 A. In this case, the thickness of the positive C plate is preferably 0.5 μm to 5 μm.
[0062] The release liner 50 may be made of any suitable resin film. Specific examples of materials that may be the main component of the resin film include polyethylene terephthalate (PET), polyethylene, and polypropylene. The resin film materials may be used alone or in combination.
[0063] A release treatment layer may be provided on the surface of the release liner 50 that comes into contact with the adhesive layer 40. Examples of release treatment agents that form the release treatment layer include silicone-based release treatment agents, fluorine-based release treatment agents, and long-chain alkyl acrylate-based release agents. These can be used alone or in combination. The thickness of the release treatment layer is typically 50 nm or more and 400 nm or less. The thickness of the release liner is, for example, 5 μm or more and 60 μm or less, and preferably 20 μm or more and 45 μm or less. Note that when a release treatment layer is applied, the thickness of the release liner includes the thickness of the release treatment layer.
[0064] A typical example of the surface protection film 60 is a laminate of a substrate film and a pressure-sensitive adhesive layer. Materials for forming the substrate film include polyester-based polymers such as polyethylene terephthalate (PET), polyethylene naphthalate (PEN), and polybutylene terephthalate (PBT); cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose; polycarbonate-based polymers; (meth)acrylic polymers such as polymethyl methacrylate; and cycloolefin-based polymers such as polynorbornene. These may be used alone or in combination of two or more. The thickness of the substrate film is, for example, 5 μm or more and 200 μm or less, and preferably 20 μm or more and 100 μm or less.
[0065] The pressure-sensitive adhesive layer of the laminate may have any suitable structure. Specific examples include acrylic pressure-sensitive adhesives, rubber pressure-sensitive adhesives, silicone pressure-sensitive adhesives, polyester pressure-sensitive adhesives, urethane pressure-sensitive adhesives, epoxy pressure-sensitive adhesives, and polyether pressure-sensitive adhesives. By adjusting the type, number, combination, and compounding ratio of the monomers forming the base resin of the pressure-sensitive adhesive, as well as the amount of cross-linking agent, reaction temperature, reaction time, etc., a pressure-sensitive adhesive having desired properties can be prepared according to the intended purpose. The base resin of the pressure-sensitive adhesive may be used alone or in combination of two or more types. The base resin is preferably an acrylic resin (specifically, the pressure-sensitive adhesive layer is preferably composed of an acrylic pressure-sensitive adhesive). The thickness of the pressure-sensitive adhesive layer is, for example, 5 μm to 15 μm.
[0066] Although not shown, each component included in the optical film is preferably integrated via an adhesive layer. The adhesive layer may be formed of an adhesive or a pressure-sensitive adhesive. The thickness of the adhesive layer is, for example, 0.05 μm to 30 μm, preferably 3 μm to 20 μm, and more preferably 5 μm to 15 μm.
[0067] The present invention will be described in detail below using examples, but the present invention is not limited to these examples. The thickness, retardation value, and peel force were measured using the following measurement methods. <Thickness> Thicknesses of 10 μm or less were measured using a scanning electron microscope (manufactured by JEOL Ltd., product name "JSM-7100F"). Thicknesses exceeding 10 μm were measured using a digital micrometer (manufactured by Anritsu Corporation, product name "KC-351C"). <Retardation Value> Retardation values at each wavelength at 23°C were measured using a Mueller matrix polarimeter (manufactured by Axometrics, product name "Axoscan"). <Peel Force> Peel force was measured by bonding a sample cut to a size of 25 mm wide and 150 mm long to a glass plate, and then peeling the sample in the longitudinal direction at a peel rate of 300 mm / min and a peel angle of 90° using a universal tensile tester, and the peel force (N / 25 mm) was measured under an environment of 23°C and 50% RH. The same sample was measured five times and the average value was calculated.
[0068] [Example 1] (Preparation of λ / 4 Member) Polymerization was carried out using a batch polymerization apparatus consisting of two vertical reactors equipped with stirring blades and reflux condensers controlled at 100° C. 29.60 parts by mass (0.046 mol) of bis[9-(2-phenoxycarbonylethyl)fluoren-9-yl]methane, 29.21 parts by mass (0.200 mol) of isosorbide (ISB), 42.28 parts by mass (0.139 mol) of spiroglycol (SPG), 63.77 parts by mass (0.298 mol) of diphenyl carbonate (DPC), and 1.19×10 calcium acetate monohydrate as a catalyst. -2 Parts by mass (6.78×10 -5mol) was charged. After purging the reactor with nitrogen under reduced pressure, heating was performed with a heat medium, and stirring was initiated when the internal temperature reached 100°C. 40 minutes after the start of the temperature increase, the internal temperature reached 220°C, and while controlling to maintain this temperature, pressure reduction was initiated. 90 minutes after reaching 220°C, the pressure was reduced to 13.3 kPa. Phenol vapor by-produced during the polymerization reaction was introduced into a reflux condenser at 100°C, and a small amount of monomer components contained in the phenol vapor were returned to the reactor, while uncondensed phenol vapor was introduced into a condenser at 45°C and recovered. Nitrogen was introduced into the first reactor, and the pressure was temporarily restored to atmospheric pressure. The oligomerized reaction liquid in the first reactor was then transferred to the second reactor. Next, heating and pressure reduction in the second reactor were initiated, and the internal temperature reached 240°C and the pressure reached 0.2 kPa in 50 minutes. Polymerization was then allowed to proceed until the predetermined stirring power was achieved. When the predetermined power was reached, nitrogen was introduced into the reactor to restore pressure, and the polyester carbonate resin produced was extruded into water, and the strands were cut to obtain pellets.
[0069] The obtained polyester carbonate resin (pellets) was vacuum dried at 80 ° C for 5 hours, and then a film-forming device equipped with a single-screw extruder (manufactured by Toshiba Machine Co., Ltd., cylinder set temperature: 250 ° C), a T-die (width 200 mm, set temperature: 250 ° C), a chill roll (set temperature: 120-130 ° C), and a winder was used to produce a long resin film with a thickness of 135 μm. The obtained long resin film was stretched in the width direction at a stretching temperature of 143 ° C and a stretch ratio of 2.8 times to obtain a stretched film with a thickness of 47 μm. The Re (550) of the obtained stretched film was 143 nm, Re (450) / Re (550) was 0.86, and the Nz coefficient was 1.12.
[0070] (Formation of Positive C Plate) A liquid crystal coating solution was prepared by dissolving 20 parts by weight of a side-chain liquid crystal polymer represented by the following chemical formula (1) (the numbers 65 and 35 in the formula indicate the mole percent of the monomer unit, and are conveniently represented as a block polymer; weight-average molecular weight 5000), 80 parts by weight of a polymerizable liquid crystal exhibiting a nematic liquid crystal phase (manufactured by BASF: trade name Paliocolor LC242), and 5 parts by weight of a photopolymerization initiator (manufactured by Ciba Specialty Chemicals: trade name Irgacure 907) in 200 parts by weight of cyclopentanone. The coating solution was then applied to a PET substrate that had been subjected to a vertical alignment treatment using a bar coater, and the liquid crystal was aligned by heating and drying at 80°C for 4 minutes. The liquid crystal layer was irradiated with ultraviolet light to harden the liquid crystal layer, thereby forming a positive C plate with a thickness of 4 μm and an Rth(550) of −100 nm on the substrate.
[0071] (Preparation of Protective Member) The following hard coat layer-forming material was applied to an acrylic film (thickness: 40 μm) having a lactone ring structure and heated at 90° C. for 1 minute. After heating, the applied layer was irradiated with a high-pressure mercury lamp at an integrated light intensity of 300 mJ / cm 2 The coating layer was cured by irradiating ultraviolet rays of 1000 W / cm 2 with the acrylic film (thickness: 44 μm) on which a hard coat layer of 4 μm in thickness was formed. Next, the antireflection layer-forming coating solution A described below was applied onto the hard coat layer using a wire bar, and the applied coating solution was heated at 80°C for 1 minute and dried to form a coating film. The dried coating film was then irradiated with ultraviolet rays of 1000 W / cm 2 with the acrylic film (thickness: 44 μm). 2 The coating film was cured by irradiating it with ultraviolet light of 1000 kJ / cm to form an antireflection layer A having a thickness of 140 nm. Subsequently, the following coating solution B for forming an antireflection layer was applied onto the antireflection layer A using a wire bar, and the applied coating solution was heated at 80°C for 1 minute and dried to form a coating film. The dried coating film was irradiated with ultraviolet light of 1000 kJ / cm to form an antireflection layer A having a thickness of 140 nm. 2 The coating film was cured by irradiation with ultraviolet light of 1000 .ANG. to form an antireflection layer B having a thickness of 105 nm. In this way, a protective member (thickness: 44 .mu.m) was obtained.
[0072] (Hard Coat Layer-Forming Material) A hard coat layer-forming material was prepared by mixing 50 parts by weight of a urethane acrylic oligomer (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Oligo UA-53H"), 30 parts by weight of a polyfunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Ltd., trade name "Viscoat #300"), 20 parts by weight of 4-hydroxybutyl acrylate (manufactured by Osaka Organic Chemical Industry Ltd.), 1 part by weight of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100"), and 3 parts by weight of a photopolymerization initiator (manufactured by Ciba Japan KK, "Irgacure 907"), and diluting the mixture with methyl isobutyl ketone to a solids concentration of 50% by weight.
[0073] (Anti-reflection layer-forming coating solution A) 100 parts by weight of a polyfunctional acrylate (manufactured by Arakawa Chemical Industries, Ltd., trade name "Opstar KZ6728", solid content 20 wt%), 3 parts by weight of a leveling agent (manufactured by DIC Corporation, "GRANDIC PC4100"), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF Corporation, trade name "OMNIRAD907", solid content 100 wt%) were mixed. This mixture was diluted with butyl acetate as a dilution solvent to a solid content of 12 wt%, and the mixture was stirred to prepare anti-reflection layer-forming coating solution A.
[0074] (Anti-Reflection Layer-Forming Coating Solution B) 100 parts by weight of a polyfunctional acrylate containing pentaerythritol triacrylate as a main component (manufactured by Osaka Organic Chemical Industry Ltd., trade name "Viscoat #300", solid content 100% by weight), 150 parts by weight of hollow nanosilica particles (manufactured by JGC Catalysts and Chemicals Industries, Ltd., trade name "Surulia 5320", solid content 20% by weight, weight average particle diameter 75 nm), 50 parts by weight of solid nanosilica particles (manufactured by Nissan Chemical Industries, Ltd., trade name "MEK-2140Z-AC", solid content 30% by weight, weight average particle diameter 10 nm), 12 parts by weight of a fluorine-containing additive (manufactured by Shin-Etsu Chemical Co., Ltd., trade name "KY-1203", solid content 20% by weight), and 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907", solid content 100% by weight) were mixed. To this mixture was added a mixed solvent of TBA (tertiary butyl alcohol), MIBK (methyl isobutyl ketone), and PMA (propylene glycol monomethyl ether acetate) in a weight ratio of 60:25:15 as a dilution solvent, so that the total solid content was 4% by weight, and the mixture was stirred to prepare coating solution B for forming an anti-reflection layer.
[0075] (Preparation of Polarizing Member) A long, amorphous, isophthalic copolymerized polyethylene terephthalate film (thickness: 100 μm) with a Tg of approximately 75°C was used as the thermoplastic resin substrate. One side of the resin substrate was subjected to a corona treatment. A PVA-based resin (100 parts by weight) containing a 9:1 mixture of polyvinyl alcohol (degree of polymerization: 4200, degree of saponification: 99.2 mol%) and acetoacetyl-modified PVA (manufactured by Mitsubishi Chemical Corporation, trade name "GOHSENEX Z410") was dissolved in water to prepare an aqueous PVA solution (coating solution). The PVA aqueous solution was applied to the corona-treated surface of the resin substrate and dried at 60°C to form a 13 μm-thick PVA-based resin layer, producing a laminate. The resulting laminate was uniaxially stretched 2.4 times in the longitudinal direction (longitudinal direction) in an oven at 130°C (in-air auxiliary stretching treatment). Next, the laminate was immersed for 30 seconds in an insolubilizing bath (a boric acid aqueous solution obtained by blending 4 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C (insolubilization treatment), then immersed for 60 seconds in a dyeing bath (an iodine aqueous solution obtained by blending iodine and potassium iodide in a weight ratio of 1:7 with 100 parts by weight of water) at a liquid temperature of 30°C while adjusting the concentration so that the single-unit transmittance (Ts) of the finally obtained absorptive polarizing film would have a desired value (dyeing treatment), then immersed for 30 seconds in a crosslinking bath (a boric acid aqueous solution obtained by blending 3 parts by weight of potassium iodide and 5 parts by weight of boric acid with 100 parts by weight of water) at a liquid temperature of 40°C (crosslinking treatment). The laminate was then immersed in a boric acid aqueous solution (boric acid concentration: 4 wt %, potassium iodide concentration: 5 wt %) at a liquid temperature of 70°C and uniaxially stretched in the longitudinal direction (machine direction) between rolls operating at different peripheral speeds to a total stretch ratio of 5.5 (underwater stretching treatment). The laminate was then immersed in a cleaning bath (aqueous solution obtained by blending 4 parts by weight of potassium iodide with 100 parts by weight of water) at a liquid temperature of 20°C (washing treatment). The laminate was then dried in an oven maintained at approximately 90°C and brought into contact with a stainless steel heated roll maintained at a surface temperature of approximately 75°C (drying shrinkage treatment). The shrinkage rate of the laminate in the width direction due to the drying shrinkage treatment was 5.2%. In this manner, an absorptive polarizing film having a thickness of approximately 5 μm was formed on the resin substrate.A cycloolefin resin film (thickness: 25 μm) was attached as a protective layer to the surface of the obtained absorptive polarizing film (the surface opposite to the resin substrate) via a UV-curable adhesive. Specifically, the curable adhesive was applied so that the total thickness was approximately 1 μm, and the films were attached using a roller. The adhesive was then cured by irradiating it with UV light from the cycloolefin resin film side. The resin substrate was then peeled off. This resulted in a polarizing element having a cycloolefin resin film / absorptive polarizing film configuration. The polarizing element had a single transmittance (Ts) of 43.4% and a polarization degree of 99.993%.
[0076] (Formation of Pressure-Sensitive Adhesive Layer) A monomer mixture containing 94.9 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid, and 0.1 parts by weight of 2-hydroxyethyl acrylate was charged into a four-neck flask equipped with a stirring blade, a thermometer, a nitrogen gas inlet tube, and a condenser. Furthermore, 0.3 parts by weight of dibenzoyl peroxide as a polymerization initiator was charged together with ethyl acetate relative to 100 parts by weight of this monomer mixture. Nitrogen gas was introduced into the flask with gentle stirring to replace the atmosphere with nitrogen, and the liquid temperature in the flask was maintained at 60°C, allowing the polymerization reaction to proceed for 7 hours. Ethyl acetate was then added to the resulting reaction solution to adjust the solids concentration to 30% by weight, thereby preparing a solution of an acrylic polymer having a weight-average molecular weight (Mw) of 2,200,000. An acrylic pressure-sensitive adhesive was prepared by blending 0.6 parts by weight of a trimethylolpropane / tolylene diisocyanate adduct (trade name: Coronate L, manufactured by Tosoh Corporation) and 0.075 parts by weight of a silane coupling agent (trade name: KBM403, manufactured by Shin-Etsu Chemical Co., Ltd.) with 100 parts by weight of the solids content of the obtained acrylic polymer solution. The obtained acrylic pressure-sensitive adhesive composition was applied to a substrate film and dried to form a pressure-sensitive adhesive layer having a thickness of 12 μm and a pressure-sensitive adhesive layer having a thickness of 15 μm.
[0077] (Production Example 1A: Preparation of Surface Protection Film A) <Acrylic Polymer A> In a reaction vessel equipped with a thermometer, a stirrer, a cooler, and a nitrogen gas inlet tube, 96.2 parts by mass of 2-ethylhexyl acrylate (2EHA) and 3.8 parts by mass of hydroxyethyl acrylate (HEA) as monomer components, and 0.2 parts by mass of 2,2'-azobisisobutyronitrile (AIBN) as a polymerization initiator were charged together with 150 parts by mass of ethyl acetate, and nitrogen gas was introduced while gently stirring at 23°C to perform nitrogen substitution. Thereafter, the liquid temperature was maintained at around 65°C and a polymerization reaction was carried out for 6 hours to prepare a solution of acrylic polymer A (concentration 40% by mass). The weight-average molecular weight of acrylic polymer A was 540,000.
[0078] <Adhesive composition A> Ethyl acetate was added to a solution of acrylic polymer A to dilute it to a concentration of 20% by mass. To 500 parts by mass (solid content 100 parts by mass) of this solution, 4 parts by mass of an isocyanurate of hexamethylene diisocyanate ("Coronate HX" manufactured by Tosoh Corporation) as a crosslinking agent and 3 parts by mass (solid content 0.03 parts by mass) of dibutyltin dilaurate (1% by mass ethyl acetate solution) as a crosslinking catalyst were added and stirred to prepare a pressure-sensitive adhesive composition A.
[0079] <Surface protection film A> Pressure-sensitive adhesive composition A was applied to one side of a substrate (PET film, "CE905-38" manufactured by KOLON Corporation, thickness 38 μm) and then dried to form a pressure-sensitive adhesive layer (thickness 15 μm). Next, a release liner (manufactured by Toyobo Co., Ltd., product number TG704) was attached to the surface of the pressure-sensitive adhesive layer opposite the substrate. In this way, surface protection film A was obtained.
[0080] (Production Example 1C: Preparation of Surface Protection Film C) A surface protection film C was obtained in the same manner as in Production Example 1A, except that a PET film ("Part Number T100C38" manufactured by Mitsubishi Chemical Corporation, thickness 38 μm) was used as the substrate and pressure-sensitive adhesive composition A was applied to the corona-treated surface to form a pressure-sensitive adhesive layer having a thickness of 5 μm.
[0081] (Preparation of Laminated Film) The positive C plate was bonded to the λ / 4 member (stretched film) via a UV-curable adhesive (thickness 1 μm after curing) to obtain a retardation member. The protective member (an acrylic film having a hard coat layer and an antireflection layer formed thereon) was bonded to the positive C plate side of the obtained retardation member via the pressure-sensitive adhesive layer (thickness: 12 μm). The acrylic film of the protective member was bonded to the positive C plate side. The surface protective film A and the surface protective film C were then bonded to the antireflection layer side of the protective member in this order after peeling off the release liners. Next, the polarizing member was bonded to the λ / 4 member side of the retardation member via the pressure-sensitive adhesive layer (thickness: 12 μm). The laminations were performed such that the slow axis of the λ / 4 member and the absorption axis of the absorptive polarizing film formed an angle of 45°. The absorptive polarizing film of the polarizing member was bonded to the λ / 4 member side. The pressure-sensitive adhesive layer (thickness: 15 μm) was then attached to the cycloolefin resin film side of the polarizing member, and a release liner (manufactured by Toyobo Co., Ltd., product number TG704) was then attached to obtain a laminated film with a thickness of 330 μm.
[0082] Twenty optical film bodies measuring 50 mm long x 60 mm wide were punched out from the obtained laminated film, and these were stacked to form a workpiece as shown in Figure 2. The obtained workpiece was fixed with a clamp, and the outer peripheral surface of the workpiece was end milled as shown in Figure 2. The feed rate of the end mill was 1200 mm / min, and the rotation speed was 4500 rpm.
[0083] After cutting, a tape (acrylic adhesive tape with a substrate) with a peeling strength of 3.5 N / 25 mm was attached to the cut surface of the workpiece and then peeled off, and this operation was continued until no fuzz generated by cutting was visually observed. In this way, an optical film was obtained.
[0084] Example 2 An optical film was obtained in the same manner as in Example 1, except that the rotation speed of the end mill in cutting was set to 3000 rpm.
[0085] Example 3 An optical film was obtained in the same manner as in Example 1, except that the rotation speed of the end mill in cutting was set to 6000 rpm.
[0086] Comparative Example 1 An optical film was obtained in the same manner as in Example 1, except that after cutting, the fluff was not removed with tape.
[0087] Comparative Example 2 An optical film was obtained in the same manner as in Example 2, except that after cutting, the fluff was not removed with tape.
[0088] Comparative Example 3 An optical film was obtained in the same manner as in Example 3, except that after cutting, the fluff was not removed with tape.
[0089] An adhesive film measuring 30 mm x 30 mm and having a peeling force of 3.5 N / 25 mm was attached to the end surface of the optical film of each example and comparative example. Specifically, the adhesive film was attached to the machined surface of the workpiece while 20 sheets were still stacked. The adhesive film was then peeled from the end surface of the optical film, and the number of foreign particles adhering to the adhesive surface of the adhesive film was counted using a surface cleanliness particle monitor (PartSens manufactured by Intechnos Japan Co., Ltd.). Here, the number of foreign particles within an area of 7 mm (in the direction of stacking) x 5 mm (in the direction of stacking) in the adhesive film was counted, and the counted number was divided by the number of optical films present within the area of 7 mm (in the direction of stacking) x 5 mm (in the direction of stacking) to convert it to the amount of foreign particles per unit length of 10 mm in the direction perpendicular to the thickness direction of the end surface of the optical film. The results are summarized in Table 1.
[0090]
[0091] The present invention is not limited to the above-described embodiment, and various modifications are possible. For example, the configurations shown in the above-described embodiment can be replaced with configurations that are substantially the same as those shown in the above-described embodiment, that have the same effects, or that can achieve the same purpose.
[0092] The optical film according to the embodiment of the present invention can be used in an image display device, and can be suitably used in, for example, VR goggles.
[0093] 2 Optical film 4 Workpiece 6 Cutting section 8 Cutting blade 10 Display system 12 Display element 14 Reflective polarizing member 16 First lens section 18 Half mirror 20 First λ / 4 member 22 Second λ / 4 member 24 Second lens section
Claims
1. An optical film comprising at least one of a polarizing member or a phase difference member, wherein the number of foreign particles having a major axis exceeding 50 μm and not exceeding 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 10 or less.
2. The optical film according to claim 1, wherein the number of foreign particles having a major axis exceeding 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 3 or less.
3. The optical film according to claim 1, wherein the number of foreign particles having a major axis exceeding 100 μm and not exceeding 150 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 3 or less.
4. The optical film according to claim 1, wherein the number of foreign particles having a major axis exceeding 15 μm and not exceeding 50 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 80 or less.
5. The optical film according to claim 1, wherein the number of foreign particles having a major axis exceeding 5 μm and not exceeding 15 μm per unit length of 10 mm in a direction perpendicular to the thickness direction of the end face is 30 or less.
6. The optical film according to claim 1, wherein the foreign matter includes a component derived from a material contained in the optical film.
Citation Information
Patent Citations
Optical film and polarizing plate
JP2005164632A
Method for manufacturing sheet product, and sheet product
JP2012143918A
Foreign matter removal device
JP2020131128A
Polarizing plate and manufacturing method therefor
JP2022147184A
Endmill for cutting optical film and optical film manufacturing method using said end mill
WO2021131120A1