Resin composition, modifier, and composition containing said modifier
The resin composition, combining ethylene-vinyl acetate copolymers and styrenic block copolymers, addresses the compatibility issues in recycling composite plastics by reducing 'fish eyes' and improving film quality, enabling effective recycling of mixed plastic waste into high-quality films.
Patent Information
- Application Number
- PCT/JP2024/009700
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-13
- Publication Date
- 2024-10-03
AI Technical Summary
The recycling of composite plastics is hindered by the poor compatibility of different plastic types, leading to deteriorated physical properties and the occurrence of 'fish eyes' when forming thermoplastic resins into films, making it difficult to recycle multilayer films or containers.
A resin composition containing a blend of ethylene-vinyl acetate copolymers with varying vinyl acetate contents and a styrenic block copolymer is used as a modifier to improve compatibility and reduce 'fish eyes' in recycled films.
The resin composition effectively suppresses the occurrence of 'fish eyes' and enhances the film appearance, allowing for the production of high-quality recycled films from mixed plastic waste, suitable for various applications.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Resin composition, modifier and composition containing the modifier
[0001] The present invention relates to a resin composition containing a composition containing at least two kinds of ethylene-vinyl acetate copolymers having different vinyl acetate contents, and a styrene-based block copolymer.
[0002] In recent years, there has been growing interest in the problem of environmental pollution caused by plastics, and material recycling of plastic products has been promoted.
[0003] In the material recycling of plastics, if different types of plastics are mixed in the collected plastic waste, the physical properties of the recycled plastics will generally be reduced due to their poor compatibility with each other.
[0004] Therefore, currently, collected plastic waste is sorted by material and then recycled into products.
[0005] However, multilayer films or containers made of laminated different types of plastics (hereinafter referred to as composite plastics) cannot be recycled because it is difficult to separate them into individual materials, and they are currently landfilled or incinerated.
[0006] Against this background, the addition of compatibilizers has been investigated as a means of recycling composite plastics.
[0007] For example, Patent Document 1 shows that the physical properties of composite plastics can be improved by adding a compatibilizer to composite plastics such as polyethylene (PE) and polyethylene terephthalate (PET), or composite plastics such as polypropylene (PP) and acrylonitrile-butadiene-styrene copolymer (ABS).
[0008] However, while the present inventors were studying the recycling of composite plastics, they found that when a resin containing polyester in polyolefin was made into a film, a defect in appearance called fisheye frequently occurred.
[0009] Japanese Patent Application Publication No. 2001-220473
[0010] The present invention aims to provide a resin composition and a modifier comprising the resin composition that are effective in reducing fisheyes that occur when a thermoplastic resin containing two or more plastic components is formed into a film. Another object of the present invention is to provide a modifier that allows a recycled film with good appearance to be obtained from waste containing multiple plastics.
[0011] As a result of intensive research aimed at solving the above problems, the present inventors have found that a resin composition containing a specific ethylene-vinyl acetate copolymer and a styrene-based block copolymer has an excellent effect of reducing fisheyes that occur when a thermoplastic resin containing two or more plastic components is formed into a film, and have thus completed the present invention.
[0012] Resin composition (A), one embodiment of the present invention, contains 50 to 99 parts by mass of composition (a1) containing at least two ethylene-vinyl acetate copolymers having different vinyl acetate contents, and 1 to 50 parts by mass of styrene-based block copolymer (a2) (where the total of (a1) and (a2) is 100 parts by mass).
[0013] The resin composition of one embodiment of the present invention is effective as a modifier for thermoplastic resins containing two or more plastic components, and films of the modified thermoplastic resin have few fisheyes and excellent film appearance, making them useful for molded articles requiring these physical properties.
[0014] The present invention will be described in detail below based on preferred embodiments thereof.
[0015] <Resin Composition (A)> Resin composition (A), which is one embodiment of the present invention, contains 50 parts by mass or more and 99 parts by mass or less of composition (a1) containing at least two kinds of ethylene-vinyl acetate copolymers differing in vinyl acetate content, and 1 part by mass or more and 50 parts by mass or less of styrene-based block copolymer (a2).
[0016] Each ethylene-vinyl acetate copolymer in the composition (a1) (hereinafter referred to as "EVA composition (a1)") comprising at least two types of ethylene-vinyl acetate copolymers differing in vinyl acetate content that constitute the resin composition (A) can be obtained by a known production method. Specific production methods include high-pressure radical polymerization, solution polymerization, and emulsion polymerization. The ethylene-vinyl acetate copolymer can be conveniently selected from commercially available products, and is commercially available from Tosoh Corporation under the trade name Ultrathene and from Lanxess K.K. under the trade name Levaprene.
[0017] The vinyl acetate content of the ethylene-vinyl acetate copolymer, as measured according to JIS K6924-1, is preferably 6% by mass or more and 90% by mass or less, more preferably 15% by mass or more and 85% by mass or less. A vinyl acetate content of 6% by mass or more is preferred because it provides excellent compatibility with polyesters, while a vinyl acetate content of 90% by mass or less is preferred because it provides excellent compatibility with polyolefins.
[0018] From the viewpoint of compatibility, the EVA composition (a1) preferably contains two or more types of ethylene-vinyl acetate copolymers, more preferably three or more types. The difference in vinyl acetate content between the ethylene-vinyl acetate copolymers is preferably 1% by mass or more, more preferably 5% by mass or more. Furthermore, the difference in vinyl acetate content between at least one pair of ethylene-vinyl acetate copolymers is preferably 40% by mass or less, more preferably 20% by mass or less, and most preferably 15% by mass or less.
[0019] Here, in the EVA composition (a1), the difference in vinyl acetate content between each ethylene-vinyl acetate copolymer can be calculated as follows, for example, in a composition containing three types of ethylene-vinyl acetate copolymers with vinyl acetate contents of 25 mass%, 50 mass%, and 80 mass% (hereinafter, the vinyl acetate contents will be referred to as VAc25, VAc50, and VAc80, respectively): VAc50 - VAc25 = 25 mass%, VAc80 - VAc50 = 30 mass%, and VAc80 - VAc25 = 55 mass%.
[0020] The styrene-based block copolymer (a2) constituting the resin composition (A) may be composed of at least one polymer block mainly composed of styrene monomer units and at least one polymer block mainly composed of conjugated diene compound monomer units. The styrene-based block copolymer (a2) may also be a hydrogenated product in which the double bonds are partially saturated or completely saturated by hydrogenation.
[0021] In this specification, a polymer block mainly composed of styrene monomer units refers to a polymer block containing 50% by mass or more of monomer units derived from styrene, where the total amount of monomer units in the polymer block is 100% by mass. The content of monomer units derived from styrene contained in the polymer block mainly composed of styrene monomer units may be 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 99% by mass or more, or 100% by mass.
[0022] In this specification, a polymer block mainly composed of conjugated diene compound monomer units refers to a polymer block containing 50% by mass or more of monomer units derived from a conjugated diene compound, where the total amount of monomer units in the polymer block is 100% by mass. The content of the monomer units derived from a conjugated diene compound contained in the polymer block mainly composed of conjugated diene compound monomer units may be 60% by mass or more, 70% by mass or more, 80% by mass or more, 90% by mass or more, 95% by mass or more, 99% by mass or more, or 100% by mass.
[0023] Examples of conjugated diene compounds constituting polymer blocks mainly composed of conjugated diene compound monomer units include 1,3-butadiene, isoprene, 1,3-pentadiene, 2,3-dimethyl-1,3-butadiene, 2-methyl-1,3-pentadiene, 1,3-hexadiene, phenylbutadiene, 4,5-diethyl-1,3-octadiene, and 3-butyl-1,3-octadiene. Polymer blocks mainly composed of conjugated diene compound monomer units may be composed of one or more of these conjugated diene compounds. Furthermore, the double bonds may be partially or completely saturated by subsequent hydrogenation.
[0024] Specific examples of the styrene block copolymer (a2) include styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), styrene-ethylene-butene-styrene block copolymer (SEBS) which is a hydrogenated product of SBS, and styrene-ethylene-propylene-styrene block copolymer (SEPS) which is a hydrogenated product of SIS. Among these, styrene-ethylene-butene-styrene block copolymer (SEBS) is preferred in terms of compatibility with ethylene-vinyl acetate copolymer and polyolefin or polyester.
[0025] The proportion of the polymer block composed of styrene in the styrene-based block copolymer is preferably 10% by mass or more and 50% by mass or less, more preferably 10% by mass or more and 30% by mass or less, where 10% by mass or more is preferred because of excellent compatibility with polyesters, and 50% by mass or less is preferred because of excellent compatibility with polyolefins.
[0026] In the resin composition (A), the mixing ratio of the EVA composition (a1) to the styrene-based block copolymer (a2) is preferably 50 to 99 parts by mass of the EVA composition (a1) and 1 to 50 parts by mass of the styrene-based block copolymer (a2) (where the total of (a1) and (a2) is 100 parts by mass), or 60 to 90 parts by mass of the EVA composition (a1) and 10 to 40 parts by mass of the styrene-based block copolymer (a2) (where the total of (a1) and (a2) is 100 parts by mass). By including 50 to 99 parts by mass of the EVA composition (a1), the film appearance of the blended resin is further improved. On the other hand, by including 1 to 50 parts by mass of the styrene-based block copolymer (a2), the fisheyes of the blended resin are further reduced.
[0027] The modifier, which is one embodiment of the present invention, will be described in detail below.
[0028] <Resin Compatibilizer (Modifier)> The resin compatibilizer (hereinafter, may be referred to as "modifier"), which is one embodiment of the present invention, contains the resin composition (A).
[0029] By blending the resin composition (A) as a modifier with a base resin, the appearance of the film when the resin is molded into a film can be improved and fisheyes can be reduced.
[0030] The base material to be blended is preferably a thermoplastic resin containing at least a polyolefin and a polyester (hereinafter referred to as "thermoplastic resin (B)").
[0031] The modifier can be used in any form such as pellets or powder.
[0032] The thermoplastic resin (B) to be blended with the modifier may contain at least a polyolefin and a polyester. That is, the thermoplastic resin (B) may contain a thermoplastic resin other than a polyolefin and a polyester. Examples of the resin component other than a polyolefin and a polyester include a polyamide, an ethylene-vinyl alcohol copolymer, and polystyrene.
[0033] Examples of polyolefins include polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-acrylate copolymer, ethylene-methacrylate copolymer, etc. Examples of polyethylenes include high-density polyethylene, low-density polyethylene, and linear low-density polyethylene.
[0034] Examples of polyester include polyethylene terephthalate, glycol-modified polyethylene terephthalate (PETG resin), polybutylene terephthalate, and polylactic acid.
[0035] Examples of polyamides include nylon 6, nylon 6,6, nylon 11, and nylon 12.
[0036] Among these, the polyolefin contained in the thermoplastic resin (B) is preferably high-density polyethylene, low-density polyethylene, linear low-density polyethylene, or polypropylene because of its excellent film formability, with low-density polyethylene and linear low-density polyethylene being more preferred. As the polyester, polyethylene terephthalate is preferred because of its excellent film appearance. As the resin other than polyolefin and polyester, at least one member of the group consisting of polyamide and ethylene-vinyl alcohol copolymer is preferred.
[0037] The ratio of the resins constituting the thermoplastic resin (B) is preferably 70 parts by mass or more and 99 parts by mass or less of polyolefin and 1 part by mass or more and 30 parts by mass or less of polyester, because the strength of the film is excellent, and more preferably 80 parts by mass or more and 99 parts by mass or less of polyolefin and 1 part by mass or more and 20 parts by mass or less of polyester. When a resin other than polyolefin and polyester is contained, the ratio of the resins constituting the thermoplastic resin (B) is preferably 70 parts by mass or more and 98 parts by mass or less of polyolefin, 1 part by mass or more and 29 parts by mass or less of polyester, and 1 part by mass or more and 29 parts by mass or less of resin other than polyolefin and polyester, and more preferably 80 parts by mass or more and 98 parts by mass or less of polyolefin, 1 part by mass or more and 19 parts by mass or less of polyester, and 1 part by mass or more and 19 parts by mass or less of resin other than polyolefin and polyester.
[0038] The thermoplastic resin (B) may be a virgin resin or a resin obtained by recovering plastic waste. That is, the thermoplastic resin (B) may be a resin in which all of the one or more resins are virgin resins, a resin in which at least one of the one or more resins is a used resin, or a resin in which all of the one or more resins are used resins.
[0039] The plastic waste is not particularly limited, but may be any of burrs or film trimming waste generated in plastic molding factories, waste that cannot be used as a product, such as off-spec products, and waste from used plastic products collected from the city or consumers. In an embodiment of the present invention, a recycled resin composition is produced as the resin composition by using plastic waste as a material for the resin composition. Furthermore, when using a resin obtained by collecting plastic waste, it may contain organic substances such as PVC resin, wax, adhesive, plasticizer, and antioxidant, and / or inorganic substances such as fillers as impurities.
[0040] <Resin Composition> A resin composition containing a resin composition (A) and a thermoplastic resin (B) is also included in one aspect of the present invention. The mixing ratio of the resin composition (A) and the thermoplastic resin (B) in the resin composition is preferably 1 part by mass or more and 15 parts by mass or less, and more preferably 1 part by mass or more and 10 parts by mass or less, per 100 parts by mass of the thermoplastic resin (B). When the resin composition (A) is 1 part by mass or more, it is preferable because it has excellent effects of improving the film appearance and suppressing fisheyes, and when it is 15 parts by mass or less, it is preferable because it has excellent film formability. Specific examples and preferred aspects of the resin composition (A) and the thermoplastic resin (B) are as described above in the section <Resin Compatibilizer (Modifier)>.
[0041] The melt mass flow rate (MFR) of the resin composition containing the resin composition (A) and the thermoplastic resin (B) is not particularly limited, but in order to achieve excellent film formability, the MFR measured under conditions of 190°C and a load of 2.16 kg is preferably 0.5 g / 10 min or more and 30 g / 10 min or less, more preferably 0.8 g / 10 min or more and 20 g / 10 min or less, and most preferably 1 g / 10 min or more and 10 g / 10 min or less.
[0042] The method for producing the resin composition containing the resin composition (A) and the thermoplastic resin (B) is not particularly limited as long as it can disperse each component, and the resin composition can be produced using a commonly used resin kneading device. Examples of kneading devices include a single-screw extruder, a twin-screw extruder, a multi-screw extruder, a Banbury mixer, a pressure kneader, a rotating roll, and an internal mixer. Among these, a twin-screw extruder is preferred because of its excellent dispersibility and continuous productivity.
[0043] The screw rotation speed when kneading with a twin-screw extruder is not particularly limited, but is preferably 50 rpm to 3000 rpm, more preferably 150 rpm to 1000 rpm. A screw rotation speed of 50 rpm or more is preferable because the dispersibility of the mixed components is improved and the resulting resin has excellent physical properties, while a screw rotation speed of 3000 rpm or less is preferable because the resin does not deteriorate due to excessive shear heat generation, and the resulting resin has excellent physical properties.
[0044] The kneading temperature is preferably from the melting point of the component with the lowest melting point among the thermoplastic resins (B) to about 300°C.
[0045] Furthermore, the resin composition containing the resin composition (A) and the thermoplastic resin (B) may contain an antistatic agent, a light stabilizer, an ultraviolet absorber, a nucleating agent, an antioxidant, an antiblocking agent, a flow improver, a mold release agent, a flame retardant, a colorant, an inorganic neutralizing agent, a hydrochloric acid absorber, a filler conductive agent, a chain extender, a hydrolysis inhibitor, and the like, as long as the effects of the present invention are not impaired.
[0046] <Molded Article> The resin composition containing the resin composition (A) and the thermoplastic resin (B) can be used in any form such as pellets or powder. A molded article made of the resin composition containing the resin composition (A) and the thermoplastic resin (B) is also included in one aspect of the present invention.
[0047] The method for molding the resin composition is not particularly limited, but examples include profile extrusion, film, sheet, blow molding, injection molding, foaming, extrusion coating, and rotational molding. Among these, film is preferred because it provides excellent moldability for the resin composition, which is one embodiment of the present invention.
[0048] A film made of the resin composition is also included in one embodiment of the present invention. The film molding method is not particularly limited, and examples thereof include inflation molding, coextrusion inflation molding, T-die molding, coextrusion T-die molding, calendar molding, and compression molding. Among these, inflation molding, coextrusion inflation molding, T-die molding, and coextrusion T-die molding are preferred because of their excellent productivity. Furthermore, the film according to one embodiment of the present invention may be laminated with other films, and the lamination method is also not particularly limited, and examples thereof include dry lamination, extrusion lamination, and sandwich lamination.
[0049] The resin composition containing the resin composition (A) and the thermoplastic resin (B) of this embodiment described above can suppress the occurrence of fisheyes when formed into a film. Fisheyes are particulate aggregates resembling fisheyes that are caused by foreign matter (such as unmelted material) that occurs in the film.
[0050] A film according to one embodiment of the present invention can be obtained by forming the resin composition into a film (molding it into a film shape). The film made of the resin composition may be a single layer or a multilayer film. The layer structure of the multilayer film is not particularly limited, but may include, for example, not only the layer (I) of the resin composition according to one embodiment of the present invention but also layers made of other components, such as a virgin resin layer (II), an adhesive layer (III), or a barrier layer (IV). Specific examples include layer (I) / layer (II), layer (II) / layer (I) / layer (II), layer (I) / layer (III) / layer (IV) / layer (III) / layer (I), and layer (I) / layer (III) / layer (IV) / layer (III) / layer (II). The " / " between layers indicates that the layers are adjacent. The thickness of the film made of the resin composition is not particularly limited, but is preferably 10 μm to 300 μm from the viewpoint of further suppressing the occurrence of fisheyes.
[0051] The film forming temperature is preferably in the range of 190° C. or higher and 250° C. or lower, more preferably in the range of 200° C. or higher and 250° C. or lower, and even more preferably in the range of 220° C. or higher and 250° C. A forming temperature of 190° C. or higher reduces the occurrence of fish eyes, and a forming temperature of 250° C. or lower is preferred because it provides excellent film formability.
[0052] The films are useful as packaging containers for food, daily necessities, industrial parts, pharmaceuticals, office supplies, chemical supplies, etc., surface protection films, agricultural films such as silage wrap, shrink films, transport bags, etc.
[0053] [Summary] That is, each aspect of the present invention is the following [1] to
[15] . [1] Resin composition (A) containing 50 to 99 parts by mass of composition (a1) containing at least two kinds of ethylene-vinyl acetate copolymers differing in vinyl acetate content, and 1 to 50 parts by mass of a styrene-based block copolymer (a2) (wherein the total of (a1) and (a2) is 100 parts by mass). [2] Resin composition (A) according to [1], wherein each ethylene-vinyl acetate copolymer contained in composition (a1) containing an ethylene-vinyl acetate copolymer has a vinyl acetate content of 6 to 90% by mass. [3] Resin composition (A) according to [1] or [2], wherein composition (a1) containing an ethylene-vinyl acetate copolymer contains three or more kinds of ethylene-vinyl acetate copolymers differing in vinyl acetate content. [4] Resin composition (A) according to any one of [1] to [3], wherein in the ethylene-vinyl acetate copolymer composition (a1), the difference in vinyl acetate content between each ethylene-vinyl acetate copolymer is 1% by mass or more, and further, the difference in vinyl acetate content between at least one pair of ethylene-vinyl acetate copolymers is 40% by mass or less. [5] Resin composition (A) according to any one of [1] to [4], wherein the styrene-based block copolymer (a2) is a block copolymer having at least one polymer block mainly composed of styrene monomer units and at least one polymer block mainly composed of conjugated diene compound monomer units, or a hydrogenated product thereof. [6] Resin composition (A) according to any one of [1] to [5], wherein the styrene-based block copolymer (a2) is a styrene-butadiene-styrene block copolymer (SBS), a styrene-isoprene-styrene block copolymer (SIS), or a hydrogenated product thereof. [7] The resin composition (A) according to any one of [1] to [6], wherein the styrene-based block copolymer (a2) is a styrene-ethylene-butylene-styrene block copolymer (SEBS). [8] The resin composition (A) according to [7], wherein the styrene block ratio of the styrene-ethylene-butylene-styrene block copolymer (SEBS) is 10% by mass or more and 50% by mass or less. [9] A resin compatibilizer comprising the resin composition (A) according to any one of [1] to [8].
[10] A resin composition comprising the resin composition (A) according to any one of [1] to [8] and a thermoplastic resin (B) containing a polyolefin and a polyester, the resin composition (A) being contained in an amount of 1 part by mass to 15 parts by mass per 100 parts by mass of the thermoplastic resin (B).
[11] The resin composition according to
[10] , wherein the polyester is polyethylene terephthalate.
[12] The resin composition according to
[10] or
[11] , wherein the resin contained in the thermoplastic resin (B) is a resin obtained by recovering plastic waste.
[13] A molded article comprising the resin composition according to any one of
[10] to
[12] .
[14] A film comprising the resin composition according to any one of
[10] to
[12] .
[15] A packaging container comprising the film according to
[14] .
[0054] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these.
[0055] [Evaluation Methods] (1) Melt Mass Flow Rate (MFR) The MFR of the resin composition, ethylene-vinyl acetate copolymer, was measured using a melt indexer (manufactured by Takara Kogyo Co., Ltd.) under conditions of 190° C. and a load of 2.16 kg.
[0056] (2) Number of fisheyes per 500 cm of the film 2 The number of fish eyes per unit area was counted visually.
[0057] (3) Total Light Transmittance As an index of film transparency, the total light transmittance was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., Model NDH7000).
[0058] (4) Surface Smoothness of Film The surface smoothness of the film was evaluated visually. Films with little surface roughness were marked with a circle, and films with great surface roughness were marked with an x.
[0059] Example 1 A resin composition having the following composition was used as the resin composition (A).
[0060] (Resin composition (A)) 2 parts by mass of an ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Tosoh Corporation, trade name Ultrathene 640); 1 part by mass of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 500); 1 part by mass of an ethylene-vinyl acetate copolymer (a1-80) having a vinyl acetate content of 80% by mass and a melt mass flow rate of 5.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 800); 1 part by mass of a styrene-ethylene butylene-styrene block copolymer (a2-13) (manufactured by KRATON, styrene content 13% by mass, trade name G1657VS).
[0061] The resin compositions were dry-blended and melt-kneaded using a twin-screw extruder (manufactured by Technovel, trade name ULTnano25TW) having a screw diameter of 25 mm at a resin temperature of 160°C and a screw rotation speed of 150 rpm to obtain pellets of resin composition (A).
[0062] The following resins were used as the thermoplastic resin (B) containing at least polyolefin and polyester.
[0063] (Thermoplastic resin (B)) Linear low-density polyethylene (manufactured by Tosoh, MFR 2.0 g / 10 min, trade name Nipolon Z HF210K) 90 parts by mass Polyethylene terephthalate (manufactured by Unitika, trade name MA-2103) 10 parts by mass
[0064] The above resins were dry blended to obtain a thermoplastic resin (B).
[0065] Five parts by mass of the resin composition (A) and 100 parts by mass of the thermoplastic resin (B) were pre-blended in a tumbler mixer. Next, using a twin-screw extruder (manufactured by Technovel, product name ULTnano25TW) with a screw diameter of 25 mm, the mixture was melt-mixed at a resin temperature of 260 ° C and a screw rotation speed of 300 rpm. After melt mixing, the mixture was cooled to room temperature to obtain resin composition pellets (molten mixture). The MFR of the resin composition was 3.0 g / 10 min.
[0066] A single layer film made of the resin composition pellets was obtained using a microcast molding machine (manufactured by Labtech Engineering).
[0067] At this time, the molding temperature was 200° C., the take-up speed was 2 m / min, the film width was 50 mm, and the total film thickness was 50 μm.
[0068] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0069] Example 2 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following composition was used as the resin composition (A). The resin composition had an MFR of 3.0 g / 10 min.
[0070] (Resin composition (A)) 2 parts by mass of an ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Tosoh Corporation, trade name Ultrathene 640); 1 part by mass of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 500); 1 part by mass of an ethylene-vinyl acetate copolymer (a1-80) having a vinyl acetate content of 80% by mass and a melt mass flow rate of 5.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 800); 1 part by mass of a styrene-ethylene butylene-styrene block copolymer (a2-30) (manufactured by KRATON, styrene content 30% by mass, trade name G1726MS).
[0071] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0072] Example 3 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following composition was used as the resin composition (A). The resin composition had an MFR of 3.0 g / 10 min. (Resin composition (A)) 1.5 parts by mass of an ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Tosoh Corporation, trade name Ultrathene 640); 0.75 parts by mass of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 500); 0.75 parts by mass of an ethylene-vinyl acetate copolymer (a1-80) having a vinyl acetate content of 80% by mass and a melt mass flow rate of 5.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 800); 2 parts by mass of a styrene-ethylene butylene-styrene block copolymer (a2-30) (manufactured by KRATON, styrene content 30% by mass, trade name G1726MS).
[0073] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0074] Comparative Example 1 A single-layer film was obtained in the same manner as in Example 1, except that 100 parts by mass of a composite resin prepared by dry blending 90 parts by mass of linear low-density polyethylene (manufactured by Tosoh Corporation, MFR 2.0 g / 10 min, product name Nipolon Z HF210K) and 10 parts by mass of polyethylene terephthalate (manufactured by Unitika Corporation, product name MA-2103) was used as the thermoplastic resin (B) containing at least polyolefin and polyester. The MFR of the resin composition was 3.0 g / 10 min.
[0075] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0076] Comparative Example 2 A single-layer film was obtained in the same manner as in Example 1, except that the resin composition (A) had the following composition. The MFR of the resin composition was 3.0 g / 10 min. (Resin composition (A)) 5 parts by mass of ethylene-vinyl acetate copolymer (a1-25) (manufactured by Tosoh Corporation, trade name Ultrathene 640) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min.
[0077] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0078] Comparative Example 3 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following formulation was used as the resin composition (A). The resin composition had an MFR of 3.0 g / 10 min.
[0079] (Resin composition (A)) 2.5 parts by mass of an ethylene-vinyl acetate copolymer (a1-25) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Tosoh Corporation, trade name Ultrathene 640); 1.25 parts by mass of an ethylene-vinyl acetate copolymer (a1-50) having a vinyl acetate content of 50% by mass and a melt mass flow rate of 3.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 500); 1.25 parts by mass of an ethylene-vinyl acetate copolymer (a1-80) having a vinyl acetate content of 80% by mass and a melt mass flow rate of 5.0 g / 10 min (manufactured by Lanxess KK, trade name Levaprene 800).
[0080] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0081] Comparative Example 4 A monolayer film was obtained in the same manner as in Example 1, except that the resin composition (A) had the following composition. The MFR of the resin composition was 3.0 g / 10 min. (Resin composition (A)) Styrene-ethylene-butylene-styrene block copolymer (a2-13) (manufactured by KRATON, styrene content 13% by mass, product name G1657VS) 5 parts by mass
[0082] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0083] Comparative Example 5 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following composition was used as the resin composition (A). The resin composition had an MFR of 3.0 g / 10 min.
[0084] (Resin composition (A)) Styrene-ethylene-butylene-styrene block copolymer (a2-30) (manufactured by KRATON, styrene content 30% by mass, product name G1726MS) 5 parts by mass
[0085] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0086] Comparative Example 6 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following composition was used as the resin composition (A). The MFR of the resin composition was 3.0 g / 10 min.
[0087] (Resin composition (A)) 4 parts by mass of ethylene-vinyl acetate copolymer (a1-25) (manufactured by Tosoh Corporation, trade name Ultrathene 640) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min; 1 part by mass of styrene-ethylene-butylene-styrene block copolymer (a2-13) (manufactured by KRATON, styrene content 13% by mass, trade name G1657VS).
[0088] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0089] Comparative Example 7 A single-layer film was obtained in the same manner as in Example 1, except that a resin composition having the following formulation was used as the resin composition (A). The resin composition had an MFR of 3.0 g / 10 min.
[0090] (Resin composition (A)) 4 parts by mass of ethylene-vinyl acetate copolymer (a1-25) (manufactured by Tosoh Corporation, trade name Ultrathene 640) having a vinyl acetate content of 25% by mass and a melt mass flow rate of 3.0 g / 10 min; 1 part by mass of styrene-ethylene-butylene-styrene block copolymer (a2-30) (manufactured by KRATON, styrene content of 30% by mass, trade name G1726MS).
[0091] The number of fisheyes generated in the obtained film, the total light transmittance, and the film surface smoothness were measured by the above-mentioned evaluation methods. The evaluation results are shown in Table 1.
[0092]
[0093] As shown in Table 1, the number of fisheyes in the films of Examples 1 to 3 was two or less, confirming that the occurrence of fisheyes was suppressed. In addition, it was confirmed that the surface smoothness was good and the film appearance was excellent.
[0094] Films made from the resin composition of the present invention are useful as packaging containers for foods, daily necessities, industrial parts, pharmaceuticals, office supplies, chemical supplies, etc., surface protection films, agricultural films such as silage wrap, shrink films, transport bags, etc.
Claims
1. Resin composition (A) comprising 50 parts by mass or more and 99 parts by mass or less of composition (a1) containing at least two kinds of ethylene-vinyl acetate copolymers having different vinyl acetate contents, and 1 part by mass or more and 50 parts by mass or less of a styrene-based block copolymer (a2) (the total of (a1) and (a2) being 100 parts by mass).
2. The resin composition (A) according to claim 1, wherein the vinyl acetate content of each ethylene-vinyl acetate copolymer contained in the composition (a1) containing an ethylene-vinyl acetate copolymer is 6% by mass or more and 90% by mass or less.
3. The resin composition (A) according to claim 1, wherein the composition (a1) containing an ethylene-vinyl acetate copolymer contains three or more types of ethylene-vinyl acetate copolymers having different vinyl acetate contents.
4. The resin composition (A) according to claim 1, wherein in the ethylene-vinyl acetate copolymer composition (a1), the difference in the vinyl acetate content of each ethylene-vinyl acetate copolymer is 1% by mass or more, and further the difference in the vinyl acetate content of at least one pair of ethylene-vinyl acetate copolymers is 40% by mass or less.
5. The resin composition (A) according to claim 1, wherein the styrene-based block copolymer (a2) is a block copolymer having at least one polymer block mainly composed of styrene monomer units and at least one polymer block mainly composed of conjugated diene compound monomer units, or a hydrogenated product thereof.
6. The resin composition (A) according to claim 1, wherein the styrene-based block copolymer (a2) is a styrene-butadiene-styrene block copolymer (SBS), a styrene-isoprene-styrene block copolymer (SIS) or a hydrogenated product thereof.
7. The resin composition (A) according to claim 1, wherein the styrene-based block copolymer (a2) is a styrene-ethylene-butylene-styrene block copolymer (SEBS).
8. The resin composition (A) according to claim 7, wherein the styrene block ratio of the styrene-ethylene-butylene-styrene block copolymer (SEBS) is from 10% by mass to 50% by mass.
9. A resin compatibilizer comprising the resin composition (A) according to any one of claims 1 to 8.
10. A resin composition comprising the resin composition (A) according to claim 1 and a thermoplastic resin (B) containing a polyolefin and a polyester, the resin composition (A) being contained in an amount of 1 part by mass or more and 15 parts by mass or less per 100 parts by mass of the thermoplastic resin (B).
11. The resin composition according to claim 10, wherein the polyester is polyethylene terephthalate.
12. The resin composition according to claim 10, wherein the resin contained in the thermoplastic resin (B) is a resin obtained by recovering plastic waste.
13. A molded article made of the resin composition according to any one of claims 10 to 12.
14. A film made of the resin composition according to any one of claims 10 to 12.
15. A packaging container comprising the film according to claim 14.
Citation Information
Patent Citations
Thermoplastic polyester resin
JP1986043656A
Thermoplastic resin composition
JP1987187758A
Soft polyolefinic resin laminated sheet
JP2002273841A
Resin composition for coating and insulated wire produced by using the same
JP2006089603A