Method for producing cured film

The method for manufacturing light-shielding films, utilizing specific resin combinations and heat treatment, improves antireflection properties and alignment, overcoming previous challenges in film production.

WO2024203335A1PCT designated stage expired Publication Date: 2024-10-03FUJIFILM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/009782
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-13
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing light-shielding films, such as those used in liquid crystal display devices and solid-state image sensors, face challenges in achieving easy mask alignment during exposure and insufficient antireflection properties in the resulting cured films.

Method used

A method involving the formation of a curable composition layer on a support, alignment with an exposure mask, exposure, development, and subsequent heat treatment, using specific resin combinations with controlled Hansen Solubility Parameters (HSP) and polymerizable compounds to create a phase-separated structure that enhances antireflection properties while allowing easy mask positioning.

Benefits of technology

The method enables the production of cured films with excellent antireflection properties and facilitates easy mask alignment during exposure, addressing the limitations of previous techniques.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
  • Figure JPOXMLDOC01-APPB-C000004
    Figure JPOXMLDOC01-APPB-C000004
Patent Text Reader

Abstract

The present invention provides a method for producing a cured film, with which it is possible to easily position a mask during exposure, and with which it is possible to obtain a cured film having excellent antireflection characteristics. This method for producing a cured film comprises: a step 1 for forming a curable composition layer on a support; a step 2 for aligning the support with an exposure mask; a step 3 for exposing the curable composition layer to light via the exposure mask; a step 4 for forming a patterned cured film by developing the exposed curable composition layer; and a step 5 for heat-treating said patterned cured film. The curable composition contains a resin A, a resin B, and a polymerizable compound. The HSP distance between the resin A and the resin B is greater than 1.5 MPa1 / 2. The HSP distance (A) between the resin A and the polymerizable compound is greater than the HSP distance (B) between the resin B and the polymerizable compound.
Need to check novelty before this filing date? Find Prior Art

Description

Method for producing cured film

[0001] The present invention relates to a method for producing a cured film.

[0002] Image display devices such as liquid crystal display devices, and solid-state imaging devices such as charge-coupled device (CCD) image sensors and complementary metal-oxide semiconductor (CMOS) image sensors often have color filters and light-shielding films arranged at predetermined positions. For example, in liquid crystal display devices, a light-shielding film called a black matrix may be arranged between colored pixels on a color filter in order to block light between the colored pixels and improve contrast. In addition, in solid-state imaging devices, a light-shielding film may be used to prevent noise generation and improve image quality.

[0003] Patent Document 1 discloses that a light-shielding film can be formed from a composition containing predetermined components such as inorganic particles.

[0004] JP 2011-145663 A

[0005] One method for forming a patterned light-shielding film involves forming a layer of a resist composition on a support such as a substrate, exposing the layer to light through an exposure mask, and then developing the layer. Here, the exposure process requires an operation called alignment, in which the exposure mask is aligned with a reference position on the support. Another characteristic required of a light-shielding film is excellent anti-reflection properties (low reflectivity). The present inventors attempted to form a light-shielding film using the composition described in Patent Document 1, and found that while alignment of the exposure mask using an alignment mark or the like was possible, the anti-reflection properties (low reflectivity) of the resulting cured film were insufficient. On the other hand, when attempting to form irregularities on the surface in order to improve the anti-reflection properties of the cured film, irregularities were formed on the surface even in the coating film state before curing, resulting in the problem of difficulty in aligning the exposure mask.

[0006] Therefore, an object of the present invention is to provide a method for producing a cured film that allows easy positioning of a mask during exposure and provides the resulting cured film with excellent anti-reflection properties.

[0007] As a result of extensive research into solving the above problems, the present inventors have found that the problems can be solved by the following configuration.

[0008] [1] A method for producing a cured film, comprising: Step 1 of forming a curable composition layer on a support; Step 2 of aligning the support with an exposure mask; Step 3 of exposing the curable composition layer through the exposure mask; Step 4 of developing the exposed curable composition layer to form a patterned cured film; and Step 5 of heat treating the patterned cured film, wherein the curable composition contains a resin A, a resin B, and a polymerizable compound, and the HSP distance between the resin A and the resin B is 1.5 MPa. 1/2and the HSP distance (A) between the resin A and the polymerizable compound is greater than the HSP distance (B) between the resin B and the polymerizable compound. [2] The method for producing a cured film according to [1], wherein the glass transition temperature of at least one of the resin A and the resin B is lower by 120°C or more than the heating temperature during the heat treatment. [3] The method for producing a cured film according to [1] or [2], wherein the glass transition temperature of the resin B is 0 to 70°C. [4] The method for producing a cured film according to any one of [1] to [3], wherein the resin A comprises a repeating unit A1 having an acid group and a repeating unit A2 having at least one of a polyoxyalkylene group having an average addition number of 3 or more and a polyoxyalkylenecarbonyl group having an average addition number of 3 or more, the content of the repeating unit A2 being 35% by mass or more relative to all repeating units of the resin A, and the resin B comprises a repeating unit B1 derived from a monomer selected from the group consisting of an alkyl acrylate and an alkyl methacrylate, a repeating unit B2 having a hydroxyl group, and a repeating unit B3 having a carboxylic acid group, the content of the repeating unit B1 being 60% by mass or more relative to all repeating units of the resin B. [5] The method for producing a cured film according to any one of [1] to [4], wherein the acid value of the resin A is 50 mgKOH / g or more. [6] The method for producing a cured film according to any one of [1] to [5], wherein the shrinkage percentage of the polymerizable compound defined by formula (X) is 7% or more. (1-ρM / ρP)×100 Formula (X) In formula (X), ρM represents the specific gravity of the polymerizable compound measured in accordance with JIS-K-2249. ρP represents the specific gravity of a cured product of the polymerizable compound measured in accordance with JIS-K-2249. [7] The method for producing a cured film according to any one of [1] to [6], wherein the curable composition further contains a colorant. [8] The method for producing a cured film according to [7], wherein the colorant contains a black colorant. [9] The method for producing a cured film according to [8], wherein the black colorant contains a black organic pigment.

[10] A method for producing a cured film, comprising: Step 11: forming a curable composition layer on a support; Step 12: aligning the support with an exposure mask; Step 13: exposing the curable composition layer through the exposure mask; and Step 14: developing the exposed curable composition layer to form a patterned cured film, wherein the curable composition contains a resin C, a resin H, and a polymerizable compound, and the HSP distance between the resin C and the resin H is 1.5 MPa. 1/2

[11] The method for producing a cured film according to

[10] , wherein the ratio T2 / T1 of the dissolution rate T2 of the resin H in the developer used in the development treatment to the dissolution rate T1 of the resin C in the developer is 10.0 or more.

[12] The method for producing a cured film according to

[10] , wherein the resin C comprises a repeating unit C1 having an acid group and a repeating unit C2 having at least one group selected from a polyoxyalkylene group having an average addition number of 3 or more and a polyoxyalkylenecarbonyl group having an average addition number of 3 or more, the content of the repeating unit C2 being 35 mass% or more with respect to all repeating units of the resin C, the resin H being an acrylic resin or a methacrylic resin, and the acid value of the resin H is higher than the acid value of the resin C by 70 mgKOH / g or more.

[13] The method for producing a cured film according to

[10] or

[12] , wherein the acid value of the resin C is 50 mgKOH / g or more.

[13] The method for producing a cured film according to any one of

[10] to

[12] , wherein the acid value of the resin H is 140 mgKOH / g or more.

[14] The method for producing a cured film according to any one of

[10] to

[13] , wherein the curable composition further contains a colorant.

[15] The method for producing a cured film according to

[14] , wherein the colorant contains a black colorant.

[16] The method for producing a cured film according to

[15] , wherein the black colorant contains a black organic pigment.

[0009] According to the present invention, a method for producing a cured film can be provided which allows for easy positioning of a mask during exposure and provides the resulting cured film with excellent antireflection properties.

[0010] 1 is a schematic plan view showing an example of the configuration of an alignment mark, and FIG. 2 is a schematic cross-sectional view taken along line AA in FIG.

[0011] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0012] The following describes the meaning of each description in this specification. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​written before and after "to" as the lower and upper limits. The compounds described in this specification may contain structural isomers, optical isomers, and isotopes, unless otherwise specified. Furthermore, structural isomers, optical isomers, and isotopes may be contained singly or in combination of two or more types. In this specification, unless otherwise specified, the bonding direction of a divalent group (e.g., -COO-) may be either "X-O-CO-Z" or "X-CO-O-Z" when Y in a compound represented by "X-Y-Z" is -COO-. Furthermore, in the description of groups (atomic groups) in this specification, descriptions that do not specify whether they are substituted or unsubstituted include both groups that do not contain a substituent and groups that contain a substituent. For example, an "alkyl group" includes not only alkyl groups that do not contain a substituent (unsubstituted alkyl groups), but also alkyl groups that contain a substituent (substituted alkyl groups).

[0013] In addition, in this specification, "actinic rays" or "radiation" refers to, for example, far ultraviolet rays, extreme ultraviolet rays (EUV: extreme ultraviolet lithography), X-rays, electron beams, etc. In addition, in this specification, "light" refers to actinic rays and radiation. Unless otherwise specified, in this specification, "exposure" includes not only exposure with far ultraviolet rays, X-rays, EUV light, etc., but also writing with particle beams such as electron beams and ion beams.

[0014] In addition, in this specification, "(meth)acrylate" represents acrylate and methacrylate. In addition, in this specification, "(meth)acryl" represents acrylic and methacryl. In addition, in this specification, "(meth)acryloyl" represents acryloyl and methacryloyl. In addition, in this specification, "(meth)acrylamide" represents acrylamide and methacrylamide. In addition, in this specification, "monomer" and "monomer" have the same meaning.

[0015] In this specification, the weight average molecular weight (Mw) is a polystyrene-equivalent value determined by gel permeation chromatography (GPC). The GPC method used in this specification is based on a method using an HLC-8020GPC (manufactured by Tosoh Corporation), TSKgel Super HZM-H, TSKgel Super HZ4000, or TSKgel Super HZ2000 (manufactured by Tosoh Corporation, 4.6 mm ID x 15 cm) as columns, and THF (tetrahydrofuran) as an eluent.

[0016] In this specification, the "acid value" can be calculated, for example, from the average content of acid groups in the compound.

[0017] In this specification, the solid content of a composition means a composition layer formed using the composition, and when the composition contains a solvent, means all components excluding the solvent. Furthermore, liquid components are also considered to be solids as long as they form a composition layer.

[0018] The method for producing a cured film of the present invention will be described in detail below. A first embodiment of the method for producing a cured film of the present invention (hereinafter also referred to as "the present production method") is a method for producing a cured film, comprising: step 1 of forming a curable composition layer on a support; step 2 of aligning the support with an exposure mask; step 3 of exposing the curable composition layer to light through the exposure mask; step 4 of developing the exposed curable composition layer to form a patterned cured film; and step 5 of heat treating the patterned cured film, wherein the curable composition contains resin A, resin B, and a polymerizable compound, and the HSP distance between resin A and resin B is 1.5 MPa. 1/2and the HSP distance (A) between the resin A and the polymerizable compound is greater than the HSP distance (B) between the resin B and the polymerizable compound.

[0019] A second embodiment of the method for producing a cured film of the present invention is a method for producing a cured film, comprising: step 11 of forming a curable composition layer on a support; step 12 of aligning the support with an exposure mask; step 13 of exposing the curable composition layer through the exposure mask; and step 14 of developing the exposed curable composition layer to form a patterned cured film, wherein the curable composition contains resin C, resin H, and a polymerizable compound, and the HSP distance between resin C and resin H is 1.5 MPa. 1/2 and the ratio T2 / T1 of the dissolution rate T2 of the resin H in the developer used in the development treatment to the dissolution rate T1 of the resin C in the developer is 10.0 or more.

[0020] The mechanism by which the above-described configuration of the cured film production method of the present invention (first embodiment or second embodiment) can solve the problems of the present invention is not necessarily clear, but the inventors speculate as follows. Note that the following speculation does not limit the mechanism by which the effects are obtained. In other words, even if the effects are obtained by a mechanism other than the one described below, it is still included in the scope of the present invention.

[0021] The curable composition used in the first embodiment has an HSP distance between resin A and resin B of 1.5 MPa. 1/2 The HSP distance (A) between the resin A and the polymerizable compound is greater than the HSP distance (B) between the resin B and the polymerizable compound. 1/2exceeding 1 / 200, the difference in compatibility between resin A and resin B results in a phase-separated structure (e.g., a sea-island structure, a cocontinuous structure, and a structure in which a sea-island structure and a cocontinuous structure coexist) in the curable composition layer, and a fine uneven structure can be formed on the cured film by the heat treatment in step 5. Furthermore, it is presumed that the affinity between resin B and the polymerizable compound is higher than the affinity between resin A and the polymerizable compound because the HSP distance (A) between resin A and the polymerizable compound is greater than the HSP distance (B) between resin B and the polymerizable compound. As a result, the polymerizable compound is more likely to be locally present in the sea portion or island portion in the curable composition layer, and the uneven structure can be more effectively formed by the cure shrinkage of the polymerizable compound in step 5, further enhancing the low reflectivity of the cured film. Here, the uneven structure based on the above-described phase-separated structure is not manifested in the alignment in step 2 and does not interfere with the visibility of alignment marks, etc., and therefore mask positioning during exposure can be easily performed.

[0022] Further, the curable composition used in the second embodiment, like the first embodiment, is characterized in that in addition to the characteristic feature of the HSP distance between resin C and resin H, the ratio T2 / T1 of the dissolution rate T2 of resin H in the developer used in the development process to the dissolution rate T1 of resin C in the developer is 10.0 or more. As above, due to the difference in compatibility between resin C and resin H, a phase separation structure occurs in the curable composition layer. In the above structure, during the development process in step 14, the large T2 / T1 ratio makes it easier for resin H to be developed relative to resin C, making it easier to form a fine uneven structure in the cured film, and a cured film with excellent low reflectivity can be obtained. In the second embodiment, the above-mentioned uneven structure is not expressed in the alignment of step 12 and does not interfere with the visibility of alignment marks, etc., so that the positioning of the mask during exposure can also be easily performed. Hereinafter, the achievement of at least one of the effects of facilitating alignment of the support and the exposure mask during exposure and of excellent antireflection properties (low reflectivity) of the cured film after carrying out all the steps of the present production method is also referred to as "the effects of the present invention are superior." Hereinafter, a first embodiment of the method for producing a cured film of the present invention (hereinafter also referred to as "the present production method") will be described in detail.

[0023] [[Method for Producing Cured Film (First Embodiment)]] The first embodiment of the present production method includes steps 1 to 5. Each step will be described in detail below.

[0024] [Step 1] The curable composition used in Step 1 (hereinafter also referred to as "curable composition 1") and the procedure will be described in detail below.

[0025] [Curable composition 1] Curable composition 1 contains resin A, resin B, and a polymerizable compound. The HSP distance between resin A and resin B is 1.5 MPa. 1/2 and the HSP distance (A) between the resin A and the polymerizable compound is greater than the HSP distance (B) between the resin B and the polymerizable compound.

[0026] Hansen's solubility parameter (HSP) is the dispersion term (δ d ), polar term (δ p ), and the hydrogen bond term (δ h ) is a type of solubility parameter expressed by the three components of HSP. The HSP distance is the distance between a point (δ d , δ p , δ h ) is a parameter that corresponds to the distance between the coordinates of two different substances. The smaller the HSP distance, the higher the affinity between the two substances.

[0027] The HSP distance between resin A and resin B is 1.5 MPa 1/2 exceeding 1 / 2, a phase-separated structure (e.g., a sea-island structure, a cocontinuous structure, and a structure in which a sea-island structure and a cocontinuous structure coexist) occurs in the curable composition layer due to the difference in compatibility between resin A and resin B, and a fine uneven structure can be formed on the cured film in step 5 described below, resulting in a cured film with excellent low reflectivity. Furthermore, it is presumed that the affinity between resin B and the polymerizable compound is higher than the affinity between resin A and the polymerizable compound because the HSP distance (A) between resin A and the polymerizable compound is longer than the HSP distance (B) between resin B and the polymerizable compound. As a result, the polymerizable compound is likely to be locally present in the sea portion or island portion in the curable composition layer, and the uneven structure can be more effectively formed by the cure shrinkage of the polymerizable compound, further improving the low reflectivity of the cured film.

[0028] The HSP of the first substance is δ d1 , δ p1 , δ h1 and the HSP of the second substance is δ d2 , δ p2 , δ h2 In this case, the HSP distance between the first substance and the second substance can be calculated by equation (2).

[0029]

[0030] Here, the HSP value at 25°C can be calculated unambiguously from the chemical structure of the components using computer software Hansen Solubility Parameter in Practice (HSPiP) (http: / / www.hansen-solubility.com). In the present invention, the dispersion term (δ) of each component at 25°C is calculated using HSPiP ver. 5.4.08 (sold by Eizou Kobo Question Co., Ltd.). d ), polar term (δ p ), and the hydrogen bond term (δ h ) values ​​were calculated, and the HSP distance between each of the above components was calculated.

[0031] The Hansen solubility parameters of resin A and resin B are calculated based on the repeating units of each resin. Specifically, the dispersion term (δ d ), polar term (δ p ), and the hydrogen bond term (δ h ) are calculated, and each of these components is multiplied by the mass fraction of each repeating unit and the sum is calculated to obtain the dispersion term (δ d ), polar term (δ p ), and the hydrogen bond term (δ h For example, when a resin has n kinds of repeating units, the hydrogen bond parameter (δ) of the jth repeating unit (j is an integer of 1 or more) of the resin is calculated. h ) and the mass fraction Nj of the j-th repeating unit relative to all repeating units, the hydrogen bond term (δ h ) can be calculated. h) = ΣδPjNj (H) More specifically, for example, if the resin has a hydrogen bond term of 4.0 MPa 1/2 The first repeating unit is 1/2 In this case, the hydrogen bond term of the resin is 4.0×0.3+7.0×0.7=6.1 MPa. 1/2 In the above calculation, the hydrogen bond term (δ h ), but the dispersion term of the resin (δ d ) and polarity term (δ p The dispersion term (δ) of each repeating unit can be calculated in the same manner. d ), polar term (δ p ), and the hydrogen bond term (δ h In calculating the dispersion term (δ), the value calculated by the above-mentioned method for a compound in which the terminal of each repeating unit structure is substituted with a hydrogen atom can be used. Specifically, for example, the dispersion term (δ) of a repeating unit derived from methyl methacrylate can be calculated by the following method. d ), polar term (δ p ), and the hydrogen bond term (δ h ) is the dispersion term of methyl propionate (δ d ), polar term (δ p ), and the hydrogen bond term (δ h ) can be used.

[0032] <Resin A> The curable composition 1 contains a resin A. The resin A is not particularly limited as long as it satisfies the above-mentioned relationship of HSP distance with the resin B and the polymerizable compound. Examples of the resin A include a (meth)acrylic resin, an ester resin, an olefin resin, and a urethane resin. Among them, the resin A preferably contains a repeating unit A1 having an acid group and at least one of a repeating unit A2 having at least one group selected from a polyoxyalkylene group having an average addition number of 3 or more and a polyoxyalkylenecarbonyl group having an average addition number of 3 or more, and more preferably contains both the repeating unit A1 and the repeating unit A2.

[0033] Repeating Unit A1 The repeating unit A1 functions as a pigment adsorptive group and can further improve the developability of the resin A in an alkaline developer. Examples of the acid group include a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group, and among these, a carboxylic acid group is preferable. The number of acid groups in the repeating unit A1 may be one or more, and may be, for example, one to six.

[0034] The specific structure of the repeating unit A1 is not particularly limited, but is preferably a repeating unit represented by the following formula (AX1), in that the effects of the present invention are more likely to be excellent.

[0035]

[0036] In the formula, R A1 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. A1 The number of carbon atoms in the alkyl group represented by the formula (I) is preferably 1 to 3, and more preferably 1.

[0037] L A1 represents a single bond, —COO—, or —CONR A2 - represents. A2 is the above R A1 The same definition and preferred embodiments are also the same.

[0038] L A2 represents a single bond or a divalent linking group. The type of the divalent linking group is not particularly limited, and examples thereof include a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, —O—, —S—, and —SO 2 -, -NR A3Examples of the divalent aliphatic hydrocarbon group include -, -CO-, and groups formed by combining two or more of these. The divalent aliphatic hydrocarbon group may be linear, branched, or cyclic. The number of carbon atoms is preferably 1 to 20, and more preferably 1 to 10. Examples of the divalent aliphatic hydrocarbon group include alkylene groups, alkenylene groups, and alkynylene groups, and among these, alkylene groups are preferred. Examples of the divalent aromatic hydrocarbon group include those having 6 to 10 carbon atoms, such as a phenylene group. The divalent aliphatic hydrocarbon group and the divalent aromatic hydrocarbon group may further have a substituent. The substituent is not particularly limited, and may be, for example, an acid group such as a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, or a phenolic hydroxyl group. The above R A3 is the above R A1 The same definition and preferred embodiments are also the same.

[0039] Among these, the divalent linking group is preferably a group formed by combining two or more groups selected from the group consisting of an alkylene group which may have a substituent, a phenylene group which may have a substituent, -O-, and -CO-.

[0040] In the above formula (AX1), -L A1 -L A2 The number of atoms excluding hydrogen atoms in the moiety represented by - is preferably less than 40, for example.

[0041] W A1 represents an acid group. Examples of the acid group include a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group, and among these, a carboxylic acid group is preferred.

[0042] As the repeating unit A1, it is preferable to include one or more repeating units selected from the group consisting of repeating units represented by formula (A11) to formula (A14), in that the effects of the present invention are more excellent. In formula (A13), n represents the average number of repeating units added and is 1 to 2.

[0043]

[0044] Resin A may contain one type of repeating unit A1 alone or two or more types. The content of repeating unit A1 in resin A is preferably 5 to 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 40 mass %, based on the total repeating units of resin A. When two or more types of repeating unit A1 are used in combination, the total content is preferably within the above range.

[0045] -Repeating Unit A2- Resin A preferably contains a repeating unit (repeating unit A2) having a group selected from the group consisting of polyoxyalkylene groups having an average addition number of 3 or more and polyoxyalkylenecarbonyl groups having an average addition number of 3 or more. The repeating unit A2 acts to prevent re-aggregation of dispersed substances such as pigments, and is also thought to contribute to the formation of a phase-separated structure when formed into a cured film.

[0046] The oxyalkylene group refers to a group represented by -O-AL-, and the oxyalkylenecarbonyl group refers to a group represented by -O-AL-CO-, where AL represents an alkylene group. The polyoxyalkylene group refers to -(O-AL) n1 The polyoxyalkylene carbonyl group is represented by -(O-AL-CO) n2 In the polyoxyalkylene group and polyoxyalkylenecarbonyl group, a plurality of oxyalkylene groups (-O-AL-) may be the same or different.

[0047] The number of carbon atoms in the alkylene group in the oxyalkylene group and the oxyalkylenecarbonyl group (the number of carbon atoms in AL) is not particularly limited, but is preferably 2 to 10, more preferably 2 to 9, and even more preferably 2 to 7. The average addition number (n1) in the polyoxyalkylene is 3 or more, preferably 4 or more, more preferably 5 or more, even more preferably 6 or more, particularly preferably 10 or more, and most preferably 15 or more. The upper limit is preferably 100 or less, more preferably 70 or less, and even more preferably 30 or less. The average addition number (n2) in the oxyalkylenecarbonyl group is 3 or more, preferably 4 or more, more preferably 5 or more, and even more preferably 6 or more. The upper limit is preferably 100 or less, more preferably 70 or less, and even more preferably 30 or less.

[0048] In a polyoxyalkylene group having an average addition number of 3 or more, the carbon numbers of the alkylene portions of the multiple oxyalkylene groups may be the same or different. When the carbon numbers of the alkylene portions of the multiple oxyalkylene groups are different, for example, a structure containing an oxyethylene group and an oxypropylene group can be mentioned. Furthermore, in a polyoxyalkylenecarbonyl group having an average addition number of 3 or more, the carbon numbers of the alkylene portions of the multiple polyoxyalkylenecarbonyl groups may be the same or different. When the carbon numbers of the alkylene portions of the multiple oxyalkylenecarbonyl groups are different, a specific example can be a structure containing an oxyethylenecarbonyl group and an oxypropylenecarbonyl group.

[0049] The repeating unit A2 is preferably a repeating unit represented by any one of the following formulas (1) to (3), and more preferably a repeating unit represented by the following formula (1) or (3).

[0050]

[0051] In formulas (1) to (3), W 1 , W 2 , and W 3 Each independently represents an oxygen atom or NH. 1 , W 2 , and W 3In formulas (1) to (3), X is preferably an oxygen atom. 1 , X 2 , and X 3 Each of X independently represents a hydrogen atom or a monovalent organic group. 1 , X 2 , and X 3 In terms of synthesis constraints, each of the groups is preferably a hydrogen atom or an alkyl group having 1 to 12 carbon atoms, more preferably a hydrogen atom or a methyl group, and even more preferably a methyl group.

[0052] In formulas (1) to (3), Y 1 , Y 2 , and Y 3 each independently represents a divalent linking group. 1 , Y 2 , and Y 3 The structure of the divalent linking group represented by the formula (1) is not particularly limited, and specific examples include the following linking groups (Y-1) to (Y-21). In the structures shown below, A and B represent the bonding sites to the left and right terminal groups in formulas (1) to (3), respectively.

[0053]

[0054] In formulas (1) to (3), Z 1 , Z 2 , and Z 3 each independently represents a hydroxyl group, an amino group, or a monovalent organic group. The organic group is not particularly limited, but specific examples include an alkyl group, an alkoxy group, an aryloxy group, a heteroaryloxy group, an alkylthioether group, an arylthioether group, and a heteroarylthioether group. Z 1 , Z 2 , and Z 3 The alkyl group, alkoxy group, and alkyl group moiety in the alkylthioether group represented by the formula (I) may be linear, branched, or cyclic, and preferably has 1 to 30 carbon atoms, for example. The methylene group in the alkoxy group may be substituted with —O—. Z 1 , Z 2 , and Z 3Among these, particularly from the viewpoint of improving dispersibility, the organic group represented by the formula (I) is preferably a group having a steric repulsion effect, more preferably an alkyl group or alkoxy group having 5 to 24 carbon atoms, and even more preferably a branched alkyl group having 5 to 24 carbon atoms, a cyclic alkyl group having 5 to 24 carbon atoms, or an alkoxy group having 5 to 24 carbon atoms. Each of the above groups may have a substituent (for example, a hydroxyl group, an ethylenically unsaturated group such as a (meth)acryloyloxy group, etc.).

[0055] In addition, in formula (1), Z 1 When is a hydroxyl group, -COZ in the formula 1 The moiety represented by is an anion (-COO - In this case, the counter cation may be a quaternary ammonium salt.

[0056] In formulas (1) and (2), n and m represent the average number of additions and are a number of 3 or more. The lower limit values ​​of n and m are preferably 4 or more, more preferably 5 or more, and even more preferably 6 or more. The upper limit values ​​of n and m are preferably 100 or less, more preferably 70 or less, even more preferably 50 or less, and particularly preferably 30 or less.

[0057] In addition, in formula (3), p represents the average number of additions and is a number of 3 or more. The lower limit of p is preferably 4 or more, more preferably 5 or more, even more preferably 6 or more, still more preferably 10 or more, particularly preferably 15 or more, and most preferably 20 or more. The upper limit of p is preferably 100 or less, more preferably 70 or less, even more preferably 50 or less, and particularly preferably 30 or less.

[0058] In formulas (1) and (2), j and k each independently represent an integer of 2 to 10. In terms of providing the curable composition with better viscosity stability over time and developability, j and k in formulas (1) and (2) are preferably integers of 2 to 9, more preferably integers of 2 to 7, even more preferably integers of 4 to 6, and particularly preferably 5.

[0059] In addition, in formula (3), R 3represents a branched or linear alkylene group. The number of carbon atoms in the alkylene is preferably 2 to 10, more preferably 2 to 9, even more preferably 2 to 7, and particularly preferably 2 or 3. When p is 2 to 100, a plurality of R 3 may be the same or different from each other.

[0060] The repeating unit A2 is preferably a repeating unit represented by the above formula (1) or (3), and more preferably a repeating unit represented by the above formula (1).

[0061] Resin A may contain one type of repeating unit A2 alone or two or more types. The content of repeating unit A2 in resin A is preferably 35% by mass or more, more preferably 40% by mass or more, and even more preferably 50% by mass or more, based on the total repeating units of resin A. The upper limit is preferably 90% by mass or less, more preferably 80% by mass or less, and even more preferably 75% by mass or less. When two or more types of repeating unit A2 are used in combination, the total content is preferably within the above range.

[0062] —Other Repeating Unit (Repeating Unit A3)— Resin A may contain a repeating unit other than the repeating unit A1 and repeating unit A2 (hereinafter also referred to as “repeating unit A3”).

[0063] Examples of the other repeating units include repeating units having various functions other than the repeating units described above, such as a hydrophobic repeating unit (hereinafter also referred to as "repeating unit A31"), a repeating unit having a curable group (hereinafter also referred to as "repeating unit A32"), a repeating unit having a functional group capable of interacting with a pigment or the like (hereinafter also referred to as "repeating unit A33"), and a repeating unit derived from a radical monomer selected from the group consisting of acrylonitriles and methacrylonitriles.

[0064] (Repeating Unit A31) Resin A may contain a hydrophobic repeating unit (repeating unit A31). Examples of the repeating unit A31 include a repeating unit represented by the following formula (AX2).

[0065]

[0066] In the formula, R A4 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. A4 The number of carbon atoms in the alkyl group represented by R is preferably 1 or 2, and more preferably 1. A5 R represents a linear or branched alkyl group having 1 to 12 carbon atoms or an aralkyl group having 7 to 18 carbon atoms, and an aralkyl group having 7 to 18 carbon atoms is preferred in that the effects of the present invention are more excellent. A5 The number of carbon atoms in the alkyl group represented by R is preferably 1 to 8, more preferably 1 to 6, and even more preferably 1 to 4. A linear alkyl group is also preferred. A5 The number of carbon atoms in the aralkyl group represented by R is preferably 7 to 18, more preferably 7 to 12, and even more preferably 7 to 10. A5 The alkyl group and aralkyl group represented by the formula (I) may have a substituent. The substituent is not particularly limited, but examples thereof include a hydroxyl group.

[0067] The repeating unit A31 is preferably a repeating unit having a benzyl group, and more preferably a repeating unit derived from benzyl (meth)acrylate, in that the effects of the present invention are more excellent.

[0068] Resin A may contain one type of repeating unit A31 alone or two or more types. The content of repeating unit A31 in Resin A is preferably 5 to 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 40 mass %, based on the total repeating units of Resin A. When two or more types of repeating unit A31 are used in combination, the total content is preferably within the above range.

[0069] (Repeating Unit A32) Resin A may contain a repeating unit (repeating unit A32) having a curable group. Examples of the curable group include ethylenically unsaturated groups (e.g., (meth)acryloyl groups, vinyl groups, and styryl groups) and cyclic ether groups (e.g., epoxy groups and oxetanyl groups). Among these, ethylenically unsaturated groups are preferred as the curable group because they allow polymerization control through radical reaction. As the ethylenically unsaturated group, a (meth)acryloyl group is preferred.

[0070] The specific structure of the repeating unit A32 is not particularly limited, but it is preferably a repeating unit represented by the following formula (AX3).

[0071]

[0072] In the formula, R A11 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. A11 The number of carbon atoms in the alkyl group represented by the formula (I) is preferably 1 to 3, and more preferably 1.

[0073] L A11 represents a single bond, —COO—, or —CONR A12 - represents. A12 is the above R A11 The same definition and preferred embodiments are also the same.

[0074] L A12 represents a single bond or a divalent linking group. The type of the divalent linking group is not particularly limited, and examples thereof include a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, —O—, —S—, and —SO 2 -, -NR A13Examples of the divalent aliphatic hydrocarbon group include -, -CO-, and groups formed by combining two or more of these. The divalent aliphatic hydrocarbon group may be linear, branched, or cyclic. The number of carbon atoms is preferably 1 to 20, and more preferably 1 to 10. Examples of the divalent aliphatic hydrocarbon group include alkylene groups, alkenylene groups, and alkynylene groups, and among these, alkylene groups are preferred. Examples of the divalent aromatic hydrocarbon group include those having 6 to 10 carbon atoms, such as a phenylene group. The divalent aliphatic hydrocarbon group and the divalent aromatic hydrocarbon group may further have a substituent. The substituent is not particularly limited, and examples include acid groups such as a carboxylic acid group, a sulfonic acid group, a phosphoric acid group, and a phenolic hydroxyl group, as well as a hydroxyl group. The R A13 is the above R A11 The same definition and preferred embodiments are also the same.

[0075] Among these, the divalent linking group is preferably a group formed by combining two or more groups selected from the group consisting of an alkylene group which may have a substituent, -O-, and -CO-.

[0076] In the above formula (AX3), -L A11 -L A12 The number of atoms excluding hydrogen atoms in the moiety represented by - is preferably less than 40, for example.

[0077] W A11 represents a curable group. A11 Examples of the curable group represented by the formula (I) include the curable groups already described above.

[0078] Resin A may contain one type of repeating unit A32 alone or two or more types. The content of repeating unit A32 in Resin A is preferably 5 to 50 mass %, more preferably 5 to 40 mass %, and even more preferably 10 to 40 mass %, based on the total repeating units of Resin A. When two or more types of repeating unit A32 are used in combination, the total content is preferably within the above range.

[0079] (Repeating Unit A33) The resin A may contain a repeating unit (repeating unit A33) containing a functional group capable of forming an interaction with a colorant (pigment, etc.) described below. Examples of the functional group capable of forming an interaction with a colorant include a basic group, a coordinating group, and a reactive functional group.

[0080] Examples of basic groups include primary amino groups, secondary amino groups, tertiary amino groups, heterocycles containing an N atom, and amide groups. Among these, tertiary amino groups are preferred because of their excellent adsorption to pigments and high dispersibility. Resin A may contain one type of repeating unit containing a basic group, or two or more types. The content of repeating units containing a basic group in Resin A is preferably 0.01 to 50% by mass, based on the total repeating units of Resin A, and more preferably 0.01 to 30% by mass from the viewpoint of suppressing development inhibition. When two or more types of repeating units containing a basic group are used in combination, the total content is preferably within the above range.

[0081] Examples of coordinating groups and reactive functional groups include acetylacetoxy groups, trialkoxysilyl groups, isocyanate groups, acid anhydrides, and acid chlorides. Of these, the acetylacetoxy group is preferred because of its good adsorption to pigments and high dispersibility of pigments. Resin A may contain one type of repeating unit containing a coordinating group, or two or more types. The content of the repeating unit containing a coordinating group in Resin A is preferably 0.01 to 50% by mass, and more preferably 0.01 to 30% by mass, based on the total repeating units of Resin A. When two or more types of repeating units containing a coordinating group are used in combination, the total content is preferably within the above range.

[0082] Resin A may contain one type of repeating unit containing a reactive functional group, or two or more types. The content of the reactive functional group in Resin A is preferably 0.01 to 50 mass %, more preferably 0.01 to 30 mass %, based on the total repeating units of Resin A. When two or more types of reactive repeating units are used in combination, the total content is preferably within the above range.

[0083] The HSP distance between resin A and resin B is 1.5 MPa. 1/2 There is no particular limitation as long as it is greater than 1.5 MPa. 1/2 Over 5.0 MPa 1/2 The following is preferable, 2.0 to 4.0 MPa 1/2 It is more preferable that the HSP distance is 1.5 MPa. 1/2 When the HSP distance is greater than an appropriate upper limit (for example, 5.0 MPa), a phase-separated structure is easily formed in the curable composition layer, which is preferable. 1/2 ) or less, this is preferable because it makes it easier to align the exposure mask with the support in step 2 described below.

[0084] The dispersion term (δ) of the Hansen solubility parameter of resin A d ) is 14.0 to 18.0 MPa 1/2 is preferable, and 15.0 to 17.0 MPa 1/2 The polar term (δ) of the Hansen solubility parameter of Resin A is more preferably p ) is 3.0 to 7.0 MPa 1/2 is preferable, and 4.0 to 6.0 MPa 1/2 The hydrogen bond term (δ) of the Hansen solubility parameter of Resin A is more preferably h ) is 3.0 to 11.0 MPa 1/2 is preferable, and 4.5 to 9.5 MPa 1/2 is more preferred.

[0085] In terms of achieving superior effects of the present invention, the glass transition temperature of resin A is preferably at least 120°C lower than the temperature during the heat treatment in step 5 described below, more preferably at least 150°C lower, and even more preferably at least 180°C lower. In other words, the difference between the temperature during the heat treatment in step 5 described below and the glass transition temperature of resin A (temperature during the heat treatment - glass transition temperature of resin A) is preferably 120°C or higher. The glass transition temperature of resin A is often at least 250°C lower than the temperature during the heat treatment in step 5 described below. In other words, the difference between the temperature during the heat treatment in step 5 described below and the glass transition temperature of resin A (temperature during the heat treatment - glass transition temperature of resin A) is often 250°C or lower. In particular, it is preferable that at least one of the glass transition temperatures of resin A and resin B described below is at least 120°C lower than the temperature during the heat treatment in step 5. More specifically, the glass transition temperature of Resin A is preferably −40 to 100° C., more preferably −30 to 80° C., and even more preferably −20 to 50° C. The glass transition temperature can be measured using a DSC 3500 Sirius (manufactured by Netzsch).

[0086] In order to obtain superior effects of the present invention, the acid value of Resin A is preferably 50 mgKOH / g or more, more preferably 55 mgKOH / g or more, and even more preferably 60 mgKOH / g or more. The upper limit is preferably 200 mgKOH / g or less, more preferably 170 mgKOH / g or less, even more preferably 100 mgKOH / g or less, and particularly preferably 80 mgKOH / g or less. Note that a resin having a desired acid value can be obtained by changing the content of repeating units containing an acid group, which are constituent components of Resin A.

[0087] The weight average molecular weight of Resin A is preferably from 5,000 to 100,000, more preferably from 6,000 to 80,000, still more preferably from 15,000 to 40,000, and most preferably from 20,000 to 40,000.

[0088] The content of resin A in the curable composition is not particularly limited, but is preferably 2 to 40 mass %, more preferably 5 to 30 mass %, and even more preferably 10 to 25 mass %, relative to the total solid content of the curable composition. Resin A may be used alone or in combination of two or more types. When two or more types of resin A are used in combination, it is preferable that the total content is within the above range.

[0089] <Resin B> The curable composition 1 contains resin B. Resin B is not particularly limited as long as it satisfies the above-mentioned relationship of HSP distance with resin A and the polymerizable compound. Examples of resin B include (meth)acrylic resins, ester resins, olefin resins, and urethane resins. In particular, resin B preferably does not contain a repeating unit having a group selected from the group consisting of polyoxyalkylene groups having an average addition number of 3 or more and polyoxyalkylenecarbonyl groups having an average addition number of 3 or more. Resin B preferably contains a repeating unit B1 derived from an alkyl (meth)acrylate, more preferably contains repeating unit B1 and at least one of repeating unit B2 having a hydroxyl group and repeating unit B3 having a carboxylic acid group, and even more preferably contains all of repeating unit B1, repeating unit B2, and repeating unit B3. Resin B having the above-mentioned configuration improves the adhesion of a cured film formed from the curable composition and can form a phase-separated structure due to the HSP distance with resin A.

[0090] -Repeating Unit B1- Resin B preferably contains a repeating unit B1 derived from an alkyl (meth)acrylate. The repeating unit B1 represents a repeating unit different from the repeating unit B2 and repeating unit B3 described below, and is a repeating unit that does not contain a hydroxyl group or a carboxylic acid group. The alkyl group linked to the ester bond in the alkyl (meth)acrylate may be linear, branched, or cyclic, but is preferably linear or branched in terms of providing better effects of the present invention. The number of carbon atoms in the alkyl group is preferably 1 or more, and is preferably 4 or more in terms of providing better effects of the present invention. The upper limit is preferably 20 or less, more preferably 12 or less, and even more preferably 10 or less. The alkyl group may or may not have a substituent, but is preferably unsubstituted in terms of providing better effects of the present invention. Examples of the substituent include groups other than hydroxyl groups and carboxylic acid groups.

[0091] Resin B may contain one type of repeating unit B1 alone or two or more types. The content of repeating unit B1 in resin B is preferably 10% by mass or more, more preferably 60% by mass or more, still more preferably 70% by mass or more, and particularly preferably 80% by mass or more, based on the total repeating units of resin B. The upper limit is not particularly limited, but is preferably 99% by mass or less, more preferably 95% by mass or less. When two or more types of repeating unit B1 are used in combination, it is preferable that the total content be within the above range.

[0092] -Repeating unit B2- Resin B preferably contains a repeating unit B2 having a hydroxyl group. Repeating unit B2 is a repeating unit different from the repeating unit B1 described above, and preferably does not have a carboxylic acid group. The number of hydroxyl groups contained in repeating unit B2 may be one or more, for example, one to six.

[0093] The specific structure of the repeating unit B2 is not particularly limited, but it is preferably a repeating unit represented by the following formula (BX1).

[0094]

[0095] In the formula, R B1 represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms. B1 The number of carbon atoms in the alkyl group represented by the formula (I) is preferably 1 to 3, and more preferably 1.

[0096] L B1 represents a single bond, —COO—, or —CONR B2 - represents. B2 is the above R B1 The same definition and preferred embodiments are also the same.

[0097] L B2 represents a single bond or a divalent linking group. The type of the divalent linking group is not particularly limited, and examples thereof include a divalent aliphatic hydrocarbon group, a divalent aromatic hydrocarbon group, —O—, —S—, and —SO 2 -, -NR B3 Examples of the divalent aliphatic hydrocarbon group include -, -CO-, and groups formed by combining two or more of these. The divalent aliphatic hydrocarbon group may be linear, branched, or cyclic. The carbon number is preferably 1 to 20, and more preferably 1 to 10. Examples of the divalent aliphatic hydrocarbon group include alkylene groups, alkenylene groups, and alkynylene groups, and among these, alkylene groups are preferred. Examples of the divalent aromatic hydrocarbon group include those having 6 to 10 carbon atoms, such as a phenylene group. The divalent aliphatic hydrocarbon group and the divalent aromatic hydrocarbon group may further have a substituent. The substituent is not particularly limited, and examples thereof include a hydroxyl group. The above R B3 is the above R B1 The same definition and preferred embodiments are also the same.

[0098] Among these, the divalent linking group is preferably an alkylene group which may have a substituent, or an alkylene group which may have a substituent and contain a group selected from —O— and —CO—, and more preferably an alkylene group having 1 to 6 carbon atoms which may have a substituent.

[0099] In the above formula (BX1), -L B1 -L B2 The number of atoms excluding hydrogen atoms in the moiety represented by - is preferably less than 40, for example.

[0100] W B1 represents a hydroxyl group.

[0101] The repeating unit B2 is preferably a repeating unit derived from 2-ethylhydroxy(meth)acrylate, as this provides better effects of the present invention.

[0102] Resin B may contain one type of repeating unit B2 alone or two or more types. The lower limit of the content of repeating unit B2 in resin B is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 5% by mass or more, based on the total repeating units of resin B. The upper limit is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less. When two or more types of repeating unit B2 are used in combination, the total content is preferably within the above range.

[0103] -Repeating Unit B3- Resin B preferably contains a repeating unit B3 having a carboxylic acid group. Repeating unit B3 is a repeating unit different from the repeating unit B1 and the repeating unit B2 described above. Repeating unit B3 preferably does not contain a hydroxyl group. The number of carboxylic acid groups in repeating unit B3 may be one or more, for example, 1 to 6. Specifically, repeating unit B3 is a repeating unit represented by formula (AX1), which is given as an example of the repeating unit A1 contained in resin A, in which W A1 The preferred embodiments are also the same as those in which the acid group represented by the formula (I) is a carboxylic acid group.

[0104] Resin B may contain one type of repeating unit B3 alone or two or more types. The content of repeating unit B3 in Resin B is preferably 5 to 40 mass %, more preferably 5 to 30 mass %, and even more preferably 10 to 30 mass %, based on the total repeating units of Resin B. When two or more types of repeating unit B3 are used in combination, the total content is preferably within the above range.

[0105] —Other Repeating Unit (Repeating Unit B4)— Resin B may contain a repeating unit other than the repeating units B1 to B3 (hereinafter also referred to as “repeating unit B4”).

[0106] The other repeating units may include repeating units having various functions other than the repeating units described above. As the other repeating units, repeating units having an aromatic ring are preferred, repeating units having a benzyl group or repeating units derived from styrenes (e.g., styrene and α-methylstyrene, etc.) are more preferred, and repeating units derived from benzyl (meth)acrylate are even more preferred. Furthermore, Resin B may include a repeating unit selected from the group consisting of repeating units A31 to A33, which are listed as examples of other repeating units that Resin A may include.

[0107] Resin B may contain one type of repeating unit B4 alone or two or more types. The content of repeating unit B4 in Resin B is preferably 1 to 15 mass %, more preferably 5 to 15 mass %, based on the total repeating units of Resin B. When two or more types of repeating unit B41 are used in combination, the total content is preferably within the above range.

[0108] The dispersion term (δ) of the Hansen solubility parameter of resin B d ) is 14.0 to 18.0 MPa 1/2 is preferable, and 15.0 to 17.0 MPa 1/2 The polar term (δ) of the Hansen solubility parameter of Resin B is more preferably p ) is 2.0 to 7.0 MPa 1/2 is preferable, and 3.0 to 6.0 MPa 1/2 The hydrogen bond term (δ) of the Hansen solubility parameter of Resin B is more preferably h ) is 3.0 to 8.0 MPa 1/2 is preferable, and 4.0 to 7.0 MPa 1/2 is more preferred.

[0109] In order to obtain superior effects of the present invention, the glass transition temperature of resin B is preferably at least 120°C lower than the temperature during the heat treatment in step 5 described below, more preferably at least 130°C lower, and even more preferably at least 150°C lower. In other words, the difference between the temperature during the heat treatment in step 5 described below and the glass transition temperature of resin B (temperature during the heat treatment - glass transition temperature of resin B) is preferably 120°C or higher. The glass transition temperature of resin B is often at least 250°C lower than the temperature during the heat treatment in step 5 described below. In other words, the difference between the temperature during the heat treatment in step 5 described below and the glass transition temperature of resin B (temperature during the heat treatment - glass transition temperature of resin B) is often 250°C or lower. The glass transition temperature of resin B is preferably -20 to 120°C, more preferably -20 to 100°C, more preferably -5 to 80°C, even more preferably 0 to 70°C, and particularly preferably 30 to 70°C. The glass transition temperature can be measured using a DSC 3500 Sirius (manufactured by Netzsch).

[0110] The acid value of Resin B is preferably 0 mgKOH / g or more, more preferably 20 mgKOH / g or more, even more preferably 40 mgKOH / g or more, and particularly preferably 55 mgKOH / g or more. The upper limit is preferably 150 mgKOH / g or less, more preferably 100 mgKOH / g or less, and even more preferably 90 mgKOH / g or less. A resin having a desired acid value can be obtained by changing the content of repeating units containing an acid group, which are a constituent of Resin B.

[0111] The weight average molecular weight of Resin B is preferably from 5,000 to 100,000, more preferably from 8,000 to 80,000, still more preferably from 15,000 to 40,000, and particularly preferably from 18,000 to 25,000.

[0112] The content of resin B in the curable composition is not particularly limited, but is preferably 2 to 40% by mass, more preferably 5 to 35% by mass, and even more preferably 10 to 30% by mass, relative to the total solid content of the curable composition. Furthermore, in terms of more excellent effects of the present invention, the ratio of the content of resin A to the total content of resin A and resin B in the curable composition (content of resin A / total content of resin A and resin B) is preferably 0.30 to 0.50, more preferably 0.33 to 0.47, and even more preferably 0.35 to 0.45. Resin B may be used alone or in combination of two or more types. When two or more types of resin B are used in combination, it is preferable that the total content is within the above range.

[0113] <Polymerizable Compound> The curable composition 1 contains a polymerizable compound. The polymerizable compound is a compound different from the resins A and B described above. The polymerizable compound is preferably a compound having a polymerizable group that can generate a radical, cation, or anion by the action of heat, light, acid, base, or the like to form a covalent bond. The curing mechanism is not particularly limited, but a thermosetting or photocurable compound is preferred. Examples of the polymerizable group include an ethylenically unsaturated group. Examples of the ethylenically unsaturated group include a vinyl group, a (meth)allyl group, a (meth)acryloyl group, a (meth)acryloyloxy group, a (meth)acrylamide group, and a vinylphenyl group.

[0114] The molecular weight of the polymerizable compound (weight average molecular weight when the polymerizable compound has a molecular weight distribution) is not particularly limited, but is preferably 2500 or less, more preferably 2000 or less, and even more preferably 1500 or less. The lower limit is preferably 50 or more.

[0115] The polymerizable compound is preferably a compound containing an ethylenically unsaturated group (a group containing an ethylenically unsaturated bond). The polymerizable compound is preferably a compound containing one or more ethylenically unsaturated bonds, more preferably a compound containing two or more ethylenically unsaturated bonds, even more preferably a compound containing three or more ethylenically unsaturated bonds, and particularly preferably a compound containing four or more ethylenically unsaturated bonds. The upper limit is, for example, 15 or less. Examples of the ethylenically unsaturated group include a vinyl group, a (meth)allyl group, and a (meth)acryloyl group. Among these, the polymerizable compound is preferably a trifunctional to 15-functional (meth)acrylate compound, and more preferably a trifunctional to hexafunctional (meth)acrylate compound.

[0116] The polymerizable compound is preferably a polyfunctional (meth)acrylate obtained by esterifying or partially esterifying a polyhydric alcohol such as trimethylolethane, ditrimethylolethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, tripentaerythritol, glycerin, diglycerol, or trimethylolmelamine with (meth)acrylic acid. More specific examples of such polyfunctional (meth)acrylates include glycerin triacrylate, trimethylolpropane ethoxy triacrylate, pentaerythritol triacrylate, and pentaerythritol tetraacrylate. Furthermore, examples of the polymerizable compound include compounds described in paragraph

[0050] of JP 2008-260927 A and paragraph

[0040] of JP 2015-068893 A, the contents of which are incorporated herein by reference.

[0117] The polymerizable compound is also preferably a compound containing one or more ethylenically unsaturated groups and having a boiling point of 100° C. or higher under normal pressure. For example, the compounds described in paragraph

[0227] of JP-A No. 2013-029760 and paragraphs

[0254] to

[0257] of JP-A No. 2008-292970 can be used by reference, and the contents of these compounds are incorporated herein by reference.

[0118] Preferred commercially available polymerizable compounds include dipentaerythritol triacrylate (commercially available products include KAYARAD D-330, manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol tetraacrylate (commercially available products include KAYARAD D-320, manufactured by Nippon Kayaku Co., Ltd.), dipentaerythritol penta(meth)acrylate (commercially available products include KAYARAD D-310, manufactured by Nippon Kayaku Co., Ltd.), and dipentaerythritol hexa(meth)acrylate (commercially available products include KAYARAD DPHA, manufactured by Nippon Kayaku Co., Ltd., and A-DPH-12E, manufactured by Shin-Nakamura Chemical Co., Ltd.), as well as structures in which the (meth)acryloyl group is connected via an ethylene glycol residue or propylene glycol residue (for example, SR454 and SR499, commercially available from Sartomer). Oligomer types of these compounds can also be used. NK Ester A-TMMT (pentaerythritol tetraacrylate, manufactured by Shin-Nakamura Chemical Co., Ltd.), KAYARAD RP-1040, KAYARAD DPEA-12LT, KAYARAD DPHA LT, KAYARAD RP-3060, and KAYARAD DPEA-12 (all trade names, manufactured by Nippon Kayaku Co., Ltd.) may also be used. Furthermore, the polymerizable compound may be a urethane (meth)acrylate compound having both a (meth)acryloyl group and a urethane bond within the compound, such as KAYARAD DPHA-40H (trade name, manufactured by Nippon Kayaku Co., Ltd.). Preferred embodiments of the polymerizable compound are shown below.

[0119] The polymerizable compound may have an acid group such as a carboxylic acid group, a sulfonic acid group, or a phosphoric acid group. The polymerizable compound containing an acid group is preferably an ester of an aliphatic polyhydroxy compound and an unsaturated carboxylic acid, more preferably a polymerizable compound in which an acid group is provided by reacting an unreacted hydroxyl group of an aliphatic polyhydroxy compound with a non-aromatic carboxylic acid anhydride, and even more preferably, in this ester, the aliphatic polyhydroxy compound is pentaerythritol and / or dipentaerythritol. Examples of commercially available products include Aronix TO-2349, M-305, M-510, and M-520 manufactured by Toagosei Co., Ltd.

[0120] The acid value of the polymerizable compound containing an acid group is preferably 0.1 to 40 mgKOH / g, more preferably 5 to 30 mgKOH / g. If the acid value of the polymerizable compound is 0.1 mgKOH / g or more, the development solubility characteristics are good, and if it is 40 mgKOH / g or less, it is advantageous in terms of production and / or handling. Furthermore, the photopolymerization performance is good and the curing properties are excellent.

[0121] A preferred embodiment of the polymerizable compound is a compound containing a caprolactone structure. The compound containing a caprolactone structure is not particularly limited as long as it contains a caprolactone structure in the molecule, and examples thereof include ε-caprolactone-modified polyfunctional (meth)acrylates obtained by esterifying or partially esterifying a polyhydric alcohol such as trimethylolethane, ditrimethylolethane, trimethylolpropane, ditrimethylolpropane, pentaerythritol, dipentaerythritol, tripentaerythritol, glycerin, diglycerol, or trimethylolmelamine with (meth)acrylic acid and ε-caprolactone. Of these, compounds containing a caprolactone structure represented by the following formula (Z-1) are preferred:

[0122]

[0123] In formula (Z-1), all of the six R's are groups represented by formula (Z-2) below, or one to five of the six R's are groups represented by formula (Z-2) below, and the remainder are groups represented by formula (Z-3) below.

[0124]

[0125] In formula (Z-2), R 1 represents a hydrogen atom or a methyl group, m represents the number 1 or 2, and * represents the bonding position.

[0126]

[0127] In formula (Z-3), R 1 represents a hydrogen atom or a methyl group, and "*" represents the bonding position.

[0128] Polymerizable compounds containing a caprolactone structure are commercially available, for example, from Nippon Kayaku as the KAYARAD DPCA series, and include DPCA-20 (where m=1 in the above formulas (Z-1) to (Z-3), the number of groups represented by formula (Z-2)=2, and R 1 are all hydrogen atoms), DPCA-30 (same formula, m=1, number of groups represented by formula (Z-2)=3, R 1 are all hydrogen atoms), DPCA-60 (same formula, m=1, number of groups represented by formula (Z-2)=6, R 1 are all hydrogen atoms) and DPCA-120 (in the formula, m=2, the number of groups represented by formula (Z-2)=6, R 1 are all hydrogen atoms). In addition, an example of a commercially available polymerizable compound containing a caprolactone structure is M-350 (trade name) (trimethylolpropane triacrylate) manufactured by Toagosei Co., Ltd.

[0129] The polymerizable compound may also be a compound represented by the following formula (Z-4) or (Z-5).

[0130]

[0131] In formula (Z-4) and formula (Z-5), E is -((CH 2 ) y CH 2 O)- or -((CH 2 ) y CH (CH 3 )O)-, y represents an integer of 0 to 10, and X represents a (meth)acryloyl group, a hydrogen atom, or a carboxylic acid group. In formula (Z-4), the total number of (meth)acryloyl groups is 3 or 4, m represents an integer of 0 to 10, and the total of all m's is an integer of 0 to 40. In formula (Z-5), the total number of (meth)acryloyl groups is 5 or 6, n represents an integer of 0 to 10, and the total of all n's is an integer of 0 to 60.

[0132] In formula (Z-4), m is preferably an integer of 0 to 6, more preferably an integer of 0 to 4. The sum of each m is preferably an integer of 2 to 40, more preferably an integer of 2 to 16, and even more preferably an integer of 4 to 8. In formula (Z-5), n is preferably an integer of 0 to 6, more preferably an integer of 0 to 4. The sum of each n is preferably an integer of 3 to 60, more preferably an integer of 3 to 24, and even more preferably an integer of 6 to 12. In formula (Z-4) or formula (Z-5), -((CH 2 ) y CH 2 O)- or -((CH 2 ) y CH (CH 3 )O)- is preferably in a form in which the terminal on the oxygen atom side is bonded to X.

[0133] The compounds represented by formula (Z-4) or formula (Z-5) may be used alone or in combination of two or more. In particular, preferred are those in which all six Xs in formula (Z-5) are acryloyl groups, and those in formula (Z-5) that are a mixture of a compound in which all six Xs are acryloyl groups and a compound in which at least one of the six Xs is a hydrogen atom. Such a configuration can further improve developability.

[0134] The total content of the compound represented by formula (Z-4) or formula (Z-5) in the polymerizable compound is preferably 20% by mass or more, more preferably 50% by mass or more. Among the compounds represented by formula (Z-4) or formula (Z-5), pentaerythritol derivatives and / or dipentaerythritol derivatives are more preferred.

[0135] The polymerizable compound may also contain a cardo skeleton. The polymerizable compound containing a cardo skeleton is preferably a polymerizable compound containing a 9,9-bisarylfluorene skeleton. Examples of polymerizable compounds containing a cardo skeleton include Oncoat EX series (manufactured by Nagase & Co., Ltd.) and Oxol (manufactured by Osaka Gas Chemicals Co., Ltd.). Compounds containing an isocyanuric acid skeleton as a central nucleus are also preferred as polymerizable compounds. Examples of such polymerizable compounds include NK Ester A-9300 (manufactured by Shin-Nakamura Chemical Co., Ltd.).

[0136] As described above, the HSP distance (A) between the resin A and the polymerizable compound is not particularly limited as long as it is greater than the HSP distance (B) between the resin B and the polymerizable compound. However, the difference between the HSP distance (A) and the HSP distance (B) (HSP distance (A) - HSP distance (B)) is 0.1 MPa or less. 1/2 More than 0.5 MPa is preferable. 1/2 More preferably, 1.0 MPa or more 1/2 More preferably, the upper limit is 5.0 MPa. 1/2 Preferably, 3.0 MPa or less 1/2 More preferably, 2.0 MPa or less 1/2 The following is even more preferred:

[0137] The dispersion term (δ) of the Hansen solubility parameter of the polymerizable compound d ) is 15.0 to 21.0 MPa 1/2 is preferable, and 16.0 to 20.0 MPa 1/2 The polar term (δ) of the Hansen solubility parameter of the polymerizable compound is more preferably p ) is 0.1 to 5.0 MPa 1/2 is preferable, and 0.1 to 4.0 MPa 1/2 The hydrogen bond term (δ) of the Hansen solubility parameter of the polymerizable compound is more preferably h ) is 2.0 to 15.0 MPa 1/2 is preferable, and 3.0 to 14.0 MPa 1/2 is more preferred.

[0138] When two or more polymerizable compounds are used, the Hansen solubility parameters of the polymerizable compounds are calculated based on the mass fraction of each polymerizable compound. Specifically, the dispersion term (δ d ), polar term (δ p ), and the hydrogen bond term (δ h ) are calculated, and each of these components is multiplied by the mass fraction of each polymerizable compound and the results are summed up to obtain the dispersion term (δ d ), polar term (δ p ), and the hydrogen bond term (δ h For example, when n types of polymerizable compounds are used, the hydrogen bond parameter (δ) of the jth (j is an integer of 1 or more) polymerizable compound is calculated. h) and the mass fraction Nj of the j-th polymerizable compound relative to all polymerizable compounds, the hydrogen bond term (δ h ) can be calculated. h ) = ΣδPjNj (I) In the above, the hydrogen bond term (δ h ), the dispersion term (δ d ) and polarity term (δ p ) can be calculated following a similar procedure.

[0139] In order to obtain superior effects of the present invention, the shrinkage percentage of the polymerizable compound is preferably 7% or more, more preferably 10% or more, and even more preferably 15% or more. The upper limit is preferably 50% or less, more preferably 30% or less. In this specification, the "shrinkage percentage of the polymerizable compound" refers to the shrinkage percentage defined by the following formula (X):

[0140] Shrinkage (%)=(1−ρM / ρP)×100 Equation (X) In equation (X), ρM represents the specific gravity of the polymerizable compound measured in accordance with JIS-K-2249. ρP represents the specific gravity of a cured product of the polymerizable compound measured in accordance with JIS-K-2249. The cured product of the polymerizable compound refers to a cured product prepared by the following procedure.

[0141] (Method for producing a cured product) A composition consisting of 0.5% by mass of a radical polymerization initiator (V-601: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 99.5% by mass of a polymerizable compound was poured into a mold composed of a glass plate and a gasket made of an ethylene-vinyl acetate copolymer, and a cured product was produced by cast polymerization. The polymerization was carried out using an air oven, and the temperature was gradually raised from 30°C to 90°C over 18 hours, and then maintained at 90°C for 2 hours. After completion of the polymerization, the polymer was removed from the glass mold of the mold, and a cured product was obtained.

[0142] The content of ethylenically unsaturated groups in the polymerizable compound (meaning the value obtained by dividing the number of ethylenically unsaturated groups in the polymerizable compound by the molecular weight (g / mol) of the polymerizable compound) is preferably 5.0 mmol / g or more, and the upper limit is preferably 20.0 mmol / g or less.

[0143] In addition, when two or more polymerizable compounds are used, the shrinkage rate represents the shrinkage rate of a mixture of these polymerizable compounds. For example, when polymerizable compound A and polymerizable compound B are used as the polymerizable compounds, and the content of polymerizable compound A relative to all polymerizable compounds is 90% by mass, and the content of polymerizable compound B relative to all polymerizable compounds is 10% by mass, the mixture of polymerizable compound A and polymerizable compound B (content of polymerizable compound A: content of polymerizable compound B = 90:10 (mass ratio)) is used as the "polymerizable compound" in the above (method for producing a cured product), and the above measurement is performed.

[0144] The content of the polymerizable compound in the curable composition is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and particularly preferably 20% by mass or more, based on the total solid content of the curable composition. The upper limit is preferably 60% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less. The polymerizable compound may be used alone or in combination with two or more types. When two or more types of polymerizable compounds are used in combination, the total amount thereof is preferably within the above range.

[0145] <Colorant> The curable composition 1 may contain a colorant, and preferably the curable composition 1 further contains a colorant. The colorant is not particularly limited, and known colorants can be used. Examples of the colorant include a black colorant, a chromatic colorant, a white colorant, and a near-infrared absorbing agent. In this specification, the white colorant includes not only pure white colorants but also light gray colorants close to white (for example, grayish white, light gray, etc.).

[0146] The colorant preferably includes at least one selected from the group consisting of a black colorant, a chromatic colorant, and a near-infrared absorbing agent, and more preferably includes at least one selected from the group consisting of a black colorant and a chromatic colorant.

[0147] The colorant preferably contains one or more black colorants or chromatic colorants and a near-infrared absorber. Alternatively, two or more chromatic colorants may be combined to form a black color. For information on combinations of two or more chromatic colorants that form a black color, see JP 2013-077009 A, JP 2014-130338 A, and WO 2015 / 166779, among others.

[0148] The colorant may be either a pigment or a dye, with pigments being preferred, and inorganic pigments being more preferred. The average primary particle diameter of the pigment is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 10 nm or more. The upper limit is preferably less than 250 nm, more preferably 200 nm or less, even more preferably 180 nm, particularly preferably 150 nm or less, and most preferably 100 nm or less. In this specification, the primary particle diameter of the pigment can be determined by the manufacturer's nominal value, such as a catalog value, if the pigment is commercially available. However, if no catalog value is available, the primary particle diameter can be determined by observing the primary particles with a transmission electron microscope and using the resulting image. Specifically, the projected area of ​​the pigment primary particles is determined, and the corresponding circle-equivalent diameter is calculated as the primary particle diameter of the pigment. In this specification, the average primary particle diameter is the arithmetic mean value of the primary particle diameters of 400 pigment primary particles. Furthermore, the term "pigment primary particles" refers to independent particles that are not aggregated.

[0149] -Black Colorant- When the cured film obtained using the cured film manufacturing method of the present invention is used as a light-shielding film, the curable composition preferably contains a black colorant. That is, the colorant preferably contains a black colorant. The black colorant is not particularly limited, and known materials can be used. In this specification, the black colorant refers to a colorant that exhibits absorption over the entire wavelength range of 400 to 700 nm. Examples of black colorants include inorganic pigments (black pigments) such as carbon black, titanium black, and graphite. The inorganic pigment preferably contains carbon black or titanium black, and more preferably titanium black.

[0150] (Black Pigment) The black pigment may be a combination of multiple pigments that cannot be used alone and adjusted to produce a black overall color, but a pigment that exhibits a black color alone is preferred. Alternatively, a black pigment that exhibits a black color alone and absorbs infrared rays may be used. Here, the infrared-absorbing black pigment has absorption in the infrared wavelength region (preferably, wavelengths of 650 to 1300 nm). A black pigment that has a maximum absorption wavelength in the wavelength region of 675 to 900 nm is also preferred.

[0151] The average particle size of the black pigment is preferably 250 nm or less, more preferably 200 nm or less, and even more preferably 150 nm or less. From the viewpoint of better handleability, the average particle size is preferably 1 nm or more, more preferably 5 nm or more, and even more preferably 20 nm or more.

[0152] The average particle size is calculated by the following method. The curable composition is diluted with propylene glycol monomethyl ether acetate (PGMEA) to prepare a measurement solution with a solids concentration of 0.2% by mass. Next, using a dynamic light scattering particle size distribution analyzer (LB-500 (product name) manufactured by Horiba, Ltd.) conforming to JIS 8826:2005, data from the measurement solution is acquired 50 times at 25°C using a 2 ml quartz measurement cell, and the obtained number-based particle sizes are arithmetically averaged to determine the average particle size. Note that, although the measurement solution is prepared using the curable composition in the above, the measurement may also be performed using a colorant dispersion in which a black pigment is dispersed. For example, if the curable composition contains particles other than the black pigment, the average particle size of the black pigment may be measured using a colorant dispersion in which the black pigment used in preparing the curable composition is dispersed. Furthermore, if the curable composition contains particles other than the black pigment, the average particle size of the black pigment may be measured after separating the black pigment from the other particles by any method.

[0153] As the black pigment, various known black pigments can be used. The black pigment may be an inorganic pigment or an organic pigment. In terms of achieving the effects of the present invention more effectively, the black pigment is preferably an inorganic pigment, and more preferably carbon black, metal nitride particles, or metal oxynitride particles.

[0154] Black Inorganic Pigment The black inorganic pigment is not particularly limited as long as it has light-shielding properties and is a particle containing an inorganic compound, and any known inorganic pigment can be used.

[0155] Examples of inorganic pigments include metal oxides, metal nitrides, and metal oxynitrides containing one or more metal elements selected from the group consisting of titanium (Ti) and zirconium (Zr), Group 4 metal elements such as vanadium (V) and niobium (Nb), yttrium (Y), aluminum (Al), cobalt (Co), chromium (Cr), copper (Cu), manganese (Mn), ruthenium (Ru), iron (Fe), nickel (Ni), tin (Sn), and silver (Ag). Among these, metal oxides, metal nitrides, and metal oxynitrides containing one or more metal elements selected from the group consisting of titanium (Ti), zirconium (Zr), vanadium (V), yttrium (Y), aluminum (Al), and iron (Fe) are preferred. In other words, the inorganic pigment may contain two or more metal atoms. The metal oxides, metal nitrides, and metal oxynitrides may contain particles containing other metal atoms. For example, metal nitride-containing particles containing an atom (preferably an oxygen atom and / or a sulfur atom) selected from the elements of Groups 13 to 17 of the Periodic Table may be used. The metal oxides, metal nitrides, and metal oxynitrides may be coated with an inorganic and / or organic substance. Examples of the inorganic substance include the metal atoms contained in the inorganic pigment. Examples of the organic substance include organic substances having a hydrophobic group, with silane compounds being preferred.

[0156] Among these, the inorganic pigment is more preferably a nitride or oxynitride of one or more metals selected from the group consisting of titanium, vanadium, zirconium, niobium, and iron, from the viewpoint of being able to suppress the occurrence of undercuts when forming a cured film, and even more preferably a nitride or oxynitride of zirconium, or a nitride or oxynitride of titanium (titanium black).

[0157] Titanium black is a black particle containing titanium oxynitride. The surface of titanium black can be modified as needed to improve dispersibility, suppress aggregation, etc. Titanium black can be coated with silicon oxide, titanium oxide, germanium oxide, aluminum oxide, magnesium oxide, or zirconium oxide, and can also be treated with a water-repellent substance as described in JP 2007-302836 A.

[0158] The particle size of titanium black is not particularly limited, but is preferably 10 to 45 nm, more preferably 12 to 20 nm. The specific surface area of ​​titanium black is not particularly limited, but in order to achieve a predetermined water repellency after surface treatment with a water repellent agent, the value measured by the BET (Brunauer, Emmett, Teller) method should be 5 to 150 m. 2 / g, and 20 to 100m 2 It is more preferable that the SiO2 content is 1 / g.

[0159] Examples of titanium black include Titanium Black 10S, 12S, 13R, 13M, 13M-C, 13R, 13R-N, and 13M-T (trade names, manufactured by Mitsubishi Materials Corporation), Tilack D (trade name, manufactured by Ako Kasei Co., Ltd.), and MT-150A (trade name, manufactured by Teika Corporation).

[0160] The curable composition also preferably contains titanium black as a dispersed substance containing titanium black and Si atoms. In this embodiment, titanium black is contained as a dispersed substance in the curable composition. The ratio of Si atoms to Ti atoms (Si / Ti) in the dispersed substance is preferably 0.05 to 0.5, more preferably 0.07 to 0.4, calculated by mass. Here, the dispersed substance includes both titanium black in the form of primary particles and titanium black in the form of aggregates (secondary particles). Furthermore, if the Si / Ti ratio of the dispersed substance is a predetermined value or higher, residues are less likely to remain in the removed areas when a composition layer using the dispersed substance is patterned by photolithography or the like. If the Si / Ti ratio of the dispersed substance is a predetermined value or lower, the light-blocking ability is likely to be good.

[0161] The following methods can be used to change the Si / Ti ratio of the dispersed substance (e.g., to 0.05 or more). First, titanium oxide and silica particles are dispersed using a disperser to obtain a dispersion, and this mixture is then reduced at a high temperature (e.g., 850 to 1000°C) to obtain a dispersed substance containing titanium black particles as the main component and Si and Ti. Titanium black with an adjusted Si / Ti ratio can be produced, for example, by the method described in paragraphs

[0005] and

[0016] to

[0021] of JP 2008-266045 A. The ratio of Si atoms to Ti atoms (Si / Ti) in the dispersed substance can be measured, for example, using method (2-1) or method (2-3) described in paragraphs

[0054] to

[0056] of WO 2011 / 049090 A.

[0162] In the dispersion containing titanium black and Si atoms, the titanium black described above can be used. Furthermore, in this dispersion, in order to adjust dispersibility, colorability, etc., one or more black pigments composed of composite oxides of multiple metals selected from Cu, Fe, Mn, V, Ni, etc., cobalt oxide, iron oxide, carbon black, aniline black, etc. may be used in combination with titanium black. In this case, it is preferable that the dispersion composed of titanium black accounts for 50% by mass or more of the total dispersion.

[0163] Examples of black inorganic pigments include carbon black. Examples of carbon black include furnace black, channel black, thermal black, acetylene black, and lamp black. Carbon black produced by a known method such as the oil furnace method may be used, or a commercially available product may be used. Examples of commercially available carbon black include inorganic pigments such as C.I. Pigment Black 7.

[0164] The carbon black is preferably surface-treated. The surface treatment can modify the particle surface state of the carbon black and improve the dispersion stability in the curable composition. Examples of surface treatments include coating with a resin, surface treatment introducing an acidic group, and surface treatment with a silane coupling agent.

[0165] The carbon black is preferably carbon black coated with a resin. Coating the surface of carbon black particles with an insulating resin can improve the light-blocking and insulating properties of the cured film. Furthermore, the reliability of image display devices can be improved by reducing leakage current, etc. This makes the cured film suitable for applications requiring light-blocking and insulating properties. Examples of coating resins include epoxy resins, polyamides, polyamideimides, novolac resins, phenolic resins, urea resins, melamine resins, polyurethanes, diallyl phthalate resins, alkylbenzene resins, polystyrene, polycarbonates, polybutylene terephthalates, and modified polyphenylene oxides. The content of the coating resin is preferably 0.1 to 40% by mass, more preferably 0.5 to 30% by mass, of the total of the carbon black and the coating resin, in order to obtain better light-blocking and insulating properties of the cured film.

[0166] Examples of inorganic pigments used as black pigments include those described in JP 2017-222559 A, WO 2019 / 130772 A, WO 2019 / 059359 A, and JP 2009-091205 A, the contents of which are incorporated herein by reference.

[0167] Black Organic Pigment The black pigment may be an organic pigment, and the black colorant preferably contains a black organic pigment. The organic pigment used as the black pigment is not particularly limited as long as it has light-shielding properties and is a particle containing an organic compound, and known organic pigments can be used. In the present invention, examples of the organic pigment include bisbenzofuranone compounds, azomethine compounds, perylene compounds, and azo compounds, and bisbenzofuranone compounds or perylene compounds are preferred.

[0168] Examples of bisbenzofuranone compounds include compounds described in JP-A-2010-534726, JP-A-2012-515233, and JP-A-2012-515234. Bisbenzofuranone compounds are available as "Irgaphor Black" (trade name) manufactured by BASF. Examples of perylene compounds include compounds described in JP-A-62-001753 and JP-B-63-026784. Perylene compounds are available as C.I. Pigment Black 21, 30, 31, 32, 33, and 34.

[0169] - Chromatic Colorant - When the cured film obtained by the cured film manufacturing method of the present invention is used as a color filter, the curable composition preferably contains a chromatic colorant. Examples of the chromatic colorant include colorants having a maximum absorption wavelength in the wavelength range of 400 to 700 nm. Examples include green colorants, red colorants, yellow colorants, purple colorants, blue colorants, and orange colorants.

[0170] Examples of the green colorant include phthalocyanine compounds and squarylium compounds, and phthalocyanine compounds are preferred. In addition, the compounds described in paragraph

[0043] of WO 2021 / 182268 can also be used as the green colorant.

[0171] Examples of the red colorant include a diketopyrrolopyrrole compound, an anthraquinone compound, an azo compound, a naphthol compound, an azomethine compound, a xanthene compound, a quinacridone compound, a perylene compound, and a thioindigo compound, and the like, preferably a diketopyrrolopyrrole compound, an anthraquinone compound, or an azo compound, and more preferably a diketopyrrolopyrrole compound. In addition, the red colorant is preferably a pigment. Specific examples of the red colorant include C.I. (Color Index) Pigment Red 1, 2, 3, 4, 5, 6, 7, 9, 10, 14, 17, 22, 23, 31, 38, 41, 48: 1, 48: 2, 48: 3, 48: 4, 49, 49: 1, 49: 2, 52: 1, 52: 2, 53: 1, 57: 1, 60: 1, 63: 1, 66, 67, 81: 1, 81: 2, 81: 3, 83, 88, 90, 105, 112, 119, 122, 123, 144, 146, 149, Examples of red pigments include 150, 155, 166, 168, 169, 170, 171, 172, 175, 176, 177, 178, 179, 184, 185, 187, 188, 190, 200, 202, 206, 207, 208, 209, 210, 216, 220, 224, 226, 242, 246, 254, 255, 264, 269, 270, 272, 279, 291, 294, 295, 296, and 297. In addition, compounds described in paragraphs

[0048] to

[0049] of WO 2021 / 182268 can also be used as red colorants.

[0172] Examples of yellow colorants include azo compounds, azomethine compounds, isoindoline compounds, pteridine compounds, quinophthalone compounds, perylene compounds, and azobarbituric acid nickel complexes. The yellow colorant is preferably a pigment, more preferably an azo pigment, azomethine pigment, isoindoline pigment, pteridine pigment, quinophthalone pigment, or perylene pigment, and more preferably an azo pigment or azomethine pigment. Specific examples of yellow colorants include C.I. Pigment Yellow 1, 2, 3, 4, 5, 6, 10, 11, 12, 13, 14, 15, 16, 17, 18, 20, 24, 31, 32, 34, 35, 35:1, 36, 36:1, 37, 37:1, 40, 42, 43, 53, 55, 60, 61, 62, 63, 65, 73, 74, 77, 81, 83, 86, 93, 94, 95, 97, 98, 100, 101, 104, 106, 108, 109, 110, 113, 114, 115, 116, 117, 118, 119, 120, 123, 125 , 126, 127, 128, 129, 137, 138, 139, 147, 148, 150, 151, 152, 153, 154, 155, 156, 161, 162, 164, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 179, 180, 181, 182, 185, 187, 188, 193, 194, 199, 213, 214, 215, 228, 231, 232, 233, 234, 235, 236 and the like.

[0173] In addition, the compounds described in paragraphs

[0045] to

[0047] of WO 2021 / 182268 can also be used as yellow colorants.

[0174] Examples of orange colorants include orange pigments such as C.I. Pigment Orange 2, 5, 13, 16, 17:1, 31, 34, 36, 38, 43, 46, 48, 49, 51, 52, 55, 59, 60, 61, 62, 64, 71, and 73.

[0175] Examples of purple colorants include purple pigments such as C.I. Pigment Violet 1, 19, 23, 27, 32, 37, 42, 60, and 61.

[0176] Examples of blue colorants include C.I. Pigment Blue 1, 2, 15, 15: 1, 15: 2, 15: 3, 15: 4, 15: 6, 16, 22, 29, 60, 64, 66, 79, 80, 87, and 88. In addition, the compounds described in paragraph

[0044] of WO 2021 / 182268 can also be used as blue colorants.

[0177] Dyes can also be used as chromatic colorants. There are no particular limitations on the dyes, and known dyes can be used. Examples include pyrazole azo dyes, anilino azo dyes, triarylmethane dyes, anthraquinone dyes, anthrapyridone dyes, benzylidene dyes, oxonol dyes, pyrazolotriazole azo dyes, pyridone azo dyes, cyanine dyes, phenothiazine dyes, pyrrolopyrazole azomethine dyes, xanthene dyes, phthalocyanine dyes, benzopyran dyes, indigo dyes, and pyrromethene dyes.

[0178] White Colorant Examples of white colorants include inorganic pigments (white pigments), such as titanium oxide, strontium titanate, barium titanate, zinc oxide, magnesium oxide, zirconium oxide, aluminum oxide, barium sulfate, silica, talc, mica, aluminum hydroxide, calcium silicate, aluminum silicate, and zinc sulfide. Furthermore, the titanium oxide described in "Titanium Oxide: Physical Properties and Application Technology," by Kiyono Manabu, pages 13-45, published June 25, 1991, published by Gihodo Publishing, can also be used as the white pigment.

[0179] The white pigment is preferably a particle having a titanium atom, more preferably titanium oxide. The white pigment is preferably a particle having a refractive index of 2.10 or more with respect to light having a wavelength of 589 nm. The refractive index is preferably 2.10 to 3.00, more preferably 2.50 to 2.75.

[0180] The white pigment may be composed not only of a single inorganic substance, but also of particles composited with other materials. For example, it is preferable to use particles having internal voids or other materials, particles having a large number of inorganic particles attached to a core particle, or core-shell composite particles consisting of a core particle made of polymer particles and a shell layer made of inorganic nanoparticles. For examples of core-shell composite particles consisting of a core particle made of polymer particles and a shell layer made of inorganic nanoparticles, see, for example, paragraphs

[0012] to

[0042] of JP 2015-047520 A, the contents of which are incorporated herein by reference. Hollow inorganic particles can also be used as the white pigment. Hollow inorganic particles are inorganic particles with a structure having a hollow interior, i.e., inorganic particles having a hollow surrounded by an outer shell. Examples of hollow inorganic particles include those described in JP 2011-075786 A, WO 2013 / 061621 A, and JP 2015-164881 A, the contents of which are incorporated herein by reference.

[0181] - Near-infrared absorber - The near-infrared absorber may be either a pigment or a dye, but is preferably a pigment, and more preferably an organic pigment. The near-infrared absorber is preferably a compound having a maximum absorption wavelength in the wavelength range of more than 700 nm to 1400 nm. The maximum absorption wavelength of the near-infrared absorber is preferably 1200 nm or less, more preferably 1000 nm or less, and even more preferably 950 nm or less. In addition, the near-infrared absorber has an absorbance A at a wavelength of 550 nm. 550 and absorbance A at the maximum absorption wavelength max A is the ratio of 550 / A max is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.03 or less, and particularly preferably 0.02 or less. The lower limit is not particularly limited, but may be, for example, 0.0001 or more, or may be 0.0005 or more.

[0182] The near-infrared absorber is not particularly limited, and examples thereof include pyrrolopyrrole compounds, copper compounds, cyanine compounds, phthalocyanine compounds, iminium compounds, thiol complex compounds, transition metal oxide compounds, squarylium compounds, naphthalocyanine compounds, quattarylene compounds, merocyanine compounds, oxonol compounds, iminium compounds, dithiol compounds, triarylmethane compounds, pyrromethene compounds, azomethine compounds, anthraquinone compounds, dibenzofuranone compounds, dithiolene metal complexes, dithiol metal complex compounds, and croconium compounds. As the phthalocyanine compounds, naphthalocyanine compounds, iminium compounds, cyanine compounds, squarylium compounds, and croconium compounds, the compounds disclosed in paragraphs 0010 to 0081 of JP 2010-111750 A may be used, the contents of which are incorporated herein by reference. For details of cyanine compounds, see, for example, "Functional Dyes, by Okawara Makoto, Matsuoka Masaru, Kitao Teijiro, and Hirashima Kosuke, published by Kodansha Scientific," the contents of which are incorporated herein by reference.

[0183] As the colorant having the above-described spectral properties, it is also possible to use the compounds disclosed in paragraphs

[0004] to

[0016] of JP-A-07-164729 and / or the compounds disclosed in paragraphs

[0027] to

[0062] of JP-A-2002-146254, and near-infrared absorbing particles comprising crystallites of an oxide containing Cu and / or P and having a number average agglomerated particle size of 5 to 200 nm, which are disclosed in paragraphs

[0034] to

[0067] of JP-A-2011-164583.

[0184] The compound having a maximum absorption wavelength in the wavelength region of 675 to 900 nm is preferably at least one selected from the group consisting of cyanine compounds, pyrrolopyrrole compounds, squarylium compounds, phthalocyanine compounds, and naphthalocyanine compounds. Regarding pyrrolopyrrole compounds, reference can be made to paragraphs

[0049] to

[0062] of JP2010-222557A, the contents of which are incorporated herein by reference. Regarding cyanine compounds and squarylium compounds, reference can be made to paragraphs

[0022] to

[0063] of WO2014 / 088063A, paragraphs

[0053] to

[0118] of WO2014 / 030628A, paragraphs

[0028] to

[0074] of JP2014-59550A, and paragraphs

[0013] to

[0091] of WO2012 / 169447A. , paragraphs 0019 to 0033 of JP 2015-176046 A, paragraphs 0053 to 0099 of JP 2014-63144 A, paragraphs 0085 to 0150 of JP 2014-52431 A, paragraphs 0076 to 0124 of JP 2014-44301 A, paragraphs 0045 to 0078 of JP 2012-8532 A, Paragraphs 0027 to 0067 of JP 2015-172102 A, paragraphs 0029 to 0067 of JP 2015-172004 A, paragraphs 0029 to 0085 of JP 2015-40895 A, paragraphs 0022 to 0036 of JP 2014-126642 A, paragraphs 0011 to 0017 of JP 2014-148567 A , paragraphs 0010 to 0025 of JP 2015-157893 A, paragraphs 0013 to 0026 of JP 2014-095007 A, paragraphs 0013 to 0047 of JP 2014-80487 A, and paragraphs 0007 to 0028 of JP 2013-227403 A can be referred to, the contents of which are incorporated herein by reference.

[0185] The content of the colorant is preferably 10 to 90 mass%, more preferably 25 to 80 mass%, still more preferably 30 to 80 mass%, and particularly preferably 30 to 70 mass%, based on the total solid content of the curable composition. The curable composition may contain only one type of colorant, or may contain two or more types. When two or more types are contained, the total amount thereof is preferably within the above range.

[0186] <Photopolymerization initiator> In addition to the components described above, the curable composition 1 preferably further contains at least one component selected from the group consisting of a photopolymerization initiator, a thermally crosslinkable compound, a surfactant, and a solvent, which will be described in detail later. Each of the above components will be described in detail below. The photopolymerization initiator is not particularly limited as long as it can initiate polymerization of the polymerizable compound, and known photopolymerization initiators can be used. For example, a photopolymerization initiator that is photosensitive to light in the ultraviolet to visible light range is preferred. Alternatively, the photopolymerization initiator may be an activator that reacts in some way with a photoexcited sensitizer to generate active radicals, or an initiator that initiates cationic polymerization depending on the type of polymerizable compound. A so-called radical polymerization initiator is preferred as the photopolymerization initiator.

[0187] Examples of the photopolymerization initiator include halogenated hydrocarbon derivatives (e.g., compounds containing a triazine skeleton, compounds containing an oxadiazole skeleton, etc.), acylphosphine compounds such as acylphosphine oxide, hexaarylbiimidazole, oxime compounds such as oxime derivatives, organic peroxides, thio compounds, ketone compounds, aromatic onium salts, aminoacetophenone compounds, and hydroxyacetophenone. Specific examples of the photopolymerization initiator can be found in, for example, paragraphs 0265 to 0268 of JP 2013-029760 A, the contents of which are incorporated herein by reference.

[0188] (Oxime Compound) As the photopolymerization initiator, an oxime ester polymerization initiator (oxime compound) is preferred. Oxime compounds are particularly preferred because they have high sensitivity and high polymerization efficiency, and are easy to design to have a high pigment content in the curable composition. Examples of oxime compounds include the compounds described in JP-A-2001-233842, JP-A-2000-080068, and JP-A-2006-342166. Examples of oxime compounds include 3-benzoyloxyiminobutan-2-one, 3-acetoxyiminobutan-2-one, 3-propionyloxyiminobutan-2-one, 2-acetoxyiminopentan-3-one, 2-acetoxyimino-1-phenylpropan-1-one, 2-benzoyloxyimino-1-phenylpropan-1-one, 3-(4-toluenesulfonyloxy)iminobutan-2-one, and 2-ethoxycarbonyloxyimino-1-phenylpropan-1-one. Further, see J. C. S. Perkin II (1979) pp. 1653-1660, J. C. S. Perkin II (1979) pp. 1653-1660, J. C. S. Perkin II (1979) pp. 1653-1660, and J. C. S. Perkin II (1979) pp. 1653-1660. 156-162, Journal of Photopolymer Science and Technology (1995) pp. 202-232, the compounds described in JP-A-2000-066385, and the compounds described in JP-A-2000-080068, JP-A-2004-534797, and JP-A-2006-342166. Commercially available products include IRGACURE-OXE01 (manufactured by BASF), IRGACURE-OXE02 (manufactured by BASF), IRGACURE-OXE03 (manufactured by BASF), and IRGACURE-OXE04 (manufactured by BASF). Other examples include TR-PBG-304 (manufactured by Changzhou Strong Electronic New Materials Co., Ltd.), ADEKA ARCLES NCI-730, ADEKA ARCLES NCI-831, ADEKA ARCLES NCI-930 (manufactured by ADEKA Corporation), and N-1919 (a carbazole oxime ester skeleton-containing photoinitiator (manufactured by ADEKA Corporation)). Also included is Omnirad 1316 (IGM).

[0189] Examples of oxime compounds other than those mentioned above include the compound disclosed in JP-T-2009-519904 A in which an oxime is linked to the N-position of the carbazole; the compound disclosed in U.S. Pat. No. 7,626,957 A in which a heterosubstituent is introduced at the benzophenone moiety; the compounds disclosed in JP-A-2010-015025 A and U.S. Patent Publication No. 2009-292039 A in which a nitro group is introduced at the dye moiety; the ketoxime compounds disclosed in WO-A-2009-131189 A; and the compound disclosed in U.S. Pat. No. 7,556,910 A containing a triazine skeleton and an oxime skeleton in the same molecule; and the compound disclosed in JP-A-2009-221114 A which has an absorption maximum at 405 nm and good sensitivity to a g-line light source. For example, see paragraphs

[0274] and

[0275] of JP-A-2013-029760 A, the contents of which are incorporated herein by reference.

[0190] The photopolymerization initiator also includes an oxime compound containing a fluorine atom. Examples of the oxime compound containing a fluorine atom include the compounds described in JP-A-2010-262028; compounds 24, 36 to 40 described in JP-A-2014-500852; and compound (C-3) described in JP-A-2013-164471. The contents of these compounds are incorporated herein by reference.

[0191] The polymerization initiator also includes compounds represented by the following formulas (1) to (4).

[0192]

[0193]

[0194] In formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 20 carbon atoms, an alicyclic hydrocarbon group having 4 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms; R 1 and R 2 When R is a phenyl group, the phenyl groups may be bonded to each other to form a fluorene group, 3 and R 4each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms, and X represents a direct bond or a carbonyl group.

[0195] In formula (2), R 1 , R 2 , R 3 , and R 4 is R in formula (1). 1 , R 2 , R 3 , and R 4 is synonymous with R 5 is -R 6 , -OR 6 , -SR 6 , -COR 6 , -CONR 6 R 6 , -NR 6 COR 6 , -OCOR 6 , -COOR 6 , -SCOR 6 , -OCSR 6 , -COSR 6 , -CSOR 6 , —CN, a halogen atom, or a hydroxyl group; R 6 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms; X represents a direct bond or a carbonyl group; and a represents an integer of 0 to 4.

[0196] In formula (3), R 1 represents an alkyl group having 1 to 20 carbon atoms, an alicyclic hydrocarbon group having 4 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, or an arylalkyl group having 7 to 30 carbon atoms; R 3 and R 4 each independently represents a hydrogen atom, an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms, and X represents a direct bond or a carbonyl group.

[0197] In formula (4), R 1 , R 3 , and R 4is R in formula (3). 1 , R 3 , and R 4 is synonymous with R 5 is -R 6 , -OR 6 , -SR 6 , -COR 6 , -CONR 6 R 6 , -NR 6 COR 6 , -OCOR 6 , -COOR 6 , -SCOR 6 , -OCSR 6 , -COSR 6 , -CSOR 6 , —CN, a halogen atom, or a hydroxyl group; R 6 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 30 carbon atoms, an arylalkyl group having 7 to 30 carbon atoms, or a heterocyclic group having 4 to 20 carbon atoms; X represents a direct bond or a carbonyl group; and a represents an integer of 0 to 4.

[0198] Examples of the compounds represented by formula (1) and formula (2) include the compounds described in paragraphs 0076 to 0079 of JP-A-2014-137466, the contents of which are incorporated herein by reference.

[0199] Furthermore, as the photopolymerization initiator, a compound represented by the following formula (1) is also preferred.

[0200]

[0201] In formula (1), R represents a group represented by the following formula (1a):

[0202]

[0203] In formula (1a), n represents an integer of 1 to 5. m represents an integer of 1 to 6. * represents a bonding position.

[0204] m is preferably 3 or 4. The compound represented by formula (1) can be synthesized, for example, according to the synthesis method described in JP-A-2012-519191.

[0205] The oxime compound preferably has a maximum absorption wavelength in the wavelength region of 350 to 500 nm, more preferably in the wavelength region of 360 to 480 nm, and even more preferably has high absorbance at wavelengths of 365 nm and 405 nm. From the viewpoint of sensitivity, the molar absorption coefficient of the oxime compound at 365 nm or 405 nm is preferably 1,000 to 300,000, more preferably 2,000 to 300,000, and even more preferably 5,000 to 200,000. The molar absorption coefficient of the compound can be measured using a known method; for example, it is preferably measured using ethyl acetate at a concentration of 0.01 g / L using an ultraviolet-visible spectrophotometer (Varian Cary-5 spectrophotometer).

[0206] In addition, as the photopolymerization initiator, compounds described in paragraph 0052 of JP-A-2008-260927, paragraphs 0033 to 0037 of JP-A-2010-097210, and paragraph 0044 of JP-A-2015-068893 can also be used, and the contents of the above are incorporated herein by reference.

[0207] The content of the photopolymerization initiator in the curable composition is preferably 0.5 to 20 mass%, more preferably 1.0 to 10 mass%, and even more preferably 1.5 to 8 mass%, based on the total solid content of the curable composition. The photopolymerization initiator may be used alone or in combination of two or more. When two or more photopolymerization initiators are used in combination, the total amount thereof is preferably within the above range.

[0208] <Thermal Crosslinkable Compound> The curable composition 1 may contain a thermal crosslinkable compound, which is often a compound containing an epoxy group. Examples of the compound containing an epoxy group include compounds having one or more epoxy groups, and compounds having two or more epoxy groups are preferred. The epoxy group preferably contains 1 to 100 epoxy groups. The upper limit may be, for example, 10 or less, or 5 or less. The lower limit is preferably 2 or more. The epoxy group-containing compound is intended to be a component different from the dispersant, alkali-soluble resin, and polymerizable compound described above.

[0209] The epoxy equivalent of the compound containing an epoxy group (=molecular weight of the compound containing an epoxy group / number of epoxy groups) is preferably 500 g / equivalent or less, more preferably 100 to 400 g / equivalent, and even more preferably 100 to 300 g / equivalent.

[0210] The compound containing an epoxy group may be a low molecular weight compound (e.g., a molecular weight of less than 2000) or a high molecular weight compound (macromolecule) (e.g., a molecular weight of 2000 or more, and in the case of a polymer, a weight average molecular weight of 2000 or more). The weight average molecular weight of the compound containing an epoxy group is preferably 200 to 100,000, more preferably 500 to 50,000. The upper limit of the weight average molecular weight is more preferably 10,000 or less, even more preferably 5,000 or less, and particularly preferably 3,000 or less.

[0211] The epoxy group-containing compound may be a commercially available product. Examples include EHPE3150 (manufactured by Daicel), EOCN-1020 (manufactured by Nippon Kayaku), EPICLON N-695 (manufactured by DIC), and CELLOXIDE 2021P (manufactured by Daicel). Examples of the epoxy group-containing compound include the compounds described in paragraphs 0034 to 0036 of JP 2013-011869 A, paragraphs 0147 to 0156 of JP 2014-043556 A, and paragraphs 0085 to 0092 of JP 2014-089408 A. The contents of these compounds are incorporated herein by reference.

[0212] The content of the thermally crosslinkable compound in the curable composition is not particularly limited, but is preferably 0.001 to 10 mass%, more preferably 0.01 to 8 mass%, and even more preferably 0.01 to 6 mass%, relative to the total solid content in the curable composition. One type of thermally crosslinkable compound may be used alone, or two or more types may be used. When the curable composition contains two or more types of thermally crosslinkable compounds, the total content thereof is preferably within the above range.

[0213] <Surfactant> The curable composition 1 may contain a surfactant. Examples of the surfactant include silicone surfactants, fluorine surfactants, nonionic surfactants, cationic surfactants, and anionic surfactants. Among these, silicone surfactants are preferred because they provide better effects of the present invention.

[0214] Examples of silicone surfactants include linear polymers composed of siloxane bonds, and modified siloxane polymers having organic groups introduced into side chains and / or terminals. As a preferred embodiment of the silicone surfactant, aromatic group-modified silicone surfactants (silicone surfactants having an aromatic group) are preferred, and phenyl-modified silicone surfactants (silicone surfactants having a phenyl group) are more preferred, in terms of achieving better effects of the present invention.

[0215] The content of the surfactant in the curable composition is not particularly limited, but is preferably 0.001 to 2.0 mass%, more preferably 0.005 to 0.5 mass%, and even more preferably 0.01 to 0.1 mass%, relative to the total solid content of the curable composition. One surfactant may be used alone, or two or more surfactants may be used in combination. When two or more surfactants are used in combination, the total amount is preferably within the above range.

[0216] <Solvent> The curable composition 1 may contain a solvent. The solvent is not particularly limited, and known solvents can be used, for example, organic solvents and water.

[0217] Examples of organic solvents include acetone, methyl ethyl ketone, cyclohexane, ethylene dichloride, tetrahydrofuran, toluene, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol dimethyl ether, 1-methoxy-2-propanol (propylene glycol monomethyl ether, PGME), propylene glycol monoethyl ether, acetylacetone, cyclohexanone, cyclopentanone, diacetone alcohol, ethylene glycol monomethyl ether acetate, ethylene glycol ethyl ether acetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether acetate, 3-methoxypropanol, Examples of the solvent include, but are not limited to, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether acetate (PGMEA), propylene glycol monoethyl ether acetate, 3-methoxypropyl acetate, N,N-dimethylformamide, dimethyl sulfoxide, γ-butyrolactone, ethyl acetate, butyl acetate, methyl lactate, N-methyl-2-pyrrolidone, ethyl lactate, 3-methoxybutanol, 1,3-butanediol, 2,3-butanediol, propylene glycol, ethylene glycol, dimethyl sulfoxide, and γ-valerolactone.

[0218] The content of the solids in the curable composition is preferably 10 to 90% by mass, more preferably 10 to 50% by mass, and even more preferably 15 to 30% by mass, relative to the total mass of the curable composition. The solvent may be used alone or in combination of two or more. When two or more solvents are used in combination, it is preferable to adjust the total solids content of the curable composition to be within the above range.

[0219] <Other Optional Components> The curable composition 1 may further contain optional components other than the components described above. Examples include a silane coupling agent, an ultraviolet absorber, a polymerization inhibitor, a sensitizer, a co-sensitizer, a crosslinking agent, a curing accelerator, a filler, a thermal curing accelerator, a plasticizer, a diluent, and an oil sensitizer. Furthermore, known additives such as an adhesion promoter to the substrate surface and other auxiliaries (e.g., conductive particles, fillers, antifoaming agents, flame retardants, leveling agents, release accelerators, antioxidants, fragrances, surface tension modifiers, and chain transfer agents) may be added as needed. These components can be found, for example, in paragraphs 0183 to 0228 of JP 2012-003225 A (corresponding paragraphs 0237 to 0309 of U.S. Patent Application Publication No. 2013 / 0034812), paragraphs 0101 to 0102, 0103 to 0104, and 0107 to 0109 of JP 2008-250074 A, and paragraphs 0159 to 0184 of JP 2013-195480 A, the contents of which are incorporated herein by reference.

[0220] The curable composition 1 preferably has a low content of particles with large particle diameters. More specifically, in the particle size distribution (volume basis) obtained by measuring the curable composition 1 with a particle size distribution analyzer, the proportion of particles with a particle diameter of 200 nm or more (hereinafter simply referred to as "specific particles") is preferably 5% or less. In particular, the proportion of specific particles is more preferably 3% or less, and even more preferably 1% or less. The lower limit is not particularly limited, but may be 0%. The particle size distribution can be measured, for example, by using a particle size distribution analyzer Nanotrac UPA (manufactured by Microtrac-Bell) to measure the curable composition or a measurement solution obtained by diluting the curable composition with a solvent (such as propylene glycol monomethyl ether acetate) to an arbitrary concentration (such as 1% by mass). Examples of particles measured with the particle size distribution analyzer include the above-mentioned colorants in particulate form (colorant particles) and fillers other than colorants.

[0221] [Method for Producing Curable Composition 1] The method for producing the curable composition 1 is not particularly limited. However, it is preferable to produce a dispersion composition in which a pigment is dispersed, and then mix the resulting dispersion composition with other components to form a composition. The dispersion composition is preferably prepared by mixing the pigment, resin A, and a solvent. It is also preferable to add a polymerization inhibitor to the dispersion composition. The dispersion composition can be prepared by mixing the above components using a known mixing method (e.g., a mixing method using a stirrer, homogenizer, high-pressure emulsifier, wet grinder, or wet disperser). After preparing the dispersion composition, the dispersion composition, resin B, a polymerizable compound, and other optional components can be mixed to prepare the curable composition. When preparing the curable composition, the components may be blended together, or each component may be dissolved or dispersed in a solvent and then blended sequentially. The order of addition and working conditions during blending are not particularly limited.

[0222] The curable composition 1 is preferably filtered through a filter for the purposes of removing foreign matter and reducing defects. The pore size of the filter is preferably 0.1 to 7.0 μm, more preferably 0.2 to 2.5 μm, even more preferably 0.2 to 1.5 μm, and particularly preferably 0.3 to 0.7 μm. Within this range, it is possible to reliably remove fine foreign matter, such as impurities and aggregates contained in the pigment, while suppressing clogging of the pigment (including the black pigment).

[0223] The curable composition 1 preferably does not contain impurities such as metals, halogen-containing metal salts, acids, and alkalis. The content of impurities contained in these materials is preferably 1 ppm by mass or less, more preferably 1 ppb by mass or less, even more preferably 100 ppt by mass or less, particularly preferably 10 ppt by mass or less, and most preferably substantially none (below the detection limit of the measuring device). The impurities can be measured using an inductively coupled plasma mass spectrometer (Agilent 7500cs, manufactured by Yokogawa Analytical Systems).

[0224] [Procedure for Step 1] Step 1 is a step of forming a curable composition layer on a support using the curable composition 1. The support is preferably a substrate having an alignment mark that serves as a reference for aligning the support and the exposure mask. When a substrate having an alignment mark is used as the support, the curable composition layer may be formed on the substrate so as to cover the alignment mark. In other words, the curable composition layer may be formed on the alignment mark. Examples of the substrate include glass substrates, silicon substrates (which may have been subjected to a hydrophobic treatment with hexamethyldisilazane, etc.), and solid-state imaging device substrates in which an imaging device (light-receiving device) such as a CCD (Charge Coupled Device) or a CMOS (Complementary Metal-Oxide Semiconductor) is provided on the silicon substrate. Furthermore, if necessary, a primer layer may be provided on the support to improve adhesion with upper layers, prevent diffusion of substances, flatten the substrate surface, etc.

[0225] Examples of methods for applying the curable composition to a support include various coating methods such as slit coating, inkjet coating, rotary coating (spin coating), casting coating, roll coating, and screen printing. The film thickness of the composition layer is preferably 0.1 to 10 μm, more preferably 0.2 to 5 μm, and even more preferably 0.2 to 3 μm. The composition layer coated on the support is preferably dried (prebaked) by heating. Prebaking can be performed, for example, using a hot plate or an oven. In terms of achieving better effects of the present invention, the prebaking temperature is preferably 50 to 140°C, more preferably 60 to 120°C, and even more preferably 70 to 100°C. In terms of achieving better effects of the present invention, the prebaking time is preferably 10 to 300 seconds, more preferably 60 to 240 seconds, and even more preferably 80 to 200 seconds. When at least one of the heating temperature and heating time is within the above range, the visibility of alignment marks and the like is not hindered, and therefore, alignment of the support and the exposure mask can be easily performed in step 2 described below.

[0226] The surface roughness of the curable composition layer obtained in step 1 is preferably within an appropriate range, since it does not interfere with the visibility of alignment marks and the like and allows for easy mask positioning during exposure. More specifically, the arithmetic mean surface roughness Ra(a), mean element length Rsm(a), and root-mean-square slope RΔq(a) of the curable composition layer obtained in step 1 are preferably within appropriate numerical ranges. Herein, Ra(a), Rsm(a), and RΔq(a) represent values ​​measured in accordance with JIS-B-0601:2013. Ra(a) is preferably 0.00 to 0.05 μm, more preferably 0.00 to 0.02 μm. Rsm(a) is preferably 3 to 200 μm, more preferably 5 to 100 μm. RΔq(a) is preferably 0.0 to 3.5°, more preferably 0.0 to 1.0°.

[0227] [Step 2] Step 2 is a step of aligning the support on which the curable composition layer has been formed in Step 1 with an exposure mask. By performing this step, the relative positional relationship between the support and the exposure mask is adjusted, so that a predetermined position of the curable composition layer is exposed during the exposure described below. Aligning the support with the exposure mask can be achieved using an alignment mark. For example, as described above, a method can be used in which a substrate having an alignment mark is used as the support, and the support and the exposure mask are aligned based on the alignment mark. As described above, the curable composition layer may be formed on an alignment mark. The shape of the alignment mark is not particularly limited, and examples include those shown in FIGS. 1 and 2. FIG. 1 shows a schematic plan view of an alignment mark. FIG. 2 is a schematic cross-sectional view taken along line A-A in FIG. 1. The alignment mark 10 shown in FIGS. 1 and 2 is disposed on a support 18. The alignment mark 10 has a square frame 12 and a cross-shaped mark formed by two intersecting lines (a vertical line 14 and a horizontal line 16) disposed inside the frame 12. In Fig. 1, L1 indicates the length of one side of the outer periphery of the frame 12, which may be, for example, about 60 µm. In Fig. 2, H1 indicates the height of the frame 12, which may be 0.6 µm.

[0228] The procedure for aligning the support and the exposure mask is not particularly limited, and known methods can be used. For example, the position of the alignment mark may be detected visually, by an optical microscope, or by image processing using an optical sensor or a camera, and the exposure mask may be aligned based on that position.

[0229] [Step 3] Step 3 is a step of exposing the curable composition layer through an exposure mask aligned in step 2 above. Specifically, the exposure treatment is a step of exposing the composition layer formed in step 1 above to actinic rays or radiation, thereby curing the light-exposed areas of the composition layer. There are no particular restrictions on the exposure mask, but it is preferable to irradiate with light through a photomask having patterned openings. Exposure is preferably carried out by irradiation with radiation, and examples of radiation that can be used for exposure include ultraviolet rays such as g-rays, h-rays, and i-rays, and a high-pressure mercury lamp is preferred as the light source. The irradiation intensity is 5 to 1500 mJ / cm. 2 is preferred, and 10 to 1000 mJ / cm 2 is more preferred.

[0230] [Step 4] Step 4 is a step in which the exposed curable composition layer is subjected to a development treatment to form a patterned cured film. This step dissolves the composition layer in the light-exposed areas in the exposure step, leaving only the photocured portions. The type of developer used in the development step is not particularly limited, but an alkaline developer is desirable as it does not damage the underlying imaging element, circuits, etc. The development temperature is preferably 20 to 30°C. The development time is preferably 20 to 90 seconds. In order to further remove residue, development is sometimes carried out for 120 to 180 seconds in recent years. Furthermore, to further improve residue removal, the process of shaking off the developer every 60 seconds and then supplying fresh developer may be repeated several times.

[0231] The alkaline developer is preferably an alkaline aqueous solution prepared by dissolving an alkaline compound in water to a concentration of 0.001 to 10% by mass (preferably 0.01 to 5% by mass). Examples of alkaline compounds include sodium hydroxide, potassium hydroxide, sodium carbonate, sodium silicate, sodium metasilicate, aqueous ammonia, ethylamine, diethylamine, dimethylethanolamine, tetramethylammonium hydroxide, tetraethylammonium hydroxide, tetrapropylammonium hydroxide, tetrabutylammonium hydroxide, benzyltrimethylammonium hydroxide, choline, pyrrole, piperidine, and 1,8-diazabicyclo[5.4.0]-7-undecene (among these, organic alkalis are preferred). When an alkaline developer is used, it is generally preferred to perform a rinse treatment with water or the like after development.

[0232] [Step 5] Step 5 is a step of subjecting the patterned cured film obtained in Step 4 to a heat treatment (post-baking). This step completely cures the polymerizable compound in the curable composition, and the curing shrinks, forming a fine uneven structure on the surface of the cured film, thereby obtaining a film with excellent anti-reflection properties. The lower limit of the heating temperature for post-baking is preferably 100°C or higher, more preferably 150°C or higher, even more preferably 200°C or higher, particularly preferably 220°C or higher, and most preferably 240°C or higher. The upper limit of the heating temperature for post-baking is preferably 300°C or lower, more preferably 260°C or lower. Post-baking can be performed continuously or batchwise using a heating means such as a hot plate, a convection oven (hot air circulation dryer), or a high-frequency heater. In particular, post-baking is preferably performed using a hot plate.

[0233] Post-baking is preferably carried out in an atmosphere with a low oxygen concentration. The oxygen concentration is preferably 19% by volume or less, more preferably 15% by volume or less, even more preferably 10% by volume or less, particularly preferably 7% by volume or less, and most preferably 3% by volume or less. There is no particular lower limit, but a concentration of 10 ppm by volume or more is practical.

[0234] [[Method for Producing Cured Film (Second Embodiment)]] The second embodiment of the present production method will be described in detail below. The second embodiment of the present production method has steps 11 to 14. Each step will be described in detail below.

[0235] [Step 11] Step 11 is a step of forming a curable composition layer on a support, the curable composition including a resin C, a resin H, and a polymerizable compound, and the HSP distance between the resin C and the resin H is 1.5 MPa. 1/2 and the ratio T2 / T1 of the dissolution rate T2 of resin H in the developer used in the development treatment to the dissolution rate T1 of resin C in the developer is 10.0 or more. The curable composition used in step 11 (hereinafter also referred to as "curable composition 2") and the procedure will be described in detail below.

[0236] [Curable composition 2] Curable composition 2 contains resin C, resin H, and a polymerizable compound. The HSP distance between resin C and resin H is 1.5 MPa. 1/2 and the ratio T2 / T1 of the dissolution rate T2 of resin H in the developer used in the development process to the dissolution rate T1 of resin C in the developer is 10.0 or more.

[0237] The definition and calculation method of the HSP distance are as described in detail for the HSP distance between resin A and resin B contained in curable composition 1. The HSP distance between resin C and resin H is 1.5 MPa. 1/2 The technical significance of "over" is that the HSP distance between resin A and resin B is 1.5 MPa. 1/2 The technical significance of being super has already been explained.

[0238] <Resin C> The curable composition 2 contains resin C. Resin C is not particularly limited as long as it satisfies the above-mentioned relationship between the HSP distance and the dissolution rate with resin H. Resin C preferably contains at least one of a repeating unit C1 having an acid group and a repeating unit C2 having at least one of a polyoxyalkylene group having an average number of additions of 3 or more and a polyoxyalkylenecarbonyl group having an average number of additions of 3 or more, and more preferably contains both repeating units C1 and C2. Specific embodiments and preferred embodiments of repeating units C1 and C2, as well as the preferred content of each repeating unit relative to the total repeating units of resin C, are the same as those of repeating units A1 and A2. In particular, the content of repeating unit C2 is preferably 35% by mass or more relative to the total repeating units of resin C. Resin C may also contain the repeating unit A3, and the preferred content of repeating unit A3 relative to the total repeating units of resin C is the same as that of resin A.

[0239] The HSP distance between resin C and resin H is 1.5 MPa. 1/2 There is no particular limitation as long as it is greater than 1.5 MPa. 1/2 Over 5.0 MPa 1/2 The following is preferable, 2.0 to 4.0 MPa 1/2 The dispersion term (δ) of the Hansen solubility parameter of Resin C is more preferably d ), polar term (δ p ) and the hydrogen bond term (δ h The preferred ranges of the Hansen solubility parameters of resin A and resin B are (δ d ), polar term (δ p ) and the hydrogen bond term (δ h The dispersion term (δ) of the Hansen solubility parameter of resin H is the same as the preferred range of d ), polar term (δ p ) and the hydrogen bond term (δ h The preferred ranges of the solubility parameters (δ) of the Hansen solubility parameter of the resin B are d ), polar term (δ p ) and the hydrogen bond term (δ h ) is the same as the preferred range of

[0240] As described above, the ratio T2 / T1 of the dissolution rate T2 (μm / sec) of resin H in the developer used in the development process to the dissolution rate T1 (μm / sec) of resin C in the developer is 10.0 or more. In order to achieve better effects of the present invention, the ratio T2 / T1 is preferably 12.0 or more, more preferably 15.0 or more. There is no particular upper limit, but it is preferably 25.0 or less. When the ratio T2 / T1 is within the above range, resin H is more easily developed relative to resin C in step 14, making it easier to form a fine uneven structure in the cured film, and a cured film with excellent low reflectivity can be obtained. T1 and T2 are values ​​obtained by the following procedure.

[0241] (Measurement of Dissolution Rate) Resin C or Resin H was diluted with PGMEA to a solid content of 30% by mass, then coated on a silicon wafer using a spin coater, and heated at 90°C for 2 minutes to dry the organic solvent, yielding a resin film with a thickness of 10 μm. Next, the resin film was immersed for 60 seconds in the developer (25°C) used in the development treatment of step 4 described below, and the film thickness after immersion was measured with a film thickness meter. From the obtained measurement results, the dissolution rate of the resin was calculated based on the following formula (T): Dissolution rate (μm / sec) = Film thickness change (μm) / Development time (sec) ... formula (T)

[0242] In order to obtain a more excellent effect of the present invention, the acid value of Resin C is preferably 50 mgKOH / g or more, more preferably 55 mgKOH / g or more, and even more preferably 60 mgKOH / g or more. The upper limit is preferably 200 mgKOH / g or less, more preferably 170 mgKOH / g or less, even more preferably 100 mgKOH / g or less, and particularly preferably 80 mgKOH / g or less. Note that a resin having a desired acid value can be obtained by changing the content of repeating units containing an acid group, which are a constituent component of Resin C.

[0243] The weight average molecular weight of Resin C is preferably 5,000 to 100,000, more preferably 6,000 to 80,000, even more preferably 15,000 to 40,000, and most preferably 20,000 to 40,000.

[0244] The content of resin C in curable composition 2 is not particularly limited, but is preferably 2 to 40 mass %, more preferably 5 to 30 mass %, and even more preferably 10 to 25 mass %, relative to the total solid content of the curable composition. Resin C may be used alone or in combination of two or more types. When two or more types of resin A are used in combination, it is preferable that the total content is within the above range.

[0245] <Resin H> The curable composition 2 contains Resin H. Resin H is not particularly limited as long as it satisfies the above-mentioned relationship between the HSP distance and the dissolution rate with Resin C, but is preferably an acrylic or methacrylic resin having an acid value that is 70 mgKOH / g or more higher than the acid value of Resin C. It is also preferable that Resin H does not contain a repeating unit having a group selected from the group consisting of polyoxyalkylene groups having an average addition number of 3 or more and polyoxyalkylenecarbonyl groups having an average addition number of 3 or more.

[0246] Resin H preferably contains a repeating unit B3 having a carboxylic acid group, and more preferably contains a repeating unit B3 having a carboxylic acid group and at least one repeating unit selected from the group consisting of a repeating unit B1 derived from an alkyl (meth)acrylate and a repeating unit B4. Resin H may also contain a repeating unit B2. Specific and preferred embodiments of repeating units B1 to B4 are as described in detail for Resin B.

[0247] In Resin H, the repeating unit B1 is preferably a repeating unit derived from alkyl(meth)acrylate, in which the alkyl moiety in the alkyl(meth)acrylate has 1 to 4 carbon atoms. In Resin H, the repeating unit B3 is preferably a repeating unit derived from acrylic acid. In Resin H, the repeating unit B4 is preferably a repeating unit derived from benzyl(meth)acrylate.

[0248] When Resin H contains the repeating unit B1, the content of the repeating unit B1 is preferably 10% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total repeating units of Resin H. The upper limit is not particularly limited, but is preferably 99% by mass or less, more preferably 95% by mass or less.

[0249] When Resin H contains repeating unit B3 having a carboxylic acid group, the content of repeating unit B3 having a carboxylic acid group is preferably 15 to 50 mass %, and more preferably 20 to 40 mass %, based on all repeating units of Resin H. When Resin H contains repeating unit B4, the content of repeating unit B4 is preferably 0 to 80 mass %, and more preferably 0 to 75 mass %, based on all repeating units of Resin H.

[0250] In terms of achieving better effects of the present invention, the acid value of resin H is preferably higher than the acid value of resin C. Specifically, the acid value of resin H is preferably 70 mgKOH / g or more higher than the acid value of resin C, more preferably 100 mgKOH / g or more higher, and even more preferably 120 mgKOH / g or more higher. Furthermore, the difference between the acid value of resin H and the acid value of resin C (acid value of resin H - acid value of resin C) is preferably 200 mgKOH / g or less. In terms of achieving better effects of the present invention, the acid value of resin H is preferably 140 mgKOH / g or more, more preferably 160 mgKOH / g or more, and even more preferably 180 mgKOH / g or more. The upper limit is preferably 250 mgKOH / g or less, more preferably 230 mgKOH / g or less, and even more preferably 200 mgKOH / g or less. A resin having a desired acid value can be obtained by changing the content of repeating units containing an acid group, which are a component of resin H.

[0251] The weight average molecular weight of Resin H is preferably 5,000 to 100,000, more preferably 8,000 to 80,000, still more preferably 15,000 to 40,000, and particularly preferably 18,000 to 25,000.

[0252] The content of resin H in curable composition 2 is not particularly limited, but is preferably 2 to 40% by mass, more preferably 5 to 35% by mass, and even more preferably 10 to 30% by mass, relative to the total solid content of the curable composition. Furthermore, in terms of more excellent effects of the present invention, the ratio of the content of resin C to the total content of resin C and resin H in curable composition 2 (content of resin C / total content of resin C and resin H) is preferably 0.30 to 0.50, more preferably 0.33 to 0.47, and even more preferably 0.35 to 0.45. Resin H may be used alone or in combination of two or more types. When two or more types of resin H are used in combination, it is preferable that the total content is within the above range.

[0253] Specific aspects and preferred aspects of each component contained in curable composition 2 other than resin C and resin H, and each component that may be contained, are the same as the specific aspects and preferred aspects of each component contained in curable composition 1, and each component that may be contained.

[0254] The curable composition 2 preferably has a low content of particles with large particle diameters. More specifically, in the particle size distribution (volume basis) obtained by measuring the curable composition 2 with a particle size distribution analyzer, the proportion of particles with a particle diameter of 200 nm or more (hereinafter also simply referred to as "specific particles") is preferably 5% or less. In particular, the proportion of specific particles is more preferably 3% or less, and even more preferably 1% or less. The lower limit is not particularly limited, but may be 0%. The particle size distribution can be measured, for example, by using a particle size distribution analyzer Nanotrac UPA (manufactured by Microtrac-Bell) to measure the curable composition or a measurement solution obtained by diluting the curable composition with a solvent (such as propylene glycol monomethyl ether acetate) to an arbitrary concentration (such as 1% by mass). Examples of particles measured with the particle size distribution analyzer include the above-mentioned colorants in particulate form (colorant particles) and fillers other than colorants.

[0255] [Method of producing curable composition 2] The method of producing the curable composition 2 is not particularly limited, and the same method as the method of producing the curable composition 1 may be used.

[0256] [Procedure of Step 11] Step 11 is a step of forming a curable composition layer on a support using the curable composition 2. The support may be the same as the support used in Step 1. The specific procedure may be the same as the procedure of Step 1.

[0257] [Step 12] Step 12 is a step of aligning an exposure mask with the support on which the curable composition layer has been formed in step 11. The specific procedure of step 12 can be performed in the same manner as the procedure of step 2 described above.

[0258] [Step 13] Step 13 is a step of exposing the curable composition layer through the exposure mask aligned in the above-mentioned step 12. The specific procedure of step 13 can be performed in the same manner as the procedure of the above-mentioned step 3.

[0259] [Step 14] Step 14 is a step of developing the exposed curable composition layer to form a patterned cured film. The specific procedure of Step 14 can be performed in the same manner as the procedure of Step 4 described above.

[0260] [Other Steps] The second embodiment of the present manufacturing method may include other steps. Examples of such other steps include a post-baking step. Performing the post-baking step after step 14 above improves the strength of the cured film, which is preferable. The post-baking step is preferably performed under the same conditions as step 5 above.

[0261] [Physical Properties of Cured Film] The physical properties of the cured film obtained by this production method are described in detail below. In order to have excellent antireflection properties (low reflectivity), the cured film preferably has an average specular reflectance of light with a wavelength of 400 to 700 nm per 3.5 μm of film thickness when light of 350 to 1200 nm is incident thereon, of less than 5%, more preferably less than 3%, and even more preferably less than 1%. The lower limit is not particularly limited, but is generally 0% or greater. More specifically, the average specular reflectance is preferably less than 2.0% when the incident angle is 5°, preferably less than 5% when the incident angle is 45°, and preferably less than 10% when the incident angle is 60°. As a method for measuring the average value of the reflectance of the light-shielding film, for example, a light-shielding film is formed on a glass substrate, and a spectrometer (for example, the VAR unit of the V7200 spectrometer manufactured by JASCO Corporation) is used to obtain a specular reflectance spectrum for an arbitrary angle of incidence (for example, 5°, 45°, or 60°), and the average value of the reflectance in the wavelength region of 400 to 700 nm is determined.

[0262] Furthermore, in order to achieve the above-mentioned low reflectivity, it is preferable that the surface roughness of the cured film be within an appropriate range. More specifically, it is preferable that the arithmetic mean surface roughness Ra(b), mean element length Rsm(b), and root mean square slope RΔq(b) of the cured film be within appropriate numerical ranges. In this specification, Ra(b), Rsm(b), and RΔq(b) represent values ​​measured in accordance with JIS-B-0601:2013. Ra(b) is preferably 0.06 to 0.50 μm, more preferably 0.15 to 0.30 μm. Furthermore, in terms of more excellent effects of the present invention, the difference between Ra(a) and Ra(b) (Ra(b) - Ra(a)) is preferably 0.05 to 0.30 μm. Rsm(b) is preferably 1 to 50 μm, more preferably 2 to 30 μm. RΔq(b) is preferably 3 to 25°, and more preferably 5 to 10°. In terms of better effects of the present invention, the difference between RΔq(a) and RΔq(b) (RΔq(b)−RΔq(a)) is preferably 3 to 15°.

[0263] The thickness of the cured film is, for example, preferably 0.1 to 6.0 μm, more preferably 1.0 to 5.0 μm, and even more preferably 1.0 to 3.5 μm. The cured film may be thinner or thicker than this range depending on the application.

[0264] The cured film obtained by the cured film manufacturing method of the present invention is preferably used as a light-shielding film. In order to have excellent light-shielding properties, the light-shielding film obtained by the cured film manufacturing method of the present invention preferably has an optical density (OD) per 3.5 μm film thickness in the wavelength range of 400 to 1100 nm of more than 2.0, more preferably 2.5 or more, and even more preferably 3.0 or more. The upper limit is not particularly limited, but is generally preferably 10 or less. In this specification, an optical density per 3.5 μm film thickness in the wavelength range of 400 to 1100 nm of 3.0 or more means an optical density per 3.5 μm film thickness of 3.0 or more over the entire wavelength range of 400 to 1100 nm. The optical density of the light-shielding film can be measured by first forming the light-shielding film on a glass substrate and then measuring the optical density using a spectrophotometer (e.g., U-4100 manufactured by Hitachi High-Technologies Corporation).

[0265] <Solid-state imaging element and solid-state imaging device> The cured film can be suitably used as a light-shielding film in a solid-state imaging element. The solid-state imaging element may include any of a variety of light-shielding elements, including a substrate having a plurality of photodiodes and light-receiving elements made of polysilicon or the like that constitute the light-receiving area of ​​the solid-state imaging element (e.g., a CCD image sensor, a CMOS image sensor, etc.), and a light-shielding film on the light-receiving element-forming side of the support (e.g., a portion other than the light-receiving portion and / or color-adjusting pixels, etc.) or on the opposite side of the forming surface. Furthermore, when the light-shielding film is used as a light-attenuating film, the dynamic range of the solid-state imaging element can be improved by arranging the light-attenuating film so that a portion of light passes through the light-attenuating film before entering the light-receiving element. A solid-state imaging device includes the solid-state imaging element.

[0266] <Image display device> The light-shielding film is also preferably applied to an image display device. In other words, the image display device of the present invention is an image display device having the light-shielding film of the present invention. An example of a form in which an image display device has a light-shielding film is a form in which a color filter having a black matrix including the light-shielding film is applied to the image display device. Next, a black matrix and a color filter including a black matrix will be described, and further, as a specific example of an image display device, a liquid crystal display device including such a color filter will be described.

[0267] (Black Matrix) The light-shielding film is preferably included in a black matrix. The black matrix may be included in image display devices such as color filters, solid-state imaging devices, and liquid crystal display devices. Examples of black matrices include those already described above: black borders provided on the periphery of image display devices such as liquid crystal display devices; grid-like and / or stripe-like black portions between red, blue, and green pixels; and dot-like and / or line-like black patterns for TFT (thin film transistor) light shielding. The definition of this black matrix is ​​described, for example, in "Liquid Crystal Display Manufacturing Equipment Terminology Dictionary," second edition, by Taihei Kanno, published by Nikkan Kogyo Shimbun, Inc., 1996, p. 64. The black matrix preferably has high light-shielding properties (optical density OD of 3 or more) to improve display contrast and, in the case of active-matrix-driven liquid crystal display devices using thin film transistors (TFTs), to prevent image quality degradation due to light current leakage.

[0268] The method for producing the black matrix is ​​not particularly limited, and it can be produced by the same method as the method for producing the light-shielding film described above. Specifically, a curable composition is applied to a substrate to form a composition layer, which is then exposed to light and developed to produce a patterned light-shielding film (black matrix). The film thickness of the light-shielding film (black matrix) is preferably 0.1 to 4.0 μm.

[0269] The substrate is not particularly limited, but preferably has a transmittance of 80% or more for visible light (wavelength 400 to 800 nm). Materials for such a substrate include, for example, glass such as soda lime glass, alkali-free glass, quartz glass, and borosilicate glass; and plastics such as polyester resins and polyolefin resins. From the viewpoint of chemical resistance and heat resistance, alkali-free glass or quartz glass is preferred.

[0270] (Color Filter) The light-shielding film is preferably included in a color filter. The form of the color filter including the light-shielding film is not particularly limited, but may be a color filter including a substrate and the black matrix. That is, an example of a color filter is a color filter including red, green, and blue colored pixels formed in openings of the black matrix formed on the substrate.

[0271] A color filter including a black matrix can be manufactured, for example, by the following method. First, a coating film (composition layer) of a curable composition containing a pigment corresponding to each color pixel of the color filter is formed in the openings of a patterned black matrix formed on a substrate. The compositions for each color are not particularly limited, and known compositions can be used. However, it is preferable to use a composition in which the black pigment in the composition described herein is replaced with a colorant corresponding to each pixel. Next, the composition layer is exposed to light through a photomask having a pattern corresponding to the openings of the black matrix. The unexposed portions are then removed by development, and the resulting layer is baked to form color pixels in the openings of the black matrix. By performing this series of operations using color compositions containing, for example, red, green, and blue pigments, a color filter having red, green, and blue pixels can be manufactured.

[0272] (Liquid Crystal Display Device) The light-shielding film is also preferably included in a liquid crystal display device. The liquid crystal display device may include a color filter including the black matrix (light-shielding film) as described above, although the embodiment is not particularly limited.

[0273] The liquid crystal display device may have, for example, a pair of substrates arranged opposite to each other and a liquid crystal compound sealed between the substrates. The substrates are as already described as the substrates for the black matrix.

[0274] A specific example of the liquid crystal display device is a laminate including, from the user's side, a polarizing plate / substrate / color filter / transparent electrode layer / alignment film / liquid crystal layer / alignment film / transparent electrode layer / TFT (Thin Film Transistor) element / substrate / polarizing plate / backlight unit in this order.

[0275] The liquid crystal display device is not limited to the above, and examples thereof include the liquid crystal display devices described in "Electronic Display Devices" (written by Akio Sasaki, published by Kogyo Chosakai Co., Ltd. in 1990) and "Display Devices" (written by Nobuaki Ibuki, published by Sangyo Tosho Co., Ltd. in 1989). Further examples thereof include the liquid crystal display devices described in "Next Generation Liquid Crystal Display Technology" (edited by Tatsuo Uchida, published by Kogyo Chosakai Co., Ltd. in 1994).

[0276] <Infrared Sensor> The light-shielding film is preferably included in the infrared sensor. Next, a solid-state imaging device to which the infrared sensor is applied will be described. The solid-state imaging device includes a lens optical system, a solid-state imaging element, an infrared light-emitting diode, and the like. Note that for each configuration of the solid-state imaging device, reference can be made to paragraphs 0032 to 0036 of Japanese Patent Laid-Open No. 2011-233983, the contents of which are incorporated herein by reference.

[0277] <Cover Glass, Optical Filter> The light-shielding film is also preferably used in optical filters and cover glasses incorporated into solid-state imaging devices. Examples of optical filters include IR cut filters. Forming this light-shielding film around the periphery of the optical filter or cover glass can suppress the occurrence of flare and ghosting. For the configurations of the optical filter with the light-shielding film and the solid-state imaging device, see paragraphs 0009 to 0012 of Japanese Patent Application Laid-Open No. 2014-132333, and for the configurations of the cover glass with the light-shielding film and the solid-state imaging device, see paragraphs 0017 to 0020, 0037, and 0040 of Japanese Patent Application Laid-Open No. 2021-092605, the contents of which are incorporated herein by reference.

[0278] The present invention will be described in more detail below with reference to the following examples. The materials, amounts used, ratios, treatment details, and treatment procedures shown in the following examples can be changed as appropriate without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be construed as being limited by the following examples.

[0279] [Preparation and Evaluation of Curable Compositions] [Various Components Used in Preparation of Curable Compositions] The components used in preparation of the curable compositions used in each evaluation will be described in detail below.

[0280] [Resin A] Table 1 shows the composition and properties of Resin A (Resins A-1 to A-10). Resins A-1 to A-10 were synthesized. An example of the synthesis of Resin A-1 is shown below. Resins A-2 to A-10 were synthesized using the same procedure as in the synthesis example of Resin A-1, except that the types and blending ratios of the raw material monomers were changed.

[0281] <Synthesis of Resin A-1> 20.0 g of methacrylic acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 130.0 g of PME-1000 (manufactured by NOF Corporation), and 50.0 g of benzyl methacrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) were added to 233% by mass of propylene glycol monomethyl ether acetate relative to the total mass of the raw material monomers, and the mixture was heated to 80°C under a nitrogen stream. Next, 2 mol% of dodecanethiol relative to the total mass of the raw material monomers and 0.5% by mass of a thermal polymerization initiator (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., V-601) relative to the total mass of the raw material monomers were added, and the mixture was stirred for 2 hours. Next, 0.5% by mass of a thermal polymerization initiator (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., V-601) relative to the total mass of the raw material monomers was added, and the mixture was stirred for another 2 hours. Thereafter, 0.5% by mass of a thermal polymerization initiator (V-601 manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) was added relative to the total mass of the raw material monomers, and the mixture was heated to 90°C and stirred for 2 hours to synthesize Resin A-1.

[0282] The weight average molecular weights of resins A-1 to A-10 were in the range of 13,000 to 45,000. Table 1 is shown below. Table 1 is composed of Table 1 (Part 1) and Table 1 (Part 2). For example, resin A-1 contains the repeating unit A1 and repeating unit A2 described in Table 1 (Part 1), and the repeating unit A3 described in Table 1 (Part 2). In Table 1, the "Content (mass%)" column indicates the content (mass%) of each repeating unit relative to the total repeating units. In Table 1, the numerical values ​​of the dispersion term (δd), polar term (δp), and hydrogen bond term (δh) of each resin listed in the "HSP" column are values ​​calculated at 25°C using HSPiP ver. 5.4.08 (sold by Eizou Kobo Question Co., Ltd.) as described above. In Table 1, the glass transition temperatures shown in the "Tg (°C)" column were measured using a differential scanning calorimetry (DSC) device (DSC 3500 Sirius, manufactured by Netzsch). The values ​​shown in the "Dissolution rate T1 (µm / sec)" column in Table 1 were measured using the following procedure.

[0283] (Measurement of Dissolution Rate) The dissolution rate of each resin was measured as follows. First, the obtained resin was diluted with PGMEA so that the solid content was 30% by mass, and then coated on a silicon wafer using a spin coater. The organic solvent was dried by heating at 90°C for 2 minutes to obtain a resin film with a film thickness of 10 μm. Next, the resin film was immersed in an alkaline developer CD-2000 (manufactured by FUJIFILM Electronic Materials Co., Ltd.) at 25°C for 60 seconds, and the film thickness after immersion was measured with a film thickness meter. From the obtained measurement results, the dissolution rate of the resin was calculated based on the following formula (T). Note that the alkaline developer CD-2000 (manufactured by FUJIFILM Electronic Materials Co., Ltd.) is a developer used in the development process, as described below. Dissolution rate (μm / sec) = film thickness change (μm) / development time (sec) Formula (T)

[0284]

[0285]

[0286] [Resin B] Table 2 shows the structure of Resin B (Resins B-1 to B-12). Resins B-1 to B-12 were synthesized. An example of the synthesis of Resin B-1 is shown below. Resins B-2 to B-12 were synthesized using the same procedure as in the synthesis example of Resin B-1, except that the types and blending ratios of the raw material monomers were changed.

[0287] <Synthesis of Resin B-1> A raw material monomer solution was prepared by mixing 172.0 g of methyl methacrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), 20.0 g of methacrylic acid (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.), and 8.0 g of 2-hydroxyethyl methacrylate (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.). Furthermore, a mixed solution A was prepared by mixing 2 mol % of a thermal polymerization initiator (V-601, manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd.) relative to the total mass of the raw material monomers and 111 mass % of 1-methoxy-2-propanol relative to the total mass of the raw material monomers. Next, a mixed solution B was prepared using the raw material monomer mixed solution and 1-methoxy-2-propanol in an amount of 74% by mass relative to the total mass of the raw material monomers, and heated to 80°C. Then, mixed solution A was added dropwise to this mixed solution B over 2 hours (drop polymerization), and after the dropwise addition, the mixture was heated at 80°C for 2 hours and then at 90°C for 3 hours, thereby synthesizing resin B-1.

[0288] The weight average molecular weights of Resins B-1 to B-12 were in the range of 12,000 to 30,000. Table 2 is shown below. Table 2 is composed of Table 2 (Part 1) and Table 2 (Part 2). In Table 2, the "Content (% by mass)" column indicates the content (% by mass) of each repeating unit relative to all repeating units. The values ​​in the "HSP" and "Tg (°C)" columns in Table 2 were calculated or measured using the same procedures as for the values ​​in Table 1.

[0289]

[0290]

[0291] [Resin H] Table 3 shows the structures of Resin H (Resins H-1 to H-4). Table 3 is composed of Table 3 (Part 1) and Table 3 (Part 2). For example, Resin H-1 contains the repeating unit B3 described in Table 3 (Part 1) and the repeating unit B4 described in Table 3 (Part 2). Resins H-1 to H-4 were synthesized using the same procedure as in the synthesis example of Resin B-1, except that the types and blending ratios of raw material monomers were changed. In Table 3, the "Content (mass%)" column indicates the content (mass%) of each repeating unit relative to all repeating units. In Table 3, the values ​​listed in the "HSP" column, "Tg (°C)" column, and "Dissolution rate T2 (μm / sec)" column were calculated or measured using the same procedure as the values ​​listed in Table 1.

[0292]

[0293]

[0294] [Polymerizable Compounds] Polymerizable compounds (C-1 to C-6) are shown in Table 4. In Table 4, the values ​​shown in the "Shrinkage (%)" column were measured by the following procedure. Polymerizable compound C-1 in Table 4 was a mixture of two types of monomers, and the mass ratio of the compound on the left side to the compound on the right side (mass of the compound on the left side: mass of the compound on the right side) was 50:50.

[0295] (Measurement of Shrinkage Ratio) The shrinkage ratio of a polymerizable compound is determined by the specific gravity ρM (g / cm 3 ) and the specific gravity ρP (g / cm 3 ) was determined and calculated using the following formula: Shrinkage (%)=(1−ρM / ρP)×100. A cured product of the polymerizable compound was prepared by the method described below, and the specific gravities of the polymerizable compound and the cured product were measured in accordance with JIS-K-2249.

[0296] (Method for producing a cured product) A composition consisting of 0.5% by mass of a radical polymerization initiator (V-601: manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) and 99.5% by mass of a polymerizable compound was poured into a mold composed of a glass plate and a gasket made of an ethylene-vinyl acetate copolymer, and a cured product was produced by cast polymerization. The polymerization was carried out using an air oven, with the temperature gradually increased from 30 to 90°C over 18 hours, and then maintained at 90°C for 2 hours. After completion of the polymerization, the polymer was removed from the glass mold to obtain a cured product.

[0297]

[0298] [Coloring Materials] The coloring materials (D-1 to D-6) are as follows: D-1: TiON (titanium oxynitride) D-2: Spectrasense Black K0087 (perylene-based black pigment) D-3: Irgaphor Black SO100 (benzodifuranone-based black pigment) D-4: CB (carbon black) D-5: Pigment Red 177 D-6: Pigment Blue 60

[0299] [Photopolymerization initiator] The photopolymerization initiators (E-1 to E-3) are shown below. E-1: IRGACURE OXE02 (manufactured by BASF, oxime ester-based polymerization initiator) E-2: ADEKA ARCLES NCI-831E (manufactured by ADEKA, oxime ester-based polymerization initiator) E-3: Compound having the following structure (oxime ester-based polymerization initiator)

[0300]

[0301] [Thermal Crosslinkable Compounds] The thermal crosslinkable compounds (F-1 to F-3) are shown below: F-1: Celloxide 2021P (manufactured by Daicel Chemical Industries, Ltd., 3,4-epoxycyclohexylmethyl 3,4-epoxycyclohexanecarboxylate) F-2: EOCN-1020 (manufactured by Nippon Kayaku Co., Ltd., cresol-novolac epoxy resin) F-3: EHPE-3150 (manufactured by Daicel Chemical Industries, Ltd., multifunctional alicyclic epoxy resin)

[0302] [Surfactant] The surfactant (W-1) is shown below: W-1: KF6001 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0303] [Solvent] The solvents are as follows: PGMEA: propylene glycol monomethyl ether acetate PGME: 1-methoxy-2-propanol butyl acetate CyP: cyclopentanone

[0304] [Preparation of Pigment Dispersions] The components shown in Table 5 were mixed in the amounts (parts by mass) shown in Table 5, and then 230 parts by mass of zirconia beads with a diameter of 0.3 mm were added. The mixture was dispersed for 5 hours using a paint shaker, and the beads were separated by filtration to produce each pigment dispersion (pigment dispersions 1 to 20). The parts by mass of Resin A are shown as parts by mass of the resin solids, excluding the solvent described in <Synthesis of Resin A-1>. Table 5 is shown below.

[0305]

[0306] [Preparation of Curable Compositions] As shown in Table 6 or Table 7, curable compositions of the Examples and Comparative Examples were prepared by mixing the components in the amounts (parts by mass) shown in the table. In Table 6, each curable composition of the Examples is a composition in the first embodiment, and in Table 7, each curable composition of the Examples is a composition in the second embodiment. In Tables 6 and 7, the parts by mass of the pigment dispersion are shown as the amount of the entire solution including the solvent, and the parts by mass of Resin B or Resin H are shown as parts by mass of the resin solids excluding the solvent described in <Synthesis Example of Resin B-1>. In Tables 6 and 7, the values ​​shown in the columns "Tg (°C)," "Shrinkage (%)," "Dissolution Rate T1 (μm / sec)," and "Dissolution Rate T2 (μm / sec)" are synonymous with the values ​​shown in Tables 1 to 4. In Tables 6 and 7, the HSP distances between the components shown in the "HSP distance" column were calculated based on the values ​​of the dispersion term (δd), polar term (δp), and hydrogen bond term (δh) of Resin A, Resin B, Resin H, and polymerizable compound shown in Tables 1 to 4. The units of the values ​​in the "HSP distance" column are MPa. 1/2 Tables 6 and 7 are shown below.

[0307]

[0308]

[0309]

[0310]

[0311]

[0312] [Evaluation] The curable compositions were evaluated by the following methods.

[0313] [Evaluation of Alignment Suitability] The ease of aligning the support and the exposure mask in the exposure step was evaluated by evaluating alignment suitability according to the following procedure. A silicon wafer (8 inches) having alignment marks with L1 = 60 μm in FIG. 1 and H1 = 0.6 μm in FIG. 2 was prepared as a substrate (support). The curable composition of each Comparative Example or Example was applied to this substrate so that the resulting curable composition layer had a film thickness of 3.5 μm. The curable composition layer was disposed so as to cover the alignment mark. In other words, the curable composition layer was disposed on the alignment mark. The coated substrate was baked on a hot plate at 90°C for 2 minutes to produce a substrate with a curable composition layer (Step 1 or Step 11). Thereafter, the wafer was placed in a semiconductor exposure apparatus (FPA-5510iZs, manufactured by Canon Inc.), and a mask corresponding to the alignment mark on the substrate was used to confirm whether alignment before the exposure treatment was possible (Step 2 or Step 12). Those for which pre-exposure alignment was possible based on the alignment marks on the substrate were judged to have alignment suitability, while those for which it was difficult to confirm the positions of the alignment marks on the substrate and alignment was not possible were judged to have no alignment suitability.

[0314] [Preparation of cured film (first embodiment)] The cured film in the first embodiment (evaluation using each curable composition listed in Table 6) was prepared by the following procedure. For each substrate with a curable composition layer that had been aligned in [Evaluation of alignment suitability], a 10000 W / m 2 Illuminance of 1000 mJ / cm 2The curable composition layer was exposed to an exposure amount of 1000 ppm. For those for which alignment was not possible, the alignment step was skipped and exposure was performed on the entire surface of the substrate (Step 3). After exposure, puddle development was performed at 23°C for 60 seconds using an alkaline developer CD-2000 (manufactured by FUJIFILM Electronic Materials Co., Ltd.). Thereafter, rinsing was performed with a spin shower and further washing with pure water (Step 4). Subsequently, the substrate was heated at 220°C for 5 minutes using a hot plate to obtain a substrate with a cured film (Step 5).

[0315] [Preparation of Cured Film (Second Embodiment)] The cured film in the second embodiment (evaluation using each curable composition listed in Table 7) was prepared by the following procedure. For each substrate with a curable composition layer that had been aligned in [Evaluation of Alignment Suitability], a 10000 W / m 2 Illuminance of 1000 mJ / cm 2 The curable composition layer was exposed to an exposure amount of 1000 ppm. In cases where alignment was not possible, the alignment step was skipped and exposure was performed on the entire surface of the substrate (Step 13). After exposure, puddle development was performed at 23°C for 60 seconds using an alkaline developer CD-2000 (manufactured by FUJIFILM Electronic Materials Co., Ltd.). Thereafter, the substrate was rinsed with a spin shower, further washed with pure water, and air-dried to obtain a substrate with a cured film (Step 14).

[0316] [Evaluation of Reflectance] Light with a wavelength of 350 to 1200 nm was incident on a substrate with a cured film prepared as described in [Preparation of Cured Film (First Embodiment)] or [Preparation of Cured Film (Second Embodiment)] using a VAR unit spectrometer V7200 (trade name) manufactured by JASCO Corporation at an incident angle of 5°, and the reflectance was evaluated from the resulting reflectance spectrum at a reflection angle of 5°. Specifically, the average value of the regular reflectance of light with a wavelength of 400 to 700 nm was used as the evaluation standard, and evaluation was performed in accordance with the following classification. In addition, evaluation was performed using angles of 45° and 60° in the same manner as for the 5° angle. In terms of the following evaluation criteria, a rating of "3" or higher is preferable in practice, and a rating of "4" or higher is more preferable.

[0317] (Evaluation criteria: angle 5°) "5": Average regular reflectance is less than 0.3% "4": Average regular reflectance is 0.3% or more and less than 1.0% "3": Average regular reflectance is 1.0% or more and less than 2.0% "2": Average regular reflectance is 2.0% or more and less than 5.0% "1": Average regular reflectance is 5.0% or more

[0318] (Evaluation criteria: 45° angle) "5": Average regular reflectance is less than 1% "4": Average regular reflectance is 1% or more but less than 3% "3": Average regular reflectance is 3% or more but less than 5% "2": Average regular reflectance is 5% or more but less than 10% "1": Average regular reflectance is 10% or more

[0319] (Evaluation criteria: angle 60°) "5": Average regular reflectance is less than 3% "4": Average regular reflectance is 3% or more and less than 6% "3": Average regular reflectance is 6% or more and less than 10% "2": Average regular reflectance is 10% or more and less than 15% "1": Average regular reflectance is 15% or more

[0320] [Evaluation of Light-Shielding Property (OD Measurement)] A substrate with a cured film was prepared in the same manner as described in the above [Preparation of Cured Film (First Embodiment)] or [Preparation of Cured Film (Second Embodiment)], except that a glass substrate was used instead of a silicon wafer. The transmittance spectrum of the cured film-coated substrate was measured at 400 to 1,100 nm using a spectrophotometer U-4100 (manufactured by Hitachi High-Technologies Corporation) and an integrating sphere light-receiving unit. The OD value was calculated from the average value of the transmittance (%) at wavelengths of 400 to 700 nm using the following formula (O1), and evaluated according to the following criteria: OD value = -log10 (transmittance / 100) ... formula (O1). Regarding the following evaluation criteria, 2.0 or higher is preferred, 2.5 or higher is more preferred, and 3.0 or higher is even more preferred.

[0321] (Evaluation criteria) "5": OD value is 3.5 or more; "4": OD value is 3.0 or more and less than 3.5; "3": OD value is 2.5 or more and less than 3.0; "2": OD value is 2.0 or more and less than 2.5; "1": OD value is less than 2.0

[0322] [Evaluation of Film Surface Roughness] The surface roughness of the curable composition layer and the cured film was evaluated by measuring the arithmetic mean surface roughness Ra, the mean element length Rsm, and the root mean square slope RΔq according to JIS-B-0601:2013. Specifically, the surface shape of the prepared cured film was measured using a 3D laser measuring microscope (LEXT OLS5000 manufactured by Olympus Corporation) with an objective lens at a magnification of 100x. The surface shape of the substrate with the curable composition layer prepared in the above [Evaluation of Alignment Suitability] (substrate after step 1 or step 11) and the substrate with the cured film prepared in the above [Evaluation of Reflectance] (substrate after step 5 or step 14) was measured, and a surface image file was obtained. The observation measurement range (horizontal) in measuring the surface shape of the sample was 129 μm × 129 μm. Next, an analysis application was launched, and the obtained surface image file was displayed, and then tilt correction was performed. The line roughness window was displayed, a horizontal line was selected from the measurement line button, and the horizontal line was displayed at any location within the surface image. The OK button was then pressed to obtain the Ra, Rsm, and RΔq values. Furthermore, horizontal lines were displayed at four different locations within the surface image, and the Ra, Rsm, and RΔq values ​​were obtained for each location. The average of the five values ​​obtained was calculated to obtain the Ra, Rsm, and RΔq values.

[0323] [Results] The results of the above evaluations are shown in Tables 8 and 9. Table 8 shows the evaluation results of each composition in the first embodiment, and Table 9 shows the evaluation results of each composition in the second embodiment.

[0324]

[0325]

[0326] The arithmetic mean surface roughness Ra(a), the mean element length Rsm(a), and the root mean square slope RΔq(a) of the curable composition layer were 0.04 μm, 7 μm, and 3°, respectively, in Example 6, 0.01 μm, 2 μm, and 1°, respectively, in Comparative Example 1, 0.01 μm, 3 μm, and 1°, respectively, in Example 101, and 0.01 μm, 2 μm, and 1°, respectively, in Comparative Example 101. The arithmetic mean surface roughness Ra(b), mean element length Rsm(b), and root mean square slope RΔq(b) of the cured film were 0.17 μm, 6 μm, and 15°, respectively, in Example 6, 0.01 μm, 2 μm, and 1°, respectively, in Comparative Example 1, and 0.06 μm, 10 μm, and 5°, respectively, in Example 101. In addition, the curable compositions of Examples 1 to 38 and Examples 101 to 104 were diluted with 0.1 parts by mass of the curable composition and 10 parts by mass of PGMEA, and then measured using a particle size distribution analyzer Nanotrac UPA (manufactured by Microtrac-Bell). In the obtained particle size distribution (volume basis), the proportion of particles having a particle size of 200 nm or more was 3% or less in all Examples.

[0327] Furthermore, Examples 201 to 205 were evaluated in the same manner as Example 6, except for the heating temperature in step 5. The results are shown in Table 10. Note that Example 203 is the same as Example 6.

[0328]

[0329] As shown in the table, it was confirmed that this manufacturing process allows for easy positioning of the mask during exposure, and that the anti-reflection properties of the resulting cured film are excellent. Furthermore, a comparison of Examples 1, 11, 13, and 15, etc., confirmed that when the curable composition contains a colorant and the colorant contains a black organic pigment, the light-blocking properties are superior, when the colorant contains carbon black, the light-blocking properties are even superior, and when the colorant contains titanium black, the light-blocking properties are particularly superior. A comparison of Examples 32 to 35, etc., confirmed that when the shrinkage percentage defined by formula (X) of the curable compound is 7% or more, the anti-reflection properties of the cured film are superior, and a comparison of Examples 1 to 10, etc. confirmed that when the HSP distance between resin A and resin B is 2.0 MPa or less, the anti-reflection properties of the cured film are superior.1/2 It was confirmed that when the HSP distance between resin A and resin B is 2.0 to 4.0 MPa or more, the anti-reflection properties of the cured film are further improved. 1/2 and the difference between the HSP distance (A) and the HSP distance (B) (HSP distance (A) - HSP distance (B)) is 1.0 MPa 1/2 It was confirmed that when the above value is met, the anti-reflection properties (regular reflectance for light incident at an angle of 45°) of the cured film are more excellent.

[0330] From a comparison of Examples 101 to 104, it was confirmed that when the ratio T2 / T1 of the dissolution rate T2 of Resin H in the developer to the dissolution rate T1 of Resin C in the developer was 15.0 or more, the anti-reflection properties (regular reflectance for incident light at angles of 5° and 45°) of the cured film were more excellent.

[0331] Furthermore, by comparing Examples 201 to 205, it was confirmed that when the heating temperature in step 5 was 180°C or higher, the antireflective properties of the cured film were superior; when the heating temperature was 200°C or higher, the antireflective properties of the cured film were even superior; when the heating temperature was 220°C or higher, the antireflective properties of the cured film were particularly superior; and when the heating temperature was 240°C or higher, the antireflective properties of the cured film were the most superior.

[0332]

[0111] Furthermore, the curable compositions of the examples shown in Table 7 were used, and the procedures described above in [Preparation of cured film (second embodiment)] were carried out. Then, the cured films were heated at 220°C for 5 minutes using a hot plate. The cured films were then evaluated as described above in [Evaluation of reflectance] and [Evaluation of light-blocking property (measurement of OD)]. It was confirmed that the same effects as those of the examples shown in Table 9 were obtained.

[0333] 10 alignment mark 12 square frame 14 vertical line 16 horizontal line 18 support

Claims

1. A method for producing a cured film, comprising the steps of: step 1 of forming a curable composition layer on a support; step 2 of aligning the support with an exposure mask; step 3 of exposing the curable composition layer through the exposure mask; step 4 of developing the exposed curable composition layer to form a patterned cured film; and step 5 of heating the patterned cured film, wherein the curable composition contains a resin A, a resin B, and a polymerizable compound, and the HSP distance between the resin A and the resin B is 1.5 MPa. 1/2 an HSP distance (A) between the resin A and the polymerizable compound is greater than an HSP distance (B) between the resin B and the polymerizable compound.

2. The method for producing a cured film according to claim 1, wherein the glass transition temperature of at least one of the resin A and the resin B is at least 120° C. lower than the heating temperature during the heat treatment.

3. The method for producing a cured film according to claim 1, wherein the glass transition temperature of the resin B is 0 to 70°C.

4. A method for producing a cured film according to claim 1, wherein the resin A comprises a repeating unit A1 having an acid group, and a repeating unit A2 having at least one of a polyoxyalkylene group having an average number of added 3 or more and a polyoxyalkylenecarbonyl group having an average number of added 3 or more, the content of the repeating unit A2 being 35 mass% or more relative to all repeating units of the resin A; the resin B comprises a repeating unit B1 derived from a monomer selected from the group consisting of alkyl acrylates and alkyl methacrylates, a repeating unit B2 having a hydroxyl group, and a repeating unit B3 having a carboxylic acid group, the content of the repeating unit B1 being 60 mass% or more relative to all repeating units of the resin B.

5. The method for producing a cured film according to claim 4, wherein the acid value of the resin A is 50 mg KOH / g or more.

6. The method for producing a cured film according to claim 1, wherein the shrinkage percentage of the polymerizable compound defined by formula (X) is 7% or more: (1-ρM / ρP) x 100 ... formula (X) In formula (X), ρM represents the specific gravity of the polymerizable compound measured in accordance with JIS-K-2249. ρP represents the specific gravity of a cured product of the polymerizable compound measured in accordance with JIS-K-2249.

7. The method for producing a cured film according to claim 1, wherein the curable composition further contains a colorant.

8. The method for producing a cured film according to claim 7, wherein the coloring material includes a black coloring material.

9. The method for producing a cured film according to claim 8, wherein the black coloring material comprises a black organic pigment.

10. A method for producing a cured film, comprising: step 11 of forming a curable composition layer on a support; step 12 of aligning the support with an exposure mask; step 13 of exposing the curable composition layer through the exposure mask; and step 14 of developing the exposed curable composition layer to form a patterned cured film, wherein the curable composition contains a resin C, a resin H, and a polymerizable compound, and the HSP distance between the resin C and the resin H is 1.5 MPa. 1/2 a ratio T2 / T1 of a dissolution rate T2 of the resin H in the developer used in the development treatment to a dissolution rate T1 of the resin C in the developer is 10.0 or more.

11. The method for producing a cured film described in claim 10, wherein the resin C comprises a repeating unit C1 having an acid group and a repeating unit C2 having at least one of a polyoxyalkylene group having an average number of added 3 or more and a polyoxyalkylenecarbonyl group having an average number of added 3 or more, the content of the repeating unit C2 being 35 mass% or more relative to the total repeating units of the resin C, the resin H being an acrylic resin or a methacrylic resin, and the acid value of the resin H being 70 mgKOH / g or more higher than the acid value of the resin C.

12. The method for producing a cured film according to claim 10, wherein the acid value of the resin C is 50 mg KOH / g or more.

13. The method for producing a cured film according to claim 10, wherein the acid value of the resin H is 140 mg KOH / g or more.

14. The method for producing a cured film according to claim 10, wherein the curable composition further contains a colorant.

15. The method for producing a cured film according to claim 14, wherein the coloring material includes a black coloring material.

16. The method for producing a cured film according to claim 15, wherein the black colorant comprises a black organic pigment.

Citation Information

Patent Citations

  • Laminate, and solid-state imaging element

    WO2019065143A1

  • Curable composition, cured film, optical element, solid-state imaging element and color filter

    WO2019171902A1