Laminated film, method for producing same, and resin-molded article
The laminated film structure, combining polycarbonate and thermoplastic acrylic resin layers with a cured acrylate intermediate layer, addresses the weather and abrasion resistance issues in resin molded products, enhancing their durability and suitability for outdoor use.
Patent Information
- Application Number
- PCT/JP2024/009971
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Resin molded products, particularly those used outdoors such as automobile exteriors, face issues with insufficient weather resistance, low heat resistance, and abrasion resistance, limiting their durability and performance in complex shapes and outdoor applications.
A laminated film structure comprising a polycarbonate resin layer, a thermoplastic acrylic resin layer, an intermediate layer with a cured product of active energy ray-curable acrylate, and optionally inorganic fine particles and silicon compounds, which provides excellent interlayer adhesion, flexibility, and abrasion resistance, suitable for in-mold lamination molding.
The laminated film enhances the weather resistance, impact resistance, and abrasion resistance of resin molded products, making them suitable for outdoor applications and complex shape molding, such as automobile exteriors, while maintaining flexibility and adhesion.
Smart Images

Figure JPOXMLDOC01-APPB-C000001 
Figure JPOXMLDOC01-APPB-C000002 
Figure JPOXMLDOC01-APPB-C000003
Abstract
Description
Laminated film, its manufacturing method and resin molded product
[0001] The present invention relates to a laminate film, a method for producing the same, and a resin molded article. More specifically, the present invention relates to a laminate film having a layer containing a polycarbonate resin and a layer containing a thermoplastic acrylic resin, a method for producing the same, and a resin molded article.
[0002] Decorated resin molded products are widely used in automobiles, home appliances, daily necessities, and the like. One proposed method for decorating resin molded products is in-mold decoration (also known as in-mold lamination), in which a resin film with a pattern or various functions is placed in a mold and, simultaneously with injection molding, the resin film is integrated with the injected resin to obtain a resin molded product. Unlike conventional surface decoration methods such as painting, printing, and vapor deposition, this decoration method offers advantages such as the ability to accommodate complex shapes through mold design, the ability to perform molding and decoration simultaneously, and a high degree of freedom in imparting various designs and functionality to the resin film.
[0003] For example, Patent Document 1 describes a method of obtaining a resin molded product with a decorated surface by placing a decorative sheet in a mold having a cavity and injecting molten resin into the mold through a gate of the mold.
[0004] Known methods for imparting functions to resin films include coating a substrate film with a coating agent capable of imparting various functions. Resin compositions containing active energy ray-curable polyfunctional (meth)acrylates are often used as coating agents from the viewpoint of productivity, etc. In this application, the term (meth)acrylate is used as a general term for acrylates and methacrylates.
[0005] It is known that decorative films proposed as the resin films use polycarbonate resin as the substrate film.
[0006] For example, Patent Document 2 discloses a decorative sheet in which one side of a laminated film is decorated, the laminated film being formed by laminating a layer of methacrylic resin and acrylic rubber particles on the surface of a polycarbonate resin layer, and a thermoplastic resin sheet is laminated on the decorated side.
[0007] Resin molded articles to which various functions have been imparted by such methods have been used in a variety of applications, such as interior parts.
[0008] However, when the resin molded article is used for outdoor purposes such as automobile exteriors, although the initial performance is excellent, the weather resistance is not sufficient, and the required performance may not be maintained for the expected period of use.
[0009] JP 2010-247493 A JP 2009-234184 A
[0010] As mentioned above, acrylic resin sheets are widely used as decorative sheets in which functionalities are imparted to resin films. However, when acrylic resin sheets are used on the surface, they have the drawback of low heat resistance and abrasion resistance, which makes them suitable for outdoor use. In addition to the above properties, there is a demand for laminated films that have excellent formability, such as interlayer adhesion in resin films and sheets and flexibility suitable for in-mold lamination molding.
[0011] An object of the present invention is to provide a novel laminated film.
[0012] Another object of the present invention is to provide a laminated film that is suitable for in-mold lamination molding and has excellent abrasion resistance, interlayer adhesion, and flexibility.
[0013] Another object of the present invention is to provide a novel method for producing the above laminated film.
[0014] Another object of the present invention is to provide a resin molded article obtained by injection molding a thermoplastic resin onto the surface of the above laminated film on the side of the base layer.
[0015] The present inventors have investigated a decorative laminate film having a polycarbonate resin substrate layer, a thermoplastic acrylic resin layer on the surface of which is provided, and a layer containing a cured product of an active energy ray-curable acrylate on the surface of the thermoplastic acrylic resin layer. In the process, they have found that the above-mentioned problems can be solved by providing an intermediate layer containing a specific acrylic resin between the thermoplastic acrylic resin layer and the cured product layer of the active energy ray-curable acrylate, and that the film has excellent weather resistance, particularly suitable for outdoor use, and have arrived at the present invention.
[0016] Means for solving the above problems include the following aspects: [1] A laminate film comprising a layer containing a polycarbonate resin (Layer A), a layer containing a thermoplastic acrylic resin (Layer B), an acrylic resin mixed intermediate layer (Layer C), and a layer containing a cured product of an active energy ray-curable acrylate (Layer D) laminated in this order, and satisfying the following (a) to (d): (a) the active energy ray-curable acrylate comprises at least one of a polyfunctional (meth)acrylate and a urethane (meth)acrylate, (b) Layer D comprises at least one of inorganic fine particles and a silicon compound hydrolysis condensate, (c) the total content of the polyfunctional (meth)acrylate and the urethane acrylate is 45% by mass to 97% by mass, and the total content of the inorganic fine particles and the silicon compound hydrolysis condensate is 3% by mass to 55% by mass, relative to the total amount of the polyfunctional (meth)acrylate, the urethane (meth)acrylate, the inorganic fine particles, and the silicon compound hydrolysis condensate, (d) The C layer contains the thermoplastic acrylic resin and a cured product of at least one of the polyfunctional (meth)acrylate and the urethane (meth)acrylate. [2] The laminate film according to [1] above, wherein, when the amount of the thermoplastic acrylic resin in the C layer is X parts by mass and the total amount of the polyfunctional (meth)acrylate and the urethane (meth)acrylate is Y parts by mass, Y / (X+Y) is 0.2 to 0.9. [3] The laminate film according to [1] or [2] above, wherein, in the C layer, the reaction rate of the double bonds of the (meth)acrylic groups of the polyfunctional (meth)acrylate and the urethane (meth)acrylate is 25 to 70%. [4] The laminate film according to any one of [1] to [3] above, wherein the ratio of the thickness of the C layer to the total thickness of the C layer and the D layer is 10 to 70%. [5] The laminate film according to any one of [1] to [4] above, wherein the thickness of the C layer is 0.3 to 5.0 μm. [6] The laminate film according to any one of [1] to [5] above, wherein the thickness of the D layer is 1.5 to 18 μm. [7] The laminate film according to any one of [1] to [6] above, wherein the total thickness of the C layer and the D layer is 3 to 20 μm.[8] The laminate film according to any one of [1] to [7], wherein the layer A contains a polyester-based thermoplastic elastomer, the polyester-based thermoplastic elastomer comprising a hard segment composed of a polybutylene terephthalate unit and a soft segment composed of a polyester unit having an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid as a dicarboxylic acid component and a diol having 5 to 15 carbon atoms as a diol component. [9] The laminate film according to [8], wherein the polyester-based thermoplastic elastomer is contained in an amount of 1 to 20 parts by weight per 100 parts by weight of the polycarbonate resin.
[10] A method for producing the laminate film described in [1] above, comprising co-extrusion lamination of a layer containing a polycarbonate resin (Layer A) and a layer containing a thermoplastic acrylic resin (Layer B), followed by coating the Layer B with a coating composition containing an organic solvent, an active energy ray-curable acrylate, and at least one of inorganic fine particles and a silicon compound hydrolysis condensate, drying the coated coating composition, and then irradiating the coated layer with active energy rays to form an acrylic resin-mixed intermediate layer (Layer C) and a cured acrylate layer (Layer D).
[11] A method for producing the laminate film described in
[10] above, wherein the Layer C contains the thermoplastic acrylic resin and a cured product of at least one of the polyfunctional (meth)acrylate and the urethane (meth)acrylate.
[12] A resin molded article having a thermoplastic resin layer in contact with the Layer A of the laminate film described in any one of [1] to [9] above.
[13] A resin molded article obtained by injection molding a thermoplastic resin onto the Layer A side of the laminate film described in any one of [1] to [9] above.
[0017] According to the present invention, a laminate film can be provided that exhibits excellent interlayer adhesion, impact resistance, flexibility, and abrasion resistance, while also exhibiting weather resistance. This laminate film is useful as a film for thermoforming, such as in-mold lamination, or as a decorative film. Resin molded products using this laminate film can be used, for example, for automotive interior materials, electrical appliances, cosmetic films, and building interior and exterior materials. Because of its particularly excellent weather resistance, the film is particularly effective industrially when used as an automotive exterior material or building exterior material.
[0018] The present disclosure will be described in detail below. The following description of the components may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments.
[0019] In this specification, the use of "to" to indicate a range of values means that the values before and after it are included as the lower and upper limits.
[0020] Furthermore, in the description of groups (atomic groups) in this specification, when a notation does not specify whether the group is substituted or unsubstituted, it encompasses both unsubstituted and substituted groups. For example, the term "alkyl group" encompasses not only alkyl groups without a substituent (unsubstituted alkyl groups) but also alkyl groups with a substituent (substituted alkyl groups).
[0021] In this specification, "(meth)acrylic" is a term used as a concept that includes both acrylic and methacrylic, and "(meth)acryloyl" is a term used as a concept that includes both acryloyl and methacryloyl.
[0022] Furthermore, the term "process" in this specification does not only refer to an independent process, but also includes a process that cannot be clearly distinguished from other processes as long as the intended purpose of the process is achieved.
[0023] In addition, in the present disclosure, "mass %" and "wt %" are synonymous, and "parts by mass" and "parts by weight" are synonymous.
[0024] Unless otherwise specified, each component in the composition or each structural unit in the polymer in the present disclosure may be contained alone or in combination of two or more types.
[0025] Furthermore, in the present disclosure, the amount of each structural unit in a polymer means, unless otherwise specified, the total amount of each of the corresponding structural units present in the polymer when there are multiple substances or structural units corresponding to each structural unit in the polymer.
[0026] Furthermore, in the present disclosure, a combination of two or more preferred aspects is a more preferred aspect.
[0027] The present invention uses a layer containing a polycarbonate resin (Layer A) as a base layer, and laminates, in order from the base layer side, a layer containing a thermoplastic acrylic resin (Layer B), an acrylic resin-mixed intermediate layer (Layer C), and a layer containing a cured product of an active energy ray-curable acrylate (Layer D). The following requirements (a) to (d) are satisfied: (a) the active energy ray-curable acrylate contains at least one of a polyfunctional (meth)acrylate and a urethane (meth)acrylate; (b) Layer D contains at least one of inorganic fine particles and a silicon compound hydrolysis condensate; and (c) the total content of the polyfunctional (meth)acrylate and the urethane acrylate is 45% by mass to 97% by mass, and the total content of the inorganic fine particles and the silicon compound hydrolysis condensate is 3% by mass to 55% by mass, relative to the total amount of the polyfunctional (meth)acrylate, the urethane (meth)acrylate, the inorganic fine particles, and the silicon compound hydrolysis condensate. (d) The layer C contains the thermoplastic acrylic resin and a cured product of at least one of the polyfunctional (meth)acrylate and the urethane (meth)acrylate.
[0028] Each layer will be described below. -Layer A- (Layer Containing Polycarbonate Resin (Layer A)) The polycarbonate resin used in the layer A of the present invention is a polymer in which dihydroxy compounds are bonded by carbonate ester bonds, and is usually obtained by reacting a dihydroxy component with a carbonate precursor by interfacial polymerization or melt polymerization.
[0029] Representative examples of dihydroxy components include 2,2-bis(4-hydroxyphenyl)propane (commonly known as bisphenol A), 2,2-bis{(4-hydroxy-3-methyl)phenyl}propane (bisphenol C), 2,2-bis(4-hydroxyphenyl)butane, 2,2-bis(4-hydroxyphenyl)-3-methylbutane, 2,2-bis(4-hydroxyphenyl)-3,3-dimethylbutane, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, and 1,1-bis(4-hydroxyphenyl)cyclohexane. Examples of suitable bisphenols include cyclohexane, 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, 1,1-bis(4-hydroxyphenyl)octane, 1,1-bis(4-hydroxyphenyl)decane, 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene, 9,9-bis(4-hydroxyphenyl)fluorene, α,α'-bis(4-hydroxyphenyl)-m-diisopropylbenzene, isosorbide, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol. These may be homopolymers using a single bisphenol, or copolymers of two or more bisphenols. Bisphenol A is preferred from the viewpoints of physical properties and cost. In the present invention, polycarbonates in which 50 mol % or more of the bisphenol component is bisphenol A and / or bisphenol C are preferred, more preferably 70 mol % or more, and even more preferably 90 mol % or more.
[0030] Specific examples of polycarbonates include homopolymers of bisphenol A, homopolymers of bisphenol C, copolymers of bisphenol A and bisphenol C, copolymers of bisphenol A and 1,1-bis(4-hydroxyphenyl)-3,3,5-trimethylcyclohexane, and copolymers of bisphenol A and 9,9-bis{(4-hydroxy-3-methyl)phenyl}fluorene. The homopolymer of bisphenol A is most preferred.
[0031] Carbonyl halides, carbonate esters, haloformates, etc. are used as carbonate precursors, and specific examples include phosgene, diphenyl carbonate, and dihaloformates of dihydric phenols.
[0032] When the dihydric dihydroxy compound and the carbonate precursor are reacted by interfacial polymerization or melt polymerization to produce a polycarbonate resin, a catalyst, a terminal terminator, an antioxidant for the dihydric phenol, etc. may be used as necessary. The polycarbonate resin may be a branched polycarbonate resin copolymerized with a trifunctional or higher polyfunctional aromatic compound, or a polyester carbonate resin copolymerized with an aromatic or aliphatic difunctional carboxylic acid, or a mixture of two or more of the obtained polycarbonate resins.
[0033] The molecular weight of the polycarbonate resin, expressed as viscosity average molecular weight, is preferably in the range of 13,000 to 40,000. If the molecular weight is lower than 13,000, the sheet may become brittle, and cracks and burrs may easily occur during thermoforming. If the molecular weight is higher than 40,000, the melt viscosity of the resin composition with a polyester-based thermoplastic elastomer may become too high, making melt film formation difficult. The molecular weight is more preferably 15,000 to 35,000, even more preferably 20,000 to 32,000, and particularly preferably 22,000 to 28,000. When the polycarbonate resin is a mixture of two or more types, the molecular weight refers to the molecular weight of the entire mixture. Here, the viscosity average molecular weight is the specific viscosity (η) at 20°C of a solution obtained by dissolving 0.7 g of polycarbonate in 100 mL of methylene chloride. sp ) was measured, and the viscosity average molecular weight (M) was calculated from the following formula:
[0034] η sp / c = [η] + 0.45 × [η] 2 c [η]=1.23×10 -4 M 0.83(where c = 0.7 g / dL, [η] is the intrinsic viscosity.) The glass transition temperature of the polycarbonate resin-containing layer (Layer A) of the present invention must be in the range of 100°C to 145°C, preferably 110°C to 140°C, and more preferably 120°C to 130°C. If the glass transition temperature is higher than the above range, the thermoforming temperature must be increased, and heat exposure during thermoforming can initiate thermal decomposition of the acrylic resin components contained in Layers B, C, and D, or thermal reaction of the double bonds of unreacted acrylate monomers contained in Layers C and D, resulting in poor appearance such as cloudiness, surface irregularities, and cracks after molding. Furthermore, if the glass transition temperature is lower than the above range, the molding temperature appropriate for thermoforming Layer A will be lower than the glass transition temperature of the thermoplastic acrylic resin-containing layer (Layer B), making thermoforming impossible. Here, the glass transition point refers to a value measured by differential scanning calorimetry (DSC).
[0035] The layer A preferably contains 50% by mass or more, more preferably 80% by mass or more, of the polycarbonate resin, and may contain 100% of the polycarbonate resin, although a polyester-based thermoplastic elastomer may be blended with the polycarbonate resin in terms of the glass transition temperature and transparency of the layer A. The polyester-based thermoplastic elastomer is preferably a multiblock copolymer composed of hard segments formed from polybutylene terephthalate units and soft segments formed from polyester units having an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid as dicarboxylic acid components and a diol having 5 to 15 carbon atoms as a diol component.
[0036] The hard segment composed of the polybutylene terephthalate unit has excellent compatibility with polycarbonate resin, is preferable in terms of transparency and thermoformability, and also has good properties in terms of strength, etc. Polybutylene terephthalate may contain other components as copolymerization components to the extent that the effects of the present invention are not impaired. The proportion of such copolymerization components is preferably 30 mol% or less, more preferably 20 mol% or less, and even more preferably 10 mol% or less, of the total components (100 mol%) of both the dicarboxylic acid component and the diol component. The intrinsic viscosity of the polymer that becomes the hard segment is preferably in the range of 0.2 to 2.0, more preferably 0.5 to 1.5.
[0037] The soft segment consisting of polyester units with an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid as the dicarboxylic acid component and a diol having 5 to 15 carbon atoms as the diol component refers to a segment in which the melting point of the polymer formed from the segment is 100°C or lower, or which is liquid and amorphous at 100°C. The intrinsic viscosity of the polymer that becomes the soft segment is preferably in the range of 0.2 to 2.0, more preferably 0.5 to 1.5. The soft segment used is a soft segment consisting of polyester units with an aromatic dicarboxylic acid and / or an aliphatic carboxylic acid as the dicarboxylic acid component and a diol having 5 to 15 carbon atoms as the diol component (hereinafter sometimes referred to as "SS-1"). SS-1 is preferred because it provides extremely good transparency.
[0038] In order to obtain better transparency, the soft segment SS-1 preferably contains 60 to 99 mol% of aromatic dicarboxylic acid and 1 to 40 mol% of aliphatic dicarboxylic acid, based on a total of 100 mol% of dicarboxylic acid components. It is more preferable that the aromatic dicarboxylic acid content is 70 to 95 mol% and the aliphatic dicarboxylic acid content is 5 to 30 mol%. It is even more preferable that the aromatic dicarboxylic acid content is 85 to 93 mol% and the aliphatic dicarboxylic acid content is 7 to 15 mol%. It is particularly preferable that the aromatic dicarboxylic acid content is 89 to 92 mol% and the aliphatic dicarboxylic acid content is 8 to 11 mol%.
[0039] The aromatic dicarboxylic acid of SS-1 is preferably at least one selected from the group consisting of terephthalic acid, isophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 4,4'-diphenylcarboxylic acid, bis(4-carboxyphenyl)methane, and bis(4-carboxyphenyl)sulfone, with terephthalic acid and isophthalic acid being more preferred, and isophthalic acid being particularly preferred from the viewpoint of reducing crystallinity.
[0040] As the aliphatic dicarboxylic acid of SS-1, straight-chain aliphatic dicarboxylic acids having 4 to 12 carbon atoms such as succinic acid, adipic acid, and sebacic acid are preferred, with sebacic acid being particularly preferred.
[0041] As the diol component having 5 to 15 carbon atoms in SS-1, linear aliphatic diols having 6 to 12 carbon atoms such as hexamethylene glycol, decamethylene glycol, 3-methylpentanediol, and 2-methyloctamethylenediol are more preferred, with hexamethylene glycol being particularly preferred.
[0042] SS-1 is particularly preferred from the viewpoints that it has high compatibility with polycarbonate resins, can produce highly transparent products, and has good surface properties and transparency after thermoforming. More specifically, SS-1 is preferably a polyester composed of isophthalic acid, sebacic acid, and hexamethylene glycol.
[0043] In the present invention, the ratio of hard segments to soft segments in the polyester-based thermoplastic elastomer is preferably 20 to 70% by weight of hard segments and 80 to 30% by weight of soft segments, and more preferably 20 to 40% by weight of hard segments and 80 to 60% by weight of soft segments, based on 100% by weight of the elastomer. The intrinsic viscosity of the polyester-based thermoplastic elastomer (measured in o-chlorophenol at 35°C) is preferably 0.6 or more, more preferably in the range of 0.8 to 1.5, and even more preferably in the range of 0.8 to 1.2. Intrinsic viscosity lower than the above range is undesirable because it may result in a decrease in sheet strength.
[0044] In the present invention, when Layer A contains a polyester-based thermoplastic elastomer, it is preferable that the polyester-based thermoplastic elastomer be contained in an amount of 1 to 20 parts by weight per 100 parts by weight of the polycarbonate resin in Layer A. If the amount of polyester-based thermoplastic elastomer is less than 1 part by weight, the effect of improving flowability during thermoforming is low, and if it exceeds 20 parts by weight, the rigidity of Layer A is likely to be insufficient.
[0045] The thickness of the layer A is preferably in the range of 25 to 500 μm, more preferably in the range of 30 to 450 μm, even more preferably in the range of 40 to 400 μm, and most preferably in the range of 50 to 350 μm.
[0046] The layer A of the present invention may contain various additives commonly used in each resin, such as a heat stabilizer, an antioxidant, an ultraviolet absorber, an antistatic agent, a dye, etc. Furthermore, the layer A may contain a reinforcing filler such as glass fiber, as long as the effect of the present invention is not impaired.
[0047] The thickness of the substrate layer (layer A) containing a polycarbonate resin can be determined by measuring the thickness of the laminate film according to the present disclosure with a micrometer and subtracting the thicknesses of layers B, C, and D measured with a scanning electron microscope (SEM) from the thickness of the laminate film.
[0048] The thicknesses of the B, C, and D layers are determined by measuring a cross section of the laminate film according to the present disclosure using a scanning electron microscope (SEM). - Layer B - (Layer Containing Thermoplastic Acrylic Resin (Layer B)) In the present invention, the thermoplastic acrylic resin used for Layer B is preferably composed primarily of a polymer of methacrylic acid ester or acrylic acid ester. When a resin other than a thermoplastic acrylic resin is used for Layer B, for example, polycarbonate resin, the surface hardness of the laminate film is low and the molded product is prone to scratches, which is undesirable. Furthermore, PET resin is undesirable because it is prone to causing poor appearance due to thickness unevenness. The thermoplastic acrylic resin is preferably a copolymer containing methyl methacrylate, preferably at least 50 mol%, more preferably at least 70 mol%, even more preferably at least 80 mol%, and particularly preferably at least 90 mol%.
[0049] Examples of copolymerization components other than methyl methacrylate include ethyl methacrylate, butyl methacrylate, 2-ethylhexyl methacrylate, methyl acrylate, ethyl acrylate, butyl acrylate, and 2-ethylhexyl acrylate. Other copolymerization components include other ethylenically unsaturated monomers. Specific examples include vinyl aromatic compounds such as styrene, α-methylstyrene, and vinyltoluene; diene compounds such as 1,3-butadiene and isoprene; alkenyl cyanide compounds such as acrylonitrile and methacrylonitrile; acrylic acid, methacrylic acid, maleic anhydride, and N-substituted maleimides. These may be used alone or in combination of two or more. The content of the copolymerization component is preferably 0 to 50% by weight, more preferably 0 to 30% by weight, and even more preferably 0 to 20% by weight. Methods for producing thermoplastic acrylic resins are generally broadly divided into emulsion polymerization, suspension polymerization, and continuous polymerization. The thermoplastic acrylic resin used in the present invention may be produced by any of these polymerization methods. Layer B may also contain various additives such as general heat stabilizers, colorants, release agents, lubricants, antistatic agents, and matting agents.
[0050] Although rubber particles may be added to Layer B of the present invention, it is preferable that Layer B does not substantially contain rubber particles. Although adding rubber particles to a thermoplastic acrylic resin to improve toughness is a well-known and widely used technique, it is preferable that Layer B does not contain rubber particles from the viewpoint of ensuring transparency and surface hardness.
[0051] The thickness of Layer B is preferably in the range of 10 to 200 μm, more preferably in the range of 20 to 150 μm, and most preferably in the range of 30 to 100 μm. Designing the thickness of Layer B within this range enables more stable film formation, and the addition of various additives makes it possible to achieve various performance properties such as weather resistance. Furthermore, it is possible to realize a laminated film with appropriate flexibility and excellent flexibility, including various performance properties such as weather resistance. -Layer C- (Acrylic Resin Mixed Intermediate Layer (Layer C)) Layer C is an intermediate layer containing a mixed acrylic resin located between Layer B and Layer D, and contains the thermoplastic acrylic resin that constitutes Layer B and a cured product of an active energy ray-curable acrylate that constitutes Layer D, which will be described later.
[0052] With respect to the composition of Layer C, when the amount of the thermoplastic acrylic resin is X parts by mass and the total amount of the polyfunctional (meth)acrylate and the urethane (meth)acrylate is Y parts by mass, Y / (X+Y) is preferably 0.2 to 0.9. By setting the ratio within this range, the difference in the linear expansion coefficient between Layer B and Layer C, and between Layer C and Layer D, can be kept to 100 ppm / K or less. This can suppress thermal shock due to the difference in the linear expansion coefficient at the Layer B / Layer C interface and the Layer C / Layer D interface, resulting in a laminate film with excellent adhesion and weather resistance. The ratio is more preferably 0.3 to 0.8, and most preferably 0.4 to 0.75.
[0053] The value of Y / (X+Y) can be adjusted appropriately by changing the film-forming conditions of the C layer and D layer, for example, the type and composition of the solvent in the coating agent for forming the D layer, or the heat drying temperature and time.
[0054] Layer C contains two types of acrylic resins that form Layer B and Layer D (described below), namely, a thermoplastic acrylic resin and a cured product of an active energy ray-curable acrylate. The state of Layer C, which contains these two types of acrylic resins, significantly affects interlayer adhesion, various durability properties, and flexibility. When performing in-mold lamination using the laminate film of the present invention, the laminate film of the present invention is placed and mounted in a mold, which may have a three-dimensional shape, and a high-temperature molten resin is injected into this mold. For this reason, the mounted laminate film must conform to the shape of the mold (even complex shapes), and various deformation stresses are applied, such as distortion due to linear expansion caused by direct contact with the high-temperature molten resin. Therefore, the flexibility of the mounted laminate film significantly affects the moldability of in-mold lamination.
[0055] Before the formation of Layer C, unreacted polyfunctional (meth)acrylate and / or urethane (meth)acrylate are present around the polymer chains of the thermoplastic acrylic resin, and it is believed that these reactions result in a structure in which the long-chain polymer chains of the thermoplastic acrylic resin become entangled in the network of three-dimensional crosslinked structures formed by the polyfunctional (meth)acrylate and / or urethane (meth)acrylate after curing. It is believed that the formation of such a structure improves the flexibility and weather resistance of the laminate film itself, and reduces stress and misalignment between Layers B and D during in-mold lamination. As a result, not only adhesion but also flex resistance can be improved, and weather resistance, which is strongly affected by stress between layers (particularly between Layers B and D), can be significantly improved.
[0056] The thermoplastic acrylic resin contained in the C layer, and the crosslinked cured product of the polyfunctional (meth)acrylate and the urethane (meth)acrylate contained in the C layer and the D layer described below, can be confirmed by microscopic-infrared spectroscopy (microscopic FT-IR method).
[0057] Specifically, the laminated film according to the present disclosure is cut before ultraviolet irradiation, and the cross sections of each of the B, C, and D layers are analyzed using a microscopic FT-IR measurement device. For example, when the C layer contains a polyfunctional acrylate, a peak (810 cm) derived from the C=C-H structure of the polyfunctional acrylate is detected. -1 ) and a peak (1740 cm ) due to the O—C═O structure of the thermoplastic acrylic resin and the multifunctional acrylate. -1 From the ratio of the components constituting Layer B and the components constituting a part of Layer D, it can be confirmed that the components constituting Layer B and the components constituting a part of Layer D are mixed together. Even if Layer C and Layer D do not contain a multifunctional acrylate, it is possible to confirm that Layer C contains both the acrylic components of Layer B and Layer D by focusing on the specific peak derived from the component of Layer B.
[0058] As described above, the thermoplastic acrylic resin may be the same as that constituting the layer B.
[0059] Examples of the active energy ray-curable acrylate constituting the C layer include polyfunctional (meth)acrylates and urethane (meth)acrylates. The C layer contains a cured product of at least one of the polyfunctional (meth)acrylates and urethane (meth)acrylates. Specifically, the C layer contains a cured product of a crosslinking reaction of a polyfunctional (meth)acrylate, a cured product of a crosslinking reaction of a urethane (meth)acrylate, a cured product (copolymer) of a crosslinking reaction of a polyfunctional (meth)acrylate and a urethane (meth)acrylate, or a mixture thereof. Here, the term "cured product" refers to a three-dimensional crosslinked body or a three-dimensional crosslinked copolymer formed by irradiation with active energy rays. In the case of a three-dimensional crosslinked copolymer, the copolymerization ratio of the polyfunctional (meth)acrylate to the urethane (meth)acrylate is, for example, 20 to 95 mol %, preferably 50 to 85 mol %, of the polyfunctional (meth)acrylate relative to the total of the polyfunctional (meth)acrylate and the urethane (meth)acrylate.
[0060] In the crosslinking reaction of polyfunctional (meth)acrylates, urethane (meth)acrylates, and copolymers thereof, the double bonds of the (meth)acrylic groups of the polyfunctional (meth)acrylates and urethane (meth)acrylates react to form a crosslinked structure, resulting in a cured product and a cured layer. In this case, the reaction rate (reaction rate) of the double bonds of the (meth)acrylic groups (when the state in which all acrylic groups have completely reacted is taken as 100%) is preferably 25 to 70%, more preferably 40 to 65%. The reaction rate can be determined by the peak (810 cm) derived from the C=C-H structure of the unreacted polyfunctional acrylate. -1 ) and a peak (1740 cm ) due to the O—C═O structure of the thermoplastic acrylic resin and the multifunctional acrylate. -1 The ratio of the peak (around 810 cm) derived from the C═C—H structure of the multifunctional acrylate in the cured C layer -1 ) and a peak (1740 cm ) due to the O—C═O structure of the thermoplastic acrylic resin and the multifunctional acrylate. -1 It can be calculated by comparing the ratio of
[0061] Specific compounds of the polyfunctional (meth)acrylate and urethane (meth)acrylate are the same as those forming the layer D. The layer D will be described later.
[0062] The thickness of Layer C is preferably 0.3 to 5.0 μm. By setting the thickness of Layer C to 0.3 to 5.0 μm, excellent weather resistance and impact resistance are achieved. It is more preferably 0.5 to 4.5 μm, and most preferably 1.0 to 4.0 μm. -Layer D- (Layer Containing a Cured Product of an Active Energy Ray-Curable Acrylate (Layer D)) Layer D is a layer containing a cured product of an active energy ray-curable acrylate. Here, the active energy ray-curable acrylate includes a polyfunctional (meth)acrylate, a urethane (meth)acrylate, or both. The cured product of an active energy ray-curable acrylate refers to a three-dimensional crosslinked product containing a polyfunctional (meth)acrylate as a monomer, a three-dimensional crosslinked product containing a urethane (meth)acrylate as a monomer, or a three-dimensional crosslinked copolymer containing a polyfunctional (meth)acrylate and a urethane (meth)acrylate as monomers. In the case of a three-dimensional cross-linked copolymer, the copolymerization ratio of the polyfunctional (meth)acrylate and the urethane (meth)acrylate is, for example, 20 to 95 mol %, preferably 50 to 85 mol %, of the polyfunctional (meth)acrylate relative to the total of the polyfunctional (meth)acrylate and the urethane (meth)acrylate. [Polyfunctional Acrylate] The polyfunctional (meth)acrylate monomer used in forming the D layer is not particularly limited as long as it has two or more (meth)acrylate groups in one molecule, and examples thereof include bifunctional (meth)acrylate monomers such as trimethylolpropane di(meth)acrylate, ethylene oxide-modified trimethylolpropane di(meth)acrylate, propylene oxide-modified trimethylolpropane di(meth)acrylate, glycerin di(meth)acrylate, and bis(2-(meth)acryloyloxyethyl)hydroxyethyl isocyanurate; trifunctional (meth)acrylate monomers such as pentaerythritol tri(meth)acrylate and ditrimethylolpropane tri(meth)acrylate; and tetrafunctional or higher functional (meth)acrylate monomers such as pentaerythritol tetra(meth)acrylate and dipentaerythritol penta(meth)acrylate.
[0063] Among these, the polyfunctional (meth)acrylate monomer used to form the D layer is preferably a difunctional to tetrafunctional (meth)acrylate monomer, and more preferably a difunctional or trifunctional (meth)acrylate monomer.
[0064] In this specification, the term "polyfunctional (meth)acrylate monomer" refers to a polyfunctional (meth)acrylate having a molecular weight of less than 2,000.
[0065] The D layer may be formed using a monofunctional (meth)acrylate monomer to balance abrasion resistance and flexibility. In this case, the polyfunctional (meth)acrylate monomer preferably accounts for 90% by mass or more, more preferably 93% by mass or more, and particularly preferably 96% by mass or more, based on the total mass of the (meth)acrylate monomers. [Di(meth)acrylate Compound] The bifunctional (meth)acrylate monomer used to form the D layer may be an aliphatic or aromatic di(meth)acrylate compound, but is preferably an aliphatic di(meth)acrylate compound.
[0066] The aliphatic di(meth)acrylate compound is preferably a compound obtained by esterifying and bonding an alkyldiol with acrylic acid or methacrylic acid.
[0067] Preferred structures of the aliphatic di(meth)acrylate compound include 1,6-hexanediol diacrylate, 1,9-nonanediol diacrylate, and 1,10-decanediol diacrylate.
[0068] The aliphatic di(meth)acrylate compound may be synthesized or may be a commercially available product, such as HDDA (manufactured by Daicel Allnex Corporation), A-HD-N, A-NOD-N, A-DOD-N (all manufactured by Shin-Nakamura Chemical Co., Ltd.), or 1,9-DA (manufactured by Kyoei Chemical Industry Co., Ltd.).
[0069] The aliphatic di(meth)acrylate monomers may be used alone or in combination of two or more.
[0070] When the polyfunctional (meth)acrylate monomer contains an aliphatic di(meth)acrylate compound, the blending ratio of the aliphatic di(meth)acrylate compound is preferably 10% by mass to 80% by mass, more preferably 20% by mass to 70% by mass, and even more preferably 25% by mass to 60% by mass, based on the total mass of the polyfunctional (meth)acrylate monomer. [Tri(meth)acrylate Compound] The trifunctional (meth)acrylate monomer used in forming the D layer may be an aliphatic tri(meth)acrylate monomer or an aromatic tri(meth)acrylate monomer, but is preferably an aliphatic tri(meth)acrylate monomer or an aromatic ring tri(meth)acrylate monomer which may contain a heteroatom, and more preferably an aliphatic tri(meth)acrylate compound or a tri(meth)acrylate monomer having an isocyanuric ring.
[0071] The aliphatic tri(meth)acrylate monomer is preferably pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, or dipentaerythritol penta(meth)acrylate, and more preferably pentaerythritol tri(meth)acrylate or pentaerythritol tetra(meth)acrylate. [Urethane (meth)acrylate] The urethane (meth)acrylate used to form Layer D is an acrylate oligomer having a urethane bond in its molecule, which can impart properties such as abrasion resistance to the laminated film. By adjusting the acrylate ratio, a layer with excellent flexibility and abrasion resistance can be formed. Urethane (meth)acrylate can be prepared by reacting a polyisocyanate compound having multiple isocyanate groups in its molecule with an acrylate having a hydroxyl group in its molecule, and various urethane (meth)acrylate products are commercially available. Commercially available urethane (meth)acrylates include 8BR-600, 8UV-085A, and 8UX-116A manufactured by Taisei Fine Chemical Co., Ltd. [Isocyanuric Ring-Containing Tri(meth)acrylate Monomer] The isocyanuric ring-containing tri(meth)acrylate monomer used to form the C layer is preferably a compound represented by the following general formula (5):
[0072]
[0073] In the above general formula (5), R 9 , R 10 and R 11 each independently represents a group represented by the following formula (5-a):
[0074]
[0075] In the above formula (5-a), n2 represents an integer of 2 to 4, and R 8 represents a hydrogen atom or a methyl group, and Q 3 and Q 4 In the repeating unit, each independently represents a hydrogen atom or an alkyl group having 1 to 5 carbon atoms.
[0076] A preferred structure of the isocyanuric ring-containing tri(meth)acrylate monomer is a compound having the structure represented by the following formula (5A).
[0077]
[0078] The isocyanuric ring-containing tri(meth)acrylate monomer may be synthesized, or a commercially available product may be used. Examples of commercially available products that can be used include M-315 (manufactured by Toagosei Co., Ltd.), A9300 (manufactured by Shin-Nakamura Chemical Co., Ltd.), FA-731A (manufactured by Hitachi Chemical Co., Ltd.), SR368 (manufactured by Sartomer), and M-370 (manufactured by MIWON). [Isocyanuric Ring-Containing Tri(meth)acrylate Compound Monomer Blending Ratio] The blending ratio of the isocyanuric ring-containing tri(meth)acrylate monomer used in forming the C layer is preferably 20% by mass to 70% by mass, more preferably 30% by mass to 69% by mass, and even more preferably 35% by mass to 68% by mass, relative to the total mass of the polyfunctional (meth)acrylate monomer.
[0079] From the viewpoints of the balance between hardness and flexibility, abrasion resistance, adhesion, and the like, the polyfunctional (meth)acrylate monomer used in forming the D layer is particularly preferably a bifunctional (meth)acrylate (preferably an aliphatic di(meth)acrylate monomer, more preferably a compound obtained by esterifying and bonding an alkyldiol with acrylic acid or methacrylic acid), and a trifunctional (meth)acrylate monomer (preferably an aliphatic tri(meth)acrylate monomer or a tri(meth)acrylate monomer having an isocyanuric ring, more preferably pentaerythritol tri(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, or a compound represented by the above general formula (5), even more preferably pentaerythritol tri(meth)acrylate, or a compound having the structure represented by the above formula (5A).
[0080] The polyfunctional (meth)acrylate contained in the layer D is preferably a polymer of the above-mentioned polyfunctional (meth)acrylate monomer (polyfunctional (meth)acrylate polymer).
[0081] The polyfunctional (meth)acrylate polymer may contain an oligomer from the viewpoint of a balance between abrasion resistance, adhesiveness, and the like.
[0082] In this specification, the term "polyfunctional (meth)acrylate oligomer" refers to a polymer of a polyfunctional (meth)acrylate having a weight-average molecular weight of 2,000 or more and less than 50,000. In this specification, the term "polyfunctional (meth)acrylate polymer" refers to a polymer of a polyfunctional (meth)acrylate having a weight-average molecular weight of 50,000 or more.
[0083] The weight average molecular weight of the polymer of the polyfunctional (meth)acrylate monomer is preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 200,000 or more, from the viewpoints of abrasion resistance and heat bending property.
[0084] The polyfunctional (meth)acrylate polymer may be a homopolymer or a copolymer, but is preferably a copolymer. [Content of Polyfunctional (meth)acrylate and / or Urethane (meth)acrylate] The polyfunctional (meth)acrylate (preferably a polyfunctional (meth)acrylate polymer) contained in the D layer may be used alone or in combination of two or more.
[0085] The content of the polyfunctional (meth)acrylate in Layer D is 35% by mass to 95% by mass, preferably 40% by mass to 90% by mass, and more preferably 50% by mass to 90% by mass, based on the total amount of the polyfunctional (meth)acrylate and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate.
[0086] When the content of the polyfunctional (meth)acrylate in the layer D is within the above range, the layer D is excellent in abrasion resistance, adhesion, and the like.
[0087] The content (mass%) of the polyfunctional (meth)acrylate in the D layer was determined by scraping off a portion of the D layer as described above, performing pyrolysis gas chromatography using the scraped D layer to identify the compounds contained in the D layer, and then measuring the content (mass%) of the polyfunctional (meth)acrylate in the D layer at 650 cm -1 From 4000 cm -1This can be determined by identifying the composition of Layer D in combination with the results of characteristic absorption in infrared spectroscopy measured in the wavenumber region of 1000 to 15000. [Reaction Rate of Polyfunctional (meth)acrylate and / or Urethane (meth)acrylate] From the viewpoints of abrasion resistance, adhesion, etc., the addition polymerization reaction rate of the (meth)acrylic groups of the polyfunctional (meth)acrylate and / or urethane (meth)acrylate (hereinafter sometimes simply referred to as "reaction rate") is preferably 30% to 70%, more preferably 40% to 68%, and even more preferably 45% to 65%.
[0088] The reaction rate of the polyfunctional (meth)acrylate and / or urethane (meth)acrylate in the D layer was determined by determining the composition of the inorganic fine particle dispersion using the above-described method for measuring the abundance ratio of the polyfunctional (meth)acrylate in the D layer, and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate. Furthermore, infrared spectroscopy (ATR-IR) measurement was performed on the D layer surface using an attenuated total reflection method, and the peak (1740 cm ) derived from the (meth)acrylic ester was detected. -1 around 810 cm) and peaks due to (meth)acrylic monomers and urethane (meth)acrylate monomers -1 The value is calculated from the calculated value (nearby) using the following formulas (1) to (4) or (5).
[0089] (1) The surface of the D layer is 650 cm -1 From 2000 cm -1 ATR-IR measurements were performed in the wave number region of 1900 cm -1 and 2000 cm -1 The background infrared absorbance αb, expressed by the following formula (2), is calculated from the measured infrared absorbance αm, expressed by the following formula (1).
[0090] Measured infrared absorbance αm (wavelength) = -Log(R (wavelength) / 100) (1) In the above formula, R represents the reflectance of attenuated total reflection at the measurement wavelength of the measurement sample. Background infrared absorbance αb (wavelength p) = 1900 cm -1 αm in (1900) + (wavelength p-1900) x (2000cm -1 αm in (2000) -1900 cm-1 αm in (1900) ) / 100 (2) (2) From the background infrared absorbance value obtained above, the converted infrared absorbance αc is calculated using the following formula (3): (波長p) Calculate αc (波長p) = αm (波長p) -αb (波長p) (3) The reaction rate r of the double bonds in the polyfunctional (meth)acrylate and the urethane (meth)acrylate is calculated from the ATR-IR measurement results before and after the curing reaction of the D layer using the following formula (4) or (5).
[0091] Reaction rate of multifunctional (meth)acrylate and double bond in urethane methacrylate r = [1-(αc1 (810) / αc1 (1740) ) / (αc0 (810) / αc0 (1740) ) × 100 (4) In other words, r = [1 - (αc1 (810) ×αc0 (1740) ) / (αc0 (810) ×αc1 (1740) ) × 100 (5)
[0092] In the above formula (3) or (4), αc0 (wavelength) represents the converted infrared absorbance of the D layer before the curing reaction, and αc1 (波長) represents the converted infrared absorbance after ATR-IR measurement.
[0093] The wavelength 810 refers to a peak derived from a (meth)acrylate functional group contained in a double bond in a polyfunctional (meth)acrylate and a urethane (meth)acrylate, and has a wave number of 1740 cm -1 means a peak derived from a (meth)acrylic ester group contained in a polyfunctional (meth)acrylate and a urethane (meth)acrylate.
[0094] From the viewpoint of excellent abrasion resistance and adhesion, the total content of the polyfunctional (meth)acrylate and the urethane (meth)acrylate relative to the total amount of the polyfunctional (meth)acrylate, the urethane (meth)acrylate, the inorganic fine particles, and the silicon compound hydrolysis condensate is preferably 45% to 97% by mass, more preferably 65 to 92% by mass. The blending ratio of the polyfunctional (meth)acrylate monomer is preferably 40% to 98% by mass, more preferably 45% to 96% by mass, and even more preferably 60% to 70% by mass. [Inorganic Fine Particles (D3)] The D layer contains at least one of inorganic fine particles and a silicon compound hydrolysis condensate. The inorganic fine particles are preferably inorganic oxide fine particles. Examples of inorganic oxide fine particles include titanium oxide, zinc oxide, cerium oxide, and silicon dioxide (silica). Among these, silica fine particles such as colloidal silica are preferred.
[0095] Examples of commercially available colloidal silica include methanol silica sol, IPA-ST, PGM-ST, MEK-ST, NBA-ST, XBA-ST, DMAC-ST, ST-UP, ST-OUP, ST-20, ST-40, ST-C, ST-N, ST-O, ST-50, and ST-OL (all of which are product names), all manufactured by Nissan Chemical Industries, Ltd.
[0096] Furthermore, the silica fine particles may be silica fine particles whose dispersibility has been improved by a known method. Examples of such silica fine particles whose dispersibility has been improved include silica fine particles whose surface has been treated with a reactive silane coupling agent having a hydrophobic group, and silica fine particles modified with a compound having a (meth)acryloyl group. Examples of commercially available colloidal silica modified with a compound having a (meth)acryloyl group include MIBK-SD, MIBK-AC, MEK-AC, and PGM-AC (all of which are product names) manufactured by Nissan Chemical Industries, Ltd.
[0097] The shape of the silica fine particles is not particularly limited, and spherical, hollow, porous, rod-like, plate-like, fibrous, or irregularly shaped particles can be used. For example, commercially available hollow silica fine particles such as Silinax (registered trademark) manufactured by Nittetsu Mining Co., Ltd. can be used.
[0098] The inorganic oxide fine particles preferably have an average primary particle size of 1 nm to 200 nm, more preferably 1 nm to 100 nm. By setting the average primary particle size of the inorganic oxide fine particles within the above range, a laminated film excellent in abrasion resistance, adhesion, etc. can be obtained.
[0099] From the viewpoint of dispersibility in the D layer, the average primary particle size of the inorganic oxide fine particles is preferably 3 nm to 500 nm, more preferably 5 nm to 300 nm, and even more preferably 10 nm to 100 nm.
[0100] From the viewpoint of dispersibility in Layer D, the inorganic oxide fine particles are preferably spherical colloidal silica having an average primary particle diameter of 5 nm to 100 nm, and more preferably colloidal silica having an average primary particle diameter of 20 nm to 60 nm.
[0101] The average primary particle size of the inorganic oxide fine particles is measured by observing the D layer in the cross section of the laminate film according to the present disclosure with a transmission electron microscope (TEM). [Inorganic Fine Particle Blending Ratio] The inorganic fine particles may be used singly or in combination of two or more types.
[0102] The blending ratio of the inorganic fine particles is preferably 5% by mass to 40% by mass relative to the total mass of the polyfunctional (meth)acrylate compound, urethane (meth)acrylate, silicon compound hydrolysis condensate, and inorganic fine particles, and from the viewpoints of abrasion resistance, adhesion, etc., it is preferably 8% by mass to 35% by mass, and more preferably 12% by mass to 30% by mass. [Silicon Compound Hydrolysis Condensate] Preferred examples of the silicon compound hydrolysis condensate include hydrolyzable silane compounds.
[0103] Examples of the hydrolyzable silane compound include hydrolysis condensates of alkoxysilane compounds.
[0104] Specific examples include alkyltrialkoxysilanes such as methylmethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, and ethyltriethoxysilane; 3-(meth)acryloyloxypropyltrialkoxysilanes such as 3-(meth)acryloyloxypropyltrimethoxysilane and 3-(meth)acryloyloxypropyltriethoxysilane; vinyltrialkoxysilanes such as vinyltrimethoxysilane and vinyltriethoxysilane; and hydrolysis condensates of alkoxysilane compounds such as aminomethyltrimethoxysilane, aminomethyltriethoxysilane, 2-aminoethyltrimethoxysilane, 2-aminoethyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-aminopropyltriethoxysilane.
[0105] The hydrolysis condensate of an alkoxysilane compound can be obtained by subjecting an alkoxysilane compound to a hydrolysis condensation reaction. In the hydrolysis condensation reaction, a condensation reaction proceeds along with hydrolysis, and it is preferred that the majority of the Si—OR hydrolyzable groups of the hydrolyzable silane compound is hydrolyzed to 100%. From the viewpoint of liquid stability, it is preferred that the majority of the OH groups formed by hydrolysis, preferably 80% or more, more preferably 85% or more, and particularly preferably 90% or more, are condensed with hydroxy groups formed by hydrolysis of other alkoxysilane compounds.
[0106] The silicon compound hydrolysis condensate may be obtained by carrying out a hydrolysis reaction of an alkoxysilane compound alone, or may be obtained by carrying out a hydrolysis reaction in the presence of the above-mentioned inorganic oxide fine particles. However, from the viewpoint of the dispersibility of the inorganic oxide fine particles, it is preferable that the silicon compound hydrolysis condensate be obtained by carrying out a hydrolysis reaction in the presence of the above-mentioned inorganic oxide fine particles.
[0107] In addition, in order to improve the dispersibility of inorganic fine particles, the silicon compound hydrolysis condensate may be a product obtained by reacting a (meth)acrylic resin having an alkoxysilyl group on a side chain or a (meth)acrylic resin having a highly polar hydroxyl group, amine group or carboxyl group on a side chain with inorganic oxide fine particles and / or a hydrolyzable silane compound. [Triazine-based UV absorber (D4)] The layer (Layer D) containing the cured product of the active energy ray-curable acrylate according to the present disclosure preferably contains a triazine-based UV absorber (D4).
[0108] The triazine-based ultraviolet absorber (D4) includes an ultraviolet absorber having a triazine skeleton in the molecular skeleton.
[0109] The triazine-based ultraviolet absorber (D4) has the above structure and therefore has excellent ultraviolet absorption ability, which contributes to the light resistance of the D layer according to the present disclosure.
[0110] Specific examples of the triazine-based ultraviolet absorber (D4) include 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2
[0033] 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine, and the like.
[0111] The triazine-based ultraviolet absorber (C4) may be synthesized or may be a commercially available product, such as TINUVIN 400 (manufactured by BASF), TINUVIN 405 (manufactured by BASF), or TINUVIN 479 (manufactured by BASF).
[0112] The triazine-based ultraviolet absorber (D4) is preferably 2-[4-(octyl-2-methylethanoate)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)]-1,3,5-triazine or 2-[4-(2-hydroxy-3-dodecyloxypropyl)oxy-2-hydroxyphenyl]-4,6-[bis(2,4-dimethylphenyl)-1,3,5-triazine.
[0113] The triazine-based ultraviolet absorber (D4) may be used alone or in combination of two or more kinds.
[0114] The amount of the triazine-based ultraviolet absorber (D4) blended is preferably 3 to 5% by mass relative to 100 parts by mass of the total of the polyfunctional (meth)acrylate and / or urethane (meth)acrylate, and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate, and from the viewpoints of abrasion resistance, adhesion after heat bending, and weather resistance, it is more preferably 3.5 to 4.5% by mass. [Hindered Amine (Light Stabilizer (D5))] The layer (Layer D) containing a cured product of an active energy ray-curable acrylate according to the present disclosure preferably contains a hindered amine light stabilizer (D5). Examples of the hindered amine light stabilizer (D5) include compounds in which two of the three substituents on the nitrogen atom in the amine compound (including compounds in which two of the substituents and the nitrogen atom form a cyclic structure) have a structure with significant steric hindrance.
[0115] The hindered amine light stabilizer (D5) has the above structure and is therefore capable of reacting with and inactivating active species (radicals) generated in the coating layer.
[0116] Specific examples of the hindered amine light stabilizer (D5) include alkyl hindered amines such as bis(1,2,2,6,6-pentamethylpiperidin-4-yl) 3,4-bis{[(1,2,2,6,6-pentamethylpiperidin-4-yl)oxy]carbonyl}hexanedioate, bis(1,2,2,6,6-pentamethyl-4-piperidyl) decanedioate, and 1,2,2,6,6-pentamethyl-4-piperidyl methacrylate; and hydrogen-type hindered amines such as bis[2,2,6,6-tetramethyl-1-(undecyloxy)piperidin-4-yl]=3,4-bis{[(2,2,6,6-tetramethylpiperidin-4-yl)oxy]carbonyl}hexanedioate and 2,2,6,6-tetramethyl-4-piperidyl methacrylate; and alkoxy-type hindered amines such as bis[2,2,6,6-tetramethyl-1-(undecyloxy)piperidin-4-yl]=carbonate and 1-octyloxy-2,2,6,6-tetramethyl-4-piperidyl octanedioate.
[0117] The hindered amine may be synthesized or a commercially available product may be used.
[0118] Commercially available products that can be used include TINUVIN123 (manufactured by BASF), LA-52 (manufactured by ADEKA Corporation), LA-57 (manufactured by ADEKA Corporation), LA-68 (manufactured by ADEKA Corporation), LA-72 (manufactured by ADEKA Corporation), LA-77 (manufactured by ADEKA Corporation), LA-81 (manufactured by ADEKA Corporation), LA-82 (manufactured by ADEKA Corporation), and LA-87 (manufactured by ADEKA Corporation).
[0119] The hindered amines may be used alone or in combination of two or more.
[0120] The amount of the hindered amine to be blended is preferably 0.5% by mass to 30% by mass relative to 100 parts by mass of the total of the polyfunctional (meth)acrylate and / or urethane (meth)acrylate, and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate, and from the viewpoints of abrasion resistance, adhesion, and weather resistance, more preferably 3% by mass to 20% by mass. [Other Components] The layer (Layer D) containing a cured product of the active energy ray-curable acrylate according to the present disclosure may contain components (other components) other than those described above, as necessary. Examples of the other components include a surface conditioner, a colorant, and a dispersion medium for adjusting the solid content and viscosity of the dispersion.
[0121] The dispersion medium may be any liquid medium that does not impair the effects of the present disclosure, and various organic solvents can be used.
[0122] When the layer (Layer D) containing the cured product of the active energy ray-curable acrylate according to the present disclosure is cured by ultraviolet light, it is preferable that the layer further contains a photopolymerization initiator. Known photopolymerization initiators may be used, and for example, one or more selected from the group consisting of acetophenones, benzil ketals, and benzophenones are preferably used. Examples of the acetophenones include diethoxyacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, and 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone. Examples of the benzil ketals include 1-hydroxycyclohexyl phenyl ketone and benzyl dimethyl ketal.
[0123] Examples of benzophenones include benzophenone, methyl o-benzoylbenzoate, and the like.
[0124] Examples of benzoins include benzoin, benzoin methyl ether, and benzoin isopropyl ether.
[0125] The photopolymerization initiator may be used alone or in combination of two or more kinds.
[0126] The amount of the photopolymerization initiator used is preferably 1% by mass to 15% by mass, and more preferably 2% by mass to 10% by mass, relative to 100 parts by mass of the total of the polyfunctional (meth)acrylate and / or urethane (meth)acrylate, and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate.
[0127] The method for measuring the abundance ratio of the cured product of at least one of the polyfunctional (meth)acrylate and urethane (meth)acrylate constituting the D layer and at least one of the inorganic fine particles and the silicon compound hydrolysis condensate can be a method of scraping off the D layer from the laminated film and analyzing the types of compounds present by pyrolysis gas chromatography, a composition identification method by elemental analysis, or infrared spectroscopy (ATR-IR) by attenuated total reflection measurement of the D layer surface, or a method of cutting the laminated film in the thickness direction and measuring the cross section of the D layer by transmission IR to detect a peak (1740 cm) derived from the polyfunctional (meth)acrylate or urethane (meth)acrylate. -1 and a peak due to at least one of inorganic fine particles and hydrolysis condensation products of silicon compounds (in the case of silica, around 1100 cm -1 and a method of comparing the abundance ratio of a compound in the vicinity of the compound.
[0128] The thickness of the D layer is not particularly limited, but from the viewpoints of abrasion resistance, heat bending property, and adhesion after heat bending, it is preferably in the range of 1.5 μm to 18 μm, more preferably in the range of 3 μm to 15 μm, and even more preferably in the range of 5 μm to 12 μm.
[0129] The thickness of the D layer can be determined by the same method as for the B and C layers.
[0130] The total thickness of the C layer and the D layer is preferably 3 to 20 μm, more preferably 4 to 15 μm, from the viewpoint of abrasion resistance and weather resistance.
[0131]
[0033] From the viewpoints of transparency (initial haze) and flexibility, the ratio of the thickness of the C layer to the total thickness of the C layer and the D layer is preferably 10% to 70%, and more preferably 25 to 60%. [Method for Producing Laminated Film] The method for producing the laminated film of the present invention is not particularly limited, but may include a method in which a layer containing a thermoplastic acrylic resin (layer B) is first formed on a layer made of a polycarbonate resin (layer A), and then an acrylic resin mixed intermediate layer (layer C) and a layer containing a cured product of an active energy ray-curable acrylate (layer D) are formed on the B layer.
[0132] The method for forming a layer containing a thermoplastic acrylic resin (Layer B) on a layer made of a polycarbonate resin (Layer A) is not particularly limited, and known methods can be used. Examples include a method in which each layer is separately formed into a sheet or film and then heated and pressure-bonded; a method in which an adhesive is applied to at least one surface of the layer beforehand to bond them; a co-extrusion method in which the polycarbonate resin and the thermoplastic acrylic resin are laminated in the die of an extruder to obtain a sheet or sheet-like product; an in-mold molding method in which a thermoplastic acrylic resin is vacuum-formed beforehand and then the polycarbonate resin substrate is injection-molded; and a method in which a coating liquid in which a thermoplastic acrylic resin is dissolved in a solvent is applied to Layer A and then dried to remove the solvent. Co-extrusion and in-mold molding are preferred for cost reduction and productivity improvement. Co-extrusion is particularly preferred in terms of cost and productivity. -Method for Forming Layers C and D-The method for forming Layers C and D is not particularly limited, and Layers C and D may be formed separately or simultaneously. For example, a composition containing a polyfunctional (meth)acrylate and / or urethane (meth)acrylate and a thermoplastic acrylic resin that forms the B layer may be applied to the surface of the B layer and cured to form the C layer, and a coating composition containing at least one of a polyfunctional (meth)acrylate and a urethane (meth)acrylate, inorganic fine particles and / or a silicon compound hydrolysis condensate, and an organic solvent for forming the D layer may be applied to the C layer and cured to form the D layer; alternatively, a coating composition containing at least one of a polyfunctional (meth)acrylate and a urethane (meth)acrylate, inorganic fine particles and / or a silicon compound hydrolysis condensate, and an organic solvent for forming the D layer may be applied to the surface of the B layer, and then heat-treated to allow part of the D layer components to penetrate into the B layer, thereby simultaneously forming the C layer and the D layer.
[0133] The latter method of simultaneously forming the C layer and the D layer is preferable because it requires fewer steps and is more productive than the former method. This method will be described below.
[0134] In the method of simultaneously forming the C layer and the D layer, the difference in solubility parameter between the value calculated from the weighted average of the solubility parameters of the components forming the D layer and the thermoplastic (meth)acrylic resin constituting the B layer is 10 ((MPa) 1/2 ) or less.
[0135] When the difference in solubility parameters is within the above range, a mixed intermediate layer (layer C) can be formed at the contact surface after coating layer D on layer B, in which the acrylic resin components forming layers B and D are mixed together through diffusion due to molecular motion.
[0136] In this method, predetermined amounts of each component (polyfunctional (meth)acrylate, urethane (meth)acrylate, inorganic fine particles, and silicon compound hydrolysis condensate) that will ultimately constitute Layer D are dissolved and dispersed in a solvent such as an organic solvent to prepare a coating composition. At this time, the predetermined amounts of each component are the desired amounts of polyfunctional (meth)acrylate and urethane (meth)acrylate that will form Layer C. Next, the coating composition is applied to the side of Layer B opposite Layer A, and then dried over a certain period of time to remove the solvent and form a coating. The coating is then irradiated with active energy rays such as ultraviolet light or electron beams to reactively cure the polyfunctional (meth)acrylate and urethane (meth)acrylate, thereby forming Layer D on Layer B via Layer C.
[0137] The method for applying the coating composition is not particularly limited, and examples thereof include known and commonly used coating methods such as brush coating, roller coating, spray coating, dip coating, flow coater coating, roll coater coating, and electrodeposition coating.
[0138] In the case of such a method in which the C layer and the D layer are simultaneously formed, the thickness of the C layer can be appropriately adjusted by changing the drying temperature and drying time.
[0139] The method for drying the coating film of the coating composition is not limited, and examples thereof include natural drying, air drying, and drying by heating.
[0140] The drying temperature is preferably 65°C to 95°C, and more preferably 70°C to 85°C.
[0141] Furthermore, the drying time is preferably 5 to 20 minutes, more preferably 5 to 15 minutes, and even more preferably 5 to 13 minutes, from the viewpoint of the thickness necessary to effectively exhibit weather resistance.
[0142] The solvent is preferably an organic solvent that can dissolve polyfunctional (meth)acrylates, urethane (meth)acrylates, etc., and dissolve or disperse inorganic fine particles and silicon compound hydrolysis condensates. For example, from the viewpoint of being able to adjust the layer thickness of the acrylic resin mixed intermediate layer (C layer) within a suitable range, examples of the organic solvent include alcohols such as methanol, ethanol, propanol, and butanol; ethers such as dimethyl ether, diethyl ether, methyl ethyl ether, methyl butyl ether, tetrahydrofuran, and dioxane; ketones such as acetone, methyl ethyl ketone (2-butanone), methyl isobutyl ketone (4-methyl-2-pentanone), and cyclohexanone; esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, and ethyl valerate; ether alcohols such as methoxyethanol, ethoxyethanol, butoxyethanol, and methoxypropanol (hereinafter, sometimes referred to as "propylene glycol monomethyl ether (PGM)"), ethoxypropanol, and butoxypropanol; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as toluene, xylene, (ethylbenzene), styrene, and stilbene.
[0143] The organic solvents can be used alone or in combination.
[0144] When an organic solvent is used alone, from the viewpoints of the solubility of the acrylate monomer contained in forming the layer (D layer) containing a cured product of an active energy ray-curable acrylate and the permeability into the thermoplastic acrylic resin layer (B layer), ether alcohols such as methoxyethanol, ethoxyethanol, butoxyethanol, methoxypropanol, ethoxypropanol, and butoxypropanol are preferably used. Among these, methoxypropanol is particularly preferably used from the viewpoints of the balance of volatility, dissolving power for acrylic resin, and permeability into the thermoplastic acrylic resin layer (B layer), and low toxicity.
[0145] When organic solvents are mixed and used, from the viewpoint of facilitating the formation of the C layer, the ether alcohols listed as organic solvents when used alone are further mixed with at least one organic solvent selected from the group consisting of acetone, methyl ethyl ketone (2-butanone), methyl isobutyl ketone (4-methyl-2-pentanone), ketones such as cyclohexanone, esters such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, and ethyl valerate, and aromatic hydrocarbons such as toluene, xylene, (ethylbenzene), styrene, and stilbene. It is preferable to use a mixed solvent in which at least one organic solvent selected from the group consisting of ether alcohols, methyl ethyl ketone, ethyl acetate, butyl acetate, and toluene is added, since the boiling point is in the range of 70 to 140 ° C., and the penetration layer does not become thicker than necessary when the substrate is thermally dried after the hard coat is applied. It is more preferable to use a mixed solvent in which at least one organic solvent selected from the group consisting of methyl ethyl ketone, ethyl acetate, butyl acetate, and toluene is added to methoxypropanol.
[0146] From the viewpoint of volatility during coating and solvent recovery, methyl ethyl ketone (MEK) or methoxypropanol (propylene glycol monomethyl ether) is preferred.
[0147] The content of the organic solvent is preferably 40 to 70 parts by mass, and more preferably 45 to 65 parts by mass, per 100 parts by mass of the inorganic fine particle dispersion.
[0148] According to the present invention, a laminate film can be provided that exhibits excellent adhesion between layers, impact resistance, flexibility, abrasion resistance, and weather resistance. Therefore, this laminate film is useful as a film for thermoforming, such as in-mold lamination, or as a decorative film. For example, when the laminate film of the present invention is used for in-mold lamination, the layer D of the laminate film is first placed in contact with a mold, and then injection molding is performed to eject a molten thermoplastic resin (e.g., polycarbonate resin) into the mold, thereby obtaining a polycarbonate resin molded article decorated with the laminate film. In such a resin molded article, a thermoplastic resin layer (e.g., a polycarbonate layer) is formed in contact with the surface of the layer A of the laminate film.
[0149] The present disclosure will be described in detail below with reference to examples, but the present disclosure is not limited thereto. In these examples, "%" and "parts" mean "mass %" and "parts by mass", respectively, unless otherwise specified. [Evaluation Method] <Total Light Transmittance (TT)> Measured according to JIS K7361-1 (1997) using an NDH-300A manufactured by Nippon Denshoku Industries Co., Ltd. <Initial Haze (H)> Measured using a haze meter NDH2000 manufactured by Nippon Denshoku Industries Co., Ltd. The haze value (H) is expressed as H = Td / Tt x 100 (Td: scattered light transmittance, Tt: total light transmittance). <Abrasion Resistance (ΔH)> The surface of an abrasive wheel (product name: CS-10F, manufactured by Taber) was ground 25 times with an ST-11 grinding stone manufactured by Taber before the Taber abrasion test to prepare the abrasive wheel. Using the abrasion wheel prepared on the surface of Layer D of the laminate film, a Taber abrasion test was carried out in accordance with ASTM D1044 under the conditions of a load of 500 g and 500 revolutions, and the change (ΔH) in the cloudiness (haze value) of the laminate film surface before and after the Taber abrasion test was measured.
[0150] The change in haze value (ΔH) was measured using a haze meter (product name: NDH2000, manufactured by Nippon Denshoku Industries Co., Ltd.) under measurement method 2 and light source A. The haze value (H) is a value expressed by H = Td / Tt × 100 (Td: scattered light transmittance, Tt: total light transmittance).
[0151] The haze value (H) was measured for three test pieces with the same polishing specifications, and the average ΔH value was evaluated according to the following evaluation criteria. The smaller the ΔH value, the better the abrasion resistance, and a ΔH value of less than 9.0 is preferred.
[0152] The abrasion wheels used in the Taber abrasion test were those that showed a change in haze value (ΔH) of 0.6 to 1.0 when commercially available float glass (plate glass) was subjected to the Taber abrasion test in the same manner as above under conditions of a load of 500 g and 1,000 revolutions. Abrasion wheels with a ΔH outside the above range were not used in the test. <Boiling water resistance (adhesion)> The laminated film was immersed in boiling water for 3 hours, then removed, and any adhering water droplets were wiped off, and then conditioned in an environment of 25°C and 50% RH for 15 minutes. The removed laminate film was scored with a cutter knife on the surface of Layer D, with 100 grids spaced 1 mm apart. Nichiban adhesive tape (trade name "Cellotape (registered trademark)") was then pressed against the surface and the film was strongly peeled off perpendicularly (in accordance with JIS K5400). A rating of "X" was given for films that partially peeled off the coating film on the first peeling attempt; a rating of "△" was given for films that did not peel off the coating film on the first peeling attempt but partially peeled off on the second peeling attempt; and a rating of "O" was given for films that did not peel off the coating film on either of the two peeling attempts. <Flexibility> The laminate film was wrapped around cylinders with diameters of 18 mm and 36 mm, with Layer D facing outward. A rating of "O" was given for films that showed no abnormalities in appearance when wrapped around an 18 mm diameter cylinder; a rating of "△" was given for films that cracked when wrapped around an 18 mm cylinder but showed no abnormalities in appearance when wrapped around a 36 mm cylinder; and a rating of "X" was given for films that cracked even when wrapped around a 36 mm cylinder. <Impact Resistance> The laminate film was placed on the platform of a DuPont impact tester (DuPont Impact Resistance Tester No. 451, manufactured by Toyo Seiki Co., Ltd.) equipped with a flat platform, with the D layer facing upward. A striking die with a conical tip radius of 12.7 mm was placed on top of the film, and a 300 g drop weight was dropped from a height of 20 cm. The laminate film was observed after the test, and a rating of ◯ was given to films that had a dent of 1 mm or less in depth on the surface of the test area but no peeling or cracking of the D layer; a rating of △ was given to films that had a dent of more than 1 mm in depth on the surface of the test area but no peeling or cracking of the D layer; and a rating of × was given to films that had peeling or cracking of the D layer. <Weather Resistance> The laminate film was placed on a Super Xenon Weather Meter SX-75 tester manufactured by Suga Test Instruments Co., Ltd., with the D layer facing the light source, and exposed to UV irradiation at a UV intensity of 180 W / m 2The laminated film was exposed for 2000 and 4000 hours under conditions of a black panel temperature of 63°C, with 18 minutes of rainfall during 120 minutes. The laminated film was removed, the appearance was observed, and the surface was lightly rubbed and cleaned with a sponge soaked in neutral detergent. 100 grids spaced 1 mm apart were then made on the surface of the D layer with a cutter knife, and Nichiban adhesive tape (trade name "Cellotape (registered trademark)") was pressed onto the grid and then strongly peeled off perpendicularly twice. Samples that showed cracks or delamination after 2000 hours were rated "X," samples that were good in appearance and adhesion after 2000 hours but showed cracks or delamination after 4000 hours were rated "△," and samples that showed good appearance and adhesion even after 4000 hours were rated "O." [Preparation Example 1] (Production of Polyester-Based Thermoplastic Elastomer) 100 parts by weight of dimethyl isophthalate, 13 parts by weight of dimethyl sebacate, and 80 parts by weight of hexamethylene glycol were subjected to a transesterification reaction using dibutyltin diacetate as a catalyst, followed by polycondensation under reduced pressure to obtain an amorphous polyester (soft segment) with an intrinsic viscosity of 1.06 and no endothermic peak due to crystalline melting as measured by DSC. 32 parts by weight of polybutylene terephthalate pellets (hard segment) with an intrinsic viscosity of 0.98 were added to 100 parts by weight of the polyester, and the mixture was further reacted at 240°C for 45 minutes. Then, 0.03 parts by weight of phenylphosphonic acid was added to terminate the reaction, yielding a polyester-based thermoplastic elastomer (X1). The resulting polymer had a melting point of 190°C and an intrinsic viscosity of 0.93. Preparation Example 2 Synthesis of Silicon Compound Hydrolysis Condensate C1 100 parts by weight of 2-propanol, 40 parts by weight of 0.1 mol / L hydrochloric acid, and 101 parts by weight of methyltrimethoxysilane were added to a reaction vessel and stirred at 30°C for 1 hour and 30 minutes. While continuing to stir, the liquid temperature was raised to 80°C to partially evaporate the contained solvent and obtain CH 3 SiO 3/2124.5 parts by weight of a silicon compound hydrolysis condensate (C1) having a solids concentration of 30% by weight in terms of carbon black equivalent was obtained. <Preparation of Coating Agent (HC-1) for Forming D Layer> 420 parts by weight of Aronix M-350 (trimethylolpropane ethylene oxide modified triacrylate) manufactured by Toagosei Co., Ltd. as a polyfunctional (meth)acrylate, 1,820 parts by weight of 1,9-DA (1,9-nonanediol diacrylate) manufactured by Kyoeisha Chemical Co., Ltd., 31.5 parts by weight of 8UX-116A (solids concentration: 63.5% by weight MEK solution) manufactured by Taisei Fine Chemical Co., Ltd. as a urethane acrylate, and 124.5 parts by weight of an organic solvent-dispersed surface-modified colloidal silica (MEK-AC-2140Z manufactured by Nissan Chemical Industries, Ltd.) as inorganic fine particles (D3) were used. 50 parts by weight of a 40% solids concentration (D4) BASF Corporation Tinuvin 405 (hydroxyphenyl triazine ultraviolet absorber) as (D4), 4 parts by weight of LA-52 (ADEKA Corporation) as a hindered amine light stabilizer (D5), 2 parts by weight of LA-52 (BASF Corporation Irgacure 184) as a photopolymerization initiator (D6), 1 part by weight of phenyl 1-hydroxyethyl ketone (BASF Corporation Irgacure 184), 2050 parts by weight of methyl ethyl ketone (MEK), 10050 parts by weight of methoxypropanol (MIBK), and 4010 parts by weight of isopropanol (IPA) were added to prepare a D layer-forming coating agent (HC-1). The composition of (HC-1) is shown in Table 1 below. <Preparation of Coating Agents for Forming D Layer (HC-2 to HC-10)> (HC-2) to (HC-10) were prepared in the same manner as in the preparation of (HC-1), except that the compositions shown in Table 1 were used.
[0153] In Table 1, M-315 refers to Aronix M-315 (a mixture of di- and triacrylates modified with ethylene oxide isocyanurate) manufactured by Toagosei Co., Ltd., and MIBK-ST refers to MIBK-ST (30% solids concentration) manufactured by Nissan Chemical Industries, Ltd. [Example 1] (Molding material A) Polycarbonate resin pellets (Panlite L1250WP (bisphenol A homopolycarbonate resin (PC-A, viscosity average molecular weight 23,900) manufactured by Teijin Limited) and the thermoplastic elastomer (X1) obtained in the above [Preparation Example 1] were each pre-dried in advance, and mixed in a V-type blender so that 92.93 parts by weight of the polycarbonate resin pellets were mixed with 7 parts by weight of the thermoplastic elastomer (X1) polymerized in Preparation Example 1 and 0.07 parts by weight of tetrakis-2,4-t-butylphenyl 4,4'-biphenylenediphosphonate (Irgafos PEP-Q manufactured by BASF) as a heat stabilizer. The mixture was then extruded at a cylinder temperature of 260°C using a twin-screw extruder to form pellets, thereby obtaining molding material A for layer A. The glass transition temperature of molding material A was 145°C. (Molding material B) An acrylic resin (Acrypet VH-001 (a thermoplastic acrylic resin copolymerized with 95 mol% methyl methacrylate and 5 mol% methyl acrylate) was prepared. (Co-extrusion) Molding materials A and B were each extruded from a 650 mm wide T-die using a feed block system using a single-screw extruder with a screw diameter of 40 mm under conditions of cylinder temperatures of 260°C (molding material A), 250°C (molding material B), and screw rotation speeds of 109 rpm (molding material A), and 11 rpm (molding material B). The molten resin was then compressed between a metal roll and a metal sleeve roll and cooled. After edge trimming, the sheet was wound up at a take-up speed of 10.3 m / min to produce a 400 mm wide laminate sheet having a two-layer structure (layer A 240 μm, layer B 60 μm). (Coating) Next, the D layer-forming coating agent (HC-1) was applied to the B layer side of the laminate sheet using a bar coater (#8), and then dried with hot air for 5 minutes in a drying oven at 100° C. A laminate film with a four-layer structure of A layer / B layer / C layer / D layer (A layer 240 μm, B layer 59 μm, C layer 1.5 μm, D layer 3.5 μm) was obtained (however, the C layer and D layer were in an uncured state).
[0154] The resulting laminated film was irradiated with a high-pressure mercury lamp at an irradiation intensity of 250 W / cm 2 , irradiation amount 2000mJ / cm 2 The C and D layers were cured by irradiating them with ultraviolet light of 1000 W at ... The resin molded article obtained had a beautiful appearance without defects such as cracks or wrinkles.
[0155] The weather resistance of the obtained molded article was evaluated in the same manner as in Example 1, and the weather resistance was found to be good (◯). [Comparative Examples 1 to 3] Each laminate film was obtained in the same manner as in Example 1, except that the coating agent prepared with the composition shown in Table 1 was used as shown in Table 2 and produced under the conditions shown in Table 3. [Comparative Example 4] A polycarbonate resin molded article was obtained in the same manner as in Example 18, except that the laminate sheet obtained in Comparative Example 1 was used. The appearance of the obtained resin molded article was free from defects such as cracks and wrinkles and had a beautiful appearance. When the weather resistance was evaluated, the weather resistance was found to be x.
[0156]
[0157]
[0158]
[0159] P1: Panlite L1250WP manufactured by Teijin Limited. X1: Polyester thermoplastic elastomer obtained in Preparation Example 1. T1: Tetrakis 2,4-t-butylphenyl 4,4'-biphenylenediphosphonate. P2: Acrypet VH-001 manufactured by Mitsubishi Rayon Co., Ltd. UV1: Tinuvin 360 manufactured by BASF Corporation (benzotriazole ultraviolet absorber). C1: Silicon compound hydrolysis condensate synthesized in Preparation Example 2. UV2: Tinuvin 405 manufactured by BASF Corporation (hydroxyphenyltriazine ultraviolet absorber). HA1: LA-52 manufactured by ADEKA Corporation (hindered amine light stabilizer).
[0160] The laminated film of the present invention has excellent adhesion, impact resistance, flexibility, and abrasion resistance, and also has weather resistance, and is therefore useful, for example, as a thermoforming film for in-mold lamination molding or as a decorative film. Therefore, resin molded articles using this laminated film can be used, for example, for automobile interior materials, electrical appliances, cosmetic films, and interior and exterior building materials, and are particularly suitable as automobile exterior materials or building exterior materials because of their excellent weather resistance.
Claims
1. A laminate film in which a layer containing a polycarbonate resin (layer A), a layer containing a thermoplastic acrylic resin (layer B), an acrylic resin mixed intermediate layer (layer C), and a layer containing a cured product of an active energy ray-curable acrylate (layer D) are laminated in this order, and which satisfies the following (a) to (d); (a) the active energy ray-curable acrylate contains at least one of a polyfunctional (meth)acrylate and a urethane (meth)acrylate, (b) layer D contains at least one of inorganic fine particles and a silicon compound hydrolysis condensate, (c) the total content of the polyfunctional (meth)acrylate and the urethane acrylate is 45% by mass to 97% by mass, and the total content of the inorganic fine particles and the silicon compound hydrolysis condensate is 3% by mass to 55% by mass, relative to the total amount of the polyfunctional (meth)acrylate, the urethane (meth)acrylate, the inorganic fine particles, and the silicon compound hydrolysis condensate, (d) The layer C includes the thermoplastic acrylic resin, and a cured product of at least one of the polyfunctional (meth)acrylate and the urethane (meth)acrylate.
2. The laminate film according to claim 1, wherein, when the amount of the thermoplastic acrylic resin in the layer C is X parts by mass and the total amount of the multifunctional (meth)acrylate and the urethane (meth)acrylate is Y parts by mass, Y / (X+Y) is 0.2 to 0.
9.
3. The laminate film according to claim 1 or 2, wherein the reaction rate of the double bonds of the (meth)acrylic groups of the polyfunctional (meth)acrylate and the urethane (meth)acrylate in the C layer is 25 to 70%.
4. The laminate film according to claim 1 or 2, wherein the ratio of the thickness of said C layer to the total thickness of said C layer and said D layer is 10 to 70%.
5. The laminate film according to claim 1 or 2, wherein the thickness of the C layer is 0.3 to 5.0 μm.
6. The laminate film according to claim 1 or 2, wherein the thickness of said layer D is 1.5 to 18 μm.
7. The laminate film according to claim 1 or 2, wherein the total thickness of the C layer and the D layer is 3 to 20 μm.
8. The laminate film according to claim 1 or 2, wherein the layer A contains a polyester-based thermoplastic elastomer, the polyester-based thermoplastic elastomer being composed of a hard segment consisting of a polybutylene terephthalate unit and a soft segment consisting of a polyester unit having an aromatic dicarboxylic acid and an aliphatic dicarboxylic acid as the dicarboxylic acid component and a diol having 5 to 15 carbon atoms as the diol component.
9. The laminate film according to claim 8, which contains 1 to 20 parts by weight of said polyester thermoplastic elastomer per 100 parts by weight of said polycarbonate resin.
10. A method for producing a laminated film according to claim 1, characterized in that a layer containing a polycarbonate resin (layer A) and a layer containing a thermoplastic acrylic resin (layer B) are laminated by co-extrusion, and then a coating composition containing an organic solvent, an active energy ray-curable acrylate, and at least one of inorganic fine particles and a silicon compound hydrolysis condensate is applied onto the layer B, and after drying the applied coating composition, an acrylic resin mixed intermediate layer (layer C) and a cured layer of acrylate (layer D) are formed.
11. The method for producing a laminated film according to claim 10, wherein the layer C contains the thermoplastic acrylic resin and a cured product of at least one of the polyfunctional (meth)acrylate and the urethane (meth)acrylate.
12. A resin molded product having a thermoplastic resin layer in contact with layer A of the laminated film according to claim 1.
13. A resin molded product obtained by injection molding a thermoplastic resin onto the surface of the layer A side of the laminated film according to claim 1.
Citation Information
Patent Citations
Multilayer film for sticking simultaneously with injection molding
JP2009234184A
Method of manufacturing in-mold decorative molded product, molded product manufactured thereby and decorative sheet
JP2010247493A
Active energy ray-curable composition and laminate
JP2010215843A
Resin film, resin laminate, and manufacturing method thereof
JP2014040017A
Polycarbonate resin laminate
JP2014162096A