Laminate and resin molded body containing same
The laminate with a urethane acrylate and hindered amine light stabilizer hard coat layer on an acrylic resin film addresses the limitations of poor formability and weather resistance, providing enhanced transparency, hardness, and long-term durability.
Patent Information
- Application Number
- PCT/JP2024/010061
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-14
- Publication Date
- 2024-10-03
AI Technical Summary
Existing laminates with hard coat layers on acrylic resin films suffer from poor secondary formability due to high crosslinking, which limits shape flexibility, and exhibit inadequate long-term weather resistance, especially in applications exposed to sunlight and weather.
A laminate comprising an acrylic resin film with a hard coat layer formed from a cured product of a curable resin composition containing urethane acrylate resin and a hindered amine light stabilizer with reactive functional groups, offering high tensile elongation and improved weather resistance.
The laminate achieves excellent transparency, surface hardness, chemical resistance, and long-term weather resistance, enabling flexible shaping and maintaining integrity under accelerated weathering tests without cracking.
Smart Images

Figure JP2024010061_03102024_PF_FP_ABST
Abstract
Description
Laminate and resin molded article including same
[0001] The present invention relates to a laminate containing an acrylic resin film and a resin molded article containing the same.
[0002] Acrylic resin films have excellent transparency, weather resistance, high formability that allows them to be laminated conforming to the surface of planar and / or three-dimensional substrates, adhesion, bonding, and printability to other substrates, and are therefore widely used in a variety of applications, such as surface protection and / or coloring and decoration of automotive interior materials, automotive exterior materials, optical components, home appliance components, architectural exterior materials, retroreflective materials, etc. Furthermore, when applying acrylic resin films to these applications, a hard coat layer is often provided to further improve surface hardness, scratch resistance, and chemical resistance to various solvents and chemicals. For example, Patent Document 1 describes a hard coat film having a substrate made of an acrylic resin film and a hard coat layer made of an electron beam-cured product of an electron beam-curable resin composition containing an electron beam-curable resin and a triazine-based ultraviolet absorber. Furthermore, Patent Document 2 describes a laminate that includes an acrylic resin film and a hard coat layer laminated on at least one surface of the acrylic resin film, the hard coat layer containing a urethane acrylate resin, and that has a crack elongation of 80% or more at 120°C.
[0003] JP 2012-207120 A International Publication No. 2022 / 185815
[0004] However, in the hard coat film described in Patent Document 1, in which a hard coat layer is provided on an acrylic resin film, the flexibility of the acrylic resin film is inhibited by the hard coat layer having a high degree of crosslinking, and secondary formability is poor, so there is a problem that there is a limitation on the shape that the hard coat film can be laminated on the surface. Also, in the case of the laminate described in Patent Document 2, for example, in the interior and exterior of an automobile, the long-term weather resistance in applications exposed to sunlight or wind and rain is not necessarily sufficient, and further improvement is required.
[0005] The present invention has been made in consideration of the above-mentioned problems, and provides a laminate that has good transparency, surface hardness, and chemical resistance, has high secondary formability, and is also excellent in long-term weather resistance, and can be used for surface protection of resin molded articles having flat and / or three-dimensional surfaces, and a resin molded article including the laminate.
[0006] One or more embodiments of the present invention relate to a laminate including an acrylic resin film and a hard coat layer laminated on at least one surface of the acrylic resin film, wherein the acrylic resin film has a tensile elongation at break of 200% or more at 120°C, the hard coat layer is formed of a cured product of a curable resin composition including a urethane acrylate resin and a hindered amine light stabilizer having a reactive functional group, and the laminate has a tensile crack elongation of 100% or more at 120°C.
[0007] One or more embodiments of the present invention relate to a resin molded product comprising the laminate and a thermoplastic resin substrate, wherein at least a portion of the thermoplastic resin substrate is covered with the laminate arranged so that the acrylic resin film faces the thermoplastic resin substrate.
[0008] According to the present invention, there are provided a laminate which has good transparency, surface hardness, and chemical resistance, has high secondary formability, and is also excellent in long-term weather resistance, and can be used for surface protection of a resin molded product having a flat and / or three-dimensional surface, and a resin molded product containing the laminate.
[0009] 1 is a schematic cross-sectional view of a laminate according to one embodiment of the present invention.
[0010] The inventors of the present invention conducted extensive research to solve the above-mentioned problems. As a result, they surprisingly discovered that, in a laminate including an acrylic resin film and a hard coat layer, by using an acrylic resin film having specific physical properties and forming the hard coat layer from a cured product of a specific curable resin composition containing a urethane acrylate resin and a hindered amine light stabilizer having a reactive functional group, the laminate has good transparency, surface hardness, and chemical resistance, and has improved post-formability and long-term weather resistance. Specifically, the laminate of one or more embodiments of the present invention has a tensile crack elongation of 100% or more at 120°C and high post-formability, making it suitable for use in, for example, molded articles having curved and / or three-dimensional shapes. Furthermore, the laminate of one or more embodiments of the present invention has improved long-term weather resistance by forming the hard coat layer from a cured product of a specific curable resin composition containing a urethane acrylate resin and a hindered amine light stabilizer having a reactive functional group. In particular, the laminate according to one or more preferred embodiments of the present invention is placed so that the hard coat layer side faces the light source, and a xenon lamp is used as the light source, and the irradiance is 180 W / m 2 An accelerated weathering test was conducted under conditions of a wavelength of 300 to 400 nm, in which 1000 cycles (total of 2000 hours) of a 120-minute cycle consisting of Step 1 with an exposure time of 102 minutes, a black panel temperature of 60±3°C, a relative humidity of 65±5%, and no rainfall, and Step 2 with an exposure time of 18 minutes, an internal temperature of 38±3°C, a relative humidity of 95±5%, and rainfall were performed (hereinafter also simply referred to as "accelerated weathering test"). Even in this case, no cracks were observed on the surface of the hard coat layer.
[0011] In this specification, when a numerical range is indicated with "to", the numerical range includes both end values (upper and lower limits). For example, a numerical range of "X to Y" includes both end values X and Y, and is the same range as "X or more and Y or less". Any number within that range and any range included within that range are specifically disclosed. In addition, when multiple numerical ranges are described in this specification, they are intended to include numerical ranges that combine the upper and lower limits of different numerical ranges as appropriate.
[0012] (Acrylic Resin Film) The acrylic resin film has a tensile breaking elongation of 200% or more at 120°C. This increases the tensile crack elongation at 120°C of the laminate with the hard coat layer, and tends to improve the secondary formability of the laminate. There is no particular upper limit to the tensile breaking elongation of the acrylic resin film at 120°C.
[0013] The acrylic resin film may have a tensile elongation at break of 200% or more at 120°C, and its composition is not particularly limited. However, it is preferable that the film be formed from an acrylic resin composition containing graft copolymer particles containing an acrylic resin and a rubber component (also referred to as a cross-linked elastomer).
[0014] <Acrylic Resin> Conventionally known acrylic resins can be used as appropriate. For example, from the viewpoint of hardness and moldability, it is preferable to use an acrylic resin (also referred to as a thermoplastic acrylic polymer) composed of 50 to 100% by mass of methyl methacrylate units and 0 to 50% by mass of other structural units, where the total amount of structural units of the acrylic resin is taken as 100% by mass. The total amount of methyl methacrylate units and other structural units in the thermoplastic acrylic polymer is 100% by mass.
[0015] Examples of the other structural units include structural units derived from acrylic acid, acrylic acid derivatives, methacrylic acid, methacrylic acid derivatives, aromatic vinyl derivatives, and vinyl cyanide derivatives. The other structural units may be glutarimide structures, lactone ring structures, N-substituted maleimide structures, and unsubstituted maleimide structures, which will be described later. The other structural units contained in the acrylic resin may be one type or a combination of two or more types.
[0016] Examples of acrylic acid derivatives include acrylic acid esters such as methyl acrylate, ethyl acrylate, n-propyl acrylate, n-butyl acrylate, isobutyl acrylate, cyclohexyl acrylate, 2-hydroxyethyl acrylate, 2-phenoxyethyl acrylate, benzyl acrylate, and glycidyl acrylate, but are not limited to these.
[0017] Examples of methacrylic acid derivatives include methacrylic acid esters such as ethyl methacrylate, n-propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, phenyl methacrylate, benzyl methacrylate, cyclohexyl methacrylate, 2-phenoxyethyl methacrylate, and isobornyl methacrylate, as well as reactive ultraviolet absorbers described below, but are not limited to these.
[0018] Examples of aromatic vinyl derivatives include, but are not limited to, styrene, vinyltoluene, and α-methylstyrene.
[0019] Vinyl cyanide derivatives include, but are not limited to, acrylonitrile, methacrylonitrile, and the like.
[0020] In order to improve the heat resistance, rigidity, surface hardness, etc. of the acrylic resin, a structural unit having a specific structure may be introduced into the acrylic resin by copolymerization, functional group modification, denaturation, etc. Examples of such specific structures include glutarimide structures as disclosed in JP-A-62-89705, JP-A-02-178310, WO 2005 / 54311, etc., lactone ring structures as disclosed in JP-A-2004-168882 and JP-A-2006-171464, etc., glutaric anhydride structures obtained by thermal cyclocondensation of (meth)acrylic acid units as disclosed in JP-A-2004-307834, etc., maleic anhydride structures as disclosed in JP-A-5-119217, and N-substituted maleimide structures and unsubstituted maleimide structures as disclosed in WO 2009 / 84541. For example, by introducing these structures into acrylic resins, the molecular chains become rigid, which can be expected to result in improved heat resistance, improved surface hardness, reduced heat shrinkage, improved chemical resistance, and other effects.
[0021] The method for producing the acrylic resin is not particularly limited, and can be, for example, a known polymerization method such as suspension polymerization, bulk polymerization, solution polymerization, emulsion polymerization, etc. Also, any of a known radical polymerization, living radical polymerization, anionic polymerization, and cationic polymerization can be used.
[0022] In 100% by mass of the acrylic resin film, the content of the acrylic resin may be 20 to 100% by mass, preferably 20 to 99% by mass, more preferably 25 to 95% by mass, and even more preferably 30 to 90% by mass.
[0023] <Graft Copolymer Containing Rubber Component> The acrylic resin film preferably contains, as the graft copolymer particles containing a rubber component, graft copolymer particles (A) having an average particle size of 20 to 200 nm. In this case, the acrylic resin film preferably contains the graft copolymer particles (A) dispersed in a matrix containing an acrylic resin or an acrylic resin and other components. Furthermore, the acrylic resin film may contain, as the graft copolymer particles containing a rubber component, in addition to the graft copolymer particles (A), graft copolymer particles (B) having an average particle size larger than that of the graft copolymer particles (A), as necessary. In this case, the acrylic resin film preferably contains the graft copolymer particles (A) and the graft copolymer particles (B) dispersed in a matrix containing an acrylic resin or an acrylic resin and other components.
[0024] The graft copolymer particles (A) preferably have a core-shell structure (multilayer structure) including a crosslinked elastomer (A1) as a rubber component and a graft polymer layer (A2) located on the surface layer side of the crosslinked elastomer (A1).
[0025] The crosslinked elastomer (A1) may be a known crosslinked elastomer. Preferably, the crosslinked elastomer (A1) is an acrylate ester-based crosslinked elastomer (a crosslinked elastomer composed of a polymer containing an acrylate ester as a main component). In this specification, the term "main component" refers to a component whose content is 50% by mass or more.
[0026] The particles of the acrylic acid ester-based crosslinked elastomer (A1) may have a concentric spherical multilayer structure in which a hard or semi-hard crosslinked resin layer is provided inside a crosslinked elastomer layer. Examples of such hard or semi-hard crosslinked resin layers include hard crosslinked methacrylic resin particles as disclosed in JP-B-55-27576, semi-hard crosslinked particles made of methyl methacrylate-acrylic acid ester-styrene as disclosed in JP-A-4-270751, and highly crosslinked rubber particles. The provision of such a hard or semi-hard crosslinked resin layer may be expected to improve transparency, color tone, and the like.
[0027] The graft copolymer particles (A) preferably have a core-shell structure formed by graft polymerizing a monomer mixture that forms the graft polymer layer (A2) in the presence of particles of the above-mentioned acrylic acid ester-based crosslinked elastomer (A1).
[0028] The average particle size of the graft copolymer particles (A) may be 20 to 200 nm, preferably 50 to 150 nm, and particularly preferably 50 to 120 nm. If the average particle size of the graft copolymer particles (A) is too small, the impact resistance and bending crack resistance of the acrylic resin film tend to decrease. If the average particle size of the graft copolymer particles (A) is too large, the transparency of the acrylic resin film tends to decrease and whitening due to bending tends to occur.
[0029] As the acrylic acid ester-based crosslinked elastomer (A1), crosslinked elastomer particles obtained by polymerizing a monomer mixture (a-1) containing (a) an acrylic acid ester, (b) a polyfunctional monomer copolymerizable with the acrylic acid ester and having two or more non-conjugated double bonds per molecule, and (c) optionally another vinyl-based monomer copolymerizable with the acrylic acid ester can be preferably used.
[0030] The acrylic acid ester, the other vinyl monomer, and the polyfunctional monomer may be mixed and polymerized in one step. Alternatively, for the purpose of adjusting the toughness, whitening resistance, etc. of the acrylic resin film, the acrylic acid ester, the other vinyl monomer, and the polyfunctional monomer may be polymerized in two or more stages by appropriately changing the composition of the acrylic acid ester, the other vinyl monomer, and the polyfunctional monomer or by keeping the same composition.
[0031] As the acrylic acid ester, from the viewpoints of excellent polymerizability, low cost, and ability to give a polymer with a low Tg, aliphatic esters of acrylic acid are preferred, alkyl acrylate esters are more preferred, and alkyl acrylate esters in which the alkyl group has 1 to 22 carbon atoms are particularly preferred. The alkyl group may have any of a linear, branched, and cyclic (also referred to as alicyclic) structure.
[0032] Specific examples of preferred alkyl acrylates include methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, isobornyl acrylate, cyclohexyl acrylate, dodecyl acrylate, stearyl acrylate, heptadecyl acrylate, and octadecyl acrylate, etc. These may be used alone or in combination of two or more.
[0033] The amount of the acrylic acid ester (preferably an alkyl acrylate, more preferably an alkyl acrylate having an alkyl group containing 1 to 22 carbon atoms) is preferably 50 to 99.9% by mass, more preferably 70 to 99% by mass, and most preferably 80 to 99% by mass, based on 100% by mass of the monomer mixture (a-1). When the amount of the acrylic acid ester is 50% by mass or more, the acrylic resin film has good impact resistance and elongation at tensile break, and is less likely to crack during secondary molding.
[0034] Examples of other vinyl monomers include methacrylic acid esters such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, phenyl methacrylate, benzyl methacrylate, cyclohexyl methacrylate, phenoxyethyl methacrylate, isobornyl methacrylate, and dicyclopentenyl methacrylate; vinyl cyanide derivatives such as acrylonitrile and methacrylonitrile; aromatic vinyl derivatives such as styrene, vinyl toluene, and α-methylstyrene; acrylic acid; acrylic acid derivatives such as β-hydroxyethyl acrylate, phenoxyethyl acrylate, benzyl acrylate, and glycidyl acrylate; methacrylic acid; methacrylic acid derivatives such as β-hydroxyethyl methacrylate, dimethylaminoethyl methacrylate, and glycidyl methacrylate; maleic anhydride; and maleic acid derivatives such as N-alkylmaleimide and N-phenylmaleimide. These may be used alone or in combination of two or more. Among these, from the viewpoints of weather resistance and transparency, one or more monomers selected from the group consisting of methacrylic acid esters and aromatic vinyl derivatives are particularly preferred as the other vinyl monomer.
[0035] The amount of the other vinyl monomer is preferably 0 to 49.9% by mass, more preferably 0 to 30% by mass, and even more preferably 0 to 20% by mass, based on 100% by mass of the monomer mixture (a-1). If the amount of the other vinyl monomer exceeds 49.9% by mass, the impact resistance of the acrylic resin film is likely to decrease, the elongation at tensile break is reduced, and cracks may be more likely to occur during secondary molding.
[0036] As the polyfunctional monomer, a monomer typically used as a crosslinking agent and / or a grafting agent can be suitably used. Examples of the polyfunctional monomer include allyl methacrylate, allyl acrylate, triallyl cyanurate, triallyl isocyanurate, diallyl phthalate, diallyl maleate, divinyl adipate, divinylbenzene, ethylene glycol dimethacrylate, propylene glycol dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, trimethylolpropane trimethacrylate, polyethylene glycol dimethacrylate, and dipropylene glycol dimethacrylate. These polyfunctional monomers may be used alone or in combination of two or more.
[0037] Among these polyfunctional monomers, those having the function of a graft crosslinking agent are more preferred because they increase the number of graft bonds of the graft polymer layer (A2) described below to the crosslinked elastomer (A1), resulting in good dispersibility of the graft copolymer particles (A) in the acrylic resin, improving the crack resistance of the acrylic resin film against tensile and bending deformation and reducing stress whitening. As such polyfunctional monomers having the function of a graft crosslinking agent, those having an allyl group such as allyl methacrylate, allyl acrylate, triallyl cyanurate, triallyl isocyanurate, diallyl phthalate, and diallyl maleate are preferred, with allyl methacrylate, allyl acrylate, etc. being particularly preferred.
[0038] The amount of the polyfunctional monomer is preferably 0.1 to 10% by mass, and more preferably 1.0 to 4% by mass, based on 100% by mass of the monomer mixture (a-1). The amount of the polyfunctional monomer within this range is preferable from the viewpoints of the resistance to cracking and whitening upon bending of the acrylic resin film, and the fluidity of the resin during molding.
[0039] In the acrylic ester-based crosslinked elastomer (A1), the amount of the polyfunctional monomer may be varied between the interior and the surface vicinity of the crosslinked elastomer (A1) for the purpose of increasing the graft coating efficiency of the graft polymer layer (A2) described below. Specifically, as shown in Japanese Patent No. 1460364 and Japanese Patent No. 1786959, by increasing the content of the polyfunctional monomer functioning as a graft crosslinking agent in the surface vicinity of the crosslinked elastomer (A1) compared to the interior, it is possible to improve the coating of the graft copolymer particles (A) with the graft polymer layer, improve dispersibility in the acrylic resin, and suppress a decrease in crack resistance due to peeling at the interface between the graft copolymer particles (A) and the acrylic resin. Furthermore, since a sufficient coating can be obtained with a relatively small amount of the graft polymer layer (A2), the amount of the graft copolymer particles (A) required to introduce a predetermined amount of the crosslinked elastomer (A1) into the acrylic resin composition can be reduced, thereby lowering the melt viscosity of the acrylic resin composition and expecting improvements in the melt processability, film processing accuracy, and surface hardness of the acrylic resin film.
[0040] A chain transfer agent may be used in addition to the monomer mixture (a-1) for the purposes of controlling the molecular weight and crosslink density of the acrylate ester-based crosslinked elastomer (A1) and controlling thermal stability and the like by reducing the double bond terminals of the polymer due to the disproportionation termination reaction during polymerization. The chain transfer agent can be selected from those typically used in radical polymerization. Preferred examples of the chain transfer agent include monofunctional or polyfunctional mercaptan compounds having 2 to 20 carbon atoms, such as n-octyl mercaptan, n-dodecyl mercaptan, and t-dodecyl mercaptan; mercapto acids; thiophenol; carbon tetrachloride; and mixtures thereof. The amount of the chain transfer agent added is preferably 0 to 1.0 part by mass, more preferably 0 to 0.2 part by mass, per 100 parts by mass of the total amount of the monomer mixture (a-1).
[0041] The particles of the crosslinked elastomer (A1) may be a single layer made of the above-mentioned acrylic ester-based crosslinked elastomer (A1), or may have a multilayer structure including two or more layers made of the above-mentioned acrylic ester-based crosslinked elastomer (A1).
[0042] The particles of the crosslinked elastomer (A1) may also be multilayer particles containing a hard or semi-hard crosslinked resin layer, and the acrylate ester crosslinked elastomer (A1) may be contained in at least one layer of the multilayer particles. Examples of monomers constituting the hard or semi-hard crosslinked resin layer include methacrylates such as methyl methacrylate, ethyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, benzyl methacrylate, and phenoxyethyl methacrylate; acrylic acid alkyl esters such as methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate; aromatic vinyl derivatives such as styrene and α-methylstyrene; vinyl cyanide derivatives such as acrylonitrile; maleic anhydride; maleic acid derivatives such as maleimides; and polyfunctional monomers having two or more non-conjugated double bonds per molecule. The polyfunctional monomer may be the same as that used in the polymerization of the acrylate ester-based crosslinked elastomer (A1) layer. Among these, one or more selected from the group consisting of methyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, styrene, and acrylonitrile are particularly preferred. Furthermore, during polymerization of the hard or semi-hard crosslinked resin layer, a chain transfer agent may be used in addition to these monomers to control the crosslink density and to control thermal stability by reducing the double bond terminals of the polymer. The same chain transfer agents as those used in the polymerization of the acrylate ester-based crosslinked elastomer (A1) layer can be used. The amount of chain transfer agent added is preferably 0 to 2 parts by mass, more preferably 0 to 0.5 parts by mass, per 100 parts by mass of the total monomer mixture constituting the hard or semi-hard crosslinked resin layer.
[0043] When the graft copolymer particle (A) has a two-layer structure consisting of a particle of crosslinked elastomer (A1) as a core particle and a graft polymer layer (A2), the graft copolymer particle (A) can typically be obtained by graft copolymerizing a monomer mixture (a-2) containing 50 to 100% by mass of a methacrylic acid ester and 0 to 50% by mass of another vinyl-based monomer copolymerizable with the methacrylic acid ester (provided that the total of the methacrylic acid ester and the other vinyl-based monomer is 100% by mass) in the presence of particles of crosslinked elastomer (A1) to form the graft polymer layer (A2).
[0044] The amount of the methacrylic acid ester in 100% by mass of the monomer mixture (a-2) is preferably 60% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 97% by mass or more, from the viewpoints of (a) ensuring compatibility with the acrylic resin matrix, and (b) preventing a decrease in toughness of the film due to solvent impregnation during coating on the acrylic resin film, and preventing whitening and cracking due to stretching during molding.
[0045] In the monomer mixture (a-2), examples of the methacrylic acid ester include alkyl methacrylates such as methyl methacrylate, ethyl methacrylate, propyl methacrylate, n-butyl methacrylate, isobutyl methacrylate, t-butyl methacrylate, hexyl methacrylate, cyclohexyl methacrylate, 2-ethylhexyl methacrylate, octyl methacrylate, phenyl methacrylate, and benzyl methacrylate. Among these, alkyl methacrylates in which the alkyl group has 1 to 4 carbon atoms are preferred.
[0046] In the monomer mixture (a-2), the other vinyl-based monomer can be an alkyl acrylate ester in which the alkyl group has 2 or more carbon atoms. As the alkyl acrylate ester in which the alkyl group has 2 or more carbon atoms, for example, one or more selected from the group consisting of ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, t-butyl acrylate, hexyl acrylate, cyclohexyl acrylate, octyl acrylate, dodecyl acrylate, and stearyl acrylate are preferred, one or more selected from the group consisting of ethyl acrylate, n-butyl acrylate, isobutyl acrylate, and t-butyl acrylate are more preferred, and n-butyl acrylate is particularly preferred.
[0047] In the monomer mixture (a-2), examples of other vinyl-based monomers that can be used include aromatic vinyl derivatives such as styrene and its nuclear-substituted derivatives, vinyl cyanide derivatives such as acrylonitrile, methacrylic acid and its derivatives, acrylic acid and its derivatives, N-substituted maleimides, maleic anhydride, methacrylamide, and acrylamide.
[0048] The monomer mixture (a-2) preferably contains a reactive ultraviolet absorber as another vinyl monomer. That is, the graft polymer layer (A2) preferably contains a structural unit derived from the reactive ultraviolet absorber. When the monomer mixture (a-2) contains a reactive ultraviolet absorber, it is easy to obtain an acrylic resin film having good weather resistance and chemical resistance.
[0049] The reactive ultraviolet absorber is not particularly limited and may be any known reactive ultraviolet absorber. In terms of the moldability and weather resistance of the acrylic resin film, the reactive ultraviolet absorber is preferably a compound represented by the following general formula (1):
[0050]
[0051] In general formula (1), X is a hydrogen atom or a halogen atom, R1 is a hydrogen atom, a methyl group, or a t-alkyl group having 4 to 6 carbon atoms, R2 is a linear or branched alkylene group having 2 to 10 carbon atoms, and R3 is a hydrogen atom or a methyl group.
[0052] Specific examples of reactive ultraviolet absorbers represented by general formula (1) include 2-(2'-hydroxy-5'-(meth)acryloyloxyethylphenyl)-2H-benzotriazoles, more specific examples include 2-(2'-hydroxy-5'-acryloyloxyethylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-5-chloro-2H-benzotriazole, 2-(2'-hydroxy-5'-methacryloyloxypropylphenyl)-2H-benzotriazole, and 2-(2'-hydroxy-5'-methacryloyloxyethyl-3'-t-butylphenyl)-2H-benzotriazole. Preferably, 2-(2'-hydroxy-5'-methacryloyloxyethylphenyl)-2H-benzotriazole is used in terms of cost and ease of handling. In this specification, (meth)acryloyl is a general term for acryloyl and methacryloyl.
[0053] The content of the structural unit derived from the reactive ultraviolet absorber in 100% by mass of the graft polymer layer (A2) is preferably from 0.01 to 5% by mass, and more preferably from 0.1 to 3% by mass.
[0054] The graft polymer layer (A2) is preferably obtained by graft copolymerizing, in at least one stage, 10 to 95 parts by mass of a monomer mixture (a-2) containing 70 to 99.5% by mass of an alkyl methacrylate, 0.5 to 30% by mass of an alkyl acrylate having an alkyl group containing two or more carbon atoms, and 0 to 19% by mass of other vinyl monomers (provided that the total of the alkyl methacrylate, alkyl acrylate, and other vinyl monomers is 100% by mass), in the presence of 5 to 90 parts by mass of crosslinked elastomer particles (A1), provided that the total amount of the particles of the crosslinked elastomer (A1) and the monomer mixture (a-2) is 100 parts by mass.
[0055] In the production of graft copolymer particles (A), particularly during the graft copolymerization of monomer mixture (a-2) in the presence of particles of crosslinked elastomer (A1), for example, particles of acrylate ester-based crosslinked elastomer (A1), polymer components (free polymers) that are not graft-bonded to the particles of acrylate ester-based crosslinked elastomer (A1) may be generated. Such free polymers can be used to constitute part or all of the acrylic resin that constitutes the matrix phase of acrylic resin compositions and acrylic resin films.
[0056] A chain transfer agent may be added to the monomer mixture (a-2) for the purposes of controlling the molecular weight of the polymer, controlling the graft rate to the crosslinked elastomer (A1) and the amount of free polymer not bonded to the crosslinked elastomer (A1) produced, and controlling thermal stability by reducing the double bond terminals of the polymer accompanying a disproportionation termination reaction during polymerization. The same chain transfer agents as those usable in the polymerization of the crosslinked elastomer (A1) can be used as such chain transfer agents. The amount of the chain transfer agent used is preferably 0 to 2 parts by mass or less, more preferably 0 to 0.5 parts by mass, per 100 parts by mass of the total amount of the monomer mixture (a-2).
[0057] The graft ratio of the monomer mixture (a-2) to the particles of the crosslinked elastomer (A1), i.e., the graft ratio of the graft copolymer particles (A), is preferably 5 to 250%, more preferably 10 to 200%, and even more preferably 20 to 150%. If the graft ratio is less than 5%, the acrylic resin film tends to have reduced resistance to whitening upon folding, reduced transparency, and reduced elongation at tensile break, making it more susceptible to cracking during secondary molding. If the graft ratio exceeds 250%, the melt viscosity of the acrylic resin composition tends to increase during film molding, resulting in reduced moldability of the acrylic resin film. Herein, the graft ratio of the graft copolymer particles (A) can be calculated by dissolving the powder of the graft copolymer particles (A) in methyl ethyl ketone, separating it into an insoluble and a soluble fraction, and using the insoluble fraction as the graft fraction, according to the following formula: Graft ratio (%)=(mass of insoluble matter−mass of crosslinked elastomer (A1)) / mass of crosslinked elastomer (A1)×100
[0058] The average particle size d (nm) of the acrylic acid ester-based crosslinked elastomer (A1) in the acrylic resin film and the amount w (mass %) of the polyfunctional monomer used in the acrylic acid ester-based crosslinked elastomer (A1) preferably satisfy the relationship: 0.015d≦w≦0.06d, more preferably 0.02d≦w≦0.05d. When the amount of the polyfunctional monomer is within the range of the above relationship, the acrylic resin film has advantages such as being less likely to reduce in elongation during secondary forming, being less likely to crack during molding or cutting, having excellent transparency, being less likely to suffer from stress whitening during bending or tensile deformation at room temperature (about 25°C), at high temperatures above the softening temperature of the acrylic resin film, or in a temperature range between room temperature and the Tg of the crosslinked elastomer (A1), and being less likely to suffer from moisture-induced clouding or whitening of the film due to moisture penetrating into the acrylic resin film upon contact with moisture.
[0059] Like the graft copolymer particles (A), the graft copolymer particles (B) also include a crosslinked elastomer (B1) as a rubber component. Like the graft copolymer particles (A), the graft copolymer particles (B) typically include a graft polymer layer (B2) located on the surface layer side of the crosslinked elastomer (B1). That is, the graft copolymer particles (B) preferably include a crosslinked elastomer (B1) and a graft polymer layer (B2).
[0060] The graft copolymer particles (B) may be generally similar to the graft copolymer particles (A) in terms of raw materials, production method, etc., except that the average particle size of the graft copolymer particles (B) is larger than that of the graft copolymer particles (A). Preferably, the particles of the acrylic ester-based crosslinked elastomer (B1) have a concentric spherical multilayer structure comprising a crosslinked elastomer layer and a hard or semi-hard crosslinked resin layer inside. Examples of such a hard or semi-hard crosslinked resin layer include hard crosslinked methacrylic resin particles as disclosed in JP-B-55-27576 and crosslinked particles having a semi-hard layer made of a methyl methacrylate-acrylic ester-styrene copolymer as disclosed in JP-A-4-270751 and WO 2014 / 41803. The incorporation of such a hard or semi-hard crosslinked resin layer can improve the transparency, resistance to whitening upon bending, resistance to cracking upon bending, etc., of the graft copolymer particles (B) having a particle size larger than that of the graft copolymer particles (A).
[0061] The average particle size of the graft copolymer particles (B) is preferably 150 to 400 nm, more preferably 200 to 350 nm. Graft copolymer particles (B) with a large average particle size more effectively induce plastic deformation (craze) in the acrylic resin phase surrounding the graft copolymer particles in response to the action of external force on the acrylic resin material. Therefore, the graft copolymer particles (B) are extremely effective in imparting impact resistance and crack resistance to the acrylic resin material. On the other hand, the graft copolymer particles (B) are inferior to the graft copolymer particles (A) in resistance to whitening due to folding and / or resistance to whitening due to solvents. For this reason, for example, by adding a small amount of graft copolymer particles (B) to an acrylic resin composition containing an acrylic resin and graft copolymer particles (A), (a) the total content of soft components in the acrylic resin film is lowered, thereby preventing a decrease in the surface hardness of the acrylic resin film and laminate, (b) the whitening tendency when an external stress is applied to the acrylic resin film, when a coating liquid containing an organic solvent is applied, and / or during molding processing is less likely to deteriorate, and (c) the cracking resistance, secondary formability, etc. of the acrylic resin film and laminate can be expected to be efficiently improved.
[0062] In this specification, the average particle size of the graft copolymer particles (A) and the graft copolymer particles (B) refers to the average particle size on a volume basis (also referred to as a mass basis if the density is uniform), and can be measured in a latex state by a dynamic light scattering method using a laser diffraction particle size distribution analyzer such as Microtrac particle size distribution analyzer MT3000 manufactured by Nikkiso Co., Ltd.
[0063] The method for producing the graft copolymer particles (A) and the graft copolymer particles (B) is not particularly limited, and known methods such as emulsion polymerization, mini-emulsion polymerization, suspension polymerization, and solution polymerization can be applied. Emulsion polymerization is particularly preferred because it allows for a wide range of adjustment of the resin structure.
[0064] The initiator used in the emulsion polymerization of the graft copolymer particles (A) and / or the graft copolymer particles (B) can be any known initiator, such as an organic peroxide, an inorganic peroxide, or an azo compound. Specific examples include organic peroxides such as t-butyl hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, benzoyl peroxide, lauroyl peroxide, alkyl peroxycarbonates, and alkyl peroxy esters; inorganic peroxides such as potassium persulfate, sodium persulfate, and ammonium persulfate; and azo compounds such as azobisisobutyronitrile. These initiators may be used alone or in combination of two or more.
[0065] These initiators may be used (a) as thermal decomposition type radical polymerization initiators, or (b) as redox type polymerization initiator systems in which these initiators are combined with a catalyst such as ferrous sulfate and a reducing agent such as sodium sulfite, sodium thiosulfate, sodium formaldehyde sulfoxylate, ascorbic acid, hydroxyacetone, etc. The catalyst may be used as a complex with 2-sodium ethylenediaminetetraacetate or the like to ensure water solubility.
[0066] The surfactant (also referred to as an emulsifier) used in the emulsion polymerization of the graft copolymer particles (A) and / or the graft copolymer particles (B) is not particularly limited. A wide variety of known surfactants can be used in emulsion polymerization. Preferred surfactants include, for example, (a) anionic surfactants such as sodium salts, potassium salts, and ammonium salts of alkyl sulfonic acid, alkyl benzene sulfonic acid, dialkyl sulfosuccinic acid (dioctyl sulfosuccinic acid, etc.), alkyl sulfate, fatty acid sodium salt, polyoxyethylene alkyl ether acetate, polyoxyethylene alkyl ether phosphate, alkyl phosphate, alkyl ether phosphate, alkyl phenyl ether phosphate, and surfactin; and (b) nonionic surfactants such as reaction products of alkylphenols and aliphatic alcohols with propylene oxide and / or ethylene oxide. These surfactants may be used alone or in combination of two or more.
[0067] The graft copolymer particles (A) or (B) can be separated and recovered from the latex of the graft copolymer particles (A) or (B) obtained by emulsion polymerization by a known method. For example, after adding a water-soluble electrolyte such as calcium chloride, magnesium sulfate, magnesium chloride, calcium acetate, sodium chloride, hydrochloric acid, acetic acid, or sulfuric acid to the latex to coagulate the graft copolymer particles, or after freezing the latex to separate and coagulate the graft copolymer particles from the aqueous phase, the graft copolymer particles (A) or (B) can be separated and recovered by filtering, washing, and drying the solids. Alternatively, the graft copolymer particles (A) or (B) can be separated and recovered by treating the latex with spray drying, freeze-drying, or the like.
[0068] For the purpose of reducing appearance defects and / or internal foreign matter in the acrylic resin film, preferably, prior to separation and recovery of the graft copolymer particles (A) or the graft copolymer particles (B), the latex of the graft copolymer particles (A) or the latex of the graft copolymer particles (B) is filtered in advance with a filter and / or a mesh to remove substances that may cause foreign matter defects, such as environmental foreign matter and polymerization scale.
[0069] The filter and mesh may be any known filter or mesh material used for filtering liquid media. The filter and mesh types, mesh openings, filtering accuracy, and filtering capacity are appropriately selected depending on the intended application and the type, size, and amount of foreign matter to be removed. The filter and mesh openings and filtering accuracy are preferably at least twice the average particle size of the graft copolymer particles (A) or the graft copolymer particles (B), respectively.
[0070] The content of the graft copolymer particles (A) in 100% by mass of the acrylic resin film is not particularly limited, but is preferably 1 to 80% by mass, more preferably 5 to 70% by mass, and even more preferably 10 to 60% by mass.
[0071] The content of the graft copolymer particles (B) in 100% by mass of the acrylic resin film is not particularly limited and can be appropriately adjusted within a preferred range depending on the intended use without impairing the quality of the laminate of the present invention, but from the viewpoint of suppressing stress whitening during stretching or bending of the acrylic resin film and clouding of the film after contact with moisture, it is desirable not to use an excessive amount, and the content is preferably 0 to 20% by mass, more preferably 0 to 10% by mass, and most preferably 0 to 5% by mass. Alternatively, the acrylic resin film may contain no graft copolymer particles (B) at all.
[0072] <Other Components> The acrylic resin film (the acrylic resin composition constituting the acrylic resin film) may contain, as necessary, a thermoplastic resin that is at least partially compatible with the acrylic resin, as long as the object of the present invention is not impaired. Examples of such thermoplastic resins include styrene-based resins, polycarbonate resins, amorphous saturated polyester resins, olefin-methacrylic acid derivative resins, olefin-acrylic acid derivative resins, polyimide resins, polylactic acid resins, and PHBH (poly(3-hydroxybutyrate-co-3-hydroxyhexanoate)) resins. Examples of styrene-based resins include styrene-acrylonitrile resins, styrene-(meth)acrylic acid resins, styrene-maleic anhydride resins, styrene-N-substituted or unsubstituted maleimide resins, styrene-acrylonitrile-butadiene resins, and styrene-acrylonitrile-acrylic ester resins. Among these, one or more thermoplastic resins selected from the group consisting of styrene-based resins, polycarbonate resins, and polyimide resins are preferred because they have excellent compatibility with acrylic resins and may be able to improve the acrylic resin film's resistance to cracking due to bending, solvent resistance, chemical resistance, low moisture absorption, etc. In this specification, (meth)acrylic acid is a general term for acrylic acid and methacrylic acid.
[0073] The acrylic resin film (the acrylic resin composition constituting the acrylic resin film) may also contain, as necessary, conventionally known additives used in acrylic resin films, as long as they do not impair the objectives of one embodiment of the present invention. Examples of such additives include antioxidants, ultraviolet absorbers (hereinafter also referred to as UVAs), light stabilizers, light diffusing agents, matting agents, lubricants, colorants such as pigments and dyes, fibrous fillers, antiblocking agents composed of organic particles and / or inorganic particles, infrared reflectors composed of metals and / or metal oxides, plasticizers, and antistatic agents. The additives are not limited to these. These additives can be used in any amount depending on the type of additive, as long as they do not impair the objectives of one embodiment of the present invention or to enhance the effects of one embodiment of the present invention.
[0074] <Physical Properties of Acrylic Resin Film> The glass transition temperature (Tg) of the acrylic resin film is preferably 145°C or lower, more preferably 140°C or lower, even more preferably 135°C or lower, and particularly preferably 130°C or lower. An acrylic resin film having a glass transition temperature of 145°C or lower has the advantage that molding is possible without increasing the molding temperature and that cracking during molding can be suppressed. The lower limit of the glass transition temperature of the acrylic resin film is not particularly limited, but is preferably 100°C or higher from the viewpoint of preventing printing misalignment during drying and improving reliability. More specifically, the glass transition temperature of the acrylic resin film may be 100 to 145°C, 100 to 140°C, 100 to 135°C, or 100 to 130°C. In this specification, the glass transition temperature of the acrylic resin film is measured by the method described in the examples.
[0075] The thickness of the acrylic resin film is not particularly limited, but is preferably 50 to 500 μm, more preferably 75 to 350 μm, even more preferably 80 to 300 μm, and particularly preferably 100 to 300 μm. When the thickness of the acrylic resin film is within the above-mentioned range, the film has sufficient stretchability and excellent handleability, and has the advantage of excellent appearance after lamination on a resin substrate during production of a molded product. In this specification, the thickness of the acrylic resin film is measured by the method described in the examples.
[0076] The pencil hardness of the acrylic resin film measured in accordance with JIS K 5600-5-4 under a load of 500 g is preferably 2B or more, more preferably B or more, and particularly preferably HB or more, from the viewpoint of excellent scratch resistance.
[0077] <Method for producing acrylic resin film> The acrylic resin film can be produced by a known processing method. Specific examples of known processing methods include melt processing, calendar molding, press molding, and solvent casting. Examples of melt processing methods include inflation and T-die extrusion. In the solvent casting method, for example, an acrylic resin composition is dissolved and dispersed in a solvent, and the resulting dispersion (dope) is then cast in the form of a film onto a belt-shaped substrate. Next, the solvent is volatilized from the cast film-like dope to obtain an acrylic resin film.
[0078] Among these methods, the melt processing method, which does not use a solvent, is preferred, and in particular, the T-die extrusion method and the calendar molding method are preferred. The melt processing method has few limitations on the thickness of the film to be produced, can produce a film with excellent surface properties with high productivity, and can reduce the burden on the natural environment and working environment caused by solvents, as well as the production cost.
[0079] When the acrylic resin composition is formed into a film by a melt processing method or a solvent casting method, it is preferable to remove environmental foreign matter, polymerization scale, deteriorated resin, and the like from the acrylic resin composition by filtration using a filter or mesh, which may cause defects in the appearance of the acrylic resin film or internal foreign matter, from the viewpoint of improving the appearance quality of the acrylic resin film.
[0080] In producing a film by melt processing, the acrylic resin composition can be filtered at any one or more of the following times: when melt-kneading the acrylic resin composition after blending raw materials such as the acrylic resin and the graft copolymer particles, and during the melt film formation process using a T-die. In addition, in the solvent casting method, the acrylic resin composition may be filtered after mixing the acrylic resin, the graft copolymer particles (A), the graft copolymer particles (B), and other components with a solvent and before cast film formation.
[0081] As such filters and meshes, known filters and meshes can be used without any particular limitation, as long as the filters and meshes have heat resistance and durability according to the melt processing conditions, and resistance to the solvents and dopes used for casting.
[0082] When producing an acrylic resin film by melt processing, a filter with a large filtration capacity and little retention of molten resin, which can cause resin deterioration and crosslinking that impair the quality of the film, is preferred, particularly in order to obtain a high-quality acrylic resin film. For example, the use of a leaf disk-type filter or a pleated-type filter is preferred from the viewpoints of filtration efficiency and productivity.
[0083] When producing an acrylic resin film by T-die extrusion, in order to improve the thickness accuracy of the film, for example, an automatic die device can be used that measures the film thickness distribution in the TD direction (direction perpendicular to the extrusion direction) of the extruded film online and automatically adjusts the lip clearance of the T-die during extrusion based on this. By applying an automatic die using an appropriate control method, it is possible to improve the thickness accuracy of the acrylic resin film.
[0084] In the production of acrylic resin films, if necessary, both sides of the molten film can be simultaneously contacted (sandwiched) with a cooling roll or cooling belt during film molding to obtain a film with superior surface properties. In this case, it is preferable to simultaneously contact the molten film with a roll or cooling belt maintained at a temperature equal to or higher than the glass transition temperature of the acrylic resin composition, preferably equal to or higher than the glass transition temperature of the acrylic resin composition, minus 80°C, and preferably equal to or higher than the glass transition temperature of the acrylic resin composition, minus 70°C. More preferably, at least one of the rolls used for such sandwiching is a roll having an elastic metal sleeve, as disclosed in, for example, JP-A Nos. 2000-153547 and 1999-235747, and a low sandwiching pressure is used to transfer a roll mirror finish or a specific surface shape. This allows for the production of (a) a film with little residual strain and excellent smoothness, and / or (b) a film with a moderate surface roughness, excellent film surface slipperiness, suppressed film-to-film blocking, and reduced internal strain.
[0085] Depending on the purpose, the film may be uniaxially or biaxially stretched after molding. The uniaxial or biaxial stretching can be performed using a known stretching device. The biaxial stretching can be performed in a known manner, such as sequential biaxial stretching, simultaneous biaxial stretching, or a method in which, after longitudinal stretching, transverse stretching is performed while relaxing the longitudinal direction to suppress the bowing phenomenon of the film.
[0086] Furthermore, depending on the application, one or both sides of the acrylic resin film may be given any surface shape, such as hairlines, prisms, unevenness, three-dimensional decoration, a matte surface, a rough surface with a certain surface roughness, or knurling on the film edge. Such surface shapes can be given by known methods. For example, a molten film immediately after extrusion or both sides of a formed film unwound from a unwinding device are sandwiched between two rolls or belts having a surface shape on at least one surface, thereby transferring the surface shape of the roll.
[0087] (Hard Coat Layer) The hard coat layer is formed from a cured product of a curable resin composition containing a urethane acrylate resin and a hindered amine-based light stabilizer having a reactive functional group. Specifically, the hard coat layer is formed by laminating a curable resin composition containing a urethane acrylate resin and a hindered amine-based light stabilizer having a reactive functional group on the surface of an acrylic resin film and then curing the composition. The hard coat layer may be laminated on one side or both sides of the acrylic resin film. The curable resin composition for the hard coat layer preferably has active energy curability, and the urethane acrylate resin preferably has active energy curability, from the viewpoints of not requiring a large-scale heating device or the like, rapid curing, and low cost.
[0088] In the laminate of one or more embodiments of the present invention, the hard coat layer is required to have high crack elongation as well as improved surface hardness. As a result, when the laminate is subjected to secondary molding into the shape of a resin molded product, breakage or significant whitening does not occur due to stretching, bending, or the like. However, in general, in a hard coat layer, a cured product of a curable resin composition containing a curable resin is highly crosslinked and / or contains a filler with high hardness, thereby suppressing deformation of the cured product surface due to external stress, thereby exhibiting surface hardness and scratch resistance. Surface hardness and scratch resistance are contradictory properties to deformability and extensibility, and it has not been easy to achieve both of these properties in a hard coat layer.
[0089] In order to impart high extensibility during secondary molding while maintaining the surface hardness of the hard coat layer, the curable resin used in the hard coat layer can be improved, for example, by the following methods (1) to (3). For the hard coat layer, any of the methods (1) to (3), for example, may be used alone or in appropriate combination. For the hard coat layer, a commercially available curable resin composition containing a urethane acrylate resin that can impart high extensibility during secondary molding while maintaining the surface hardness of the hard coat layer may be used as appropriate. (1) The glass transition temperature of the curable resin (specifically, the urethane acrylate resin) is designed to be between room temperature (20±5°C) and the secondary molding temperature (e.g., approximately 110 to 140°C), so that the resin is hard at room temperature but softens and becomes deformable at the secondary molding temperature. As a result, the cured product of the curable resin (hard coat layer) exhibits high surface hardness at room temperature while exhibiting high extensibility during secondary molding. (2) By using a combination of multiple curable resins with different structures, the crosslinked structure of the cured curable resin is designed to be not uniform but to have areas with high crosslink density and areas with low crosslink density and large plastic deformation, resulting in a heterogeneous microstructure. As a result, the high crosslink density areas in the cured product of the curable resin (hard coat layer) exhibit high surface hardness, and during secondary molding, the low crosslink density areas deform, resulting in high extensibility. (3) A low-crosslinking or non-crosslinked resin component and / or a low elastic modulus resin component is blended into the curable resin. As a result, after curing of the curable resin, a structure is formed in which low-crosslinking or non-crosslinked and / or low elastic modulus fine regions (domains) are dispersed in the high crosslink density curable resin phase, thereby imparting deformability and extensibility to the cured product of the curable resin (hard coat layer) while maintaining a certain degree of surface hardness.Examples of such low-crosslinking, non-crosslinking, or low-elastic modulus resin components include: (a) thermoplastic resins such as thermoplastic methacrylic resins, styrene-acrylonitrile resins, aliphatic polycarbonate resins, aromatic polycarbonate resins, polyester resins, phenoxy resins, cellulose acylate resins, fluororesins, and polyurethane resins; (b) crosslinked or non-crosslinked soft resins such as acrylic rubber, silicone rubber, hydrogenated styrene butadiene rubber, acrylonitrile butadiene rubber, olefin rubber, and urethane rubber, which may have a reactive functional group as needed; thermoplastic elastomer materials such as polyester, polyurethane, acrylic, olefin, styrene, silicone, and fluororesin; and (c) core-shell rubber particles in which a thermoplastic resin is graft-polymerized onto the surface of crosslinked rubber particles.
[0090] <Urethane acrylate resin> The urethane acrylate resin can be obtained, for example, by mixing a polyhydric alcohol, a polyisocyanate, and a hydroxyl group-containing (meth)acrylate and allowing the isocyanate group and the hydroxyl group to react to form a urethane bond. In this specification, (meth)acrylate is a general term for acrylate and methacrylate.
[0091] Alternatively, a urethane acrylate resin can be obtained by reacting a polyhydric alcohol with a polyisocyanate to form a (meth)acryloyl group at the end or in the side chain of a polyurethane compound, which is obtained by reacting the isocyanate group at the end or in the side chain, with a hydroxyl group-containing (meth)acrylate. In this specification, the term "(meth)acryloyl group" encompasses both methacryloyl and acryloyl groups.
[0092] The various properties of the urethane acrylate resin are not particularly limited, and can be adjusted appropriately by adjusting the structure of the polyhydric alcohol, the type of polyisocyanate, and the number of acryloyl groups or methacryloyl groups (CH═CH—CO— or CH═C(CH)—CO—) derived from the hydroxyl group-containing (meth)acrylate, such as the molecular weight, composition, main chain structure (e.g., linear or branched), and number of functional groups. Further examples of the urethane acrylate resin include urethane acrylate resins commercially available as ultraviolet-curable hard coating agents.
[0093] The polyvalent isocyanate is not particularly limited as long as it is a compound containing two or more isocyanate groups. Examples of polyisocyanate compounds include 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, 1,5-naphthalene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 3,3'-dimethyl-4,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane triisocyanate, 3,3'-dimethylphenylene diisocyanate, 4,4'-biphenylene diisocyanate, 1,6-hexane diisocyanate, isophorone diisocyanate, methylenebis(4-cyclohexyl isocyanate), 2,2,4-trimethylhexamethylene diisocyanate, bis(2-isocyanatoethyl) fumarate, 6-isopropyl methyl ... Propyl-1,3-phenyl diisocyanate, 4-diphenylpropane diisocyanate, tolidine diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, tetramethylxylylene diisocyanate, 2,5-bis(isocyanatemethyl)-bicyclo[2.2.1]heptane, 2,6-bis(isocyanatemethyl)-bicyclo[2.2.1]heptane, trimethylolpropane adduct of triethylene diisocyanate, isocyanurate of triethylene diisocyanate, oligomer of diphenylmethane-4,4'-diisocyanate, biuret of hexamethylene diisocyanate, isocyanurate of hexamethylene diisocyanate, uretdione of hexamethylene diisocyanate, isocyanurate of isophorone diisocyanate, and the like. Among these, polyvalent isocyanate compounds that do not contain an aromatic skeleton but have a saturated aliphatic skeleton or an alicyclic skeleton are preferred because they provide a structure that is more excellent in weather resistance.Examples of such polyisocyanate compounds include 1,6-hexane diisocyanate, isophorone diisocyanate, methylenebis(4-cyclohexylisocyanate), 2,2,4-trimethylhexamethylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, 2,5-bis(isocyanatemethyl)-bicyclo[2.2.1]heptane, 2,6-bis(isocyanatemethyl)-bicyclo[2.2.1]heptane, etc. These polyisocyanates can be used alone or in combination of two or more.
[0094] Specific examples of polyhydric alcohols include ethylene glycol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, 2-methyl-1,8-octanediol, cyclohexanediol, 1,4-cyclohexanedimethanol, glycerol, pentaerythritol, dipentaerythritol, polycaprolactone diol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, polyester diol, polycarbonate diol, polyurethane diol, bisphenol compounds, biphenol compounds, norbornadiol, dicyclopentanediol, and adamantanediol. Among these, polyhydric alcohols that do not contain an aromatic skeleton and have a saturated aliphatic skeleton or an alicyclic skeleton are preferred because they provide a structure that is more excellent in weather resistance. These polyhydric alcohols may be used alone or in combination of two or more.
[0095] The hydroxyl group-containing (meth)acrylate is not particularly limited, and examples thereof include 2-hydroxyethyl acrylate and 2-hydroxyethyl methacrylate. If necessary, (a) a compound having an ethylenically unsaturated bond and at least one hydroxyl group, such as 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl acrylate, polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, trimethylpropane mono(meth)acrylate, trimethylolpropane di(meth)acrylate, allyl alcohol, ethylene glycol allyl ether, glycerin (mono- or di-)allyl ether, N-methylol(meth)acrylamide, and the like, (b) or a mixture thereof may be added.
[0096] An organotin urethanization catalyst is used to promote the reaction between the isocyanate group and the hydroxyl group of the isocyanate component. The organotin urethanization catalyst may be any catalyst commonly used in urethanization reactions, such as dibutyltin dilaurate, dibutyltin diacetate, dibutyltin dialkyl maleate, tin stearate, and tin octoate.
[0097] In one or more embodiments of the present invention, at least a portion of the curable resin composition for the hard coat layer may be a curable resin composition containing a commercially available urethane acrylate resin. Examples of such commercially available products include "Z-607-27L" manufactured by Aica Kogyo Co., Ltd., "Beamset 1200W" manufactured by Arakawa Chemical Industries, Ltd., "Acrit 8UX-116A" manufactured by Taisei Fine Chemical Co., Ltd., "NXD-004AP" manufactured by Nippon Kako Toryo Co., Ltd., "P-5820TAH-1" and "P-5820TA-20J" manufactured by Daido Chemical Industry Co., Ltd., and "Lioduras MOL7200" manufactured by Toyochem Co., Ltd. These commercially available curable resin compositions containing urethane acrylate resins have high elongation even after curing, and their use can further increase the crack elongation of the laminate at 120°C.
[0098] <Light Stabilizer> The curable resin composition for a hard coat layer contains a light stabilizer. The inclusion of a light stabilizer improves the stability of the hard coat layer against ultraviolet degradation and light degradation, and suppresses weathering deterioration such as surface cracking and peeling in a portion or application exposed to sunlight outdoors or indoors of a resin molded article coated with a laminate including the hard coat layer.
[0099] The curable resin composition for the hard coat layer contains a hindered amine light stabilizer (hereinafter also referred to as "reactive HALS") having at least a reactive functional group as a light stabilizer. In the reactive HALS, the reactive functional group may be any group reactive with the urethane acrylate resin, such as a functional group having an ethylenic double bond. More specifically, it preferably contains one or more groups selected from the group consisting of methacryloyl groups, acryloyl groups, vinyl groups, and allyl groups, and more preferably contains one or more groups selected from the group consisting of methacryloyl groups and acryloyl groups. Furthermore, the substituent on the nitrogen atom of the amine functional group may be hydrogen, or may be a substituent such as an alkyl group (e.g., methyl, ethyl, or propyl), a phenyl group, a benzyl group, an alkyloxy group, an acyl group, or an acyloxy group. Since the hindered amine light stabilizer has a reactive functional group, when the urethane acrylate resin is cured, the hindered amine light stabilizer molecule reacts with the urethane acrylate resin and is introduced in a chemically bonded state into the cured product that forms the hard coat layer. This prevents the hindered amine light stabilizer from migrating or flowing out from the surface of the hard coat layer even under outdoor exposure and other environments, thereby preventing deterioration in the weather resistance of the hard coat layer for a longer period of time.
[0100] Examples of reactive HALS include 4-(meth)acryloyloxy-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-(meth)acryloyloxy-1,2,2,6,6-pentamethylpiperidine, 4-(meth)acryloylamino-1,2,2,6,6-pentamethylpiperidine, 4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 4-crotonoyloxy- Examples of reactive HALS include, but are not limited to, 2,2,6,6-tetramethylpiperidine, 4-crotonoylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, 1-(meth)acryloyl-4-cyano-4-(meth)acryloylamino-2,2,6,6-tetramethylpiperidine, and 1-crotonoyl-4-crotoyloxy-2,2,6,6-tetramethylpiperidine. These reactive HALS may be used alone or in combination of two or more.
[0101] As the reactive HALS, for example, commercially available products such as 1,2,2,6,6-pentamethyl-4-piperidinyl methacrylate (manufactured by ADEKA Corporation under the trade name "ADK STAB LA-82", or manufactured by Hitachi Chemical Co., Ltd. under the trade name "FA-711MM"), 2,2,6,6-tetramethyl-piperidinyl methacrylate (also known as 4-methacryloyloxy-2,2,6,6-tetramethylpiperidine, manufactured by ADEKA Corporation under the trade name "ADK STAB LA-87", or manufactured by Hitachi Chemical Co., Ltd. under the trade name "FA-712HM") may be used.
[0102] The curable resin composition for the hard coat layer preferably contains 1 to 10 parts by mass, more preferably 1.5 to 6 parts by mass, and even more preferably 2 to 4 parts by mass of a reactive HALS per 100 parts by mass of the urethane acrylate resin. By containing 1 part by mass or more of the reactive HALS, long-term weather resistance is improved. Furthermore, when the reactive HALS is 10 parts by mass or less, weather resistance can be improved without impairing the quality of the hard coat layer.
[0103] In addition to the reactive HALS, the curable resin composition for the hard coat layer may contain, if necessary, other light stabilizers such as hindered amine light stabilizers (hereinafter also referred to as HALS) that do not have a reactive functional group. Examples of HALS include bis(1,2,2,6,6-pentamethyl-4-piperidyl)sebacate, bis(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, methyl(1,2,2,6,6-pentamethyl-4-piperidinyl)sebacate, and 2,4-bis[N-butyl-N-(1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine. In this case, from the viewpoint of further improving weather resistance without causing bleed-out or curing inhibition during curing of the hard coat layer, the curable resin composition for the hard coat layer may contain a total of 1 to 10 parts by mass, 1.5 to 6 parts by mass, or 2 to 4 parts by mass of the light stabilizer relative to 100 parts by mass of the urethane acrylate resin.
[0104] <Other Components> The curable resin composition for the hard coat layer may contain other components in addition to the urethane acrylate resin and light stabilizer. Examples of other components that can be used in combination include (meth)acrylate compounds, epoxy acrylate monomers, polyester acrylates, polyacrylic acrylates, and other monomers, oligomers, resins, or mixtures thereof having radical-reactive functional groups. Furthermore, the urethane acrylate resin may be used in combination with a composition containing, for example, (a) a hydrolysis condensate of a di- to tetrafunctional silane compound, and / or (b) a monomer, oligomer, resin, or mixtures thereof having cationically curable and / or anionically curable functional groups such as epoxy groups and oxetane groups. These other components may be used alone or in combination.
[0105] The (meth)acrylate compound is not particularly limited as long as it has at least one (meth)acryloyl group.Specific examples thereof include alicyclic (meth)acrylates such as alkyl (meth)acrylate, aryl (meth)acrylate, phenoxyethyl (meth)acrylate, isobornyl (meth)acrylate, etc.; polyfunctional (meth)acrylates such as polyalkylene glycol di(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, hexanediol di(meth)acrylate, and diethylene glycol di(meth)acrylate. These may be used alone or in combination of two or more. Further examples of the (meth)acrylate compound include those commercially available as ultraviolet-curable hard coating agents.
[0106] The epoxy acrylate monomer is not particularly limited, and specific examples include glycidyl (meth)acrylate, β-methylglycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and vinylcyclohexene monoxide (i.e., 1,2-epoxy-4-vinylcyclohexane).
[0107] When forming a hard coat layer, a known method can be applied to harden the resin layer (curable resin composition). As a hard coat layer forming method, a method of irradiating with active energy rays, such as ultraviolet rays or electron beam rays, is preferred. When hardening is performed by irradiating with ultraviolet rays, a photopolymerization initiator is used.
[0108] Specific examples of the photopolymerization initiator include acetophenone, benzophenone, benzoyl methyl ether, benzoyl ethyl ether, benzoin isopropyl ether, benzoin isobutyl ether, dibenzyl, 1-hydroxycyclohexylphenyl ketone, 2,2-dimethoxy-2-phenylacetophenone, tetramethylthiuram monosulfide, tetramethylthiuram disulfide, thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, and 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one compounds, etc. Among these, 1-hydroxycyclohexylphenyl ketone is preferred from the viewpoint of excellent compatibility with urethane acrylate resins.
[0109] A hard coat layer can be formed by applying a curable composition to one or both sides of an acrylic resin film and curing the resin layer (coating film) composed of the curable composition. In this case, various known leveling agents and antifouling agents may be blended into the curable composition for purposes such as improving coatability, scratch resistance after curing, antifouling properties, and smoothness. Examples of leveling agents and antifouling agents that can be used include fluorine-based, acrylic-based, and silicone-based compounds, as well as adducts or mixtures thereof. These leveling agents and antifouling agents may contain a functional group reactive with the urethane acrylate resin. The amount of the leveling agent or antifouling agent blended is not particularly limited, but may be, for example, 0.03 to 3.0 parts by mass per 100 parts by mass of the curable composition.
[0110] When a hard coat layer is formed by applying a curable composition to one or both surfaces of an acrylic resin film and curing the coating, various additives such as an ultraviolet absorber, an antifoaming agent, an antioxidant, a light diffusing agent, a matting agent, an antifouling agent, a lubricant, a coloring agent such as a pigment or a dye, organic particles, inorganic particles, and an antistatic agent may be added to the curable composition as needed. The additives are not limited to these.
[0111] Furthermore, the curable resin composition for the hard coat layer may contain inorganic particles, provided that the object of the present invention is not impaired. Examples of inorganic particles include, but are not limited to, silica, alumina, titanium oxide, zinc oxide, zirconia, graphene, nanocarbon, carbon black, nanodiamond, mica, barium titanate, boron nitride, metallic silver, and metallic copper. These particles may be used without surface treatment, or may be surface-treated in advance by a known method to control the dispersion state and maintain good stretchability, thereby appropriately controlling the affinity with the hard coat layer.
[0112] Furthermore, within a range that does not impair the object of the present invention, the curable resin composition for the hard coat layer may contain particles from the viewpoint of enhancing the antiglare property of the laminate. With regard to the particles blended into the hard coat layer for the purpose of imparting antiglare property, etc., in order to obtain a balance of various properties such as the desired antiglare property, clarity of a transmitted image, glare, jet-black surface, surface hardness, slip property, and antistatic property, the material of the particles, the blending number, the type of particle dispersion solvent, particle diameter, dispersed particle diameter, thickness of the hard coat layer, the relative refractive index difference with the hard coat substrate, the affinity and reactivity of the particle surface with the hard coat substrate or solvent, etc. can be appropriately adjusted within known technical ranges that do not impair the effect of the present invention.
[0113] The material of the particles incorporated into the hard coat layer is not particularly limited as long as it enhances the antiglare properties of the laminate within a range that does not impair the objectives of the present invention, and for example, inorganic particles and / or organic particles can be used. Examples of inorganic particles include silica, alumina, glass beads, glass flakes, mica, clay, titanium oxide, zinc oxide, zirconia, and metal particles. Examples of organic particles include crosslinked organic resin particles containing one or more main components selected from the group consisting of alkyl (meth)acrylate units, aromatic vinyl units, and organic functional group-substituted siloxane units, as well as core-shell multilayer structure resin particles. In terms of ease of availability and ease of designing antiglare properties according to the application, the particles are preferably one or more selected from the group consisting of inorganic oxide particles (e.g., silica, alumina, titanium oxide, zinc oxide, zirconia, etc.) and crosslinked organic resin particles (e.g., crosslinked silicone resin, crosslinked acrylic resin, crosslinked aromatic vinyl resin, etc.), and more preferably one or more selected from the group consisting of silica, alumina, zirconia, and crosslinked organic resin particles. In addition, from the viewpoint of the balance of physical properties such as antiglare property, dispersibility, and surface hardness, it is particularly preferable that the particles are one or more selected from the group consisting of silica, alumina, and crosslinked organic resin particles. In addition, from the viewpoint of controlling dispersibility, these particles may be subjected to surface treatment and / or graft polymerization treatment using a known method such as a silane coupling agent or reactive monomer which may have a reactive substituent, plasma treatment, or corona treatment. Since there is a possibility that the interfacial adhesion between the particles and the hard coat layer is improved, and the dispersibility of the particles and cracking and / or whitening during stretching can be improved, it is preferable that at least some of the particles contain a reactive functional group reactive with a urethane acrylate resin on the surface of the particles. Examples of reactive functional groups reactive with urethane acrylate resins include (a) radically reactive functional groups such as vinyl groups and (meth)acryloyl groups, (b) ionic functional groups such as epoxy groups, oxetane groups, hydroxyl groups, carboxyl groups, mercapto groups, isocyanyl groups, hydroxyl groups, and amino groups, and (c) moisture-curable functional groups such as silyl groups and alkoxysilyl groups.
[0114] In the hard coat layer, the "particles" may be dispersed in the state of primary particles as they are, or in the state of agglomerates of multiple particles, depending on the size of the primary particles. The size of the region (dispersion domain) where these particles or their agglomerates are distributed is defined as the "average dispersed particle size." When the primary particles are large, the average dispersed particle size may be the same as the primary (basic) particle size.
[0115] The average dispersed particle diameter of the particles (e.g., silica particles) is not particularly limited as long as the effects of the present invention are achieved, but may be, for example, 0.1 to 50.0 μm, 0.2 to 25.0 μm, or 0.5 to 10 μm, etc. In this specification, a cross-sectional photograph of the laminate, 1200 nm × 800 nm, measured at a magnification of 200,000 times using an electron microscope (Hitachi High-Technologies Corporation, H7650) is observed, and the arithmetic mean value of particle diameters of 10 dispersed domains of particles in the hard coat layer is calculated, and the obtained value is defined as the average dispersed particle diameter of the particles in the hard coat layer.
[0116] The content of the particles in the hard coat layer is not particularly limited as long as it can enhance the antiglare property of the laminate within a range that does not impair the object of the present invention, and may be, for example, 0.1 to 30.0 mass %, 0.5 to 20.0 mass %, or 1.0 to 15.0 mass %, etc.
[0117] In order to impart appropriate coatability to the curable composition, an organic solvent is usually blended. The organic solvent is not particularly limited as long as it can impart the desired coatability to the curable composition and form a hard coat layer with the desired thickness and performance. The boiling point of the organic solvent is preferably 50 to 150°C from the viewpoints of coatability and drying properties of the formed resin layer (coating film).
[0118] Specific examples of organic solvents include saturated hydrocarbons such as hexane, aromatic hydrocarbons such as toluene and xylene, halogenated hydrocarbons such as chloroform and methylene chloride, alcohols such as methanol, ethanol, isopropyl alcohol and butanol, esters such as methyl acetate, ethyl acetate and butyl acetate, ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone and cyclohexanone, ethers such as tetrahydrofuran, dioxane, propylene glycol monoethyl ether, methyl cellosolve and ethyl cellosolve, and amides such as N-methylpyrrolidone and dimethylformamide. The organic solvents can be used alone or in combination of two or more.
[0119] When the curable composition is applied to one or both sides of the acrylic resin film, any method can be used as the application method without any particular limitation. Examples of the application method include reverse coating, gravure coating, bar coating, die coating, spray coating, kiss coating, wire bar coating, and curtain coating. These application methods may be used alone or in combination.
[0120] The above-described curable composition for a hard coat layer is applied to one or both surfaces of an acrylic resin film to form a resin layer (coating film), and then the organic solvent is removed from the coating film by drying, and the resin layer is cured by irradiation with active energy rays such as ultraviolet light, thereby forming a hard coat layer.
[0121] The drying temperature for removing the organic solvent from the resin layer after coating is preferably 60 to 120°C, more preferably 70 to 100°C. If the drying temperature is too low, the organic solvent may remain in the resin layer (coating film). If the drying temperature is too high, the acrylic resin film may be thermally deformed, which may impair the flatness of the laminate (hard coat layer).
[0122] The wavelength of the ultraviolet light irradiated when curing the resin layer (coating film) is preferably in the range of 200 to 400 nm. The integrated amount of ultraviolet (UV) light is, for example, 150 to 700 mJ / cm.2 is preferably 180 to 500 mJ / cm 2 More preferably, it is 200 to 400 mJ / cm 2 It is more preferable that the integrated light amount of the UV irradiation is within the above-mentioned range, and the hard coat layer can have an appropriate hardness while ensuring moldability. As the irradiation device for the ultraviolet exposure light, for example, an irradiation device equipped with either (a) a lamp light source such as a high-pressure mercury lamp, a low-pressure mercury lamp, a metal halide lamp, an electrodeless lamp, or an excimer lamp, and / or (b) a pulsed or continuous laser light source such as an argon ion laser or a helium-neon laser can be used.
[0123] Furthermore, for the purpose of further improving the surface hardness, chemical resistance, weather resistance, etc. of a resin molded article having the laminate of the present invention disposed on its surface, an operation of irradiating active energy rays such as ultraviolet rays may be further carried out after secondary molding by vacuum and / or pressure molding of the laminate, or on at least a part of the resin molded article having the laminate disposed on its surface.
[0124] (Laminate) In one or more embodiments of the present invention, as shown in FIG. 1 , a laminate 1 includes an acrylic resin film 2 and a hard coat layer 3 laminated on one side of the acrylic resin film 2. Although not shown, hard coat layers may be laminated on both sides of the acrylic resin film. Furthermore, the laminate may include another functional layer laminated between the acrylic resin film and the hard coat layer and / or on the hard coat layer, as necessary, within a range that does not impair the effects of the present invention. Furthermore, the laminate may have another functional layer laminated on the side opposite to the hard coat layer.
[0125] The other functional layers are not particularly limited, and a wide range of conventionally known layers can be used. Examples include a low refractive index layer, a primer layer, a high refractive index layer, an adhesive layer, an anti-glare layer, an anti-fouling layer, a fingerprint-resistant layer, a scratch-resistant layer, an antistatic layer, an ultraviolet shielding layer, an infrared shielding layer, a surface irregularity layer, a light diffusion layer, a matte layer, a polarizing layer, a colored layer, a design layer, a printed layer, an embossed layer, a conductive layer, a gas barrier layer, and a gas absorbing layer. The laminate may include two or more types of other functional layers in combination. Furthermore, one functional layer may have two or more functions.
[0126] The laminate has a crack elongation of 100% or more at 120 ° C. As a result, when the laminate is laminated on a thermoplastic resin substrate and the thermoplastic resin substrate is covered with the laminate, particularly when the laminate is vacuum molded under heating, shaped by pressure molding, laminated onto a substrate, or if necessary, when the shaped laminate is placed on a mold surface and then molded by insert injection molding, defects such as cracks and whitening can be suppressed from occurring in the laminate, resulting in good secondary moldability. The crack elongation of the laminate at 120 ° C. is preferably 110% or more, more preferably 120% or more, even more preferably 130% or more, and particularly preferably 140% or more. In this specification, the crack elongation of the laminate at 120 ° C. can be measured by the method described in the examples.
[0127] From the viewpoint of excellent long-term weather resistance, the laminate was placed so that the hard coat layer side faced the light source, and a xenon lamp was used as the light source, with an irradiance of 180 W / m 2It is preferable that no cracks occur on the surface of the hard coat layer of the laminate even after undergoing an accelerated weathering test in which 1000 cycles of a total of 120 minutes each consisting of Step 1, an exposure time of 102 minutes, a black panel temperature of 60±3°C, a relative humidity of 65±5%, and no rainfall, and Step 2, an exposure time of 18 minutes, an internal temperature of 38±3°C, a humidity of 95±5%, and rainfall, are performed for a total of 2000 hours under conditions of (300 to 400 nm). Furthermore, the color difference ΔE of the laminate after the accelerated weathering test relative to the laminate before the accelerated weathering test is preferably 0.5 or less, and more preferably 0.3 or less. In particular, even when direct sunlight is simulated, specifically when a filter configuration is used in which quartz glass is used on the inside and polysilicate #275 is used on the outside, and the accelerated weather resistance test described above is conducted for 2000 hours, it is preferable that no cracks occur on the surface of the hard coat layer of the laminate, and the color difference ΔE of the laminate after the accelerated weather resistance test compared to the laminate before the accelerated weather resistance test is 0.5 or less, more preferably 0.3 or less.
[0128] From the viewpoint of transparency, the laminate preferably has a haze (Hz) of 2.0% or less, more preferably 1.5% or less, even more preferably 1.0% or less, even more preferably 0.8% or less, and particularly preferably 0.4% or less. However, this does not necessarily apply when components such as a matting agent or an antiglare agent are introduced into the acrylic resin film substrate and / or hard coat layer based on requirements for quality such as appearance. In this specification, the haze can be measured by the method described in the examples.
[0129] From the viewpoint of excellent surface hardness and enhancing the scratch resistance of a resin molded article using the laminate, the pencil hardness of the hard coat layer side is preferably B or higher under a 500 g load, more preferably HB or higher, even more preferably F or higher, and particularly preferably H or higher.
[0130] From the viewpoint of excellent chemical resistance, the laminate preferably shows no visual change in appearance when about 0.02 mL of isopropyl alcohol is dropped onto the surface of the hard coat layer and left to stand at 23° C. for 6 hours. Also, from the viewpoint of excellent chemical resistance, the laminate preferably shows no visual change in appearance when about 0.02 mL of acetone is dropped onto the surface of the hard coat layer and left to stand at 23° C. for 6 hours.
[0131] From the viewpoint of suppressing whitening of the edges when trimmed after molding, the Δhaze (ΔHz) of the laminate when stretched 20% at room temperature is preferably 3% or less, more preferably 2% or less, and even more preferably 1.5% or less. In this specification, the ΔHz of the laminate when stretched 20% at room temperature can be measured by the method described in the Examples.
[0132] From the viewpoint of suppressing whitening during molding, the ΔHz of the laminate when stretched 80% at 120° C. is preferably 3% or less, more preferably 2% or less, even more preferably 1% or less, even more preferably 0.8% or less, and particularly preferably 0.4% or less. In this specification, the ΔHz of the laminate when stretched 80% at 120° C. can be measured by the method described in the examples.
[0133] (Resin Molded Article) The resin molded article includes a thermoplastic resin substrate and a laminate, and at least a portion of the thermoplastic resin substrate is covered with a laminate arranged so that the acrylic resin film faces the thermoplastic resin substrate. The laminate has a high crack elongation at 120°C, so that a thermoplastic resin substrate having at least a portion of a non-planar curved shape and / or a three-dimensional shape can be coated with the laminate, thereby suitably obtaining a resin molded article having a three-dimensional shape. By coating the thermoplastic resin substrate in resin molded articles having various shapes, the laminate can impart various functionalities such as long-term weather resistance, scratch resistance, and chemical resistance to the resin molded article.
[0134] The thermoplastic resin substrate may be composed of, for example, a polycarbonate resin having a bisphenol skeleton, a fluorene skeleton, or an isosorbide skeleton, an acrylic resin, a styrene resin (such as AS resin, ABS resin, MAS resin, styrene maleimide resin, and styrene maleic anhydride resin), a saturated polyester resin, a polyvinyl chloride resin, a polyarylate resin, a PPS resin, a POM resin, a polyamide resin, a polylactic acid resin, a cellulose acylate resin, and a polyolefin resin. Among these, one or more selected from the group consisting of polycarbonate resin, acrylic resin, styrene resin, and amorphous polyolefin resin are preferred because of their excellent transparency, and polycarbonate resin and / or acrylic resin are more preferred because of their good adhesion to the laminate, and polycarbonate resin is even more preferred from the viewpoints of high rigidity, high heat resistance, and high impact resistance.
[0135] The resin molded article can be used, for example, as an automobile interior material, an automobile exterior material, an optical component, a home appliance component, and an architectural exterior material. Since the laminate has excellent long-term weather resistance, a resin molded article using the laminate can be suitably used as an automobile exterior material, an architectural exterior material, and the like. Examples of automobile exterior materials include, but are not limited to, door mirrors, windows, headlamp covers, taillamp covers, windshield parts, weatherstrips, bumpers, bumper guards, side mudguards, body panels, spoilers, flon ruffles, strut mounts, wheel caps, center pillars, center ornaments, side moldings, door moldings, and window moldings. Examples of architectural exterior materials include exterior wall materials such as siding, fences, roofs, gates, and gable boards.
[0136] The method for producing a resin molded article is not particularly limited, as long as it is a molding method that can cover at least a portion of a thermoplastic resin substrate with a laminate arranged so that the acrylic resin film side faces the thermoplastic resin substrate side. Furthermore, the laminate may have the other functional layers described above formed thereon as appropriate prior to lamination to the substrate. Using such a laminate, for example, a resin molded article having a laminate arranged on its surface can be produced by insert injection molding. Furthermore, prior to insert injection molding, the laminate may be preformed, as necessary, by methods such as vacuum forming, pressure forming, and compression molding. Alternatively, the laminate may be heated and / or pressurized under reduced pressure and / or pressure conditions, and the laminate may be placed on the surface of a thermoplastic resin substrate having at least a non-planar three-dimensional shape (curved shape) to produce a resin molded article, known as three-dimensional laminate molding. Furthermore, the laminate may be heated, stretched appropriately, and manually laminated onto the surface of a thermoplastic resin substrate to produce a resin molded article.
[0137] The present invention will be described in more detail below based on examples. The present invention is not limited to these examples. In the following, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0138] The measurement and evaluation methods used in the examples and comparative examples will be explained below.
[0139] (Glass Transition Temperature) A differential scanning calorimeter (DSC, manufactured by Seiko Instruments, model number "SSC-5200") was used. The sample was initially heated to 200°C at a rate of 25°C / min, held at that temperature for 10 minutes, and then pre-conditioned by lowering the temperature to 50°C at a rate of 25°C / min. DSC measurement was then performed while the sample was heated to 200°C at a rate of 10°C / min. The differential value (SSDC) was determined from the resulting DSC curve, and the glass transition temperature was determined from the maximum point.
[0140] (Tensile elongation at break at 120°C) The acrylic resin film was cut into a size of 10 mm (width) x 100 mm (length) in the machine direction (MD) during extrusion molding to prepare a sample. A tensile test was performed using a Tensilon tensile tester (manufactured by Shimadzu Corporation, model number "AG-2000D") equipped with a high-temperature bath set to 120°C, under the conditions of a preheating time of 2 minutes, a chuck distance of 40 mm, and a tensile speed of 200 mm / min. The elongation at break of the test piece was measured, and the average value of the test results obtained by measuring three samples was taken as the elongation at break at 120°C.
[0141] (Crack elongation at 120°C) The laminate was cut into a 10 mm (width) x 100 mm (length) sample and subjected to a tensile test using a Tensilon tensile tester (manufactured by Shimadzu Corporation, model number "AG-2000D") equipped with a high-temperature bath set to 120°C under the conditions of a preheating time of 2 minutes, a chuck distance of 40 mm, and a tensile speed of 200 mm / min. The elongation was measured when cracks occurred in the hard coat layer, and the average value of the test results obtained by measuring three samples was taken as the crack elongation at 120°C.
[0142] (Thickness) The thickness of the acrylic resin film was measured using a PEACOCK Dial Gauge No. 25 (manufactured by Ozaki Manufacturing Co., Ltd.). The thickness of the hard coat layer was measured using an F20 Film Thickness Measurement System (manufactured by Filmetrics Inc.). The surface opposite the hard coat layer was painted black with a felt-tip pen, and the refractive index of the acrylic resin film was set to 1.49, and the refractive index of the hard coat layer was set to 1.50.
[0143] (Haze) Haze was measured in accordance with ISO 14782 using a haze meter NDH4000 (manufactured by Nippon Denshoku Industries Co., Ltd.).
[0144] (ΔHz after 80% stretching at 120°C) The laminate was cut into a 10 mm (width) x 100 mm (length) sample, and a tensile test was performed using a Tensilon tensile tester (Shimadzu Corporation, AG-2000D) equipped with a high-temperature bath set at 120°C under the conditions of a preheating time of 2 minutes, a chuck distance of 40 mm, and a tensile speed of 200 mm / min. The haze of the sample before the tensile test was measured to determine the haze of the laminate before stretching, and the haze of the sample after 80% stretching at 120°C was measured to determine the haze of the laminate after 80% stretching at 120°C. The difference in haze of the laminate after 80% stretching at 120°C relative to the haze of the laminate before stretching was determined as ΔHz after 80% stretching at 120°C. ΔHz after 80% stretching of the laminate at 120°C = haze of the laminate after 80% stretching at 120°C - haze of the laminate before stretching
[0145] (ΔHz after 20% stretching at room temperature) The laminate was cut into a size of 10 mm (width) x 100 mm (length) to prepare a sample, and a tensile test was performed using a Tensilon tensile tester (manufactured by Shimadzu Corporation, model number "AG-2000D") at 23°C, with a chuck distance of 40 mm and a tensile speed of 200 mm / min, resulting in 20% stretching. The sample after 20% stretching was allowed to stand at 23°C for 12 hours, and then its haze was measured, which was taken as the haze of the laminate after 20% stretching at room temperature. The haze of the sample measured before the tensile test was taken as the haze of the laminate before stretching. The difference in haze of the laminate after 20% stretching at room temperature relative to the haze of the laminate before stretching was taken as ΔHz after 20% stretching at room temperature. ΔHz after 20% stretching at room temperature of laminate = haze of laminate after 20% stretching at room temperature - haze of laminate before stretching
[0146] (Pencil Hardness) Pencil hardness was measured under a load of 500 g in accordance with JIS K 5600-5-4:1999.
[0147] (Accelerated Weathering Test) A super xenon weather meter (SX2D-75, manufactured by Suga Test Instruments Co., Ltd.) was used. The filter configuration used quartz glass on the inside and polysilicate #275 on the outside to simulate direct sunlight. A laminate sample (40 mm x 50 mm) was placed with the hard coat layer side facing the light source, and an accelerated weathering test was carried out by carrying out 1000 cycles (2000 hours) of a cycle consisting of the following Step 1 and Step 2 (total of 120 minutes). Step 1: Exposure time 102 minutes, irradiance 180 W / m 2 (300-400 nm), black panel temperature 60±3°C, relative humidity 65±5%, no rain Step 2: exposure time 18 minutes, irradiance 180 W / m 2 (300-400 nm), temperature inside the chamber 38±3°C, relative humidity 95±5%, with rainfall. After the accelerated weathering test, the surface of the hard coat layer of the sample was visually observed to check for cracks. If no cracks were found, it was determined that the long-term weathering resistance was good. The color difference of the laminate after the weathering test compared to the laminate before the weathering test was determined. The color difference (ΔE) was measured using a spectrocolorimeter SE7700 (manufactured by Nippon Denshoku Kogyo Co., Ltd.) under the following conditions: Mode: Transmission, Light source: D65, Field of view: 2°, Measurement diameter: 28 mm
[0148] (Chemical resistance test) A laminate sample cut into a 5 cm x 5 cm square was placed on a horizontal surface with the hard coat layer side facing up, and one drop (approximately 0.02 mL) of isopropyl alcohol (hereinafter also referred to as IPA) taken with a dropper was dropped onto it, and after leaving it as it is at room temperature (23°C) for 6 hours, the surface was observed and the chemical resistance was evaluated according to the following criteria. Good: No change in appearance Slightly poor: Outline remains Poor: Appearance as if dissolved
[0149] (Paint 1) A highly extensible curable resin composition (containing a urethane acrylate resin, manufactured by Daido Chemical Industry Co., Ltd., product name "P5820TA-20J", solid content 25%) was blended with methyl ethyl ketone (MEK) to make the solid content 23%.
[0150] (Paint 2) Methyl ethyl ketone (MEK) was blended into a low-stretch curable resin composition (containing a urethane acrylate resin, manufactured by DIC Corporation, product name "ENS-102", solid content 99%) so that the solid content became 23%.
[0151] (Example 1) <Preparation of acrylic resin film> Multilayer structure particles (C4) having an average particle size of 85 nm prepared by the same method as in Production Example 4 of JP 2020-147653 A were used as the graft copolymer particles (A-1), and poly(methyl methacrylate) (manufactured by Sumitomo Chemical, product name "Sumipex (registered trademark) MG") was used as the acrylic resin (D-1). 100 parts of a resin mixture 1 consisting of 38% graft copolymer particles (A-1) and 62% acrylic resin (D-1), 0.3 parts of a hindered phenol-based antioxidant (manufactured by BASF, product name "Irganox 1010"), and 1.5 parts of an ultraviolet absorber (benzotriazole-based ultraviolet absorber, manufactured by ADEKA, product name "ADK STAB LA-31") were mixed using a Henschel mixer. Next, using a vented co-rotating twin-screw extruder (manufactured by Toshiba Machine Co., Ltd., model number "TEM58", L / D = 41.7) with a cylinder temperature adjusted to 190 to 250 ° C., the extrusion diameter was 58 mm, and the extrusion was melt-kneaded at a screw rotation speed of 150 rpm and a discharge rate of 180 kg / h. The extrusion was taken up in a strand shape, cooled in a water bath, and cut using a pelletizer to obtain pellets. The resulting pellets were melt-kneaded using a single-screw extruder with a T-die and a cylinder setting temperature of 180 to 240 ° C. at a discharge rate of 150 kg / h, and extruded from the T-die at a die temperature of 240 ° C. The extrusion was performed by contacting both sides with a metal casting roll temperature-controlled at 90 ° C. and a touch roll equipped with an elastic metal sleeve temperature-controlled at 60 ° C., and the film was formed while cooling and solidifying, and then wound up to obtain a 75 μm thick acrylic resin film (D1).
[0152] <Preparation of Laminate> A curable resin composition for a hard coat layer was applied to one side of the obtained acrylic resin film using a bar coater. The film was then dried at 80°C for 2 minutes to volatilize the solvent, and then irradiated with an ultraviolet (UV) irradiator under a nitrogen atmosphere (oxygen concentration 1% or less) at a UV integrated light dose of 460 mJ to form a hard coat layer (thickness 5 μm), thereby obtaining a laminate. As the curable resin composition for the hard coat layer, a composition was used in which reactive HALS (manufactured by ADEKA Corporation, product name "ADK STAB LA-82", hereinafter also referred to as LA82) was added to Coating 1 so that the amount was 2 parts per 100 parts of the solids content of Coating 1.
[0153] Example 2 An acrylic graft copolymer (A) having an average particle size of 80 nm, prepared in the same manner as in Reference Example 4 of JP-A 2004-137299, was used as the graft copolymer particles (A-2), and poly(methyl methacrylate) (Sumipex (registered trademark) EX, manufactured by Sumitomo Chemical Co., Ltd.) was used as the acrylic resin (D-2). An acrylic resin film (D2) and a laminate were obtained in the same manner as in Example 1, except that 100 parts of a resin mixture 2 consisting of 70% of the graft copolymer particles (A-2) and 30% of the acrylic resin (D-2) was used and the discharge rate from the T-die was 110 kg / hr.
[0154] Example 3 A multilayer structure acrylic resin having an average particle size of 130 nm, prepared in the same manner as in A-3 in Table 1 of JP-A No. 2015-7255, was used as the graft copolymer particles (A-3). An acrylic resin film (D3) and a laminate were obtained in the same manner as in Example 1, except that 100 parts of a resin mixture 3 consisting of 40% of the graft copolymer particles (A-3) and 60% of the acrylic resin (D-2) was used.
[0155] (Example 4) Graft copolymer particles (A-4) were prepared in the same manner as in Production Example 1 of WO 2019 / 181752 using graft copolymer particles (A) having an average particle size of 80 nm, and graft copolymer particles (B-1) were prepared in the same manner as in Production Example 12 of WO 2019 / 181752 using graft copolymer particles (B) having an average particle size of 230 nm. An acrylic resin film (D4) and a laminate were obtained in the same manner as in Example 1, except that 100 parts of a resin mixture 4 consisting of 30% graft copolymer particles (A-4), 4% graft copolymer particles (B-1), and 66% acrylic resin (D-2) was used.
[0156] Comparative Example 1 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that Paint 1 was used as the curable resin composition for the hard coat layer.
[0157] Comparative Example 2 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which a hydroxyphenyltriazine-based ultraviolet absorber (manufactured by BASF, trade name "Tinuvin (registered trademark) 400", hereinafter also referred to as Tinuvin 400) was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0158] Comparative Example 3 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which a hydroxyphenyltriazine-based ultraviolet absorber (manufactured by BASF, product name "Tinuvin (registered trademark) 479" (hereinafter also referred to as Tinuvin 479) was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0159] Comparative Example 4 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which Tinuvin 400 and HALS (trade name "ADK STAB LA-81", manufactured by BASF, hereinafter also referred to as LA81) were added to Coating 1 so that the amounts were 2 parts and 1 part, respectively, per 100 parts of the solid content of Coating 1, was used as the curable resin composition for the hard coat layer.
[0160] Comparative Example 5 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which LA81 was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0161] Comparative Example 6 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which LA82 was added to Coating 2 so that the amount was 2 parts per 100 parts of the solid content of Coating 2 was used as the curable resin composition for the hard coat layer.
[0162] Comparative Example 7 An acrylic resin film and a laminate were obtained in the same manner as in Example 2, except that Paint 1 was used as the curable resin composition for the hard coat layer.
[0163] (Comparative Example 8) An acrylic resin film and a laminate were obtained in the same manner as in Example 2, except that a composition in which Tinuvin 400 was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0164] (Comparative Example 9) An acrylic resin film and a laminate were obtained in the same manner as in Example 2, except that a composition in which Tinuvin 479 was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0165] (Comparative Example 10) An acrylic resin film and a laminate were obtained in the same manner as in Example 2, except that a composition in which Tinuvin 400 and LA81 were added to Coating 1 so that the amounts were 2 parts and 1 part, respectively, per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0166] Comparative Example 11 An acrylic resin film and a laminate were obtained in the same manner as in Example 1, except that a composition in which LA81 was added to Coating 1 so that the amount was 2 parts per 100 parts of the solid content of Coating 1 was used as the curable resin composition for the hard coat layer.
[0167] Reference Example 1 An acrylic resin film was prepared in the same manner as in Example 1.
[0168] Reference Example 2 An acrylic resin film was prepared in the same manner as in Example 2 as Reference Example 2.
[0169] In the examples and comparative examples, the crack elongation at 120°C, ΔHz after 80% stretching at 120°C, ΔHz after 20% stretching at room temperature, haze, pencil hardness, chemical resistance, and weather resistance of the laminates were measured as described above, and the results are shown in Tables 1 and 2 below. In the examples and comparative examples, the thickness of the acrylic resin film, the tensile break elongation at 120°C, and glass transition temperature, as well as the thickness of the hard coat layer, were measured as described above, and the results are shown in Tables 1 and 2 below. Tables 1 and 2 below also show the composition of the hard coat layer, with the blending amount in parts by mass relative to 100 parts by mass of the solids content of the coating. In the reference examples, the crack elongation at 120°C, ΔHz after 80% stretching at 120°C, ΔHz after 20% stretching at room temperature, haze, pencil hardness, chemical resistance, and weather resistance of the acrylic resin film were measured as described above, and the results are shown in the laminate column in Table 2 below. In Tables 1 and 2 below, "-" means not measured.
[0170]
[0171]
[0172] As can be seen from Table 1 above, the laminates of Examples 1 to 4 had a crack elongation of 100% or more at 120°C and exhibited good secondary formability. Furthermore, even after 2000 hours of accelerated weather resistance testing, the laminates of Examples 1 to 4 did not develop cracks on the surface of the hard coat layer and had a color difference of 0.3 or less, demonstrating good long-term weather resistance.
[0173] On the other hand, as can be seen from Tables 1 and 2 above, the laminates of Comparative Examples 1 to 5 and 7 to 11, in which the hard coat layer did not contain a reactive HALS, showed cracks on the surface of the hard coat layer after 1000 hours or 2000 hours of accelerated weather resistance testing, and had poor long-term weather resistance. Furthermore, the laminate of Comparative Example 6, in which a low-stretch coating material was used as the curable resin composition for the hard coat layer, had a crack elongation of less than 100% at 120°C, and thus had poor secondary formability.
[0174] The present invention is not particularly limited, and may include, for example, the following embodiments: [1] A laminate including an acrylic resin film and a hard coat layer laminated on at least one surface of the acrylic resin film, wherein the acrylic resin film has a tensile elongation at break of 200% or more at 120°C, the hard coat layer is formed of a cured product of a curable resin composition containing a urethane acrylate resin and a hindered amine light stabilizer having a reactive functional group, and the laminate has a tensile crack elongation of 100% or more at 120°C. [2] The laminate is placed so that the hard coat layer side faces a light source, and a xenon lamp is used as the light source to simulate direct sunlight, with an irradiance of 180 W / m 2[1] The laminate according to [1], wherein after an accelerated weathering test under conditions of (300-400 nm), the laminate exhibits no cracking on the surface of the hard coat layer after 1,000 cycles (2,000 hours in total) of a 120-minute cycle consisting of Step 1: 102 minutes of exposure, black panel temperature 60±3°C, relative humidity 65±5%, and no rainfall, and Step 2: 18 minutes of exposure, chamber temperature 38±3°C, relative humidity 95±5%, and rainfall. [3] The laminate according to [1] or [2], wherein the hard coat layer side of the laminate has a pencil hardness of B or higher under a 500 g load, and there is no visible change in appearance when approximately 0.02 mL of isopropyl alcohol or acetone is dropped onto the surface of the hard coat layer and allowed to stand at 23°C for 6 hours. [4] The laminate according to any one of [1] to [3], wherein the change in color difference ΔE of the laminate after the accelerated weathering test (2,000 hours in total) is less than 0.5. [5] The laminate according to any one of [1] to [4], wherein the urethane acrylate resin is active energy ray-curable. [6] The laminate according to any one of [1] to [5], wherein the reactive functional group comprises at least one selected from the group consisting of a methacryloyl group and an acryloyl group. [7] The laminate according to any one of [1] to [6], wherein the curable resin composition comprises 1 to 10 parts by mass of a hindered amine light stabilizer having a reactive functional group per 100 parts by mass of the urethane acrylate resin. [8] A resin molded product comprising the laminate according to any one of [1] to [7] and a thermoplastic resin substrate, wherein at least a portion of the thermoplastic resin substrate is coated with the laminate in such a manner that the acrylic resin film faces the thermoplastic resin substrate. [9] The resin molded product according to [8], wherein the thermoplastic resin substrate has a three-dimensional shape.
[0175] The embodiments described above are not independent of each other, and those skilled in the art can combine them as appropriate without needing to go into excessive detail. Furthermore, components from different embodiments may be combined as appropriate.
[0176] 1 Laminate 2 Acrylic resin film 3 Hard coat layer
Claims
1. A laminate comprising an acrylic resin film and a hard coat layer laminated on at least one side of the acrylic resin film, wherein the acrylic resin film has a tensile break elongation of 200% or more at 120°C, the hard coat layer is formed from a cured product of a curable resin composition containing a urethane acrylate resin and a hindered amine light stabilizer having a reactive functional group, and the laminate has a tensile crack elongation of 100% or more at 120°C.
2. The laminate was placed so that the hard coat layer side was facing the light source. A xenon lamp was used as the light source to simulate direct sunlight, and the irradiance was 180 W / m 2 2. The laminate according to claim 1, wherein after an accelerated weathering test is performed under conditions of (300 to 400 nm), in which a cycle of 120 minutes in total consisting of step 1 with an exposure time of 102 minutes, a black panel temperature of 60±3° C., a relative humidity of 65±5%, and no rainfall, and step 2 with an exposure time of 18 minutes, a tank temperature of 38±3° C., a relative humidity of 95±5%, and rainfall is performed for 1000 cycles (total of 2000 hours), no cracks are generated on the surface of the hard coat layer of the laminate.
3. The laminate according to claim 1, wherein the pencil hardness of the hard coat layer side is B or higher under a load of 500 g, and when approximately 0.02 mL of isopropyl alcohol or acetone is dropped onto the surface of the hard coat layer and allowed to stand at 23° C. for 6 hours, there is no visible change in appearance.
4. The laminate according to claim 1, wherein the change in color difference ΔE of the laminate after the accelerated weather resistance test (total of 2000 hours) is less than 0.
5.
5. The laminate according to claim 1, wherein the urethane acrylate resin is curable by active energy rays.
6. The laminate according to claim 1, wherein the reactive functional group includes at least one selected from the group consisting of a methacryloyl group and an acryloyl group.
7. The laminate according to claim 1, wherein the curable resin composition contains 1 to 10 parts by mass of a hindered amine-based light stabilizer having a reactive functional group per 100 parts by mass of the urethane acrylate resin.
8. A resin molded product comprising the laminate according to any one of claims 1 to 7 and a thermoplastic resin substrate, wherein at least a portion of the thermoplastic resin substrate is covered with the laminate in such a manner that the acrylic resin film faces the thermoplastic resin substrate.
9. The resin molded article according to claim 8, wherein the thermoplastic resin substrate has a three-dimensional shape.
Citation Information
Patent Citations
Hardcoat film, and hardcoat resin-molded product using the hardcoat film
JP2012207120A
Method of manufacturing weather resistant hard coat film
JP2012210739A
Decorative sheet for three-dimensional molding, method for producing the decorative sheet, decorative resin molding, and method for producing the decorative resin molding
JP2012213926A
Film for lamination of organic glass
JP5267700B1
Laminating film for use in organic glass
WO2015015553A1
Cited By
Molding film
WO2026155097A1