Aqueous dispersion and multilayer body
The use of ethylene-unsaturated carboxylic acid copolymers with specific carboxyl group content ratios in an aqueous dispersion improves storage stability and bonding efficiency by forming a stable adhesive layer, addressing the limitations of conventional dispersions in heat sealing processes.
Patent Information
- Application Number
- PCT/JP2024/010668
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional aqueous dispersions used in heat sealing lack sufficient storage stability, leading to decreased compatibility and uniformity of resin phases, which affects the bonding process and productivity in laminates.
An aqueous dispersion comprising a blend of ethylene-unsaturated carboxylic acid copolymers with specific carboxyl group content ratios, including a first, second, and third copolymer with varying carboxyl group contents, is used to form a stable adhesive layer that enhances storage stability and bonding efficiency.
The dispersion achieves improved storage stability and uniform particle formation, resulting in enhanced bonding efficiency and productivity through a sea-island structure formation, where the differences in carboxyl group content between the copolymers are within predetermined ranges.
Smart Images

Figure JP2024010668_03102024_PF_FP_ABST
Abstract
Description
Water dispersion and laminate
[0001] The present invention relates to an aqueous dispersion and a laminate.
[0002] It has been known in various industrial fields to bond substrates such as plastic films, vapor-deposited films, metal foils, paper, nonwoven fabrics, etc. together by heat and pressure (i.e., heat sealing). In heat sealing, an adhesive layer is usually formed on the substrate in advance, and the substrates are bonded to each other or to another adherend via the adhesive layer.
[0003] Aqueous dispersions containing resins are known as materials used for adhesive layers. For example, an aqueous dispersion containing water, resin A (ethylene-acrylic acid copolymer (acrylic acid content: 20.5% by mass)), resin B (ethylene-methacrylic acid copolymer (methacrylic acid content: 15% by mass)), and resin C (ethylene-methacrylic acid copolymer (methacrylic acid content: 10% by mass)) has been proposed (see, for example, aqueous dispersion 2 in Patent Document 1).
[0004] International Publication No. 2022 / 014588 Pamphlet
[0005] On the other hand, the aqueous dispersion is required to have better storage stability.
[0006] The present invention provides an aqueous dispersion having excellent storage stability, and a laminate having an adhesive layer which is a dried product of the aqueous dispersion.
[0007] The present invention [1] is an aqueous dispersion comprising a resin component and water, wherein the resin component comprises an ethylene-unsaturated carboxylic acid copolymer, and the ethylene-unsaturated carboxylic acid copolymer comprises a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer, each of which has a different carboxyl group content, wherein the difference (C-B) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg and is 0.50 mmol / kg or less, and the difference (B-A) between the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg and is 0.80 mmol / kg or less.
[0008] The present invention [2] includes the aqueous dispersion according to the above [1], wherein the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer is 1.00 mmol / kg or more and less than 1.40 mmol / kg, the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer is 1.40 mmol / kg or more and less than 1.80 mmol / kg, and the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer is 1.80 mmol / kg or more and less than 2.30 mmol / kg.
[0009] The present invention [3] includes the aqueous dispersion according to the above [1] or [2], wherein the content of the first ethylene-unsaturated carboxylic acid copolymer is 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer; the content of the second ethylene-unsaturated carboxylic acid copolymer is 5 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer; and the content of the third ethylene-unsaturated carboxylic acid copolymer is 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer.
[0010] The present invention [4] includes the aqueous dispersion according to any one of the above [1] to [3], in which the content of the third ethylene-unsaturated carboxylic acid copolymer is equal to or greater than the content of the first ethylene-unsaturated carboxylic acid copolymer, and the content of the first ethylene-unsaturated carboxylic acid copolymer is greater than the content of the second ethylene-unsaturated carboxylic acid copolymer.
[0011] The present invention [5] includes the aqueous dispersion according to any one of the above [1] to [4], wherein the first ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid, the second ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid, and the third ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and acrylic acid.
[0012] The present invention [6] includes a laminate comprising a substrate and an adhesive layer in this order toward one side in the thickness direction, and the adhesive layer is a dried product of the aqueous dispersion according to any one of the above [1] to [5].
[0013] In the aqueous dispersion of the present invention, the ethylene-unsaturated carboxylic acid copolymer includes a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer, each of which has a different carboxyl group content. The difference (C-B) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer, and the difference (B-A) between the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer are within a predetermined range. Therefore, the aqueous dispersion has excellent storage stability.
[0014] The laminate of the present invention has an adhesive layer which is a dried product of the aqueous dispersion of the present invention, and therefore has excellent productivity.
[0015] FIG. 1 is a schematic diagram showing one embodiment of a laminate of the present invention. FIGS. 2A to 2C are schematic diagrams showing one embodiment of a method for producing a laminate of the present invention and a method for bonding substrates together using this laminate. FIG. 2A shows a first step of preparing a first substrate. FIG. 2B shows a second step of disposing an adhesive layer on one thickness-wise surface of the first substrate. FIG. 2C shows a step of disposing a second substrate on one thickness-wise surface of the adhesive layer and bonding the first substrate and second substrate by thermocompression bonding. FIGS. 3A and 3B show modified examples of the method for producing a laminate of the present invention. FIG. 3A shows a step of disposing an adhesive layer on each of the first substrate and the second substrate. FIG. 3B shows a step of bonding the first substrate and the second substrate via the adhesive layer. FIG. 4 shows a schematic diagram of an ethylene-unsaturated carboxylic acid copolymer in an aqueous dispersion.
[0016] The aqueous dispersion contains a resin component and water.
[0017] <Resin Component> The resin component contains an ethylene-unsaturated carboxylic acid copolymer.
[0018] [Ethylene-unsaturated carboxylic acid copolymer] The ethylene-unsaturated carboxylic acid copolymer includes a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer, each of which has a different carboxyl group content.
[0019] (First ethylene-unsaturated carboxylic acid copolymer) The first ethylene-unsaturated carboxylic acid copolymer will be described in detail later, but is a resin having a relatively low carboxyl group content compared to the second ethylene-unsaturated carboxylic acid copolymer and the third ethylene-unsaturated carboxylic acid copolymer.
[0020] The first ethylene-unsaturated carboxylic acid copolymer is obtained by polymerizing a first monomer component comprising ethylene and a first unsaturated carboxylic acid.
[0021] The first unsaturated carboxylic acid is a monomer having both at least one ethylenically unsaturated bond and a carboxy group. Examples of the first unsaturated carboxylic acid include monobasic acids and dibasic acids. Examples of the monobasic acids include acrylic acid, methacrylic acid, and crotonic acid. Examples of the dibasic acids include maleic acid, fumaric acid, and itaconic acid. Preferably, the first unsaturated carboxylic acid is a monobasic acid. From the viewpoint of improving storage stability, more preferably, the first unsaturated carboxylic acid is methacrylic acid. In other words, more preferably, the first ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid.
[0022] The primary unsaturated carboxylic acids may be used alone or in combination of two or more kinds.
[0023] In the first monomer component, the ethylene content and the first unsaturated carboxylic acid content are appropriately adjusted so that the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer described below falls within a predetermined range. Specifically, when the first unsaturated carboxylic acid is methacrylic acid, the first unsaturated carboxylic acid content is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and for example, 12% by mass or less, preferably 10% by mass or less, based on the total amount of ethylene and the first unsaturated carboxylic acid. Furthermore, the ethylene content is, for example, 88% by mass or more, preferably 90% by mass or more, and for example, 99% by mass or less, preferably 95% by mass or less, more preferably 92% by mass or less, based on the total amount of ethylene and the first unsaturated carboxylic acid.
[0024] The polymerization of the first monomer component is not particularly limited, and a known polymerization method may be adopted, such as a method of contacting the first monomer component with a polymerization initiator (peroxide) under high temperature and high pressure conditions.
[0025] This results in the production of the first ethylene-unsaturated carboxylic acid copolymer. Alternatively, the first ethylene-unsaturated carboxylic acid copolymer can be prepared as a dispersion in which particles of the first ethylene-unsaturated carboxylic acid copolymer are dispersed in water.
[0026] The weight average molecular weight of the first ethylene-unsaturated carboxylic acid copolymer, as calculated using standard polystyrene standards by gel permeation chromatography (GPC), is, for example, 8,000 or more, preferably 10,000 or more, and for example, 150,000 or less, preferably 100,000 or less.
[0027] The carboxyl group content A and the content ratio of the first ethylene-unsaturated carboxylic acid copolymer will be described later.
[0028] (Second Ethylene-Unsaturated Carboxylic Acid Copolymer) The second ethylene-unsaturated carboxylic acid copolymer will be described in detail later, but is a resin having a relatively higher carboxyl group content than the first ethylene-unsaturated carboxylic acid copolymer and a relatively lower carboxyl group content than the third ethylene-unsaturated carboxylic acid copolymer.
[0029] The second ethylene-unsaturated carboxylic acid copolymer is obtained by polymerizing a second monomer component comprising ethylene and a second unsaturated carboxylic acid.
[0030] Examples of the second unsaturated carboxylic acid include the same unsaturated carboxylic acids as the first unsaturated carboxylic acid. Preferably, the second unsaturated carboxylic acid is a monobasic acid. From the viewpoint of improving storage stability, more preferably, the second unsaturated carboxylic acid is methacrylic acid. In other words, more preferably, the second ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid.
[0031] The secondary unsaturated carboxylic acids may be used alone or in combination of two or more kinds.
[0032] In the second monomer component, the ethylene content and the second unsaturated carboxylic acid content are appropriately adjusted so that the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer described below falls within a predetermined range. Specifically, when the second unsaturated carboxylic acid is methacrylic acid, the second unsaturated carboxylic acid content is, for example, more than 12% by mass, preferably 14% by mass or more, and for example, 20% by mass or less, preferably 16% by mass or less, based on the total amount of ethylene and the second unsaturated carboxylic acid. Furthermore, the ethylene content is, for example, 80% by mass or more, preferably 84% by mass or more, and for example, less than 88% by mass, preferably 86% by mass or less, based on the total amount of ethylene and the second unsaturated carboxylic acid.
[0033] The polymerization method for the second monomer component is the same as the polymerization method for the first monomer component.
[0034] This results in the second ethylene-unsaturated carboxylic acid copolymer. The second ethylene-unsaturated carboxylic acid copolymer can also be prepared as a dispersion in which particles of the second ethylene-unsaturated carboxylic acid copolymer are dispersed in water.
[0035] The weight average molecular weight of the second ethylene-unsaturated carboxylic acid copolymer, as calculated using standard polystyrene standards by gel permeation chromatography (GPC), is, for example, 8,000 or more, preferably 10,000 or more, and for example, 150,000 or less, preferably 100,000 or less.
[0036] The carboxyl group content B and the content ratio of the second ethylene-unsaturated carboxylic acid copolymer will be described later.
[0037] (Third Ethylene-Unsaturated Carboxylic Acid Copolymer) The third ethylene-unsaturated carboxylic acid copolymer will be described in detail later, but is a resin having a relatively high carboxyl group content compared to the first ethylene-unsaturated carboxylic acid copolymer and the second ethylene-unsaturated carboxylic acid copolymer.
[0038] The third ethylene-unsaturated carboxylic acid copolymer is obtained by polymerizing a third monomer component comprising ethylene and a tertiary unsaturated carboxylic acid.
[0039] Examples of the tertiary unsaturated carboxylic acid include unsaturated carboxylic acids similar to those of the first unsaturated carboxylic acid. Preferably, the tertiary unsaturated carboxylic acid is a monobasic acid. From the viewpoint of improving storage stability, more preferably, the tertiary unsaturated carboxylic acid is acrylic acid. In other words, more preferably, the tertiary ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and acrylic acid.
[0040] If the first ethylene-unsaturated carboxylic acid copolymer and the second ethylene-unsaturated carboxylic acid copolymer are copolymers of ethylene and methacrylic acid, while the third ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and acrylic acid, the storage stability can be further improved.
[0041] The tertiary unsaturated carboxylic acids can be used alone or in combination of two or more kinds.
[0042] In the third monomer component, the ethylene content and the tertiary unsaturated carboxylic acid content are appropriately adjusted so that the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer described below falls within a predetermined range. Specifically, when the tertiary unsaturated carboxylic acid is acrylic acid, the tertiary unsaturated carboxylic acid content is, for example, more than 12% by mass, preferably 14% by mass or more, and for example, 20% by mass or less, preferably 16% by mass or less, based on the total amount of ethylene and the tertiary unsaturated carboxylic acid. Furthermore, the ethylene content is, for example, 80% by mass or more, preferably 84% by mass or more, and for example, less than 88% by mass, preferably 86% by mass or less, based on the total amount of ethylene and the tertiary unsaturated carboxylic acid.
[0043] The polymerization method for the third monomer component is the same as the polymerization method for the first monomer component.
[0044] This results in a third ethylene-unsaturated carboxylic acid copolymer. Alternatively, the third ethylene-unsaturated carboxylic acid copolymer can be prepared as a dispersion in which particles of the third ethylene-unsaturated carboxylic acid copolymer are dispersed in water.
[0045] The weight average molecular weight of the third ethylene-unsaturated carboxylic acid copolymer, as measured by gel permeation chromatography (GPC) and converted into standard polystyrene, is, for example, 8,000 or more, preferably 10,000 or more, and for example, 150,000 or less, preferably 100,000 or less.
[0046] The carboxyl group content C and the content ratio of the third ethylene-unsaturated carboxylic acid copolymer will be described later.
[0047] [Carboxyl Group Content and Content Ratio] As described above, the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer have different carboxyl group contents.
[0048] The carboxyl group content can be calculated from the charged amount. Specifically, it can be calculated based on the following formula (1): (carboxyl group content [mmol / kg]) = 1 [Kg] × weight content of carboxyl group-containing monomer [%] / (molar mass of carboxyl group-containing monomer [kg / mol]) × 1000 (1)
[0049] Specifically, the carboxyl group contents are adjusted to increase in the order of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer. In other words, the first ethylene-unsaturated carboxylic acid copolymer has a relatively low carboxyl group content, the second ethylene-unsaturated carboxylic acid copolymer has a relatively medium carboxyl group content, and the third ethylene-unsaturated carboxylic acid copolymer has a relatively high carboxyl group content.
[0050] In this aqueous dispersion, the difference (C-B) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer having a relatively high carboxyl group content and the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content, and the difference (B-A) between the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer having a relatively low carboxyl group content are adjusted to be within predetermined ranges.
[0051] Specifically, the difference (C - B) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg, and is preferably 0.10 mmol / kg or more, more preferably 0.20 mmol / kg or more, even more preferably 0.30 mmol / kg or more, and is 0.50 mmol / kg or less, preferably 0.40 mmol / kg or less, more preferably 0.35 mmol / kg or less.
[0052] Furthermore, the difference (B - A) between the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg, and is preferably 0.20 mmol / kg or more, more preferably 0.40 mmol / kg or more, even more preferably 0.50 mmol / kg or more, and is 0.80 mmol / kg or less, preferably 0.70 mmol / kg or less, more preferably 0.60 mmol / kg or less.
[0053] When the differences ((C−B) and (B−A)) are within the above ranges, the storage stability can be improved.
[0054] On the other hand, if the differences ((C−B) and (B−A)) are outside the above ranges, the storage stability will be reduced.
[0055] Furthermore, the difference (C - A) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg, for example, and is preferably 0.20 mmol / kg or more, more preferably 0.40 mmol / kg or more, even more preferably 0.60 mmol / kg or more, particularly preferably 0.90 mmol / kg or more, and is, for example, 1.30 mmol / kg or less, preferably 1.20 mmol / kg or less, more preferably 1.10 mmol / kg or less, even more preferably 1.00 mmol / kg or less, particularly preferably 0.95 mmol / kg or less.
[0056] If the difference ((C−A)) is within the above range, the storage stability can be further improved.
[0057] The carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer is, for example, 1.00 mmol / kg or more, preferably 1.04 mmol / kg or more, more preferably 1.10 mmol / kg or more, and even more preferably 1.15 mmol / kg or more, and for example, less than 1.40 mmol / kg, preferably 1.30 mmol / kg or less, and more preferably 1.20 mmol / kg or less.
[0058] The carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer is, for example, 1.40 mmol / kg or more, preferably 1.50 mmol / kg or more, more preferably 1.60 mmol / kg or more, and even more preferably 1.70 mmol / kg or more, and for example, less than 1.80 mmol / kg, preferably 1.75 mmol / kg or less.
[0059] The carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer is, for example, 1.80 mmol / kg or more, preferably 1.90 mmol / kg or more, more preferably 2.00 mmol / kg or more, and for example, less than 2.30 mmol / kg, preferably 2.20 mmol / kg or less, more preferably 2.10 mmol / kg or less.
[0060] When the carboxyl group contents A to C are within the above ranges, the storage stability can be further improved.
[0061] The content of the first ethylene-unsaturated carboxylic acid copolymer is, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer, is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, more preferably more than 20 parts by mass, even more preferably 20 parts by mass or more, particularly preferably 30 parts by mass or more, and for example, 70 parts by mass or less, preferably 60 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, particularly preferably 35 parts by mass or less.
[0062] The content ratio of the second ethylene-unsaturated carboxylic acid copolymer relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and for example, 50 parts by mass or less, preferably 40 parts by mass or less, more preferably 30 parts by mass or less, and even more preferably 20 parts by mass or less.
[0063] The content of the third ethylene-unsaturated carboxylic acid copolymer, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer, is, for example, 20 parts by mass or more, preferably 30 parts by mass or more, more preferably 40 parts by mass or more, even more preferably more than 40 parts by mass, particularly preferably 45 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less.
[0064] When the content is within the above range, the storage stability can be further improved.
[0065] From the viewpoint of improving storage stability, the content of the third ethylene-unsaturated carboxylic acid copolymer is preferably equal to or greater than the content of the first ethylene-unsaturated carboxylic acid copolymer, and the content of the first ethylene-unsaturated carboxylic acid copolymer is preferably greater than the content of the second ethylene-unsaturated carboxylic acid copolymer.
[0066] In such a case, the content of the second ethylene-unsaturated carboxylic acid copolymer is, for example, 5 parts by mass or more, preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and for example, 20 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer.
[0067] The content of the first ethylene-unsaturated carboxylic acid copolymer is, for example, more than 20 parts by mass, preferably 25 parts by mass or more, more preferably 30 parts by mass or more, and for example, 40 parts by mass or less, preferably 35 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer.
[0068] The content of the third ethylene-unsaturated carboxylic acid copolymer is, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer, for example, 40 parts by mass or more, preferably more than 40 parts by mass, more preferably 45 parts by mass or more, and for example, 80 parts by mass or less, preferably 70 parts by mass or less, more preferably 60 parts by mass or less, and even more preferably 50 parts by mass or less.
[0069] [Preparation of Ethylene-Unsaturated Carboxylic Acid Copolymer] The ethylene-unsaturated carboxylic acid copolymer is prepared by mixing the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer, and melt-kneading the mixture using a known kneading device.
[0070] The ethylene-unsaturated carboxylic acid copolymer is preferably prepared as a dispersion in which particles of the ethylene-unsaturated carboxylic acid copolymer are dispersed in water.
[0071] Furthermore, additives may be blended into the ethylene-unsaturated carboxylic acid copolymer dispersion in order to improve production stability. Examples of additives include pH adjusters, sequestering agents (e.g., ethylenediaminetetraacetic acid and its salts), molecular weight regulators (chain transfer agents, e.g., mercaptans and low-molecular-weight halogen compounds), and lubricants (e.g., N-oleyl palmitamide, ethylene bisoleamide, N-stearyl erucamide). The blending ratio of the additives is appropriately determined depending on the purpose and application.
[0072] Furthermore, the carboxy groups of the ethylene-unsaturated carboxylic acid copolymers (specifically, the carboxy groups of the first ethylene-unsaturated carboxylic acid copolymer, the carboxy groups of the second ethylene-unsaturated carboxylic acid copolymer, and the carboxy groups of the third ethylene-unsaturated carboxylic acid copolymer) are preferably neutralized from the viewpoint of dispersion stability.
[0073] To neutralize the ethylene-unsaturated carboxylic acid copolymer, for example, a neutralizing agent is added to a dispersion of the ethylene-unsaturated carboxylic acid copolymer.
[0074] Examples of the neutralizing agent include basic compounds. Examples of the basic compound include inorganic basic compounds and organic basic compounds. Examples of the inorganic basic compound include sodium hydroxide, potassium hydroxide, lithium hydroxide, rubidium hydroxide, and cesium hydroxide. Examples of the organic basic compound include ammonia, triethylamine, triethanolamine, diethylamine, and dimethylethanolamine. Examples of the neutralizing agent include inorganic basic compounds. Examples of the neutralizing agent include potassium hydroxide.
[0075] The amount of the neutralizing agent added is, for example, 5 mol or more and, for example, 200 mol or less, preferably 150 mol or less, per 100 mol of carboxy groups in the ethylene-unsaturated carboxylic acid copolymer.
[0076] The neutralizing agents can be used alone or in combination of two or more kinds.
[0077] After the neutralizing agent is added, the dispersion of the ethylene-unsaturated carboxylic acid copolymer is preferably maintained at a predetermined temperature for a predetermined time.
[0078] The holding conditions include a holding temperature of, for example, 40° C. or higher, preferably 50° C. or higher, more preferably 100° C. or higher, and for example, 190° C. or lower, preferably 180° C. or lower. The holding time is, for example, 30 minutes or longer, preferably 1 hour or longer, more preferably 2 hours or longer, and for example, 12 hours or shorter, preferably 10 hours or shorter, more preferably 6 hours or shorter.
[0079] This neutralizes the carboxy groups of the ethylene-unsaturated carboxylic acid copolymer.
[0080] The degree of neutralization is, for example, 10% or more, preferably 15% or more, and for example, 60% or less, preferably 50% or less, more preferably 40% or less.
[0081] The degree of neutralization can be measured by infrared absorption spectroscopy.
[0082] In addition, in the dispersion of the ethylene-unsaturated carboxylic acid copolymer, the solids concentration of the ethylene-unsaturated carboxylic acid copolymer is, for example, 10% by mass or more, preferably 20% by mass or more, more preferably 30% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less.
[0083] The content of the ethylene-unsaturated carboxylic acid copolymer relative to the resin component is, for example, 80% by mass or more, preferably 90% by mass or more, more preferably 95% by mass or more, or, for example, 100% by mass.
[0084] [Other Resins] The resin component may contain other resins as needed.
[0085] Examples of other resins include polyolefin resins, such as polyethylene (e.g., linear low-density polyethylene, high-density polyethylene), polypropylene, propylene-ethylene copolymers, and ethylene-butene copolymers.
[0086] The other resins may be used alone or in combination of two or more kinds.
[0087] The other resin preferably does not contain any other resin and comprises an ethylene-unsaturated carboxylic acid copolymer.
[0088] The blending ratio of the resin component relative to the aqueous dispersion is, for example, 10 mass % or more, preferably 20 mass % or more, more preferably 30 mass % or more, and for example, 60 mass % or less, preferably 50 mass % or less.
[0089] [Method for producing aqueous dispersion] The aqueous dispersion is produced by blending a resin component and optional additives. Specifically, the aqueous dispersion is produced by blending a dispersion of an ethylene-unsaturated carboxylic acid copolymer (ethylene-unsaturated carboxylic acid copolymer and water), optional other resins, and optional additives.
[0090] Examples of additives include curing agents, crosslinking agents, film-forming aids, antifoaming agents, tackifiers, hardness-imparting agents, preservatives, thickeners, antifreeze agents, dispersants, inorganic pigments, and organic pigments. The additives are blended in appropriate ratios. The additives can be used alone or in combination of two or more types.
[0091] This gives an aqueous dispersion.
[0092] The viscosity (25°C) of the aqueous dispersion is, for example, 100 mPa·s or more, preferably 120 mPa·s or more, more preferably 140 mPa·s or more, and even more preferably 150 mPa·s or more, and for example, 400 mPa·s or less, preferably 350 mPa·s or less, and more preferably 300 mPa·s or less.
[0093] The viscosity can be measured, for example, by a Brookfield viscometer.
[0094] This aqueous dispersion can be suitably used as an adhesive for bonding substrates together. That is, such an adhesive contains the aqueous dispersion. The adhesive containing the aqueous dispersion is a thermocompression (thermal fusion) type adhesive.
[0095] <Laminate> One embodiment of a laminate 10 will be described in detail with reference to FIG.
[0096] In Figure 1, the up-down direction of the paper surface is the up-down direction (thickness direction), and the upper side of the paper surface is the upper side (one side in the thickness direction), and the lower side of the paper surface is the lower side (the other side in the thickness direction). The left-right direction and the depth direction of the paper surface are surface directions perpendicular to the up-down direction. Specifically, they correspond to the directional arrows in each figure.
[0097] As shown in FIG. 1, the laminate 10 includes a first base material 1 as a base material and an adhesive layer 2 in this order toward one side in the thickness direction.
[0098] [First Substrate] The first substrate 1 has a film shape. The first substrate 1 is disposed on the entire lower surface of the adhesive layer 2 so as to be in contact with the lower surface of the adhesive layer 2 .
[0099] The first substrate 1 is not particularly limited. Examples of the first substrate 1 include resin films, metal films, and paper. Examples of materials for the resin film include polymeric materials. Examples of polymeric materials include olefin resins (e.g., polyethylene and polypropylene), acrylic resins, polyester resins, polycarbonate resins, acrylonitrile-styrene-butadiene copolymer resins (ABS resins), polyamide resins (e.g., nylon), and polyphenylene sulfide resins. Examples of materials for the metal film include aluminum, gold, silver, copper, nickel, zinc, titanium, cobalt, indium, and chromium. Examples of materials for the paper include cellulose.
[0100] The first substrate 1 may be subjected to a surface treatment as needed. Examples of the surface treatment include ink (solvent-based or water-based) coating treatment, plating treatment, coupling treatment, and vacuum plasma treatment.
[0101] There are no particular limitations on the thickness of the first substrate 1. The thickness of the first substrate 1 is, for example, 10 μm or more and, for example, 100 μm or less.
[0102] [Adhesive Layer] The adhesive layer 2 is a dried product of an aqueous dispersion. The adhesive layer 2 is a heat seal layer.
[0103] The thickness of the adhesive layer 2 is, for example, 0.1 μm or more and, for example, 10 μm or less.
[0104] [Method for Manufacturing Laminate] One embodiment of a method for manufacturing the laminate 10 will be described in detail with reference to FIGS. 2A and 2B.
[0105] The method for manufacturing the laminate 10 includes a first step of preparing a first substrate 1 and a second step of arranging an adhesive layer 2 on one surface of the first substrate 1 in the thickness direction.
[0106] [First Step] In the first step, as shown in FIG. 2A, a first substrate 1 is prepared.
[0107] [Second Step] In the second step, as shown in FIG. 2B, the adhesive layer 2 is disposed on one surface of the first substrate 1 in the thickness direction.
[0108] To dispose the adhesive layer 2 on one surface in the thickness direction of the first substrate 1, the above-mentioned aqueous dispersion is applied to one surface in the thickness direction of the first substrate 1, and then dried.
[0109] Examples of the coating method include known coating methods such as a bar coater method, a curtain coating method, a roll coating method, and a blade coating method.
[0110] The drying temperature is, for example, 50° C. or more, or preferably 80° C. or more, and for example, 120° C. or less. The drying time is, for example, 10 seconds or more, and for example, 120 seconds or less.
[0111] As a result, the adhesive layer 2, which is a dried product of the aqueous dispersion, is disposed on one surface of the first substrate 1 in the thickness direction.
[0112] In this way, the laminate 10 is manufactured.
[0113] The laminate 10 includes the adhesive layer 2, which is a dried product of the aqueous dispersion, and therefore has excellent productivity.
[0114] Next, a method for bonding substrates together (first substrate 1 and second substrate 3 together) using laminate 10 will be described in detail.
[0115] In this method, as shown in FIG. 2C, the second substrate 3 is placed on one surface in the thickness direction of the adhesive layer 2, and the first substrate 1 and the second substrate 3 are bonded together by thermocompression bonding (heat sealing).
[0116] There are no particular limitations on the second substrate 3. As the second substrate 3, a substrate similar to the first substrate 1 described above is selected.
[0117] The first substrate 1 and the second substrate 3 may be the same or different from each other. Preferably, the first substrate 1 and the second substrate 3 are the same, and more preferably, both are metal films (e.g., aluminum films).
[0118] As conditions for thermocompression bonding, the temperature for thermocompression bonding is, for example, 80° C. or more, preferably 100° C. or more, and for example, 190° C. or less, preferably 170° C. or less. The pressure for thermocompression bonding is 1.5 kg / cm. 3 3.5kg / cm or more 3The following is the result.
[0119] This bonds the first substrate 1 and the second substrate 3 together, producing a laminate 10 having the first substrate 1, the adhesive layer 2, and the second substrate 3 in that order toward one side in the thickness direction.
[0120] In the above description, in the laminate 10, the adhesive layer 2 is disposed on one thickness-wise surface of the first substrate 1, but the adhesive layer 2 may be disposed on one thickness-wise surface and the other thickness-wise surface of the first substrate 1. In such a case, the second substrate 3 can be disposed on one thickness-wise surface and the other thickness-wise surface of the adhesive layer 2.
[0121] In the above description, the adhesive layer 2 is placed on the first substrate 1, and the first substrate 1 and the second substrate 3 are bonded together via the adhesive layer 2. However, as shown in FIG. 3A, the adhesive layer 2 can be placed on each of the first substrate 1 and the second substrate 3, and then the first substrate 1 and the second substrate 3 can be bonded together via the adhesive layer 2 as shown in FIG. 3B.
[0122] Furthermore, an adhesive layer 2 is disposed on the first substrate 1 to produce a laminate 10. The laminate 10 can then be folded so that the adhesive layers 2 face each other, and the first substrates 1 can be bonded together. This allows a bag to be produced. The laminate 10 used to produce a bag is a bag material.
[0123] <Effects> In the aqueous dispersion, the ethylene-unsaturated carboxylic acid copolymer includes a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer, each of which has a different carboxyl group content. The difference (C-B) between the carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer, and the difference (B-A) between the carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer and the carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer are within a predetermined range. Therefore, the storage stability is excellent.
[0124] More specifically, it is presumed that the reason is as follows: That is, when the ethylene-unsaturated carboxylic acid copolymer contains a first ethylene-unsaturated carboxylic acid copolymer having a relatively low carboxyl group content, a second ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content, and a third ethylene-unsaturated carboxylic acid copolymer having a relatively high carboxyl group content, the aqueous dispersion forms a sea-island structure separated into three phases, namely, a first phase 11, a second phase 12, and a third phase 13, as shown in Fig. 4 .
[0125] The first phase 11 is a dispersed phase dispersed within the second phase 12 and is composed of an ethylene-unsaturated carboxylic acid copolymer having a relatively low carboxyl group content (i.e., a first ethylene-unsaturated carboxylic acid copolymer).
[0126] The second phase 12 is a dispersed phase dispersed within the third phase 13, and is made of an ethylene-unsaturated carboxylic acid copolymer (i.e., a second ethylene-unsaturated carboxylic acid copolymer) having a relatively medium carboxyl group content.
[0127] The third phase 13 is made of an ethylene-unsaturated carboxylic acid copolymer having a relatively high carboxyl group content (ie, a third ethylene-unsaturated carboxylic acid copolymer).
[0128] On the other hand, the aqueous dispersion 2 of Patent Document 1 contains water, a resin A (ethylene-acrylic acid copolymer (acrylic acid content: 20.5% by mass)), a resin B (ethylene-methacrylic acid copolymer (methacrylic acid content: 15% by mass)), and a resin C (ethylene-methacrylic acid copolymer (methacrylic acid content: 10% by mass)).
[0129] In such a case, since resin A has a relatively high carboxyl group content, resin A forms the third phase 13. Since resin B has a relatively medium carboxyl group content, resin B forms the second phase 12. Furthermore, since resin C has a relatively low carboxyl group content, resin C forms the first phase 11.
[0130] On the other hand, in the aqueous dispersion 2 of Patent Document 1, the difference (resin A - resin B) between resin A having a relatively high carboxyl group content and resin B having a relatively medium carboxyl group content is large.
[0131] Therefore, the compatibility between resin A and resin B decreases, resin B particles tend to gather together, and the second phase 12 becomes larger. As a result, uniform particles cannot be formed, and storage stability decreases.
[0132] In contrast to this, the above-mentioned aqueous dispersion is adjusted so that the difference in carboxyl group content ((C−B) and (B−A)) is small.
[0133] This improves the compatibility of the third ethylene-unsaturated carboxylic acid copolymer having a relatively high carboxyl group content with the first ethylene-unsaturated carboxylic acid copolymer having a relatively low carboxyl group content and the second ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content, and allows the resins B and C to be uniformly dispersed, thereby reducing the size of the first phase 11 and the second phase 12. As a result, uniform particles can be formed, and storage stability can be improved.
[0134] The laminate 10 includes the adhesive layer 2, which is a dried product of the aqueous dispersion, and therefore has excellent productivity.
[0135] <Modifications> In the modification, the same components and steps as those in the first embodiment are denoted by the same reference numerals, and detailed descriptions thereof will be omitted. Furthermore, the modification can achieve the same effects as those in the first embodiment unless otherwise specified. Furthermore, the first embodiment and its modification can be combined as appropriate.
[0136] In the above description, the ethylene-unsaturated carboxylic acid copolymer includes three ethylene-unsaturated carboxylic acid copolymers (a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer), but is not limited thereto, and the ethylene-unsaturated carboxylic acid copolymer may also include four or more ethylene-unsaturated carboxylic acid copolymers.
[0137] That is, in three of the four or more ethylene-unsaturated carboxylic acid copolymers, the number of ethylene-unsaturated carboxylic acid copolymers is not limited as long as the difference between the carboxyl group content of the ethylene-unsaturated carboxylic acid copolymer having a relatively high carboxyl group content and the carboxyl group content of the ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content, and the difference between the carboxyl group content of the ethylene-unsaturated carboxylic acid copolymer having a relatively medium carboxyl group content and the carboxyl group content of the ethylene-unsaturated carboxylic acid copolymer having a relatively low carboxyl group content, are adjusted to fall within predetermined ranges.
[0138] Preferably, the ethylene-unsaturated carboxylic acid copolymer comprises three ethylene-unsaturated carboxylic acid copolymers (a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer).
[0139] Specific numerical values of the blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "not more than" or "less than") or lower limit values (numerical values defined as "not less than" or "exceeding") of the corresponding blending ratios (content ratios), physical property values, parameters, etc. described in the above "Modes for Carrying Out the Invention." Furthermore, unless otherwise specified in the following description, "parts" and "%" are based on mass.
[0140] <Details of Components> Details of the abbreviations used in each example and each comparative example are described below. Resin 1: ethylene-methacrylic acid copolymer, methacrylic acid content 9% by mass, carboxyl group content 1.05 mmol / kg Resin 2: ethylene-methacrylic acid copolymer, methacrylic acid content 10% by mass, carboxyl group content 1.16 mmol / kg Resin 3: ethylene-methacrylic acid copolymer, methacrylic acid content 15% by mass, carboxyl group content 1.74 mmol / kg Resin 4: ethylene-acrylic acid copolymer, acrylic acid content 15% by mass, carboxyl group content 2.08 mmol / kg Resin 5: ethylene-acrylic acid copolymer, acrylic acid content 18% by mass, carboxyl group content 2.50 mmol / kg
[0141] Examples 1 to 7 <Production of aqueous dispersion> After melt-kneading the components according to the formulations shown in Table 1, 3.5 parts by mass of potassium hydroxide and 165 parts by mass of deionized water were added to a reaction vessel and stirred. The mixture was then heated to 150°C and maintained for 4 hours, and then cooled to room temperature to obtain an aqueous dispersion (solid concentration: 38% by mass).
[0142] <Evaluation> [Viscosity] The viscosity of the aqueous dispersions of each Example and Comparative Example was measured at 25° C. using a B-type viscometer (manufactured by Toki Sangyo Co., Ltd.) The results are shown in Table 1.
[0143] [Degree of Neutralization] The ethylene-unsaturated carboxylic acid copolymers of each Example and Comparative Example were measured for infrared absorption spectrum, and the neutralization was carried out at 1700 cm corresponding to the carboxy group. -1 The peak height a of the absorption was determined. The peak height a corresponds to the number of carboxyl groups in the resin that are not ionically bonded.
[0144] Next, the ethylene-unsaturated carboxylic acid copolymer was brought into contact with hydrochloric acid to remove metal ions in the ethylene-unsaturated carboxylic acid copolymer (demetallation), thereby obtaining an acid copolymer having ionic bonds (intramolecular crosslinks). The infrared absorption spectrum of this acid copolymer was measured, and it was found to have a peak at 1700 cm -1The peak height b of the absorption of the acid copolymer was determined. The peak height b corresponds to the number of all carboxyl groups in the acid copolymer. The degree of neutralization [%] was calculated from the obtained peak height a and the following formula (2). The results are shown in Table 1. Degree of neutralization [%] = 100 × (1 - a / b) (1)
[0145] [Heat sealability] The heat sealability of the aqueous dispersion of each example was evaluated.
[0146] Specifically, the laminate was produced according to the following procedure.
[0147] In the first step, an aluminum foil was prepared as a first substrate.
[0148] In the second step, an adhesive layer was disposed on one surface of the first substrate in the thickness direction. Specifically, the aqueous dispersion of each example was applied to one surface of the first substrate in the thickness direction in an amount of 3 g / m. 2 The adhesive was applied with a wire bar so that the thickness became 100 μm, and then dried at 180° C. for 10 seconds. As a result, an adhesive layer was disposed on one surface of the first substrate in the thickness direction.
[0149] In the third step, an aluminum foil as a second substrate was placed on one surface of the adhesive layer in the thickness direction, and the resulting laminate was subjected to thermocompression bonding (heat sealing) at 10° C. and a pressure of 2 kg / cm for 0.5 seconds, thereby producing a laminate.
[0150] In the obtained laminate, adhesion between the first substrate and the second substrate was confirmed, which indicates that the aqueous dispersions of the examples have good heat sealability.
[0151] [Storage Stability] 100 g of the aqueous dispersion of each Example and Comparative Example was placed in a 100 mL polyethylene bottle and stored at 40°C for 3 months. Thereafter, the presence or absence of emulsion separation (upper layer: emulsion containing resin, lower layer: aqueous layer) was visually confirmed. The separation rate was calculated based on the following formula (3): Separation rate (%) = length of separated lower layer (aqueous layer) [mm] / total length of emulsion [mm] × 100 (2)
[0152] Storage stability was evaluated based on the following criteria. The results are shown in Table 1. {Criteria} 5: Separation rate was less than 3%. 4: Separation rate was 3% or more and less than 10%. 3: Separation rate was 10% or more and less than 15%. 2: Separation rate was 15% or more and less than 30%. 1: Separation rate was 30% or more.
[0153]
[0154] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.
[0155] The aqueous dispersion and laminate of the present invention can be used, for example, in the production of packaging materials.
[0156] 1 substrate 2 adhesive layer 10 laminate
Claims
1. An aqueous dispersion comprising a resin component and water, wherein the resin component comprises an ethylene-unsaturated carboxylic acid copolymer, the ethylene-unsaturated carboxylic acid copolymer comprises a first ethylene-unsaturated carboxylic acid copolymer, a second ethylene-unsaturated carboxylic acid copolymer, and a third ethylene-unsaturated carboxylic acid copolymer, each of which has a different carboxyl group content, wherein a difference (C-B) between a carboxyl group content C of the third ethylene-unsaturated carboxylic acid copolymer and a carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg and is 0.50 mmol / kg or less, and a difference (B-A) between a carboxyl group content B of the second ethylene-unsaturated carboxylic acid copolymer and a carboxyl group content A of the first ethylene-unsaturated carboxylic acid copolymer exceeds 0 mmol / kg and is 0.80 mmol / kg or less.
2. The aqueous dispersion according to claim 1, wherein the first ethylene-unsaturated carboxylic acid copolymer has a carboxyl group content A of 1.00 mmol / kg or more and less than 1.40 mmol / kg, the second ethylene-unsaturated carboxylic acid copolymer has a carboxyl group content B of 1.40 mmol / kg or more and less than 1.80 mmol / kg, and the third ethylene-unsaturated carboxylic acid copolymer has a carboxyl group content C of 1.80 mmol / kg or more and less than 2.30 mmol / kg.
3. The aqueous dispersion according to claim 1 or 2, wherein the content of the first ethylene-unsaturated carboxylic acid copolymer is 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer; the content of the second ethylene-unsaturated carboxylic acid copolymer is 5 parts by mass or more and 20 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer; and the content of the third ethylene-unsaturated carboxylic acid copolymer is 30 parts by mass or more and 50 parts by mass or less, relative to 100 parts by mass of the total amount of the first ethylene-unsaturated carboxylic acid copolymer, the second ethylene-unsaturated carboxylic acid copolymer, and the third ethylene-unsaturated carboxylic acid copolymer.
4. The aqueous dispersion according to claim 1 or 2, wherein the content of the third ethylene-unsaturated carboxylic acid copolymer is greater than or equal to the content of the first ethylene-unsaturated carboxylic acid copolymer, and the content of the first ethylene-unsaturated carboxylic acid copolymer is greater than the content of the second ethylene-unsaturated carboxylic acid copolymer.
5. The aqueous dispersion according to claim 1 or 2, wherein the first ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid, the second ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and methacrylic acid, and the third ethylene-unsaturated carboxylic acid copolymer is a copolymer of ethylene and acrylic acid.
6. A laminate comprising a substrate and an adhesive layer in that order toward one side in the thickness direction, the adhesive layer being a dried product of the aqueous dispersion according to claim 1 or 2.
Citation Information
Patent Citations
Preparing aqueous dispersion
JP1980098242A
Aqueous copolymer dispersion, preparation thereof, and coating film formed therefrom
JP1991210349A
Ethylenic resin aqueous dispersion and ethylenic resin coating film obtained from the aqueous dispersion
JP2000007860A
Aqueous dispersion composition
JP2010043186A
Transparent elastomer nanocomposite blends
JP2021533226A