Adhesive and article using same
A water-based adhesive with cellulose fibers and a water-dispersible resin absorbs water to swell and peel off, addressing the lack of effective water absorption and recyclability in current adhesives, while maintaining adhesiveness and suitable for various materials.
Patent Information
- Application Number
- PCT/JP2024/010704
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
Current adhesives do not effectively absorb water and peel off after adhesion, limiting their recyclability despite advancements in adhesives with cellulose fibers for releasability.
A water-based adhesive comprising a water-dispersible resin and cellulose fibers, where the cellulose fibers swell upon water absorption, enabling easy peeling, with preferred ratios and types of cellulose nanofibers and anionic groups for enhanced releasability.
The adhesive maintains adhesiveness while allowing for easy removal after water absorption, improving recyclability by swelling cellulose fibers, which absorb water to facilitate peeling, and can be used as a primer for various materials.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Adhesives and articles using them
[0001] The present invention relates to an adhesive used in applications where adhesion is followed by water absorption and subsequent delamination, and to an article using the adhesive.
[0002] In recent years, there has been a demand for adhesives that are easily peelable from the perspective of recycling, etc. For example, Patent Document 1 discloses the use of an aqueous dispersion of cellulose nanofibers as an easily peelable adhesive composition that has high adhesive strength and does not require special treatment for peeling.
[0003] Patent Document 2 discloses a pressure-sensitive adhesive composition having excellent adhesion and removability, which is obtained by blending modified cellulose fibers with a matrix resin such as an acrylic pressure-sensitive adhesive.
[0004] Patent Document 3 discloses an adhesive composition having a high ratio of shear strength to peel strength, which contains cellulose nanofibers and a resin such as an acrylic resin, a urethane resin, or an epoxy resin.
[0005] JP 2017-025130 A JP 2020-076075 A JP 2020-152829 A
[0006] The above Patent Documents 1 to 3 disclose adhesives containing cellulose fibers as peelable adhesives, but do not describe their use in applications where they are peeled off by absorbing water after adhesion.
[0007] An object of an embodiment of the present invention is to provide an adhesive that can be used in applications where adhesion is followed by water absorption and subsequent debonding.
[0008] The present invention includes the following embodiments. [1] An adhesive used in applications where water absorption occurs after adhesion and then peeling occurs, the adhesive comprising (A) an aqueous resin and (B) cellulose fibers, the cellulose fibers comprising 0.1 to 10 parts by mass per 100 parts by mass of the aqueous resin. [2] The adhesive according to [1], wherein the aqueous resin comprises a water-dispersible resin. [3] The adhesive according to [2], wherein the water-dispersible resin comprises an anionic water-dispersible resin and / or a nonionic water-dispersible resin. [4] The adhesive according to any one of [1] to [3], wherein the cellulose fibers comprise cellulose nanofibers. [5] The adhesive according to any one of [1] to [4], wherein the cellulose fibers have anionic groups. [6] The adhesive according to any one of [1] to [5], wherein the adhesive is a primer. [7] An article comprising a first member, a second member, and an adhesive layer formed from the adhesive according to any one of [1] to [6], which bonds the first member and the second member.
[0009] In the case of the adhesive according to the embodiment of the present invention, the cellulose fibers swell when they are allowed to absorb water after bonding, and therefore can be easily peeled off.
[0010] The adhesive according to the embodiment is a blend of (A) an aqueous resin and (B) cellulose fibers.
[0011] [(A) Water-based Resin] The water-based resin is a component (adhesive component) that exhibits adhesive properties in the adhesive. Therefore, the adhesive according to the embodiment can be said to be a mixture of a water-based adhesive containing a water-based resin and cellulose fibers or an aqueous dispersion thereof. By blending cellulose fibers, it is possible to impart releasability by swelling of the cellulose fibers upon water absorption while maintaining the adhesive properties of the water-based resin.
[0012] The aqueous resin refers to a resin that disperses or dissolves in water, and examples thereof include water-dispersible resins and water-soluble resins. As the aqueous resin, either a water-dispersible resin or a water-soluble resin may be used, or both may be used in combination. Preferably, a water-dispersible resin is used. That is, in one embodiment, the aqueous resin contains a water-dispersible resin. In this case, the aqueous resin preferably contains a water-dispersible resin as a main component, and the amount of the water-dispersible resin in 100% by mass of the aqueous resin is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may even be 100% by mass.
[0013] The water-dispersible resin refers to a resin that forms an emulsion or suspension by emulsifying or dispersing in water as a dispersion medium. Therefore, the water-dispersible resin may be a resin contained in an emulsion in which the dispersoid resin is a liquid (i.e., a water-based emulsion resin), or a resin contained in a suspension in which the dispersoid resin is a solid (i.e., a water-based suspension resin).
[0014] The water-dispersible resin is preferably an aqueous emulsion resin. The aqueous emulsion may be a forced emulsification type or a self-emulsification type. The forced emulsification type refers to a resin that is forcedly emulsified with a surfactant. The self-emulsification type refers to a resin that is made self-dispersible by adding a hydrophilic group or hydrophilic segment to the molecule.
[0015] Examples of water-dispersible resins include water-dispersible urethane resins, water-dispersible acrylic resins, water-dispersible vinyl acetate resins, water-dispersible polyester resins, water-dispersible polyepoxy resins, water-dispersible polystyrene resins, etc. These may be used alone or in combination of two or more.
[0016] The water-dispersible urethane resin is obtained by reacting a polyol with a polyisocyanate, and a known urethane emulsion can be used, for example. Examples of the polyol include at least one selected from the group consisting of polyester polyols, polyether polyols, polycarbonate polyols, and polybutadiene polyols. In addition to or in place of these polyols, low-molecular-weight polyols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propanediol, dipropylene glycol, tripropylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, glycerin, trimethylolpropane, ditrimethylolpropane, pentaerythritol, and bisphenol A can also be used.
[0017] Examples of polyisocyanates include aliphatic polyisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate, alicyclic diisocyanates such as hydrogenated diphenylmethane diisocyanate (hydrogenated MDI), isophorone diisocyanate, and methylcyclohexylene diisocyanate, aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate, and xylylene diisocyanate, as well as modified products and polynuclear products thereof. These may be used alone or in combination of two or more types.
[0018] The water-dispersible acrylic resin is a resin obtained using (meth)acrylic acid and / or a (meth)acrylic acid ester as a monomer, and may be a copolymer using these monomers together with other monomers such as ethylene, styrene, etc. For example, a known acrylic emulsion can be used. Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and (meth)acrylic acid aryl esters such as benzyl (meth)acrylate.
[0019] The water-dispersible vinyl acetate resin is a resin obtained using vinyl acetate as a monomer, and may be a copolymer of vinyl acetate and other monomers. For example, a known vinyl acetate emulsion can be used.
[0020] The water-dispersible polyester resin is a polycondensate obtained by dehydration condensation of a polycarboxylic acid and a polyol to form an ester bond, and a known polyester emulsion can be used as an example.
[0021] The water-dispersible polyepoxy resin and water-dispersible polystyrene resin are also not particularly limited, and known polyepoxy emulsions and polystyrene emulsions can be used, for example.
[0022] The water-dispersible resin may be anionic, nonionic, or cationic, or a combination thereof. In one embodiment, the water-dispersible resin contains an anionic water-dispersible resin and / or a nonionic water-dispersible resin. In this case, the water-dispersible resin preferably contains an anionic water-dispersible resin and / or a nonionic water-dispersible resin as a main component, and the amount of the anionic water-dispersible resin and / or the nonionic water-dispersible resin in 100% by mass of the water-dispersible resin is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass.
[0023] Examples of anionic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which anionic groups such as carboxyl groups or sulfonic acid groups have been introduced into the resin. Examples of nonionic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which nonionic hydrophilic groups or hydrophilic segments such as polyethylene glycol have been introduced into the resin. Examples of cationic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which cationic groups such as quaternary ammonium salt groups have been introduced into the resin.
[0024] [(B) Cellulose Fibers] As the cellulose fibers, cellulose fibers having a number average fiber diameter of more than 500 nm on the order of μm may be used, or cellulose nanofibers having a number average fiber diameter of 500 nm or less may be used, or both may be used in combination.
[0025] From the viewpoint of not impairing initial adhesiveness, it is preferable to use cellulose nanofibers as the cellulose fibers. Furthermore, from the viewpoint of increasing the degree of swelling when water is absorbed after adhesion, thereby enhancing the effect of improving releasability, it is preferable to use cellulose nanofibers as the cellulose fibers. That is, in one embodiment, the cellulose fibers contain cellulose nanofibers. In this case, it is preferable that the cellulose fibers contain cellulose nanofibers as a main component, and the amount of cellulose nanofibers in 100% by mass of cellulose fibers is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass.
[0026] The number average fiber diameter of the cellulose nanofibers is preferably 1 to 500 nm, more preferably 1.5 to 200 nm, even more preferably 2 to 100 nm, even more preferably 2.5 to 50 nm, and even more preferably 3 to 20 nm.
[0027] The average aspect ratio of the cellulose nanofibers is not particularly limited, but is preferably 10 to 1,000, more preferably 50 to 700, even more preferably 100 to 500, and even more preferably 200 to 400.
[0028] The number-average fiber diameter and average aspect ratio of cellulose nanofibers can be determined by observation using an atomic force microscope (AFM). For example, after casting an aqueous dispersion of cellulose nanofibers on a mica substrate, 10 AFM images are taken using an atomic force microscope (AFM, manufactured by Hitachi High-Tech Corporation), and 25 cellulose nanofibers are selected from the images and their fiber diameters and lengths are measured. From the obtained fiber diameter and fiber length data, the arithmetic means are calculated to determine the number-average fiber diameter [nm] and number-average fiber length [nm], and the average aspect ratio is calculated according to the following formula: Average aspect ratio = Number-average fiber length [nm] / Number-average fiber diameter [nm]
[0029] The cellulose nanofibers preferably have a cellulose type I crystal structure. The cellulose type I crystal structure is the crystalline form of natural cellulose, and the cellulose fiber (B) is water-insoluble and can maintain its fibrous form in water. The presence of a cellulose type I crystal structure can be identified by the presence of typical peaks at two positions, near 2θ = 14° to 17° and near 2θ = 22° to 23°, in a diffraction profile obtained by wide-angle X-ray diffraction image measurement.
[0030] The cellulose fibers (preferably cellulose nanofibers) may be unmodified cellulose fibers that do not have anionic groups introduced therein, but it is preferable to use cellulose fibers that have anionic groups. That is, in one embodiment, it is preferable that the cellulose fibers have anionic groups, and more preferably, cellulose nanofibers that have anionic groups are used as the cellulose fibers. The presence of anionic groups can increase the degree of swelling when the cellulose fibers absorb water after adhesion, thereby enhancing the effect of improving releasability.
[0031] Examples of anionic groups include at least one selected from the group consisting of a carboxyl group, a phosphate group, a sulfonate group, a nitrate group, a borate group, and a sulfate group. These anionic groups may be directly or indirectly bonded to glucose units, which are structural units of cellulose molecules. When indirectly bonded, an alkylene group having 1 to 4 carbon atoms may be present between the glucose unit and the anionic group. One or more anionic groups may be bonded to all glucose units constituting the cellulose molecule, or one or more anionic groups may be bonded to a portion of the glucose units constituting the cellulose molecule.
[0032] The carboxyl group as the anionic group conceptually includes not only the acid form (-COOH) but also the salt form, i.e., carboxylate group (-COOX, where X is a cation that forms a salt with a carboxylic acid), and the acid form and the salt form may be mixed. Similarly, the phosphate group, sulfonate group, nitrate group, borate group, and sulfate group conceptually include not only the acid form but also the salt form, and the acid form and the salt form may be mixed. The salt is not particularly limited, and examples thereof include alkali metal salts such as sodium salts and potassium salts, alkaline earth metal salts such as magnesium salts and calcium salts, onium salts such as ammonium salts and phosphonium salts, and amine salts such as primary amines, secondary amines, and tertiary amines.
[0033] When the cellulose fibers have anionic groups, the amount of the anionic groups is not particularly limited and may be, for example, 0.5 to 4.0 mmol / g or 1.0 to 3.0 mmol / g per dry mass of the cellulose fibers. For example, in the case of carboxy groups, the amount of anionic groups can be determined by preparing 60 mL of a cellulose fiber-containing slurry adjusted to a concentration of 0.1 to 1% by mass, adjusting the pH to approximately 2.5 with a 0.1 mol / L aqueous hydrochloric acid solution, adding a 0.05 mol / L aqueous sodium hydroxide solution dropwise, measuring the electrical conductivity, and continuing until the pH reaches approximately 11. The amount of sodium hydroxide (V) consumed during the neutralization stage of the weak acid, where the electrical conductivity changes slowly, can be calculated according to the following formula. Phosphate groups can also be measured by similar electrical conductivity measurements. Other anionic groups can also be measured using known methods. In this specification, the term "dry mass" refers to the mass after drying at 140°C until the mass change rate per minute is 0.05% or less. Amount of anionic group (mmol / g) = V (mL) × [0.05 / mass of cellulose fiber (g)]
[0034] In one embodiment, examples of cellulose nanofibers having carboxy groups as anionic groups include oxidized cellulose nanofibers obtained by oxidizing the hydroxyl groups of glucose units in cellulose molecules, and carboxymethylated cellulose nanofibers obtained by carboxymethylating the hydroxyl groups of glucose units in cellulose molecules.
[0035] Oxidized cellulose nanofibers include those in which the hydroxyl group at the C6 position of the glucose unit in the cellulose molecule has been selectively oxidized to a carboxyl group. Oxidized cellulose nanofibers are obtained by oxidizing natural cellulose, such as wood pulp, using a co-oxidant in the presence of an N-oxyl compound and then defibrating (refining) it. The N-oxyl compound used is a compound containing a nitroxy radical, which is commonly used as an oxidation catalyst. For example, a piperidine nitroxyoxy radical is used. 2,2,6,6-tetramethylpiperidinoxy radical (TEMPO) or 4-acetamido-TEMPO is particularly preferred. Cellulose fibers oxidized and refined with TEMPO are generally referred to as TEMPO-oxidized cellulose nanofibers (TOCN). The oxidized cellulose nanofibers may also contain aldehyde or ketone groups in addition to carboxyl groups.
[0036] When cellulose fibers are defibrated to obtain cellulose nanofibers, the defibration treatment may be carried out after or before the introduction of anionic groups. The defibration treatment can be carried out by treating an aqueous dispersion of cellulose fibers using, for example, a homomixer, a high-pressure homogenizer, an ultrasonic dispersion processor, a beater, a disk refiner, a conical refiner, a double-disc refiner, a grinder, or the like under high-speed rotation, to obtain an aqueous dispersion of cellulose nanofibers.
[0037] [Adhesive] The adhesive according to the embodiment is an aqueous adhesive containing the aqueous resin and cellulose fibers. Therefore, the adhesive is a liquid adhesive containing water as well as the aqueous resin and cellulose fibers. The cellulose fibers are water-insoluble and dispersed in water, which is a dispersion medium. When the aqueous resin is a water-dispersible resin, the aqueous resin is dispersed in water, which is a dispersion medium. Therefore, in this case, the adhesive is an aqueous dispersion containing the water-dispersible resin and cellulose fibers dispersed in water, which is a dispersion medium.
[0038] The aqueous dispersion contains water as a dispersion medium, but the dispersion medium may be water alone, or may contain water together with a water-soluble organic solvent such as ethanol or isopropyl alcohol, as long as the effect is not impaired. When an organic solvent is contained, the amount of water in 100% by mass of the dispersion medium is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 100% by mass. In addition, the dispersion medium may be an aqueous solution containing an acid, an alkali, or a salt thereof, as long as the effect is not impaired.
[0039] In the adhesive, the amount of cellulose fiber per 100 parts by mass of aqueous resin is 0.1 to 10 parts by mass. By having the amount of cellulose fiber at 0.1 parts by mass or more, the degree of swelling when water is absorbed after adhesion can be increased, thereby improving releasability. Furthermore, by having the amount of cellulose fiber at 10 parts by mass or less, the adhesive has good coatability. The amount of cellulose fiber per 100 parts by mass of aqueous resin is more preferably 0.2 to 9 parts by mass, even more preferably 0.3 to 6 parts by mass, even more preferably 0.5 to 5 parts by mass, and even more preferably 0.6 to 3 parts by mass.
[0040] In the adhesive, the content (concentration) of the aqueous resin is not particularly limited and may be, for example, 1 to 70% by mass or 5 to 50% by mass. The content (concentration) of the cellulose fiber is also not particularly limited and may be, for example, 0.001 to 7% by mass or 0.005 to 5% by mass.
[0041] In addition to the aqueous resin, cellulose fiber, and water described above, the adhesive according to the embodiment may contain additives such as colorants, fillers, preservatives, antifoaming agents, film-forming aids, antiblocking agents, flow improvers, viscosity modifiers, adhesion promoters, conductive agents, antioxidants, light stabilizers, and ultraviolet absorbers.
[0042] In the adhesive according to the embodiment, after the adhesive is used to bond the adherend, the cellulose fibers contained in the adhesive layer are allowed to absorb water in a dry state, causing the adhesive layer to swell. This makes it easier for the adherend to peel at the interface with the adhesive layer, allowing for easier peeling. Water absorption into the adhesive layer (i.e., water uptake into the adhesive layer) can be achieved by treating the adhesive layer with water, such as by immersing the part containing the adhesive layer in water or spraying water on it.
[0043] In one embodiment, the adhesive can be used as a primer (i.e., an undercoat adhesive). Specifically, the adhesive is applied as a primer to a substrate, and a topcoat is applied thereon to form a coating film (one or more coating films including an intermediate coating). When recycling a substrate from a product thus obtained, the adhesive layer formed as a primer can be treated with water as described above to absorb water, thereby easily peeling the coating film including the adhesive layer from the substrate. When the coating film is peeled off after absorbing water, the adhesive layer may peel off together with the coating film, or the adhesive layer may remain on the substrate side. Even if the adhesive layer remains on the substrate side, the remaining adhesive layer can be peeled off and removed by further treating the coating film with water to absorb water, allowing the substrate to be recycled. Furthermore, if the adhesive layer remains on the coating film, the remaining adhesive layer on the coating film may be further treated with water to peel off and remove the adhesive layer from the coating film, thereby recycling the coating film.
[0044] The substrate is not particularly limited, and examples thereof include inorganic substrates such as glass plates and concrete, as well as organic substrates such as synthetic resin substrates such as films, sheets, and plates made of synthetic resins such as polyester (PET, PEN, etc.), polyvinylidene chloride, polyvinyl chloride, polyethylene, polypropylene, polycarbonate, polystyrene, polyacrylate, and polyolefin, and wood substrates.
[0045] The method for applying the adhesive is not particularly limited, and the adhesive can be applied by, for example, a knife coater, a roll coater, a spray, or the like.
[0046] The thickness of the adhesive layer is not particularly limited, and may be, for example, 0.1 to 500 μm, or 0.5 to 100 μm.
[0047] An article according to one embodiment includes an adhesive layer formed from the adhesive. That is, the article includes a first member and a second member as adherends, and an adhesive layer that bonds the first member and the second member, the adhesive layer being formed from the adhesive. The adhesive layer is formed by applying and drying the adhesive, and therefore is formed from the non-volatile component of the adhesive.
[0048] The first and second members as the adherends are materials that form part of an article, and their shapes are not particularly limited. For example, one of the first and second members may be a substrate for the primer application, and the other may be a coating film formed by a topcoat paint. The substrates may be bonded to each other with the adhesive.
[0049] Examples will be described in detail below along with comparative examples, but the present invention is not limited to these examples.
[0050] Details of the components used in the examples and comparative examples are as follows.
[0051] [Water-based resin] Water-based resin 1: "Superflex 460" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / carbonate-based, non-volatile content 38% by mass)
[0052] Water-based resin 2: "Superflex 150" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / ester-ether type, non-volatile content 30% by mass)
[0053] Water-based resin 3: "Superflex 210" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / ester-based, non-volatile content 35% by mass)
[0054] Water-based resin 4: "Superflex 500M" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (nonionic urethane emulsion / ester-based, nonvolatile content 45% by mass)
[0055] Water-based resin 5: "Superflex 620" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (cationic urethane emulsion / ester type, non-volatile content 30% by mass)
[0056] Water-based resin 6: "Movinyl 730L" manufactured by Japan Coating Resins Co., Ltd. (nonionic acrylic emulsion, nonvolatile content 46% by mass)
[0057] Water-based resin 7: "Movinyl 51" manufactured by Japan Coating Resins Co., Ltd. (nonionic vinyl acetate emulsion, nonvolatile content 50% by mass)
[0058] Water-based resin 8: "Pluscoat RZ-105" (anionic polyester emulsion, non-volatile content 25% by mass) manufactured by GOO Chemical Industry Co., Ltd.
[0059] [Cellulose Fibers] Cellulose Fiber 1: TEMPO-oxidized cellulose nanofibers obtained by Production Example 1 below, with a number-average fiber diameter of 3 nm, an average aspect ratio of 300, and a carboxyl group content of 2.0 mmol / g. [Production Example 1] 2 g of softwood pulp was mixed with 150 mL of water, 0.25 g of sodium bromide, and 0.025 g of TEMPO, thoroughly stirred to disperse the mixture. A 13% by mass aqueous solution of sodium hypochlorite (co-oxidant) was then added to 1.0 g of the pulp to achieve a sodium hypochlorite content of 5.2 mmol / g, initiating the reaction. As the reaction progressed, the pH decreased. While maintaining the pH at 10-11, 0.5 N aqueous sodium hydroxide was added dropwise, and the reaction was continued until no further change in pH was observed (reaction time: 120 minutes). After completion of the reaction, the pH was adjusted to 2 by adding 0.1 N hydrochloric acid, and the mixture was purified by repeated filtration and water washing to obtain surface-oxidized cellulose fibers. This was diluted with pure water to a cellulose fiber concentration of 2% by mass, and 10% by mass of sodium hydroxide was added to adjust the pH to 7. This was treated once at a pressure of 100 MPa using a high-pressure homogenizer (H11, manufactured by Sanwa Engineering Co., Ltd.) to prepare Cellulose Fiber 1.
[0060] Cellulose fiber 2: TEMPO-oxidized cellulose nanofibers having a number-average fiber diameter of 3 nm, an average aspect ratio of 300, and a carboxyl group amount of 2.0 mmol / g, obtained by the following Production Example 2. [Production Example 2] Cellulose fiber 2 was obtained by the same production method as in Production Example 1, except that tetrabutylammonium hydroxide was used instead of sodium hydroxide in the neutralization step.
[0061] Cellulose fiber 3: Phosphorylated cellulose nanofibers obtained by Production Example 3 below, having a number-average fiber diameter of 3 nm, an average aspect ratio of 200, and a phosphate group content of 2.5 mmol / g. [Production Example 3] This was prepared by the method described in Production Example 1 of JP 2020-100845 A. Specifically, 100 g of urea, 55.3 g of sodium dihydrogen phosphate dihydrate, and 41.3 g of disodium hydrogen phosphate were dissolved in 110 g of water. 100 g of bleached softwood kraft pulp was then added and reacted at 140°C for 2 hours. The fibers were then removed and washed with water, and the pH was adjusted to 12-13 by adding a 2N aqueous sodium hydroxide solution as a neutralizer. The fibers were then washed again with water. After dehydration, the fibers were diluted with water to a cellulose fiber concentration of 2.0% by mass. Subsequently, a microfluidizer treatment (150 MPa, 10 passes) was performed as a micronization process to obtain cellulose fiber 3.
[0062] Cellulose fiber 4: Unmodified cellulose nanofibers with a number-average fiber diameter of 35 nm and an average aspect ratio of 250, obtained by Production Example 4 below. [Production Example 4] 50.0 g of softwood pulp was dispersed in 950.0 g of water, pulverized in a household mixer, defibrated in a stone mill, and further water was added to obtain an aqueous dispersion with a cellulose fiber concentration of 2% by mass. The obtained 2% by mass aqueous dispersion was treated with a microfluidizer (150 MPa, 1 pass), to obtain Cellulose fiber 4.
[0063] [Preparation of adhesives] Adhesives for Examples 1 to 14 and Comparative Examples 1 to 3 were prepared by mixing aqueous resin emulsions (aqueous resins 1 to 8) and aqueous cellulose fiber dispersions (cellulose fibers 1 to 4) according to the formulations shown in Table 1 below. The formulations in Table 1 are the mass ratios of the aqueous resin to the nonvolatile content of the cellulose fiber, with the resin nonvolatile content being 100 parts by mass. Each adhesive was prepared by diluting with water so that the resin nonvolatile content concentration was 10% by mass (5% by mass in Comparative Example 1).
[0064] The resulting adhesive was evaluated for water absorption (mass), water absorption (thickness), adhesion (before water absorption), and peelability (after water absorption) using the following evaluation methods.
[0065] [Water absorption rate (mass)] The above adhesive was applied to release paper and dried at 40°C for 24 hours to obtain a film with a dry thickness of 500 μm. The obtained film was cut into a 2 cm x 4 cm size to prepare a test piece. The test piece was conditioned at 23°C and a relative humidity of 50% for 24 hours, after which its mass (Wd) was measured. In addition, the test piece was immersed in ion-exchanged water at room temperature for 24 hours, then removed from the ion-exchanged water, water droplets on the surface were wiped off, and the mass (W) of the test piece was immediately measured. The water absorption rate (mass) was calculated using the following formula: Water absorption rate (mass) = {(W - Wd) / Wd} x 100
[0066] [Water absorption (thickness)] In the same manner as for the water absorption (mass), test pieces were prepared, and the thickness (Dd) of the obtained test pieces was measured after conditioning them at 23°C and a relative humidity of 50% for 24 hours. In addition, the test pieces were immersed in ion-exchanged water at room temperature for 24 hours, and the thickness (D) of the test pieces was measured immediately after removing them from the ion-exchanged water. The water absorption (thickness) was calculated using the following formula and evaluated according to the following evaluation criteria: Water absorption (thickness) = {(D - Dd) / Dd} x 100 <Evaluation criteria> ○: The water absorption (thickness) value is 50 or more △: The water absorption (thickness) value is 20 or more but less than 50 ×: The water absorption (thickness) value is less than 20
[0067] [Adhesion (before water absorption)] The above adhesive was applied to a substrate and dried at 80°C for 10 minutes to form a coating film with a dry thickness of 20 μm. A glass plate was used as the substrate in Examples 1 to 8 and Comparative Examples 1 and 2, and a corona-treated PET film was used in Examples 9 to 14 and Comparative Example 3. A photocurable resin liquid was then applied to the coating film and dried at 80°C for 10 minutes to form a photocurable resin layer with a dry thickness of 20 μm, thereby obtaining a laminate. The photocurable resin liquid used was a mixed liquid prepared by mixing a photocurable resin oligomer ("New Frontier R-1220" manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) with 3% by mass of a photopolymerization initiator ("Omnirad 184" manufactured by IGM Resins B.V.). The resulting laminate was irradiated with ultraviolet light to prepare a test specimen. The ultraviolet irradiation conditions were a nitrogen atmosphere (oxygen concentration 0.3%), a high-pressure mercury lamp of 80 W / cm, and an integrated illuminance of 250 mJ / cm. 2 The test conditions were: 1) a thickness of 100 mm, 2) a line speed of 5 m / min, and 3) a power of 2 kW. A cross-cut peel test was carried out on the prepared test pieces in accordance with JIS K5400 8.5.2:1990 ... 100 squares where the number of points where each layer was adhered was 70 or more, a cross-cut peel test was 20 or more but less than 70, and a cross-cut peel test was 20 or more but less than 70.
[0068] [Removability (after water absorption)] Test pieces were prepared in the same manner as for adhesion (before water absorption), immersed in ion-exchanged water at 80°C for 24 hours, removed from the ion-exchanged water, and dried at 40°C for 24 hours, after which a cross-cut peel test was carried out in accordance with JIS K5400 8.5.2:1990. Of 100 cross-cuts, an increase of 30 or more peeled locations compared to the test results before water absorption was evaluated as "Good," an increase of 15 to less than 30 was evaluated as "Good," and an increase of less than 15 was evaluated as "Poor."
[0069]
[0070] The results are shown in Table 1. Examples 1 to 8 and Comparative Examples 1 and 2 are examples in which glass plates were used as the substrates. In this case, Comparative Example 2, which contained only aqueous resin 1 as the adhesive component and no cellulose fiber, had excellent adhesion before water absorption, but had low water absorption when immersed in water and poor releasability after water absorption. In Comparative Example 1, the viscosity of the mixed liquid was high, making application difficult, so evaluations of water absorption (mass), water absorption (thickness), adhesion, and releasability were not performed, and these are indicated as "-" in Table 1.
[0071] In contrast, Examples 1 to 8, which contained cellulose fibers 1 to 4 in addition to aqueous resins 1 and 2, exhibited excellent adhesion before water absorption, a large change in thickness after immersion in water, and excellent peelability after water absorption. Comparing Examples 1 to 3 with Example 4, the cellulose fibers containing anionic groups had higher water absorption rates (mass) and thicknesses than unmodified fibers. Furthermore, the greater the amount of cellulose fiber, the higher the water absorption rates (mass) and thicknesses, but the lower the coatability.
[0072] Examples 9 to 14 and Comparative Example 3 are examples in which a PET film was used as the substrate. In Comparative Example 3, which contained only Waterborne Resin 6 as the adhesive component and no cellulose fiber, the adhesiveness before water absorption was excellent, but the change in thickness when immersed in water was small, and the peelability after water absorption was poor.
[0073] In contrast, Examples 9 to 14, which blended cellulose fiber 1 with water-based resins 3 to 8, had excellent adhesion before water absorption, a large change in thickness after immersion in water, and excellent releasability after water absorption. A comparison of Examples 9 to 11 showed that, with regard to the type of urethane emulsion used as the water-based resin, nonionic emulsions tended to be better than cationic ones, and anionic emulsions tended to be better than nonionic ones in terms of adhesion before water absorption and releasability after water absorption.
[0074] In the evaluation of adhesion (before water absorption) and peelability (after water absorption), in all of the Examples and Comparative Examples, the adhesion between the adhesive layer and the photocured resin layer was good, and no peeling was observed at the interface between the adhesive layer and the photocured resin layer.
[0075] The various numerical ranges described in this specification can be arbitrarily combined with their respective upper and lower limit values, and all such combinations are considered to be preferred numerical ranges described in this specification. Furthermore, a numerical range described as "X to Y" means from X to Y.
[0076] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the spirit of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included within the scope and spirit of the invention, as well as within the scope of the invention described in the claims and their equivalents.
Claims
1. An adhesive used in applications where the adhesive absorbs water after bonding and then peels off, comprising (A) an aqueous resin and (B) cellulose fibers, the adhesive comprising 0.1 to 10 parts by mass of the cellulose fibers per 100 parts by mass of the aqueous resin.
2. The adhesive of claim 1, wherein the water-based resin comprises a water-dispersible resin.
3. The adhesive according to claim 2, wherein the water-dispersible resin comprises an anionic water-dispersible resin and / or a nonionic water-dispersible resin.
4. The adhesive of claim 1, wherein the cellulose fibers comprise cellulose nanofibers.
5. The adhesive of claim 1, wherein the cellulose fibers have anionic groups.
6. The adhesive of claim 1 which is a primer.
7. An article comprising a first member, a second member, and an adhesive layer formed from the adhesive according to any one of claims 1 to 6, which bonds the first member and the second member.