Tire rubber composition, and tire

The rubber composition for tires, featuring a blend of rosin-modified phenolic resin and diene rubber with specific properties, addresses the challenges of dry grip and stability, enhancing performance and wear resistance for tire applications.

WO2024203632A1PCT designated stage expired Publication Date: 2024-10-03THE YOKOHAMA RUBBER CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010791
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing tire rubber compositions face challenges in achieving high dry grip performance, handling stability, and wear resistance, particularly when using high specific surface area fillers or high softening point resins, which can lead to deterioration in abrasion resistance and handling stability.

Method used

A rubber composition is developed by blending 1 to 100 parts by mass of rosin-modified phenolic resin with an acid value of less than 30 mgKOH/g with 100 parts by mass of diene rubber, specifically utilizing rosin-modified phenolic resin with a weight average molecular weight of 2,000 to 5,000 and a softening point of 100 to 160°C, along with carbon black and a liquid aromatic vinyl-conjugated diene rubber to enhance compatibility and performance.

Benefits of technology

The composition improves dry grip performance, handling stability, and wear resistance, making it suitable for tire treads, especially race tire treads, while maintaining optimal hardness and breaking strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

This tire rubber composition is obtained by blending 100 parts by mass of a diene rubber with 1-100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mg KOH / g.
Need to check novelty before this filing date? Find Prior Art

Description

Rubber composition for tires and tires

[0001] The present invention relates to a rubber composition for tires and a tire using the same, and more particularly to a rubber composition for tires that improves dry grip performance and has excellent steering stability and abrasion resistance, and a tire using the same.

[0002] Generally, tires are required to have a wide range of performance characteristics, among which high levels of grip performance, handling stability, and wear resistance are required. This requirement also exists for racing tires intended for circuit driving. Conventional techniques involve compounding large amounts of fillers with a high specific surface area or resins with a high softening point (high-softening-point resins). However, compounding large amounts of fillers with a high specific surface area leads to problems such as a decrease in breaking strength and a deterioration in wear resistance, while compounding large amounts of high-softening-point resins leads to problems such as a decrease in hardness and a deterioration in handling stability.

[0003] In addition, in the following Patent Document 1, the nitrogen adsorption specific surface area (N 2 SA) is 100 to 500m 2 The document discloses a rubber composition for tires, characterized by blending 50 to 200 parts by mass of carbon black having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more with 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more. However, the document does not disclose or suggest a rosin-modified phenol resin having an acid value of less than 30 mgKOH / g, as described below.

[0004] Patent No. 6791277

[0005] Therefore, an object of the present invention is to provide a rubber composition for tires which has improved dry grip performance and excellent steering stability and abrasion resistance, and a tire using the same.

[0006] As a result of extensive research, the inventors have discovered that the above-mentioned problems can be solved by blending a specific amount of a rosin-modified phenolic resin having an acid value within a specific range with a diene rubber, and have thus completed the present invention.

[0007] That is, the present invention provides a rubber composition for tires, characterized by blending 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g with 100 parts by mass of diene rubber.

[0008] The rubber composition for tires of the present invention is characterized by comprising 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g blended with 100 parts by mass of diene rubber, and therefore can provide a rubber composition for tires having improved dry grip performance and excellent steering stability and abrasion resistance, and a tire using the same.

[0009] The rosin-modified phenolic resin used in the present invention has excellent compatibility with diene rubbers, and because it has a low acid value, it is possible to fully utilize the functions of alkaline components (e.g., vulcanization accelerators) in the rubber composition, and it is presumed that this improves dry grip performance, handling stability, and abrasion resistance.

[0010] The present invention will now be described in further detail.

[0011] (Diene Rubber) The diene rubber used in the present invention can be any diene rubber that can be blended into a typical rubber composition, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), and acrylonitrile-butadiene copolymer rubber (NBR). These may be used alone or in combination of two or more. There are no particular restrictions on the molecular weight or microstructure, and the diene rubber may be terminally modified with an amine, amide, silyl, alkoxysilyl, carboxyl, or hydroxyl group, or may be epoxidized. Of these diene rubbers, SBR is preferred in terms of the effects of the present invention. For example, when used for racing, the blending amount of SBR is preferably 80 parts by mass or more, and more preferably 100 parts by mass.

[0012] Furthermore, when the styrene content of the SBR is less than 35% by mass, the effects of the present invention, particularly dry grip performance, can be further enhanced.The styrene content is more preferably 30 to 10% by mass.

[0013] (Rosin-Modified Phenolic Resin) The rosin-modified phenolic resin used in the present invention can be a reaction product of a rosin-based resin, a phenol, formaldehyde, and a polyol. Examples of rosin-based resins include unmodified rosins such as gum rosin, tall oil rosin, and wood rosin; polymerized rosins derived from unmodified rosin; disproportionates or hydrogenated products of unmodified rosin or polymerized rosin; and unsaturated carboxylic acid-modified rosins obtained by reacting unmodified rosin or polymerized rosin with an unsaturated carboxylic acid. Examples of phenols include phenol; alkylphenols such as methylphenol (cresol), butylphenol, pentylcresol, octylphenol, nonylphenol, decylphenol, dodecylphenol, tetradecylphenol, and hexyldecylphenol. Examples of formaldehyde include formalin and paraformaldehyde. Examples of polyols include diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol; triols such as glycerin, trimethylolpropane, and trimethylolethane; and tetraols such as pentaerythritol, diglycerin, ditrimethylolpropane, and ditrimethylolethane.

[0014] The amounts of the rosin resin, formaldehyde, phenols, and polyol used are not particularly limited and may be appropriately determined taking into consideration, for example, the desired molecular weight, softening point, etc. The reaction method may include, for example, a method in which the rosin resin, phenols / formaldehyde (condensate), and polyol are charged all at once and reacted, and the reaction temperature is usually about 100 to 300°C, and the reaction time is usually about 1 to 24 hours.

[0015] The rosin-modified phenolic resin used in the present invention must have an acid value adjusted to less than 30 mgKOH / g. The method for adjusting the acid value to less than 30 mgKOH / g is not particularly limited, but a preferred method involves esterifying the rosin-modified phenolic resin prepared as described above or a commercially available rosin-modified phenolic resin (which typically has an acid value of 30 mgKOH / g or more) to reduce the acid value to less than 30 mgKOH / g. The esterification can be carried out by conventional methods, using a polyhydric alcohol as the alcohol and at a reaction temperature of 150 to 300°C. Since the use of a dihydric alcohol such as ethylene glycol results in a resin with a low softening point, a trihydric or higher alcohol is preferably used. The acid value can be adjusted by the amount of alcohol charged. The rosin-modified phenolic resin prepared by the preferred method contains ester bonds within its interior, which enhances its compatibility with diene rubbers and further enhances the effects of the rosin-modified phenolic resin. The acid value of the rosin-modified phenolic resin used in the present invention is preferably 5 to 25 mgKOH / g, more preferably 10 to 20 mgKOH / g.

[0016] The rosin-modified phenolic resin used in the present invention preferably has a weight-average molecular weight of 2,000 to 5,000, more preferably 2,500 to 4,500, from the viewpoint of further enhancing the effects of the present invention. The softening point is preferably 100 to 160°C, more preferably 110 to 150°C. The weight-average molecular weight referred to in the present invention means the weight-average molecular weight in terms of polystyrene analyzed by gel permeation chromatography (GPC). The softening point is measured in accordance with JIS K6220-1.

[0017] (Bulking ratio) The rubber composition of the present invention is characterized by blending 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g per 100 parts by mass of diene rubber. If the blending amount of the rosin-modified phenolic resin is less than 1 part by mass, the blending amount is too small to achieve the effects of the present invention. Conversely, if the blending amount exceeds 100 parts by mass, hardness and breaking strength decrease, and handling stability and abrasion resistance cannot be improved. The blending amount of the rosin-modified phenolic resin is preferably 5 to 85 parts by mass, more preferably 10 to 70 parts by mass, per 100 parts by mass of diene rubber.

[0018] The rubber composition for a tire of the present invention is preferably a rubber composition having a nitrogen adsorption specific surface area (N 2 SA) is 100 to 500m 2 It is preferable to blend carbon black having a nitrogen adsorption specific surface area (N 2 SA) is 125-450m 2 The amount of carbon black to be compounded is preferably 50 to 200 parts by mass, more preferably 80 to 170 parts by mass, per 100 parts by mass of the diene rubber (A). The nitrogen adsorption specific surface area (N 2 SA) is a value determined in accordance with JIS K6217-2.

[0019] (Liquid Aromatic Vinyl-Conjugated Diene Rubber) The rubber composition for tires of the present invention preferably contains a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher. By incorporating such a liquid aromatic vinyl-conjugated diene rubber, the glass transition temperature (Tg) of the rubber composition is increased, thereby improving dry grip performance. Furthermore, the liquid aromatic vinyl-conjugated diene rubber is compatible with diene rubbers and improves the dispersibility of the rosin-modified phenolic resin used in the present invention, thereby enhancing the effects of the present invention. A preferred liquid aromatic vinyl-conjugated diene rubber is liquid styrene-butadiene copolymer (liquid SBR). The liquid SBR has a weight-average molecular weight of 2,000 to 40,000, preferably 3,000 to 20,000. The glass transition temperature of the liquid SBR is -40°C or higher, as described above, and is more preferably -20°C to -5°C. Commercially available liquid SBRs can be used, such as RICON 100 manufactured by Cray Valley and L-SBR 820 manufactured by Kuraray Co., Ltd. The Tg used in the present invention is the midpoint temperature of the transition region measured by differential scanning calorimetry (DSC) at a heating rate of 20°C / min. The liquid aromatic vinyl-conjugated diene rubber used in the present invention is a liquid at 23°C. Therefore, it is distinguished from the diene rubber, which is solid at this temperature. The amount of the liquid aromatic vinyl-conjugated diene rubber compounded is preferably 5 to 50 parts by mass, more preferably 10 to 45 parts by mass, per 100 parts by mass of the diene rubber.

[0020] (Other Components) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives that are generally compounded in rubber compositions, such as vulcanizing or crosslinking agents; vulcanizing or crosslinking accelerators; zinc oxide; various fillers such as clay, talc, and calcium carbonate; antioxidants; and plasticizers. These additives can be kneaded by a general method to form a composition, which can then be used for vulcanization or crosslinking. The amounts of these additives that can be compounded may be conventional amounts, as long as they do not deviate from the object of the present invention.

[0021] In addition to the rosin-modified phenolic resin, other resins can also be blended as needed. Examples include phenolic resins (e.g., phenolic resin, phenol-acetylene resin, phenol-formaldehyde resin), coumarone resins (e.g., coumarone resin, coumarone-indene resin, coumarone-indene-styrene resin), terpene resins (e.g., terpene resin, modified terpene resin (aromatic modified terpene resin, etc.), terpene phenolic resin), styrene resin, acrylic resin, petroleum resins (e.g., C5 petroleum resins such as dicyclopentazine resin, C9 petroleum resin, alicyclic petroleum resin, C5 / C9 copolymer petroleum resin), xylene resins (e.g., xylene resin, xylene-acetylene resin, xylene-formaldehyde resin), α-pinene resin, and aliphatic saturated hydrocarbon resin. The blending amount of these other resins is, for example, 10 to 150 parts by mass per 100 parts by mass of diene rubber.

[0022] The rubber composition of the present invention improves dry grip performance and has excellent handling stability and abrasion resistance, and therefore can be suitably used for tire treads, particularly cap treads, preferably racing tire treads, particularly cap treads. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, or other gases.

[0023] The present invention will be further explained below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0024] Preparation of Samples: Standard Examples 1-2, Examples 1-10, and Comparative Examples 1-7. In the formulations (parts by mass) shown in Tables 1 or 2, the components excluding the vulcanization accelerator and sulfur were kneaded for 5 minutes in a 1.7-liter internal Banbury mixer, and the rubber was discharged from the mixer and cooled to room temperature. The rubber was then re-introduced into the same mixer, and the vulcanization accelerator and sulfur were added and further kneaded to obtain a rubber composition. The resulting rubber composition was then press-vulcanized in a specified mold at 160°C for 20 minutes to obtain vulcanized rubber test pieces, and the physical properties of the vulcanized rubber test pieces were measured using the test methods shown below.

[0025] Dry grip performance: In accordance with JIS K6394, tan δ (100°C) was measured using a viscoelasticity spectrometer manufactured by Toyo Seiki Seisakusho, Ltd., under conditions of initial strain = 10%, amplitude = ±2%, and frequency = 20 Hz, and the dry grip performance was evaluated based on this value. The results were expressed as an index, with the value of Standard Example 1 or 2 being 100. A higher index indicates better dry grip performance. Hardness (100°C): Measured at 100°C in accordance with JIS K6253. The results were expressed as an index, with the value of Standard Example 1 or 2 being 100. A higher index indicates higher hardness and better handling stability. Breaking strength: In accordance with JIS K6251, No. 3 dumbbell-shaped sample pieces were punched out from the vulcanized rubber test pieces and subjected to a tensile test at a tensile speed of 500 mm / min to measure the breaking elongation (%). The results were expressed as an index, with the value of Standard Example 1 or 2 being 100. A higher index indicates better breaking strength and wear resistance. The results are shown in Tables 1 and 2. Standard Example 1 is compared with Examples 1 to 6 and Comparative Examples 1 to 3, and Standard Example 2 is compared with Examples 7 to 10 and Comparative Examples 4 to 7.

[0026]

[0027]

[0028] *1: SBR1 (Nipol 1739 manufactured by ZEON (styrene content = 40% by mass)) *2: SBR2 (Nipol 1723 manufactured by ZEON (styrene content = 23.5% by mass)) *3: Carbon black 1 (Showblack N339, N manufactured by Cabot Japan) 2 SA=94m 2 / g) *4: Carbon black 2 (Seast 9, N manufactured by Tokai Carbon Co., Ltd. 2 SA=142m 2 / g) *5: Resin 1 (Yasuhara Chemical Co., Ltd. YS Polystar S145, phenol-modified terpene resin, acid value = 0 mg KOH / g) *6: Resin 2 (Arakawa Chemical Industries, Ltd. Tamanol 803L, rosin phenolic resin, acid value = 52 mg KOH / g) *7: Resin 3 (Arakawa Chemical Industries, Ltd. Marquid No. 5, maleic acid-modified rosin resin, acid value = 19 mg KOH / g) *8: Resin 4 (Arakawa Chemical Industries, Ltd. Pencel KK, rosin ester resin, acid value = 19 mg KOH / g) *9: Resin 5 (rosin-modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. acid value = 15 mg KOH / g) *10: Resin 6 (rosin-modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. acid value = 17 mg KOH / g) *11: Resin 7 (Neopolymer 140 manufactured by ENEOS) *12: Liquid SBR (RICON 100 manufactured by Cray Valley, weight average molecular weight = 6400, Tg = -15 ° C) *13: Oil (Extract No. 4 S manufactured by Showa Shell Sekiyu K.K.) *14: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *15: Zinc oxide (Zinc oxide 3 types manufactured by Seido Chemical Industry Co., Ltd.) *16: Antiaging agent (6PPD manufactured by Flexis) *17: Vulcanization accelerator (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) *18: Sulfur (Kinka brand oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.)

[0029] The results in Tables 1 and 2 show that the rubber compositions of the examples, which contain 1 to 100 parts by mass of a rosin-modified phenolic resin with an acid value of less than 30 mgKOH / g per 100 parts by mass of diene rubber, simultaneously exhibit improved dry grip performance, handling stability, and abrasion resistance compared to Reference Examples 1 and 2. In contrast, Comparative Example 1 exhibited poor dry grip performance and hardness because the acid value of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention. Comparative Example 2 exhibited poor dry grip performance because a maleic acid-modified rosin resin was used. Comparative Example 3 exhibited poor dry grip performance because a rosin ester resin was used. Comparative Example 4 exhibited poor dry grip performance and hardness because the acid value of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention. Comparative Example 5 exhibited poor dry grip performance because a maleic acid-modified rosin resin was used. Comparative Example 6 exhibited poor dry grip performance because a rosin ester resin was used. In Comparative Example 7, the blend amount of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention, and therefore the hardness and breaking strength were deteriorated.

[0030] The present disclosure encompasses the following inventions. Invention [1]: A rubber composition for tires, characterized by comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g. Invention [2]: A rubber composition for tires, characterized by comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g. Invention [3]: A rubber composition for tires, characterized by comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g. 2 SA) is 100 to 500m 2The rubber composition for a tire according to Invention 1, characterized in that it is blended with 50 to 200 parts by mass of carbon black having a styrene content of less than 35% by mass. Invention [3]: The rubber composition for a tire according to Invention 1 or 2, characterized in that the diene rubber comprises a styrene-butadiene copolymer rubber having a styrene content of less than 35% by mass. Invention [4]: ​​The rubber composition for a tire according to any of Inventions 1 to 3, characterized in that it further comprises a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher per 100 parts by mass of the diene rubber. Invention [5]: The rubber composition for a tire according to any of Inventions 1 to 4, characterized in that the diene rubber consists solely of styrene-butadiene copolymer rubber. Invention [6]: The rubber composition for a tire according to any of Inventions 1 to 5, characterized in that the rosin-modified phenolic resin has an acid value of 5 to 25 mgKOH / g. Invention [7]: A rubber composition for a tire according to Invention 4, characterized in that the liquid aromatic vinyl-conjugated diene rubber is a liquid styrene-butadiene copolymer having a weight average molecular weight of 2000 to 40000. Invention [8]: A rubber composition for a tire according to Invention 4, characterized in that the glass transition temperature (Tg) of the liquid aromatic vinyl-conjugated diene rubber is -20°C to -5°C. Invention [9]: A tire using the rubber composition for a tire according to any one of Inventions 1 to 8 in a cap tread.

Claims

1. A rubber composition for tires, comprising 100 parts by mass of diene rubber and 1 to 100 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g.

2. For 100 parts by mass of the diene rubber, a nitrogen adsorption specific surface area (N 2 SA) is 100 to 500m 2 2. The rubber composition for tires according to claim 1, characterized in that 50 to 200 parts by mass of carbon black having a molecular weight of 1 / g is blended.

3. The rubber composition for tires according to claim 1, characterized in that the diene rubber contains a styrene-butadiene copolymer rubber having a styrene content of less than 35 mass %.

4. The rubber composition for tires according to claim 1, further comprising a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher per 100 parts by mass of the diene rubber.

5. A rubber composition for tires according to claim 1, characterized in that the diene rubber consists solely of a styrene-butadiene copolymer rubber.

6. The rubber composition for tires according to claim 1, wherein the acid value of the rosin-modified phenolic resin is 5 to 25 mgKOH / g.

7. A rubber composition for tires according to claim 4, wherein the liquid aromatic vinyl-conjugated diene rubber is a liquid styrene-butadiene copolymer having a weight average molecular weight of 2,000 to 40,000.

8. The rubber composition for tires according to claim 4, characterized in that the glass transition temperature (Tg) of the liquid aromatic vinyl-conjugated diene rubber is -20°C to -5°C.

9. A tire in which the rubber composition for tires according to claim 1 is used in the cap tread.

Citation Information

Patent Citations

  • Rubber composition for tires and pneumatic tire using same

    JP6791277B2

  • Flame-retardant chlorinated polyethylene waterproof roll and preparation method thereof

    CN110539540A

  • Light-colored low-molecular-weight phenol-modified rosin ester

    JP2002526592A

  • Rubber composition for tire

    JP2009051975A

  • Adhesive tape

    JP2017200978A