4-methyl-1-pentene-based copolymer, 4-methyl-1-pentene-based copolymer composition, molded body, laminate, and method for producing laminate

The 4-methyl-1-pentene copolymer composition, incorporating specific monomers and crosslinking agents, addresses the heat resistance and rigidity issues in conventional copolymers, ensuring strength and dielectric properties above the melting point, making it suitable for high-frequency circuit boards and other heat-resistant applications.

WO2024203635A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/010794
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-08
Filing Date
2024-03-19
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional 4-methyl-1-pentene copolymers lack sufficient heat resistance and soldering heat resistance, particularly in high-frequency circuit boards, where they lose strength and deform when exposed to temperatures above their melting point, and do not maintain rigidity and dielectric properties effectively.

Method used

A 4-methyl-1-pentene copolymer composition with a structural unit derived from 4-methyl-1-pentene and at least one monomer from symmetric or asymmetric dienes and allylic-substituted olefins, crosslinked using a crosslinking agent or auxiliary agent, and processed with a fiber base material to create a laminate with improved heat resistance and dielectric properties.

Benefits of technology

The copolymer maintains strength and rigidity above its melting point, exhibits excellent heat-resistant and dielectric properties, and is suitable for high-frequency circuit boards and other applications requiring heat resistance and lightweight materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

The present invention pertains to: a 4-methyl-1-pentene-based copolymer; a composition containing said copolymer; a molded body; a laminate; and a method for producing the laminate. The 4-methyl-1-pentene-based copolymer includes a structural unit (A) derived from 4-methyl-1-pentene and a structural unit (B) derived from at least one monomer selected from the group consisting of symmetric dienes, asymmetric dienes, and allyl-position-substituted olefins.
Need to check novelty before this filing date? Find Prior Art

Description

4-methyl-1-pentene copolymer, 4-methyl-1-pentene copolymer composition, molded article, laminate, and method for producing laminate

[0001] The present invention relates to a 4-methyl-1-pentene copolymer, a composition containing the copolymer, a molded article containing the composition, a laminate containing the composition, and a method for producing the laminate.

[0002] 4-methyl-1-pentene copolymers (also referred to as polymethylpentene, PMP, etc.) have been used in a variety of applications because they have the characteristics of excellent stain resistance due to extremely low surface tension, excellent transparency and scratch resistance, and high heat resistance.

[0003] In this regard, there is a technology for forming crosslinks in polyolefin resins by electron beam irradiation in order to improve their mechanical properties and heat resistance. 4-methyl-1-pentene copolymers are a type of polyolefin resin, but because they contain side chains, crosslinking occurs and decomposition of the molecular chains proceeds simultaneously upon electron beam irradiation. For this reason, various attempts have been made to improve the physical properties of 4-methyl-1-pentene copolymers by electron beam irradiation.

[0004] For example, Patent Document 1 discloses an electron beam curable resin composition containing polymethylpentene and a specific crosslinking agent, and a cured product obtained by irradiating the electron beam curable resin composition with an electron beam. Patent Document 1 also describes that the electron beam curable resin composition has excellent heat resistance and can be used for resin frames for reflectors, reflectors, and semiconductor light emitting devices.

[0005] Furthermore, Patent Document 2 discloses an attempt to modify a polymethylpentene resin by irradiating a composite fiber made of a polymethylpentene resin and a thermoplastic resin other than a polymethylpentene resin with an electron beam. Here, Patent Document 2 also describes that when the polymethylpentene resin is exposed to an electron beam, the bonds between the molecules are broken and radicals are generated, and that the generated radicals bond with each other to crosslink the polymethylpentene resin, thereby improving heat resistance and abrasion resistance.

[0006] JP 2017-031429 A JP 2019-178442 A

[0007] As described above, 4-methyl-1-pentene copolymers have excellent heat resistance, and thus attempts have been made to apply them to fields such as synthetic leather release paper and semiconductor sealing films for electronic components. Furthermore, because 4-methyl-1-pentene copolymers have excellent electrical properties in addition to excellent heat resistance, attempts have also been made to apply them to the field of electronic components, particularly to electronic components including high-frequency circuit boards, which require both excellent heat resistance and electrical properties. However, in these fields, resins may be subjected to heat exceeding their melting points. In such cases, even 4-methyl-1-pentene copolymers may suffer a significant decrease in strength due to heat, and even molded articles may be deformed. The 4-methyl-1-pentene copolymer described in Patent Document 1 does not fully solve these problems, and a 4-methyl-1-pentene copolymer with even higher heat resistance has been desired. In particular, when considering high-frequency circuit boards, conventional 4-methyl-1-pentene copolymers have excellent dielectric properties but lack solder heat resistance (heat resistance to 288°C). The problem to be solved by one embodiment of the present invention is to provide a 4-methyl-1-pentene copolymer that can maintain a certain strength and have excellent rigidity even in a temperature range equal to or higher than the melting point (Tm), a composition containing the copolymer, and a molded article. Another problem to be solved by one embodiment of the present invention is to provide a method for producing a laminate that has excellent dielectric properties and solder heat resistance.

[0008] As a result of extensive research, the present inventors have found that the above problems can be solved, and have completed the present invention.

[0009] Means for solving the above problems include the following embodiments [1] to

[12] . [1] A 4-methyl-1-pentene copolymer comprising: a structural unit (A) derived from 4-methyl-1-pentene; and a structural unit (B) derived from at least one monomer selected from the group consisting of symmetric dienes, asymmetric dienes, and allylic-substituted olefins. [2] The 4-methyl-1-pentene copolymer according to [1], wherein the structural unit (B) comprises a structural unit derived from at least one monomer selected from the group consisting of asymmetric dienes and allylic-substituted olefins. [3] The 4-methyl-1-pentene copolymer according to [1] or [2], wherein the structural unit (B) comprises a structural unit derived from at least one monomer selected from the group consisting of 7-methyl-1,6-octadiene and 4-vinyl-1-cyclohexene. [4] The 4-methyl-1-pentene copolymer according to any one of [1] to [3], wherein the content of the structural unit (B) is 0.1 to 10.0 mol % when the total content of the structural unit (A) and the structural unit (B) is taken as 100 mol %. [5] A 4-methyl-1-pentene copolymer composition comprising the 4-methyl-1-pentene copolymer according to any one of [1] to [4], and at least one selected from the group consisting of a crosslinking agent and a crosslinking aid, in an amount of 0 to 10 parts by mass per 100 parts by mass of the 4-methyl-1-pentene copolymer. [6] A molded article comprising the 4-methyl-1-pentene copolymer according to any one of [1] to [4] or the 4-methyl-1-pentene copolymer composition according to [5]. [7] The molded article according to [6], which is a film. [8] A laminate comprising the film according to [7], and a fibrous substrate containing at least one type of fiber selected from the group consisting of inorganic fibers and organic fibers. [9] The laminate according to [8], wherein the fibers are glass fibers.

[10] A method for producing a laminate, comprising: laminating a molded article containing the 4-methyl-1-pentene copolymer according to any one of [1] to [4] and a fibrous substrate containing at least one type of fiber selected from inorganic fibers and organic fibers so that they are in contact with each other, and heating the laminate at a temperature of 230 to 350°C; and crosslinking the 4-methyl-1-pentene copolymer.

[11] A method for producing the laminate according to

[10] , further comprising a step of producing the molded article.

[12] A method for producing the laminate according to

[10] or

[11] , further comprising a step of producing the 4-methyl-1-pentene copolymer.

[0010] According to the present invention, it is possible to provide a 4-methyl-1-pentene copolymer that can maintain a certain level of strength even in a temperature range equal to or higher than the melting point (Tm) and has excellent rigidity, as well as a composition and molded article containing the copolymer. Furthermore, according to the present invention, it is possible to provide a laminate that not only has excellent dielectric properties and soldering heat resistance, but also has excellent heat-resistant rigidity and is lightweight by devising processing conditions during impregnation of the fiber base material, making it suitable for use in high-frequency circuit boards.

[0011] In the present disclosure, the expressions "XX or more and YY or less" and "XX to YY" representing a numerical range mean a numerical range including the lower and upper limits, which are the endpoints, unless otherwise specified. Furthermore, when a numerical range is described in stages, the upper and lower limits of each numerical range can be combined arbitrarily. Furthermore, the various monomers in the present disclosure may be derived from fossil raw materials or biomass.

[0012] [4-Methyl-1-pentene Copolymer] The 4-methyl-1-pentene copolymer of the present invention comprises a structural unit (A) derived from 4-methyl-1-pentene and a structural unit (B) derived from at least one monomer selected from the group consisting of symmetric dienes, asymmetric dienes, and allylic-substituted olefins.

[0013] <Structural Unit (A)> The 4-methyl-1-pentene copolymer of the present invention has a structural unit (A) derived from 4-methyl-1-pentene.

[0014] The content of the structural unit (A) is preferably 90.0 to 99.9 mol %, more preferably 93.0 to 99.7 mol %, even more preferably 94.5 to 99.5 mol %, and particularly preferably 95.0 to 99.0 mol %, provided that the total content of the structural unit (A) and the structural unit (B) is 100 mol %.

[0015] <Structural Unit (B)> The 4-methyl-1-pentene copolymer of the present invention has a structural unit (B) derived from at least one monomer selected from the group consisting of symmetric dienes, asymmetric dienes, and allylic-substituted olefins. Among the symmetric and asymmetric dienes, those that also qualify as allylic-substituted olefins are classified as allylic-substituted olefins. The structural unit (B) imparts crosslinkability to the 4-methyl-1-pentene copolymer, and a 4-methyl-1-pentene copolymer having the structural unit (B) can be crosslinked by any method. By crosslinking a 4-methyl-1-pentene copolymer having the structural unit (B), a 4-methyl-1-pentene copolymer having higher heat resistance than conventional copolymers can be obtained. In other words, a 4-methyl-1-pentene copolymer can be obtained that can maintain a certain level of strength even in a temperature range above the melting point (Tm).

[0016] The content of the structural unit (B) is preferably 0.1 to 10.0 mol%, more preferably 0.3 to 7.0 mol%, even more preferably 0.5 to 5.5 mol%, and particularly preferably 1.0 to 5.0 mol%. When the content of the structural unit (B) is 0.1 mol% or more, crosslinking to the 4-methyl-1-pentene copolymer is likely to be sufficient, and a 4-methyl-1-pentene copolymer having superior heat resistance can be obtained. When the content of the structural unit (B) is 10.0 mol% or less, the melting point and heat of fusion of the 4-methyl-1-pentene copolymer are less likely to decrease, which is preferable in terms of heat resistance and rigidity.

[0017] Examples of symmetric dienes from which the structural unit (B) can be derived include conjugated dienes such as 1,3-butadiene and 1,3-octadiene, and non-conjugated polyenes such as 1,4-pentadiene, 1,5-hexadiene, 1,7-octadiene and cyclohexadiene.

[0018] Examples of asymmetric dienes from which the structural unit (B) can be derived include conjugated dienes such as 1,3-pentadiene, 4-methyl-1,3-pentadiene, and 1,3-hexadiene, and non-conjugated polyenes such as 1,4-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, and 7-methyl-1,6-octadiene.

[0019] The allylic-substituted olefin from which the structural unit (B) can be derived refers to an olefin having a substituent other than a hydrogen atom at the allylic position of the olefin. When the allylic-substituted olefin has multiple allylic positions, it is sufficient that the allylic-substituted olefin has a substituent other than a hydrogen atom at at least one allylic position. The allylic-substituted olefin may be any of a terminal olefin, an internal olefin, and a cyclic olefin. Among these, cyclic olefins are preferred. Examples of the allylic-substituted olefin include terminal olefins such as isoprene, chloroprene, 2,3-dimethyl-1,3-butadiene, and vinylcyclohexane, and cyclic olefins such as 4-vinyl-1-cyclohexene. The allyl-substituted olefin may have a crosslinked structure at the allyl position of the olefin, and examples thereof include cyclic olefins such as 5-methyl-2-norbornene, dicyclopentadiene, dicyclooctadiene, methylenenorbornene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, and 2-ethylidene-3-isopropylidene-5-norbornene.

[0020] Of these, it is preferable that the structural unit (B) contains a structural unit derived from at least one monomer selected from the group consisting of asymmetric dienes and allylic-substituted olefins, it is more preferable that it contains a structural unit derived from at least one monomer selected from the group consisting of 7-methyl-1,6-octadiene and 4-vinyl-1-cyclohexene, and it is even more preferable that it contains a structural unit derived from 7-methyl-1,6-octadiene.

[0021] <Other Structural Units> The 4-methyl-1-pentene copolymer of the present invention may have other structural units in addition to the structural unit (A) and the structural unit (B). The content of the other structural units in the 4-methyl-1-pentene copolymer is preferably 0.0 to 5.0 mol %, and more preferably 0.0 to 1.0 mol %.

[0022] Examples of the monomers from which the other structural units can be derived include cyclic olefins, aromatic vinyl compounds, conjugated dienes, non-conjugated polyenes, and functional vinyl compounds.

[0023] Examples of cyclic olefins from which the other structural units can be derived include compounds having 4 to 20 carbon atoms, preferably 5 to 15 carbon atoms, such as cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, and tetracyclododecene, which do not fall into the category of symmetric dienes, asymmetric dienes, or allylic-substituted olefins.

[0024] Examples of aromatic vinyl compounds from which the other structural units can be derived include styrene; and mono- or polyalkylstyrenes such as α-methylstyrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylstyrene, m-ethylstyrene, and p-ethylstyrene.

[0025] Examples of conjugated dienes from which the other structural units can be derived include compounds having 4 to 20, preferably 4 to 10, carbon atoms, such as 1,3-butadiene, isoprene, chloroprene, 1,3-pentadiene, 2,3-dimethylbutadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-octadiene, which do not fall into the category of symmetrical dienes, asymmetrical dienes, or allylic-substituted olefins.

[0026] Examples of non-conjugated polyenes from which the other structural units can be derived include 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, cyclohexadiene, dicyclooctadiene, methylenenorbol Among compounds having 5 to 20, preferably 5 to 10, carbon atoms, such as norbornene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, and 2-propenyl-2,2-norbornadiene, compounds which do not fall into the category of symmetric dienes, asymmetric dienes, or allylic-substituted olefins are also included.

[0027] Examples of functional vinyl compounds from which the other structural units can be derived include hydroxyl group-containing olefins; halogenated olefins; unsaturated carboxylic acids such as acrylic acid, propionic acid, 3-butenoic acid, 4-pentenoic acid, 5-hexenoic acid, 6-heptenoic acid, 7-octenoic acid, 8-nonenoic acid, and 9-decenoic acid; unsaturated amines such as allylamine, 5-hexenamine, and 6-heptenamine; unsaturated acid anhydrides such as (2,7-octadienyl)succinic anhydride, pentapropenylsuccinic anhydride, and acid anhydrides of the above-mentioned unsaturated carboxylic acids; halides of the above-mentioned unsaturated carboxylic acids; and unsaturated epoxy compounds such as 4-epoxy-1-butene, 5-epoxy-1-pentene, 6-epoxy-1-hexene, 7-epoxy-1-heptene, 8-epoxy-1-octene, 9-epoxy-1-nonene, 10-epoxy-1-decene, and 11-epoxy-1-undecene.

[0028] The hydroxyl group-containing olefin from which the other structural units can be derived is not particularly limited as long as it is an olefinic compound having a hydroxyl group, but is preferably a terminally hydroxylated olefin compound. Examples of the terminally hydroxylated olefin compound include linear hydroxylated α-olefins having 4 to 20, preferably 2 to 10, carbon atoms, such as vinyl alcohol, allyl alcohol, hydroxylated 1-butene, hydroxylated 1-pentene, hydroxylated 1-hexene, hydroxylated 1-octene, hydroxylated 1-decene, hydroxylated 1-dodecene, hydroxylated 1-tetradecene, hydroxylated 1-hexadecene, hydroxylated 1-octadecene, and hydroxylated 1-eicosene; and hydroxylated α-olefins, such as hydroxylated 4-methyl-1-pentene, hydroxylated 3-methyl-1-pentene, hydroxylated 3-ethyl-1-pentene, hydroxylated 4,4-dimethyl-1-pentene, hydroxylated 4-methyl-1-hexene, hydroxylated 4,4-dimethyl-1-hexene, hydroxylated 4-ethyl-1-hexene, and hydroxylated 3-ethyl-1-hexene.

[0029] Examples of the halogenated olefins from which the other structural units can be derived include linear halogenated α-olefins having 4 to 20, preferably 4 to 10, carbon atoms, such as halogenated 1-butene, halogenated 1-pentene, halogenated 1-hexene, halogenated 1-octene, halogenated 1-decene, halogenated 1-dodecene, halogenated 1-tetradecene, halogenated 1-hexadecene, halogenated 1-octadecene, and halogenated 1-eicosene; Included are branched halogenated α-olefins having 5 to 20, more preferably 5 to 10, carbon atoms, such as methyl-1-butene, halogenated 4-methyl-1-pentene, halogenated 3-methyl-1-pentene, halogenated 3-ethyl-1-pentene, halogenated 4,4-dimethyl-1-pentene, halogenated 4-methyl-1-hexene, halogenated 4,4-dimethyl-1-hexene, halogenated 4-ethyl-1-hexene, and halogenated 3-ethyl-1-hexene.

[0030] <Physical Properties> Preferred physical properties of the 4-methyl-1-pentene copolymer of the present invention will be described in detail below.

[0031] The 4-methyl-1-pentene copolymer of the present invention has an intrinsic viscosity [η] measured in decalin at 135°C of preferably 0.1 to 20 dL / g, more preferably 0.5 to 20 dL / g, and even more preferably 1.0 to 5.0 dL / g. The intrinsic viscosity [η] can be measured according to the method described in the Examples below. The value of the intrinsic viscosity [η] can be adjusted, for example, by the amount of hydrogen added in the polymerization step when producing the 4-methyl-1-pentene copolymer.

[0032] The 4-methyl-1-pentene copolymer of the present invention has a melting point (Tm) measured by differential scanning calorimetry (DSC) (heating rate: 10° C. / min) of preferably 100 to 250° C., more preferably 150 to 250° C., 200 to 245° C., 205 to 245° C., and particularly preferably 210 to 245° C. The melting point (Tm) can be measured according to the method described in the examples below.

[0033] The melting point being in the range of 100 to 250° C. means that, in the case where there are multiple melting points, all of the melting points are in the above range.

[0034] The melting point (Tm) value tends to depend on the stereoregularity of the 4-methyl-1-pentene copolymer and the content of the structural unit (B) in the 4-methyl-1-pentene copolymer. Therefore, the melting point (Tm) can be adjusted by using an olefin polymerization catalyst described below and further controlling the content of the structural unit (B).

[0035] <Method for Producing 4-Methyl-1-Pentene Copolymer> The method for producing the 4-methyl-1-pentene copolymer is not particularly limited. The production method includes a step of copolymerizing 4-methyl-1-pentene, a monomer from which the structural unit (B) can be derived, and, if necessary, a monomer from which the other structural units can be derived, by a method such as a gas phase method, a solution method, or a slurry method. In this step, an olefin polymerization catalyst described below is preferably used.

[0036] (Olefin Polymerization Catalyst) The olefin polymerization catalyst used in the production of the 4-methyl-1-pentene copolymer is not particularly limited as long as it can produce the 4-methyl-1-pentene copolymer of the present invention. For example, known catalysts such as solid titanium catalysts and metallocene catalysts can be used. The solid titanium catalyst may be one commonly used in the field to which the present invention pertains. For example, a solid titanium catalyst component containing titanium, magnesium, and a halogen element, as well as a 2,2-dialkyl-1,3-dialkoxypropane such as 2-isobutyl-2-isopropyl-1,3-dimethoxypropane is preferred. Specific examples include the solid titanium catalyst components described in WO 2006 / 054613. The olefin polymerization catalyst used in the production of the 4-methyl-1-pentene copolymer preferably contains the following metallocene compound (I):

[0037] Metallocene Compound (I) As the metallocene compound (I), for example, compounds disclosed in WO 2005 / 121192, WO 2014 / 050817, WO 2014 / 123212, and WO 2017 / 150265 can be used.

[0038] Compound (II) The olefin polymerization catalyst preferably contains at least one compound (hereinafter also referred to as "compound (II)") selected from: (II-1) an organometallic compound; (II-2) an organoaluminum oxy compound; and (II-3) a compound that reacts with the metallocene compound (I) to form an ion pair.

[0039] Compound (II), the carrier (III) described later, and the organic compound component (IV) may be, for example, compounds disclosed in WO 2014 / 050817, JP 2015-183141 A, and WO 2014 / 123212.

[0040] Support (III) The olefin polymerization catalyst preferably further contains a support (III).

[0041] From the viewpoints of high activity and suppressing the amount of solvent-soluble components, the support (III) is preferably a support containing aluminum atoms. The content of aluminum atoms in the support (III) is preferably 20% by mass or more, more preferably 20 to 60% by mass, even more preferably 30 to 50% by mass, and particularly preferably 35 to 47% by mass.

[0042] The median diameter D50 of the carrier (III) in terms of volume statistics is preferably 1 to 500 μm, more preferably 2 to 200 μm, and even more preferably 5 to 50 μm. The median diameter D50 in terms of volume statistics can be determined by a laser diffraction / scattering method using, for example, an MT3300EX II manufactured by Microtrac.

[0043] As such a carrier (III), a solid aluminoxane is preferred, and for example, the solid aluminoxanes disclosed in WO 2010 / 055652, WO 2013 / 146337, and WO 2014 / 123212 can be used.

[0044] As the solid aluminoxane, solid polymethylaluminoxane is preferred, and for example, the solid polymethylaluminoxane disclosed in WO 2014 / 123212 can be used.

[0045] Organic Compound Component (IV) The olefin polymerization catalyst may further contain an organic compound component (IV) as needed. The organic compound component (IV) is used as needed to improve the polymerization performance and the physical properties of the resulting polymer. Examples of the organic compound (IV) include alcohols, phenolic compounds, carboxylic acids, phosphorus compounds, amides, polyethers, and sulfonates.

[0046] [4-Methyl-1-pentene Copolymer Composition] The 4-methyl-1-pentene copolymer composition according to the present invention contains the 4-methyl-1-pentene copolymer as an essential constituent component, and also contains various other components depending on the application of the molded article according to the present invention. In a preferred embodiment of the present invention, the 4-methyl-1-pentene copolymer composition contains the 4-methyl-1-pentene copolymer and at least one selected from the group consisting of a crosslinking agent and a crosslinking aid in an amount of 0 to 10 parts by mass per 100 parts by mass of the 4-methyl-1-pentene copolymer. Here, the phrase "the content of at least one selected from the group consisting of a crosslinking agent and a crosslinking aid is 0 to 10 parts by mass" means that the composition may or may not contain a crosslinking agent and a crosslinking aid, but if it does contain one, the total amount of the crosslinking agent and the crosslinking aid is 10 parts by mass or less.

[0047] <Crosslinking Agent> The 4-methyl-1-pentene copolymer composition according to the present invention is a crosslinkable composition, and by crosslinking the composition, a molded article as described below can be produced. Crosslinking may be carried out by heating or the like using a crosslinking agent or a crosslinking aid as described below, or may be carried out by radiation crosslinking, in which crosslinking is carried out by irradiating with electromagnetic waves such as electron beams, X-rays, γ-rays, α-rays, and β-rays. Among radiation crosslinking methods, electron beam crosslinking is preferred.

[0048] The molded article according to the present invention is preferably produced by crosslinking using radiation crosslinking, particularly electron beam crosslinking. In this case, the 4-methyl-1-pentene copolymer composition may or may not contain a crosslinking agent. Furthermore, when the 4-methyl-1-pentene copolymer composition is crosslinked by heating, the 4-methyl-1-pentene copolymer composition preferably contains a crosslinking agent. Note that the crosslinking agent may be used alone or in combination of two or more types.

[0049] The content of the crosslinking agent is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably less than 0.1 parts by mass, and particularly preferably less than 0.01 parts by mass, relative to 100 parts by mass of the 4-methyl-1-pentene copolymer. On the other hand, the lower limit of the content is 0 parts by mass or more, relative to 100 parts by mass of the 4-methyl-1-pentene copolymer. When the content of the crosslinking agent is within the above range, bleeding of the crosslinking agent onto the surface of the obtained molded article is unlikely to occur, and the 4-methyl-1-pentene copolymer composition exhibits excellent crosslinking properties.

[0050] Examples of crosslinking agents include sulfur-based compounds, organic peroxides, phenolic resins, hydrosilicone-based compounds, amino resins, quinone or its derivatives, amine-based compounds, azo-based compounds, epoxy-based compounds, isocyanates, and quinone dioxime-based crosslinking agents such as p-quinone dioxime. Of these crosslinking agents, sulfur-based compounds, organic peroxides, and phenolic resins are preferred.

[0051] When the crosslinking agent is an organic peroxide, examples thereof include dicumyl peroxide, di-tert-butyl peroxide, 2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxyisopropyl)benzene, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, n-butyl-4,4-bis(tert-butylperoxy)valerate, benzoyl peroxide, p-chlorobenzoyl peroxide, 2,4-dichlorobenzoyl peroxide, tert-butylperoxybenzoate, tert-butylperoxyisopropyl carbonate, diacetyl peroxide, lauroyl peroxide, and tert-butylcumyl peroxide.

[0052] When an organic peroxide is used as the crosslinking agent, the 4-methyl-1-pentene copolymer composition preferably contains a crosslinking aid, which will be described later. The amount of the crosslinking aid is preferably 0.5 to 10 mol, more preferably 0.5 to 7 mol, and even more preferably 1 to 5 mol, per mol of the organic peroxide.

[0053] When the crosslinking agent is a sulfur-based compound, examples thereof include sulfur, sulfur chloride, sulfur dichloride, morpholine disulfide, alkylphenol disulfide, tetramethylthiuram disulfide, and selenium dithiocarbamate. Although sulfur is not a compound, it is conveniently classified as a sulfur-based compound in this specification.

[0054] When a sulfur-based compound is used as a crosslinking agent, the 4-methyl-1-pentene copolymer composition preferably contains a vulcanization accelerator. Specific examples of the vulcanization accelerator include thiazole-based accelerators such as N-cyclohexyl-2-benzothiazole sulfenamide (CBS) (for example, "Noccela NS" (trade name; manufactured by Ouchi Shinko Co., Ltd.)), N-oxydiethylene-2-benzothiazole sulfenamide, N,N'-diisopropyl-2-benzothiazole sulfenamide, 2-mercaptobenzothiazole (for example, "Suncerer M" (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(4-morpholinodithio)benzothiazole (for example, "Noccela MDB-P" (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, 2-(2,6-diethyl-4-morpholinothio)benzothiazole, and dibenzothiazyl disulfide; guanidine-based accelerators such as diphenyl guanidine, triphenyl guanidine, and diorthotolyl guanidine; Aldehyde amine-based compounds such as acetaldehyde-aniline condensates and butylaldehyde-aniline condensates; imidazoline-based compounds such as 2-mercaptoimidazoline; thiourea-based compounds such as diethylthiourea and dibutylthiourea; thiuram-based compounds such as tetramethylthiuram monosulfide and tetramethylthiuram disulfide (TMTD) (for example, "Noccela TT" (trade name; manufactured by Ouchi Shinko Co., Ltd.)); dithioacid salt-based compounds such as zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate (ZnBDC) (for example, "Suncera Bz" (trade name; manufactured by Sanshin Chemical Industry Co., Ltd.)) and tellurium diethyldithiocarbamate; thiourea-based compounds such as ethylenethiourea, N,N'-diethylthiourea, N,N'-dibutylthiourea; and xanthate-based compounds such as zinc dibutylxatogenate.

[0055] When a sulfur-based compound is used as the crosslinking agent, the 4-methyl-1-pentene copolymer composition preferably contains a vulcanization accelerator.

[0056] The vulcanization accelerator aid can be appropriately selected depending on the application, and can be used alone or in combination of two or more. Specific examples of the vulcanization accelerator aid include magnesium oxide and zinc oxide (for example, zinc oxide such as "Zinc Oxide Type 2" (trade name; manufactured by Hakusui Tech Co., Ltd.)).

[0057] <Crosslinking Auxiliary Agent> The crosslinking auxiliary agent is a compound that acts as a crosslinking reaction catalyst when blended together with a crosslinking agent when the 4-methyl-1-pentene copolymer composition is crosslinked by heating. On the other hand, when the 4-methyl-1-pentene copolymer composition is crosslinked by electron beam crosslinking, the crosslinking auxiliary agent may be used alone. As with the above-mentioned crosslinking agent, when the 4-methyl-1-pentene copolymer composition is crosslinked by electron beam crosslinking, the 4-methyl-1-pentene copolymer composition may or may not contain a crosslinking auxiliary.

[0058] In addition, when the 4-methyl-1-pentene copolymer composition is crosslinked by heating, the 4-methyl-1-pentene copolymer composition preferably contains a crosslinking aid. The crosslinking aid may be used alone or in combination of two or more.

[0059] The content of the crosslinking aid is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably less than 0.1 parts by mass, and particularly preferably less than 0.01 parts by mass, relative to 100 parts by mass of the 4-methyl-1-pentene copolymer. On the other hand, the lower limit of the content is 0 parts by mass or more, relative to 100 parts by mass of the 4-methyl-1-pentene copolymer. When the content of the crosslinking aid is within the above range, bleeding of the crosslinking aid onto the surface of the obtained molded article is unlikely to occur, and the 4-methyl-1-pentene copolymer composition exhibits excellent crosslinking properties.

[0060] The crosslinking aid is not particularly limited as long as the object of the present invention is achieved, but examples thereof include acrylic crosslinking aids such as ethylene glycol dimethacrylate and trimethylolpropane trimethacrylate; allyl crosslinking aids such as diallyl phthalate and triallyl isocyanurate; other maleimide crosslinking aids; and divinylbenzene. Among these, allyl crosslinking aids are preferred, and triallyl isocyanurate is more preferred.

[0061] Furthermore, in addition to the crosslinking aids exemplified above, the crosslinking aid (P) described in detail below can be used. A 4-methyl-1-pentene copolymer composition containing the crosslinking aid (P) can suppress blocking of the 4-methyl-1-pentene copolymer and can also suppress bleeding of the crosslinking aid.

[0062] Crosslinking Coagent (P) The crosslinking coagent (P) is a compound containing two or more cyclic structures represented by the following formula (1) in one molecule.

[0063]

[0064] A preferred example of the crosslinking aid (P) is a polymer of a compound represented by the following formula (2).

[0065] (In formula (2), R 1 ~R 3 are each independently an allyl-based substituent selected from an allyl group, a methallyl group, an allyl group via an ester bond, and a methallyl group via an ester bond.

[0066] The crosslinking aid (P) may, for example, be triallyl isocyanate prepolymer.

[0067] <Other Components> The 4-methyl-1-pentene copolymer composition according to the present invention may further contain other components (hereinafter referred to as "other components") that do not fall under any of the 4-methyl-1-pentene copolymer, the crosslinking agent, and the crosslinking aid. Examples of other components include resins other than the 4-methyl-1-pentene copolymer, and additives other than the crosslinking agent and the crosslinking aid.

[0068] Resins Other Than 4-Methyl-1-Pentene Copolymers The 4-methyl-1-pentene copolymer composition according to the present invention may contain resins other than the 4-methyl-1-pentene copolymers, and the amount of these resins added is preferably 0.1 to 30% by mass relative to the total mass of the 4-methyl-1-pentene copolymer composition.

[0069] Examples of resins other than 4-methyl-1-pentene copolymers include thermoplastic resins such as thermoplastic polyolefin resins other than 4-methyl-1-pentene copolymers, thermoplastic polyamide resins, thermoplastic polyester resins, and thermoplastic vinyl aromatic resins, as well as thermosetting resins such as unsaturated polyester resins, epoxy resins, phenol resins, urea resins, melamine resins, diallyl phthalate resins, and silicone resins. One of the above resins can be used alone, or two or more can be used in combination.

[0070] Additives other than crosslinking agent and crosslinking aid The 4-methyl-1-pentene copolymer composition according to the present invention may contain additives other than the crosslinking agent and crosslinking aid. The total content of these additives can be determined depending on the application within a range that does not impair the object of the present invention, and is not particularly limited, but is preferably 0.1 to 30 mass% with respect to the total mass of the 4-methyl-1-pentene copolymer composition.

[0071] Examples of additives other than the crosslinking agent and the crosslinking aid include weather stabilizers, heat stabilizers, antioxidants, ultraviolet absorbers, antistatic agents, antislip agents, antiblocking agents, antifogging agents, nucleating agents, lubricants, pigments, dyes, antioxidants, hydrochloric acid absorbers, inorganic or organic fillers, organic or inorganic foaming agents, adhesives, softeners, and flame retardants. These additives can be used alone or in combination of two or more.

[0072] <Method for Preparing 4-Methyl-1-pentene Copolymer Composition> The method for preparing the 4-methyl-1-pentene copolymer composition according to the present invention is not particularly limited. For example, the 4-methyl-1-pentene copolymer and other components are mixed in the above-mentioned addition ratio, followed by melt-kneading to obtain the 4-methyl-1-pentene copolymer composition.

[0073] The melt-kneading method is not particularly limited, and the melt-kneading can be carried out using a melt-kneading device such as a commercially available extruder.

[0074] For example, the cylinder temperature of the kneading section of the kneader is usually 220 to 320°C, preferably 250 to 300°C. If the cylinder temperature is lower than 220°C, kneading will be insufficient due to insufficient melting, and improvement in the physical properties of the 4-methyl-1-pentene copolymer composition will be difficult to achieve. On the other hand, if the temperature is higher than 320°C, thermal decomposition of the 4-methyl-1-pentene copolymer may occur. The kneading time is usually 0.1 to 30 minutes, particularly preferably 0.5 to 5 minutes. If the kneading time is less than 0.1 minute, sufficient melt-kneading will not be achieved, and if the kneading time exceeds 30 minutes, thermal decomposition of the 4-methyl-1-pentene copolymer may occur.

[0075] The 4-methyl-1-pentene copolymer composition according to the present invention is a crosslinkable composition, and the composition after crosslinking is referred to as a crosslinked 4-methyl-1-pentene copolymer composition. The crosslinked 4-methyl-1-pentene copolymer composition will be described in detail below.

[0076] [Crosslinked 4-methyl-1-pentene copolymer composition and production method thereof] A crosslinked 4-methyl-1-pentene copolymer composition (hereinafter also simply referred to as "crosslinked composition") is obtained by crosslinking the 4-methyl-1-pentene copolymer composition. That is, the crosslinked composition has a crosslinked structure formed by crosslinking molecules of the 4-methyl-1-pentene copolymer with each other.

[0077] The crosslinked composition can be obtained by crosslinking the 4-methyl-1-pentene copolymer composition. In a preferred embodiment of the present invention, the crosslinked composition can be obtained by a production method including a step of crosslinking the 4-methyl-1-pentene copolymer composition by irradiation.

[0078] The radiation that can be used for the radiation irradiation may be any radiation that can crosslink the 4-methyl-1-pentene copolymer composition, and examples thereof include electromagnetic waves such as X-rays, γ-rays, α-rays, and β-rays, and electron beams. Of these, electron beams are preferred.

[0079] The acceleration voltage of the electron beam can be appropriately selected depending on the composition of the 4-methyl-1-pentene copolymer composition, the size and shape of the molded article, etc. For example, in the case of a molded article having a thickness of about 2 mm, an acceleration voltage of 500 to 1000 kV is preferred. The absorbed dose during electron beam irradiation can be appropriately set depending on the composition of the 4-methyl-1-pentene copolymer composition, but is preferably 50 to 800 kGy from the viewpoint of efficient crosslinking. The electron beam source is not particularly limited, and various electron beam accelerators such as Cockcroft-Walton type, Van de Graaf type, resonant transformer type, insulating core transformer type, linear type, dynamitron type, and high frequency type can be used.

[0080] In another preferred embodiment of the present invention, the method for producing a crosslinked composition preferably includes a step (SA-1) of molding the 4-methyl-1-pentene copolymer composition by compression molding or other appropriate molding method before the radiation irradiation.

[0081] [Molded Article] The molded article according to the present invention contains the 4-methyl-1-pentene copolymer or the 4-methyl-1-pentene copolymer composition. In a typical embodiment of the present invention, the crosslinked 4-methyl-1-pentene copolymer composition is used in the form of a molded article. In other words, the molded article according to the present invention contains the crosslinked composition.

[0082] (1) Thermal Properties The decomposition temperature Td (temperature at which the weight is reduced by 5%) of the molded article according to the present invention, as measured by thermogravimetric analysis (TGA), is preferably 260°C or higher, more preferably 275°C or higher, and even more preferably 280°C or higher. When the decomposition temperature Td is 260°C or higher, molecular chains are less likely to break and harmful gases are less likely to be generated even when used in high-temperature ranges. Details of the method for measuring the decomposition temperature Td are as described in the Examples. The upper limit of the decomposition temperature Td is not particularly limited, but can be set to, for example, 500°C or lower. The decomposition temperature Td can be adjusted by the content of the structural unit (B) in the 4-methyl-1-pentene copolymer of the present invention, the type of monomer that derives the structural unit (B), and the type and content of the crosslinking agent and crosslinking aid in the 4-methyl-1-pentene copolymer composition.

[0083] (2) Production Method The production method of the molded article according to the present invention is not particularly limited. In a preferred embodiment of the present invention, the molded article can be obtained by a production method including: (SA-1) a step of molding the 4-methyl-1-pentene copolymer composition; and (SA-2) a step of irradiating the precursor molded article obtained by the step (SA-1). In this aspect, the "step of crosslinking the 4-methyl-1-pentene copolymer composition by irradiation" described above in [Crosslinked 4-methyl-1-pentene copolymer composition and production method thereof] is carried out as the step (SA-2).

[0084] For example, when the molded article is in the form of a film, the step (SA-1) can be carried out using a molding method commonly used for film molding, and may be a known film molding method. When the molded article has the shape of a laminated film, the step (SA-1) can be carried out using a molding method commonly used for producing laminated films.

[0085] The molded article according to the present invention is not limited to those produced by the above-described embodiment, and may be obtained, for example, by a production method including: (SB-1) a step of crosslinking the 4-methyl-1-pentene copolymer composition by irradiation with radiation; and (SB-2) a step of molding the 4-methyl-1-pentene copolymer composition crosslinked in the step (SB-1).

[0086] (3) Shape The shape of the molded product is not particularly limited. For example, it may be a tube, film, sheet, membrane, tape, plate, rod, fiber, or nonwoven fabric. The molded product may also be a laminate such as a laminated film.

[0087] (4) Applications The molded article according to the present invention can be used without restriction in applications in which conventional 4-methyl-1-pentene copolymers can be used, but is more suitable for applications requiring heat resistance, such as high-temperature release films, oven-safe containers, semiconductor sealing films, automotive parts, raw materials for fibers, automotive radomes, heat-sealing materials, electrical cable tubes, rubber substitute materials, processing aids (substrate modifiers / liquid crystal reflectors), rubber modifiers, and aerospace-related parts.

[0088] [Resin Film] A resin film according to one embodiment of the present invention is obtained by mixing the above-described 4-methyl-1-pentene copolymer with other components as necessary, melting the 4-methyl-1-pentene copolymer, and molding the mixture into a film. The thickness of the resin film is usually 5 to 5,000 μm. As the other components, the above-described crosslinking agent, crosslinking aid, and components listed in the <Other Components> section can be used.

[0089] [Laminate] A laminate according to one embodiment of the present invention comprises a film containing the above-mentioned 4-methyl-1-pentene copolymer and a fiber substrate.

[0090] <Fiber Substrate> The fiber substrate contains at least one type of fiber selected from the group consisting of inorganic fibers and organic fibers.

[0091] Examples of inorganic fibers include glass fibers, asbestos fibers, carbon fibers, silica fibers, silica-alumina fibers, alumina fibers, zirconia fibers, potassium titanate fibers, Tyranno fibers, and silicon carbide fibers, as well as metal fibers such as amorphous metal fibers, stainless steel fibers, superelastic NT (nickel-titanium) alloy wires, and titanium wires. Examples of organic fibers include ultra-high molecular weight polyethylene fibers, polyacetal fibers, aliphatic or aromatic polyamide fibers, polyarylate fibers, fluorine fibers, boron fibers, polyacrylonitrile fibers, and aramid fibers. These fibers can be used alone or in combination of two or more.

[0092] Among these fibers, inorganic fibers, particularly glass fibers, are preferred in terms of heat resistance and mechanical strength. Furthermore, the type of glass fiber is not particularly limited, and any glass fiber such as E-glass, C-glass, S-glass, D-glass, NE-glass, T-glass, Q-glass, ECR-glass, A-glass, or AR-glass can be used. The average diameter of the fiber is, for example, 0.1 to 100 μm, preferably 0.5 to 50 μm, more preferably 1 to 30 μm, and particularly preferably about 1 to 10 μm. The basis weight of the fiber substrate is, for example, 1 to 200 g / m 2 , preferably 5 to 150 g / m 2 , more preferably 10 to 100 g / m 2 , particularly preferably 20 to 80 g / m 2 If the basis weight is too small, the strength of the fiber base material will be insufficient.

[0093] In a preferred embodiment of the present invention, the glass fiber substrate is preferably glass cloth. The glass cloth is woven with warp and weft threads, each thread being made by twisting together several tens to several hundreds of glass threads (filaments) with a diameter of about 5 to 15 μm. The thickness of the glass cloth is preferably about 30 μm to 190 μm.

[0094] Examples of such glass cloths that can be used include "E15A04 (product name)" (manufactured by Unitika Ltd., thickness 120 μm) and "WEA18T" (manufactured by Nitto Boseki Co., Ltd., thickness 190 μm). One or more such glass cloths may be laminated for use. In addition to glass fibers, the glass cloth may contain a binder, a surface treatment agent that improves adhesion between the glass fibers and the binder, synthetic fibers, etc.

[0095] Examples of such glass cloths that can be used include "Grabest (trade name)" (manufactured by Olivest Co., Ltd., fiber diameter 6 to 20 μm, fiber length 6 to 38 mm) and "Surface Mat (trade name)" (manufactured by Nitto Boseki Co., Ltd.). One or more such glass cloths may be used in a laminated form.

[0096] The ratio of the resin film to the fiber substrate in the laminate is not particularly limited, but it is preferable to adjust the ratio of the fiber substrate to 10 to 60% by mass. This is particularly suitable for applications such as prepregs. If the ratio of the fiber substrate in the laminate is less than 10% by mass, a substrate with sufficient strength tends to be obtained, and if it exceeds 60% by mass, a substrate with satisfactory dielectric properties tends to be obtained. There is no limit to the thickness of the laminate, but it is usually 5 mm to 10 cm.

[0097] <Uses> The laminate can be used for various purposes. In addition, the laminate can be used by laminating another layer, such as a conductor layer of copper or aluminum, on the laminate by a method such as film formation, sputtering, vapor deposition, or plating.

[0098] [Method for Producing Laminate] The method for producing a laminate of the present invention includes the steps of: laminating a molded article containing a 4-methyl-1-pentene copolymer, the molded article comprising a structural unit (A) derived from 4-methyl-1-pentene and a structural unit (B) derived from at least one monomer selected from the group consisting of a symmetric diene, an asymmetric diene, and an allylic-substituted olefin, and a fibrous substrate containing at least one type of fiber selected from inorganic fibers and organic fibers so that the molded article and a fibrous substrate are in contact with each other, and heating the laminate to a temperature of 230 to 350°C; and crosslinking the 4-methyl-1-pentene copolymer.

[0099] The method for producing a laminate of the present invention includes a step of laminating the above-mentioned molded article (e.g., a resin film) and a fibrous substrate so that they are in contact with each other. In this step, the resin film and the fibrous substrate are superimposed and heated to integrate them. During integration, it is preferable to apply pressure simultaneously with heating. Multiple resin films and fibrous substrates are used so that they are sandwiched between each other, typically 2 to 16 sheets of each. Heating is typically performed at 230 to 350°C. Pressurization is typically performed at 1.0 to 10 MPa. This heating, and further pressurization, melts at least a portion of the 4-methyl-1-pentene copolymer in the resin film and impregnates between the fibers of the fibrous substrate, thereby integrating the resin film and the fibrous substrate (impregnation step). In this step, heating may be performed after laminating the resin film and the fibrous substrate, or the resin film and the fibrous substrate may be laminated after heating. However, heating is preferably performed after laminating the resin film and the fibrous substrate.

[0100] The step of crosslinking the 4-methyl-1-pentene copolymer can employ the methods described above in [Crosslinked 4-methyl-1-pentene copolymer composition and method for producing the same].

[0101] Furthermore, the method for producing a laminate of the present invention preferably includes, in addition to the above steps, a step of producing a 4-methyl-1-pentene copolymer. The step of producing the 4-methyl-1-pentene copolymer can employ the methods described above in <Method for preparing a 4-methyl-1-pentene copolymer composition>. The method for producing a laminate of the present invention preferably includes, in addition to the above steps, a step of producing a molded article containing the 4-methyl-1-pentene copolymer. The step of producing the molded article containing the 4-methyl-1-pentene copolymer can employ the methods described above in (2) Production method in the [Molded article] section.

[0102] The present disclosure will be described in more detail below with reference to examples and comparative examples, but the present disclosure is not limited thereto. Note that the number of parts in the examples and comparative examples is by mass unless otherwise specified.

[0103] Evaluation of polymers, compositions, and molded articles [Monomer composition measurement] The contents of structural units derived from the monomers 4-methyl-1-pentene, symmetric dienes, asymmetric dienes, and allylic olefins were measured using the following apparatus and conditions: 13 Calculated from the C-NMR spectrum.

[0104] A Bruker Biospin AVANCE III cryo-500 nuclear magnetic resonance spectrometer was used. The solvent was a mixed solvent of o-dichlorobenzene / benzene-d6 (volume ratio 4 / 1), the sample concentration was 60 mg / 0.6 mL, the measurement temperature was 120 °C, and the observed nuclei were 13 Measurements were performed with a C (125 MHz) sequence using single-pulse proton broadband decoupling, a pulse width of 5.0 μs (45° pulse), a repetition time of 5.5 s, and 128 integrations, with 128 ppm of benzene-d as the reference value for chemical shift. The content of structural units derived from comonomers was calculated using the integral value of the main-chain methine signal according to the following formula:

[0105] Content (%) of structural units derived from comonomers = [P / (P+M)] × 100, where P represents the total peak area of ​​comonomer main chain methine signals, and M represents the total peak area of ​​4-methyl-1-pentene main chain methine signals.

[0106] [Measurement of intrinsic viscosity [η]] The intrinsic viscosity [η] was measured at 135 ° C. using decalin solvent. Specifically, approximately 20 mg of sample was dissolved in 15 mL of decalin, and the specific viscosity ηsp was measured in an oil bath at 135 ° C. After diluting this decalin solution with 5 mL of decalin solvent, the specific viscosity ηsp was measured in the same manner. This dilution operation was repeated two more times, and the value of ηsp / C when the concentration (C) was extrapolated to 0 was calculated as the intrinsic viscosity (see the formula below). [η] = lim(ηsp / C) (C → 0)

[0107] [Melt Point (Tm) Measurement] An exothermic / endothermic curve was obtained using a Seiko Instruments Inc. DSC measuring device (DSC220C), and the temperature at the maximum melting peak during heating was taken as the melting point (Tm). The measurement was performed as follows. Approximately 5 mg of a sample was cut out from a 0.5 mm thick press sheet, placed in an aluminum pan for measurement, heated from 20°C to 280°C at a heating rate of 10°C / min, held at 280°C for 5 minutes, cooled to 20°C at a cooling rate of 10°C / min, held at 20°C for 5 minutes, then heated again from 20°C to 280°C at a heating rate of 10°C / min, and cooled again to 50°C at a cooling rate of 50°C / min. The melting peak that appeared during the second heating was taken as the melting point (Tm). If multiple melting peaks appeared during the second heating, it was considered that multiple melting points were observed, and in the following description, the multiple melting points were written together as "XX°C / YY°C".

[0108] Synthesis Example 1 (8-octamethylfluoren-12′-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride was synthesized according to the method described in Preliminary Experiment 5 of WO 2014 / 123212.

[0109] Synthesis Example 2 Production of Olefin Polymerization Catalyst A 200 mL three-necked flask equipped with a stirrer and thoroughly purged with nitrogen was charged at 30°C under a nitrogen stream with 30 mL of purified decane and 14.65 mmol, in terms of aluminum atoms, of particulate solid polymethylaluminoxane (synthesized using the method described in WO 2014 / 123212 ) having a median diameter D50 of 28 μm in volume statistics and an aluminum atom content of 43 mass % (hereinafter also referred to as “solid MAO”) to form a suspension. To this suspension was added 50.0 mg (0.0586 mmol) of the transition metal compound (8-octamethylfluoren-12'-yl-(2-(adamantan-1-yl)-8-methyl-3,3b,4,5,6,7,7a,8-octahydrocyclopenta[a]indene))zirconium dichloride described in Synthesis Example 1 as a 4.58 mmol / L toluene solution with stirring. After 1 hour, stirring was stopped, and the resulting mixture was washed with 100 mL of decane by decantation, followed by addition of decane to make 50 mL of a slurry (Zr loading rate: 98%). Note that the "Zr loading rate" refers to the proportion (by mass) of Zr atoms loaded on the solid catalyst component out of the Zr atoms in the added transition metal compound.

[0110] Synthesis Example 3 Preparation of Prepolymerized Catalyst Component To the slurry liquid prepared in Synthesis Example 2, 1.0 mL of a decane solution of diisobutylaluminum hydride (hereinafter referred to as DIBAL-H) ​​(0.5 mol / L in terms of aluminum atom) was charged under a nitrogen stream at 25°C. After cooling to 15°C, 10 mL of 4-methyl-1-pentene was charged into the reactor over 60 minutes. The start of the charging was defined as the start of prepolymerization. 2.0 hours after the start of polymerization, stirring was stopped, and the resulting mixture was washed three times with 100 mL of decane by decantation. A decane slurry (9.5 g / L, 0.56 mmol / L in terms of zirconium atom) was used as the prepolymerized catalyst component.

[0111] Synthesis Example 4 Production of Olefin Polymerization Catalyst and Preparation of Prepolymerized Catalyst Component A solid titanium catalyst component was prepared in the same manner as in Example 1 described in WO 2006 / 054613. The solid titanium catalyst component was then prepolymerized in the same manner as in Example 3 described in WO 2006 / 054613 to obtain a prepolymerized solid titanium catalyst component.

[0112] Example 1-1 Preparation of Polymer 1 At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After reaching 40°C, 0.8 mL (0.4 mmol in terms of aluminum atom) of a decane solution of DIBAL-H was added, followed by 0.00075 mmol in terms of zirconium atom of the decane slurry of the prepolymerized catalyst component of Synthesis Example 3 prepared previously. 35 mL of hydrogen was then added, followed by a mixed solution of 239 mL of 4-methyl-1-pentene and 13 mL of 7-methyl-1,6-octadiene (hereinafter also referred to as MOD) being continuously charged into the polymerization vessel at a constant rate over 2 hours. The start of this charging marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 35 mL of hydrogen was added one hour and two hours after the start of polymerization, respectively. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 1. The yield was 148 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 1 was 95.6 mol%, and the content of structural units derived from MOD was 4.4 mol%. The melting point (Tm) of Polymer 1 was 209°C / 217°C, and the intrinsic viscosity [η] was 1.99 dL / g.

[0113] <Preparation of Measurement Samples> (Preparation of Press Sheet) A powder sample of polymer 1 was processed using a vacuum press molding machine manufactured by Kansai Roll Co., Ltd. After placing aluminum sheet / polyimide film / spacer / sample / spacer / polyimide film / aluminum sheet between press plates in this order, the sample was vacuumed at 250°C for 7 minutes, preheated at 250°C and 2.5 MPa for 3 minutes, and defoamed 20 times. The spacer size was 80 mm x 80 mm x 0.5 mmt, and the sample weight was approximately 3.1 g. The polyimide film used was Upilex manufactured by UBE Corporation. The sample was then heated and pressurized at 250°C and 10 MPa for 3 minutes, and cooled at 20°C and 10 MPa for 4 minutes to obtain a press sheet.

[0114] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under the conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy or 500kGy in air, or without irradiation with an electron beam, to obtain a sample for physical property measurement.

[0115] Example 1-2 Preparation of Composition 1 A powder sample of Polymer 1 was kneaded with triallyl isocyanurate (5 parts by mass per 100 parts by mass of Polymer 1; 5 phr) as a crosslinking aid using a KZW-15 (screw diameter 15 mm, L / D = 30) manufactured by Technovel Corporation at a set temperature of 270°C, a resin extrusion rate of 1.4 kg / h, a rotation speed of 200 rpm, and under N2, to obtain Composition 1.

[0116] <Production of Measurement Sample> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that the powder sample of Polymer 1 was changed to Composition 1.

[0117] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under the conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy or 500kGy in air to obtain a sample for physical property measurement.

[0118] Example 1-3 Preparation of Polymer 2 At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After reaching 40°C, 0.8 mL (0.4 mmol in terms of aluminum atom) of a decane solution of DIBAL-H was charged, followed by 0.00075 mmol in terms of zirconium atom of the decane slurry of the prepolymerized catalyst component of Synthesis Example 3 prepared previously. 35 mL of hydrogen was charged, and then a mixed solution of 246 mL of 4-methyl-1-pentene and 6.5 mL of MOD was continuously charged into the polymerization vessel at a constant rate over 2 hours. The start of this charging marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 35 mL of hydrogen was charged one hour and two hours after the start of polymerization, respectively. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 2. The yield was 149 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 2 was 97.9 mol%, and the content of structural units derived from MOD was 2.1 mol%. The melting point (Tm) of Polymer 2 was 222°C / 228°C, and the intrinsic viscosity [η] was 1.85 dL / g.

[0119] <Production of Measurement Samples> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that the powdered sample of polymer 2 was used instead of the powdered sample of polymer 1.

[0120] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under the conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy or 500kGy in air, or without irradiation with an electron beam, to obtain a sample for physical property measurement.

[0121] [Example 1-4] <Preparation of Polymer 3> At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After reaching 40°C, 0.8 mL (0.4 mmol in terms of aluminum atom) of a decane solution of DIBAL-H was charged, followed by 0.00075 mmol in terms of zirconium atom of the decane slurry of the prepolymerized catalyst component of Synthesis Example 3 prepared previously. 35 mL of hydrogen was charged, and then a mixed solution of 232 mL of 4-methyl-1-pentene and 20 mL of 4-vinyl-1-cyclohexene (hereinafter also referred to as VCH) was continuously charged into the polymerization vessel at a constant rate over 2 hours. The start of this charging marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 35 mL of hydrogen was charged one hour and two hours after the start of polymerization, respectively. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 3. The yield was 129 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 3 was 99.2 mol%, and the content of structural units derived from VCH was 0.8 mol%. The melting point (Tm) of Polymer 3 was 238°C / 240°C, and the intrinsic viscosity [η] was 1.42 dL / g.

[0122] <Production of Measurement Samples> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that the powdered sample of Polymer 3 was used instead of the powdered sample of Polymer 1.

[0123] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 500kGy in air to obtain a sample for physical property measurement.

[0124] Example 1-5 Preparation of Polymer 4 At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After the temperature reached 40°C, 0.8 mL (0.4 mmol in terms of aluminum atom) of a decane solution of DIBAL-H was charged, followed by 0.00075 mmol in terms of zirconium atom of the decane slurry of the prepolymerized catalyst component of Synthesis Example 3 prepared previously. 35 mL of hydrogen was charged, and then a mixed solution of 249 mL of 4-methyl-1-pentene and 3.3 mL of MOD was continuously charged into the polymerization vessel at a constant rate over 2 hours. The start of this charging marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 35 mL of hydrogen was charged one hour and two hours after the start of polymerization, respectively. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 4. The yield was 147 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 4 was 99.0 mol%, and the content of structural units derived from MOD was 1.0 mol%. The melting point (Tm) of Polymer 4 was 233°C, and the intrinsic viscosity [η] was 1.70 dL / g.

[0125] <Preparation of Composition 2> A powder sample of Polymer 4 was kneaded with triallyl isocyanurate (5 parts by mass per 100 parts by mass of Polymer 4; 5 phr) as a crosslinking aid using a KZW-15 (screw diameter 15 mm, L / D = 30) manufactured by Technovel Corporation at a set temperature of 270°C, a resin extrusion rate of 1.4 kg / h, a rotation speed of 200 rpm, and under N2, to obtain Composition 2.

[0126] <Production of Measurement Sample> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that the powder sample of Polymer 1 was changed to Composition 2.

[0127] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 500kGy in air to obtain a sample for physical property measurement.

[0128] Example 1-6 Preparation of Polymer 5 At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After the temperature reached 40°C, 0.64 mL (0.32 mmol in terms of aluminum atom) of a decane solution of triethylaluminum (hereinafter referred to as TEAL) was added, followed by 26.5 μmol in terms of titanium atom of the decane slurry of the prepolymerized catalyst component of Synthesis Example 4 prepared previously. 150 mL of hydrogen was then added, and then a mixed solution of 196 mL of 4-methyl-1-pentene and 12 mL of MOD was continuously added to the polymerization vessel at a constant rate over 3 hours. The start of this addition marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 150 mL of hydrogen was added 1.5 hours, 3 hours, and 4.3 hours after the start of polymerization. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 5. The yield was 102 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 5 was 95.0 mol%, and the content of structural units derived from MOD was 5.0 mol%. The melting point (Tm) of Polymer 5 was 219°C / 225°C, and the intrinsic viscosity [η] was 1.91 dL / g.

[0129] <Production of Measurement Samples> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that the powdered sample of Polymer 5 was used instead of the powdered sample of Polymer 1.

[0130] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 500kGy in air, or without irradiating with an electron beam to obtain a sample for physical property measurement.

[0131] [Examples 1-7] <Preparation of Composition 3> A powder sample of Polymer 5 was kneaded with triallyl isocyanurate (5 parts by mass per 100 parts by mass of Polymer 5; 5 phr) as a crosslinking aid using a KZW-15 (screw diameter 15 mm, L / D = 30) manufactured by Technovel Corporation at a set temperature of 270°C, a resin extrusion rate of 1.4 kg / h, a rotation speed of 200 rpm, and under N2, to obtain Composition 3.

[0132] <Production of Measurement Sample> (Production of Press Sheet) A press sheet was obtained in the same manner as in Example 1-1, except that the powder sample of Polymer 5 was changed to Composition 3.

[0133] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 500kGy in air to obtain a sample for physical property measurement.

[0134] [Example 1-8] <Preparation of Polymer 6> At room temperature under a nitrogen stream, 425 mL of purified decane was placed in a 1 L stainless steel polymerization vessel equipped with a stirrer, and the temperature was raised to 40°C. After reaching 40°C, 0.64 mL (0.32 mmol in terms of aluminum atom) of a decane solution of TEAL was charged, followed by 26.5 μmol in terms of titanium atom of a decane slurry of the prepolymerized catalyst component of Synthesis Example 4 prepared previously. 150 mL of hydrogen was charged, and then a mixed solution of 196 mL of 4-methyl-1-pentene and 2.6 mL of MOD was continuously charged into the polymerization vessel at a constant rate over 3 hours. The start of this charging marked the start of polymerization, and the temperature was maintained at 45°C for 4.5 hours. 150 mL of hydrogen was charged 1.5 hours, 3 hours, and 4.3 hours after the start of polymerization. After 4.5 hours from the start of polymerization, the temperature was lowered to room temperature, the pressure was released, and the polymerization liquid containing a white solid was immediately filtered to obtain a solid substance. This solid substance was dried under reduced pressure at 80°C for 8 hours to obtain Polymer 6. The yield was 102 g. The content of structural units derived from 4-methyl-1-pentene in Polymer 6 was 98.8 mol%, and the content of structural units derived from MOD was 1.2 mol%. The melting point (Tm) of Polymer 6 was 233°C, and the intrinsic viscosity [η] was 1.76 dL / g.

[0135] <Preparation of Composition 4> A powder sample of Polymer 6 was kneaded with triallyl isocyanurate (5 parts by mass per 100 parts by mass of Polymer 6; 5 phr) as a crosslinking aid using a KZW-15 (screw diameter 15 mm, L / D = 30) manufactured by Technovel Corporation at a set temperature of 270°C, a resin extrusion rate of 1.4 kg / h, a rotation speed of 200 rpm, and under N2, to obtain Composition 4.

[0136] <Production of Measurement Samples> (Production of Press Sheets) Press sheets of Polymer 6 or Composition 4 were obtained in the same manner as in Example 1-1, except that the powder sample of Polymer 1 was changed to Polymer 6 or Composition 4, respectively.

[0137] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 500kGy in air, or without irradiating with an electron beam to obtain a sample for physical property measurement.

[0138] Comparative Example 1-1 Preparation of Polymer 7 In Example 17 of WO 2006 / 054613, the amounts of 4-methyl-1-pentene, α-olefin, and hydrogen charged were changed so that the physical properties of the resulting copolymer would be as described below, thereby obtaining a 4-methyl-1-pentene / 1-hexadecene / 1-octadecene copolymer (Polymer 7), which is a polymer that does not contain structural unit (B). The content of structural units derived from 4-methyl-1-pentene in Polymer 7 was 97.3 mol %, and the content of structural units derived from comonomers in Polymer 7 was 2.7 mol %. The melting point (Tm) of Polymer 7 was 224°C, and the intrinsic viscosity [η] was 2.79 dL / g.

[0139] <Production of Measurement Samples> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that Polymer 7 was used instead of the powder sample of Polymer 1.

[0140] (Production of Samples for Physical Property Measurement) The above-mentioned press sheet was irradiated with an electron beam using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy or 500kGy in air, or without irradiation with an electron beam, to obtain a sample for physical property measurement.

[0141] [Comparative Example 1-2] <Preparation of Polymer 8> In Example 2A of JP 2021-155486 A, the amounts of 4-methyl-1-pentene, α-olefin, and hydrogen charged were changed so that the physical properties of the resulting copolymer would be as described below, thereby obtaining a 4-methyl-1-pentene / 1-hexadecene / 1-octadecene copolymer (polymer 8), which is a polymer that does not contain structural unit (B). The content of structural units derived from 4-methyl-1-pentene in polymer 8 was 93.9 mol%, and the content of structural units derived from comonomers in polymer 8 was 6.1 mol%. The melting point (Tm) of polymer 8 was 238 ° C., and the intrinsic viscosity [η] was 3.5 dL / g.

[0142] <Production of Measurement Samples> (Production of Pressed Sheet) A pressed sheet was obtained in the same manner as in Example 1-1, except that Polymer 8 was used instead of the powder sample of Polymer 1.

[0143] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with electron beams using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy in air to obtain a sample for physical property measurement.

[0144] Comparative Example 1-3 Preparation of Polymer 9 In Production Example 1 of JP 2018-162408 A, the amounts of 4-methyl-1-pentene, α-olefin, and hydrogen charged were changed so that the physical properties of the resulting copolymer would be as described below, thereby obtaining a 4-methyl-1-pentene / 1-hexadecene / 1-octadecene copolymer (polymer 9), which is a polymer that does not contain structural unit (B). The content of structural units derived from 4-methyl-1-pentene in polymer 9 was 89.5 mol%, and the content of structural units derived from comonomers in polymer 9 was 10.5 mol%. The melting point (Tm) of polymer 9 was 231°C, and the intrinsic viscosity [η] was 2.58 dL / g.

[0145] <Preparation of Composition 5> A powder sample of Polymer 9 was kneaded with triallyl isocyanurate (5 parts by mass per 100 parts by mass of Polymer 9; 5 phr) as a crosslinking aid using a KZW-15 (screw diameter 15 mm, L / D = 30) manufactured by Technovel Corporation at a set temperature of 270°C, a resin extrusion rate of 1.4 kg / h, a rotation speed of 200 rpm, and under N2, to obtain Composition 5.

[0146] <Production of Measurement Samples> (Production of Press Sheets) Press sheets of Polymer 9 or Composition 5 were obtained in the same manner as in Example 1-1, except that the powder sample of Polymer 1 was changed to Polymer 9 or Composition 5, respectively.

[0147] (Production of Sample for Physical Property Measurement) The above-mentioned press sheet was irradiated with electron beams using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 400kGy in air to obtain a sample for physical property measurement.

[0148] [Evaluation] The following evaluations were carried out using the measurement samples obtained in the Examples and Comparative Examples. (Thermal Properties) Decomposition Temperature Td The decomposition temperature Td was measured by thermogravimetric analysis (TGA) using a TGA 5500C manufactured by TA Corporation. The temperature at which the weight decreased by 5% when the temperature was raised from 30°C to 400°C in air at a temperature rise rate of 20°C / min was read as Td. A higher Td indicates a better result.

[0149] Heat resistance rigidity Heat resistance rigidity (elastic modulus in the rubber-like plateau region) was measured in a solid viscoelasticity measurement using an RSA-G2 manufactured by TA Instruments. The elastic modulus was read when the rubber-like plateau region was reached in measurements at a temperature rise rate of 4°C / min, a frequency of 1 Hz, and under N2 at a temperature range of -50°C to 300°C. The fact that this elastic modulus can be read indicates that the polymer is able to maintain a certain level of strength even in a temperature range above the melting point of the polymer, and the larger the value of this elastic modulus, the better the strength that can be maintained. Note that if no numerical value is listed, this means that the elastic modulus cannot be read (uncrosslinked or insufficiently crosslinked).

[0150] (Tensile Properties) Tensile properties were measured using an AG-X-5 manufactured by Shimadzu Corporation. The shape of the test specimen was JIS K7113-2-1 / 2, and the breaking strength, gauge length elongation, and apparent modulus of elasticity were calculated at 23°C and a tensile speed of 50 mm / min. A higher breaking strength value indicates better durability. Furthermore, a gauge length elongation value within the range of 1% to 60% is preferable because it provides a good balance between toughness and rigidity. Furthermore, a higher apparent modulus of elasticity indicates better rigidity.

[0151] (Dielectric Properties) Using a synthesized sweeper and network analyzer manufactured by YHP Corporation, a copper cylindrical cavity resonator with an internal mirror finish, and a semi-rigid cable for signal transmission, the dielectric properties were measured at 10 GHz and 24 GHz in TE mode in accordance with JIS R1641, IEC 62810, etc. A 50 mm square x 0.5 mm thick sheet was used as a test piece, and the measurements were carried out at 23°C. The smaller the relative dielectric constant and dielectric loss tangent, the better the dielectric properties.

[0152] (Degree of Crosslinking) The samples for measuring the degree of crosslinking obtained in Examples 1-1 to 1-8 and Comparative Examples 1-1 to 1-3 were each wrapped in a mesh, shaken and dissolved in 20 mL of o-dichlorobenzene at 145°C for 2 hours, the metal mesh was removed, washed multiple times with o-dichlorobenzene, and the o-dichlorobenzene-insoluble portion remaining in the metal mesh was dried and weighed, and the resulting value was used as the gel fraction, which is an index of the degree of crosslinking. Degree of crosslinking (gel fraction; %) = (mass (mg) of the o-dichlorobenzene-insoluble portion remaining in the metal mesh) / 50 x 100

[0153]

[0154]

[0155] Film and laminate evaluation

[0156] [Production Example 2-1] (Production of Resin Film) A powder sample of Composition 1 was processed using a press manufactured by Shinto Metal Works Co., Ltd. The components were placed between press plates in the following order: aluminum sheet / polyimide film / spacer / sample / polyimide film / aluminum sheet. After preheating at 250°C for 2 minutes, defoaming was performed 20 times. The spacer size was 80 mm x 80 mm x 0.5 mmt, and the sample weight was approximately 3.1 g. The polyimide film used was Upilex manufactured by UBE Corporation. The sample was then heated and pressurized at 250°C and 5.0 MPa for 1.5 minutes, and then cooled at 20°C and 1.0 MPa for 4 minutes to obtain a resin film.

[0157] [Example 2-1] (Production of Glass Cloth Laminate) A laminate was obtained using the above resin film and Featherfield glass cloth (#100, thickness t ≒ 0.096 mm). The laminate structure was 4 plies (thickness t ≒ 0.500 mm) consisting of resin film / glass cloth / resin film / glass cloth / resin film / glass cloth / resin film / glass cloth / resin film, with one glass cloth layer being considered as 1 ply (lamination unit). The laminate was placed between press plates in the order of aluminum sheet / polyimide film / laminate / polyimide film / aluminum sheet, and then heated and pressurized at 230 ° C. and 1.0 MPa for 5 minutes (impregnation step), followed by cooling at 20 ° C. and 1.0 MPa for 4 minutes to obtain a glass cloth laminate. This glass cloth laminate was irradiated with electron beams using an electron beam irradiation device EPS-750kV manufactured by NHV Corporation under the conditions of an acceleration voltage of 500kV and an electron beam irradiation intensity of 200kGy or 500kGy in air to obtain a glass cloth laminate for measuring physical properties.

[0158] Example 2-2 A glass cloth laminate was produced in the same manner as in Example 2-1, except that the temperature in the impregnation step during the production of the glass cloth laminate was set to 250°C.

[0159] [Example 2-3] A resin film was produced by the same method as in Production Example 2-1 (Production of resin film) using Polymer 1 instead of Composition 1, and a glass cloth laminate was produced by the same method as in Example 2-1 (Production of glass cloth laminate), except that the temperature in the impregnation step during production of the glass cloth laminate was set to 280°C.

[0160] Example 2-4 A glass cloth laminate was produced in the same manner as in Example 2-1, except that the temperature in the impregnation step during the production of the glass cloth laminate was set to 280°C.

[0161] Example 2-5 A glass cloth laminate was produced in the same manner as in Example 2-1, except that the temperature in the impregnation step during the production of the glass cloth laminate was set to 310°C.

[0162] Example 2-6 A glass cloth laminate was produced in the same manner as in Example 2-1, except that the temperature in the impregnation step during the production of the glass cloth laminate was set to 340°C.

[0163] Comparative Examples 2-1 and 2-2 Using the polymer 7 obtained in Comparative Example 1-1, a resin film was produced in the same manner as in Production Example 2-1 (production of resin film).

[0164] [Evaluation] The following evaluations were performed using the resin films obtained in the examples and comparative examples. (Thermal Properties) - Heat Resistance Rigidity Heat resistance rigidity (elastic modulus in the rubber-like plateau region) was measured by solid viscoelasticity measurement using an RSA-G2 manufactured by TA Instruments. Measurements were taken from -50°C to 300°C at a temperature rise rate of 4°C / min, a frequency of 1 Hz, and under N2, and the elastic modulus was read at 288°C, which is assumed to be solder heat resistance. Since this temperature is above Tm, the fact that this elastic modulus can be read indicates that the polymer is able to maintain a certain level of strength even in a temperature range above the melting point of the polymer, and the higher the elastic modulus value, the better the retained strength. Note that if a numerical value is not listed, it means that the elastic modulus cannot be read (uncrosslinked or insufficiently crosslinked).

[0165] (Dielectric Properties) Using a synthesized sweeper and network analyzer manufactured by YHP Corporation, a copper cylindrical cavity resonator with an internal mirror finish, and a semi-rigid cable for signal transmission, the dielectric properties were measured at 10 GHz and 24 GHz in TE mode in accordance with JIS R1641, IEC 62810, etc. A 50 mm square x 0.5 mm thick sheet was used as a test piece, and the measurements were carried out at 23°C. The smaller the relative dielectric constant and dielectric loss tangent, the better the dielectric properties.

[0166]

[0167] In Table 2, "Not yet" indicates that data has not been obtained.

Claims

1. A 4-methyl-1-pentene copolymer comprising: a structural unit (A) derived from 4-methyl-1-pentene; and a structural unit (B) derived from at least one monomer selected from the group consisting of symmetric dienes, asymmetric dienes, and allylic-substituted olefins.

2. The 4-methyl-1-pentene copolymer according to claim 1, wherein the structural unit (B) comprises a structural unit derived from at least one monomer selected from the group consisting of asymmetric dienes and allylic-substituted olefins.

3. The 4-methyl-1-pentene copolymer according to claim 1, wherein the structural unit (B) includes a structural unit derived from at least one monomer selected from the group consisting of 7-methyl-1,6-octadiene and 4-vinyl-1-cyclohexene.

4. The 4-methyl-1-pentene copolymer according to claim 1, wherein the content of the structural unit (A) derived from 4-methyl-1-pentene is 90.0 to 99.9 mol %, and the content of the structural unit (B) is 0.1 to 10.0 mol %, when the total content of the structural unit (A) and the structural unit (B) is 100 mol %.

5. A 4-methyl-1-pentene copolymer composition comprising: the 4-methyl-1-pentene copolymer according to any one of claims 1 to 4; and at least one selected from the group consisting of a crosslinking agent and a crosslinking auxiliary, in an amount of 0 to 10 parts by mass per 100 parts by mass of the 4-methyl-1-pentene copolymer.

6. A molded article comprising the 4-methyl-1-pentene copolymer according to any one of claims 1 to 4 or the 4-methyl-1-pentene copolymer composition according to claim 5.

7. The molded article according to claim 6, which is a film.

8. A laminate comprising the film according to claim 7 and a fiber substrate containing at least one type of fiber selected from the group consisting of inorganic fibers and organic fibers.

9. The laminate of claim 8, wherein said fibers are glass fibers.

10. A method for producing a laminate, comprising the steps of: laminating a molded product containing the 4-methyl-1-pentene copolymer according to any one of claims 1 to 4 and a fiber substrate containing at least one type of fiber selected from inorganic fibers and organic fibers so as to be in contact with each other, and heating the laminate to a temperature of 230 to 350°C; and crosslinking the 4-methyl-1-pentene copolymer.

11. The method for producing the laminate according to claim 10, further comprising the step of producing the molded body.

12. The method for producing a laminate according to claim 11, further comprising the step of producing the 4-methyl-1-pentene copolymer.

Citation Information

Patent Citations

  • Copolymers

    GB1002366A

  • Branched alpha-olefin random copolymer and its production

    JP1989129007A

  • Wiper blade rubber molding and its production

    JP1992076034A

  • Molded article of rubber for roll and its production

    JP1992096940A

  • Electrically conductive rubber

    JP1992154856A