Aromatic polyether ketone molded body and method for producing same
The aromatic polyetherketone molded article with a matrix phase and dispersed phase of carbon black or nanotubes achieves both high mechanical strength and elongation in the surface layer and impact absorption in the inner part, enhancing durability and stress resistance, addressing the limitations of existing resin technologies for sliding members.
Patent Information
- Application Number
- PCT/JP2024/010844
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-19
- Publication Date
- 2024-10-03
AI Technical Summary
There is a lack of technology that effectively achieves both high mechanical strength and high elongation in resin molded articles, particularly for sliding members like gear members, where durability and impact absorption are crucial.
An aromatic polyetherketone molded article is developed with a matrix phase composed of aromatic polyetherketone and a dispersed phase of carbon black or carbon nanotubes, where the surface layer has larger crystallite size than the inner portion, enhancing mechanical strength and elongation in the surface layer while maintaining high impact absorption properties in the inner part.
The aromatic polyetherketone molded article achieves high mechanical strength and large elongation in the surface layer, combined with high impact absorption in the inner part, resulting in improved durability and resistance to stress concentration, effectively addressing the limitations of existing technologies.
Smart Images

Figure JP2024010844_03102024_PF_FP_ABST
Abstract
Description
Aromatic polyether ketone molded article and method for producing same
[0001] The present invention relates to an aromatic polyether ketone molded article that can be used for various parts.
[0002] In the field of industrial machinery, there is a demand for replacing metal parts with resin molded bodies from the viewpoint of weight reduction, etc. Patent Document 1 discloses a technique for improving the mechanical strength of resin molded bodies. This technique can improve the mechanical strength of resin molded bodies by increasing the crystallinity of the resin component and restricting the degree of freedom of molecular motion.
[0003] JP 2015-150984 A
[0004] Parts for which resin molded articles are expected to replace metal parts include sliding members such as gear members. For sliding members, high mechanical strength and high elongation are advantageous for improving durability. However, little is known about technologies that can achieve both high mechanical strength and high elongation in resin molded articles.
[0005] In view of the above circumstances, an object of the present invention is to provide an aromatic polyether ketone molded article that has both high mechanical strength and large elongation in the surface layer portion.
[0006] In order to achieve the above object, an aromatic polyether ketone molded article according to one embodiment of the present invention includes a matrix phase and a dispersed phase dispersed in the matrix phase. The matrix phase is composed of aromatic polyether ketone. The dispersed phase is composed of at least one of carbon black and carbon nanotubes. The aromatic polyether ketone molded article is composed of a surface layer portion and an inner portion. The crystallite size of the matrix phase in the surface layer portion is larger than 63 Å. The inner portion constitutes the inside of the surface layer portion, and the crystallite size of the matrix phase is smaller than that in the surface layer portion.
[0007] In this aromatic polyether ketone molded article, the crystallite size is larger in the surface layer portion constituting the surface than in the inner portion inside the surface layer portion. As a result, this aromatic polyether ketone molded article not only has the high mechanical strength inherent to aromatic polyether ketone, but also has large elongation in the surface layer portion, which is more susceptible to external force application. On the other hand, this aromatic polyether ketone molded article has high impact absorption in the inner portion, where the crystallite size is small, so that impacts applied to the surface layer portion are absorbed by the inner portion. As a result, this aromatic polyether ketone molded article is less likely to be subjected to large localized stress in the surface layer portion, thereby achieving even higher durability.
[0008] The aromatic polyether ketone constituting the matrix phase may have a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. The dispersed phase may be composed of carbon black, and the area ratio of the region in the surface layer portion occupied by the dispersed phase having a particle size of 0.1 μm or more may be 0.6% or more. The dispersed phase may be composed of carbon nanotubes, and the area ratio of the region in the surface layer portion occupied by the dispersed phase having a particle size of 0.1 μm or more may be 1.9% or more. The matrix phase may be composed of polyether ether ketone. The aromatic polyether ketone molded article may be configured as a sliding member. The aromatic polyether ketone molded article may be configured as a gear member.
[0009] In a method for producing an aromatic polyether ketone molded article according to one embodiment of the present invention, a molded article is produced by injection molding, in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of aromatic polyether ketone, and the surface of the molded article is irradiated with an electron beam.
[0010] In the above configuration, at least one of carbon black and carbon nanotubes is dispersed in a matrix phase, and a molded article obtained by injection molding is irradiated with an electron beam. The electron beam irradiation applies a large amount of energy to the surface layer of the molded article, thereby activating the molecular motion of the aromatic polyether ketone present in the surface layer. In the surface layer of the molded article, at least one of the carbon black and carbon nanotubes that constitute the dispersed phase in the matrix phase where molecular motion has been activated serves as the nuclei of crystallites, thereby promoting the grain growth of the crystallites. This results in an aromatic polyether ketone molded article having a matrix phase with large crystallite size in the surface layer.
[0011] As described above, the present invention can provide an aromatic polyether ketone molded article that has both high mechanical strength and high elongation in the surface layer portion.
[0012] 1 is a flowchart showing a method for manufacturing a resin molded body according to an embodiment of the present invention; FIG. 2 is a plan view showing an example in which the resin molded body is configured as a gear member;
[0013] [Description of Resin Molded Article] The present invention relates to an aromatic polyether ketone molded article, which is a resin molded article formed mainly from aromatic polyether ketone. More specifically, the resin molded article according to this embodiment includes a matrix phase made of aromatic polyether ketone and a dispersed phase made of carbon powder dispersed in the matrix phase. The carbon powder constituting the dispersed phase is made of at least one of carbon black and carbon nanotubes.
[0014] The aromatic polyether ketone constituting the matrix phase is a resin composed of a benzene ring, an ether, and a ketone. In the resin molded product according to the present embodiment, it is preferable to use polyether ether ketone (PEEK), which has excellent heat resistance and mechanical strength, as the aromatic polyether ketone constituting the matrix phase.
[0015] In the resin molded article according to this embodiment, the aromatic polyether ketone constituting the matrix phase preferably has a large molecular weight, specifically, a molecular weight distribution with a maximum peak molecular weight in the range of 50,000 or more, whereby the resin molded article according to this embodiment can obtain high mechanical strength by mutually binding the long molecular chains.
[0016] The resin molded article according to this embodiment is composed of a surface layer portion in which the crystallite size of the matrix phase is large, and an inner portion that forms the inside of the surface layer portion and in which the crystallite size of the matrix phase is smaller than that of the surface layer portion. Specifically, in the resin molded article according to this embodiment, the crystallite size of the matrix phase in the surface layer portion is larger than 63 Å.
[0017] As a result, in the surface layer portion of the resin molded article according to this embodiment, the molecular chains constituting each crystallite are less likely to break even when a large tensile stress is applied, and large elongation can be obtained. Therefore, in the resin molded article according to this embodiment, large elongation can be obtained selectively in the surface layer portion constituting the surface vicinity to which large external stress is easily applied.
[0018] In other words, in the resin molded article according to this embodiment, the matrix phase is composed of long molecular chains, and the crystallite size of the matrix phase in the surface layer portion is large, so that both high mechanical strength and large elongation can be achieved in the surface layer portion, which allows the resin molded article according to this embodiment to achieve high durability when used in applications such as sliding members.
[0019] The molecular weight distribution of the aromatic polyether ketone constituting the matrix phase can be measured by, for example, gel permeation chromatography. The maximum peak molecular weight refers to the molecular weight corresponding to the number of molecules (frequency) that forms a peak value in the molecular weight distribution curve obtained by molecular weight measurement.
[0020] The crystallite size of the matrix phase can be measured using a diffraction pattern obtained by X-ray diffraction (XRD). That is, the crystallite size of the matrix phase can be calculated based on the Scherrer formula by measuring the half-width of the maximum peak corresponding to the aromatic polyether ketone in the diffraction pattern.
[0021] The crystallite size of the matrix phase in the surface layer portion should be larger than 63 Å, and although no disadvantages due to an excessively large size have been confirmed at this stage, it is believed that there is a limit to the improvement in mechanical strength that can be achieved by increasing the crystallite size. From this perspective, the upper limit of the crystallite size of the matrix phase in the surface layer portion is assumed to be, for example, 250 Å.
[0022] Furthermore, in the resin molded article according to this embodiment, high impact absorption is achieved in the inner portion where the crystallite size in the matrix phase is smaller than that in the surface layer portion, and therefore impacts applied to the surface layer portion are well absorbed. As a result, in the resin molded article according to this embodiment, large stress is less likely to be applied locally to the surface layer portion, and therefore even higher durability is achieved.
[0023] That is, in the resin molded article according to this embodiment, the crystallite size of the matrix phase is increased in the surface layer portion, while the crystallite size of the matrix phase is intentionally kept small in the inner portion. With this configuration, the resin molded article according to this embodiment can more effectively improve durability through the synergistic effect between the surface layer portion and the inner portion.
[0024] The thickness of the surface layer portion of the resin molded article according to this embodiment can be determined appropriately depending on the application, etc. For example, from the viewpoint of more reliably obtaining the above-described effect of the surface layer portion, it is preferable that the thickness of the surface layer portion is 50 μm or more. On the other hand, from the viewpoint of more effectively obtaining the impact absorption property of the inner portion, it is preferable that the thickness of the surface layer portion is kept to 700 μm or less.
[0025] 1 is a flowchart showing a method for producing a resin molded article according to this embodiment. First, in step S01, a raw material is prepared. The raw material prepared in step S01 is prepared as a kneaded mixture of, for example, aromatic polyether ketone constituting a matrix phase and carbon powder constituting a dispersed phase.
[0026] In step S01, it is preferable to use an aromatic polyether ketone having a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. Also, in step S01, it is possible to use a carbon powder having an appropriate particle size distribution in order to obtain the effect described in step S03 below.
[0027] The kneaded material as a raw material can be obtained, for example, by kneading aromatic polyether ketone and carbon powder using a single-screw extruder, a twin-screw extruder, etc. In step S01, the kneaded material as a raw material can also be prepared as a commercially available product in which aromatic polyether ketone and carbon powder are kneaded in advance.
[0028] Next, in step S02, the raw material prepared in step S01 is molded into a shape appropriate for the intended use. The raw material can be molded by injection molding. The raw material compact obtained in step S02 has a matrix phase made of aromatic polyether ketone and a dispersed phase made of carbon powder dispersed therein.
[0029] In the raw material compact obtained in step S02, the crystallite size of the matrix phase is substantially uniform, and a surface layer portion and an inner portion in which the crystallite size of the matrix phase differs from each other are not formed. In this embodiment, step S03 is performed to form a surface layer portion in which the crystallite size of the matrix phase is large.
[0030] In step S03, the surface of the raw material compact obtained in step S02 is irradiated with an electron beam. As a result, a large amount of energy is selectively applied to the surface layer portion of the raw material compact that constitutes the surface vicinity. In step S03, in order to sufficiently increase the energy applied to the surface layer portion of the raw material compact, it is preferable to set the irradiation dose of the electron beam to 50 kGy or more.
[0031] In the matrix phase of the raw material compact, molecular motion becomes active in the surface layer where a large amount of energy is applied by electron beam irradiation, and grain growth of crystallites occurs with the carbon powder constituting the dispersed phase as nuclei. Furthermore, the carbon nanotubes constituting the dispersed phase also have the effect of improving the thermal conductivity of the raw material compact as a whole, including the matrix phase. Therefore, in a raw material compact whose dispersed phase is composed of carbon nanotubes, electron beam irradiation further activates molecular motion of the matrix phase in the surface layer, further promoting grain growth of the crystallites. Meanwhile, the crystallite size is maintained in the inner portion, which is not affected by electron beam irradiation, resulting in a difference in crystallite size of the matrix phase between the surface and inner portions.
[0032] In particular, in the resin molded article according to this embodiment, the synergistic effect of the dispersion of carbon powder and the irradiation of electron beams can promote the growth of crystallites even in the matrix phase with a large molecular weight, where the growth of crystallites is difficult to promote, thereby obtaining a resin molded article having both high mechanical strength and large elongation in the surface layer portion.
[0033] The effect of promoting particle growth by becoming the nuclei of crystallites in the dispersed phase is believed to be obtained regardless of the size of the dispersed phase, but is more effectively obtained by making the dispersed phase larger to a certain extent. In this regard, in the resin molded product according to this embodiment, when the dispersed phase is composed of carbon black, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer is 0.6% or more. Furthermore, when the dispersed phase is composed of carbon nanotubes, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer is 1.9% or more.
[0034] On the other hand, in the resin molded article according to the present embodiment, from the viewpoint of moldability, the area ratio of the region in the surface layer portion occupied by the dispersed phase having a particle size of 0.1 μm or more is preferably 20% or less, and more preferably 10% or less. The area ratio of the dispersed phase of the resin molded article can be determined from a photograph of the resin molded article taken with a fluorescence microscope.
[0035] Furthermore, in the resin molded product according to this embodiment, the portion where crystallites grow by electron beam irradiation is limited to the surface layer, and the crystallite size of the inner portion, which accounts for the majority of the surface layer, is not changed. Therefore, in this resin molded product, the dimensional change due to the change in crystallite size from the raw material molded product can be kept small.
[0036] The thickness of the surface layer of the resin molded body can be controlled in various ways by changing the conditions for irradiating the electron beam. In addition, in step S03, by irradiating the electron beam while heating the raw material molded body, it is possible to more effectively promote grain growth of the crystallites of the matrix phase in the surface layer.
[0037] The resin molded article according to this embodiment is particularly suitable for application to parts where stress is likely to concentrate on the surface. Examples of such parts include sliding members such as gear members, seal rings, thrust washers, and bearings. The resin molded article according to this embodiment configured as a sliding member exhibits high durability.
[0038] 2 shows a gear member as an application example of the resin molded article according to this embodiment as a sliding member. In gear members, stress tends to concentrate at the roots of the multiple teeth T arranged continuously along the outer periphery, but by configuring the resin molded article according to this embodiment, chipping of the teeth T can be effectively suppressed.
[0039] [Examples and Comparative Examples] Examples and comparative examples of the above embodiment will be described.
[0040] (Examples 1 to 3 and Comparative Examples 1 and 2) In Examples 1 to 3 and Comparative Examples 1 and 2, samples of resin molded bodies were prepared and each sample was evaluated. In all of Examples 1 to 3 and Comparative Example 2, carbon black was used as the carbon powder constituting the dispersed phase. Comparative Example 1 differs from the above-described embodiments in that no dispersed phase was used and no electron beam irradiation was performed. Comparative Example 2 differs from the above-described embodiments in that no electron beam irradiation was performed.
[0041] A common aromatic polyether ketone was used in all of Examples 1 to 3 and Comparative Examples 1 and 2. Specifically, in all of Examples 1 to 3 and Comparative Examples 1 and 2, the polyether ether ketone "Vestakeep (registered trademark) 5000G" manufactured by Polypla-Evonik was used as the aromatic polyether ketone.
[0042] The same carbon black was used in Examples 1 to 3 and Comparative Example 2. Specifically, carbon black "#750B" manufactured by Mitsubishi Chemical Corporation was used in Examples 1 to 3 and Comparative Example 2. In Comparative Example 1, no carbon black was used, that is, only aromatic polyether ketone was used.
[0043] Table 1 shows the electron beam irradiation temperatures and irradiation doses in Examples 1 to 3. In Examples 1 and 3, the electron beam was irradiated onto a sample at room temperature, while in Example 2, the electron beam was irradiated onto a sample heated to 250° C. Table 1 also shows the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the samples of Examples 1 to 3 and Comparative Examples 1 and 2, and the crystallite size of the matrix phase of the samples.
[0044] The area ratio of the dispersed phase of each sample was determined from a photograph of each sample taken with a fluorescent microscope "BX53M" manufactured by Olympus Corp. The crystallite size of the matrix phase of each sample was determined from the diffraction pattern of each sample obtained by measurement with an X-ray diffractometer "Samartlab" manufactured by Rigaku Corporation.
[0045] The area ratio of the dispersed phase and the crystallite size of the matrix phase were determined in the surface layer portion for all of the samples according to Examples 1 to 3. That is, the area ratio of the dispersed phase and the crystallite size of the matrix phase shown in Table 1 are the results obtained for the surface layer portion of the sample.
[0046] As shown in Table 1, the crystallite size of the matrix phase in all of Examples 1 to 3 was larger than that in Comparative Example 1. In contrast, the crystallite size of the matrix phase in Comparative Example 2 was equivalent to that in Comparative Example 1. This confirmed that electron beam irradiation is effective for increasing the crystallite size of the matrix phase in the surface layer portion. In particular, the crystallite size was the largest in Example 2, and it was confirmed that heating the sample during electron beam irradiation is even more effective in increasing the crystallite size.
[0047]
[0048] A tensile test was conducted to evaluate the fracture properties of each sample of Examples 1 to 3 and Comparative Examples 1 and 2. An "AGX" manufactured by Shimadzu Corporation was used for the tensile test. In the tensile test, each sample was formed into an A12 dumbbell shape in accordance with JIS K7139 (2009), and the tensile speed was 10 mm / min, with the other conditions being the same.
[0049] As a result, Table 2 shows the yield strength, yield stroke, and tensile product for Examples 1 to 3 and Comparative Examples 1 and 2 as percentage changes (%) relative to Comparative Example 1. The yield strength and yield stroke were determined from the stress-strain curve obtained in the tensile test, and the tensile product was calculated from the yield strength and yield stroke.
[0050] In all of Examples 1 to 3, the yield stroke was significantly improved compared to Comparative Example 1, resulting in a tensile product that was 15% or higher. On the other hand, in Comparative Example 2, the yield stroke was smaller than in Examples 1 to 3. This confirmed that large elongation could be obtained by increasing the crystallite size of the matrix phase in the surface layer portion.
[0051] Next, a gear durability test was conducted on each sample according to Examples 1 to 3 and Comparative Examples 1 and 2 to evaluate the product characteristics as a gear member. In the gear durability test, each sample had a gear shape. In the gear durability test for each sample, a gear member (made of S45C) was used as the mating member, and the sample was rotated while meshing with the mating member.
[0052] In addition, the gear durability tests for each sample were conducted under the same conditions, with a rotation speed of 1,000 rpm and a torque of 10 N m. Grease was used as a lubricant between each sample and the mating material during rotation. Each sample was rated as "OK" or "NG" based on the presence or absence of tooth chipping after 1.1 million rotations.
[0053] Table 2 shows the results of the gear durability test for Examples 1 to 3 and Comparative Examples 1 and 2. No tooth chipping occurred in any of the samples according to Examples 1 to 3, whereas tooth chipping occurred in all of the samples according to Comparative Examples 1 and 2. This shows that Examples 1 to 3 provide high product characteristics as gear members.
[0054]
[0055] Examples 4 and 5 In Examples 4 and 5, samples of resin molded bodies were prepared and evaluated. In both Examples 4 and 5, carbon nanotubes were used as the carbon powder constituting the dispersed phase. In both Examples 4 and 5, aromatic polyether ketone, which is the same as in Examples 1 to 3 and Comparative Examples 1 and 2, was used.
[0056] The same carbon nanotubes were used in both Examples 4 and 5. Specifically, the carbon nanotubes "NC7000" manufactured by Nanocyl Corporation were used in both Examples 4 and 5.
[0057] Table 3 shows the electron beam irradiation temperatures and irradiation doses in Examples 4 and 5. In Example 4, the sample heated to 250°C was irradiated with the electron beam, while in Example 5, the sample at room temperature was irradiated with the electron beam. Table 3 also shows the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the samples of Examples 4 and 5 and Comparative Example 1, and the crystallite size of the matrix phase of the samples. The area ratio of the dispersed phase and the crystallite size of the matrix phase in each sample were determined by the same methods as in Examples 1 to 3 and Comparative Examples 1 and 2.
[0058] The area ratio of the dispersed phase and the crystallite size of the matrix phase were determined in the surface layer portion for each of the samples according to Examples 4 and 5. That is, the area ratio of the dispersed phase and the crystallite size of the matrix phase shown in Table 3 are the results obtained for the surface layer portion of each sample.
[0059] As shown in Table 3, in both Examples 4 and 5, the crystallite size of the matrix phase was larger than that of Comparative Example 1. In particular, in Example 4, in which the area ratio of the dispersed phase was large, a significantly larger crystallite size was obtained. This confirmed that the effect of promoting grain growth of crystallites was obtained by having a large amount of carbon nanotubes with high thermal conductivity.
[0060]
[0061] To evaluate the fracture properties of each sample according to Examples 4 and 5, a tensile test was carried out in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. As a result, Table 4 shows the yield strength, yield stroke, and tensile product of Examples 4 and 5 and Comparative Example 1 as percentage changes (%) compared to Comparative Example 1.
[0062] In both Examples 4 and 5, the yield strength and yield stroke were both improved compared to Comparative Example 1, resulting in a tensile product that was 35% or more higher. In particular, in Example 4, in which the area ratio of the dispersed phase was large, both the yield strength and yield stroke were significantly larger. This confirmed that a large tensile product could be obtained by increasing the crystallite size of the matrix phase.
[0063] Next, in order to evaluate the product characteristics as gear members for each sample of Examples 4 and 5 and Comparative Example 1, a gear durability test was conducted in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. Table 4 shows the results of the gear durability test for Examples 4 and 5 and Comparative Example 1. No chipped teeth occurred in any of the samples of Examples 4 and 5. This shows that Examples 4 and 5 have excellent product characteristics as gear members.
[0064]
[0065] [Other Embodiments] Although the embodiments of the present invention have been described above, it goes without saying that the present invention is not limited to the above-described embodiments and various modifications can be made.
[0066] For example, the molecular weight of the aromatic polyether ketone constituting the matrix phase is not particularly limited as long as the resin molded article of the present invention has sufficient mechanical strength depending on the application, etc. In other words, the aromatic polyether ketone constituting the matrix phase may have a maximum peak molecular weight in any range in its molecular weight distribution.
[0067] Furthermore, the aromatic polyether ketone constituting the matrix phase of the resin molded article of the present invention may be other than polyether ether ketone (PEEK), and may be, for example, polyether ketone (PEK), polyether ketone ketone (PEKK), polyether ether ketone ketone (PEEKK), polyether ketone ether ketone ketone (PEKEKK), etc. Furthermore, the matrix phase of the resin molded article of the present invention may be configured as a blend of multiple types of aromatic polyether ketones.
[0068] Furthermore, in the present invention, the method for increasing the crystallite size of the surface layer portion of the aromatic polyether ketone molded article is not limited to electron beam irradiation, and other methods for increasing the crystallite size of the surface layer portion include, for example, laser irradiation, UV irradiation, excimer irradiation, plasma irradiation, corona irradiation, flame treatment, and chemical treatment.
Claims
1. An aromatic polyether ketone molded body comprising: a matrix phase composed of aromatic polyether ketone; and a dispersed phase composed of at least one of carbon black and carbon nanotubes and dispersed in the matrix phase; the aromatic polyether ketone molded body comprising: a surface layer portion in which the crystallite size of the matrix phase is larger than 63 Å; and an inner layer portion constituting the inside of the surface layer portion, the crystallite size of the matrix phase being smaller than that of the surface layer portion.
2. An aromatic polyether ketone molded article according to claim 1, wherein the aromatic polyether ketone constituting the matrix phase has a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more.
3. An aromatic polyether ketone molded article according to claim 1, wherein the dispersed phase is composed of carbon black, and the area ratio of the region in the surface layer occupied by the dispersed phase having a particle size of 0.1 μm or more is 0.6% or more.
4. An aromatic polyether ketone molded article according to claim 1, wherein the dispersed phase is composed of carbon nanotubes, and the area ratio of the region in the surface layer occupied by the dispersed phase having a particle size of 0.1 μm or more is 1.9% or more.
5. An aromatic polyether ketone molded article according to claim 1, wherein the matrix phase is composed of polyether ether ketone.
6. An aromatic polyether ketone molded article according to claim 1, which is configured as a sliding member.
7. The aromatic polyether ketone molding according to claim 6, which is configured as a gear member.
8. A method for producing an aromatic polyether ketone molded article, comprising: producing a molded article in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of aromatic polyether ketone by injection molding; and irradiating an electron beam onto the surface of the molded article.
Citation Information
Patent Citations
Resin composition
JP1997040864A
Method for modifying plastic by irradiation with electron beam
JP2000080181A
Method for producing crosslinked body of enginnering plastic and method for producing cocrosslinked body of enginnering plastic and fluororesin
JP2002265630A
Resin crystallization promoter and resin composition
JP2004339484A
Method for enhancing chemical resistance of resin molded article by electromagnetic wave irradiation
JP2018047569A