Laminate and packaging material

The laminate structure, featuring a polyurethane gas barrier layer and an anionic polyolefin heat seal layer, addresses the limitations of conventional gas barrier paper packaging by enhancing both gas barrier and heat sealability, ensuring effective oxygen and water vapor barrier performance and heat sealing capabilities.

WO2024203674A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC

Patent Information

Application Number
PCT/JP2024/010897
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional gas barrier paper packaging lacks sufficient gas barrier properties and heat sealability, requiring improvements to achieve both excellent oxygen and water vapor barrier properties along with reliable heat sealing capabilities.

Method used

A laminate structure comprising a paper base material, a gas barrier layer made from a polyurethane resin with a reaction product of an isocyanate group-terminated prepolymer and a chain extender, and a heat seal layer containing an anionic group-containing polyolefin resin, with a sealing layer optionally interposed between the paper base material and the gas barrier layer to enhance performance.

Benefits of technology

The laminate achieves both excellent gas barrier properties and heat sealability by optimizing the gas barrier layer's oxygen permeability and the heat seal layer's adhesive strength, ensuring effective oxygen and water vapor barrier performance while maintaining sufficient heat sealing properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024010897_03102024_PF_FP_ABST
    Figure JP2024010897_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a laminate and a packaging material which have both excellent gas barrier properties and excellent heat sealing properties. A laminate according to the present invention comprises a paper base material, a gas barrier layer that is disposed on at least one side of the paper base material, and a heat seal layer that is disposed on at least one side of the gas barrier layer, wherein the amount of the heat seal layer is 1.0-7.0 g / m2 <sp / >.
Need to check novelty before this filing date? Find Prior Art

Description

Laminates and packaging materials

[0001] The present invention relates to a laminate and a packaging material, and more particularly to a laminate including a gas barrier layer and a heat seal layer.

[0002] BACKGROUND ART Laminates comprising a paper substrate, a gas barrier layer, and a heat seal layer have been known in the art, and are used, for example, as packaging materials.

[0003] More specifically, the following gas barrier paper-based packaging has been proposed as a laminate: The gas barrier paper-based packaging includes a paper substrate. A sealing resin composition (e.g., an acrylic resin aqueous emulsion) is applied to one side of the paper substrate at a rate of 2 g / m. 2 A gas barrier resin composition (for example, a urethane-based hybrid gas barrier resin composition) is applied to the surface of the fixing filling layer at a concentration of 2.5 g / m. 2 A heat sealing agent (for example, a dispersion of a polyethylene resin) is applied to the surface of the gas barrier layer at a rate of 10 g / m. 2 A heat seal layer of the above formula is formed (see, for example, Patent Document 1 (Example Ca10)).

[0004] The gas barrier layer imparts gas barrier properties to the gas barrier paper-based packaging body, and the heat seal layer imparts heat seal properties to the gas barrier paper-based packaging body.

[0005] Japanese Patent Application Laid-Open No. 2022-155999

[0006] On the other hand, the above-mentioned gas barrier paper-based packaging materials may not have sufficient gas barrier properties (oxygen barrier properties and water vapor barrier properties), and there are cases where gas barrier paper-based packaging materials are required to have excellent heat seal properties.

[0007] The present invention provides a laminate and a packaging material that have both excellent gas barrier properties and excellent heat sealability.

[0008] The present invention [1] is a paper substrate, a gas barrier layer disposed on at least one side of the paper substrate, and a heat seal layer disposed on at least one side of the gas barrier layer, wherein the amount of the heat seal layer is 1.0 g / m2 7.0g / m or more 2 The laminate includes:

[0009] The present invention [2] includes the laminate according to the above [1], in which a sealing layer is interposed between the paper substrate and the gas barrier layer.

[0010] The present invention [3] includes the laminate according to the above [1] or [2], wherein the gas barrier layer contains a gas barrier resin.

[0011] The present invention [4] includes the laminate according to the above [3], wherein the gas barrier resin contains a gas barrier polyurethane resin.

[0012] The present invention [5] includes the laminate according to the above [4], wherein the gas barrier polyurethane resin contains a reaction product of an isocyanate group-terminated prepolymer and a chain extender, the isocyanate group-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, and the active hydrogen group-containing component contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.

[0013] The present invention [6] includes the laminate according to any one of the above [1] to [5], wherein the heat seal layer contains an anionic group-containing heat sealable resin, and the anionic group-containing heat sealable resin contains at least one resin selected from the group consisting of an anionic group-containing polyolefin resin, an anionic group-containing (meth)acrylic resin, and an anionic group-containing polyurethane resin.

[0014] The present invention [7] includes the laminate according to the above [6], wherein the anionic group-containing heat-sealable resin is neutralized with a neutralizing agent, and the neutralizing agent contains at least one selected from the group consisting of alkali metal hydroxides, ammonia, and amine compounds.

[0015] The present invention [8] includes the laminate according to the above [6] or [7], wherein the anionic group-containing heat-sealable resin has a moisture absorption expansion coefficient of 5000 ppm / RH% or more and 10000 ppm / RH% or less.

[0016] The present invention [9] includes a packaging material containing the laminate according to any one of the above [1] to [8].

[0017] The laminate of the present invention comprises a paper substrate, a gas barrier layer, and a heat seal layer. The amount of the heat seal layer in the laminate is adjusted to a predetermined range. Therefore, the laminate is prevented from deteriorating in gas barrier properties due to the heat seal layer, and excellent heat seal properties are obtained. As a result, the laminate has both excellent gas barrier properties and excellent heat seal properties.

[0018] The packaging material of the present invention contains the above laminate, and therefore has both excellent gas barrier properties and excellent heat sealability.

[0019] FIG. 1 is a schematic diagram showing one embodiment of the laminate of the present invention.

[0020] 1. Laminate In FIG. 1, the laminate 1 includes a paper base material 2, a gas barrier layer 4 disposed on at least one side in the thickness direction of the paper base material 2 (upper side in the drawing), and a heat seal layer 5 disposed on at least one side in the thickness direction of the gas barrier layer 4 (upper side in the drawing).

[0021] Furthermore, the laminate 1 can further include, as an optional layer, a sealing layer 3 interposed between the paper base material 2 and the gas barrier layer 4. In Fig. 1, the laminate 1 includes the sealing layer 3. That is, in Fig. 1, the laminate 1 includes the paper base material 2, the sealing layer 3, the gas barrier layer 4, and the heat seal layer 5, in that order from the other side (the lower side of the drawing) to one side (the upper side of the drawing) in the thickness direction.

[0022] (1) Paper Base Material The paper base material 2 is a base material formed from paper. Examples of the paper base material 2 include paper made from pulp. Examples of pulp include natural pulp and synthetic pulp. More specific examples of the paper base material 2 include glassine paper, coated paper, one-side gloss kraft paper, roll paper, and cup base paper. The paper base material 2 may be a single-layer paper or may be a multi-layer paper. The paper base material 2 is appropriately selected depending on the application of the laminate 1.

[0023] The shape of the paper substrate 2 is not particularly limited and may be appropriately set. Examples of the shape of the paper substrate 2 include a sheet shape, a bottle shape, and a cup shape. A preferred shape of the paper substrate 2 is a sheet shape.

[0024] The paper substrate 2 may be subjected to a surface treatment as required, such as a corona discharge treatment, a surface coating treatment, or a vapor deposition treatment.

[0025] The thickness of the paper base material 2 is, for example, 3 μm or more, or preferably 5 μm or more, and for example, 500 μm or less, or preferably 200 μm or less.

[0026] The basis weight of the paper base material 2 is, for example, 20 g / m 2 More than 30 g / m 2 The basis weight of the paper base material 2 is, for example, 400 g / m 2 Preferably, 300 g / m or less 2 The following is the result.

[0027] (2) Filler layer The filler layer 3 is laminated on the paper base material 2 to suppress impregnation of the gas barrier coating material (described later) into the paper base material 2. The filler layer 3 is also laminated on the paper base material 2 to absorb unevenness on the surface of the paper base material 2 and smooth the surface. More specifically, the filler layer 3 is disposed on at least one surface of the paper base material 2. The filler layer 3 may be disposed on both surfaces of the paper base material 2. The filler layer 3 is preferably disposed on only one surface of the paper base material 2.

[0028] The filling layer 3 contains, for example, a filling resin. More specifically, the filling layer 3 is formed, for example, by applying a coating material containing a filling resin (hereinafter, referred to as a filling coating material) to the surface of the paper base material 2 and drying it.

[0029] The filler coating material is not particularly limited, and examples thereof include coating materials containing known filler resins. More specifically, examples of the filler coating material include a solution obtained by dissolving a filler resin in a solvent and a dispersion obtained by dispersing a filler resin in a solvent.

[0030] The filler resin is a resin that inhibits the impregnation of a gas barrier coating material (described later) into the paper substrate 2. Examples of filler resins include polyolefin resins, polyester resins, polyamide resins, polyvinyl resins, (meth)acrylic resins, polycarbonate resins, and cellulose resins. These can be used alone or in combination of two or more. Preferred filler resins include polyolefin resins and (meth)acrylic resins.

[0031] The solvent is not particularly limited, but examples thereof include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents can be used alone or in combination of two or more.

[0032] More specifically, examples of the filler coating material include a resin dispersion and a resin emulsion containing a filler resin and a solvent.

[0033] The solid content concentration of the filler coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.

[0034] The method for applying the filler coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions for the filler coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.

[0035] This forms the filling layer 3. The amount (dry mass) of the filling layer 3 is, for example, 1 g / m 2 More than 3 g / m 2 The amount (dry mass) of the filling layer 3 is, for example, 30 g / m 2 Preferably, 15 g / m or less 2 The following is the result.

[0036] (3) Gas Barrier Layer The gas barrier layer 4 is a layer having gas barrier properties. Gas barrier properties are the property of reducing oxygen permeability. More specifically, the gas barrier layer 4 is made of a gas barrier resin having an oxygen permeability of a predetermined value or less. For example, the oxygen permeability of a gas barrier layer 4 having a thickness of 10 μm is, for example, 1 (cc / m) at room temperature. 2 ·day·atm) or less. The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).

[0037] The gas barrier layer 4 is disposed on the surface of the filling layer 3. That is, the gas barrier layer 4 is disposed on the surface of the filling layer 3 on the side of the paper base material 2 on which the filling layer 3 is disposed. The gas barrier layer 4 may be disposed on both sides of the paper base material 2 together with the filling layer 3. The gas barrier layer 4 is preferably disposed on only one surface of the paper base material 2 together with the filling layer 3.

[0038] Examples of the gas barrier layer 4 include inorganic layers and resin layers. The inorganic layer contains, for example, a metal and / or a metal oxide. Examples of the metal include aluminum. Examples of the metal oxide include aluminum oxide and silicon oxide. More specifically, examples of the inorganic layer include a metal thin film layer and a metal vapor deposition layer. The resin layer contains, for example, a gas barrier resin. More specifically, examples of the resin layer include a barrier coat layer and a barrier film layer.

[0039] The gas barrier layer 4 is preferably a barrier coating layer containing a gas barrier resin. More specifically, the gas barrier layer 4 is formed, for example, by applying a coating material containing a gas barrier resin (hereinafter, referred to as a gas barrier coating material) to the filling layer 3 and drying the coating material.

[0040] The gas barrier resin is a resin having an oxygen permeability of a predetermined value or less. More specifically, the oxygen permeability of a 10 μm thick film made of a gas barrier resin is, for example, 1 (cc / m) at room temperature. 2 ·day·atm) or less. The oxygen permeability is measured in accordance with JIS K7126 (2006) Method B using an oxygen permeability measuring device (MOCON, OX-TRAN2 / 22H). The measurement conditions are 20°C and 80% RH (relative humidity).

[0041] The gas barrier resin is not particularly limited. Examples of the gas barrier resin include a gas barrier polyurethane resin and a gas barrier acrylic resin. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, a gas barrier polyurethane resin is preferably used as the gas barrier resin. That is, the gas barrier resin preferably contains a gas barrier polyurethane resin, and more preferably consists of a gas barrier polyurethane resin.

[0042] The gas barrier polyurethane resin is a resin having an oxygen permeability equal to or less than the above-mentioned predetermined value. The gas barrier polyurethane resin is not particularly limited, and a known gas barrier polyurethane resin can be used. For example, the gas barrier polyurethane resin is contained in a polyurethane dispersion (PUD) as a gas barrier coating material.

[0043] The gas barrier polyurethane resin and the polyurethane dispersion are produced, for example, in accordance with the description of paragraphs

[0026] to

[0111] of JP 2015-044396 A and paragraphs

[0048] to

[0141] of JP 2021-115802 A.

[0044] More specifically, the gas barrier polyurethane resin contains, for example, a reaction product of an isocyanate-terminated prepolymer and a chain extender, preferably a reaction product of an isocyanate-terminated prepolymer and a chain extender. The isocyanate-terminated prepolymer contains, for example, a reaction product of a polyisocyanate component and an active hydrogen group-containing component, preferably a reaction product of a polyisocyanate component and an active hydrogen group-containing component.

[0045] That is, the primary reaction product of the polyisocyanate component and the active hydrogen group-containing component is an isocyanate-terminated prepolymer, and the secondary reaction product of the isocyanate-terminated prepolymer and the chain extender is a gas-barrier polyurethane resin.

[0046] Examples of the polyisocyanate component include known polyisocyanate components. From the viewpoint of gas barrier properties, the polyisocyanate component preferably contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate. Furthermore, the polyisocyanate component may contain other polyisocyanates (polyisocyanates excluding xylylene diisocyanate and hydrogenated xylylene diisocyanate) as needed. Examples of other polyisocyanates include polyisocyanates commonly used industrially. More specific examples of other polyisocyanates include pentamethylene diisocyanate (PDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), norbornene diisocyanate (NBDI), methylenebis(cyclohexyl isocyanate) (H 12 Examples of the polyisocyanate include diphenylmethane diisocyanate (MDI), tolylene diisocyanate (TDI), toluidine diisocyanate (TODI), naphthalene diisocyanate (NDI), and tetramethylxylylene diisocyanate (TMXDI). These may be used alone or in combination of two or more. Other preferred polyisocyanates include methylenebis(cyclohexyl isocyanate) (H 12 MDI). The polyisocyanate component may be a monomer or a derivative. Examples of the derivative include a polymer, an isocyanurate-modified product, an allophanate-modified product, a polyol adduct, a biuret-modified product, a urea-modified product, an oxadiazinetrione-modified product, and a carbodiimide-modified product. These may be used alone or in combination of two or more types.

[0047] The polyisocyanate component preferably contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate and another polyisocyanate (preferably methylenebis(cyclohexylisocyanate)). The content ratio of these components is appropriately set depending on the purpose and application.

[0048] The active hydrogen group-containing component is an organic compound containing an active hydrogen group. Examples of the active hydrogen group include a hydroxyl group and an amino group, and preferably a hydroxyl group. Examples of the active hydrogen group-containing component include known active hydrogen group-containing compounds. From the viewpoint of gas barrier properties, the active hydrogen group-containing component preferably contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen group-containing compound containing an anionic group.

[0049] The short-chain diol having 2 to 6 carbon atoms is an organic compound having 2 to 6 carbon atoms and two hydroxyl groups per molecule. Examples of short-chain diols include alkanediols having 2 to 6 carbon atoms and etherdiols having 2 to 6 carbon atoms, preferably alkanediols having 2 to 6 carbon atoms. Examples of alkanediols having 2 to 6 carbon atoms include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butylene glycol, 1,3-butylene glycol, 1,2-butylene glycol, 1,5-pentanediol, 1,6-hexanediol, and neopentyl glycol. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, ethylene glycol is preferred.

[0050] As the active hydrogen group-containing compound containing an anionic group, preferably, an organic compound having one carboxy group and two or more hydroxyl groups in one molecule is used, and more preferably, an organic compound having one carboxy group and two hydroxyl groups in one molecule is used. Examples of organic compounds having one carboxy group and two hydroxyl groups in one molecule include carboxy group-containing diols. Examples of carboxy group-containing diols include dihydroxyalkanoic acids. Examples of dihydroxyalkanoic acids include 2,2-dimethylolacetic acid, 2,2-dimethylollactic acid, 2,2-dimethylolpropionic acid (also known as dimethylolpropionic acid), 2,2-dimethylolbutanoic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvaleric acid. These can be used alone or in combination of two or more. From the viewpoint of water dispersibility, 2,2-dimethylolpropionic acid is preferred.

[0051] In the active hydrogen group-containing component, the content of the short-chain diol having 2 to 6 carbon atoms and the content of the active hydrogen group-containing compound having an anionic group are appropriately set depending on the purpose and application.

[0052] The active hydrogen group-containing component can further contain other polyols. Examples of other polyols include low-molecular-weight polyols with trihydric or higher hydricity, short-chain diols with 7 or more carbon atoms, and high-molecular-weight polyols. These can be used alone or in combination of two or more. Preferred examples of other polyols include low-molecular-weight polyols with trihydric or higher hydricity, and preferably trihydric alcohols and tetrahydric alcohols. Examples of trihydric alcohols include glycerin, 2-methyl-2-hydroxymethyl-1,3-propanediol, 2,4-dihydroxy-3-hydroxymethylpentane, 1,2,6-hexanetriol, trimethylolpropane, and 2,2-bis(hydroxymethyl)-3-butanol. Examples of tetrahydric alcohols include tetramethylolmethane (pentaerythritol) and diglycerin. These can be used alone or in combination of two or more. More preferred examples of low-molecular-weight polyols with trihydric or higher hydricity include trihydric alcohols, and even more preferred examples include trimethylolpropane. In addition, as the other polyol, for example, an active hydrogen group-containing compound containing a nonionic group can be mentioned. The active hydrogen group-containing compound containing a nonionic group can be used together with the above-mentioned active hydrogen compound containing an anionic group. In addition, the active hydrogen group-containing compound containing a nonionic group can be used instead of the above-mentioned active hydrogen compound containing an anionic group. In the active hydrogen group-containing component, the content ratio of the other polyol can be appropriately set according to the purpose and application.

[0053] The method for synthesizing the isocyanate-terminated prepolymer is not particularly limited. For example, the above-mentioned components are mixed in a predetermined equivalent ratio and reacted. Examples of the reaction method include bulk polymerization and solution polymerization, and solution polymerization is preferred. In the above reaction, a urethane catalyst can be added in an appropriate ratio as needed.

[0054] Furthermore, when the isocyanate group-terminated prepolymer has an anionic group derived from an active hydrogen compound containing an anionic group, the isocyanate group-terminated prepolymer is neutralized with a known neutralizing agent (e.g., triethylamine) to form a salt of the anionic group.

[0055] The isocyanate group concentration of the isocyanate group-terminated prepolymer is, for example, 4% by mass or more, preferably 5% by mass or more, more preferably 6% by mass or more, and for example, 25% by mass or less, preferably 20% by mass or less, more preferably 17% by mass or less, and even more preferably 15% by mass or less.

[0056] Next, in this method, the isocyanate-terminated prepolymer (primary reaction product) is reacted with a chain extender to obtain a gas-barrier polyurethane resin (secondary reaction product). For example, by reacting the isocyanate-terminated prepolymer with the chain extender in water, the gas-barrier polyurethane resin is produced and dispersed in water.

[0057] The chain extender is an organic compound that causes a chain extension reaction of the isocyanate-terminated prepolymer. The chain extender has multiple active hydrogen groups. Examples of the chain extender include polyamines, amino-group-containing alkoxysilyl compounds, and amino alcohols (e.g., 2-((2-aminoethyl)amino)ethanol).

[0058] The method for reacting the isocyanate-terminated prepolymer with the chain extender in water is not particularly limited. For example, the isocyanate-terminated prepolymer is first dispersed in water. Next, the chain extender is added to the water in which the isocyanate-terminated prepolymer is dispersed, and the isocyanate-terminated prepolymer is chain-extended in water. In this method, water can be added after completion of the reaction to adjust the solids concentration.

[0059] The chain extension reaction described above produces an aqueous dispersion of a gas-barrier polyurethane resin (hereinafter referred to as a primary polyurethane dispersion, or primary PUD). The primary polyurethane dispersion (primary PUD) is an aqueous dispersion containing a gas-barrier polyurethane resin but not containing the additives described below.

[0060] The gas barrier resin is not limited to the gas barrier polyurethane resin described above, and is preferably prepared as an aqueous dispersion (primary aqueous dispersion) of the gas barrier resin.

[0061] The solid content concentration of the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin is, for example, 10% by mass or more, preferably 15% by mass or more, and more preferably 20% by mass or more. The solid content concentration of the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin is, for example, 60% by mass or less, preferably 50% by mass or less, and more preferably 40% by mass or less.

[0062] The aqueous dispersion (primary aqueous dispersion) of the gas barrier resin can be used as it is as a gas barrier coating material. That is, the gas barrier coating material can be made of, for example, the aqueous dispersion (primary aqueous dispersion) of the gas barrier resin.

[0063] The gas barrier coating material may contain an additive. Preferably, the gas barrier coating material contains an additive. That is, preferably, an aqueous dispersion (secondary aqueous dispersion) containing the gas barrier resin and the additive is used as the gas barrier coating material.

[0064] Examples of additives include layered inorganic compounds, thickening inhibitors, heat stabilizers, antioxidants, light stabilizers, UV absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, nucleating agents, and curing agents. These can be used alone or in combination of two or more. From the viewpoint of gas barrier properties, layered inorganic compounds are preferred as additives. That is, the gas barrier layer 4 preferably contains a layered inorganic compound. The amount and timing of addition of the additives are appropriately determined depending on the purpose and application.

[0065] The solid content concentration of the gas barrier coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.

[0066] The method for applying the gas barrier coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions for the gas barrier coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.

[0067] This forms the gas barrier layer 4. The amount (dry mass) of the gas barrier layer 4 is, for example, 0.1 g / m 2 More than 0.2 g / m 2 The amount (dry mass) of the gas barrier layer 4 is, for example, 10 g / m 2 Preferably, 7 g / m or less 2 The following is the result.

[0068] (4) Heat-seal layer The heat-seal layer 5 is a resin layer with heat-sealing properties. The heat-seal layer 5 is disposed on the surface of the gas barrier layer 4. That is, the heat-seal layer 5 is disposed on the surface of the gas barrier layer 4 on the side of the paper base material 2 on which the gas barrier layer 4 is disposed. The heat-seal layer 5 may be disposed on both sides of the paper base material 2 together with the gas barrier layer 4. The heat-seal layer 5 is preferably disposed on only one surface of the paper base material 2 together with the gas barrier layer 4.

[0069] The heat seal layer 5 contains, for example, a heat sealable resin. More specifically, the heat seal layer 5 is formed, for example, by applying a coating material containing a heat sealable resin (hereinafter referred to as a heat sealable coating material) to the gas barrier layer 4 and drying it.

[0070] The heat-sealable resin is a resin that can be heat-sealed (thermally fused) to itself. The heat-sealable resin is not particularly limited, and known heat-sealable resins can be used. More specific examples of the heat-sealable resin include polyolefin resins, (meth)acrylic resins, and polyurethane resins. These resins can be used alone or in combination of two or more.

[0071] From the viewpoint of manufacturability of the heat-sealable coating material, the heat-sealable resin preferably contains an anionic group. That is, the heat-sealable resin is preferably an anionic group-containing heat-sealable resin. If the heat-sealable resin contains an anionic group, the heat-sealable resin is easily dissolved and / or dispersed in water, thereby efficiently producing the heat-sealable coating material. Examples of the anionic group include a carboxy group (carboxylic acid group) and a sulfo group (sulfonic acid group), and preferably a carboxy group. Examples of the anionic group-containing heat-sealable resin include an anionic group-containing polyolefin resin, an anionic group-containing (meth)acrylic resin, and an anionic group-containing polyurethane resin. In other words, the anionic group-containing heat-sealable resin contains at least one resin selected from the group consisting of an anionic group-containing polyolefin resin, an anionic group-containing (meth)acrylic resin, and an anionic group-containing polyurethane resin.

[0072] [Anionic Group-Containing Polyolefin Resin] Anionic group-containing polyolefin resin is a resin containing an anionic group and a structural unit derived from an olefin. Examples of anionic group-containing polyolefin resins include unsaturated carboxylic acid-modified polyolefin resins. Unsaturated carboxylic acid-modified polyolefin resins are obtained by copolymerization of monomer components (hereinafter referred to as olefin raw material monomer components) as a raw material composition.

[0073] The olefin raw material monomer component contains, for example, an olefin and an unsaturated carboxylic acid.

[0074] Examples of olefins include α-olefins. Examples of α-olefins include α-olefins having 1 to 20 carbon atoms. Examples of α-olefins having 1 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, and 1-eicosene. These can be used alone or in combination of two or more. Preferred α-olefins include olefins having 2 to 3 carbon atoms, more preferably ethylene and / or propylene, and even more preferably ethylene.

[0075] The olefin content, relative to the total amount of the olefin raw material monomer components, is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and, relative to the total amount of the olefin raw material monomer components, is, for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less.

[0076] The content of the olefin in the olefin raw material monomer component is substantially synonymous with the content of the olefin-derived structural units in the unsaturated carboxylic acid-modified polyolefin resin.

[0077] That is, the content of the olefin-derived structural units is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin. Also, the content of the olefin-derived structural units is, for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin.

[0078] In the polyolefin resin, the content of the olefin-derived structural units is, as described above, 50% by mass or more, preferably 60% by mass or more, based on the total amount of the polyolefin resin. The polyolefin resin is distinguished from other resins containing olefin-derived structural units by the content of the olefin-derived structural units.

[0079] More specifically, in a resin other than a polyolefin resin containing a structural unit derived from an olefin (for example, a (meth)acrylic resin described later), the content of the structural unit derived from an olefin is less than 50% by mass, preferably 40% by mass or less.

[0080] Examples of unsaturated carboxylic acids include unsaturated monocarboxylic acids and unsaturated dicarboxylic acids. Examples of unsaturated monocarboxylic acids include (meth)acrylic acid, crotonic acid, and isocrotonic acid. Examples of unsaturated dicarboxylic acids include maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, and norbornene dicarboxylic acid, and their acid anhydrides. The unsaturated carboxylic acids can be used alone or in combination of two or more. Preferable examples of unsaturated carboxylic acids include unsaturated monocarboxylic acids and acid anhydrides of unsaturated dicarboxylic acids, and more preferably (meth)acrylic acid.

[0081] The term "(meth)acrylic" refers to acrylic and / or methacrylic. The same applies to (meth)acrylate. As the (meth)acrylic acid, preferably, acrylic acid or methacrylic acid is used alone.

[0082] The content of the unsaturated carboxylic acid is appropriately adjusted, for example, to achieve a balance between heat sealability and hydrophilicity. For example, from the viewpoint of hydrophilicity, the content of the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the olefin raw material monomer components. Furthermore, from the viewpoint of heat sealability, the content of the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the olefin raw material monomer components.

[0083] The content of the unsaturated carboxylic acid in the olefin raw material monomer component is substantially synonymous with the content of the structural unit derived from the unsaturated carboxylic acid in the unsaturated carboxylic acid-modified polyolefin resin.

[0084] That is, the content of the structural units derived from the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin. Also, the content of the structural units derived from the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin.

[0085] The olefin raw material monomer component may contain a copolymerizable monomer in an appropriate ratio, if necessary. The copolymerizable monomer is a monomer that can be copolymerized with an olefin and / or an unsaturated carboxylic acid.

[0086] Examples of copolymerizable monomers include unsaturated carboxylic acid esters, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers, acetoacetoxy group-containing vinyl monomers, phosphate group-containing vinyl monomers, amide group-containing vinyl monomers, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, dienes, and vinyl esters. These can be used alone or in combination of two or more. From the viewpoint of heat-sealing properties, unsaturated carboxylic acid esters are preferred as copolymerizable monomers.

[0087] Examples of unsaturated carboxylic acid esters include alkyl esters of the above-mentioned unsaturated carboxylic acids. Preferable examples of unsaturated carboxylic acid esters include (meth)acrylic acid esters. Examples of (meth)acrylic acid esters include (meth)acrylic acid esters having an alkyl moiety with 1 to 12 carbon atoms. More specific examples of (meth)acrylic acid esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and lauryl (meth)acrylate. These may be used alone or in combination of two or more.

[0088] The (meth)acrylic acid ester is preferably a (meth)acrylic acid ester having an alkyl moiety having 1 to 4 carbon atoms. More specific examples include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and isobutyl (meth)acrylate.

[0089] More preferred (meth)acrylic acid esters include (meth)acrylic acid esters having an alkyl moiety with 2 to 4 carbon atoms. More specific examples include ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, and isobutyl (meth)acrylate. More preferred (meth)acrylic acid esters include butyl acrylate and isobutyl acrylate, and particularly preferred is isobutyl acrylate.

[0090] The content of the unsaturated carboxylic acid ester is, for example, 0% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, and particularly preferably 10% by mass or more, relative to the total amount of the olefin raw material monomer components. The content of the unsaturated carboxylic acid ester is, for example, 30% by mass or less, preferably 25% by mass or less, and more preferably 20% by mass or less, relative to the total amount of the olefin raw material monomer components.

[0091] The content of the unsaturated carboxylic acid ester in the olefin raw material monomer component is substantially synonymous with the content of the structural units derived from the unsaturated carboxylic acid ester in the unsaturated carboxylic acid-modified polyolefin resin.

[0092] That is, the content of the structural units derived from the unsaturated carboxylic acid ester is, for example, 0% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 8% by mass or more, and particularly preferably 10% by mass or more, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin. Also, the content of the structural units derived from the unsaturated carboxylic acid ester is, for example, 30% by mass or less, preferably 25% by mass or less, and more preferably 20% by mass or less, relative to the total amount of the unsaturated carboxylic acid-modified polyolefin resin.

[0093] The olefin raw material monomer component is preferably a ternary monomer component consisting of ethylene, an unsaturated carboxylic acid, and an unsaturated carboxylic acid ester, or may be a binary monomer component consisting of ethylene and an unsaturated carboxylic acid.

[0094] In other words, the unsaturated carboxylic acid-modified polyolefin resin preferably includes a two-component copolymer consisting of ethylene and an unsaturated carboxylic acid (hereinafter referred to as an ethylene-unsaturated carboxylic acid copolymer).Furthermore, the unsaturated carboxylic acid-modified polyolefin resin preferably includes a three-component copolymer consisting of ethylene, an unsaturated carboxylic acid ester, and an unsaturated carboxylic acid (hereinafter referred to as an ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer).

[0095] From the viewpoint of achieving a balance between heat sealability and hydrophilicity, a more preferred unsaturated carboxylic acid-modified polyolefin resin is a combination of an ethylene-unsaturated carboxylic acid copolymer and an ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer. The ratio of the ethylene-unsaturated carboxylic acid copolymer and the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer used in combination is appropriately adjusted from the viewpoint of achieving a balance between heat sealability and hydrophilicity.

[0096] For example, the content of the ethylene-unsaturated carboxylic acid copolymer relative to the total amount of the ethylene-unsaturated carboxylic acid copolymer and the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer is, for example, 20% by mass or more, preferably 40% by mass or more. Also, the content of the ethylene-unsaturated carboxylic acid copolymer relative to the total amount of the ethylene-unsaturated carboxylic acid copolymer and the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer is, for example, 80% by mass or less, preferably 60% by mass or less.

[0097] The content of the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer relative to the total amount of the ethylene-unsaturated carboxylic acid copolymer and the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer is, for example, 20% by mass or more, preferably 40% by mass or more. The content of the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer relative to the total amount of the ethylene-unsaturated carboxylic acid copolymer and the ethylene-unsaturated carboxylic acid ester-unsaturated carboxylic acid copolymer is, for example, 80% by mass or less, preferably 60% by mass or less.

[0098] The method for producing the unsaturated carboxylic acid-modified polyolefin resin is not particularly limited, and a known method can be used. For example, the above-mentioned olefin raw material monomer components are contacted with a known polymerization initiator (such as a peroxide) under high temperature and high pressure conditions. This results in an unsaturated carboxylic acid-modified polyolefin resin as a polymerization product of the olefin raw material monomer components.

[0099] [Anionic Group-Containing (Meth)acrylic Resin] The anionic group-containing (meth)acrylic resin is a resin containing an anionic group and a structural unit derived from a (meth)acrylic acid ester. Examples of the anionic group-containing (meth)acrylic resin include anionic group-containing (meth)acrylic resin. The anionic group-containing (meth)acrylic resin is obtained by copolymerization of monomer components (hereinafter referred to as acrylic raw material monomer components) as a raw material composition.

[0100] The acrylic raw material monomer component contains, for example, a (meth)acrylic acid ester and an unsaturated carboxylic acid.

[0101] Examples of the (meth)acrylic acid ester include the (meth)acrylic acid esters described above as the olefin raw material monomer component. These may be used alone or in combination of two or more.

[0102] The content of the (meth)acrylic acid ester relative to the total amount of the acrylic raw material monomer components is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less, relative to the total amount of the acrylic raw material monomer components.

[0103] The content of the (meth)acrylic acid ester in the acrylic raw material monomer component is substantially synonymous with the content of the structural units derived from the (meth)acrylic acid ester in the anionic group-containing (meth)acrylic resin.

[0104] That is, the content of the structural units derived from the (meth)acrylic acid ester, relative to the total amount of the anionic group-containing (meth)acrylic resin, is, for example, 50% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and the content of the structural units derived from the (meth)acrylic acid ester, relative to the total amount of the anionic group-containing (meth)acrylic resin, is, for example, 99% by mass or less, preferably 97% by mass or less, more preferably 95% by mass or less, even more preferably 93% by mass or less, and particularly preferably 90% by mass or less.

[0105] Examples of the unsaturated carboxylic acid include the unsaturated carboxylic acids mentioned above in connection with the olefin raw material monomer component. These may be used alone or in combination of two or more.

[0106] The content of the unsaturated carboxylic acid is appropriately adjusted, for example, to achieve a balance between heat-sealability and hydrophilicity. For example, from the viewpoint of hydrophilicity, the content of the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the acrylic raw material monomer components. Furthermore, from the viewpoint of heat-sealability, the content of the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the acrylic raw material monomer components.

[0107] The content of the unsaturated carboxylic acid in the acrylic raw material monomer component is substantially synonymous with the content of the structural unit derived from the unsaturated carboxylic acid in the anionic group-containing (meth)acrylic resin.

[0108] That is, the content of the structural units derived from the unsaturated carboxylic acid is, for example, 1% by mass or more, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more, relative to the total amount of the anionic group-containing (meth)acrylic resin. Also, the content of the structural units derived from the unsaturated carboxylic acid is, for example, less than 50% by mass, preferably 40% by mass or less, more preferably 30% by mass or less, and even more preferably 25% by mass or less, relative to the total amount of the anionic group-containing (meth)acrylic resin.

[0109] The acrylic raw material monomer component may contain a copolymerizable monomer in an appropriate ratio as needed. The copolymerizable monomer is a monomer copolymerizable with a (meth)acrylic acid ester and / or an unsaturated carboxylic acid.

[0110] Examples of copolymerizable monomers include olefins, hydroxyl group-containing vinyl monomers, amino group-containing vinyl monomers, glycidyl group-containing vinyl monomers, cyano group-containing vinyl monomers, sulfonic acid group-containing vinyl monomers, acetoacetoxy group-containing vinyl monomers, phosphoric acid group-containing vinyl monomers, amide group-containing vinyl monomers, aromatic vinyl monomers, N-substituted unsaturated carboxylic acid amides, heterocyclic vinyl compounds, vinylidene halide compounds, dienes, and vinyl esters. These can be used alone or in combination of two or more. The content ratio of the copolymerizable monomers is appropriately set depending on the purpose and application.

[0111] When the acrylic raw material monomer component contains an olefin, the content of structural units derived from the olefin in the anionic group-containing (meth)acrylic resin is less than 50% by mass, preferably 40% by mass or less, relative to the total amount of the anionic group-containing (meth)acrylic resin. The anionic group-containing (meth)acrylic resin is distinguished from the above-mentioned anionic group-containing polyolefin resin by the content of structural units derived from the olefin.

[0112] The method for producing the unsaturated carboxylic acid-modified (meth)acrylic resin is not particularly limited, and known methods can be used. For example, the above-mentioned acrylic raw material monomer components are contacted with a known polymerization initiator (such as a peroxide) under high temperature and high pressure conditions. This results in an anionic group-containing (meth)acrylic resin being obtained as a polymerization product of the acrylic raw material monomer components.

[0113] [Anionic Group-Containing Polyurethane Resin] The anionic group-containing polyurethane resin is a resin containing an anionic group and a urethane group. Examples of the anionic group-containing polyurethane resin include a reaction product of the polyisocyanate compound, the polyol compound, the active hydrogen compound containing the anionic group, and the chain extender.

[0114] The method for producing the anionic group-containing polyurethane resin is not particularly limited. For example, a polyisocyanate compound, a polyol compound, and an active hydrogen compound containing an anionic group are reacted by the above-mentioned method to obtain an isocyanate group-terminated prepolymer. Then, the isocyanate group-terminated prepolymer is reacted with a chain extender by the above-mentioned method. This results in an anionic group-containing polyurethane resin.

[0115] The anionic group-containing heat-sealable resin may be used alone or in combination of two or more thereof. As the anionic group-containing heat-sealable resin, a preferred example is an anionic group-containing polyolefin resin.

[0116] The anionic group-containing heat-sealable resin is preferably neutralized with a neutralizing agent. That is, the anionic group-containing heat-sealable resin is preferably an anionic group-containing heat-sealable resin neutralized with a neutralizing agent. The method for neutralizing the anionic group-containing heat-sealable resin is not particularly limited, and the anionic group and the neutralizing agent are brought into contact with each other at any time.

[0117] Examples of neutralizing agents include basic compounds, more specifically inorganic basic compounds and organic basic compounds. Examples of inorganic basic compounds include alkali metal hydroxides. Examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide. Examples of organic basic compounds include ammonia and amine compounds. Examples of amine compounds include triethylamine (TEA), triethanolamine, dimethylethanolamine, diethanolamine, diethylamine (DEA), methylamine (MA), and N,N-dimethylethanolamine. These compounds can be used alone or in combination of two or more. From the viewpoint of adjusting the moisture absorption rate and moisture absorption expansion coefficient of the anionic group-containing heat-sealable resin and achieving excellent water vapor barrier properties, preferred neutralizing agents include alkali metal hydroxides, ammonia, and amine compounds. In other words, the neutralizing agent preferably contains at least one selected from the group consisting of alkali metal hydroxides, ammonia, and amine compounds. From the viewpoint of adjusting the moisture absorption rate and moisture absorption expansion coefficient of the anionic group-containing heat sealable resin and obtaining excellent water vapor barrier properties, the neutralizing agent is more preferably a metal-free neutralizing agent, even more preferably ammonia and an amine compound, even more preferably ammonia and diethylamine (DEA), and particularly preferably ammonia.

[0118] The amount of the neutralizing agent added is, for example, 0.4 equivalents or more, preferably 0.6 equivalents or more, relative to 1 equivalent of the anionic group, and for example, 1.2 equivalents or less, preferably 1.0 equivalents or less, relative to 1 equivalent of the anionic group.

[0119] When the amount of the heat-seal layer 5 is within the range described below, from the viewpoint of obtaining better water vapor barrier properties, the moisture absorption expansion coefficient of the anionic group-containing heat-sealable resin is, for example, 1000 ppm / RH% or more, preferably 3000 ppm / RH% or more, more preferably 5000 ppm / RH% or more, and even more preferably 6000 ppm / RH% or more. Furthermore, when the amount of the heat-seal layer 5 is within the range described below, from the viewpoint of obtaining better water vapor barrier properties, the moisture absorption expansion coefficient of the anionic group-containing heat-sealable resin is, for example, 20000 ppm / RH% or less, preferably 15000 ppm / RH% or less, more preferably 10000 ppm / RH% or less, and even more preferably 9000 ppm / RH% or less. That is, the moisture expansion coefficient of the anionic group-containing heat-sealable resin is, for example, 1,000 ppm / RH% or more and 20,000 ppm / RH% or less, preferably 3,000 ppm / RH% or more and 15,000 ppm / RH% or less, more preferably 5,000 ppm / RH% or more and 10,000 ppm / RH% or less, and even more preferably 6,000 ppm / RH% or more and 9,000 ppm / RH% or less. When the amount of the heat-sealable layer 5 is within the range described below, if the moisture expansion coefficient of the anionic group-containing heat-sealable resin is within the above range, particularly excellent water vapor barrier properties can be obtained. The moisture expansion coefficient is measured under the following conditions in accordance with the examples described below.

[0120] Sample size: 23 mm x 5 mm x 200 μm Chuck distance: 20 mm Measurement method: Tensile load method Load: 30 g Temperature: 20°C Measurement humidity range: 40 to 80 RH% Humidity increase conditions: Humidity was increased in stages. The humidity at each stage was 20 RH%, 40 RH%, 60 RH%, 70 RH%, and 80 RH%. The sample was held for 300 minutes at each humidity level (20 RH%, 40 RH%, 60 RH%, 70 RH%, and 80 RH%). Detection method: Total expansion method Chuck mass: 2 g

[0121] The anionic group-containing heat-sealable resin is prepared, for example, as a solution and / or dispersion in which it is dissolved and / or dispersed in a solvent. For example, the anionic group-containing heat-sealable resin is synthesized in a solvent. This results in a solution and / or dispersion of the anionic group-containing heat-sealable resin.

[0122] The solvent is not particularly limited, but examples thereof include water, methanol, ethanol, propanol, isopropanol, acetone, methyl ethyl ketone, ethyl acetate, tetrahydrofuran, and acetonitrile. These solvents can be used alone or in combination of two or more. The solids concentration of the sealing coating material is not particularly limited and can be appropriately set depending on the purpose and application.

[0123] More specifically, examples of the heat-sealable coating material include a polyolefin dispersion containing an anionic group-containing polyolefin resin, an acrylic emulsion containing an anionic group-containing (meth)acrylic resin, and a polyurethane dispersion containing an anionic group-containing polyurethane resin. A preferred example of the heat-sealable coating material is a polyolefin dispersion containing an anionic group-containing polyolefin resin.

[0124] The heat-sealable coating material can contain additives. That is, the heat-sealable coating material can contain the above-mentioned heat-sealable resin and additives. Examples of additives include heat stabilizers, antioxidants, light stabilizers, ultraviolet absorbers, plasticizers, antistatic agents, lubricants, antiblocking agents, pigments, dyes, crystal nucleating agents, and curing agents. These can be used alone or in combination of two or more. The amount and timing of addition of the additives can be appropriately determined depending on the purpose and application.

[0125] The solid content concentration of the heat-sealable coating material is, for example, 10% by mass or more, preferably 15% by mass or more, more preferably 20% by mass or more, and for example, 60% by mass or less, preferably 50% by mass or less, more preferably 40% by mass or less.

[0126] The application method of the heat-sealable coating material is not particularly limited. Examples of application methods include dip coating, gravure coating, reverse coating, roll coating, bar coating, spray coating, and air knife coating. The drying conditions of the gas barrier coating material are not particularly limited. For example, the drying temperature is, for example, 40°C or higher, preferably 50°C or higher. The drying temperature is, for example, 200°C or lower, preferably 180°C or lower. The drying time is, for example, 1 second or longer, preferably 30 seconds or longer. The drying time is, for example, 10 minutes or shorter, preferably 5 minutes or shorter.

[0127] This forms the heat seal layer 5. The amount (dry mass) of the heat seal layer 5 is set from the viewpoint of achieving both gas barrier properties and heat sealability.

[0128] More specifically, from the viewpoint of heat sealing property, the amount (dry mass) of the heat seal layer 5 is 1.0 g / m 2 More than 1.0 g / m 2 More preferably, 1.1 g / m 2 More preferably, 1.5 g / m 2 More preferably, 1.8 g / m 2 In addition, from the viewpoint of gas barrier properties, the amount (dry mass) of the heat seal layer 5 is 7.0 g / m 2 Preferably, 5.0 g / m or less 2 less than 4.9 g / m 2 More preferably, 4.0 g / m 2 Below, particularly preferably 3.5 g / m 2 The following is the result.

[0129] (5) Laminate The laminate 1 has a total thickness of, for example, 5 μm or more, or preferably 10 μm or more. The laminate 1 has a total thickness of, for example, 1 mm or less, or preferably 0.5 mm or less.

[0130] 2. Effects The laminate 1 includes a paper substrate 2, a gas barrier layer 4, and a heat seal layer 5, and the amount of the heat seal layer 5 is adjusted to fall within the above-mentioned predetermined range. Therefore, the laminate 1 has both excellent gas barrier properties (oxygen barrier properties and water vapor barrier properties) and excellent heat seal properties.

[0131] More specifically, the heat seal layer 5 adsorbs oxygen and water vapor. 2 When the heat seal layer 5 is formed on the surface of the gas barrier layer 4, the gas barrier properties of the gas barrier layer 4 may be reduced.

[0132] In particular, when a paper substrate 2 is used as the substrate instead of a resin substrate, the gas barrier properties of the laminate 1 as a whole depend on the gas barrier properties of the gas barrier layer 4 .

[0133] Therefore, if the gas barrier properties of the gas barrier layer 4 are reduced by the heat seal layer 5, the gas barrier properties of the laminate 1 as a whole may become insufficient.

[0134] On the other hand, in order to prevent the gas barrier properties of the gas barrier layer 4 from being deteriorated, it has been considered to reduce the amount of the heat seal layer 5 laminated and thereby reduce the amount of oxygen and water vapor adsorbed.

[0135] However, if the amount of the heat seal layer 5 is reduced, there is a problem in that sufficient heat sealability (adhesion strength) cannot be obtained.

[0136] Therefore, in the laminate 1, the amount (dry mass) of the heat seal layer 5 is set within a particularly narrow range from the viewpoint of achieving both gas barrier properties and heat sealability. That is, in the laminate 1, the amount of the heat seal layer 5 is adjusted to the above-mentioned predetermined range.

[0137] Therefore, in the laminate 1, deterioration of the gas barrier property due to the heat seal layer 5 is suppressed, and excellent heat sealability is obtained. As a result, the laminate 1 has both excellent gas barrier property and excellent heat sealability.

[0138] 3. Uses The laminate 1 is suitable for use in various industrial fields that require gas barrier properties and heat sealability. More specifically, the laminate 1 is suitable for use as a packaging material. That is, the packaging material preferably contains the laminate 1, and more preferably consists of the laminate 1.

[0139] Such a packaging material has both excellent gas barrier properties and excellent heat sealing properties because it contains the laminate 1. Such a packaging material is used in various industrial fields. Preferably, the packaging material is used in the food packaging field.

[0140] 4. Modifications In the laminate 1 and packaging material described above, the sealing layer 3 is interposed between the paper base material 2 and the gas barrier layer 4, but the sealing layer 3 does not have to be interposed between the paper base material 2 and the gas barrier layer 4. For example, depending on the type of paper base material 2 and the type of gas barrier layer 4, the sealing layer 3 may be omitted.

[0141] As described above, the heat seal layer 5 may be laminated directly on the gas barrier layer 4. Alternatively, the heat seal layer 5 may be bonded to the gas barrier layer 4 with a known adhesive. In other words, an adhesive layer (not shown) may be interposed between the gas barrier layer 4 and the heat seal layer 5.

[0142] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are by mass unless otherwise specified. Furthermore, specific numerical values ​​such as blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be substituted with the corresponding upper limit values ​​(numeric values ​​defined as "equal to or less than") or lower limit values ​​(numeric values ​​defined as "equal to or more than" or "exceeding") of the blending ratios (content ratios), physical property values, parameters, etc. described in the above "Modes for Carrying Out the Invention."

[0143] 1. Paper Base Material Preparation Example 1 As the paper base material, one-sided glossy (bleached) kraft paper (product name: Hakugin, manufactured by Nippon Paper Industries Co., Ltd., basis weight 67 g / m 2 ) was prepared.

[0144] 2. Filler Coating Material Preparation Example 1 (Acrylic Emulsion) A reaction vessel equipped with a stirrer, a reflux condenser, a dropping device, and a thermometer was charged with 2,193 parts by mass of ion-exchanged water (solvent) and 2.5 parts by mass of sodium dodecyl sulfate (surfactant). The contents of the reaction vessel were heated to 75°C while stirring and purging with nitrogen.

[0145] While maintaining the internal temperature of the reaction vessel at 75° C., 7.5 parts by mass of potassium persulfate (polymerization initiator) was added to the reaction vessel and dissolved in the contents of the reaction vessel. Thereafter, a monomer emulsion prepared in advance was continuously added dropwise to the reaction vessel over a period of 5 hours.

[0146] The monomer emulsion is a raw material composition containing the following components: Ion-exchanged water (solvent) 900 parts by mass Sodium dodecyl sulfate (surfactant) 5 parts by mass Acrylamide (raw material monomer) 25 parts by mass Methyl methacrylate (raw material monomer) 175 parts by mass 2-ethylhexyl acrylate (raw material monomer) 1088 parts by mass Methacrylic acid (raw material monomer) 80 parts by mass Styrene (raw material monomer) 1133 parts by mass

[0147] After the dropwise addition of the monomer emulsion was completed, the contents of the reaction vessel were aged for 3 hours. This allowed the raw material monomers to polymerize, yielding a (meth)acrylic resin. Also, an acrylic emulsion in which the (meth)acrylic resin was dispersed in water was obtained.

[0148] The acrylic emulsion was cooled to room temperature, and then ion-exchanged water and ammonia water (neutralizer) were added to the acrylic emulsion to adjust the solid content to 41% by mass and the pH to 8.0.

[0149] This resulted in an acrylic emulsion in which the (meth)acrylic resin was dispersed in water. The average particle size of the acrylic emulsion was 140 nm. The average particle size was measured by dynamic light scattering (measurement device FPAR-1000, manufactured by Otsuka Electronics Co., Ltd.) (the same applies hereinafter).

[0150] Thereafter, water was further added to the above acrylic emulsion (solid content concentration 41% by mass), and the mixture was mixed for 5 minutes using a mixer to prepare a sealing coating material (solid content concentration 40% by mass).

[0151] 3. Gas Barrier Coating Material Preparation Example 2 (Polyurethane Dispersion) (1) Primary PUD The following components were mixed and reacted under a nitrogen atmosphere at 65 to 70°C until the isocyanate group concentration (NCO%) reached 6.11% by mass or less. This gave a transparent isocyanate-terminated prepolymer reaction product liquid.

[0152] 1,3-xylylene diisocyanate (Takenate 500, 1,3-XDI, manufactured by Mitsui Chemicals, Inc.) 143.2 parts by mass Methylenebis(cyclohexyl isocyanate) (VestanatH 12 MDI, H 12 MDI (manufactured by Evonik) 25.0 parts by weight Ethylene glycol 29.2 parts by weight Trimethylolpropane 2.7 parts by weight Dimethylolpropionic acid 14.8 parts by weight Methyl ethyl ketone (solvent) 121.6 parts by weight

[0153] The reaction product liquid was then cooled to 40° C. Next, 11.0 parts by mass of triethylamine (TEA) was added to the reaction product liquid, thereby neutralizing the isocyanate-terminated prepolymer.

[0154] Next, the reaction product liquid was dispersed in 838.0 parts by mass of ion-exchanged water using a Homodisper. Next, an amine aqueous solution was added to the obtained dispersion liquid to carry out a chain extension reaction. The reaction product liquid of the chain extension reaction was aged for 1 hour. This resulted in a gas barrier polyurethane resin. The amine aqueous solution was a mixed liquid of 48.4 parts by mass of ion-exchanged water and 24.2 parts by mass of 2-((2-aminoethyl)amino)ethanol. Thereafter, methyl ethyl ketone and ion-exchanged water were distilled off from the reaction product liquid using an evaporator. This adjusted the solids concentration to 30% by mass.

[0155] As a result of the above, a primary polyurethane dispersion (primary PUD) in which the gas barrier polyurethane resin was dispersed in water was obtained.

[0156] The pH of the primary polyurethane dispersion (primary PUD) was 8.6, and the average particle size of the polyurethane dispersion (primary PUD) was 58 nm.

[0157] (2) Secondary PUD 20.2 parts by mass of water, 28.9 parts by mass of a dispersion of a swellable layered inorganic compound (product name: ME-300-B4T, synthetic mica, manufactured by Katakura Co-op Agri Co., Ltd., solid content 7.8%), and 0.5 parts by mass of 25% ammonia water (thickening inhibitor) were blended and mixed for 5 minutes in a mixer. This gave a dispersion of the additive.

[0158] Next, the additive dispersion (49.6 parts by mass in total) and 51.0 parts by mass of the primary PUD were mixed in a mixer for 5 minutes. This resulted in a secondary polyurethane dispersion (secondary PUD) in which the gas barrier polyurethane resin and the additive were dispersed in water. The solids concentration of the secondary PUD was 15% by mass. The secondary PUD was used as a gas barrier coating material.

[0159] 4. Heat-sealable coating material (1) Anionic group-containing heat-sealable resin Production Example 1 (polyolefin dispersion, potassium hydroxide neutralized product) 50 parts by mass of ethylene-acrylic acid copolymer and 50 parts by mass of ethylene-isobutyl acrylate-methacrylic acid copolymer were melt-kneaded to obtain a resin composition (anionic group-containing polyolefin resin) as an anionic group-containing heat-sealable resin.

[0160] The content of structural units derived from ethylene relative to the total amount of the ethylene-acrylic acid copolymer was 79.5% by mass, and the content of structural units derived from acrylic acid was 20.5% by mass.

[0161] Furthermore, relative to the total amount of the ethylene-isobutyl acrylate-methacrylic acid copolymer, the content of structural units derived from ethylene was 80.0% by mass, the content of structural units derived from isobutyl acrylate was 10.0% by mass, and the content of structural units derived from methacrylic acid was 10.0% by mass.

[0162] The above resin composition, 4.0 parts by mass of potassium hydroxide (neutralizing agent), and 140 parts by mass of deionized water were placed in a reaction vessel and stirred. The contents of the reaction vessel were heated to 150°C and kept at that temperature for 4 hours. This neutralized the resin composition with potassium hydroxide (neutralizing agent). In other words, a resin composition (anionic group-containing heat-sealable resin) neutralized with the neutralizing agent was obtained. The contents of the reaction vessel were then cooled to room temperature.

[0163] This resulted in an aqueous dispersion (Aqueous Dispersion 1) of the resin composition (Resin 1). The aqueous dispersion 1 was a polyolefin dispersion. The solids concentration of the aqueous dispersion 1 was 42 mass%. The average particle size of the aqueous dispersion 1 was 0.5 μm. The aqueous dispersion 1 was used as a heat-sealable coating material.

[0164] Production Example 2 (Polyolefin Dispersion, Sodium Hydroxide Neutralized Product) 2.5 parts by mass of sodium hydroxide was used instead of 4.0 parts by mass of potassium hydroxide. An aqueous dispersion (Aqueous Dispersion 2) of a resin composition (Resin 2) was obtained in the same manner as in Production Example 1. The solids concentration of Aqueous Dispersion 2 was 42% by mass. The average particle size of Aqueous Dispersion 2 was 0.6 μm. Aqueous Dispersion 2 was used as a heat-sealable coating material.

[0165] Production Example 3 (Polyolefin Dispersion, Ammonia Neutralized Product) 13.7 parts by mass of aqueous ammonia (25% by mass) was used instead of 4.0 parts by mass of potassium hydroxide. The amount of deionized water used was changed to 285 parts by mass. A water dispersion (Water Dispersion 3) of a resin composition (Resin 3) was otherwise obtained in the same manner as in Production Example 1. The solids concentration of Water Dispersion 3 was 25% by mass. The average particle size of Water Dispersion 3 was 0.6 μm. Water Dispersion 3 was used as a heat-sealable coating material.

[0166] Production Example 4 (Polyolefin Dispersion), Amine Neutralized Product: 11.7 parts by mass of diethylamine (DEA) was used instead of 4.0 parts by mass of potassium hydroxide. The amount of deionized water used was changed to 285 parts by mass. A water dispersion (Water Dispersion 4) of a resin composition (Resin 4) was otherwise obtained in the same manner as in Production Example 1. The solids concentration of Water Dispersion 4 was 25% by mass. The average particle size of Water Dispersion 4 was 0.5 μm. Water Dispersion 4 was used as a heat-sealable coating material.

[0167] Production Example 5 (Polyolefin Dispersion), Amine Neutralized Product: 5.0 parts by mass of methylamine (MA) was used instead of 4.0 parts by mass of potassium hydroxide. The amount of deionized water used was changed to 285 parts by mass. A water dispersion (Water Dispersion 5) of a resin composition (Resin 5) was otherwise obtained in the same manner as in Production Example 1. The solids concentration of Water Dispersion 5 was 25% by mass. The average particle size of Water Dispersion 5 was 0.6 μm. Water Dispersion 5 was used as a heat-sealable coating material.

[0168] (2) Moisture Swelling Coefficient The moisture swelling coefficient of each of the resin compositions of Production Examples 1 to 5 (that is, the anionic group-containing heat-sealable resin neutralized with a neutralizing agent) was measured by the following method.

[0169] More specifically, the heat-sealable coating materials of Production Examples 1 to 5 were poured into a polypropylene tray, dried overnight at room temperature, and then dried for 10 minutes at 100° C. to obtain a film. The amount of heat-sealable coating material was adjusted so that a film with a thickness of 200 μm was obtained.

[0170] Next, the 200 μm thick film was cut into 20 mm x 5 mm to obtain a sample (20 mm x 5 mm x 200 μm). The moisture expansion coefficient of the sample was measured under the following conditions using a moisture expansion measuring device (NETZSCH, HC-TMA4000SE, HC9700). The moisture expansion coefficient was measured in the range of 40 to 80 RH%. However, the resin composition of Production Example 1 broke before the humidity condition reached 80 RH%. Therefore, the moisture expansion coefficient of the resin composition of Production Example 1 was measured in the range of 40 to 70 RH%.

[0171] Sample size: 23 mm x 5 mm x 200 μm Chuck distance: 20 mm Measurement method: Tensile load method Load: 30 g Temperature: 20°C Measurement humidity range: 40 to 80 RH% Humidity increase conditions: Humidity was increased in stages. The humidity at each stage was 20 RH%, 40 RH%, 60 RH%, 70 RH%, and 80 RH%. The sample was held for 300 minutes at each humidity level (20 RH%, 40 RH%, 60 RH%, 70 RH%, and 80 RH%). Detection method: Total expansion method Chuck mass: 2 g

[0172] Tables 1 and 2 show the types of anionic group-containing heat-sealable resins and their moisture absorption expansion coefficients.

[0173] 5. Laminates Examples 1 to 12 and Comparative Examples 1 to 4 (Laminates) The sealing coating material (Preparation Example 1) was applied to the glossy side of a paper substrate (one-sided gloss kraft paper) using a bar coater. 2 The coating amount was adjusted so that the coating film of the filler coating material was then dried at 120° C. for 60 seconds, thereby forming a filler layer.

[0174] Next, a gas barrier coating material (Preparation Example 2) was applied to the surface of the sealing layer using a bar coater. 2 The coating amount was adjusted so that the coating film of the gas barrier coating material was then dried at 120° C. for 60 seconds, thereby forming a gas barrier layer on the surface of the filling layer.

[0175] Thereafter, the heat-sealable coating material shown in Tables 1 and 2 was applied to the surface of the gas barrier layer using a bar coater. 2 The amount of coating was adjusted so that the coating film of the heat-sealable coating material was 100%. The coating film of the heat-sealable coating material was then dried at 120°C for 60 seconds. This formed a heat-sealable layer on the surface of the gas barrier layer. The layer structure of the laminate was as follows:

[0176] Paper base material / Sealing layer / Gas barrier layer / Heat seal layer

[0177] The dry mass of the filling layer was calculated by subtracting the mass of the paper substrate from the total mass of the laminate (two layers) including the paper substrate and the filling layer.

[0178] The dry mass of the gas barrier layer was calculated by subtracting the total mass of the laminate (two layers) comprising the paper substrate and the filling layer from the total mass of the laminate (three layers) comprising the paper substrate, the filling layer, and the gas barrier layer.

[0179] The dry mass of the heat seal layer was calculated by subtracting the total mass of the laminate (3 layers) comprising the paper substrate, the sealing layer, and the gas barrier layer from the total mass of the laminate (4 layers) comprising the paper substrate, the sealing layer, the gas barrier layer, and the heat seal layer.

[0180] 6. Evaluation (1) Oxygen transmission rate (OTR) of laminated body Oxygen transmission rate (cc / m 2 The oxygen permeability (°C) and relative humidity (RH%) were measured using an oxygen permeability measuring device (MOCON, OX-TRAN 2 / 22H). The measurement conditions (temperature (°C) and relative humidity (RH%)) are shown in Tables 1 and 2.

[0181] (2) Water Vapor Transmission Rate (WVTR) of Laminate 2 The water vapor transmission rate (day) was measured using a water vapor transmission rate measuring device (MOCON, PARMATRAN-W 3 / 34 G). The measurement conditions (temperature (°C) and relative humidity (RH%)) are shown in Tables 1 and 2.

[0182] (3) Heat-seal strength Two of each laminate were prepared. The heat-sealable layers of the two laminates were brought into contact with each other and subjected to heat-sealing at 140°C for 1 second and 2 kg / cm. 2 The heat seal strength (kg / 15 mm) was measured using an Intesco tensile tester (product number 201X). The results are shown in Tables 1 and 2.

[0183]

[0184]

[0185] The above invention is provided as an exemplary embodiment of the present invention, but it is merely an example and should not be interpreted as being limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.

[0186] The laminate and packaging material of the present invention are suitable for use in the field of food packaging materials.

[0187] REFERENCE SIGNS LIST 1 laminate 2 substrate 3 sealing layer 4 gas barrier layer 5 heat seal layer

Claims

1. A paper substrate, a gas barrier layer disposed on at least one side of the paper substrate, and a heat seal layer disposed on at least one side of the gas barrier layer, wherein the amount of the heat seal layer is 1.0 g / m 2 7.0g / m or more 2 The laminate is as follows:

2. The laminate according to claim 1, wherein a sealing layer is interposed between the paper substrate and the gas barrier layer.

3. The laminate according to claim 1, wherein the gas barrier layer contains a gas barrier resin.

4. The laminate according to claim 3, wherein the gas barrier resin contains a gas barrier polyurethane resin.

5. The laminate according to claim 4, wherein the gas barrier polyurethane resin contains a reaction product of an isocyanate-terminated prepolymer and a chain extender, the isocyanate-terminated prepolymer contains a reaction product of a polyisocyanate component and an active hydrogen group-containing component, the polyisocyanate component contains xylylene diisocyanate and / or hydrogenated xylylene diisocyanate, and the active hydrogen group-containing component contains a short-chain diol having 2 to 6 carbon atoms and an active hydrogen compound containing an anionic group.

6. The laminate according to claim 1, wherein the heat seal layer contains an anionic group-containing heat sealable resin, and the anionic group-containing heat sealable resin contains at least one resin selected from the group consisting of an anionic group-containing polyolefin resin, an anionic group-containing (meth)acrylic resin, and an anionic group-containing polyurethane resin.

7. The laminate according to claim 6, wherein the anionic group-containing heat-sealable resin is neutralized with a neutralizing agent, and the neutralizing agent contains at least one selected from the group consisting of alkali metal hydroxides, ammonia and amine compounds.

8. The laminate according to claim 6, wherein the anionic group-containing heat sealable resin has a moisture absorption expansion coefficient of 5,000 ppm / RH % or more and 10,000 ppm / RH % or less.

9. A packaging material comprising the laminate according to claim 1.

Citation Information

Patent Citations

  • Polyurethane laminated body

    JP2015044396A

  • Laminate

    JP2021115802A

  • Barrier paper

    JP2022155999A

  • Aqueous dispersion of ethylenic resin, and film of ethylenic resin obtained from the aqueous dispersion

    JP2001049054A

  • Barrier packaging material

    JP2021020398A

Cited By

  • Aqueous dispersion, adhesive composition for dry lamination, laminate, and method for manufacturing the laminate.

    JP7941407B1