Two-part curable resin composition and laminated body
The two-component curable resin composition, with a hydroxyl group-containing acrylic resin and alicyclic structure-containing vinyl monomers, addresses the adhesion issues in conventional paints by ensuring strong bonding to various substrates, improving the coating's durability and performance.
Patent Information
- Application Number
- PCT/JP2024/010899
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional two-component curable resin compositions used in vehicle and home appliance paints often experience decreased adhesion between the substrate and the coating layer, depending on the type of substrate, leading to suboptimal performance.
A two-component curable resin composition featuring a hydroxyl group-containing acrylic resin copolymerized with alicyclic structure-containing vinyl monomers, where the alicyclic structure-containing vinyl monomer content is between 15.0% to 60.0% by mass, and the glass transition temperature and SP value are within specific ranges, ensuring excellent adhesion to various substrates.
The composition achieves excellent adhesion to multiple substrate types, enhancing the durability and performance of the coating layer by maintaining strong bonding between the substrate and the cured resin coating.
Smart Images

Figure JP2024010899_03102024_PF_FP_ABST
Abstract
Description
Two-component curable resin composition and laminate
[0001] The present invention relates to a two-component curable resin composition and a laminate.
[0002] BACKGROUND ART Two-component curable resin compositions containing a base agent containing a hydroxyl group-containing acrylic resin and a curing agent have been known in the fields of vehicle paints and home appliance paints.
[0003] As such a two-component curable resin composition, for example, a clear coating composition containing a hydroxyl group-containing acrylic resin and a polyisocyanate compound has been proposed (see, for example, Patent Document 1).
[0004] JP 2015-66543 A
[0005] Such a two-component curable resin composition is used by applying it to a substrate. Specifically, the two-component curable resin composition is applied to a substrate and then cured to form a coating layer made of a cured product of the two-component curable resin composition.
[0006] On the other hand, depending on the type of substrate, the adhesion between the substrate and the coating layer may decrease.
[0007] The present invention provides a two-component curable resin composition that has excellent adhesion to many types of substrates, and a laminate that includes, in order, a coating made of a cured product of the two-component curable resin composition.
[0008] The present invention [1] provides a composition for a composition comprising a base agent and a curing agent, wherein the base agent comprises a hydroxyl group-containing acrylic resin, the hydroxyl group-containing acrylic resin being a copolymer of polymerization components comprising a hydroxyl group-containing (meth)acrylate and an alicyclic structure-containing vinyl monomer, the alicyclic structure-containing vinyl monomer being composed of a bicycloalkyl group-containing vinyl monomer and / or a cycloalkyl group-containing vinyl monomer, the content of the alicyclic structure-containing vinyl monomer being 15.0 mass% or more and 60.0 mass% or less relative to the polymerization components, the glass transition temperature of the hydroxyl group-containing acrylic resin being 10°C or more, and the SP value of the hydroxyl group-containing acrylic resin being 9.40 (cal / cm 3 ) 1/2 11.00 (cal / cm) 3) 1/2 or less, and the hydroxyl value of the hydroxyl group-containing acrylic resin is less than 100 mgKOH / g.
[0009] The present invention [2] includes the two-component curing resin composition according to the above [1], wherein the glass transition temperature of the hydroxyl group-containing acrylic resin is 60°C or higher.
[0010] The present invention [3] includes the two-component curing resin composition according to the above [1] or [2], in which the content of the alicyclic structure-containing vinyl monomer is 30.1 mass% or more relative to the polymerization components, and the glass transition temperature of the hydroxyl group-containing acrylic resin is 130°C or less.
[0011] The present invention [4] includes the two-component curing resin composition according to any one of the above [1] to [3], wherein the curing agent includes a (poly)isocyanate.
[0012] The present invention [5] includes a laminate comprising, in order, a substrate and a coating layer made of a cured product of the two-component curing resin composition according to any one of the above [1] to [4].
[0013] The present invention [6] includes the laminate according to the above [5], wherein the substrate is one selected from the group consisting of nylon, stainless steel, and glass.
[0014] In the two-component curing resin composition of the present invention, the base resin contains a hydroxyl-containing acrylic resin, which is a copolymer of polymerization components including a hydroxyl-containing (meth)acrylate and an alicyclic-structure-containing vinyl monomer. The content of the alicyclic-structure-containing vinyl monomer is within a predetermined range relative to the polymerization components. The glass transition temperature, SP value, and hydroxyl value of the hydroxyl-containing acrylic resin are within predetermined ranges. Therefore, a coating layer obtained using this two-component curing resin composition has excellent adhesion to many types of substrates.
[0015] The laminate of the present invention has a coating layer made of a cured product of the two-component curing resin composition of the present invention, and therefore has excellent adhesion to many types of substrates.
[0016] Figure 1 shows one embodiment of the method for producing a laminate of the present invention. Figure 1A shows the first step of preparing a substrate. Figure 1B shows the second step of applying a two-component curing resin composition to the surface of the substrate (one surface in the thickness direction) to form a coating film. Figure 1C shows the third step of heating the coating film to form a coating layer.
[0017] The two-component curing resin composition contains a base component and a curing agent. The base component and the curing agent are each prepared as independent packages. When using the two-component curing resin composition, the base component and the curing agent are mixed together.
[0018] 1. Base The base contains an acrylic resin containing a hydroxyl group.
[0019] <Hydroxyl Group-Containing Acrylic Resin> The hydroxyl group-containing acrylic resin is a copolymer of polymerization components containing a hydroxyl group-containing (meth)acrylate and an alicyclic structure-containing vinyl monomer. Here, (meth)acrylate refers to acrylate and / or methacrylate.
[0020] [Hydroxyl Group-Containing (Meth)acrylate] Examples of the hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, hydroxybutyl (meth)acrylate, 2,2-dihydroxymethylbutyl (meth)acrylate, polyhydroxyalkyl maleate, and polyhydroxyalkyl fumarate. Preferred examples of the hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl (meth)acrylate. More preferred examples of the hydroxyl group-containing (meth)acrylate include 2-hydroxyethyl methacrylate.
[0021] The hydroxyl group-containing (meth)acrylates can be used alone or in combination of two or more kinds.
[0022] The content of the hydroxyl group-containing (meth)acrylate relative to the polymerization components is, for example, 5.0 mass % or more, preferably 8.0 mass % or more, and for example, 20.0 mass % or less, preferably 15.0 mass % or less.
[0023] [Alicyclic Structure-Containing Vinyl Monomer] The alicyclic structure-containing vinyl monomer comprises a bicycloalkyl group-containing vinyl monomer and / or a cycloalkyl group-containing vinyl monomer.
[0024] Examples of the bicycloalkyl group-containing vinyl monomer include isobornyl(meth)acrylate, bicycloheptyl(meth)acrylate, bicyclooctyl(meth)acrylate, and decahydro-2-2-naphthyl(meth)acrylate. A preferred example of the bicycloalkyl group-containing vinyl monomer is isobornyl(meth)acrylate. A more preferred example of the bicycloalkyl group-containing vinyl monomer is isobornyl methacrylate.
[0025] Examples of the cycloalkyl group-containing vinyl monomer include cyclopentyl (meth)acrylate and cyclohexyl (meth)acrylate. Preferred examples of the cycloalkyl group-containing vinyl monomer include cyclohexyl (meth)acrylate. More preferred examples of the cycloalkyl group-containing vinyl monomer include cyclohexyl methacrylate.
[0026] As the alicyclic structure-containing vinyl monomer, from the viewpoint of improving adhesion to many types of substrates, a bicycloalkyl group-containing vinyl monomer is preferably used.
[0027] The alicyclic structure-containing vinyl monomer can be used alone or in combination of two or more types. Preferably, a bicycloalkyl group-containing vinyl monomer is used alone, and a cycloalkyl group-containing vinyl monomer is used alone. That is, preferably, the alicyclic structure-containing vinyl monomer is composed of a bicycloalkyl group-containing vinyl monomer or a cycloalkyl group-containing vinyl monomer. More preferably, a bicycloalkyl group-containing vinyl monomer is used alone. That is, more preferably, the alicyclic structure-containing vinyl monomer is composed of a bicycloalkyl group-containing vinyl monomer, but does not contain a cycloalkyl group-containing vinyl monomer.
[0028] The content of the alicyclic structure-containing vinyl monomer is, relative to the polymerization components, 15.0% by mass or more, preferably 20.0% by mass or more, more preferably 30.0% by mass or more, even more preferably more than 30.0% by mass, particularly preferably 30.1% by mass or more, most preferably 40.0% by mass or more, even more preferably 45.0% by mass or more, and is 60.0% by mass or less, preferably 55.0% by mass or less.
[0029] When the content of the alicyclic structure-containing vinyl monomer is within the above range, the adhesiveness to many types of substrates can be improved.
[0030] On the other hand, if the content of the alicyclic structure-containing vinyl monomer is outside the above range, it is not possible to improve the adhesion to many types of substrates.
[0031] [Other Ring Structure-Containing Vinyl Monomers] The alicyclic structure-containing vinyl monomer may also contain other ring structure-containing vinyl monomers.
[0032] The other ring structure-containing vinyl monomers are vinyl monomers having a ring structure other than the above-mentioned alicyclic structure-containing vinyl monomers, and examples thereof include tricycloalkyl group-containing vinyl monomers and aromatic ring-containing vinyl monomers.
[0033] An example of a tricycloalkyl group-containing vinyl monomer is adamantyl (meth)acrylate.
[0034] Examples of aromatic ring-containing vinyl monomers include styrene, vinyl toluene, and α-methyl styrene.
[0035] The content of the other ring structure-containing vinyl monomers relative to the polymerization components is, for example, 1 mass % or more, preferably 10 mass % or more, and for example, 20 mass % or less.
[0036] [Copolymerizable Monomer] The polymerization components may also contain copolymerizable monomers copolymerizable with the hydroxyl group-containing (meth)acrylate, alicyclic structure-containing vinyl monomer, and other ring structure-containing vinyl monomers.
[0037] Examples of copolymerizable vinyl monomers include alkyl (meth)acrylates, cyano group-containing vinyl monomers, and carboxyl group-containing vinyl monomers.
[0038] Examples of alkyl (meth)acrylates include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, pentyl (meth)acrylate, isopentyl (meth)acrylate, and hexyl (meth)acrylate. Examples of cyano group-containing vinyl monomers include (meth)acrylonitrile. Examples of carboxyl group-containing vinyl monomers include (meth)acrylic acid, fumaric acid, maleic acid, and itaconic acid.
[0039] The copolymerizable vinyl monomer is preferably an alkyl(meth)acrylate. The copolymerizable vinyl monomer is more preferably an alkyl(meth)acrylate having 1 to 4 carbon atoms. The copolymerizable vinyl monomer is further preferably methyl(meth)acrylate and butyl(meth)acrylate. The copolymerizable vinyl monomer is particularly preferably methyl methacrylate and butyl acrylate.
[0040] The copolymerizable vinyl monomers can be used alone or in combination of two or more kinds.
[0041] The content of the copolymerizable vinyl monomer relative to the polymerization components is, for example, 40.0 mass% or more, and, for example, 85.0 mass% or less, preferably 75.0 mass% or less, more preferably 65.0 mass% or less, even more preferably 55.0 mass% or less, and particularly preferably 45.0 mass% or less.
[0042] The above-mentioned hydroxyl group-containing (meth)acrylate, alicyclic structure-containing vinyl monomer, other cyclic structure-containing vinyl monomer, and copolymerizable monomer are biomass-derived monomers from the viewpoint of reducing environmental impact. In other words, the hydroxyl group-containing acrylic resin is preferably a copolymer of polymerization components including biomass-derived monomers. The biomass content of such hydroxyl group-containing acrylic resin is, for example, 15% or more, preferably 20% or more, more preferably 25% or more, even more preferably 30% or more, and particularly preferably 35% or more.
[0043] The hydroxyl group-containing acrylic resin can be obtained by polymerizing polymerization components.
[0044] The polymerization method is not particularly limited, and examples of the polymerization method include bulk polymerization and solution polymerization.
[0045] When solution polymerization is employed as the polymerization method, the polymerization components and, if necessary, a polymerization initiator are blended in a solvent (for example, butyl acetate) and polymerization is carried out.
[0046] Examples of the polymerization initiator include known thermal polymerization initiators (for example, azo-based radical polymerization initiators (for example, azobisisobutyronitrile) and peroxide-based radical polymerization initiators (for example, t-butylperoxy-2-ethylhexanoate).
[0047] As a result, an acrylic resin containing hydroxyl groups (a solution of an acrylic resin containing hydroxyl groups) is obtained.
[0048] In the solution containing the hydroxyl group-containing acrylic resin, the solids concentration of the hydroxyl group-containing acrylic resin is, for example, 20 mass % or more, preferably 40 mass % or more, and for example, 70 mass % or less.
[0049] The glass transition temperature of the hydroxyl group-containing acrylic resin is 10°C or higher, preferably 30°C or higher, more preferably 50°C or higher, and even more preferably 56°C or higher. From the viewpoint of further improving adhesion, it is particularly preferably 60°C or higher, most preferably 70°C or higher, and even more preferably 75°C or higher, and for example, 130°C or lower, preferably 115°C or lower, more preferably 105°C or lower, even more preferably 95°C or lower, and especially preferably 85°C or lower.
[0050] When the glass transition temperature is equal to or higher than the lower limit, the adhesiveness to many types of substrates can be improved.
[0051] On the other hand, if the glass transition temperature is below the lower limit, it is not possible to improve the adhesion to many types of substrates.
[0052] Furthermore, if the glass transition temperature is equal to or lower than the upper limit, the adhesiveness to many types of substrates can be improved.
[0053] The glass transition temperature can be calculated by the FOX formula, in which the Tg of each polymerization component (each monomer) can be determined from the values listed in Table 10-2 (Main raw material monomers for acrylic resins for paints) on pages 168-169 of "New Polymer Library, Vol. 7, Introduction to Synthetic Resins for Paints" (Kiyozo Kitaoka, Polymer Publishing Association, Kyoto, 1974).
[0054] The SP value of the acrylic resin containing hydroxyl groups is 9.40 (cal / cm 3 ) 1/2 Above, 11.00 (cal / cm 3 ) 1/2 Preferably, 10.50 (cal / cm 3 ) 1/2 or less, more preferably 10.00 (cal / cm 3 ) 1/2 More preferably, 9.80 (cal / cm 3 ) 1/2 The following is the result.
[0055] When the SP value is equal to or greater than the lower limit, the adhesion to many types of substrates can be improved.
[0056] On the other hand, if the SP value is less than the lower limit, it is not possible to improve the adhesion to many types of substrates.
[0057] Furthermore, if the SP value is equal to or less than the upper limit, the adhesion to many types of substrates can be improved.
[0058] On the other hand, if the SP value exceeds the upper limit, it is not possible to improve the adhesion to many types of substrates.
[0059] The SP value can be determined by a known method (described in RF Fedors, Polym. Eng. Sci., 14, (2), pp. 147-154 (1974)).
[0060] The hydroxyl value of the hydroxyl group-containing acrylic resin is less than 100 mgKOH / g, preferably 80 mgKOH / g or less, more preferably 60 mgKOH / g or less, even more preferably 50 mgKOH / g or less, and for example, 10 mgKOH / g or more, preferably 30 mgKOH / g or more.
[0061] When the hydroxyl value is less than the upper limit, adhesion to many types of substrates can be improved.
[0062] On the other hand, if the hydroxyl value is equal to or greater than the upper limit, it is not possible to improve the adhesion to many types of substrates.
[0063] Furthermore, when the hydroxyl value is equal to or greater than the lower limit, the adhesiveness to many types of substrates can be improved.
[0064] The hydroxyl value can be determined, for example, according to JIS K 0070-1992 (acetylation method).
[0065] As described above, in this two-component curing resin composition, the adhesion can be improved by setting the content ratio of the alicyclic structure-containing vinyl monomer relative to the polymerization components, the glass transition temperature of the hydroxyl group-containing acrylic resin, the SP value of the hydroxyl group-containing acrylic resin, and the hydroxyl value of the hydroxyl group-containing acrylic resin within predetermined ranges. In particular, from the viewpoint of further improving adhesion, the content ratio of the alicyclic structure-containing vinyl monomer relative to the polymerization components is set to 30.1 mass% or more, and the glass transition temperature of the hydroxyl group-containing acrylic resin is set to 130°C or less.
[0066] The weight average molecular weight (Mw) of the hydroxyl group-containing acrylic resin, measured by gel permeation chromatography (GPC) in terms of polystyrene, is, for example, 5,000 or more, preferably 10,000 or more, and for example, 100,000 or less, preferably 50,000 or less.
[0067] When two or more types of hydroxyl group-containing acrylic resins are used in combination, the average value of the weight average molecular weights (Mw) of these hydroxyl group-containing acrylic resins is adjusted to fall within the above-mentioned range.
[0068] The hydroxyl group-containing acrylic resins can be used alone or in combination of two or more kinds.
[0069] The content of the hydroxyl group-containing acrylic resin relative to the base resin is, for example, 80 mass % or more, preferably 90 mass % or more, more preferably 95 mass % or more, and for example, 100 mass % or less.
[0070] <Other Components> The base resin may contain other components in addition to the hydroxyl group-containing acrylic resin, if necessary.
[0071] Other components include, for example, castor oil, polyacrylic resin, polyester resin, and low molecular weight polyol.
[0072] From the viewpoint of improving adhesion, the base resin preferably does not contain any other components and is made of an acrylic resin containing a hydroxyl group.
[0073] <Preparation of Base Component> The base component is prepared by mixing the hydroxyl group-containing acrylic resin (a solution of the hydroxyl group-containing acrylic resin) with other components that are blended as required.
[0074] 2. Curing Agent The curing agent includes a (poly)isocyanate (isocyanate and / or polyisocyanate). The curing agent is preferably composed of a polyisocyanate.
[0075] Examples of polyisocyanates include aliphatic polyisocyanates, alicyclic polyisocyanates, aromatic polyisocyanates, and araliphatic polyisocyanates.
[0076] Examples of aliphatic polyisocyanates include aliphatic diisocyanates. Examples of aliphatic diisocyanates include 1,6-hexamethylene diisocyanate (1,6-HDI), 1,5-pentamethylene diisocyanate (1,5-PDI), tetramethylene diisocyanate, trimethylene diisocyanate, 1,2-, 2,3-, or 1,3-butylene diisocyanate, and 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate. Preferred examples of aliphatic polyisocyanates include 1,6-HDI and 1,5-PDI. More preferred examples of aliphatic polyisocyanates include 1,6-HDI.
[0077] Examples of alicyclic polyisocyanates include alicyclic diisocyanates, such as 3-isocyanatomethyl-3,5,5-trimethylcyclohexyl isocyanate (isophorone diisocyanate, IPDI), 4,4'-, 2,4'-, or 2,2'-methylenebis(cyclohexyl isocyanate), or mixtures thereof (H 12 MDI), 1,3- or 1,4-bis(isocyanatomethyl)cyclohexane or a mixture thereof (H 6bis(isocyanatomethyl)norbornane (NBDI), 1,3-cyclopentene diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, methyl-2,4-cyclohexane diisocyanate, and methyl-2,6-cyclohexane diisocyanate.
[0078] Examples of aromatic polyisocyanates include aromatic diisocyanates, such as 4,4'-, 2,4'-, or 2,2'-diphenylmethane diisocyanate or a mixture thereof (MDI), 2,4- or 2,6-tolylene diisocyanate or a mixture thereof (TDI), o-tolidine diisocyanate, 1,5-naphthalene diisocyanate (NDI), m- or p-phenylene diisocyanate or a mixture thereof, 4,4'-diphenyl diisocyanate, and 4,4'-diphenyl ether diisocyanate.
[0079] Examples of araliphatic polyisocyanates include araliphatic diisocyanates, such as xylylene diisocyanate (1,2-, 1,3-, or 1,4-xylylene diisocyanate or a mixture thereof) (XDI), 1,3- or 1,4-tetramethylxylylene diisocyanate or a mixture thereof (TMXDI), and ω,ω'-diisocyanato-1,4-diethylbenzene.
[0080] The polyisocyanate also includes derivatives of the polyisocyanate.
[0081] Examples of polyisocyanate derivatives include isocyanurate derivatives, allophanate derivatives, polyol derivatives, biuret derivatives, urea derivatives, oxadiazinetrione derivatives, carbodiimide derivatives, uretdione derivatives, and uretonimine derivatives of the above-mentioned polyisocyanates.Preferably, the polyisocyanate derivatives include isocyanurate derivatives and biuret derivatives.More preferably, the polyisocyanate derivatives include isocyanurate derivatives.
[0082] The polyisocyanate is preferably a polyisocyanate derivative. More preferably, the polyisocyanate is an isocyanurate derivative of 1,6-HDI, a biuret derivative of 1,6-HDI, and an isocyanurate derivative of 1,5-PDI. Even more preferably, the polyisocyanate is an isocyanurate derivative of 1,6-HDI and a biuret derivative of 1,6-HDI.
[0083] The polyisocyanates can be used alone or in combination of two or more kinds.
[0084] 3. Additives The two-component curable resin composition may contain additives in an appropriate ratio, if necessary.
[0085] Examples of additives include catalysts (e.g., dioctyltin dilaurate, bismuth carboxylate, titanium, aluminum catalysts, and amine catalysts), plasticizers, antiblocking agents, heat stabilizers, light stabilizers, antioxidants, release agents, pigments, pigment dispersants, dyes, lubricants, fillers, thixotropic agents, leveling agents, and hydrolysis inhibitors.
[0086] The timing of blending the additives is set appropriately. Specifically, the additives can be blended in advance with the base resin and / or curing agent, or the additives can be blended when the base resin and curing agent are mixed.
[0087] The additives can be used alone or in combination of two or more kinds.
[0088] 4. Preparation of Two-Part Curing Resin Composition In a two-part curing resin composition, the base resin and the curing agent are prepared separately and then mixed immediately before use. When the base resin and / or the curing agent are prepared as a solution, the two-part curing resin composition is prepared as a solution.
[0089] Regarding the blending ratio of the base agent and the curing agent, particularly when the curing agent is polyisocyanate, the equivalent ratio (NCO / OH) of the isocyanate groups of the polyisocyanate in the curing agent to the hydroxyl groups of the hydroxyl group-containing acrylic resin in the base agent is, for example, 0.7 or more, preferably 0.9 or more, and for example, 2.0 or less, preferably 1.5 or less, more preferably 1.1 or less.
[0090] In this way, a two-component curable resin composition is prepared.
[0091] 5. Method for Producing Laminate (Method for Using Two-Part Curable Resin Composition) The two-part curable resin composition is used, for example, to coat the surface of a substrate. By coating the substrate, a laminate is produced.
[0092] One embodiment of a method for manufacturing a coating and laminate will now be described with reference to Figures 1-1C.
[0093] 1A to 1C, the up-down direction of the paper surface is the up-down direction (thickness direction), and the upper side of the paper surface is the upper side (one side in the thickness direction), and the lower side of the paper surface is the lower side (the other side in the thickness direction). Also, the left-right direction and the depth direction of the paper surface are surface directions perpendicular to the up-down direction. Specifically, they conform to the directional arrows in each figure.
[0094] The method for manufacturing the laminate 1 includes a first step of preparing a substrate 2, a second step of applying a two-component curing resin composition to the surface (one surface in the thickness direction) of the substrate 2 to form a coating film 3, and a third step of heating the coating film 3 to form a coating layer 4.
[0095] [First Step] In the first step, as shown in FIG. 1A, first, a substrate 2 is prepared.
[0096] The substrate 2 is a body to be coated, and the coating layer 4 imparts various physical properties to its surface (one surface in the thickness direction).
[0097] In FIG. 1A, the substrate 2 has a flat plate shape, but the shape of the substrate 2 is not particularly limited, and various shapes can be selected.
[0098] The substrate 2 is not particularly limited, but examples thereof include resin, metal, and glass.
[0099] Examples of resins include polyester resins, (meth)acrylic resins (including acrylic resins and / or methacrylic resins), polyolefin resins, polycarbonate resins, polyamide resins, polyimide resins, acrylonitrile-styrene-butadiene copolymer resins (ABS resins), polystyrene resins, polyvinylidene chloride, styrene-acrylonitrile copolymer resins, and cellulose acetate. Examples of polyester resins include polyethylene terephthalate (PET), polybutylene terephthalate, and polyethylene naphthalate. Examples of (meth)acrylic resins include polymethyl methacrylate resins (PMMA). Examples of polyolefin resins include polyethylene resins and polypropylene resins. Examples of polyamide resins include nylon. Examples of resins include polyamide resins. Examples of resins include nylon.
[0100] Examples of the metal include iron, aluminum, zinc, steel plate, and stainless steel. Preferably, the metal is stainless steel.
[0101] From the viewpoint of heat resistance and chemical resistance, the substrate 2 is preferably one selected from the group consisting of nylon, stainless steel, and glass.
[0102] If necessary, the substrate 2 may be subjected to a surface treatment. If necessary, a primer may be formed on the substrate 2 in advance.
[0103] [Second Step] In the second step, as shown in FIG. 1B, a two-component curable resin composition is applied to the surface (one surface in the thickness direction) of the substrate 2 to form a coating film 3.
[0104] Examples of the coating method include spray coating, dip coating, roll coating, gravure coating, spin coating, bar coating, and doctor blade coating. Preferred examples of the coating method include bar coating and spray coating.
[0105] As a result, a coating film 3 which is a coating of the two-component curable resin composition (a solution of the two-component curable resin composition) is formed on the surface (one surface in the thickness direction) of the substrate 2 .
[0106] [Third Step] In the third step, as shown in FIG. 1C, the coating film 3 is heated to form a coating layer 4.
[0107] Regarding the heating conditions, the heating temperature is, for example, 120° C. or less, preferably 90° C. or less, or for example, 60° C. or more. The heating time is, for example, 1 minute or more, preferably 5 minutes or more, more preferably 10 minutes or more, or for example, 60 minutes or less, preferably 40 minutes or less.
[0108] The heating may be carried out in two or more stages, and may also be carried out under reduced pressure or in an inert atmosphere.
[0109] As a result, the coating film 3 dries and hardens, forming a coating layer 4 made of a hardened product of the coating film 3 (two-component curing resin composition).
[0110] The coating layer 4 has a thickness of 5 μm or more, preferably 10 μm or more, and for example, 50 μm or less, preferably 20 μm or less.
[0111] As described above, the laminate 1 having the substrate 2 and the coating layer 4 in this order is manufactured.
[0112] In the above description, the coating layer 4 is placed on the surface (one side in the thickness direction) of the substrate 2, but the coating layer 4 can also be placed on both sides of the substrate 2 (one side in the thickness direction and the other side in the thickness direction).
[0113] 6. Effects and Benefits In this two-component curing resin composition, the main component contains a hydroxyl-containing acrylic resin, which is a copolymer of polymerization components including a hydroxyl-containing (meth)acrylate and an alicyclic-structure-containing vinyl monomer. The content of the alicyclic-structure-containing vinyl monomer is within a predetermined range relative to the polymerization components. The glass transition temperature, SP value, and hydroxyl value of the hydroxyl-containing acrylic resin are within predetermined ranges. Therefore, the coating layer 4 obtained using this two-component curing resin composition has excellent adhesion to many types of substrates 2.
[0114] The laminate 1 has a coating layer 4 made of a cured product of a two-component curing resin composition, and therefore has excellent adhesion to many types of substrates 2.
[0115] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited to the following examples. Note that "parts" and "%" are by mass unless otherwise specified. Furthermore, specific numerical values such as blending ratios (content ratios), physical property values, parameters, etc. used in the following description can be substituted with the corresponding upper limit values (numeric values defined as "equal to or less than") or lower limit values (numeric values defined as "equal to or more than" or "exceeding") of the blending ratios (content ratios), physical property values, parameters, etc. described in the above "Modes for Carrying Out the Invention."
[0116] <Details of Components> Abbreviations for components used in each example and each comparative example are described in detail below. HEMA: 2-hydroxyethyl methacrylate, IBX: isobornyl methacrylate, CHMA: cyclohexyl methacrylate, ADMA: adamantyl methacrylate, St: styrene, MMA: methyl methacrylate, BA: butyl acrylate, EMA: ethyl methacrylate, 2EHA: 2-ethylhexyl acrylate, TKA-100: 1,6-HDI isocyanurate derivative, manufactured by Asahi Kasei Corporation, 24A-100: 1,6-HDI biuret derivative, manufactured by Asahi Kasei Corporation, D-370N: 1,5-PDI isocyanurate derivative, manufactured by Mitsui Chemicals, Inc., PMMA: polymethyl methacrylate resin, PC: polycarbonate, PC / ABS: polycarbonate and ABS alloy (Loa EFN800-04, manufactured by Sumitomo Bakelite), SUS304: stainless steel, 66Ny: nylon.
[0117] <Preparation of Two-Component Curing Resin Compositions> Examples 1 to 11 and Comparative Examples 1 to 11 (Preparation of Main Agent (Hydroxyl Group-Containing Acrylic Resin)) Under nitrogen, 710.4 parts by mass of butyl acetate was heated to 100°C. Next, a solution prepared by mixing 14.2 parts by mass of azobisisobutyronitrile with a total of 1,000 parts by mass of the polymerization components mixed in the mass% shown in Tables 1 and 2 was charged over 4 hours. The values shown in Tables 1 and 2 are in mass%.
[0118] After charging, the mixture was heated at 100°C for 1 hour, and then 1.64 parts by mass of t-butylperoxy-2-ethylhexanoate (Perbutyl O (NOF Corporation)) was added. This step of reacting at 100°C for another 1 hour was repeated twice, and then 229.0 g parts by mass of butyl acetate was added to obtain a solution of an acrylic resin containing hydroxyl groups (solid concentration 52%). This was used as the main agent.
[0119] (Preparation of Curing Agent) The curing agents shown in Tables 1 and 2 were prepared.
[0120] (Preparation of two-component curing resin composition) 30 parts by mass of the base agent (a solution of an acrylic resin containing hydroxyl groups (solids concentration 52%)), 2.27 parts by mass of a curing agent (TKA-100), and 39.17 g of butyl acetate were mixed. Next, 0.18 parts by mass of Neostan U810 (dioctyltin dilaurate, manufactured by Nitto Kasei Co., Ltd.) diluted to 1% by weight with butyl acetate was added. This resulted in a two-component curing resin composition. The equivalent ratio (NCO / OH) was as shown in Tables 1 and 2.
[0121] In Example 2, 30 parts by mass of the base agent (a solution of an acrylic resin containing hydroxyl groups (solid concentration 52%)), 2.16 parts by mass of a curing agent (24A-100), and 40.17 g of butyl acetate were mixed. Next, 0.18 parts by mass of Neostan U810 (dioctyltin dilaurate, manufactured by Nitto Kasei Co., Ltd.) diluted to 1% by weight with butyl acetate was added. This resulted in a two-component curing resin composition.
[0122] In Example 3, 30 parts by mass of the base agent (a solution of an acrylic resin containing hydroxyl groups (solids concentration 52%)), 2.05 parts by mass of a curing agent (24A-100), and 40.48 g of butyl acetate were mixed. Next, 0.18 parts by mass of Neostan U810 (dioctyltin dilaurate, manufactured by Nitto Kasei Co., Ltd.) diluted to 1% by weight with butyl acetate was added. This produced a two-component curable resin composition.
[0123] <Evaluation> [Production of Laminate] (First Step) PMMA, PC, PC / ABS, glass, SUS304 and 66Ny were prepared as substrates.
[0124] (Second Step) A solution of a two-component curable resin composition was applied to one surface in the thickness direction of each substrate using a bar coater #40 to form a coating film.
[0125] (Third Step) The coating film was heated and cured at 80° C. for 30 minutes, thereby forming a coating layer (film thickness: approximately 10 μm).
[0126] [Adhesion] Using a knife, 100 1 mm x 1 mm grid-like cross-cuts (100 squares) were made on the laminate of each Example and Comparative Example so as to reach the substrate. Next, adhesive tape was adhered to the surface, and the state of the coating layer after instantaneous peeling was visually observed. Adhesion was evaluated based on the following criteria. The results are shown in Tables 1 and 2. {Criteria} ⊚: The number of squares that adhered without peeling was 76 to 100. ◯: The number of squares that adhered without peeling was 51 to 75. Δ: The number of squares that adhered without peeling was 26 to 50. ×: The number of squares that adhered without peeling was 0 to 25.
[0127] The marks were assigned with 3 points for "◎", 2 points for "◯", 1 point for "△", and 0 point for "×", and the total of the marks for each substrate was calculated as a score. The results are shown in Tables 1 and 2.
[0128]
[0129]
[0130] The above invention is provided as an exemplary embodiment of the present invention, but this is merely an example and should not be interpreted as limiting. Modifications of the present invention that are obvious to those skilled in the art are intended to be included in the scope of the following claims.
[0131] The two-component curable resin composition and laminate of the present invention are suitably used in the fields of vehicle paints and home appliance paints.
[0132] REFERENCE SIGNS LIST 1 laminate 2 substrate 4 coating layer
Claims
1. A composition comprising a base agent and a curing agent, wherein the base agent comprises a hydroxyl group-containing acrylic resin, the hydroxyl group-containing acrylic resin is a copolymer of polymerization components comprising a hydroxyl group-containing (meth)acrylate and an alicyclic structure-containing vinyl monomer, the alicyclic structure-containing vinyl monomer is composed of a bicycloalkyl group-containing vinyl monomer and / or a cycloalkyl group-containing vinyl monomer, the content of the alicyclic structure-containing vinyl monomer is 15.0% by mass or more and 60.0% by mass or less relative to the polymerization components, the glass transition temperature of the hydroxyl group-containing acrylic resin is 10°C or more, and the SP value of the hydroxyl group-containing acrylic resin is 9.40 (cal / cm 3 ) 1/2 11.00 (cal / cm) 3 ) 1/2 or less, and the hydroxyl value of the hydroxyl group-containing acrylic resin is less than 100 mgKOH / g.
2. The two-component curing resin composition according to claim 1, wherein the glass transition temperature of the hydroxyl-containing acrylic resin is 60° C. or higher.
3. The two-component curing resin composition according to claim 1, wherein the content of the alicyclic structure-containing vinyl monomer is 30.1 mass% or more relative to the polymerization components, and the glass transition temperature of the hydroxyl group-containing acrylic resin is 130°C or less.
4. The two-component curing resin composition according to claim 1, wherein the curing agent comprises a (poly)isocyanate.
5. A laminate comprising, in order, a substrate and a coating layer made of a cured product of the two-component curing resin composition according to any one of claims 1 to 4.
6. The laminate according to claim 5, wherein the substrate is one selected from the group consisting of nylon, stainless steel and glass.
Citation Information
Patent Citations
Adhesive for print laminate
JP2008050489A
Substrate film forming method
JP2015217333A
Back sheet for solar battery module
JP2016111064A
Low infrared radiation coating composition
JP2020019903A
Aqueous multi-liquid type polyurethane coating composition
JP2020111723A
Cited By
Thermosetting resin composition, cured product, and laminate
WO2026141168A1