Multilayer piezoelectric body and method for producing same

The laminated piezoelectric material with a fluororesin film, antistatic, and hard coat layers addresses static and scratch issues, achieving high piezoelectricity and antiblocking while maintaining visibility, improving capacitive touch panel reliability.

WO2024203685A1PCT designated stage expired Publication Date: 2024-10-03KUREHA CORPORATION

Patent Information

Application Number
PCT/JP2024/010932
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Capacitive touch panels using piezoelectric films face issues with static electricity, scratch resistance, and coating unevenness, leading to reduced visibility and reliability, particularly with fluororesin-based films which have low piezoelectric constants and are prone to sticking due to poor surface properties.

Method used

A laminated piezoelectric material with a fluororesin-based film, an antistatic layer, and a hard coat layer, where the antistatic layer has a thickness of 10 nm to 250 nm and the hard coat layer has a maximum surface height Rz of 40 nm to 150 nm, providing antistatic and antiblocking properties while maintaining high piezoelectricity and transparency.

Benefits of technology

The solution achieves high piezoelectricity, antistatic properties, and antiblocking without reducing visibility, enhancing the reliability and performance of capacitive touch panels by adjusting the thickness and surface roughness of the antistatic and hard coat layers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Disclosed is a multilayer piezoelectric body which comprises: a piezoelectric film that contains a fluorine-based resin as a main component; an antistatic layer that is disposed on at least one surface of the piezoelectric film and has a thickness of 10 nm to 250 nm (inclusive); and a hard coating layer that is disposed on the antistatic layer and has a maximum height Rz of the surface of 40 nm to 150 nm (inclusive). The surface resistivity of the multilayer piezoelectric body as measured on the hard coating layer is 1.0 × 106 Ω / sq. to 1.0 × 1012 Ω / sq. (inclusive); the total light transmittance of the multilayer piezoelectric body is 85% or more; and the piezoelectric constant d33 is 7 pC / N to 40 pC / N (inclusive).
Need to check novelty before this filing date? Find Prior Art

Description

Multilayer piezoelectric element and its manufacturing method

[0001] The present invention relates to a laminated piezoelectric element and a method for manufacturing the same.

[0002] Touch panels are attached to the displays of electronic devices and are used to operate them. There are various types of touch panels, but the capacitive type is often used because it has a simple structure, is inexpensive to make, and can be made relatively large. However, capacitive touch panels are prone to malfunction due to the complex signal processing required.

[0003] Generally, a touch panel detects a two-dimensional position (position coordinates) on the touch panel surface by touching the surface with a finger, a pen, or the like. To avoid misidentification of inputs on a touch panel, it is desirable to separate selection and execution. Specifically, it is desirable to select a two-dimensional position on the touch surface and then execute the selection by applying pressure to the touch surface. Therefore, it has been studied to improve reliability by applying a pressure-sensitive sensor to the touch panel and further detecting the magnitude of pressure (see, for example, Patent Document 1).

[0004] As a pressure-sensitive sensor for touch panels, the use of piezoelectric films that generate voltage in response to pressure has been proposed. Known piezoelectric films include those containing polymeric materials such as polylactic acid and fluorine-based resins.

[0005] Although these piezoelectric films have excellent transparency, they are prone to charging due to friction and vibration, generating static electricity. Static electricity can easily attract foreign matter to the piezoelectric film, potentially resulting in a deterioration in quality. Furthermore, scratches on the film surface during handling can easily reduce visibility when used in touch panels. Therefore, there is a demand for piezoelectric films that are antistatic and scratch-resistant.

[0006] In contrast, Patent Document 2 discloses a laminated piezoelectric body including a piezoelectric film containing polylactic acid and a surface layer disposed thereon that contains a conductive material (A) and a polymer (B). In this document, the surface layer is a hard coat layer having antistatic properties, and therefore the laminated piezoelectric body is said to have good antistatic properties and scratch resistance.

[0007] JP 2010-26938 A International Publication No. 2016 / 098597

[0008] However, according to the investigations of the present inventors, the laminated piezoelectric body of Patent Document 2 has a problem in that the surface of the hard coat layer has poor slipperiness, and when wound into a roll, for example, the laminated piezoelectric bodies tend to adhere to each other and stick together (blocking). Also, the piezoelectric film containing polylactic acid used in Patent Document 2 has a piezoelectric constant d 14 However, since the piezoelectric constant is as low as 6.4 pC / N, it is difficult to obtain a sufficient piezoelectric effect.

[0009] In contrast, the inventors have found that the piezoelectric constant d 33 When an antistatic layer was formed on a piezoelectric film containing a fluororesin having high electrical conductivity and sufficient piezoelectric effect, a new problem was found in that coating spots occurred in the resulting laminated piezoelectric body, resulting in reduced visibility.

[0010] Therefore, there is a demand for a laminated piezoelectric material that exhibits high piezoelectricity and has anti-blocking and anti-static properties without reducing visibility.

[0011] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a laminated piezoelectric material having high piezoelectricity, anti-blocking properties, and anti-static properties without reducing visibility, and a method for manufacturing the same.

[0012] [1] A laminated piezoelectric body comprising: a piezoelectric film containing a fluorine-based resin as a main component; an antistatic layer having a thickness of 10 nm to 250 nm and disposed on at least one surface of the piezoelectric film; and a hard coat layer disposed on the antistatic layer and having a maximum surface height Rz of 40 nm to 150 nm, wherein the surface resistivity of the laminated piezoelectric body measured on the hard coat layer is 1.0×10 6Ω / sq. More than 1.0×10 12 Ω / sq. or less, the total light transmittance of the laminated piezoelectric body is 85% or more, and the piezoelectric constant d 33 A laminated piezoelectric element having a piezoelectric constant d of 7 pC / N or more and 40 pC / N or less. [2] The laminated piezoelectric element according to [1], wherein the fluororesin is a polymer containing, as a main component, a structural unit derived from vinylidene fluoride. [3] The laminated piezoelectric element according to [1] or [2], wherein the fluororesin is a vinylidene fluoride homopolymer. [4] The laminated piezoelectric element according to any one of [1] to [3], wherein the antistatic layer contains carbon nanotubes. [5] The laminated piezoelectric element according to any one of [1] to [4], wherein the hard coat layer has a thickness of 300 nm or more and 3000 nm or less. [6] The laminated piezoelectric element according to any one of [1] to [5], wherein the hard coat layer contains silica particles having an average particle diameter of 10 nm or more and 200 nm or less. [7] A method for producing a laminated piezoelectric element according to any one of [1] to [5], wherein the hard coat layer contains a fluororesin as a main component and has a piezoelectric constant d 33 A method for manufacturing a laminated piezoelectric body, comprising the steps of: preparing a piezoelectric film having a resistivity of 7 pC / N or more and 40 pC / N or less; applying an antistatic material to at least one surface of the piezoelectric film to form an antistatic layer; and applying a curable composition to the antistatic layer and curing the composition to form a hard coat layer. [8] The method for manufacturing a laminated piezoelectric body according to [7], wherein the step of preparing the piezoelectric film comprises forming a film containing a fluororesin as a main component by extrusion molding. [9] The method for manufacturing a laminated piezoelectric body according to [7] or [8], wherein the step of preparing the piezoelectric film comprises stretching a film containing a fluororesin as a main component and then subjecting it to a polarization treatment.

[10] The method for manufacturing a laminated piezoelectric body according to any one of [7] to [9], wherein the step of forming the antistatic layer comprises drying the piezoelectric film coated with the antistatic material by heat treatment at 100°C or more and 150°C or less.

[0013] According to the present invention, it is possible to provide a laminated piezoelectric material having high piezoelectricity, anti-blocking properties, and anti-static properties without reducing visibility, and a method for producing the same.

[0014] As described above, it has been newly discovered that a laminated piezoelectric element having a piezoelectric film containing a fluororesin as a main component causes coating irregularities, which were not an issue with a laminated piezoelectric element having a piezoelectric film made of polylactic acid.

[0015] According to the inventors' investigations, the coating irregularities are due to uneven coating of the antistatic layer. The uneven coating is thought to be caused by picking up minute irregularities on the surface of the piezoelectric film. The irregularities on the surface of the piezoelectric film are responsible for the high piezoelectric effect (piezoelectric constant d 33 It is believed that wrinkles are formed during the process of stretching or poling a film containing a fluororesin as a main component to develop the characteristic of the piezoelectric film. Specifically, it is believed that wrinkles occur on the surface of a piezoelectric film containing a fluororesin due to the disruption of the crystalline structure caused by the polarization process, which causes the fluororesin crystals to transition from α-type to β-type, and the relaxation of molecular chains associated with this change in crystalline structure. On the other hand, piezoelectric films made of polylactic acid have low crystallinity and are not subjected to polarization process, so it is believed that wrinkles are less likely to occur (or do not occur) on the surface of the piezoelectric film.

[0016] In contrast, in one embodiment of the present invention, the thickness of the antistatic layer disposed on the piezoelectric film containing a fluororesin is set to a predetermined value or less. If the antistatic layer is applied thickly, the antistatic layer will be applied thickly to the recessed portions of the piezoelectric film, resulting in large coating irregularities of the antistatic layer on the laminated piezoelectric element. In contrast, if the antistatic layer is applied thinly, thickness irregularities of the antistatic layer are reduced, and the variation caused by the unevenness of the surface of the piezoelectric film is also reduced, making it less likely that coating irregularities will occur. As a result, coating irregularities on the laminated piezoelectric element can be reduced, and a decrease in visibility can be suppressed.

[0017] Furthermore, by laminating the antistatic layer and a hard coat layer with an adjusted surface roughness (Rz) so that the surface resistivity is a predetermined value or less, it is possible to achieve a high level of both antiblocking properties and antistatic properties.

[0018] A laminated piezoelectric element according to one embodiment of the present invention and a method for manufacturing the same will be specifically described below.

[0019] 1. Laminated Piezoelectric Body The laminated piezoelectric body according to this embodiment includes a piezoelectric film, an antistatic layer, and a hard coat layer.

[0020] 1-1. Piezoelectric film Piezoelectric film is a film containing fluorine-based resin as its main component, and has a piezoelectric constant d 33 The piezoelectric constant d of the piezoelectric film is adjusted to 7 pC / N or more and 40 pC / N or less. 33 When the piezoelectric constant d of the piezoelectric film is 7 pC / N or more, the amount of charge generated by the piezoelectric effect is sufficient, and therefore high pressure sensitivity is easily obtained. 33 When the piezoelectric constant d of the piezoelectric film is 40 pC / N or less, for example, unevenness on the film surface caused by polarization treatment can be further reduced, and therefore, defects in appearance can be reduced. 33 is more preferably 10 pC / N or more and 35 pC / N or less, further preferably 10 pC / N or more and 27 pC / N or less, and particularly preferably 10 pC / N or more and 24 pC / N or less.

[0021] Piezoelectric constant d 33 is one of the indices that shows the polarization behavior when a certain pressure is applied. 33 The larger the σ, the greater the polarization that occurs when a certain pressure is applied, and the greater the charge density, and therefore the greater the degree of charging of the piezoelectric film.

[0022] Piezoelectric constant d of the piezoelectric film 33 is the direct quasi-static method (d 33 The piezoelectric constant d of the piezoelectric ceramic measured by the Meter method and the Berlincoat method 33 Test method: Piezoelectric constant d according to ISO 19622:2018 33 Specifically, a piezoelectric constant measuring device (for example, Piezometer System PM300 manufactured by PIEZOTEST) is used to clip a piezoelectric film sample with 1.0 N, and the generated charge is read when a force of 0.15 N, 110 Hz is applied.

[0023] Piezoelectric constant d of the piezoelectric film 33can be adjusted mainly by the type of resin contained in the piezoelectric film and the manufacturing conditions (conditions for polarization and stretching). For example, among fluorine-based resins, the more structural units derived from vinylidene fluoride a resin contains, the lower the piezoelectric constant d 33 In addition, by strengthening the polarization process or stretching process, the piezoelectric constant d 33 tends to become large.

[0024] As described above, the piezoelectric film contains a fluororesin as a main component. "Containing a fluororesin as a main component" means that the content of resins containing fluororesin as a structural unit (including the fluororesin itself) in the total mass of resins constituting the piezoelectric film is 50% by mass or more. The fluororesin content is preferably 60% by mass or more, and more preferably 80% by mass or more. The upper limit of the content is not particularly limited and may be 100% by mass or 90% by mass or less.

[0025] Among fluororesins, from the viewpoint that a high piezoelectric effect is easily obtained, the fluororesin is preferably a polymer containing a structural unit derived from vinylidene fluoride as a main component.

[0026] The content of the structural units derived from vinylidene fluoride contained as a main component in the polymer is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and particularly preferably 90% by mass or more, relative to the total amount of the structural units of the polymer. The higher the content, the more likely it is that a higher piezoelectric effect will be obtained. The upper limit of the content is not particularly limited and may be 100% by mass or 90% by mass or less.

[0027] The polymer may further contain a structural unit derived from a monomer copolymerizable with vinylidene fluoride, provided that the effects of the present invention are not impaired. Examples of the monomer copolymerizable with vinylidene fluoride include fluorine-containing monomers such as trifluoroethylene, tetrafluoroethylene, hexafluoropropylene, trifluorochloroethylene, and vinyl fluoride. Two or more of these monomers may be contained.

[0028] Among them, the piezoelectric constant d 33 From the viewpoint of easily increasing the size and increasing the sensitivity of a pressure-sensitive sensor to which a piezoelectric film is applied, vinylidene fluoride homopolymer is preferred.

[0029] The thickness of the piezoelectric film is preferably, for example, 25 μm or more and 120 μm or less. When the thickness of the piezoelectric film is 25 μm or more, the amount of charge generated by the piezoelectric effect becomes larger, and higher piezoelectricity is likely to be obtained. The thickness of the piezoelectric film is more preferably 30 μm or more, and even more preferably 35 μm or more. When the thickness of the piezoelectric film is 120 μm or less, the transparency of the piezoelectric film is less likely to be impaired, and 100 μm or less is more preferable, and 80 μm or less is even more preferable. From the same viewpoint, the thickness of the piezoelectric film is more preferably 35 μm or more and 80 μm or less.

[0030] 1-2. Antistatic Layer The antistatic layer has the function of preventing the laminated piezoelectric element from being charged. The antistatic layer is disposed on at least one surface of the piezoelectric film.

[0031] The surface resistivity of the antistatic layer is adjusted so that the surface resistivity measured on the hard coat layer falls within the range described below. Therefore, the surface resistivity of the antistatic layer is preferably lower than the surface resistivity measured on the hard coat layer, specifically, 1.0×10 4 Ω / sq. More than 1.0×10 9 Ω / sq. or less, and preferably 1.0×10 5 Ω / sq. More than 1.0×10 8 It is more preferable that the surface resistivity of the antistatic layer is 1.0×10 / sq. or less. 9 When the surface resistivity is Ω / sq. or less, the surface resistivity measured on the hard coat layer can be easily reduced, and sufficient antistatic properties can be easily imparted. The surface resistivity can be measured, for example, using a known resistivity meter in accordance with JIS K 6911.

[0032] The surface resistivity can be adjusted by the thickness of the antistatic layer and the type and content of the conductive material contained in the antistatic layer. For example, the thicker the antistatic layer, the lower the surface resistivity. Also, the higher the content of the conductive material, the lower the surface resistivity.

[0033] The antistatic layer includes a conductive material. In this embodiment, the antistatic layer may include a cured product of a curable composition including a conductive material, a polymerizable compound, and an optional curing agent.

[0034] The conductive material may be any material that provides the antistatic layer with a surface resistivity in the above range, and may be an ion-conductive conductive material or an electron-conductive conductive material.

[0035] Examples of the ion-conductive conductive material include: (a) cationic antistatic agents having a cationic group such as a quaternary ammonium salt, a pyridinium salt, or a primary, secondary, or tertiary amino group; (b) anionic antistatic agents having an anionic group such as a sulfonate group, a sulfate ester group, a phosphate ester group, or a phosphonate group; (c) amphoteric antistatic agents such as amino acid-based or amino sulfate-based; and (d) nonionic antistatic agents such as amino alcohol-based, glycerin-based, or polyethylene glycol-based.

[0036] Examples of electron-conductive conductive materials include conductive polymers and other conductive materials. Examples of conductive polymers include polyacetylene or its derivatives, polythiophene or its derivatives, polypyrrole or its derivatives, and polyaniline or its derivatives. Among them, polythiophene or its derivatives are preferred from the viewpoint of high transparency and high conductivity. Examples of conductive materials other than conductive polymers include carbon nanotubes, graphene, etc.

[0037] Among these, it is preferable to contain an electron-conductive conductive material from the viewpoint of easily reducing the surface resistivity of the laminated piezoelectric body and preventing bleed-out. Among the electron-conductive conductive materials, carbon nanotubes are more preferable from the viewpoint of further reducing the surface resistivity of the antistatic layer and thereby further reducing the surface resistivity measured on the hard coat layer.

[0038] The polymerizable compound may be a thermally polymerizable compound or a photopolymerizable compound, and examples thereof include acrylic compounds, epoxy compounds, oxetane compounds, polyurethane compounds, polyimide resins, melamine resins, silicone compounds, vinyl acetate, etc. For example, the same polymerizable compounds as those for forming the hard coat layer described below may be used.

[0039] The thickness of the antistatic layer may be within a range that provides antistatic properties, for example, 10 nm to 250 nm. When the thickness of the antistatic layer is 10 nm or more, the surface resistivity of the antistatic layer can be further reduced, which makes it easier to reduce the surface resistivity measured on the hard coat layer and achieve high antistatic properties. When the thickness of the antistatic layer is 250 nm or less, coating unevenness due to the unevenness of the surface of the piezoelectric film is less likely to occur, making it even more unlikely that coating spots will occur. From the same perspective, the thickness of the antistatic layer is more preferably 15 nm to 220 nm, even more preferably 20 nm to 190 nm, and particularly preferably 20 nm to 160 nm.

[0040] 1-3. Hard Coat Layer The hard coat layer has the function of increasing the scratch resistance of the surface of the laminated piezoelectric body, as well as increasing the slipperiness and suppressing blocking.

[0041] The hard coat layer may be a single layer or multiple layers. At least one hard coat layer is preferably disposed on the antistatic layer. Also, at least one hard coat layer is preferably disposed on the outermost surface of the laminated piezoelectric element.

[0042] The hard coat layer preferably has a moderate surface roughness from the viewpoint of suppressing blocking. Specifically, the maximum height Rz of the surface of the hard coat layer is adjusted to 40 nm or more and 150 nm or less. When the Rz of the surface of the hard coat layer is 40 nm or more, sufficient slipperiness is provided, thereby suppressing blocking between the laminated piezoelectric bodies. When the Rz of the surface of the hard coat layer is 150 nm or less, a decrease in transparency due to an increase in haze can be suppressed. From the same viewpoint, the Rz of the surface of the hard coat layer is more preferably 40 nm or more and 100 nm or less, even more preferably 40 nm or more and 80 nm or less, and particularly preferably 40 nm or more and 60 nm or less.

[0043] The Rz of the surface of the hard coat layer can be measured using a surface roughness measuring instrument (for example, "SURFCOM1500" manufactured by Tokyo Seimitsu Co., Ltd.) by a method conforming to JIS B 0601-2013. Rz is measured in the width direction (TD direction) of the laminated piezoelectric body at any 10 points on the hard coat layer, and the average value is calculated.

[0044] The Rz of the surface of the hard coat layer can be adjusted by the average particle size of the particles contained in the hard coat layer, etc. For example, if the average particle size of the particles contained in the hard coat layer is increased, the Rz tends to increase.

[0045] The hard coat layer may be a resin layer containing particles. From the viewpoint of improving scratch resistance, the resin layer containing particles is preferably obtained by curing a curable composition containing a polymerizable compound and particles.

[0046] (Polymerizable Compound) The polymerizable compound may be any one of a monomer, an oligomer, or a polymer. The polymerizable compound may be a thermosetting compound or an ionizing radiation compound, but is preferably an ionizing radiation compound. The ionizing radiation may usually be ultraviolet (UV) or an electron beam (EB).

[0047] The ionizing radiation-curable compound is a compound having an ionizing radiation-curable functional group. Examples of the ionizing radiation-curable functional group include ethylenically unsaturated bond groups such as (meth)acryloyl groups, vinyl groups, and allyl groups, and ring-opening polymerizable groups such as epoxy groups and oxetanyl groups. Among these, compounds having an ethylenically unsaturated bond group are preferred, compounds having two or more ethylenically unsaturated bond groups are more preferred, and polyfunctional (meth)acrylate compounds are even more preferred.

[0048] Among the polyfunctional (meth)acrylate compounds, examples of bifunctional (meth)acrylate monomers include ethylene glycol di(meth)acrylate, bisphenol A tetraethoxydiacrylate, bisphenol A tetrapropoxydiacrylate, 1,6-hexanediol diacrylate, etc. Examples of trifunctional or higher functional (meth)acrylate monomers include trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol tetra(meth)acrylate, isocyanuric acid-modified tri(meth)acrylate, etc. Furthermore, the above-mentioned (meth)acrylate monomers may be partially modified in the molecular skeleton, and those modified with ethylene oxide, propylene oxide, caprolactone, isocyanuric acid, alkyl, cyclic alkyl, aromatic, bisphenol, etc. can also be used.

[0049] Examples of polyfunctional (meth)acrylate oligomers include acrylate polymers such as urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, etc. Urethane (meth)acrylate can be obtained, for example, by reacting a polyhydric alcohol and an organic diisocyanate with a hydroxy (meth)acrylate.

[0050] (Polymerization Initiator) When the ionizing radiation-curable compound is an ultraviolet-curable compound, the curable composition preferably contains a photopolymerization initiator. Examples of the photopolymerization initiator include one or more selected from acetophenone, benzophenone, α-hydroxyalkylphenone, Michler's ketone, benzoin, benzyl methyl ketal, benzoyl benzoate, α-acyloxime ester, thioxanthones, etc.

[0051] (Particles) The particles may be inorganic particles or organic particles.

[0052] Examples of inorganic particles include silica particles, titanium dioxide particles, zirconia particles, aluminum oxide particles, diamond powder, sapphire particles, boron carbide particles, silicon carbide particles, antimony pentoxide particles, etc. Examples of organic particles include resin particles such as acrylic resin, acrylic-styrene copolymer, and silicone resin. Among these, inorganic particles are preferred, and silica particles are more preferred, as they are less likely to impair the transparency of the hard coat layer. The surfaces of the inorganic particles may be treated with a surface modifier such as a silane coupling agent.

[0053] The average primary particle size of the particles is preferably 10 nm or more and 200 nm or less, and more preferably 30 nm or more and 100 nm or less. By setting the average primary particle size of the particles in the above range, the Rz of the surface of the hard coat layer can be adjusted to the above range.

[0054] The average primary particle size of the particles in the hard coat layer can be measured by observing 10 points on the surface of the hard coat layer using a scanning electron microscope (SEM) at an acceleration voltage of 2.0 kV and a magnification of 50,000 times, and taking the average value of the observed values. The diameter of each of any 10 particles can be determined by measuring the area of ​​each particle, calculating the diameter corresponding to a circle with the area, and then taking the arithmetic mean value of the diameters of each particle as the average primary particle size.

[0055] The particle content in the hard coat layer is preferably 3% by mass or more and 80% by mass or less, and more preferably 6% by mass or more and 70% by mass or less, relative to the curable composition. When the particle content is 3% by mass or more, the Rz of the surface of the hard coat layer tends to be larger, and the anti-blocking property tends to be further improved. When the particle content is 80% by mass or less, the decrease in transparency due to an increase in haze can be further suppressed.

[0056] The thickness of the hard coat layer is preferably 300 nm or more and 3000 nm or less. When the thickness of the hard coat layer is 300 nm or more, the scratch resistance of the laminated piezoelectric body is more likely to be improved. When the thickness of the hard coat layer is 3000 nm or less, the surface resistivity of the laminated piezoelectric body can be further reduced, and therefore higher antistatic properties are more likely to be obtained. From the same viewpoint, the surface thickness of the hard coat layer is more preferably 500 nm or more and 1500 nm or less, and even more preferably 700 nm or more and 1200 nm or less.

[0057] Furthermore, from the viewpoint of easily adjusting the surface resistivity of the laminated piezoelectric body within the above range, the ratio (T2 / T1) of the thickness (T2) of the hard coat layer to the thickness (T1) of the antistatic layer may be, for example, 3 to 26, although this ratio depends on the surface resistivity of the antistatic layer. The smaller the ratio, the thinner the hard coat layer and the thicker the antistatic layer, and therefore the lower the surface resistivity measured on the hard coat layer can be.

[0058] The thickness of each layer constituting the laminated piezoelectric body can be measured using a spectral interference film thickness meter (for example, "Optical NanoGauge C13027-11" manufactured by Hamamatsu Photonics K.K.). The refractive index of each layer can be measured by the method described in JIS K7142, where, for example, the refractive index of the substrate is set to 1.42 and the refractive index of the coating film is set to 1.50. Then, the thickness of each layer in a range including the center of the surface of the laminated piezoelectric body is measured at three or more points at 5 mm intervals, and the arithmetic mean value of the measurements can be calculated as the thickness of each layer.

[0059] 1-4. Layer Structure The antistatic layer and hard coat layer included in the laminated piezoelectric body may each be one layer or two or more layers. The laminated piezoelectric body may further include layers other than those described above. However, from the viewpoint of easily obtaining high antistatic properties, it is preferable that the antistatic layer and the hard coat layer be in contact with each other.

[0060] For example, the laminated piezoelectric element can have the following layer configuration: piezoelectric film / antistatic layer / hard coat layer hard coat layer / piezoelectric film / antistatic layer / hard coat layer

[0061] 1-5. Physical Properties (Surface Resistivity) The laminated piezoelectric body according to this embodiment includes an antistatic layer, and therefore has a reduced surface resistivity. Specifically, the surface resistivity measured on the hard coat layer of the laminated piezoelectric body is 1.0×10 6 Ω / sq. More than 1.0×10 12 The surface resistivity of the laminated piezoelectric body is 1.0×10 12 When the surface resistivity of the laminated piezoelectric body is 1.0×10 Ω / sq. or less, sufficient antistatic properties are easily obtained. 6 From the same viewpoint, the surface resistivity of the laminated piezoelectric body is 1.0×10 8 Ω / sq. More than 5.0×10 11 The surface resistivity of the laminated piezoelectric body can be measured in the same manner as the surface resistivity of the antistatic layer.

[0062] The surface resistivity of the laminated piezoelectric body can be adjusted mainly by the surface resistivity of the antistatic layer and the thickness of the hard coat layer. By reducing the surface resistivity of the antistatic layer and the thickness of the hard coat layer, the surface resistivity of the laminated piezoelectric body tends to be reduced.

[0063] (Total Light Transmittance) From the viewpoint of application to a touch panel mounted on an image display device, the laminated piezoelectric body preferably has high transparency. Specifically, the total light transmittance of the laminated piezoelectric body is preferably 85% or more, and more preferably 90% or more.

[0064] The total light transmittance of the laminated piezoelectric body can be measured using a haze meter (for example, NDH7000SP II manufactured by Nippon Denshoku Industries Co., Ltd.) based on the method described in JIS K 7361-1.

[0065] The total light transmittance of the laminated piezoelectric body can be adjusted by the thickness of the antistatic layer and the average particle size of the particles contained in the hard coat layer. For example, reducing the thickness of the antistatic layer makes it less likely that coating spots will occur, and the total light transmittance tends to be higher. Furthermore, reducing the average particle size of the particles in the hard coat layer tends to increase the total light transmittance.

[0066] (Piezoelectric constant of laminated piezoelectric body) Piezoelectric constant d of laminated piezoelectric body 33 The piezoelectric constant d of the laminated piezoelectric material is adjusted to be 7 pC / N or more and 40 pC / N or less. 33 When the piezoelectric constant d of the laminated piezoelectric material is 7 pC / N or more, the amount of charge generated by the piezoelectric effect is sufficient, and therefore high pressure sensitivity is easily obtained. 33 When the piezoelectric constant d of the laminated piezoelectric body is 40 pC / N or less, the unevenness of the film surface caused by the polarization treatment can be further reduced, and therefore, the appearance defect can be reduced. 33 is more preferably 10 pC / N or more and 40 pC / N or less, further preferably 10 pC / N or more and 27 pC / N or less, and particularly preferably 13 pC / N or more and 24 pC / N or less.

[0067] Piezoelectric constant d of the laminated piezoelectric material 33 is mainly the piezoelectric constant d 33 The piezoelectric constant d of the piezoelectric film can be adjusted by 33 When the piezoelectric constant d 33 It is also likely to be expensive.

[0068] 1-6. Operation The laminated piezoelectric element according to the above embodiment has a piezoelectric constant d 33Since the laminated piezoelectric body contains a piezoelectric film having a predetermined Rz or more, it has high piezoelectricity. Furthermore, the laminated piezoelectric body has a laminated structure of an antistatic layer and a hard coat layer having a predetermined Rz or more, and the surface resistivity of the hard coat layer of the laminated piezoelectric body is adjusted to a predetermined value or less. This makes it possible to achieve both antistatic resistance and antiblocking properties. Furthermore, the thickness of the antistatic layer is adjusted to a predetermined value or less. This reduces unevenness in the application of the antistatic layer due to the unevenness of the surface of the piezoelectric film containing a fluorine-based resin, thereby suppressing the resulting coating spots. This makes it possible to suppress a decrease in visibility.

[0069] 2. Manufacturing Method of Laminated Piezoelectric Body The laminated piezoelectric body according to this embodiment can be manufactured through the following steps: (1) preparing a piezoelectric film containing a fluorine-based resin; (2) applying an antistatic material to at least one surface of the prepared piezoelectric film and drying the applied material to form an antistatic layer; and (3) applying a curable resin composition to the antistatic layer and curing the applied material to form a hard coat layer. The piezoelectric film, antistatic layer, and hard coat layer are the same as those described above, respectively.

[0070] (1) Step of Preparing Piezoelectric Film The piezoelectric film containing a fluorine-based resin may be a commercially available product or may be manufactured.

[0071] When producing a piezoelectric film containing a fluororesin, the piezoelectric film can be obtained through a process of poling a film containing a fluororesin. The film containing a fluororesin may be a stretched film or an unstretched film. In this embodiment, from the viewpoint of exhibiting a high piezoelectric effect, it is preferable to stretch the film containing a fluororesin and then perform a polarization process.

[0072] The film containing a fluororesin can be produced by any method, such as a melt extrusion method (extrusion molding method) or a solution casting method. Among them, the film containing a fluororesin is preferably produced by a melt extrusion method, from the viewpoint of easily obtaining a piezoelectric film having a predetermined thickness or more. In the melt extrusion method, the fluororesin and any additives are heated and melted in the cylinder of an extruder, and then extruded through a die to obtain a film.

[0073] The obtained film has a structure in which α-type crystals (main chain has a helical structure) and β-type crystals (main chain has a planar zigzag structure) are mixed. β-type crystals have a large polarization structure. Stretching the film can convert α-type crystals into β-type crystals, and the stretching step is preferably performed as needed to convert the fluororesin into β-type crystals. The stretching direction may be either the TD direction or the MD direction, with the MD direction being more preferred.

[0074] The stretching method is not particularly limited, and can be a known stretching method such as a tenter method or a drum method.

[0075] The stretching ratio is, for example, 3.0 times or more and 6.0 times or less. When the stretching ratio is 3.0 times or more, it is easy to adjust the thickness and polarity of the film to a more appropriate range. When the stretching ratio is 3.0 times or more, the rearrangement reaction of the β-type crystals proceeds sufficiently, making it easy to exhibit higher piezoelectricity and also improving transparency. When the stretching ratio is 6.0 times or less, breakage due to stretching can be further suppressed.

[0076] The resulting stretched film is subjected to a polarization treatment. The polarization treatment can be performed, for example, by applying a DC voltage between a ground electrode and a needle-like electrode. The voltage may be adjusted depending on the thickness of the stretched film, and may be, for example, 1 kV to 50 kV.

[0077] In this manner, in this embodiment, a piezoelectric film can be obtained by polarizing a stretched film.

[0078] (2) Step of Forming Antistatic Layer A curable composition containing, for example, the above-described conductive material is applied to the obtained piezoelectric film, and then dried and cured to form an antistatic layer.

[0079] The antistatic material may further contain water or a solvent, examples of which include alcohol-based solvents such as methanol, ethanol, and isopropyl alcohol.

[0080] The coating method is not particularly limited, and may be any of spin coating, gravure coating, die coating, bar coating, dip coating, and the like.

[0081] The drying method is a method of heating the applied antistatic material. The heating temperature is preferably a temperature at which the solvent can be removed or higher and a temperature at which the fluorine-based resin constituting the piezoelectric film is thermally deformed or distorted, and can be, for example, 100° C. or higher and 150° C. or lower. The thermal deformation temperature can be measured, for example, in accordance with JIS K 7191-2:2015.

[0082] (3) Step of Forming a Hard Coat Layer A coating liquid containing the above-described curable composition is applied onto the obtained antistatic layer, and then dried and cured to form a hard coat layer.

[0083] The coating liquid may further contain a dilution solvent as needed. The dilution solvent preferably has a polarity similar to that of the particles. Examples of the dilution solvent include organic solvents such as alcohol-based solvents, ketone-based solvents, ester-based solvents, carbonate-based solvents, and aromatic solvents.

[0084] The coating liquid can be applied by the same method as the coating method described above. The coating liquid can also be dried by the same method as the drying method described above. The heating temperature may be any temperature that is within a range that allows the solvent to be volatilized and is equal to or lower than the heat distortion temperature of the fluorine-based resin that constitutes the piezoelectric film, and may be, for example, 60°C or higher and 100°C or lower.

[0085] Curing may be performed by heat or by ionizing radiation. Curing by ionizing radiation can be performed by irradiation with ultraviolet rays or electron beams. Furthermore, curing by heat and curing by ionizing radiation may be performed in combination.

[0086] The laminated piezoelectric element according to this embodiment can be used for various applications. In particular, since the laminated piezoelectric element according to this embodiment exhibits high piezoelectricity while having high transparency and visibility, it can be preferably used as a pressure-sensitive sensor for touch panels mounted on various electronic devices.

[0087] The present invention will be further described below with reference to examples and comparative examples, but the technical scope of the present invention is not limited thereto.

[0088] 1. Evaluation of Physical Properties (1) Layer Thickness The thickness of each layer was measured using a spectral interference film thickness meter ("Optical NanoGauge C13027-11" manufactured by Hamamatsu Photonics K.K.). The thickness of each layer in an area including the center of the surface of the laminated piezoelectric body was measured at 30 points at 5 mm intervals, and the arithmetic mean value was calculated. The refractive index of each layer was set for each material of the layer, and was set to 1.42 for the piezoelectric film containing PVDF, 1.50 for the antistatic layer, and 1.50 for the hard coat layer.

[0089] (2) Particle size The surface of the hard coat layer of the laminated piezoelectric body was observed using a scanning electron microscope ("SU3800", manufactured by Hitachi High-Technologies Corporation) under conditions of an acceleration voltage of 2.0 kV and a magnification of 50,000 times. Measurements were taken at 10 points, and the average was taken as the particle size of the nano-inorganic particles.

[0090] (3) Piezoelectric constant (piezoelectric constant d 33 ) direct quasi-static method (d 33 The piezoelectric constant d of the piezoelectric ceramic measured by the Meter method and the Berlincoat method 33 Test method: Piezoelectric constant d according to ISO 19622:2018 33 Specifically, the piezoelectric constant d 33The piezoelectric constant d was measured by using a piezoelectric constant measuring device ("Piezometer System PM300", manufactured by PIEZOTEST Co., Ltd.) to clip the sample with 1 N and apply a force of 0.15 N, 110 Hz, and read the generated charge. 33 The measured values ​​are measured at a temperature of 25° C. and may be positive or negative depending on whether the film is measured on the front or back, but absolute values ​​are shown in this specification.

[0091] (d 14 ) Al was vapor-deposited on both surfaces of the laminated piezoelectric element, and the piezoelectric film was cut into a rectangular film measuring 120 mm x 10 mm, cut at a 45° angle to the stretching direction (MD) of the piezoelectric film and a 10 mm cut in a direction perpendicular to the 45° angle. This was used as the measurement sample. The sample was then placed in a tensile tester with a chuck distance of 70 mm to prevent slack. Next, a force was applied to the sample at a speed of 5 mm / min, oscillating between 4 N and 9 N. To measure the amount of charge generated in the sample in response to the applied force, a capacitor with a capacitance of Qm (F) was connected in parallel to the sample, and the terminal voltage Vm of this capacitor Cm (95 nF) was measured via a buffer amplifier. The generated charge Q (C) was calculated as the product of the capacitor capacitance Cm and the terminal voltage Vm. Piezoelectric constant d 14 was calculated using the following formula: 14 = (2 x t) / L x Cm ΔVm / ΔF t: sample thickness (m) L: distance between chucks (m) Cm: capacitance of parallel-connected capacitors (F) ΔVm / ΔF: ratio of voltage change between capacitor terminals to change in force

[0092] 2. Preparation and Evaluation of Laminated Piezoelectric Body [Example 1] (1) Preparation of Piezoelectric Film A polyvinylidene fluoride film (manufactured by Kureha Corporation, a film containing 100% by mass of vinylidene fluoride homopolymer) was stretched in the MD direction at a stretching ratio of 4.2 times, and then a DC voltage was applied between the ground electrode and the needle-shaped electrode while increasing from 0 kV to 11.0 kV, thereby performing a polarization treatment, and a piezoelectric film with a thickness of 42 μm was obtained. The piezoelectric constant d of the piezoelectric film 33 When measured by the above method, it was 15 pC / N.

[0093] (2) Formation of Antistatic Layer A solution obtained by mixing a paint P-400MP-A (manufactured by Nagase ChemteX Corporation) containing PEDOT:PSS as a conductive polymer and a paint P-400MP-B (manufactured by Nagase ChemteX Corporation) containing a crosslinking agent and a conductivity improver in a ratio of 4:1 was applied to surface A of the obtained piezoelectric film using a multi-coater (manufactured by Hirano Tecseed Co., Ltd.), and the film was heat-treated at 130°C for 0.67 minutes to form an antistatic layer with a thickness of 50 nm on the piezoelectric film.

[0094] (3) Formation of Hard Coat Layer Next, a hard coat agent (BS-CH271 manufactured by Arakawa Chemical Industries, Ltd., amorphous silica having an average particle size of 60 nm) was applied onto the antistatic layer using a multi-coater, and then heat-treated at 80°C for 2 minutes. 2 The resulting laminate was photocured by irradiating it with UV rays of 1000 W to form a hard coat layer having a thickness of 700 nm, thereby obtaining a laminated piezoelectric body having a laminated structure of piezoelectric film / antistatic layer / hard coat layer.

[0095] Example 2 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the hard coat layer was changed to 2000 nm.

[0096] Example 3 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the antistatic layer was changed to 140 nm.

[0097] Example 4 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the heat treatment conditions for forming the antistatic layer were changed to 120° C. for 60 minutes.

[0098] Example 5 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that a solution (C-169PF) obtained by mixing a paint C-169PF-A (manufactured by Nagase ChemteX Corporation) containing single-walled carbon nanotubes and a paint C-169PF-B (manufactured by Nagase ChemteX Corporation) containing a crosslinking agent in a ratio of 3:2 was applied to side A of the piezoelectric film using a multi-coater (manufactured by Hirano Techseed Co., Ltd.), and the film was heat-treated at 130°C for 1 minute to form an antistatic layer.

[0099] [Example 6] A laminated piezoelectric body was obtained by further forming a hard coat layer having a thickness of 700 nm on side B of the piezoelectric film of the laminated piezoelectric body produced in Example 1 in the same manner as in Example 1. In this way, a laminated piezoelectric body having a laminated structure of hard coat layer / piezoelectric film / antistatic layer / hard coat layer was obtained.

[0100] Example 7 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the hard coating agent was changed to TYAB-M101 (average particle size of amorphous silica: 80 nm) manufactured by Toyochem Co., Ltd.

[0101] Comparative Example 1 Neither the antistatic layer nor the hard coat layer was formed, and the piezoelectric film of Example 1 was used as it was.

[0102] Comparative Example 2 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the hard coating agent containing amorphous silica was changed to a hard coating agent not containing amorphous silica (BS-575, manufactured by Arakawa Chemical Industries, Ltd.).

[0103] Comparative Example 3 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the antistatic layer was changed to 5 nm.

[0104] Comparative Example 4 A laminated piezoelectric body was obtained in the same manner as in Example 1, except that the thickness of the antistatic layer was changed to 260 nm.

[0105] [Comparative Example 5] An antistatic layer was formed in the same manner as in Example 1, except that the heat treatment conditions during the formation of the antistatic layer were changed to 160°C and 60 minutes. However, the appearance of the laminated piezoelectric body was poor, and a hard coat layer was not formed.

[0106] Comparative Example 6 An attempt was made to form an antistatic layer in the same manner as in Example 1, except that the heat treatment conditions during the formation of the antistatic layer were changed to 80°C and 0.67 minutes. However, the antistatic layer was not sufficiently cured, and a hard coat layer was not formed.

[0107] Comparative Example 7 An antistatic hard coating agent (MT-3 / manufactured by Arakawa Chemical Industries, Ltd.) was applied to the piezoelectric film of Example 1 using a multi-coater, and the film was heat-treated at 80°C for 2 minutes. After that, the film was irradiated with 400 mJ / cm using a UV irradiation device CSOT-40 (manufactured by GS Yuasa Corporation). 2The laminated piezoelectric body was obtained by irradiating the film with UV light at an integrated light amount of 10 ...

[0108] Comparative Example 8 (1) Preparation of Piezoelectric Film Containing Polylactic Acid To 100 parts by mass of polylactic acid (trade name: Ingeo™ biopolymer) manufactured by NatureWorks LLC, 1.0 part by mass of a stabilizer (a mixture of Stabaxol P400 (10 parts by mass) manufactured by Rhein Chemie, Stabaxol I (70 parts by mass) manufactured by Rhein Chemie, and Carbodilite LA-1 (20 parts by mass) manufactured by Nisshinbo Chemical Inc.) was added and dry-blended to prepare a raw material. The raw material was then placed in the hopper of an extrusion molding machine, extruded through a T-die while heated to 210°C, and brought into contact with a casting roll at 50°C to form a pre-crystallized film with a thickness of 150 μm. The pre-crystallized film was uniaxially stretched in the MD direction to 3.5 times its original size at 70°C using a roll-to-roll method to obtain a uniaxially stretched film. The thickness of the obtained uniaxially stretched film was 49.2 μm. The obtained uniaxially stretched film was then annealed by contacting it with a roll at 145° C. for 15 seconds in a roll-to-roll manner, and then rapidly cooled to produce a piezoelectric film containing polylactic acid. The piezoelectric constant d of the piezoelectric film 14 When measured by the above method, it was 6 pC / N.

[0109] (2) Formation of Antistatic Hard Coat Layer An antistatic hard coat coating material (Sepulgida (registered trademark) HC-A, manufactured by Shin-Etsu Polymer) was applied to one side of the obtained piezoelectric film using a multi-coater, dried at 60°C for 5 minutes, and then irradiated with a metal halide lamp with an integrated light intensity of 1000 mJ / cm. 2 The film was irradiated with ultraviolet light of 1000 W at ...

[0110] [Evaluation] The surface resistivity, charge amount, blocking resistance, maximum surface height Rz, and total light transmittance of the obtained laminated piezoelectric body were evaluated by the following methods.

[0111] (1) Surface Resistivity A sample was obtained by cutting a laminated piezoelectric element or a piezoelectric film into a size of 100 mm x 100 mm. The surface resistivity of the hard coat layer of the sample was measured using a surface resistivity meter F-109 (manufactured by Hozan Corporation) in accordance with JIS 6911. The measurement was performed under the condition of an output of 100 W, and the value was read after 10 seconds.

[0112] (2) Charge Amount The surface potential (kV) of the film in a wound state (film roll) was measured using an electrostatic potential meter (SK-H050 manufactured by Keyence Corporation) at a position 10 cm from the film surface on the outside of the roll.

[0113] (3) Blocking Resistance Two test pieces measuring 10 cm in length and 10 cm in width were cut out from the laminated piezoelectric body or piezoelectric film, and one hard-coated surface of the two test pieces was placed on the other hard-coated surface. The films were rubbed together and the degree of sticking was visually confirmed and evaluated according to the following criteria: ○: No sticking ×: Sticking

[0114] (4) Maximum Height Rz The maximum height Rz of the surface of the hard coat layer of the laminated piezoelectric body was measured using a surface roughness measuring instrument (SURFCOM1500, manufactured by Tokyo Seimitsu Co., Ltd.) according to a method in accordance with JIS B 0601-2013. The maximum heights Rz were measured in the width direction (TD) of the laminated piezoelectric film at any 10 points on the hard coat layer, and the average value was calculated.

[0115] (5) Total Light Transmittance The total light transmittance of the laminated piezoelectric body was measured using a haze meter ("NDH7000SP II", manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the method described in JIS K 7361-1.

[0116] (6) Color Unevenness Whether color unevenness of the laminated piezoelectric body was visually recognized along the MD direction was evaluated according to the following criteria: ◯: Color unevenness was not visible; ×: Color unevenness was visible.

[0117] (7) Piezoelectric constant of laminated piezoelectric body The piezoelectric constant d of the laminated piezoelectric body was measured in the same manner as above. 33 or d 14 was measured.

[0118] The manufacturing conditions and layer structures of the laminated piezoelectric bodies of Examples 1 to 7 and Comparative Examples 1 to 8 are shown in Table 1. The evaluation results of the laminated piezoelectric bodies of Examples 1 to 7 and Comparative Examples 2 to 4 and 7 are shown in Table 2.

[0119]

[0120]

[0121] As shown in Table 2, the laminated piezoelectric bodies of Comparative Examples 2 and 7, which have hard coat layers with Rz values ​​of less than 40 nm, exhibit poor blocking resistance. Furthermore, the piezoelectric film of Comparative Example 1, which does not have an antistatic layer, and the laminated piezoelectric body of Comparative Example 3, which has an antistatic layer thickness of less than 10 nm, exhibit high surface resistivity and poor antistatic properties. Furthermore, the laminated piezoelectric body of Comparative Example 4, which has an antistatic layer thickness of more than 250 nm, exhibits sufficient antistatic properties but exhibits color unevenness. Furthermore, the laminated piezoelectric body of Comparative Example 8, which uses a piezoelectric film containing polylactic acid, exhibits a low piezoelectric constant.

[0122] In contrast, the laminated piezoelectric elements of Examples 1 to 7 all exhibited high piezoelectric constants without color unevenness, and were found to have high blocking resistance and antistatic properties.

[0123] In particular, it is suggested that by making the thickness of the hard coat layer thinner, the surface resistivity becomes smaller and the antistatic properties become more improved (comparison between Examples 1 and 2).

[0124] It is also clear that the total light transmittance can be increased by reducing the thickness of the antistatic layer (comparison between Examples 1 and 3).

[0125] This application claims priority from Japanese Patent Application No. 2023-48031, filed March 24, 2023, the entire contents of which are incorporated herein by reference.

[0126] The laminated piezoelectric material of the present invention has high piezoelectricity, anti-blocking properties, and anti-static properties without reducing visibility, and is therefore suitable for use as a pressure-sensitive sensor in a touch panel.

Claims

1. A laminated piezoelectric body comprising: a piezoelectric film containing a fluororesin as a main component; an antistatic layer having a thickness of 10 nm to 250 nm and disposed on at least one surface of the piezoelectric film; and a hard coat layer disposed on the antistatic layer and having a maximum surface height Rz of 40 nm to 150 nm, wherein the surface resistivity of the laminated piezoelectric body measured on the hard coat layer is 1.0×10 6 Ω / sq. More than 1.0×10 12 The total light transmittance of the laminated piezoelectric body is 85% or more, and the piezoelectric constant d 33 A laminated piezoelectric material having a dielectric constant of 7 pC / N or more and 40 pC / N or less.

2. The laminated piezoelectric element according to claim 1, wherein the fluororesin is a polymer containing, as a main component, a structural unit derived from vinylidene fluoride.

3. The laminated piezoelectric element according to claim 1, wherein the fluororesin is a vinylidene fluoride homopolymer.

4. The laminated piezoelectric element according to claim 1, wherein the antistatic layer contains carbon nanotubes.

5. The laminated piezoelectric element according to claim 1, wherein the hard coat layer has a thickness of 300 nm or more and 3000 nm or less.

6. The laminated piezoelectric element according to claim 1, wherein the hard coat layer contains silica particles having an average particle size of 10 nm or more and 200 nm or less.

7. A method for producing the laminated piezoelectric element according to claim 1, comprising the steps of: 33 1. A method for manufacturing a laminated piezoelectric body, comprising: preparing a piezoelectric film having a resistivity of 7 pC / N or more and 40 pC / N or less; applying an antistatic material to at least one surface of the piezoelectric film to form an antistatic layer; and applying a curable composition onto the antistatic layer, followed by curing the composition to form a hard coat layer.

8. The method for producing a laminated piezoelectric element according to claim 7, wherein in the step of preparing the piezoelectric film, a film containing a fluorine-based resin as a main component is formed by extrusion molding.

9. The method for producing a laminated piezoelectric element according to claim 7, wherein in the step of preparing the piezoelectric film, a film containing a fluorine-based resin as a main component is stretched and then polarized.

10. The method for manufacturing a laminated piezoelectric element according to claim 7, wherein in the step of forming the antistatic layer, the piezoelectric film on which the antistatic material has been applied is heat-treated at 100°C or higher and 150°C or lower to dry it.

Citation Information

Patent Citations

  • Touch panel

    JP2010026938A

  • Ceramic sanitary ware

    JP2023048031A

  • Laminated body

    WO2016098597A1

  • Piezoelectric film and piezoelectric sensor

    WO2019102635A1

  • Piezoelectric film, touch panel, and piezoelectric film manufacturing method

    WO2022091828A1

Cited By

  • Laminated piezoelectric body and manufacturing method for same

    WO2026205506A1