Chloroprene / unsaturated nitrile copolymer latex, rubber component, rubber composition, vulcanized molded body, and production method for chloroprene / unsaturated nitrile copolymer latex

The chloroprene-unsaturated nitrile copolymer latex addresses storage stability and heat generation issues in conventional chloroprene-based latexes by incorporating a specific nitrogen-containing functional group and controlled unsaturated nitrile content, resulting in stable and oil-resistant vulcanized products.

WO2024203716A1PCT designated stage expired Publication Date: 2024-10-03DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011009
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-21
Publication Date
2024-10-03

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

Problem: To provide a chloroprene / unsaturated nitrile copolymer latex that has excellent storage stability at high temperatures over long periods of time, the chloroprene / unsaturated nitrile copolymer latex being such that vulcanized molded bodies of a rubber composition that uses a rubber component of the chloroprene / unsaturated nitrile copolymer latex have excellent oil resistance and generate little heat. Solution: The present invention provides a chloroprene / unsaturated nitrile copolymer latex that includes a chloroprene / unsaturated nitrile copolymer that includes chloroprene monomer units and unsaturated nitrile monomer units, the nitrogen content of the chloroprene / unsaturated nitrile copolymer as measured by the combustion method being at least 0.5 mass%, the chloroprene / unsaturated nitrile copolymer having a functional group that has the structure represented by chemical formula (1), and the unsaturated nitrile hydrolysate content of the chloroprene / unsaturated nitrile copolymer latex being 0.10–9.00 parts by mass per 100 parts by mass of the chloroprene / unsaturated nitrile copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

Chloroprene-unsaturated nitrile copolymer latex, rubber component, rubber composition, vulcanized molded product, and method for producing chloroprene-unsaturated nitrile copolymer latex

[0001] The present invention relates to a chloroprene-unsaturated nitrile copolymer latex, a rubber component, a rubber composition, a vulcanized molded article, and a method for producing the chloroprene-unsaturated nitrile copolymer latex.

[0002] Chloroprene-based latex and chloroprene-based rubber containing chloroprene-based polymers have excellent mechanical properties, ozone resistance, and chemical resistance, and these properties are utilized in a wide range of fields, such as automotive parts, adhesives, and various industrial rubber parts.

[0003] For example, Patent Document 1 discloses a copolymer in which the proportions of the respective monomers constituting the polymer are, when the total amount of all monomers is taken as 100% by mass, 80 to 97% by mass of 2-chloro-1,3-butadiene (chloroprene) (C-1) and 20 to 3% by mass of 2,3-dichloro-1,3-butadiene (C-2), or a copolymer in which 79.8 to 96.8% by mass of 2-chloro-1,3-butadiene (chloroprene) (C-1), 20 to 3% by mass of 2,3-dichloro-1,3-butadiene (C-2) and 0.2 to 17% by mass of a monomer (C-3) copolymerizable therewith. The present invention discloses a composition for chloroprene-based vulcanized rubber, which comprises 100 parts by mass of a polymer for chloroprene-based vulcanized rubber, the polymer being a copolymer consisting of the above copolymer and having a Mooney viscosity (ML1+4(100°C)) in the range of 100 to 135, 0.5 to 6 parts by mass of an acid acceptor, 0.2 to 3 parts by mass of a lubricant, 1 to 5 parts by mass of an antioxidant, 10 to 120 parts by mass of carbon black, 0.1 to 20 parts by mass of a filler other than carbon black, 2 to 40 parts by mass of a softener, 0.2 to 5 parts by mass of a processing aid, 0.5 to 10 parts by mass of a metal oxide, and 0.5 to 5 parts by mass of a vulcanization accelerator. Patent Document 2 also discloses a rubber composition for flame-retardant hoses, which contains a rubber component, carbon black, and silica, and the rubber component is either chloroprene rubber alone or chloroprene rubber and styrene-butadiene rubber alone.

[0004] Patent Document 3 discloses a statistical copolymer latex containing chloroprene monomer units and unsaturated nitrile monomer units, with an unsaturated nitrile monomer unit content of 5 to 20% by mass, wherein the statistical copolymer latex is freeze-dried to obtain a statistical copolymer with a toluene-insoluble content of 50 to 100% by mass relative to 100% by mass of the statistical copolymer.

[0005] JP 2012-211345 A JP 2017-019947 A WO2019 / 211975

[0006] However, conventional chloroprene-based latexes have room for improvement in storage stability at high temperatures for a long time. Also, it has been difficult to obtain a chloroprene-based latex which has excellent storage stability at high temperatures for a long time, and which provides excellent oil resistance to a vulcanized molded product of a rubber composition using a rubber component of the chloroprene-based latex, and which generates little heat under dynamic conditions.

[0007] The present invention has been made in view of the above circumstances and provides a chloroprene-unsaturated nitrile copolymer latex that has excellent storage stability at high temperatures for long periods of time, and that has excellent oil resistance and generates little heat under dynamic environments when vulcanized molded articles of rubber compositions using the chloroprene-unsaturated nitrile copolymer latex as a rubber component. The present invention also provides a rubber component of the chloroprene-unsaturated nitrile copolymer latex, a rubber composition containing the rubber component, a vulcanized molded article of the rubber composition, and a method for producing the chloroprene-unsaturated nitrile copolymer latex.

[0008] According to the present invention, there is provided a chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units, wherein the chloroprene-unsaturated nitrile copolymer has a nitrogen content of 0.5% by mass or more as measured by a combustion method, and the chloroprene-unsaturated nitrile copolymer has a functional group having a structure represented by chemical formula (1), and the content of an unsaturated nitrile hydrolysate in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer.

[0009]

[0010] In chemical formula (1), R 1 represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a substituted or unsubstituted mercapto group, and a substituted or unsubstituted heterocyclyl group.

[0011] As a result of extensive investigations, the present inventors have found that by adjusting the production conditions of a chloroprene-unsaturated nitrile copolymer latex and controlling the nitrogen content and structure of the chloroprene-unsaturated nitrile copolymer and the content of unsaturated nitrile hydrolysates in the chloroprene-unsaturated nitrile copolymer latex, it is possible to obtain a chloroprene-unsaturated nitrile copolymer latex which has excellent storage stability at high temperatures for long periods of time, in which a vulcanized molded product of a rubber composition using the rubber component of the chloroprene-unsaturated nitrile copolymer latex has excellent oil resistance and generates little heat under dynamic environments, and have thus completed the present invention.

[0012] Various embodiments of the present invention will be exemplified below. The embodiments shown below can be combined with each other. [1] A chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units, wherein the chloroprene-unsaturated nitrile copolymer has a nitrogen content of 0.5% by mass or more as measured by a combustion method and has a functional group having a structure represented by chemical formula (1), and the content of an unsaturated nitrile hydrolysate in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer.

[0013] (In chemical formula (1), R 1represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a substituted or unsubstituted mercapto group, and a substituted or unsubstituted heterocyclyl group.) [2] The chloroprene-unsaturated nitrile copolymer latex according to [1], wherein the unsaturated nitrile monomer units are acrylonitrile monomer units, the chloroprene-unsaturated nitrile copolymer has an acrylonitrile bond amount of 2 mass% or more measured in accordance with JIS K6451-1, and the chloroprene-unsaturated nitrile copolymer latex has an acrylonitrile hydrolyzate content of 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer. [3] A rubber component of the chloroprene-unsaturated nitrile copolymer latex according to [1] or [2]. [4] A rubber composition comprising the rubber component according to [3]. [5] A vulcanized molded article of the rubber composition according to [4]. [6] The vulcanized molded article according to [5], which is a power transmission belt, a conveyor belt, a hose, a wiper, a dipping product, a sealing part, an adhesive, a boot, a rubber-coated cloth, a rubber roll, a vibration-proof rubber, or a sponge product. [7] A method for producing a chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units, the production method comprising a polymerization step of polymerizing raw material monomers containing chloroprene monomers and unsaturated nitrile monomers in an aqueous solution containing water in the presence of a xanthogen compound to obtain the chloroprene-unsaturated nitrile copolymer, wherein the amount of the water is less than 150 parts by mass when the total amount of the raw material monomers used in the polymerization step is 100 parts by mass.

[0014] The chloroprene-unsaturated nitrile copolymer latex according to the present invention has excellent storage stability at high temperatures for long periods of time. Furthermore, a vulcanized molded article of a rubber composition containing the chloroprene-unsaturated nitrile copolymer latex according to the present invention as a rubber component has excellent oil resistance and generates little heat under dynamic conditions. Because the chloroprene-unsaturated nitrile copolymer latex according to the present invention has excellent storage stability at high temperatures for long periods of time, it can be stored while maintaining its excellent quality in the state of the chloroprene-unsaturated nitrile copolymer latex. Furthermore, a vulcanized molded article of a rubber composition using the rubber component has excellent oil resistance and generates little heat under dynamic conditions. Taking advantage of these properties, the chloroprene-unsaturated nitrile copolymer latex according to the present invention can be used in a variety of applications and components.

[0015] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.

[0016] 1. Chloroprene-unsaturated nitrile copolymer latex The chloroprene-unsaturated nitrile copolymer latex according to the present invention contains a chloroprene-unsaturated nitrile copolymer. The chloroprene-unsaturated nitrile copolymer has a nitrogen content of 0.5% by mass or more as measured by a combustion method, has a functional group having a structure represented by chemical formula (1), and the content of the unsaturated nitrile hydrolysate in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer.

[0017] 1.1 Chloroprene-unsaturated nitrile copolymer The chloroprene-unsaturated nitrile copolymer according to the present invention contains chloroprene monomer units and unsaturated nitrile monomer units. That is, the chloroprene-unsaturated nitrile copolymer according to the present invention contains monomer units (monomer units = structural units) derived from chloroprene (2-chloro-1,3-butadiene) and also contains monomer units derived from an unsaturated nitrile. The chloroprene-unsaturated nitrile copolymer according to the present invention may have a structure derived from monomer units other than the chloroprene monomer units and unsaturated nitrile monomer units, as long as the object of the present invention is not impaired.

[0018] Commercially available 2-chloro-1,3-butadiene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene can also be used as the chloroprene monomer of this embodiment.

[0019] Examples of unsaturated nitriles include acrylonitrile, methacrylonitrile, ethacrylonitrile, and phenylacrylonitrile. The unsaturated nitriles may be used alone or in combination of two or more. The unsaturated nitrile preferably contains acrylonitrile, from the viewpoint of easily obtaining excellent moldability and easily obtaining excellent breaking strength, breaking elongation, hardness, tear strength, and oil resistance in a vulcanized molded product.

[0020] The chloroprene-unsaturated nitrile copolymer according to the present invention has a nitrogen content of 0.5% by mass or more as measured by a combustion method, and the nitrogen content may be, for example, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0% by mass, or may be within a range between any two of the values ​​exemplified here.

[0021] The nitrogen content of the chloroprene-unsaturated nitrile copolymer can be determined by analyzing the chloroprene-unsaturated nitrile copolymer obtained by freeze-drying or methanol precipitation from the chloroprene-unsaturated nitrile copolymer latex using an elemental analyzer by a combustion method. Specifically, the analysis can be performed by the method described in the Examples. The nitrogen in the chloroprene-unsaturated nitrile copolymer can be derived from unsaturated nitrile monomer units in the chloroprene-unsaturated nitrile copolymer, and can be controlled by adjusting the amount of unsaturated nitrile in the raw material monomers during polymerization of the chloroprene-unsaturated nitrile copolymer.

[0022] The chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention preferably has an unsaturated nitrile monomer unit content of 2.0% by mass or more, and the content of the unsaturated nitrile monomer unit may be, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25% by mass, or may be within a range between any two of the values ​​exemplified here.

[0023] The chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention preferably has an acrylonitrile bond amount (content of acrylonitrile monomer units) of 2% by mass or more, as measured in accordance with JIS K 6451-1. The acrylonitrile bond amount (content of acrylonitrile monomer units) is, for example, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25% by mass, and may be within a range between any two of the values ​​exemplified here.

[0024] The content of unsaturated nitrile monomer units and the content of acrylonitrile monomer units in the chloroprene-unsaturated nitrile copolymer can be calculated based on the nitrogen content measured by a combustion method. In particular, the acrylonitrile bond amount (content of acrylonitrile monomer units) can be calculated based on JIS K 6451-1. Specifically, the analysis can be performed by the method described in the Examples. By setting the content of unsaturated nitrile monomer units and acrylonitrile monomer units to the above-mentioned lower limits or more, the resulting rubber composition and vulcanized molded article will have sufficient oil resistance. Furthermore, by setting the content of unsaturated nitrile monomer units and acrylonitrile monomer units to the above-mentioned upper limits or less, the water resistance and cold resistance of the resulting rubber composition and vulcanized molded article will be further improved.

[0025] The chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention preferably contains 60 to 100% by mass of chloroprene monomer units when the chloroprene-unsaturated nitrile copolymer is taken as 100% by mass. The content of chloroprene monomer units in the chloroprene-unsaturated nitrile copolymer is, for example, 60, 65, 70, 75, 80, 85, 90, 95, 99, or 100% by mass, and may be within a range between any two of the values ​​exemplified here. By setting the content of chloroprene monomer units within the above range, a rubber composition can be obtained that can give a molded product having an excellent balance of hardness, tensile strength, and cold resistance.

[0026] The chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention may also have a monomer unit other than the chloroprene monomer and the unsaturated nitrile monomer. The monomer unit other than the chloroprene monomer and the unsaturated nitrile monomer is not particularly limited as long as it is copolymerizable with the chloroprene monomer or the chloroprene monomer and the unsaturated nitrile monomer, and examples thereof include (meth)acrylic acid esters (methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc.), hydroxyalkyl (meth)acrylates (2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, etc.), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, sulfur, etc.

[0027] A chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention may contain 0 to 20 mass% of monomer units other than chloroprene monomer and unsaturated nitrile monomer, when the chloroprene-unsaturated nitrile copolymer is taken as 100 mass%. The content of monomer units other than chloroprene monomer and unsaturated nitrile monomer in the chloroprene-unsaturated nitrile copolymer may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 mass%, and may be within a range between any two of the values ​​exemplified here. By adjusting the copolymerization amount of monomers other than chloroprene monomer and unsaturated nitrile monomer within this range, the effects of copolymerizing these monomers can be achieved without impairing the properties of the resulting rubber composition. Furthermore, a chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention may also be composed solely of chloroprene monomer units and unsaturated nitrile monomer units.

[0028] The chloroprene-unsaturated nitrile copolymer latex according to one embodiment of the present invention may contain one kind of chloroprene-unsaturated nitrile copolymer or two or more kinds of chloroprene-unsaturated nitrile copolymers. When the chloroprene-unsaturated nitrile copolymer latex according to one embodiment of the present invention contains two or more kinds of chloroprene-unsaturated nitrile copolymers, it is preferable that the contents based on the total mass of all nitrogen, all unsaturated nitrile monomer units, all acrylonitrile monomer units, etc. contained in the two or more chloroprene-unsaturated nitrile copolymers are within the above-mentioned numerical ranges, relative to 100% by mass of the total of the two or more chloroprene-unsaturated nitrile copolymers contained in the chloroprene-unsaturated nitrile copolymer latex.

[0029] A chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention has a functional group having a structure represented by chemical formula (1).

[0030]

[0031] In chemical formula (1), R 1 represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a substituted or unsubstituted mercapto group, and a substituted or unsubstituted heterocyclyl group.

[0032] The functional group having the structure represented by chemical formula (1) can be introduced by carrying out the polymerization process of the chloroprene-unsaturated nitrile copolymer in the presence of a xanthogen compound. Xanthogen compounds that can be used to introduce the functional group having the structure represented by chemical formula (1) will be described later in the section on production method. A vulcanized molded article of a rubber composition containing a rubber component of the chloroprene-unsaturated nitrile copolymer latex according to the present invention has excellent oil resistance and generates little heat in a dynamic environment because the chloroprene-unsaturated nitrile copolymer has a functional group having the structure represented by chemical formula (1).

[0033] 1.2 Hydrolyzed Product of Unsaturated Nitrile In the chloroprene-unsaturated nitrile copolymer according to the present invention, the content of the hydrolyzed product of the unsaturated nitrile in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer. Generally, it is believed that unsaturated nitriles are hydrolyzed to form amides, alcohols, or ethers, and are ultimately decomposed into carboxylic acids and ammonia. In the present invention, the hydrolyzed product of the unsaturated nitrile may contain amides, nitriles, alcohols, ethers, carboxylic acids, and ammonia derived from the unsaturated nitrile. In the present invention, the hydrolyzed product of the unsaturated nitrile may be a compound derived from the unsaturated nitrile, such as a compound containing a cyano group, a compound containing an amide group, a compound containing a carboxy group, or a compound containing an amino group (including ammonia).

[0034] When the unsaturated nitrile is acrylonitrile, the hydrolysate of the unsaturated nitrile may contain acrylamide, 2-cyanoethanol, 2-cyanoethyl ether, acrylic acid, and ammonia, or may be acrylamide, 2-cyanoethanol, 2-cyanoethyl ether, acrylic acid, and ammonia.When the unsaturated nitrile is methacrylonitrile, the hydrolysate of the unsaturated nitrile may contain methacrylamide, 3-hydroxy-2-methylpropanenitrile, 3-(2-cyanopropoxy)-2-methylpropanenitrile, methacrylic acid, and ammonia, or may be methacrylamide, 3-hydroxy-2-methylpropanenitrile, 3-(2-cyanopropoxy)-2-methylpropanenitrile, methacrylic acid, and ammonia. In the case of phenylacrylonitrile, it may include 3-phenylpropionamide, α-(hydroxymethyl)benzeneacetonitrile, α,α'-[oxybis(methylene)]bis[α-methylbenzeneacetonitrile], 2-phenylpropionic acid, and ammonia, and may be 3-phenylpropionamide, α-(hydroxymethyl)benzeneacetonitrile, α,α'-[oxybis(methylene)]bis[α-methylbenzeneacetonitrile], 2-phenylpropionic acid, and ammonia.

[0035] In the chloroprene-unsaturated nitrile copolymer according to the present invention, the content of the unsaturated nitrile hydrolysate in the chloroprene-unsaturated nitrile copolymer latex relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer is 0.10 to 9.00 parts by mass, for example, 0.10, 0.20, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00, 5.50, 6.00, 6.50, 7.00, 7.50, 8.00, 8.50, or 9.00 mass%, and may be within a range between any two of the numerical values ​​exemplified here. Furthermore, in the chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention, the total content of the unsaturated nitrile-derived amide, nitrile, alcohol, ether, carboxylic acid, and ammonia may be within the above numerical range, and the contents of the unsaturated nitrile-derived amide, nitrile, alcohol, and ether may also be within the above numerical range. Furthermore, in the chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention, the total content of acrylamide, 2-cyanoethanol, 2-cyanoethyl ether, acrylic acid, ammonia, methacrylamide, 3-hydroxy-2-methylpropanenitrile, 3-(2-cyanopropoxy)-2-methylpropanenitrile, methacrylic acid, 3-phenylpropionamide, α-(hydroxymethyl)benzeneacetonitrile, α,α'-[oxybis(methylene)]bis[α-methylbenzeneacetonitrile], and 2-phenylpropionic acid may be within the above-mentioned numerical range, and the total content of acrylamide, 2-cyanoethanol, 2-cyanoethyl ether, methacrylamide, 3-hydroxy-2-methylpropanenitrile, 3-(2-cyanopropoxy)-2-methylpropanenitrile, 3-phenylpropionamide, α-(hydroxymethyl)benzeneacetonitrile, and α,α'-[oxybis(methylene)]bis[α-methylbenzeneacetonitrile] may be within the above-mentioned numerical range.

[0036] In the chloroprene-unsaturated nitrile copolymer according to the present invention, the content of acrylonitrile hydrolysates in the chloroprene-unsaturated nitrile copolymer latex relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer is preferably within the above-mentioned numerical range. In one example, the content of unsaturated nitrile hydrolysates can be the total content of 2-cyanoethanol, 2-cyanoethyl ether, and acrylamide, and the content of acrylonitrile hydrolysates can be the total content of 2-cyanoethanol, 2-cyanoethyl ether, and acrylamide. In the chloroprene-unsaturated nitrile copolymer according to the present invention, the total content of 2-cyanoethanol, 2-cyanoethyl ether, and acrylamide in the chloroprene-unsaturated nitrile copolymer latex relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer is preferably within the above-mentioned numerical range.

[0037] In a chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention, the 2-cyanoethanol content in the chloroprene-unsaturated nitrile copolymer latex may be 0.05 to 8.00 parts by mass relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer. The 2-cyanoethanol content may be, for example, 0.05, 0.10, 0.20, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00, 5.50, 6.00, 6.50, 7.00, 7.50, or 8.00% by mass, or may be within a range between any two of the values ​​exemplified here.

[0038] In a chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention, the 2-cyanoethyl ether content in the chloroprene-unsaturated nitrile copolymer latex relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer can be 0.05 to 8.00 parts by mass. The 2-cyanoethyl ether content is, for example, 0.05, 0.10, 0.20, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00, 5.50, 6.00, 6.50, 7.00, 7.50, or 8.00 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0039] In the chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention, the acrylamide content in the chloroprene-unsaturated nitrile copolymer latex can be 0.05 to 8.00 parts by mass relative to 100 parts by mass of the chloroprene-unsaturated nitrile copolymer. The acrylamide content is, for example, 0.05, 0.10, 0.20, 0.50, 1.00, 1.50, 2.00, 2.50, 3.00, 3.50, 4.00, 4.50, 5.00, 5.50, 6.00, 6.50, 7.00, 7.50, or 8.00% by mass, and may be within a range between any two of the values ​​exemplified here.

[0040] The chloroprene-unsaturated nitrile copolymer according to one embodiment of the present invention has an unsaturated nitrile hydrolysate content within the above-mentioned range, and therefore has excellent storage stability at high temperatures for long periods of time. Furthermore, a vulcanized molded article of a rubber composition containing a chloroprene-unsaturated nitrile copolymer latex as a rubber component has excellent oil resistance and generates little heat in a dynamic environment. The content of the unsaturated nitrile hydrolysate can be controlled by adjusting the production conditions during polymerization of the chloroprene-unsaturated nitrile copolymer, particularly the amount of water and alkali relative to the raw material monomers used in polymerization, the type and amount of raw material monomers blended, the timing of portionwise addition, the polymerization temperature, and the concentration of each monomer in the polymerization solution.

[0041] The content of unsaturated nitrile hydrolysates in chloroprene-unsaturated nitrile copolymer latex can be determined by analyzing a solution obtained by diluting chloroprene-unsaturated nitrile copolymer latex with tetrahydrofuran using gas chromatography, for example, a gas chromatograph (GC) system. Specifically, the analysis can be performed using the method described in the Examples. As an alternative method, since ammonia, one of the unsaturated nitrile hydrolysates, has a strong irritating odor, its generation can be confirmed by the presence or absence of an irritating odor in the polymerization solution. Furthermore, since carboxylic acid is thought to be generated simultaneously with ammonia based on the decomposition mechanism, the presence or absence of carboxylic acid generation can be confirmed by the presence or absence of ammonia generation. For example, if the ammonia concentration in chloroprene-unsaturated nitrile copolymer latex is 1 ppm or higher, the irritating odor can be detected in the working environment. For example, the ammonia concentration in chloroprene-unsaturated nitrile copolymer latex can be less than 1 ppm. Furthermore, the ammonia concentration can be analyzed by ion chromatography. Furthermore, carboxylic acid can also be analyzed by ion chromatography, liquid chromatography, or gas chromatography.

[0042] The chloroprene-unsaturated nitrile copolymer latex according to one embodiment of the present invention can contain, in addition to the chloroprene-unsaturated nitrile copolymer and the hydrolyzate of the unsaturated nitrile, a compound used in polymerizing the chloroprene-unsaturated nitrile copolymer, and the like.

[0043] 1.3 Characteristics of Chloroprene-Unsaturated Nitrile Copolymer Latex The solid content concentration of the chloroprene-unsaturated nitrile copolymer latex according to one embodiment of the present invention can be adjusted depending on the application. The solid content concentration is not particularly limited, but may be, for example, 40, 45, 50, 55, 60, 65, or 70 mass%, or may be within a range between any two of the values ​​exemplified here.

[0044] When the chloroprene-unsaturated nitrile copolymer latex according to one embodiment of the present invention is adjusted to a solids concentration of 50% by mass and stored at 40°C for 4 months, the viscosity is preferably less than 1,000 cps. The viscosity after storage at 40°C for 4 months is, for example, 100, 200, 300, 400, 500, 600, 700, 800, 900, or 950 cps, and may be within a range between any two of the values ​​exemplified here. The viscosity can be measured using a Brookfield viscometer, and specifically, can be analyzed by the method described in the examples.

[0045] 2. Method for Producing Chloroprene-Unsaturated Nitrile Copolymer Latex The method for producing the chloroprene-unsaturated nitrile copolymer latex according to the present invention is not particularly limited. A method for producing a chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units according to one embodiment of the present invention may include a polymerization step of polymerizing raw material monomers including chloroprene monomers and unsaturated nitrile monomers in an aqueous solution containing water in the presence of a xanthogen compound to obtain the chloroprene-unsaturated nitrile copolymer. Furthermore, the amount of water may be less than 150 parts by mass, relative to 100 parts by mass of all raw material monomers used in the polymerization step.

[0046] In the polymerization step, raw material monomers including a chloroprene monomer and an unsaturated nitrile monomer are polymerized in an aqueous solution containing water to obtain a chloroprene-unsaturated nitrile copolymer.

[0047] The raw material monomers include a chloroprene monomer and an unsaturated nitrile monomer, and may also include other monomers in addition to the chloroprene monomer and the unsaturated nitrile monomer. Examples of such other monomers are as described above. The blending ratio of each monomer in the raw material monomers is preferably adjusted so that the contents of the chloroprene monomer units, unsaturated nitrile monomer units, and other monomer units in the resulting chloroprene-unsaturated nitrile copolymer fall within the above-described numerical ranges.

[0048] A portion of the raw material monomers may be initially added, and a portion thereof may be added in portions after the initiation of polymerization. For example, the polymerization process may include a first addition step of adding at least a portion of the raw material monomers including chloroprene and an unsaturated nitrile, and a second addition step of adding the remaining raw material monomers.

[0049] In the first addition step according to one embodiment of the present invention, when the total amount of chloroprene monomers added in the polymerization step is taken as 100 parts by mass, at least 10 parts by mass of chloroprene monomer can be added. For example, 10, 20, 30, 40, 50, 60, or 70 parts by mass can be added, and the amount may be within a range between any two of the values ​​exemplified here. Furthermore, in the first addition step, when the total amount of unsaturated nitriles added in the polymerization step is taken as 100 parts by mass, at least 50 parts by mass of unsaturated nitrile can be added. For example, 50, 60, 70, 80, 90, or 100 parts by mass can be added, and the amount may be within a range between any two of the values ​​exemplified here. In the first addition step according to one embodiment of the present invention, the above-mentioned amounts of raw material monomers, emulsifier, and, if necessary, RAFT agent and molecular weight additive are added to water. Thereafter, a polymerization initiator is added to initiate polymerization.

[0050] In the second addition step according to one embodiment of the present invention, when the total amount of chloroprene monomers added in the polymerization step is taken as 100 parts by mass, at least 30 parts by mass of chloroprene monomer may be added. For example, 30, 40, 50, 60, or 70 parts by mass may be added, and the amount may be within a range between any two of the values ​​exemplified herein. Furthermore, when the total amount of unsaturated nitriles added in the polymerization step is taken as 100 parts by mass, 0, 10, 20, or 30 parts by mass of unsaturated nitrile may be added, and the amount may be within a range between any two of the values ​​exemplified herein. In the second addition step, no unsaturated nitrile may be added. In the second addition step, it is preferable to add the remaining raw material monomers in two or more divided additions. In the second addition step, the remaining raw material monomers may be added in divided additions, for example, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 divided additions, and the number of divided additions may be within a range between any two of the values ​​exemplified herein. In the second addition step, the remaining raw material monomers can also be added continuously at a constant flow rate.

[0051] During the polymerization, it is preferable to add raw material monomers in portions so that the amount of unsaturated nitrile monomer in the polymerization liquid is maintained at 20 to 90 parts by mass, assuming that the amount of unreacted monomer in the polymerization liquid (e.g., the total of chloroprene monomer and acrylonitrile monomer) is 100 parts by mass. The amount of unsaturated nitrile monomer per 100 parts by mass of unreacted monomer in the polymerization liquid is, for example, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, or 90 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here.

[0052] In a polymerization process according to one embodiment of the present invention, the amount of water can be less than 150 parts by mass, assuming that the total amount of raw material monomers used in the polymerization process is 100 parts by mass. The amount of water may be, for example, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, or 149 parts by mass, and may be within a range between any two of the values ​​exemplified here. In a polymerization process according to one embodiment of the present invention, by reducing the amount of water compared to conventional production methods, the amount of unsaturated nitrile hydrolysate produced can be reduced. Furthermore, unsaturated nitrile hydrolysates, such as acrylamide, 2-cyanoethanol, and 2-cyanoethyl ether, place a heavy burden on wastewater treatment, and reducing the production of these hydrolysates is advantageous in terms of reducing the environmental impact and reducing the effort and cost of wastewater treatment.

[0053] The emulsifier used in emulsion polymerization is not particularly limited, and any known emulsifier generally used in emulsion polymerization of chloroprene polymers can be used. Examples of the emulsifier include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g., potassium rosinate), and alkali metal salts of formalin condensates of β-naphthalenesulfonic acid (e.g., sodium salt).

[0054] The amount of emulsifier added is preferably 0.2 to 20 parts by mass, more preferably 2 to 10 parts by mass, based on 100 parts by mass of all raw material monomers used in the polymerization step.

[0055] As a molecular weight modifier used in emulsion polymerization, at least a xanthogen compound is used. In the polymerization step according to one embodiment of the present invention, in addition to the xanthogen compound, a known molecular weight modifier generally used in emulsion polymerization of chloroprene can be used in combination. Examples of other molecular weight modifiers include mercaptan compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds.

[0056] In the polymerization step according to the present invention, the terminal structure represented by chemical formula (1) can be introduced into the chloroprene-unsaturated nitrile copolymer by carrying out the polymerization in the presence of a xanthogen compound.

[0057] In chemical formula (1), R 1 represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a substituted or unsubstituted mercapto group, and a substituted or unsubstituted heterocyclyl group.

[0058] Examples of xanthogen compounds include dialkyl xanthogen disulfides such as dimethyl xanthogen disulfide, diethyl xanthogen disulfide, diisopropyl xanthogen disulfide, and dibutyl xanthogen trisulfide. Other examples include dialkyl xanthogen trisulfides such as diethyl xanthogen trisulfide, diisopropyl xanthogen trisulfide, and dibutyl xanthogen trisulfide. Furthermore, dialkyl xanthogens having four or more sulfur atoms linking the xanthogens, such as dialkyl xanthogen polysulfides such as diethyl xanthogen polysulfide, diisopropyl xanthogen polysulfide, and dibutyl xanthogen polysulfide, can also be used. The number of carbon atoms in the alkyl group of these dialkyl xanthogen sulfide compounds is preferably 1 to 10, and more preferably 1 to 6, from the viewpoint of solubility in chloroprene monomer.

[0059] The amount of molecular weight modifier added is not particularly limited, but is preferably 0.002 to 20 parts by mass per 100 parts by mass of the total of the chloroprene monomer and the unsaturated nitrile monomer. The amount of xanthogen compound added is preferably 0.002 to 20 parts by mass per 100 parts by mass of the total of the chloroprene monomer and the unsaturated nitrile monomer. By setting the amount within this range, the polymerization reaction can be easily controlled, and an appropriate amount of the functional group represented by chemical formula (1) can be introduced into the chloroprene-unsaturated nitrile copolymer.

[0060] As the polymerization initiator, a known radical polymerization initiator can be used, such as potassium persulfate, benzoyl peroxide, hydrogen peroxide, or an azo compound. A known RAFT agent can also be used during polymerization. In one embodiment of the present invention, a RAFT agent need not be used during polymerization.

[0061] The polymerization temperature and the final conversion rate of the monomer are not particularly limited, but the polymerization temperature may be, for example, 0 to 50°C or 10 to 50°C. The polymerization may be carried out so that the final conversion rate of the monomer falls within the range of 40 to 95% by mass. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.

[0062] The polymerization terminator is not particularly limited, and any known polymerization terminator generally used in emulsion polymerization of chloroprene can be used, such as phenothiazine (thiodiphenylamine), 4-t-butylcatechol, and 2,2-methylenebis-4-methyl-6-t-butylphenol.

[0063] Furthermore, to the chloroprene-unsaturated nitrile copolymer latex obtained by the production method of one embodiment of the present invention, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, and the like can be optionally added after polymerization within a range that does not impair the effects of the present invention.

[0064] 3. Rubber Component of Chloroprene-Unsaturated Nitrile Copolymer Latex One embodiment of the present invention is a rubber component of the above-mentioned chloroprene-unsaturated nitrile copolymer. There are no particular limitations on the method for obtaining the rubber component of the chloroprene-unsaturated nitrile copolymer latex. For example, the rubber component of the chloroprene-unsaturated nitrile copolymer can be obtained by mixing the chloroprene-unsaturated nitrile copolymer latex with a large amount of methanol, precipitating, filtering, and drying. For example, the rubber component of the chloroprene-unsaturated nitrile copolymer can be obtained by freeze-drying the chloroprene-unsaturated nitrile copolymer latex. Specifically, the rubber component of the chloroprene-unsaturated nitrile copolymer can be obtained by adjusting the pH of the chloroprene-unsaturated nitrile copolymer latex, freeze-drying it, washing it with water, and drying it with hot air. The rubber component of the chloroprene-unsaturated nitrile copolymer includes a methanol precipitate of the chloroprene-unsaturated nitrile copolymer latex and a freeze-dried product of the chloroprene-unsaturated nitrile copolymer latex.

[0065] In the rubber component according to one embodiment of the present invention, a rubber composition having the composition described in the examples is prepared, and the rubber composition is press-vulcanized in accordance with JIS K 6250 at 170°C for 20 minutes to produce a vulcanized molded product. When the vulcanized molded product is immersed in a test oil (high-temperature lubricating oil for automobiles, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours, the volume change is preferably less than 45% by mass.

[0066] The rubber component according to one embodiment of the present invention is prepared by preparing a rubber composition having the composition described in the examples, press-vulcanizing the rubber composition at 170°C for 20 minutes to produce a cylindrical vulcanized molded article having a diameter of 15 mm and a height of 25 mm, and evaluating the vulcanized molded article in a constant strain flexometer test according to JIS K 6265:2018 under conditions of 50°C, strain of 0.175 inches, load of 55 pounds, and frequency of 1,800 vibrations per minute. The heat buildup (ΔT) determined by the test is preferably less than 45°C. Heat buildup can be evaluated using a Goodrich Flexometer (JIS K 6265:2018). The Goodrich Flexometer is a testing method for evaluating fatigue characteristics due to heat generation inside a test piece of vulcanized rubber or the like by applying a dynamic, repeated load to the test piece. More specifically, a static initial load is applied to the test piece under constant temperature conditions, and then a sinusoidal vibration of constant amplitude is applied, and the heat generation temperature and creep amount of the test piece, which change over time, are measured.

[0067] 4. Rubber Composition A rubber composition according to one embodiment of the present invention includes the rubber component described above. In addition to the rubber component described above, the rubber composition according to the present invention may include, as necessary, a vulcanizing agent, a vulcanization accelerator, an antioxidant, a filler, a reinforcing material, a silane coupling agent, a plasticizer, a softener, a lubricant, and a processing aid, and may further include components such as a stabilizer, a flame retardant, and a vulcanization retarder, as long as the effects of the present invention are not impaired.

[0068] 4.1 Vulcanizing Agent The rubber composition according to the present invention may contain a vulcanizing agent. The type of vulcanizing agent is not particularly limited as long as it does not impair the effects of the present invention. The vulcanizing agent is preferably a vulcanizing agent that can be used to vulcanize chloroprene-based rubber. One or more vulcanizing agents can be freely selected and used. Examples of vulcanizing agents include sulfur, zinc oxide, and organic peroxides.

[0069] An example of the metal oxide is zinc oxide. The metal oxide preferably contains zinc oxide, and more preferably is zinc oxide.

[0070] Examples of organic peroxides include dicumyl peroxide, benzoyl peroxide, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, diisobutyryl peroxide, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl)peroxydicarbonate, and di(2-ethylhexyl)peroxydicarbonate. butylperoxyneodecanoate, t-butylperoxyneoheptanoate, t-hexylperoxypivalate, t-butylperoxypivalate, di(3,5,5-trimethylhexanoyl)peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, t-butylperoxy-2-ethylhexanoate, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, dibenzoyl peroxide, 1,1-di(t-butylperoxy)-2-methylcyclohexane, 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2, 2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexylperoxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, 2,Examples of such peroxides include 2-di-(t-butylperoxy)butane, t-butyl peroxybenzoate, n-butyl 4,4-di-(t-butylperoxy)valerate, 1,4-bis[(t-butylperoxy)isopropyl]benzene, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-butyl peroxide, p-menthane hydroperoxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide. Among these, at least one selected from dicumyl peroxide, 1,4-bis[(t-butylperoxy)isopropyl]benzene, t-butyl-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3 is preferred, and 1,4-bis[(t-butylperoxy)isopropyl]benzene is particularly preferred.

[0071] From the viewpoint of ensuring processing safety and obtaining a good vulcanizate, the rubber composition according to the present invention preferably contains 3 to 15 parts by mass of a vulcanizing agent relative to the rubber component contained in the rubber composition. The content of the vulcanizing agent is, for example, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass relative to 100 parts by mass of the rubber component contained in the rubber composition, and may be within a range between any two of the numerical values ​​exemplified here.

[0072] 4.2 Acid Acceptor The rubber composition according to one embodiment of the present invention may contain an acid acceptor. Examples of the acid acceptor include magnesium oxide, lead oxide, trimead tetroxide, iron trioxide, titanium dioxide, calcium oxide, and hydrotalcite. As the hydrotalcite, one represented by the following formula can be used: [M 2+ 1-x M 3+ x (OH) 2 ] x+ [A n-x/n ・mH2 O] x-

[0073] In the above formula, M 2+ : Mg 2+ , Zn 2+ At least one divalent metal ion M selected from 3+ :Al 3+ , Fe 3+ At least one trivalent metal ion selected from the following: n- :CO 3 2- , Cl ― , NO 3 2- At least one n-type anion selected from the following: X: 0<X≦0.33.

[0074] As the hydrotalcite, Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 ・3.5H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 , Mg 4 Al 2 (OH) 12 CO 3 ・3.5H 2 O, Mg 6 Al 2 (OH) 16 CO 3 ・4H 2 O, Mg 5 Al 2 (OH) 14 CO 3 ・4H 2 O, Mg 3 Al 2 (OH) 10 CO 3 ・1.7H2 O, and particularly preferably Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 It is O.

[0075] The amount of the acid acceptor added may be 0.1 to 15 parts by mass per 100 parts by mass of the rubber component. The amount of the hydrotalcite added may be, for example, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, and may be within a range between any two of the numerical values ​​exemplified here. The hydrotalcites may be used alone or in combination of two or more.

[0076] 4.3 Vulcanization Accelerator The rubber composition according to the present invention may contain a vulcanization accelerator, and may contain 0.3 to 5.0 parts by mass of the vulcanization accelerator per 100 parts by mass of the rubber composition contained in the rubber composition. The content of the vulcanization accelerator is, for example, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass, and may be within a range between any two of the values ​​exemplified here. Note that the rubber composition according to the present invention may not contain a vulcanization accelerator.

[0077] The type of vulcanization accelerator is not particularly limited as long as it does not impair the effects of the present invention. The vulcanization accelerator is preferably a vulcanization accelerator that can be used for vulcanizing chloroprene-based rubber. One or more vulcanization accelerators can be freely selected and used. Examples of vulcanization accelerators include thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthogenate-based, and thiazole-based accelerators.

[0078] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, etc. Examples of dithiocarbamate vulcanization accelerators include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, tellurium diethyldithiocarbamate, etc. Examples of thiourea-based vulcanization accelerators include thiourea compounds such as ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), and 1,3-trimethylene-2-thiourea. Examples of guanidine-based vulcanization accelerators include 1,3-diphenyl guanidine, 1,3-di-o-tolyl guanidine, 1-o-tolyl biguanide, and di-o-tolyl guanidine salt of dicatechol borate. Examples of xanthate-based vulcanization accelerators include zinc butyl xanthogenate and zinc isopropyl xanthogenate. Examples of thiazole vulcanization accelerators include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, 2-(4'-morpholinodithio)benzothiazole, N-cyclohexylbenzothiazole-2-sulfenamide, etc. These may be used alone or in combination of two or more.

[0079] 4.4 Filler (Reinforcing Material) The rubber composition according to the present invention may contain a filler. Examples of the filler (reinforcing material) include furnace carbon black such as SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, and SRF, modified carbon black such as hydrophilic carbon black, thermal carbon such as channel black, lamp black, FT, and MT, acetylene black, ketjen black, silica, clay, talc, and calcium carbonate. These may be used alone or in combination of two or more.

[0080] A rubber composition according to one embodiment of the present invention may contain 5 to 130 parts by mass of a filler per 100 parts by mass of the rubber component. The filler content may be, for example, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, or 130 parts by mass, or may be within a range between any two of the values ​​exemplified here. By containing the filler content within the above range, the rubber composition according to one embodiment of the present invention can appropriately adjust the hardness of the vulcanized molded product.

[0081] 4.5 Silane Coupling Agent The rubber composition according to one embodiment of the present invention may contain a silane coupling agent. When the rubber composition according to one embodiment of the present invention contains silica as a filler, it preferably contains a silane coupling agent. The silane coupling agent is not particularly limited, and those used in commercially available rubber compositions can be used, for example, vinyl coupling agents, epoxy coupling agents, styryl coupling agents, methacrylic coupling agents, acrylic coupling agents, amino coupling agents, polysulfide coupling agents, and mercapto coupling agents. In particular, from the viewpoint of scorch resistance and reinforcing effect, vinyl coupling agents, methacrylic coupling agents, and acrylic coupling agents, which initiate reaction under high temperature conditions during crosslinking, are preferred.

[0082] The rubber composition according to one embodiment of the present invention may contain 0.5 to 15 parts by mass of a silane coupling agent per 100 parts by mass of silica contained in the rubber composition, for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, or may be within a range between any two of the values ​​exemplified here. These may be used alone or in combination of two or more. By including the above-mentioned silane coupling agent and setting the content of the silane coupling agent within the above-mentioned range, the dispersibility of the silica filler in the rubber and the reinforcing effect between the rubber and the silica filler can be improved, and the occurrence of scorch can be suppressed.

[0083] 4.6 Plasticizer The plasticizer is not particularly limited as long as it is compatible with the chloroprene-unsaturated nitrile copolymer rubber. Examples include vegetable oils such as rapeseed oil, phthalate-based plasticizers, dioctyl sebacate (DOS), dibutyl sebacate (DBS), dioctyl adipate (DOA), ester-based plasticizers, ether ester-based plasticizers, thioether-based plasticizers, aromatic oils, and naphthenic oils. These may be used alone or in combination of two or more. The amount of plasticizer added may be 0 to 50 parts by mass per 100 parts by mass of the rubber component contained in the rubber composition, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, and may be within a range between any two of the values ​​exemplified here.

[0084] 4.7 Lubricants and Processing Aids The rubber composition according to the present invention may further contain a lubricant and / or a processing aid. Lubricants and processing aids are added primarily to improve processability, such as by making the rubber composition easier to release from rolls, molding dies, extruder screws, etc. Examples of lubricants and processing aids include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, fatty acid amides, petrolatum, and factice. These may be used alone or in combination of two or more. The rubber composition according to the present invention may contain 0.5 to 15 parts by mass of lubricant and processing aid per 100 parts by mass of the rubber component, and may also contain 1 to 10 parts by mass. The content of the lubricant and processing aid may be, for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, and may fall within a range between any two of the values ​​exemplified herein.

[0085] 4.8 Others In addition to the above-mentioned components, the rubber composition according to the present invention may further contain components such as antioxidants, antioxidants, flame retardants, and vulcanization retarders, as long as the effects of the present invention are not impaired. Examples of antioxidants and antioxidants include ozone antioxidants, phenolic antioxidants, amine antioxidants, acrylate antioxidants, imidazole antioxidants, aromatic secondary amine antioxidants, carbamic acid metal salts, waxes, phosphorus-based antioxidants, and sulfur-based antioxidants. Examples of imidazole antioxidants include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and zinc salts of 2-mercaptobenzimidazole. The rubber composition according to the present invention may contain a total of 0.1 to 10 parts by mass of antioxidants and antioxidants per 100 parts by mass of the rubber component contained in the rubber composition.

[0086] 5. Method for Producing Rubber Composition The rubber composition according to one embodiment of the present invention is obtained by kneading a rubber component, a chloroprene-unsaturated nitrile copolymer latex, and other necessary components at a temperature equal to or lower than the vulcanization temperature. Examples of devices for kneading the raw material components include conventionally known kneading devices such as mixers, Banbury mixers, kneader mixers, and open rolls.

[0087] 6. Unvulcanized molded body, vulcanized product, and vulcanized molded body The unvulcanized molded body according to one embodiment of the present invention uses the rubber composition according to one embodiment of the present invention, and is a molded body (molded article) of the rubber composition (unvulcanized state) according to one embodiment of the present invention. A method for producing an unvulcanized molded body according to one embodiment of the present invention includes a step of molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The unvulcanized molded body according to one embodiment of the present invention is made of the rubber composition (unvulcanized state) according to one embodiment of the present invention.

[0088] A vulcanizate according to one embodiment of the present invention is a vulcanizate of the rubber composition according to one embodiment of the present invention. A method for producing a vulcanizate according to one embodiment of the present invention includes a step of vulcanizing the rubber composition according to one embodiment of the present invention.

[0089] A vulcanization molded article according to one embodiment of the present invention is a vulcanization molded article of a rubber composition according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention uses a vulcanizate according to one embodiment of the present invention and is a molded article (molded product) of the vulcanizate according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention is made of a vulcanizate according to one embodiment of the present invention.

[0090] The vulcanized molded article according to one embodiment of the present invention can be obtained by molding a vulcanizate obtained by vulcanizing the rubber composition (unvulcanized state) according to one embodiment of the present invention, and can also be obtained by vulcanizing a molded article obtained by molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention can be obtained by vulcanizing the rubber composition according to one embodiment of the present invention after molding or during molding. A method for producing a vulcanized molded article according to one embodiment of the present invention comprises a step of molding a vulcanized article according to one embodiment of the present invention, or a step of vulcanizing an unvulcanized molded article according to one embodiment of the present invention.

[0091] The vulcanized molded article according to one embodiment of the present invention preferably exhibits a volume change of less than 45% by mass when immersed for 72 hours in a test oil (high-grade automotive lubricating oil, ASTM No. 3, IRM 903 oil) at 130° C. Furthermore, the vulcanized molded article according to one embodiment of the present invention is preferably cylindrical with a diameter of 15 mm and a height of 25 mm, and exhibits a heat release (ΔT) of less than 45° C. as determined by a constant strain flexometer test according to JIS K 6265:2018 under conditions of 50° C., a strain of 0.175 inches, a load of 55 pounds, and a frequency of 1,800 vibrations per minute.

[0092] The unvulcanized molded article, vulcanized product, and vulcanized molded article according to one embodiment of the present invention can be used as rubber parts in various industrial fields, such as buildings, structures, ships, railways, coal mines, and automobiles. The rubber composition according to the present invention has excellent oil resistance and generates little heat in dynamic environments, so it can be used for various components where these properties are required. The rubber composition, vulcanized product, and vulcanized molded article according to one embodiment of the present invention can be used as rubber parts in various industrial fields, such as buildings, structures, ships, railways, coal mines, and automobiles, and can be used for rubber parts such as automotive rubber components (e.g., automotive seals), hose materials, rubber molds, gaskets, rubber rolls, industrial cables, industrial conveyor belts, and sponges. In particular, they can be used as transmission belts, conveyor belts, hoses, wipers, immersion products, sealing parts, adhesives, boots, rubber-coated fabrics, rubber rolls, vibration-proof rubber, or sponge products.

[0093] (Automotive Rubber Components) Automotive rubber components include gaskets, oil seals, and packings, which are used to prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust into machinery and equipment. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets whose sealing parts are fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can enhance oil resistance and reduce heat generation in dynamic environments. This makes it possible to manufacture automotive parts with excellent oil resistance and reduced heat generation in dynamic environments, something that was difficult to achieve with conventional rubber compositions.

[0094] (Hose Material) Hose materials are flexible pipes, and specific examples include high- and low-pressure hoses for water supply, oil supply, air supply, steam supply, and hydraulic applications. The rubber composition of the present invention can improve the oil resistance of the hose material and reduce heat generation in dynamic environments while maintaining the processability of the unvulcanized product. This makes it possible to produce, for example, a hose material that has excellent oil resistance and generates less heat in dynamic environments, which was difficult to achieve with conventional rubber compositions.

[0095] (Rubber molded products) Examples of rubber molded products include vibration-isolating rubber, vibration-damping materials, and boots. Vibration-isolating rubber and vibration-damping materials are rubbers that prevent the transmission and spread of vibration. Specific examples include torsional dampers, engine mounts, and muffler hangers for automobiles and various other vehicles that absorb vibrations and prevent noise when the engine is running. The rubber composition of the present invention can improve the oil resistance of vibration-isolating rubber and vibration-damping materials and reduce heat generation in dynamic environments. This makes it possible to produce vibration-isolating rubber and vibration-damping materials that have excellent oil resistance and generate less heat in dynamic environments, which was difficult to achieve with conventional rubber compositions. Boots are bellows-shaped components whose outer diameter gradually increases from one end to the other. Specific examples include boots for constant velocity joint covers, boots for ball joint covers (dust cover boots), and boots for rack and pinion gears that protect drive parts such as automobile drive systems. The rubber composition of the present invention can improve oil resistance and reduce heat generation in dynamic environments. This makes it possible to produce boots that can be used in harsher environments than conventional rubber compositions.

[0096] (Gaskets, etc.) Gaskets, oil seals, and packings are components in machines and equipment that prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust into the interior. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets whose sealing parts are fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can improve the oil resistance of these components and reduce heat generation in dynamic environments. This makes it possible to produce sealing components with excellent oil resistance and low heat generation in dynamic environments, which was difficult to achieve with conventional rubber compositions.

[0097] (Rubber Roll) A rubber roll is manufactured by adhesively coating a metal core, such as an iron core, with rubber, and is generally manufactured by spirally winding a rubber sheet around a metal iron core. Rubber materials such as NBR, EPDM, and CR are used for rubber rolls depending on the required characteristics for various applications, such as papermaking, various metal manufacturing, film manufacturing, printing, general industrial use, agricultural machinery such as rice hullers, and food processing. CR has good mechanical strength that can withstand the friction of the objects being conveyed, and is therefore used in a wide range of rubber roll applications. Furthermore, rubber rolls that convey heavy loads have the problem of deformation under load, and improvements are needed. The rubber composition of the present invention can improve the oil resistance of rubber rolls and reduce heat generation under dynamic environments. This makes it possible to manufacture embossing rubber rolls that have excellent oil resistance and low heat generation under dynamic environments, which was difficult to achieve with conventional rubber compositions.

[0098] (Industrial Cable) Industrial cables are linear components for transmitting electrical or optical signals. They are made by covering a good conductor such as copper or a copper alloy, or an optical fiber, with an insulating coating layer, and a wide variety of industrial cables are manufactured depending on their structure and installation location. The rubber composition of the present invention can improve the oil resistance of industrial cables and reduce heat generation in dynamic environments. This makes it possible to manufacture industrial cables that have excellent oil resistance and reduce heat generation in dynamic environments, which was difficult to achieve with conventional rubber compositions.

[0099] (Industrial Conveyor Belts) Industrial conveyor belts are available in rubber, resin, and metal, and are selected to suit a wide variety of uses. Among these, rubber conveyor belts are inexpensive and widely used, but when used in environments where there is a lot of friction and collision with the conveyed materials, they have been prone to damage due to deterioration. The rubber composition of the present invention can improve the oil resistance of industrial conveyor belts and reduce heat generation in dynamic environments. This makes it possible to produce industrial conveyor belts that have excellent oil resistance and generate little heat in dynamic environments, allowing them to be used in harsh environments, which was difficult with conventional rubber compositions.

[0100] (Sponge) Sponges are porous materials with countless fine pores inside, and are specifically used in vibration-damping materials, sponge sealing parts, wetsuits, shoes, etc. The rubber composition of the present invention can improve the acid resistance and water resistance of the sponge. Furthermore, the use of chloroprene-unsaturated nitrile copolymer rubber can also improve the flame retardancy of the sponge. This makes it possible to produce sponges with excellent oil resistance and low heat generation in dynamic environments, which can be used in harsh environments, something that was difficult to achieve with conventional rubber compositions, as well as sponges with excellent flame retardancy. Furthermore, the hardness of the resulting sponge can be appropriately adjusted by adjusting the content of the blowing agent, etc.

[0101] Methods for molding the rubber composition (unvulcanized state) and vulcanized product according to one embodiment of the present invention include press molding, extrusion molding, calendar molding, etc. The temperature for vulcanizing the rubber composition may be appropriately set in accordance with the composition of the rubber composition, and may be 140 to 220°C or 160 to 190°C. The vulcanization time for vulcanizing the rubber composition may be appropriately set depending on the composition of the rubber composition, the shape of the unvulcanized molded product, etc.

[0102] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.

[0103] Example 1 A 3-liter polymerization vessel equipped with a heating / cooling jacket and a stirrer was charged with 23 parts by mass of chloroprene monomer, 35 parts by mass of acrylonitrile monomer, 100 parts by mass of pure water, 5.0 parts by mass of disproportionated potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.4 parts by mass of potassium hydroxide, 1.0 part by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation), and 0.5 parts by mass of diisopropyl xanthogen disulfide. 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and emulsion polymerization was carried out at a polymerization temperature of 40°C under a nitrogen gas flow. During the polymerization, the chloroprene monomer was added in portions so that the amount of unsaturated nitrile monomer in the polymerization solution was maintained at 70 parts by mass ± 20 parts by mass when the unreacted monomer (total of chloroprene monomer and acrylonitrile monomer) in the polymerization solution was taken as 100 parts by mass. The chloroprene monomer was added in portions starting 20 seconds after the start of polymerization, and the portion-by-portion addition flow rate was adjusted using a solenoid valve based on the change in the heat quantity of the refrigerant over the first 10 seconds from the start of polymerization. Thereafter, the flow rate was readjusted every 10 seconds, and the polymerization was continued continuously. When the conversion rate relative to the total amount of chloroprene and acrylonitrile reached 65%, the polymerization was terminated by adding 0.02 parts by mass of phenothiazine as a polymerization terminator. Next, the unreacted monomers, organic solvents, etc. were removed and the mixture was concentrated by distillation under reduced pressure to obtain a chloroprene-unsaturated nitrile copolymer latex 1 having a solids content of 50% by mass.

[0104] (Example 2, Comparative Examples 1 to 4) Chloroprene-unsaturated nitrile copolymer latexes 2 to 6 were obtained in the same manner as in Example 1, except that the amounts of the chloroprene monomer initially added, the amount of the acrylonitrile monomer, the amount of water, and the amount of the chloroprene monomer added in portions, as well as the amount of the unsaturated nitrile monomer relative to the unreacted monomer in the polymerization liquid maintained during polymerization, were as shown in Table 1.

[0105] Comparative Example 5 A chloroprene-unsaturated nitrile copolymer latex 7 was obtained in the same manner as in Example, except that the amounts of the chloroprene monomer initially added, the amount of the acrylonitrile monomer, the amount of water, and the amount of the chloroprene monomer added in portions, as well as the amount of the unsaturated nitrile monomer relative to the unreacted monomers in the polymerization solution maintained during polymerization were as shown in Table 1, and 0.2 parts by mass of benzyl butyl trithiocarbonate was used instead of 0.5 parts by mass of diisopropyl xanthogen disulfide.

[0106] (Contents of Unsaturated Nitrile Hydrolysate in Chloroprene-Unsaturated Nitrile Copolymer Latex) Approximately 1 g of the chloroprene-unsaturated nitrile copolymer latex according to each of the Examples and Comparative Examples was weighed out and diluted to 25 ml with tetrahydrofuran. The obtained solution was analyzed by pyrolysis gas chromatography, and the contents of the chloroprene-unsaturated nitrile copolymer, acrylamide, 2-cyanoethanol, and 2-cyanoethyl ether in the chloroprene-unsaturated nitrile copolymer latex were calculated. Gas chromatography Apparatus name: Agilent Technologies 8890GC system Column: DB-1 0.32 mmφ×30 m (film thickness 5.0 μm) Column temperature: 50°C (5 min) → 50°C / min → 100°C → 15°C / min → 300°C (30 min) Injection port temperature: 270°C Detector temperature: 300°C Detector: FID Note that the chloroprene-unsaturated nitrile copolymer latexes according to the examples and comparative examples did not give off an irritating odor, and generation of ammonia and carboxylic acid was not confirmed.

[0107] (Viscosity after storage at 40°C for 4 months) After storing the chloroprene-unsaturated nitrile copolymer latex (solid content concentration 50% by mass) according to each Example and Comparative Example at 40°C for 4 months, the viscosity was measured using a Brookfield viscometer under the following conditions: Measuring instrument: "VISCOMETER TVB-20L" manufactured by Toki Sangyo Co., Ltd. Spindle rotor: 2M (disc-shaped with a radius of 19 mm and a thickness of 7 mm) Rotation speed: 30 rpm

[0108] The evaluation was based on the following criteria: ○: Less than 1000 cps ×: 1000 cps or more

[0109] <Precipitation of Rubber Component> The pH of the chloroprene-unsaturated nitrile copolymer latex according to each Example and Comparative Example was adjusted to 7.0 using acetic acid or sodium hydroxide, and then the chloroprene-acrylonitrile copolymer latex was demulsified by freeze-coagulating it on a metal plate cooled to −20° C. to obtain a sheet. This sheet was washed with water and then dried at 130° C. for 15 minutes to obtain solid chloroprene-acrylonitrile copolymer rubber components (chloroprene-acrylonitrile copolymers 1 to 7).

[0110] (Nitrogen Content and Acrylonitrile Bond Amount) The nitrogen contents in the chloroprene-unsaturated nitrile copolymers 1 to 7 were measured by a combustion method, and the acrylonitrile bond amount was calculated from the nitrogen contents. The analysis method was based on JIS K6451-1:2016, and an automatic analyzer was used to calculate the nitrogen contents in the samples by the combustion method (Dumas method), and the content of acrylonitrile monomer units (bound acrylonitrile amount) was calculated from the nitrogen contents.

[0111] Specifically, an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Service Co., Ltd.) was used to measure the nitrogen atom content in 100 mg of chloroprene-unsaturated nitrile copolymer, and the content of acrylonitrile monomer units was calculated. Elemental analysis was performed as follows. The electric furnace temperatures were set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen gas was flowed at 0.2 mL / min as the combustion gas and helium gas was flowed at 80 mL / min as the carrier gas. A calibration curve was prepared using aspartic acid (10.52%), which has a known nitrogen content, as a standard substance.

[0112] <Preparation of Rubber Compositions> Rubber compositions were prepared using the rubber components (chloroprene-acrylonitrile copolymers 1 to 7) in the chloroprene-unsaturated nitrile copolymer latexes obtained by freeze-drying the chloroprene-acrylonitrile copolymer latexes 1 to 7 as described above. Specifically, for 100 parts by mass of the rubber component, 3 parts by mass of antioxidant (4,4'-bis(α,α-dimethylbenzyl)diphenylamine (Nocrac CD, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), 1 part by mass of antioxidant (N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine (Nocrac 6C, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 4 parts by mass of acid acceptor (magnesium oxide (Kyowamag 150, manufactured by Kyowa Chemical Industry Co., Ltd.)), 5 parts by mass of zinc oxide (zinc oxide type 2, manufactured by Sakai Chemical Industry Co., Ltd.), 1 part by mass of vulcanization accelerator (trimethylthiourea (Noccela TMU, manufactured by Ouchi Shinko Chemical Industry Co., Ltd.)), 50 parts by mass of filler (carbon black FEF (Asahi Carbon Co., Ltd. Asahi #60)), 10 parts by mass of a plasticizer (an ether ester plasticizer (ADEKA CORPORATION, Adeka Cizer RS-700)), and 1 part by mass of a lubricant (stearic acid (New Japan Chemical Co., Ltd., Stearic Acid 50S)). These were added and kneaded with an 8-inch open roll to obtain rubber compositions 1 to 7.

[0113] <Preparation of Vulcanized Molded Articles> Vulcanized molded articles were prepared using the above rubber compositions 1 to 7. Specifically, the obtained rubber compositions 1 to 7 were press-vulcanized at 170°C for 20 minutes in accordance with JIS K 6250 to prepare sheet-shaped vulcanized molded articles having a thickness of 2 mm. Furthermore, rubber compositions 1 to 7 were press-vulcanized at 170°C for 20 minutes to prepare vulcanized molded articles (cylindrical vulcanized molded articles having a diameter of 15 mm and a height of 25 mm) for Goodrich testing.

[0114] (Oil Resistance) Test specimens measuring 25 mm in length and 20 mm in width were punched out from the above-mentioned sheet-like vulcanized molded article to obtain test specimens. The obtained test specimens were immersed in a test oil (high-grade lubricating oil for automobiles, ASTM No. 3, IRM 903 oil) at 130°C for 72 hours. The volume change rate ΔV was calculated in accordance with JIS K 6258. The obtained volume change rate ΔV was evaluated according to the following criteria: ○: Less than 45% by mass ×: 45% by mass or more

[0115] (Heat generation) Evaluation of heat generation was performed using a Goodrich Flexometer (JIS K 6265:2018). The Goodrich Flexometer is a test method for applying a dynamic repeated load to a test piece such as vulcanized rubber to evaluate fatigue properties due to heat generation inside the test piece. Specifically, a static initial load is applied to the test piece under constant temperature conditions, and a sinusoidal vibration of constant amplitude is further applied to measure the heat generation temperature and creep amount of the test piece that change over time. The test method conforms to JIS K 6265:2018, and heat generation (ΔT) was measured under conditions of 50°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, and evaluated according to the following evaluation criteria. ○: Less than 45°C ×: 45°C or higher

[0116]

Claims

1. A chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units, wherein the chloroprene-unsaturated nitrile copolymer has a nitrogen content of 0.5% by mass or more as measured by a combustion method, and the chloroprene-unsaturated nitrile copolymer has a functional group having a structure represented by chemical formula (1), and the content of an unsaturated nitrile hydrolyzate in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer. (In chemical formula (1), R 1 represents any one of hydrogen, chlorine, a substituted or unsubstituted alkyl group, a substituted or unsubstituted alkenyl group, a substituted or unsubstituted aryl group, a substituted or unsubstituted mercapto group, and a substituted or unsubstituted heterocyclyl group.

2. The chloroprene-unsaturated nitrile copolymer latex according to claim 1, wherein the unsaturated nitrile monomer unit is an acrylonitrile monomer unit, the chloroprene-unsaturated nitrile copolymer has an acrylonitrile bond amount of 2 mass% or more measured in accordance with JIS K 6451-1, and the content of acrylonitrile hydrolysate in the chloroprene-unsaturated nitrile copolymer latex is 0.10 to 9.00 parts by mass per 100 parts by mass of the chloroprene-unsaturated nitrile copolymer.

3. A rubber component of the chloroprene-unsaturated nitrile copolymer latex according to claim 1 or 2.

4. A rubber composition comprising the rubber component according to claim 3.

5. A vulcanized molded article of the rubber composition according to claim 4.

6. The vulcanized molded article according to claim 5, which is a power transmission belt, a conveyor belt, a hose, a wiper, a dipping product, a sealing part, an adhesive, a boot, a rubber-coated cloth, a rubber roll, a vibration-proof rubber or a sponge product.

7. A method for producing a chloroprene-unsaturated nitrile copolymer latex containing a chloroprene-unsaturated nitrile copolymer containing chloroprene monomer units and unsaturated nitrile monomer units, the method comprising a polymerization step of polymerizing raw material monomers containing chloroprene monomers and unsaturated nitrile monomers in an aqueous solution containing water in the presence of a xanthogen compound to obtain a chloroprene-unsaturated nitrile copolymer, wherein the amount of the water is less than 150 parts by mass when the total amount of raw material monomers used in the polymerization step is 100 parts by mass.

Citation Information

Patent Citations

  • Copolymerization of chloroprene with unsaturated nitrile

    JP1980099907A

  • Production of retroreflective sheet of wide angle characteristic

    JP1982010102A

  • Method for producing statistical copolymer containing chloroprene monomer unit and unsaturated nitrile monomer unit, statistical copolymer, latex and use of same

    WO2018207940A1

  • Chloroprene polymer and production method therefor

    WO2019017470A1

  • Sulfur-modified chloroprene rubber composition, vulcanized product, molded article using said vulcanized product and method for producing sulfur-modified chloroprene rubber composition

    WO2019102898A1