Electromagnetic wave absorber and paste for forming electromagnetic wave absorber

The electromagnetic wave absorber, featuring a magnetic material, thermally stable binder resin, and non-dielectric material, addresses the issue of high-temperature degradation, ensuring reliable absorption of high-frequency waves in various systems.

WO2024203732A1PCT designated stage expired Publication Date: 2024-10-03THE UNIV OF TOKYO +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011051
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-24
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing electromagnetic wave absorbers deteriorate in high-temperature environments, affecting their ability to reliably absorb high-frequency electromagnetic waves in applications such as automobile driving support systems and communication systems.

Method used

An electromagnetic wave absorber comprising an electromagnetic wave absorption layer with a magnetic material, a binder resin having specific temperature characteristics, and a non-dielectric material, where the binder resin includes an amorphous or crystalline resin with a glass transition point of 80°C or higher and/or a melting point of 150°C or higher, and the non-dielectric material is distinct from the magnetic material, enhancing thermal stability and absorption performance.

Benefits of technology

The solution provides an electromagnetic wave absorber with stable absorption characteristics even under prolonged high-temperature exposure, maintaining effective performance in high-frequency bands without significant deterioration, suitable for applications in information and communication systems and automotive support systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided are: an electromagnetic wave absorber, the electromagnetic wave absorption characteristics of which are not susceptible to deterioration even when exposed to a high temperature for a long time; and a paste for forming the electromagnetic wave absorber, said paste favorably being used for manufacturing the electromagnetic wave absorber. The electromagnetic wave absorber comprises an electromagnetic wave absorption layer, the electromagnetic wave absorption layer containing a magnetic body, a binder resin, and a non-dielectric material, the binder resin including an amorphous resin that has a glass transition point of 80°C or higher and / or a crystalline resin that has a melting point of 150°C or higher, and the non-dielectric material being different from the magnetic body.
Need to check novelty before this filing date? Find Prior Art

Description

Electromagnetic wave absorber and paste for forming electromagnetic wave absorber

[0001] The present invention relates to an electromagnetic wave absorber and a paste for forming an electromagnetic wave absorber.

[0002] The use of high-frequency electromagnetic waves is becoming widespread in various information and communication systems, such as mobile phones, wireless LANs, ETC systems, intelligent road transport systems, driving assistance systems, and satellite broadcasting. However, the expanded use of high-frequency electromagnetic waves raises concerns that interference between electronic components may cause breakdowns or malfunctions in electronic devices. To address this issue, a method has been adopted in which unwanted electromagnetic waves are absorbed by electromagnetic wave absorbers.

[0003] For this reason, even in radars and the like that use electromagnetic waves in the high frequency band, electromagnetic wave absorbers are used to reduce the effects of unnecessary electromagnetic waves that should not be received. To meet such demands, various electromagnetic wave absorbers that can effectively absorb electromagnetic waves in the high frequency band have been proposed. A specific example is an electromagnetic wave absorbing sheet containing carbon nanocoils and a resin (for example, Patent Document 1).

[0004] Among applications of electromagnetic waves in the high frequency band, research has progressed in the field of automobile driving assistance systems. In such automobile driving assistance systems, electromagnetic waves in the 76 GHz band are used in on-board radar for detecting inter-vehicle distances, etc. It is predicted that the use of electromagnetic waves in high frequency bands, for example, 100 GHz or higher, will expand not only to automobile driving assistance systems but also to various other applications. For this reason, there is a demand for electromagnetic wave absorbers that can effectively absorb electromagnetic waves in the 76 GHz band and higher frequency bands.

[0005] In order to meet such a demand, as an electromagnetic wave absorber that can effectively absorb electromagnetic waves over a wide range in the high frequency band, for example, ε-Fe 2 O 3 An electromagnetic wave absorber having an electromagnetic wave absorbing layer containing magnetic crystals made of iron oxide of the above system has been proposed (for example, Patent Document 2, Non-Patent Documents 1 to 4).

[0006] JP 2009-060060 A JP 2008-277726 A

[0007] A. Namai, S. Sakurai, M. Nakajima, T. Suemoto, K. Matsumoto, M. Goto, S. Sasaki, and S. Ohkoshi, J. Am. Chem. Soc., 131, 1170-1173 (2009). A. Namai, M. Yoshikiyo, K. Yamada, S. Sakurai, T. Goto, T. Yoshida, T. Miyazaki, M. Nakajima, T. Suemoto, H. Tokoro, and S. Ohkoshi, Nature Communications, 3, 1035 / 1-6 (2012). S. Ohkoshi, S. Kuroki, S. Sakurai, K. Matsumoto, K. Sato, and S. Sasaki, Angew. Chem. Int. Ed. , 46, 8392-8395 (2007). A. Namai, K. Ogata, M. Yoshikiyo, and S. Ohkoshi, Bull. Chem. Soc. Jpn. , 93, 20-25 (2020).

[0008] However, when the electromagnetic wave absorber described in Patent Document 1 is exposed to high temperatures for a long period of time, the electromagnetic wave absorption characteristics may deteriorate.

[0009] The present invention has been made in consideration of the above-mentioned problems of the conventional technology, and aims to provide an electromagnetic wave absorber whose electromagnetic wave absorption properties are resistant to deterioration even when exposed to high temperatures for a long period of time, and a paste for forming an electromagnetic wave absorber that is suitable for use in producing such an electromagnetic wave absorber.

[0010] The present inventors have found that the above-mentioned problems can be solved by incorporating a magnetic material, a binder resin having predetermined temperature characteristics, and a non-dielectric material into an electromagnetic wave absorbing layer of an electromagnetic wave absorber, and have thus completed the present invention. Specifically, the present invention provides the following.

[0011] [1] An electromagnetic wave absorber comprising an electromagnetic wave absorbing layer, wherein the electromagnetic wave absorbing layer comprises a magnetic substance, a binder resin, and a non-dielectric material, the binder resin comprises an amorphous resin having a glass transition point of 80°C or higher and / or a crystalline resin having a melting point of 150°C or higher, and the non-dielectric material is different from the magnetic substance.

[0012] [2] The electromagnetic wave absorber according to [1], wherein the electromagnetic wave absorbing layer contains carbon nanotubes.

[0013] [3] The electromagnetic wave absorber according to [1] or [2], wherein the magnetic material contains epsilon iron oxide.

[0014] [4] The electromagnetic wave absorber according to any one of [1] to [3], wherein the amorphous resin and / or the crystalline resin comprises at least one selected from the group consisting of polyurethane resin, polyester-urethane resin, urethane polyamide resin, polycarbonate resin, polyester resin, FR-AS resin, FR-ABS resin, AS resin, ABS resin, polyphenylene oxide resin, polyphenylene sulfide resin, polysulfone resin, polyether sulfone resin, polyether ether ketone resin, fluorine-based resin, polyimide resin, polyamide imide resin, polyamide bismaleimide resin, polyetherimide resin, polybenzoxazole resin, polybenzothiazole resin, polybenzimidazole resin, BT resin, polymethylpentene, ultra-high molecular weight polyethylene, FR-polypropylene, cellulose resin, (meth)acrylic resin, and polystyrene.

[0015] [5] The electromagnetic wave absorber according to any one of [1] to [4], wherein the non-dielectric material comprises at least one selected from the group consisting of barium sulfate, aluminum oxide, aluminum nitride, boron nitride, silicon carbide, silicon dioxide, calcium carbonate, and talc.

[0016] [6] The electromagnetic wave absorber according to any one of [1] to [5], wherein the electromagnetic wave absorbing layer is laminated on a base layer and has a film shape.

[0017] [7] A paste for forming an electromagnetic wave absorber, comprising a magnetic substance, a binder resin, and a non-dielectric material, wherein the binder resin comprises an amorphous resin having a glass transition point of 80°C or higher and / or a crystalline resin having a melting point of 150°C or higher, and the non-dielectric material is different from the magnetic substance.

[0018] According to the present invention, it is possible to provide an electromagnetic wave absorber whose electromagnetic wave absorption properties are resistant to deterioration even when exposed to high temperatures for a long period of time, and a paste for forming an electromagnetic wave absorber that is suitably used for producing the electromagnetic wave absorber.

[0019] Hereinafter, embodiments of the present invention will be described in detail, but the present invention is not limited to the following embodiments and can be implemented with appropriate modifications within the scope of the object of the present invention.

[0020] <Electromagnetic Wave Absorber> The electromagnetic wave absorber includes an electromagnetic wave absorbing layer. The electromagnetic wave absorber may consist of only the electromagnetic wave absorbing layer, or may include a substrate layer that supports the electromagnetic wave absorbing layer.

[0021] From the viewpoint of more reliably absorbing high-frequency electromagnetic waves in the millimeter wave band or higher, the electromagnetic wave absorber preferably absorbs electromagnetic waves in a frequency band of 30 gigahertz (GHz) or higher, preferably 30 GHz or higher and 300 GHz or lower, more preferably 40 GHz or higher and 200 GHz or lower. Furthermore, it is preferable that the return loss of the electromagnetic wave absorber has a peak with an absolute value of 15 dB or higher. The return loss is a value measured on the surface where the electromagnetic wave absorbing layer is exposed.

[0022] The form of the electromagnetic wave absorber is not particularly limited, but is preferably a sheet or film, and more preferably a film. When the electromagnetic wave absorber is in the form of a film, the film may have a curved surface or may be composed of only a flat surface, and is preferably a flat plate. From the viewpoint of making the film thinner or smaller without impairing the effects of the present invention, the thickness of the film as an electromagnetic wave absorber is preferably 1000 μm or less, more preferably 900 μm or less, even more preferably 450 μm or less, and particularly preferably 300 μm or less. The thickness of the film as an electromagnetic wave absorber may be uniform or non-uniform.

[0023] <Electromagnetic Wave Absorbing Layer> The electromagnetic wave absorbing layer includes a magnetic material, a binder resin having predetermined temperature characteristics, and a non-dielectric material. By using a binder resin having predetermined temperature characteristics in combination with a non-dielectric material in an electromagnetic wave absorbing layer containing a magnetic material, an electromagnetic wave absorber is obtained whose electromagnetic wave absorbing characteristics are less likely to deteriorate even when exposed to high temperatures for a long period of time than when either material is used alone. The reason for this effect is not entirely clear, but it is thought to be because the combined use of the two materials can suppress deformation and flow of the electromagnetic wave absorbing layer at high temperatures, making it less likely for the components in the electromagnetic wave absorbing layer to separate.

[0024] The thickness of the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The thickness of the electromagnetic wave absorbing layer is preferably 150 μm or less, more preferably 100 μm or less, from the viewpoint of the balance between thinning of the electromagnetic wave absorber and electromagnetic wave absorption performance. The lower limit of the thickness of the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the effects of the present invention, and examples include 1 μm or more, 10 μm or more, etc. The thickness of the electromagnetic wave absorbing layer may be uniform or non-uniform.

[0025] The essential and optional components of the electromagnetic wave absorbing layer will be described below.

[0026] [Magnetic material (ferromagnetic material)] The electromagnetic wave absorbing layer contains a magnetic material (ferromagnetic material). The type of magnetic material is not particularly limited as long as the electromagnetic wave absorber exhibits desired electromagnetic wave absorption characteristics. From the viewpoint of being able to absorb high-frequency electromagnetic waves of the millimeter wave band or higher, the magnetic material is preferably a magnetic material that magnetically resonates in a frequency band of 30 GHz or higher, and more preferably a magnetic material that magnetically resonates in a frequency band of 30 GHz or higher and 300 GHz or lower.

[0027] The magnetic resonance may be magnetic resonance based on the precession motion of electrons in atoms when they spin in a frequency band equal to or greater than the millimeter wave band. Natural magnetic resonance due to the gyromagnetic effect based on the precession motion in a frequency band equal to or greater than the millimeter wave band is preferred.

[0028] The magnetic material is not particularly limited as long as it can absorb high-frequency electromagnetic waves in the millimeter wave band or higher. Preferred magnetic materials include magnetic materials containing at least one selected from the group consisting of epsilon-type iron oxide, barium ferrite magnetic material, and strontium ferrite magnetic material. Of these, epsilon-type iron oxide is more preferred. In terms of good electromagnetic wave absorption characteristics of the electromagnetic wave absorber, the ratio of the mass of epsilon-type iron oxide to the total mass of the epsilon-type iron oxide and the magnetic material other than epsilon-type iron oxide is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 95 mass% or more, and particularly preferably 100 mass%. Epsilon-type iron oxide will be described below.

[0029] (Epsilon-type iron oxide) As the epsilon-type iron oxide, ε-Fe 2 O 3 Crystal, and crystal structure and space group are ε-Fe 2 O 3 and ε-Fe 2 O 3 A part of the Fe site of the crystal is substituted with an element M other than Fe, and has the formula ε-M x Fe 2-x O 3where x is 0 or more and 2 or less (preferably 0 or more and less than 2). Since such epsilon-type iron oxide crystals are magnetic crystals, the crystals may be referred to as "magnetic crystals" in the present specification.

[0030] ε-Fe 2 O 3 Any crystal can be used. The crystal structure and space group are ε-Fe 2 O 3 and ε-Fe 2 O 3 A part of the Fe site of the crystal is substituted with an element M other than Fe, and has the formula ε-M x Fe 2-x O 3 In this specification, the crystal represented by the formula (1) where x is 0 or more and 2 or less (preferably 0 or more and less than 2) will be described later. 2 O 3 ε-M in which part of the Fe site of the crystal is replaced by a substitution element M x Fe 2-x O 3 "M-substituted ε-Fe 2 O 3 " is also called.

[0031] ε-Fe 2 O 3 Crystalline and / or M-substituted ε-Fe 2 O 3 The particle size of the particles having magnetic crystals in the magnetic phase is not particularly limited as long as it does not impair the object of the present invention. For example, particles having magnetic crystals of epsilon-type iron oxide in the magnetic phase, produced by the method described below, have an average particle size measured from a TEM (transmission electron microscope) photograph in the range of 5 nm to 200 nm. Furthermore, the coefficient of variation (standard deviation of particle size / average particle size) of particles having magnetic crystals of epsilon-type iron oxide in the magnetic layer, produced by the method described below, is in the range of less than 80%, and they are a group of relatively fine particles with a uniform particle size.

[0032] In a preferred electromagnetic wave absorbing layer, magnetic particles of such epsilon iron oxide (i.e., ε-Fe 2 O 3Crystalline and / or M-substituted ε-Fe 2 O 3 The powder of ε-Fe (particles with crystals in the magnetic phase) is used as the magnetic material in the electromagnetic wave absorbing layer. The "magnetic phase" here refers to the part of the powder that is responsible for its magnetism. 2 O 3 Crystalline and / or M-substituted ε-Fe 2 O 3 "Having crystals in the magnetic phase" means that the magnetic phase is ε-Fe 2 O 3 Crystalline and / or M-substituted ε-Fe 2 O 3 This means that the magnetic phase is made up of crystals, and includes the case where the magnetic phase contains impurity magnetic crystals that are unavoidable during manufacturing.

[0033] The magnetic crystal of epsilon-type iron oxide is ε-Fe 2 O 3 Impurity crystals of iron oxides that have different space groups and oxidation states from the crystals (specifically, α-Fe 2 O 3 , γ-Fe 2 O 3 , FeO, and Fe 3 O 4 , and in these crystals, a part of the Fe may be substituted with other elements). When the magnetic crystals of epsilon-type iron oxide contain impurity crystals, ε-Fe 2 O 3 and / or M-substituted ε-Fe 2 O 3 It is preferable that the magnetic crystal of ε-Fe is the main phase. 2 O 3 and / or M-substituted ε-Fe 2 O 3 The proportion of the magnetic crystals is preferably 50 mol % or more in terms of molar ratio as a compound.

[0034] The abundance ratio of the crystals can be determined by analysis using the Rietveld method based on the X-ray diffraction pattern. The silica (SiO 2 ) and other non-magnetic compounds may adhere to the surface.

[0035] (M-substituted ε-Fe 2 O3 ) The crystal and space group are ε-Fe 2 O 3 and ε-Fe 2 O 3 As long as the condition that a part of the Fe site of the crystal is substituted with an element M other than Fe is satisfied, M-substituted ε-Fe 2 O 3 The type of element M in the formula is not particularly limited. 2 O 3 may contain a plurality of elements M other than Fe.

[0036] Suitable examples of the element M include In, Ga, Al, Sc, Cr, Sm, Yb, Ce, Ru, Rh, Ti, Co, Ni, Mn, Zn, Zr, and Y. Among these, In, Ga, Al, Ti, Co, and Rh are preferred. When M is Al, ε-M x Fe 2-x O 3 In the composition represented by the formula (I), x is preferably, for example, in the range of 0 or more and less than 0.8. When M is Ga, x is preferably, for example, in the range of 0 or more and less than 0.8. When M is In, x is preferably, for example, in the range of 0 or more and less than 0.3. When M is Rh, x is preferably, for example, in the range of 0 or more and less than 0.3. When M is Ti and Co, x is preferably, for example, in the range of 0 or more and less than 1.

[0037] The frequency at which the amount of electromagnetic wave absorption is maximum is M-substituted ε-Fe 2 O 3 The amount of substitution of element M can be adjusted by adjusting at least one of the type and the amount of substitution of element M in the above.

[0038] Such M-substituted ε-Fe 2 O 3 The magnetic crystals can be synthesized, for example, by a process combining a reverse micelle method and a sol-gel method, and a firing process, as described later. Furthermore, as disclosed in Japanese Patent Laid-Open Publication No. 2008-174405, M-substituted ε-Fe can be synthesized by a process combining a direct synthesis method and a sol-gel method, and a firing process. 2 O 3 Magnetic crystals can be synthesized.

[0039] Specifically, Jian Jin, Shin-ichi Ohkoshi and Kazuki Hashimoto, ADVANCED MATERIALS 2004, 16, No. 1, January 5, p. 48-51, Shin-ichi Ohkoshi, Shunsuke Sakurai, Jian Jin, Kazuhito Hashimoto, JOURNAL OF APPLIED PHYSICS, 97, 10K312 (2005), Shunsuke Sakurai, Jian Jin, Kazuhito Hashimoto and Shin-ichi Ohkoshi, JOURNAL OF THE PHYSICAL SOCIETY OF JAPAN, Vol. 74, No. 7, July, 2005, p. As described in "1946-1949," Asuka Namai, Shunsuke Sakurai, Makoto Nakajima, Tohru Suemoto, Kazuki Matsumoto, Masahiro Goto, Shinya Sasaki, and Shin-ichi Ohkoshi, Journal of the American Chemical Society, Vol. 131, pp. 1170-1173, 2009, etc., M-substituted ε-Fe was synthesized by a process combining a reverse micelle method and a sol-gel method and a baking process. 2 O 3 Magnetic crystals can be obtained.

[0040] In the reverse micelle method, two types of micellar solutions containing surfactants, namely micellar solution I (raw micelles) and micellar solution II (neutralizer micelles), are mixed together to allow the precipitation reaction of iron hydroxide to proceed within the micelles. Next, a silica coating is applied to the surface of the iron hydroxide fine particles produced within the micelles by the sol-gel method. After being separated from the liquid, the iron hydroxide fine particles with the silica coating layer are subjected to heat treatment in an air atmosphere at a predetermined temperature (within the range of 700 to 1300°C). This heat treatment results in the formation of ε-Fe 2 O 3 Fine particles of crystals are obtained.

[0041] More specifically, for example, M-substituted ε-Fe can be prepared as follows: 2O 3 Magnetic crystals are produced.

[0042] First, iron (III) nitrate as an iron source, M nitrate salts as M element sources for substituting part of the iron (aluminum (III) nitrate nonahydrate in the case of Al, gallium (III) nitrate hydrate in the case of Ga, indium (III) nitrate trihydrate in the case of In, titanium (IV) sulfate hydrate and cobalt (II) nitrate hexahydrate in the cases of Ti and Co), and a surfactant (e.g., cetyltrimethylammonium bromide) are dissolved in the aqueous phase of micellar solution I, which has n-octane as the oil phase.

[0043] An appropriate amount of alkaline earth metal (Ba, Sr, Ca, etc.) nitrate can be dissolved in the aqueous phase of micellar solution I. This nitrate acts as a shape control agent. When alkaline earth metals are present in the solution, rod-shaped M-substituted ε-Fe ions are eventually formed. 2 O 3 In the absence of a shape control agent, particles of magnetic crystals are obtained. 2 O 3 Magnetic crystalline particles are obtained.

[0044] The alkaline earth metal added as a shape control agent is used to form M-substituted ε-Fe. 2 O 3 It may remain in the surface layer of the magnetic crystal. M-substituted ε-Fe 2 O 3 The mass of alkaline earth metal in magnetic crystal is M-substituted ε-Fe 2 O 3 The amount of the substitution element M is preferably 20% by mass or less, and more preferably 10% by mass or less, of the total mass of the substitution element M and the mass of Fe in the magnetic crystal.

[0045] Aqueous ammonia solution is used as the aqueous phase of micellar solution II, which uses n-octane as the oil phase.

[0046] After mixing micellar solutions I and II, the sol-gel method is applied. Specifically, silane (e.g., tetraethylorthosilane) is added dropwise to the mixed micellar solution while stirring is continued, and a reaction to form iron hydroxide or iron hydroxide containing element M is allowed to proceed within the micelles. As a result, the particle surfaces of the fine iron hydroxide precipitate formed within the micelles are coated with silica formed by hydrolysis of the silane.

[0047] Next, the silica-coated M element-containing iron hydroxide particles are separated from the liquid, washed, and dried to obtain a particle powder, which is then charged into a furnace and heat-treated (fired) in air at a temperature range of 700°C to 1300°C, preferably 900°C to 1200°C, and more preferably 950°C to 1150°C. This heat treatment causes an oxidation reaction to proceed within the silica coating, converting the fine particles of M element-containing iron hydroxide into fine M-substituted ε-Fe. 2 O 3 particles.

[0048] During this oxidation reaction, the presence of the silica coating 2 O 3 and γ-Fe 2 O 3 ε-Fe crystals, not 2 O 3 M-substituted ε-Fe with the same space group as 2 O 3 It contributes to the formation of crystals and also prevents sintering of particles. Furthermore, when an appropriate amount of alkaline earth metal is present, the particles tend to grow into rod-like shapes.

[0049] As described above, as disclosed in Japanese Patent Laid-Open No. 2008-174405, M-substituted ε-Fe can be obtained by a process combining a direct synthesis method and a sol-gel method and a firing process. 2 O 3 Magnetic crystals can be synthesized more economically.

[0050] Briefly, a precursor consisting of iron hydroxide (which may be partially substituted with another element) is formed by first adding a neutralizing agent such as aqueous ammonia to an aqueous solvent in which a trivalent iron salt and a salt of a substitution element M (Ga, Al, etc.) are dissolved, while stirring.

[0051] Then, a sol-gel method is applied to form a silica coating layer on the surface of the precursor particles. After separating the silica-coated particles from the liquid, they are heat-treated (fired) at a predetermined temperature to form M-substituted ε-Fe 2 O 3 Fine particles of magnetic crystals are obtained.

[0052] M-substituted ε-Fe as described above 2 O 3 In the synthesis of ε-Fe 2 O 3 Iron oxide crystals (impurity crystals) with different space groups and oxidation states from the crystals may be generated. 2 O 3 The most common polymorphism that has a different crystal structure while having the same composition is α-Fe. 2 O 3 and γ-Fe 2 O 3 Other iron oxides include FeO and Fe 3 O 4 The inclusion of such impurity crystals is due to the M-substituted ε-Fe 2 O 3 Although this is not desirable in terms of maximizing the properties of the crystal, it is acceptable within the range that does not impair the effects of the present invention.

[0053] Also, M-substituted ε-Fe 2 O 3 Coercive force H of magnetic crystals c changes depending on the amount of substitution by the substitution element M. That is, M-substituted ε-Fe 2 O 3 By adjusting the amount of substitution by the substitution element M in the magnetic crystal, M-substituted ε-Fe 2 O 3 Coercive force H of magnetic crystals c Specifically, when Al, Ga, or the like is used as the substitution element M, the more the substitution amount increases, the more the M-substituted ε-Fe 2 O 3 Coercive force H of magnetic crystals c On the other hand, when Rh or the like is used as the substitution element M, the more the substitution amount increases, the more the M-substituted ε-Fe 2 O3 Coercive force H of magnetic crystals c The M-substituted ε-Fe increases depending on the amount of substitution by the substitution element M. 2 O 3 Coercive force H of magnetic crystals c In terms of ease of adjusting the value of the substitution element M, Ga, Al, In, Ti, Co and Rh are preferred.

[0054] And this coercive force H c As the M element substitution rate decreases, the peak frequency at which the electromagnetic wave absorption of epsilon iron oxide is maximized also shifts to the lower or higher frequency side. In other words, the peak frequency of the electromagnetic wave absorption can be controlled by the amount of M element substitution.

[0055] In the case of commonly used electromagnetic wave absorbers, if the incident angle or frequency of the electromagnetic wave deviates from the designed values, the absorption amount becomes almost zero. In contrast, when epsilon-type iron oxide is used, electromagnetic wave absorption is exhibited over a wide frequency range and electromagnetic wave incident angle even if the values ​​deviate slightly. Therefore, it is possible to provide an electromagnetic wave absorbing layer that can absorb electromagnetic waves over a wide frequency band.

[0056] The particle size of epsilon-type iron oxide can be controlled, for example, by adjusting the heat treatment (calcination) temperature in the above-mentioned process. According to the aforementioned method combining the reverse micelle method and the sol-gel method, or the method combining the direct synthesis method and the sol-gel method disclosed in JP 2008-174405 A, it is possible to synthesize epsilon-type iron oxide particles having an average particle size measured from a TEM (transmission electron microscope) photograph in the range of 5 nm to 200 nm. The average particle size of epsilon-type iron oxide is preferably 10 nm or more, and more preferably 20 nm or more. When calculating the average particle size, which is the number-average particle size, if the epsilon-type iron oxide particles are rod-shaped, the diameter in the major axis direction of the particles observed in the TEM image is used as the diameter of the particles. The number of particles to be measured when calculating the average particle size is not particularly limited as long as it is a sufficiently large number for calculating the average value, but 300 or more is preferred.

[0057] In addition, the silica coating on the surface of iron hydroxide particles by the sol-gel method is 2 O 3 It may be present on the surface of the magnetic crystal. The presence of a non-magnetic compound such as silica on the surface of the crystal is preferable in terms of improving the handleability, durability, weather resistance, etc. of the magnetic crystal. Suitable examples of non-magnetic compounds include silica, as well as heat-resistant compounds such as alumina and zirconia.

[0058] However, if the amount of the non-magnetic compound attached is too large, the particles may aggregate violently, which is not preferable. 2 O 3 The mass of Si in the magnetic crystal is M-substituted ε-Fe 2 O 3 It is preferable that the amount of M substituted ε-Fe is 100% by mass or less relative to the total mass of the substitution element M and the mass of Fe in the magnetic crystal. 2 O 3 A part or most of the silica attached to the magnetic crystals can be removed by immersing them in an alkaline solution, and the amount of silica attached can be adjusted to any desired amount by this method.

[0059] The relative permeability of the electromagnetic wave absorbing layer is not particularly limited, but is preferably 1.0 or more and 1.5 or less. The method for adjusting the relative permeability of the electromagnetic wave absorbing layer is not particularly limited. Examples of methods for adjusting the relative permeability of the electromagnetic wave absorbing layer include a method for adjusting the amount of substitution by the substitution element M in the epsilon-type iron oxide, and a method for adjusting the content of epsilon-type iron oxide and other magnetic materials other than epsilon-type iron oxide in the electromagnetic wave absorbing layer.

[0060] The content of the magnetic material in the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The content of the magnetic material is preferably 5% by mass or more, more preferably 5% by mass or more and 90% by mass or less, particularly preferably 5% by mass or more and 70% by mass or less, and most preferably 5% by mass or more and 60% by mass or less, relative to the mass of the electromagnetic wave absorbing layer.

[0061] [Binder Resin] The electromagnetic wave absorbing layer contains a binder resin. The binder resin includes an amorphous resin having a glass transition point of 80°C or higher and / or a crystalline resin having a melting point of 150°C or higher. In this specification, a crystalline resin refers to a resin having crystalline portions in which molecular chains are regularly oriented and having a glass transition point and a melting point in differential scanning calorimetry (DSC). In addition, an amorphous resin refers to a resin having a structure in which molecular chains are randomly entangled and having only a glass transition point but no melting point in DSC.

[0062] The glass transition point of the amorphous resin is preferably 101° C. or higher. There is no particular upper limit to the glass transition point of the amorphous resin as long as the effects of the present invention are not impaired, and examples include 300° C. or lower, 200° C. or lower, and 150° C. or lower. The glass transition point of the amorphous resin can be determined based on the change in viscoelasticity measured using a dynamic mechanical analysis (DMA) device at a frequency of 1 Hz, by increasing the temperature from 25° C. to 300° C. at a heating rate of 5° C. / min.

[0063] The upper limit of the melting point of the crystalline resin is not particularly limited as long as the effects of the present invention are not impaired, and examples thereof include 500° C. or less, 400° C. or less, 300° C. or less, and 200° C. or less. The melting point of the crystalline resin is, for example, the temperature corresponding to the maximum value on the heat of fusion curve when the temperature is increased at a rate of 10° C. / min using a differential scanning calorimetry (DSC) device.

[0064] The weight average molecular weight (Mw) of the amorphous resin or crystalline resin is preferably from 5,000 to 1,000,000, and more preferably from 10,000 to 800,000. The weight average molecular weight (Mw) is the weight average molecular weight measured by GPC and converted into polystyrene.

[0065] Suitable examples of amorphous resins and crystalline resins include polyurethane resins, polyester-urethane resins, urethane polyamide resins, polycarbonate resins, polyester resins, FR-AS resins, FR-ABS resins, AS resins, ABS resins, polyphenylene oxide resins, polyphenylene sulfide resins, polysulfone resins, polyethersulfone resins, polyetheretherketone resins, fluorine-based resins, polyimide resins, polyamideimide resins, polyamide bismaleimide resins, polyetherimide resins, polybenzoxazole resins, polybenzothiazole resins, polybenzimidazole resins, BT resins, polymethylpentene, ultra-high molecular weight polyethylene, FR-polypropylene, cellulose resins, (meth)acrylic resins, and polystyrene. Of these, polyester-urethane resins and fluorine-based resins are more preferred.

[0066] The polyester-urethane resin is a copolymer containing an ester bond (-CO-O-) and a urethane bond (-NH-CO-O-). Suitable examples of the polyester-urethane resin include an aromatic ester-urethane copolymer and an aliphatic ester-urethane copolymer. Of these, an aromatic ester-urethane copolymer is more preferred.

[0067] The aromatic ester-urethane copolymer is a copolymer containing an ester bond (-CO-O-) and a urethane bond (-NH-CO-O-), and containing an aromatic group in the main chain skeleton. The aromatic group in the main chain skeleton may be an aromatic hydrocarbon group or a heterocyclic aromatic group, with an aromatic hydrocarbon group being preferred. The aromatic ester-urethane copolymer may be a random copolymer in which ester bonds and urethane bonds are randomly introduced into the molecular chain, or may be a block copolymer consisting of one or more ester blocks and one or more urethane blocks.

[0068] The method for producing the aromatic ester-urethane copolymer is not particularly limited. The aromatic ester-urethane copolymer can typically be produced by polymerizing one or more monomers selected from the group consisting of a diol component (a1), a dicarboxylic acid (a2), a hydroxycarboxylic acid component (a3), and a diisocyanate component (a4) in one step or multiple steps.

[0069] The dicarboxylic acid component (a2) and the hydroxycarboxylic acid component (a3) ​​may be used as ester derivatives such as methyl esters and ethyl esters, carboxylic acid halides such as carboxylic acid chlorides, or urethane-forming derivatives.

[0070] The monomer used in the production of the aromatic ester-urethane copolymer is preferably a compound in which two functional groups selected from the group consisting of a hydroxyl group, a carboxyl group, and an isocyanate group are bonded to an unbranched divalent hydrocarbon group. Examples of the unbranched divalent hydrocarbon group include an alkylene group, an alkenylene group, an alkynylene group, an arylene group, or a combination of these groups. The alkylene group, alkenylene group, and alkynylene group preferably have a linear structure.

[0071] When the unbranched divalent hydrocarbon group is an alkylene group, an alkenylene group, or an alkynylene group, the number of carbon atoms in these groups is preferably 1 or more and 8 or less, more preferably 2 or more and 6 or less, and even more preferably 2 or more and 4 or less.

[0072] When the unbranched divalent hydrocarbon group is an arylene group, the arylene group is preferably a phenylene group or a naphthylene group, more preferably a phenylene group, and even more preferably a p-phenylene group.

[0073] Of the divalent hydrocarbon groups having an unbranched structure described above, alkylene groups, arylene groups, and combinations of alkylene groups and arylene groups are preferred.

[0074] Specific preferred examples of the diol component (a1) include ethylene glycol, 1,3-propanediol, 1,4-butanediol, neopentyl glycol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, and 1,5-pentanediol. Specific preferred examples of the dicarboxylic acid (a2) include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, succinic acid, glutaric acid, adipic acid, oxalic acid, and malonic acid. Specific preferred examples of the hydroxycarboxylic acid component (a3) ​​include 4-hydroxybenzoic acid, 3-hydroxybenzoic acid, 6-hydroxynaphthalene-2-carboxylic acid, glycolic acid, lactic acid, and γ-hydroxybutyric acid. Specific preferred examples of the diisocyanate component (a4) include ethylene diisocyanate, trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, m-xylylene diisocyanate, p-phenylene diisocyanate, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and 1,5-naphthalene diisocyanate.

[0075] Commercially available aromatic ester-urethane copolymers include the Vylon series (product name) (manufactured by Toyobo Co., Ltd.) etc. More specifically, Vylon UR-1400, Vylon UR-1410, Vylon UR-1700, Vylon UR-2300, Vylon UR-3200, Vylon UR-3210, Vylon UR-3500, Vylon UR-6100, Vylon UR-8300, and Vylon UR-8700 etc. can be preferably used.

[0076] Suitable examples of fluorine-based resins include tetrafluoroethylene / perfluoroalkyl ether copolymer (PFA), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), polyvinyl fluoride (PVF), polychlorotrifluoroethylene (PCTFE), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), ethylene / chlorotrifluoroethylene copolymer (ECTFE), vinylidene fluoride / chlorotrifluoroethylene copolymer, ethylene / tetrafluoroethylene copolymer, chlorotrifluoroethylene / tetrafluoroethylene copolymer, vinylidene fluoride / tetrafluoroethylene copolymer, Examples of the vinyl fluoride include vinylene / hexafluoropropylene copolymer, ethylene / tetrafluoroethylene / hexafluoropropylene copolymer, vinylidene fluoride / tetrafluoroethylene copolymer, vinylidene fluoride / hexafluoropropylene copolymer, vinylidene fluoride / pentafluoropropylene copolymer, tetrafluoroethylene / hexafluoropropylene / vinylidene fluoride copolymer (THV), vinylidene fluoride / pentafluoropropylene / tetrafluoroethylene copolymer, vinylidene fluoride / perfluoroalkyl vinyl ether / tetrafluoroethylene copolymer, perfluoroalkoxy / tetrafluoromethylene copolymer, etc. Among these, polyvinylidene fluoride is more preferred.

[0077] The binder resin may be, for example, an elastic material such as an elastomer or rubber. The binder resin may also be a curable resin. When the binder resin is a curable resin, the curable resin may be a photocurable resin or a thermosetting resin.

[0078] Suitable examples of the binder resin that is an elastic material include olefin-based elastomers, styrene-based elastomers, polyamide-based elastomers, polyester-based elastomers, and polyurethane-based elastomers.

[0079] Suitable examples of the binder resin when it is a thermosetting resin include phenol resin, melamine resin, epoxy resin, alkyd resin, etc. As the photocurable resin, resins obtained by photocuring various vinyl monomers and monomers having unsaturated bonds such as various (meth)acrylic acid esters can be used.

[0080] In the binder resin, the mass ratio of the amorphous resin having a glass transition point of 80°C or higher and the crystalline resin having a melting point of 150°C or higher is preferably 70% by mass or higher, more preferably 80% by mass or higher, even more preferably 90% by mass or higher, still more preferably 95% by mass or higher, and particularly preferably 100% by mass.

[0081] The content of the binder resin in the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The content of the binder resin is preferably 5% by mass or more and 30% by mass or less, more preferably 5% by mass or more and 25% by mass or less, based on the mass of the electromagnetic wave absorbing layer.

[0082] [Non-Dielectric Material] The electromagnetic wave absorbing layer contains a non-dielectric material other than a magnetic material. The non-dielectric material is not particularly limited as long as it is a material other than materials recognized by those skilled in the art as ferroelectric or ferromagnetic.

[0083] Examples of non-dielectric materials include inorganic fillers. Suitable examples of such inorganic fillers include barium sulfate, aluminum oxide (alumina), aluminum nitride, boron nitride, silicon carbide, silicon dioxide (silica), calcium carbonate, and talc. Among these, barium sulfate, aluminum oxide, and silicon dioxide are more preferred, and barium sulfate is particularly preferred.

[0084] The electromagnetic wave absorbing layer typically contains a powder of a non-dielectric material. The particle size of the non-dielectric material powder is not particularly limited as long as it does not impair the object of the present invention. The average particle size of the non-dielectric material powder is preferably 1 nm or more and 20 μm or less, and more preferably 5 nm or more and 10 μm or less. Here, the average particle size of the non-dielectric material powder is the number average size of primary particles of the non-dielectric material powder observed with an electron microscope.

[0085] The content of the non-dielectric material in the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention, and is preferably 10% by mass or more and 80% by mass or less, more preferably 20% by mass or more and 75% by mass or less, relative to the mass of the electromagnetic wave absorbing layer.

[0086] [Dielectric (Ferroelectric)] The electromagnetic wave absorbing layer may contain a dielectric (ferroelectric) for the purpose of adjusting the relative dielectric constant of the electromagnetic wave absorbing layer. The relative dielectric constant of the electromagnetic wave absorbing layer can be adjusted by adjusting the content of the dielectric in the electromagnetic wave absorbing layer. There are no particular restrictions on the relative dielectric constant of the electromagnetic wave absorbing layer, but it is preferably 6.5 or more and 65 or less, more preferably 10 or more and 50 or less, and even more preferably 15 or more and 30 or less.

[0087] Suitable examples of the dielectric include barium titanate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, zirconium titanate, zinc titanate, and titanium dioxide. The electromagnetic wave absorbing layer may contain a combination of powders of multiple types of dielectrics.

[0088] The particle size of the dielectric powder used to adjust the relative dielectric constant of the electromagnetic wave absorbing layer is not particularly limited as long as it does not impair the object of the present invention. The average particle size of the dielectric powder is preferably 1 nm or more and 100 nm or less, and more preferably 5 nm or more and 50 nm or less. Here, the average particle size of the dielectric powder is the number average size of the primary particles of the dielectric powder observed with an electron microscope.

[0089] When adjusting the relative permittivity of the electromagnetic wave absorbing layer using a dielectric powder, the amount of the dielectric powder used is not particularly limited as long as the relative permittivity of the electromagnetic wave absorbing layer is within a predetermined range. The amount of the dielectric powder used is preferably 0% by mass or more and 20% by mass or less, and more preferably 5% by mass or more and 10% by mass or less, relative to the mass of the electromagnetic wave absorbing layer.

[0090] [Carbon nanotubes] The electromagnetic wave absorbing layer may contain carbon nanotubes. By incorporating carbon nanotubes into the electromagnetic wave absorbing layer, the relative dielectric constant of the electromagnetic wave absorbing layer can be adjusted. The carbon nanotubes may be used in combination with the above-mentioned dielectric powder.

[0091] The amount of carbon nanotubes blended into the electromagnetic wave absorbing layer is not particularly limited as long as the relative dielectric constant of the electromagnetic wave absorbing layer is within the above-mentioned range. However, since carbon nanotubes are also a conductive material, if the amount of carbon nanotubes used is excessive, the electromagnetic wave absorption properties provided by the electromagnetic wave absorbing layer may be impaired. The amount of carbon nanotubes used is preferably 0% by mass or more and 20% by mass or less, and more preferably 1% by mass or more and 10% by mass or less, relative to the mass of the electromagnetic wave absorbing layer.

[0092] [Other Components] The electromagnetic wave absorbing layer may contain various additives other than the above-mentioned components, as long as they do not impair the object of the present invention. Examples of additives that the electromagnetic wave absorbing layer may contain include dispersants, colorants, antioxidants, ultraviolet absorbers, flame retardants, flame retardant assistants, plasticizers, surfactants, etc. These additives are used in amounts that are conventionally used, as long as they do not impair the object of the present invention.

[0093] By forming a film from the components described above, for example, by a method using a paste for forming an electromagnetic wave absorber, which will be described later, an electromagnetic wave absorbing layer can be obtained that can be used as an electromagnetic wave absorber whose electromagnetic wave absorption properties are not easily deteriorated even when exposed to high temperatures for a long period of time.

[0094] <Substrate Layer> The electromagnetic wave absorbing layer described above may be laminated on a substrate layer. The substrate layer may be a layer containing any substrate as long as it does not impair the effects of the present invention, and examples thereof include layers containing resins. Examples of the resin include polyethylene terephthalate (PET), polyethylene naphthalate (PEN), acrylic (PMMA), polycarbonate (PC), cycloolefin polymer (COP), polyethersulfone, polyimide, polyamideimide, etc. Among these, PET and PEN are preferred because of their excellent heat resistance and good balance between dimensional stability and cost.

[0095] The shape of the substrate layer may have a curved surface or may be composed of only a flat surface, and a flat plate shape is preferred. The thickness of the substrate layer is preferably 800 μm or less, more preferably 500 μm or less, even more preferably 300 μm or less, and particularly preferably 150 μm or less, from the viewpoint of making the film thinner and smaller without impairing the effects of the present invention. The lower limit of the thickness of the substrate layer is not particularly limited as long as the effects of the present invention are not impaired, and examples thereof include 1 μm or more, 10 μm or more, and 50 μm or more.

[0096] <Metal Layer> When the electromagnetic wave absorber includes a substrate layer, a metal layer may be provided on the surface of the electromagnetic wave absorber opposite to the surface on which the substrate layer is provided. When a metal layer is provided, electromagnetic waves reflected by the metal layer can be attenuated. Examples of metals constituting the metal layer include aluminum, titanium, SUS, copper, brass, silver, gold, and platinum. The thickness of the metal layer is not particularly limited, and from the viewpoint of making the electromagnetic wave absorber thin, it is preferably 600 μm or less, more preferably 400 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. There is no particular limit to the lower limit of the thickness of the metal layer as long as it does not impair the effects of the present invention, and examples thereof include 0.1 μm or more, 1 μm or more, 5 μm or more, and 10 μm or more.

[0097] By combining the electromagnetic wave absorbing layer containing the specified components described above with a substrate layer, or a substrate layer and a metal layer as needed, an electromagnetic wave absorber whose electromagnetic wave absorption properties are resistant to deterioration even when exposed to high temperatures for a long period of time can be obtained.

[0098] The electromagnetic wave absorber may have an adhesive layer or pressure-sensitive adhesive layer provided at any position. Examples of the adhesive layer or pressure-sensitive adhesive layer include an acrylic pressure-sensitive adhesive layer, a rubber pressure-sensitive adhesive layer, a silicone pressure-sensitive adhesive layer, and a urethane pressure-sensitive adhesive layer.

[0099] The electromagnetic wave absorber described above can be preferably used as an electromagnetic wave absorbing film for use in various elements (including in-vehicle elements, high-frequency antenna elements, etc.) in various information and communication systems such as mobile phones, wireless LANs, ETC systems, intelligent road transport systems, automobile driving assistance road systems, and satellite broadcasting.

[0100] <<Electromagnetic Wave Absorber Forming Paste>> A preferred method for forming an electromagnetic wave absorber is to use an electromagnetic wave absorber forming paste, since it allows for highly efficient formation of an electromagnetic wave absorbing layer without any particular thickness restrictions and allows for the electromagnetic wave absorbing layer to be formed directly on a substrate layer. The electromagnetic wave absorber forming paste contains the magnetic material, a binder resin, and a non-dielectric material. The electromagnetic wave absorber forming paste may contain the aforementioned substances added to adjust the relative permittivity, relative magnetic permeability, etc., as well as other components. Note that when the binder resin contains a curable resin, the electromagnetic wave absorber forming paste contains a compound that is a precursor of the curable resin. In this case, the electromagnetic wave absorber forming paste may contain a curing agent, a curing accelerator, a polymerization initiator, etc., as necessary.

[0101] Furthermore, when the paste for forming an electromagnetic wave absorber contains a photopolymerizable or thermally polymerizable compound, the coated film may be exposed to light or heated as necessary to form an electromagnetic wave absorbing layer.

[0102] The paste for forming an electromagnetic wave absorber preferably further contains a dispersion medium. As the dispersion medium, water, an organic solvent, or an aqueous solution of an organic solvent can be used. As the dispersion medium, an organic solvent is preferred because it is easy to dissolve organic components and has a low latent heat of vaporization and is easily removed by drying.

[0103] Suitable examples of organic solvents used as dispersion media include nitrogen-containing polar solvents such as N,N,N',N'-tetramethylurea (TMU), N-methyl-2-pyrrolidone (NMP), N,N-dimethylacetamide (DMAc), N,N-dimethylisobutyramide, N,N-diethylacetamide, N,N-dimethylformamide (DMF), N,N-diethylformamide, N-methylcaprolactam, 1,3-dimethyl-2-imidazolidinone (DMI), and pyridine; ketones such as diethyl ketone, methyl butyl ketone, dipropyl ketone, and cyclohexanone; alcohols such as n-pentanol, 4-methyl-2-pentanol, cyclohexanol, and diacetone alcohol; ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monomethyl ether. Ether alcohols such as ethylene glycol dimethyl ether and diethylene glycol diethyl ether; saturated aliphatic monocarboxylic acid alkyl esters such as n-butyl acetate and amyl acetate; lactate esters such as ethyl lactate and n-butyl lactate; ketones such as acetone, methyl ethyl ketone, cyclohexanone, acetophenone, and benzophenone; methyl cellosolve acetate, ethyl cellosolve acetate, propylene glycol monomethyl ether acetate, and propylene glycol Examples of such ether esters include monoethyl ether acetate, ethyl 3-ethoxypropionate, 2-methoxybutyl acetate, 3-methoxybutyl acetate, 4-methoxybutyl acetate, 2-methyl-3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, 3-ethyl-3-methoxybutyl acetate, 2-ethoxybutyl acetate, 4-ethoxybutyl acetate, 4-propoxybutyl acetate, and 2-methoxypentyl acetate. These may be used alone or in combination of two or more.

[0104] The solid content concentration of the paste for forming an electromagnetic wave absorber is adjusted as appropriate depending on the method for applying the paste for forming an electromagnetic wave absorber, the thickness of the electromagnetic wave absorbing layer, etc. Typically, the solid content concentration of the paste for forming an electromagnetic wave absorber is preferably 3% by mass or more and 60% by mass or less, and more preferably 10% by mass or more and 50% by mass or less. The solid content concentration of the paste is a value calculated as the mass of the solid content, which is the sum of the mass of the components not dissolved in the dispersion medium and the mass of the components dissolved in the dispersion medium.

[0105] (Dispersant) The paste for forming an electromagnetic wave absorber may contain a dispersant for the purpose of dispersing well the magnetic material or the substance used to adjust the relative permittivity and relative permeability of the electromagnetic wave absorbing layer in the electromagnetic wave absorbing layer. The dispersant may be mixed uniformly with the magnetic material and binder resin. The dispersant may be blended into the binder resin. Furthermore, the magnetic material or the substance added to adjust the relative permittivity and relative permeability, which has been pre-treated with a dispersant, may be blended into the material constituting the electromagnetic wave absorbing layer.

[0106] The type of dispersant is not particularly limited as long as it does not impair the object of the present invention, and can be selected from various dispersants that have been conventionally used for dispersing various inorganic and organic fine particles.

[0107] Suitable examples of the dispersant include a silane coupling agent (for example, phenyltrimethoxysilane), a titanate coupling agent, a zirconate coupling agent, and an aluminate coupling agent.

[0108] The content of the dispersant is not particularly limited as long as it does not impair the object of the present invention. The content of the dispersant is preferably 0.1% by mass or more and 30% by mass or less, more preferably 1% by mass or more and 15% by mass or less, and particularly preferably 1% by mass or more and 10% by mass or less, relative to the solid content mass of the paste for forming an electromagnetic wave absorber.

[0109] <<Method for Manufacturing Electromagnetic Wave Absorber>> The method for manufacturing the aforementioned electromagnetic wave absorber is not particularly limited as long as it can produce an electromagnetic wave absorber of a predetermined structure. A preferred method includes an electromagnetic wave absorbing layer forming step in which the aforementioned paste containing a magnetic material, a binder resin, and a non-dielectric material is applied to a substrate layer to form a coating film, and then the coating film is dried to form an electromagnetic wave absorbing layer. As described above, the paste may contain substances, dispersion mediums, dispersants, and other components added to adjust the relative permittivity, relative magnetic permeability, etc.

[0110] The method for applying the paste for forming an electromagnetic wave absorber onto the substrate layer is not particularly limited as long as it can form an electromagnetic wave absorber of the desired thickness. Examples of application methods include spray coating, dip coating, roll coating, curtain coating, spin coating, screen printing, doctor blade coating, slot die coating, bank coating (knife coating), and applicator coating. The coating film formed by the above method is dried to remove the dispersion medium, forming an electromagnetic wave absorbing layer on the substrate layer, thereby obtaining an electromagnetic wave absorber. The thickness of the coating film is appropriately adjusted so that the thickness of the electromagnetic wave absorbing layer obtained after drying is the desired thickness. The drying method is not particularly limited, and examples include: (1) drying on a hot plate at a temperature of 80°C to 180°C, preferably 90°C to 160°C, for 1 minute to 30 minutes; (2) leaving the paste at room temperature for several hours to several days; and (3) removing the solvent by placing the paste in a hot air heater or infrared heater for several tens of minutes to several hours.

[0111] The method for manufacturing an electromagnetic wave absorber may include a cutting step of cutting the electromagnetic wave absorbing layer or a laminate comprising a base layer and an electromagnetic wave absorbing layer obtained in the electromagnetic wave absorbing layer forming step to obtain electromagnetic wave absorbers of a predetermined size. As described above, the electromagnetic wave absorbing layer contains a magnetic material, a binder resin having predetermined temperature characteristics, and a non-dielectric material, and therefore the electromagnetic wave absorbing characteristics are unlikely to deteriorate even when exposed to high temperatures for a long period of time.

[0112] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.

[0113] Example 1 (Preparation of Paste for Forming Electromagnetic Wave Absorber) To 100.0 parts by mass of DMI (1,3-dimethyl-2-imidazolidinone), 34.0 parts by mass of the following epsilon-type iron oxide, 4.0 parts by mass of the following carbon nanotubes (CNT), 12.0 parts by mass of binder resin 1, 50.0 parts by mass of granular alumina powder, and 3.4 parts by mass of the following dispersant were added. Binder resin 1 was added as the following binder resin solution 1. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0114] ε-Al as epsilon-type iron oxide a Ti b Co c Fe 2-(a+b+c) O 3 The formula was used. a, b, and c were each greater than 0 and less than 2, and a + b + c was greater than 0 and less than 2. The average particle size of epsilon-type iron oxide was 20 nm or greater and 30 nm or less. As the CNTs, multi-walled carbon nanotubes (product name VGCF-H; manufactured by Showa Denko K.K.) with a major axis of 150 nm were used. The average particle size of the alumina powder was 1 μm. Phenyltrimethoxysilane was used as the dispersant. As the binder resin solution 1, a polyester-urethane copolymer (manufactured by Toyobo Co., Ltd., product name UR-1400, glass transition point 83°C, weight average molecular weight 40,000, consisting of 30.0 parts by mass of resin, 35.0 parts by mass of methyl ethyl ketone, and 35.0 parts by mass of toluene) was used.

[0115] (Production of electromagnetic wave absorber) The above-mentioned paste for forming an electromagnetic wave absorber was applied to an aluminum plate (thickness: 2 mm) using an applicator. Thereafter, the applied film was dried under conditions of 90°C for 10 minutes and 130°C for 10 minutes to form an electromagnetic wave absorbing layer with a thickness of 35 µm, and an electromagnetic wave absorber was obtained.

[0116] <Heat Resistance Test> Electromagnetic waves of 40 to 120 GHz were incident on the electromagnetic wave absorber before heat treatment, and the return loss was measured using a terahertz time domain spectrometer (TAS7400 manufactured by Advantest Corporation). The return loss RL(f) at frequency f was calculated by RL(f) = -10 Log(R(f) / 100), where R(f) is the reflectance (%).

[0117] Next, each electromagnetic wave absorber was heat-treated under one of the following conditions: High temperature storage test: treated at 125°C for 2000 hours Heat cycle test: treated for 2000 cycles of 125°C <=> -45°C (1 hour) Pressure cooker test: treated at 121°C, 98% RH for 192 hours

[0118] The return loss of each electromagnetic wave absorber after the heat treatment was measured in the same manner as before the heat treatment. At the frequency at which the return loss was maximum before the heat treatment, the change in the return loss after the heat treatment relative to the return loss before the heat treatment was calculated and evaluated according to the following criteria. The results are shown in Table 2. A: Less than 10% B: 10% or more but less than 20% C: 20% or more

[0119] Example 2 To 100.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of binder resin 2, 50.0 parts by mass of the alumina powder, and 3.4 parts by mass of the dispersant were added. Binder resin 2 was added as the following binder resin solution 2. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0120] As the binder resin solution 2, a polyester-urethane copolymer (manufactured by Toyobo Co., Ltd., product name UR-4800, glass transition point 106°C, weight average molecular weight 25,000, consisting of 30.0 parts by mass of resin, 35.0 parts by mass of methyl ethyl ketone, and 35.0 parts by mass of toluene) was used.

[0121] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 1. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 1. The results are shown in Table 2.

[0122] Example 3 (Preparation of paste for forming electromagnetic wave absorber) 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of binder resin 3, 50.0 parts by mass of granular silica powder, and 3.4 parts by mass of the dispersant were added to 230.0 parts by mass of DMI. Binder resin 3 was added as the following binder resin solution 3. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0123] Polyvinylidene fluoride (manufactured by Kureha Corporation, trade name KF Polymer W#7200, melting point 173°C, weight average molecular weight 630,000, consisting of 10.0 parts by mass of resin and 90.0 parts by mass of DMI) was used as the binder resin solution 3. The average particle diameter of the silica powder was 1 μm.

[0124] (Production of Electromagnetic Wave Absorber) The above-mentioned paste for forming an electromagnetic wave absorber was applied to the side opposite the adhesive layer of a PEN film (thickness 125 μm) laminated with an adhesive layer using an applicator. The coated film was then dried under conditions of 90°C for 10 minutes and 130°C for 10 minutes to form an electromagnetic wave absorbing layer with a thickness of 35 μm, thereby obtaining a film-like electromagnetic wave absorber. Immediately after drying, the obtained film-like electromagnetic wave absorber was cut into a square shape of 5 cm on each side to prepare test pieces for the following evaluations.

[0125] <Heat Resistance Test> A 5 ​​cm square film-shaped electromagnetic wave absorber sample was attached to an aluminum plate. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 1. The results are shown in Table 2.

[0126] Example 4: To 230.0 parts by mass of DMI, 54.5 parts by mass of the epsilon-type iron oxide, 3.5 parts by mass of the CNT, 12.0 parts by mass of the binder resin 3, 30.0 parts by mass of granular barium sulfate powder, and 5.5 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorber. The average particle size of the barium sulfate powder was 30 nm.

[0127] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0128] [Example 5] To 230.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 3, 50.0 parts by mass of the barium sulfate powder, and 3.4 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0129] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0130] [Example 6] 25.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 3, 59.0 parts by mass of the barium sulfate powder, and 2.5 parts by mass of the dispersant were added to 230.0 parts by mass of DMI. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0131] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0132] [Example 7] 20.0 parts by mass of the epsilon-type iron oxide, 5.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 3, 63.0 parts by mass of the barium sulfate powder, and 2.0 parts by mass of the dispersant were added to 230.0 parts by mass of DMI. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0133] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0134] [Example 8] To 230.0 parts by mass of DMI, 9.0 parts by mass of the epsilon-type iron oxide, 9.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 3, 70.0 parts by mass of the barium sulfate powder, and 0.9 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0135] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0136] Comparative Example 1 To 100.0 parts by mass of DMI, 78.0 parts by mass of the epsilon-type iron oxide, 5.0 parts by mass of the CNT, 17.0 parts by mass of binder resin 4, and 7.8 parts by mass of the dispersant were added. Binder resin 4 was added as the following binder resin solution 4. The mixture was stirred with a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0137] As the binder resin solution 4, a polyester-urethane copolymer (manufactured by Toyobo Co., Ltd., trade name UR-3210, glass transition point -3°C, weight average molecular weight 40,000, consisting of 30.0 parts by mass of resin and 70.0 parts by mass of methyl ethyl ketone) was used.

[0138] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0139] Comparative Example 2 To 100.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 4, 50.0 parts by mass of the alumina powder, and 3.4 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0140] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 1. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 1. The results are shown in Table 2.

[0141] Comparative Example 3 To 100.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of binder resin 5, 50.0 parts by mass of the alumina powder, and 3.4 parts by mass of the dispersant were added. Binder resin 5 was added as the following binder resin solution 5. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse each component, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0142] As the binder resin solution 5, a polyester-urethane copolymer (manufactured by Toyobo Co., Ltd., product name UR-1350, glass transition point 46°C, weight average molecular weight 40,000, consisting of 30.0 parts by mass of resin, 45.0 parts by mass of methyl ethyl ketone, and 25.0 parts by mass of toluene) was used.

[0143] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 1. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 1. The results are shown in Table 2.

[0144] Comparative Example 4 To 100.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 4, 50.0 parts by mass of the silica powder, and 3.4 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0145] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0146] Comparative Example 5 To 100.0 parts by mass of DMI, 34.0 parts by mass of the epsilon-type iron oxide, 4.0 parts by mass of the CNT, 12.0 parts by mass of the binder resin 4, 50.0 parts by mass of the barium sulfate powder, and 3.4 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0147] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0148] Comparative Example 6 To 100.0 parts by mass of DMI, 78.0 parts by mass of the epsilon-type iron oxide, 5.0 parts by mass of the CNT, 17.0 parts by mass of the binder resin 1, and 7.8 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0149] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0150] Comparative Example 7 To 230.0 parts by mass of DMI, 78.0 parts by mass of the epsilon-type iron oxide, 5.0 parts by mass of the CNT, 17.0 parts by mass of the binder resin 3, and 7.8 parts by mass of the dispersant were added. The mixture was stirred using a rotation / revolution mixer to uniformly dissolve or disperse the components, thereby obtaining a paste for forming an electromagnetic wave absorber.

[0151] The above paste for forming an electromagnetic wave absorber was used to obtain an electromagnetic wave absorber in the same manner as in Example 3. The obtained electromagnetic wave absorber was subjected to a heat resistance test in the same manner as in Example 3. The results are shown in Table 2.

[0152] Table 1 shows the blending amounts (parts by mass) of the magnetic material, CNT, binder resin, and non-dielectric material in the examples and comparative examples.

[0153]

[0154]

[0155] Tables 1 and 2 show that the electromagnetic wave absorbers of Examples 1 to 8, which contain both a binder resin having predetermined temperature characteristics and a non-dielectric material in an electromagnetic wave absorbing layer containing a magnetic substance, are resistant to deterioration in electromagnetic wave absorbing properties even when exposed to high temperatures for a long period of time. On the other hand, Comparative Examples 1 to 7 show that the electromagnetic wave absorbing properties are significantly reduced when exposed to high temperatures for a long period of time in all cases where the absorbers do not contain both a binder resin having predetermined temperature characteristics and a non-dielectric material, where the absorbers contain only a binder resin having predetermined temperature characteristics, or where the absorbers contain only a non-dielectric material.

Claims

1. An electromagnetic wave absorber having an electromagnetic wave absorbing layer, the electromagnetic wave absorbing layer comprising a magnetic material, a binder resin, and a non-dielectric material, the binder resin comprising an amorphous resin having a glass transition point of 80°C or higher and / or a crystalline resin having a melting point of 150°C or higher, and the non-dielectric material being different from the magnetic material.

2. The electromagnetic wave absorber according to claim 1, wherein said electromagnetic wave absorbing layer comprises carbon nanotubes.

3. The electromagnetic wave absorber according to claim 1, wherein the magnetic material comprises epsilon type iron oxide.

4. The electromagnetic wave absorber according to claim 1, wherein the amorphous resin and / or the crystalline resin comprises at least one selected from the group consisting of polyurethane resin, polyester-urethane resin, urethane polyamide resin, polycarbonate resin, polyester resin, FR-AS resin, FR-ABS resin, AS resin, ABS resin, polyphenylene oxide resin, polyphenylene sulfide resin, polysulfone resin, polyethersulfone resin, polyetheretherketone resin, fluorine-based resin, polyimide resin, polyamideimide resin, polyamide bismaleimide resin, polyetherimide resin, polybenzoxazole resin, polybenzothiazole resin, polybenzimidazole resin, BT resin, polymethylpentene, ultra-high molecular weight polyethylene, FR-polypropylene, cellulose resin, (meth)acrylic resin, and polystyrene.

5. The electromagnetic wave absorber according to claim 1, wherein the non-dielectric material comprises at least one selected from the group consisting of barium sulfate, aluminum oxide, aluminum nitride, boron nitride, silicon carbide, silicon dioxide, calcium carbonate, and talc.

6. The electromagnetic wave absorber according to any one of claims 1 to 5, wherein the electromagnetic wave absorbing layer is laminated on a substrate layer and has a film shape.

7. A paste for forming an electromagnetic wave absorber comprising a magnetic substance, a binder resin, and a non-dielectric material, wherein the binder resin comprises an amorphous resin having a glass transition point of 80°C or higher and / or a crystalline resin having a melting point of 150°C or higher, and the non-dielectric material is different from the magnetic substance.

Citation Information

Patent Citations

  • Electromagnetic wave absorber and its manufacturing method

    JP2001156487A

  • Manufacturing method of wave absorber and wave absorber

    JP2012074668A

  • Method of manufacturing radio wave absorber and radio wave absorber

    JP2012178469A

  • Electromagnetic wave absorber and method of manufacturing the same

    JP2015023036A

  • High frequency antenna element and high frequency antenna module

    JP2017184106A