Resin powder and method for producing same
By spray-drying an aqueous dispersion of thermoplastic resin and crosslinked polyhydroxyalkanoate resin particles, the challenges of handling and aggregation are overcome, resulting in a resin powder with enhanced properties for biodegradable applications.
Patent Information
- Application Number
- PCT/JP2024/011088
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-21
- Publication Date
- 2024-10-03
AI Technical Summary
Current methods for producing small-sized crosslinked resin particles from biodegradable plastics, such as polyhydroxyalkanoate, face challenges in handling due to aggregation and adhesion, making it difficult to separate and process these particles effectively.
The production of crosslinked resin particles is achieved through an aqueous dispersion of thermoplastic resin and polyhydroxyalkanoate resin, which is then spray-dried to create a resin powder with improved handling properties, characterized by a specific particle size range and gel fraction, facilitating easier separation and use.
The resulting resin powder exhibits good handling properties and maintains the biodegradability and performance benefits of crosslinked polyhydroxyalkanoate resin particles, addressing the aggregation issues of previous methods and enabling their effective application in various uses.
Smart Images

Figure JPOXMLDOC01-APPB-T000001
Abstract
Description
Resin powder and its manufacturing method
[0001] The present invention relates to a resin powder containing crosslinked resin particles and a method for producing the same.
[0002] It has been known that introducing a crosslinked structure into a resin can improve the resin's hardness, heat resistance, solvent resistance, etc. Small resin particles composed of resins with such crosslinked structures are used in a variety of applications, such as modifiers for thermoplastic resins, spacers, antiblocking agents, and matting agents.
[0003] Known resin materials constituting such crosslinked resin particles include acrylic resins, acrylic silicone resins, polystyrene, and the like (see, for example, Patent Documents 1 and 2).
[0004] On the other hand, plastic waste is a burden on the global environment, affecting ecosystems, emitting harmful gases when burned, and contributing to global warming due to the large amount of heat generated by combustion. Therefore, there has been active development of biodegradable plastics as a material that can solve these problems.
[0005] Patent Document 3 describes crosslinking of poly(3-hydroxyalkanoate), a type of biodegradable plastic, by melt-kneading the resin in the presence of an organic peroxide. However, it describes that the crosslinked resin produced by melt-kneading in this way is used to form films or sheets, and does not describe at all the production of small particle size crosslinked resin particles.
[0006] JP 2009-56770 A JP 2003-82191 A International Publication No. 2019 / 022008
[0007] To date, small-sized crosslinked resin particles made of biodegradable plastics and exhibiting biodegradability have not been known. The present inventors have succeeded in producing crosslinked resin particles made of polyhydroxyalkanoate resin, a biodegradable resin, in an aqueous dispersion. These crosslinked resin particles are expected to address the problem of plastic waste and be useful as environmentally friendly crosslinked resin particles. However, when attempting to separate the crosslinked resin particles from the aqueous dispersion, the crosslinked resin particles adhere to each other as the water evaporates, forming rubber-like sheets or lumpy solids, making it difficult to separate them in an easily handleable form.
[0008] In view of the above-mentioned current situation, an object of the present invention is to provide crosslinked resin particles made of a polyhydroxyalkanoate resin in a form that is easy to handle.
[0009] As a result of extensive research, the present inventors have discovered that a resin powder containing crosslinked resin particles, which is easy to handle, can be obtained by preparing an aqueous dispersion in which a thermoplastic resin is dispersed together with crosslinked resin particles composed of a polyhydroxyalkanoate resin, and spray-drying the aqueous dispersion, thereby completing the present invention.
[0010] That is, the present invention relates to a resin powder having a median diameter of 20 to 1000 μm, the resin powder containing a thermoplastic resin (A) and crosslinked resin particles (B), the crosslinked resin particles (B) containing a polyhydroxyalkanoate resin, a gel fraction of 50% or more, and a volume average particle diameter of 0.1 μm to 10 μm. The present invention also relates to a method for producing the resin powder, the method comprising the steps of preparing an aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B), and spray-drying the aqueous dispersion.
[0011] According to the present invention, crosslinked resin particles made of a polyhydroxyalkanoate resin can be provided in a form that is easy to handle.
[0012] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to the following embodiments.
[0013] The resin powder according to the present embodiment contains at least a thermoplastic resin (A) and crosslinked resin particles (B). The resin powder has a particle size within a specific range, and therefore has good handleability. First, the crosslinked resin particles (B) will be described.
[0014] <Crosslinked Resin Particles (B)> The crosslinked resin particles (B) are particles composed of a polyhydroxyalkanoate-based resin as a main resin component. Hereinafter, the polyhydroxyalkanoate-based resin may be abbreviated as "PHA."
[0015] <PHA> "PHA" is a general term for polymers having hydroxyalkanoic acid as a monomer unit, and is generally biodegradable. PHA is an aliphatic polyester, preferably a polyester not containing an aromatic ring.
[0016] The PHA is not particularly limited, but examples thereof include polyglycolic acid, poly(3-hydroxyalkanoate)-based resins, and poly(4-hydroxyalkanoate)-based resins. Only one type of PHA may be used, or two or more types may be used in combination. Of these, poly(3-hydroxyalkanoate)-based resins are preferred. Hereinafter, poly(3-hydroxyalkanoate)-based resins may be abbreviated as "P3HA."
[0017] The P3HA has the formula: [—CHR—CH 2 3-hydroxyalkanoic acid repeating units represented by the formula: —CO—O— (wherein R is C n H 2n+1 where n is an integer of 1 to 15.) as an essential repeating unit. The P3HA preferably contains 50 mol % or more, and more preferably 70 mol % or more, of the total monomer repeating units (100 mol %) of the 3-hydroxyalkanoic acid repeating units.
[0018] P3HA is not particularly limited and may be a homopolymer containing the repeating unit described above, or a copolymer containing the repeating unit described above. Examples of the copolymer include copolymers of 3-hydroxybutanoic acid (hereinafter sometimes referred to as "3HB") and one or more monomers selected from the group consisting of 3-hydroxypropionic acid, 3-hydroxypentanoic acid, 3-hydroxyhexanoic acid, 3-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 3-hydroxydecanoic acid, 3-hydroxyundecanoic acid, 3-hydroxydodecanoic acid, 3-hydroxytridecanoic acid, 3-hydroxytetradecanoic acid, 3-hydroxyhexadecanoic acid, and 3-hydroxyoctadecanoic acid. Other examples of the copolymer include copolymers of 3HB and one or more monomers selected from the group consisting of 4-hydroxybutanoic acid, 4-hydroxypentanoic acid, 4-hydroxyhexanoic acid, 4-hydroxyheptanoic acid, 4-hydroxyoctanoic acid, 4-hydroxynonanoic acid, 4-hydroxydecanoic acid, 4-hydroxyundecanoic acid, 4-hydroxydodecanoic acid, 4-hydroxytridecanoic acid, 4-hydroxytetradecanoic acid, 4-hydroxyhexadecanoic acid, and 4-hydroxyoctadecanoic acid.
[0019] Specific examples of the homopolymer or copolymer include, but are not limited to, poly(3-hydroxybutyrate) (abbreviation: P3HB), poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (abbreviation: P3HB3HH), poly(3-hydroxybutyrate-co-4-hydroxybutyrate) (abbreviation: P3HB4HB), etc. As P3HA, only one type may be used, or two or more types may be used in combination.
[0020] As used herein, the term "poly(X-co-Y)" refers to a copolymer containing X repeating units and Y repeating units, obtained by copolymerizing a monomer from which the X repeating units are derived and a monomer from which the Y repeating units are derived.
[0021] Furthermore, during the production of P3HA, a small amount (less than 1 mol%) of a monomer may be copolymerized. However, if this does not significantly affect the physical properties of the resulting P3HA, the monomer is considered not to be copolymerized, and the product will be referred to by a name that does not include that monomer.
[0022] P3HA can be produced by microorganisms. Such microbially produced P3HA is usually P3HA composed only of D-form (R-form) hydroxyalkanoic acid repeating units. Among microbially produced P3HAs, P3HB, P3HB3HH, and P3HB4HB are preferred, with P3HB3HH and P3HB4HB being more preferred, due to ease of industrial production.
[0023] When P3HA contains 3-hydroxybutanoic acid (3HB) repeating units, from the viewpoint of the balance between flexibility and strength, the composition ratio of 3HB repeating units in all monomer repeating units (100 mol%) is preferably 60 to 99 mol%, more preferably 61 to 97 mol%, and even more preferably 62 to 95 mol%. Having a composition ratio of 3HB repeating units of 60 mol% or more facilitates handling of the crosslinked resin particles (B) or the resin particles before crosslinking treatment. On the other hand, having a composition ratio of 3HB repeating units of 99 mol% or less tends to ensure the flexibility of the crosslinked resin particles (B). The monomer composition ratio of P3HA can be measured by gas chromatography or the like (see, for example, WO 2014 / 020838). Two or more types of P3HA having different composition ratios of 3HB repeating units may be used in combination.
[0024] The microorganism that produces P3HA is not particularly limited as long as it has the ability to produce P3HA. For example, the first P3HB-producing bacterium was Bacillus megaterium, discovered in 1925. Other known natural microorganisms include Cupriavidus necator (formerly classified as Alcaligenes eutrophus, Ralstonia eutropha) and Alcaligenes latus. In these microorganisms, P3HB accumulates intracellularly.
[0025] Known examples of bacteria that produce copolymers of 3HB and other hydroxyalkanoates include Aeromonas caviae, which produces P3HB3HH, and Alcaligenes eutrophus, which produces poly(3-hydroxybutyrate-co-4-hydroxybutyrate). In particular, Alcaligenes eutrophus AC32 (FERM BP-6038) (T. Fukui, Y. Doi, J. Bateriol., 179, pp. 4821-4830 (1997)), into which genes encoding P3HA synthases have been introduced, is preferred in order to increase the productivity of P3HB3HH. Microbial cells obtained by culturing such microorganisms under appropriate conditions and allowing P3HA to accumulate within the cells are used. In addition to the above, genetically modified microorganisms into which various P3HA synthesis-related genes have been introduced may be used depending on the P3HA to be produced, or culture conditions, including the type of substrate, may be optimized.
[0026] The molecular weight of the PHA is not particularly limited, but the weight-average molecular weight is preferably 50,000 to 3,000,000, more preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,500,000. By setting the weight-average molecular weight to 50,000 or more, it is possible to avoid the tendency for the crosslinked resin particles (B) to have a low strength or to be sticky due to low molecular weight components. On the other hand, by setting the weight-average molecular weight to 3,000,000 or less, it is possible to facilitate the production and handling of the PHA. The weight-average molecular weight is a value measured before the PHA is subjected to a crosslinking treatment.
[0027] The weight-average molecular weight can be measured using gel permeation chromatography (GPC) (Shimadzu Corporation's "High Performance Liquid Chromatograph 20A System"), using polystyrene gel (Showa Denko K.K.'s "K-G 4A" or "K-806M" or the like) as a column, and chloroform as a mobile phase, and can be determined as a molecular weight converted into polystyrene. In this case, a calibration curve can be prepared using polystyrenes with weight-average molecular weights of 31,400, 197,000, 668,000, and 1,920,000. As the column for the GPC, a column appropriate for measuring the molecular weight can be used.
[0028] <Gel fraction> The crosslinked resin particles (B) have a crosslinked structure in which molecular chains of PHA are bonded to each other. Since the crosslinked resin particles (B) have a certain amount or more of such crosslinked structure, they exhibit a high gel fraction, specifically, a gel fraction of 50% or more. By exhibiting such a high gel fraction, the hardness, heat resistance, solvent resistance, etc. of the resin particles containing PHA can be improved.
[0029] The gel fraction is preferably 60% or more, more preferably 70% or more, even more preferably 75% or more, and particularly preferably 80% or more. It may also be 85% or more, or even 90% or more. The upper limit of the gel fraction is not particularly limited as long as it is 100% or less. From the viewpoint of production efficiency of the crosslinked resin particles (B), however, it is preferably 99.5% or less, more preferably 99% or less. It may also be 98% or less, 97% or less, or 96% or less.
[0030] The gel fraction is a value measured as follows. A dried product of crosslinked resin particles (B) is added to chloroform so that the concentration becomes 0.7% by weight, and the mixture is dissolved at 60°C for 30 minutes to obtain a chloroform solution. After that, the mixture is left to stand at room temperature for 3 hours, and the chloroform solution is filtered through a membrane filter with a pore size of 0.45 µm. The gel remaining on the filter is dried, and the weight of the filter is measured, and the gel fraction is calculated using the following formula: Gel fraction = (weight of filter including dried gel - weight of filter only) / weight of crosslinked resin particles used for measurement x 100 (%)
[0031] <Average particle size> The crosslinked resin particles (B) have a volume average particle size in the range of 0.1 μm to 10 μm. By having such a particle size, a resin powder having a particle size within the specific range according to the present embodiment can be formed, and can be used for various applications as described below. From the viewpoint of practical use, the lower limit of the particle size is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. Furthermore, from the viewpoint of productivity (such as PHA production and crosslinking treatment), the upper limit of the particle size is preferably 8 μm or less, more preferably 5 μm or less.
[0032] The volume average particle diameter is a value measured when the crosslinked resin particles (B) are dispersed in an aqueous solvent. A general-purpose measuring device can be used as the measuring device, and an example of such a device is Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.
[0033] <Peroxide> The crosslinking type of the crosslinked resin particles (B) is not particularly limited, but it is preferable that the crosslinking is performed using a peroxide. When a peroxide is used, radicals generated by decomposition of the peroxide act on PHA molecules to directly bond PHA molecular chains to each other, thereby forming the crosslinked structure.
[0034] The peroxide may be an organic peroxide or an inorganic peroxide, but is preferably an organic peroxide because it can increase the gel fraction more efficiently.
[0035] As the organic peroxide, it is preferable to use at least one selected from the group consisting of diacyl peroxides, alkyl peroxy esters, dialkyl peroxides, hydroperoxides, peroxyketals, peroxycarbonates, and peroxydicarbonates, taking into consideration the heating temperature and time during the crosslinking treatment.
[0036] Specific examples of such organic peroxides include butyl peroxy neododecanoate, octanoyl peroxide, dilauroyl peroxide, succinic peroxide, a mixture of toluoyl peroxide and benzoyl peroxide, benzoyl peroxide, bis(butylperoxy)trimethylcyclohexane, butyl peroxylaurate, dimethyldi(benzoylperoxy)hexane, bis(butylperoxy)methylcyclohexane, bis(butylperoxy)cyclohexane, and butylperoxybenzo ester, butyl bis(butylperoxy)valerate, dicumyl peroxide, di-t-hexyl peroxide, t-butylperoxy 2-ethylhexanoate, t-butylperoxyisobutyrate, t-butylperoxypivalate, t-hexylperoxypivalate, t-butylperoxymethyl monocarbonate, t-pentylperoxymethyl monocarbonate, t-hexylperoxymethyl monocarbonate, t-heptylperoxymethyl monocarbonate, t-octylperoxymethyl monocarbonate, 1 , 1,3,3-tetramethylbutylperoxymethyl monocarbonate, t-butylperoxyethyl monocarbonate, t-pentylperoxyethyl monocarbonate, t-hexylperoxyethyl monocarbonate, t-heptylperoxyethyl monocarbonate, t-octylperoxyethyl monocarbonate, 1,1,3,3-tetramethylbutylperoxyethyl monocarbonate, t-butylperoxy n-propyl monocarbonate, t-pentylperoxy n-propyl monocarbonate, t-hexylperoxy peroxy isopropyl monocarbonate, t-heptylperoxy isopropyl monocarbonate, t-octylperoxy isopropyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy isopropyl monocarbonate, t-butylperoxy isopropyl monocarbonate, t-pentylperoxy isopropyl monocarbonate, t-hexylperoxy isopropyl monocarbonate, t-heptylperoxy isopropyl monocarbonate, t-octylperoxy isopropyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy isopropyl monocarbonate, t-butylperoxy n-butyl monocarbonate, t-pentylperoxy n-butyl monocarbonate, t-hexylperoxy n-butyl monocarbonate, t-heptylperoxy n-butyl monocarbonate, t-octylperoxy n-butyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy n-butyl monocarbonate, t-butylperoxy isobutyl monocarbonate, t-pentylperoxy isobutyl monocarbonate, t -Hexylperoxy isobutyl monocarbonate, t-heptylperoxy isobutyl monocarbonate, t-octylperoxy isobutyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy isobutyl monocarbonate, t-butylperoxy sec-butyl monocarbonate, t-pentylperoxy sec-butyl monocarbonate, t-hexylperoxy sec-butyl monocarbonate, t-heptylperoxy sec-butyl monocarbonate, t-octylperoxy sec-butyl monocarbonate t-butylperoxy t-butyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy sec-butyl monocarbonate, t-butylperoxy t-butyl monocarbonate, t-pentylperoxy t-butyl monocarbonate, t-hexylperoxy t-butyl monocarbonate, t-heptylperoxy t-butyl monocarbonate, t-octylperoxy t-butyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy t-butyl monocarbonate, t-butylperoxy 2-ethylhexyl monocarbonate, t-pentylperoxy 2-ethylhexyl monocarbonate ethylhexyl monocarbonate, t-hexylperoxy 2-ethylhexyl monocarbonate, t-heptylperoxy 2-ethylhexyl monocarbonate, t-octylperoxy 2-ethylhexyl monocarbonate, 1,1,3,3-tetramethylbutylperoxy 2-ethylhexyl monocarbonate, diisobutyl peroxide, cumyl peroxy neodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, bis(4-t-butylcyclohexyl) peroxydicarbonate, bis(2-ethylhexyl) peroxydicarbonate, t-hexyl peroxyneodecanoate, t-butyl peroxyneodecanoate, t-butyl peroxyneoheptanoate, t-hexyl peroxypivalate, t-butyl peroxypivalate, di(3,5,5-trimethylhexanoyl) peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-bis(2-ethylhexanoylperoxy) Examples of organic peroxides include hexane, t-hexylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxy-2-ethylhexyl carbonate, t-butylperoxyisopropyl carbonate, 1,6-bis(t-butylperoxycarbonyloxy)hexane, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxyacetate, t-butylperoxybenzoate, t-amylperoxy-3,5,5-trimethylhexanoate, 2,2-bis(4,4-di-t-butylperoxycyclohexyl)propane, and 2,2-di-t-butylperoxybutane. One organic peroxide may be used alone, or two or more organic peroxides may be used in combination.
[0037] Among these, t-butylperoxyisopropyl monocarbonate, t-pentylperoxyisopropyl monocarbonate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxy2-ethylhexyl monocarbonate, t-pentylperoxy2-ethylhexyl monocarbonate, t-hexylperoxy2-ethylhexyl monocarbonate, t-amylperoxyisopropyl monocarbonate, di-t-hexyl peroxide, t-butylperoxy2-ethylhexyl monocarbonate, Peroxymethylbutylperoxyisobutyrate, t-hexylperoxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy 2-ethylhexanoate, t-butylperoxypivalate, t-hexylperoxypivalate, t-butylperoxyneodecanoate, t-hexylperoxyneodecanoate, and 1,1,3,3-tetramethylbutylperoxyneodecanoate are preferred organic peroxides because they can efficiently promote crosslinking of PHA.
[0038] The peroxide is preferably a compound having a one-hour half-life temperature of 200° C. or less, more preferably 170° C. or less, and even more preferably 140° C. or less, so that the heating temperature during the crosslinking treatment can be set low. The lower limit may be 50° C. or more, 60° C. or more, or 70° C. or more.
[0039] Particularly preferred organic peroxides exhibiting such a one-hour half-life temperature include t-butylperoxyisopropyl monocarbonate, t-butylperoxy 2-ethylhexyl monocarbonate, di-sec-butylperoxydicarbonate, t-butylperoxy 2-ethylhexanoate, t-butylperoxyisobutyrate, t-hexylperoxy 2-ethylhexanoate, 1,1,3,3-tetramethylbutylperoxy 2-ethylhexanoate, t-butylperoxypivalate, t-hexylperoxypivalate, t-butylperoxyneodecanoate, t-hexylperoxyneodecanoate, and 1,1,3,3-tetramethylbutylperoxyneodecanoate.
[0040] When the peroxide is an inorganic peroxide, examples of the inorganic peroxide include hydrogen peroxide, potassium peroxide, calcium peroxide, sodium peroxide, magnesium peroxide, potassium persulfate, sodium persulfate, and ammonium persulfate, taking into consideration the heating temperature and time during the crosslinking treatment. Among these, hydrogen peroxide, potassium persulfate, sodium persulfate, and ammonium persulfate are preferred because they are easy to handle and have decomposition temperatures suitable for the heating temperature during the crosslinking treatment. One type of inorganic peroxide may be used alone, or two or more types may be used in combination. Furthermore, an organic peroxide and an inorganic peroxide may be used in combination.
[0041] <Polyfunctional Compound> The crosslinked structure in the crosslinked resin particles (B) may be introduced using only a peroxide, or may be introduced using both a peroxide and a polyfunctional compound, which makes it possible to increase the gel fraction of the crosslinked resin particles (B) with a smaller amount of peroxide.
[0042] The polyfunctional compound refers to a compound having two or more functional groups capable of crosslinking PHA in one molecule. Although not particularly limited, a compound having reactivity with radicals generated from peroxide is preferred, and a compound having two or more radical reactive groups in one molecule is particularly preferred. The radical reactive group is preferably at least one selected from the group consisting of a vinyl group, an allyl group, an acryloyl group, or a methacryloyl group.
[0043] Such polyfunctional compounds are not particularly limited, but examples thereof include allyl (meth)acrylate, allyl alkyl (meth)acrylates, allyloxyalkyl (meth)acrylates, polyfunctional (meth)acrylates having two or more (meth)acrylic groups such as ethylene glycol di(meth)acrylate, butanediol di(meth)acrylate, triethylene glycol di(meth)acrylate, tetraethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and pentaerythritol (meth)acrylate, divinylbenzene, diallyl phthalate, triallyl cyanurate, triallyl isocyanurate, and divinylbenzene. Preferred are allyl methacrylate, triallyl isocyanurate, butanediol di(meth)acrylate, and divinylbenzene, and particularly preferred are allyl methacrylate and triallyl isocyanurate.
[0044] When a crosslinked structure is formed in the presence of a polyfunctional compound, the resulting crosslinked resin particles (B) may generally contain a structure derived from the polyfunctional compound, in which case molecular chains of the PHA are bonded to each other via the structure derived from the polyfunctional compound.
[0045] The crosslinked resin particles (B) may be composed solely of a PHA having a crosslinked structure, or may further contain components other than the PHA having a crosslinked structure, such as resins other than PHA, antioxidants, hydrolysis inhibitors, antiblocking agents, crystal nucleating agents, and ultraviolet absorbers.
[0046] The proportion of PHA in the crosslinked resin particles (B) is not particularly limited, but may be 50% by weight or more, preferably 70% by weight or more, more preferably 80% by weight or more, even more preferably 90% by weight or more, and particularly preferably 95% by weight or more. It may also be 99% by weight or more. The upper limit is not particularly limited, and it may be 100% by weight or less.
[0047] Examples of resins other than PHA include polycaprolactone (PCL), polylactic acid (PLA), aliphatic polyesters having a structure in which an aliphatic diol and an aliphatic dicarboxylic acid are polycondensed, and aliphatic-aromatic polyesters having both an aliphatic compound and an aromatic compound as monomers. Examples of the aliphatic polyesters include polyethylene succinate, polybutylene succinate (PBS), polyhexamethylene succinate, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polybutylene succinate adipate (PBSA), polyethylene sebacate, and polybutylene sebacate. Examples of the aliphatic aromatic polyester include poly(butylene adipate-co-butylene terephthalate) (PBAT), poly(butylene sebacate-co-butylene terephthalate), poly(butylene azelate-co-butylene terephthalate), poly(butylene succinate-co-butylene terephthalate) (PBST), etc. One type of the other resin may be used alone, or two or more types may be used in combination.
[0048] The crosslinked resin particles (B) are different from the expanded resin particles disclosed in WO 2007 / 049694 and WO 2019 / 146555, and are preferably non-expanded, i.e., do not contain substantially any air bubbles inside the particles.
[0049] When not expanded, the crosslinked resin particles (B) have a relatively high apparent density of 0.6 g / cm 3 It is preferable that the density exceeds 0.7 g / cm 3 More preferably, it is 0.9 g / cm or more. 3 The apparent density of the crosslinked resin particles (B) can be determined by the method described in JIS K0061 (Method for measuring density and specific gravity of chemical products) or JIS Z8807 (Method for measuring density and specific gravity of solids).
[0050] The average weight per particle of the crosslinked resin particles (B) is not particularly limited, but since the crosslinked resin particles (B) have a small particle size with a volume average particle diameter of 10 μm or less, the value is far less than 0.1 mg.
[0051] <Method for producing crosslinked resin particles (B)> An example of a method for producing crosslinked resin particles (B) will be specifically described. The crosslinked resin particles (B) can be produced by crosslinking PHA in the presence of a peroxide in an aqueous dispersion containing PHA particles before crosslinking treatment. In order to efficiently crosslink the PHA, it is preferable to heat the aqueous dispersion of PHA particles containing a peroxide to a temperature suitable for decomposing the peroxide.
[0052] More specifically, the method for producing the crosslinked resin particles (B) preferably includes the steps of: (1) preparing an aqueous dispersion of PHA particles in which pre-crosslinked PHA particles are dispersed in water; (2) adding a peroxide to the aqueous dispersion of PHA particles to impregnate the PHA particles with the peroxide; and (3) heating the aqueous dispersion of PHA particles impregnated with the peroxide to a heating temperature to crosslink the PHA. Furthermore, the method more preferably includes the step of (4) maintaining the heating temperature after all the peroxide has been added.
[0053] In step (1), the aqueous dispersion of PHA particles may be an aqueous dispersion obtained by culturing a PHA-producing microorganism to accumulate PHA in the cells, disrupting the cells in the culture solution, and separating and removing the cell components, or an aqueous dispersion obtained by concentrating or diluting the aqueous dispersion. According to such a method, the process from producing PHA particles by culturing a PHA-producing microorganism to crosslinking treatment can be carried out without separating the PHA particles from water.
[0054] Alternatively, an aqueous dispersion of PHA particles can be prepared by dispersing dried PHA particles in water. The aqueous dispersion may contain, in addition to water, a water-compatible organic solvent as described below.
[0055] In the aqueous dispersion, the volume average particle diameter of the PHA particles is preferably within the same range as that of the crosslinked resin particles (B) described above. In the case of PHA particles produced by a PHA-producing microorganism, the volume average particle diameter can usually be within the above range, so that an aqueous dispersion of PHA particles having a desired volume average particle diameter can be obtained without carrying out a special step for adjusting the particle diameter.
[0056] The concentration of the PHA particles in the aqueous dispersion is not particularly limited and can be set appropriately, but may be, for example, about 1 to 70% by weight, preferably about 5 to 50% by weight.
[0057] The aqueous dispersion of PHA particles preferably contains a dispersant, in order to improve the dispersibility of PHA particles and make the crosslinking reaction proceed uniformly.As dispersants, for example, anionic surfactants such as dioctyl sodium sulfosuccinate, sodium dodecyl sulfate, sodium lauryl sulfate, sodium oleate, etc.; cationic surfactants such as lauryl trimethyl ammonium chloride, etc.; nonionic surfactants such as glycerin fatty acid ester, sorbitan fatty acid ester, sucrose fatty acid ester, polyoxyethylene alkyl ether, polyoxyethylene alkylphenyl ether, polyoxyethylene polyoxypropylene glycol, etc.; water-soluble polymers such as polyvinyl alcohol, ethylene-modified polyvinyl alcohol, polyvinylpyrrolidone, methyl cellulose, ethyl cellulose, hydroxymethyl cellulose, hydroxyethyl cellulose, polyacrylic acid, sodium polyacrylate, potassium polyacrylate, polymethacrylic acid, sodium polymethacrylate, etc.These dispersants may be used alone or in combination of two or more.
[0058] When a dispersant is used, the amount thereof to be added is not particularly limited, but may be, for example, 0.1 to 10 parts by weight, preferably 0.5 to 5 parts by weight, and particularly preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of PHA particles.
[0059] In step (2), a peroxide is added to the aqueous dispersion of PHA particles obtained in step (1) to impregnate the PHA particles with the peroxide. The peroxide may be any of those described above. The peroxide may be added in various forms, such as a solid or liquid. Alternatively, a liquid diluted with a diluent or the like may be added. The peroxide may be added all at once, continuously, or in portions.
[0060] When a peroxide and the polyfunctional compound are used in combination, it is preferable to add the polyfunctional compound to the aqueous dispersion of PHA particles in this step (2). The polyfunctional compound can be any of those described above. The polyfunctional compound can be added in various forms, such as solid or liquid. A liquid diluted with a diluent or the like may also be added. The polyfunctional compound may be added all at once, continuously, or in portions.
[0061] To impregnate the PHA particles with the peroxide and any polyfunctional compound, after or while adding these compounds to an aqueous dispersion of the PHA particles, the temperature of the aqueous dispersion is set to, for example, 0°C or higher but lower than a temperature suitable for decomposing the peroxide employed in the next step (3), and the aqueous dispersion is stirred while maintaining this temperature for, for example, about 1 minute to 5 hours. The temperature of the aqueous dispersion during impregnation may specifically be about 10 to 60°C.
[0062] The amount of peroxide used can be appropriately set in consideration of the gel fraction of the crosslinked resin particles (B), and is, for example, preferably 0.01 to 10 parts by weight, more preferably 0.1 to 8 parts by weight, even more preferably 0.3 to 5 parts by weight, and particularly preferably 0.5 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0063] According to the manufacturing method of crosslinking PHA particles in an aqueous dispersion using peroxide, crosslinking can be easily carried out while maintaining the particle size (volume) before crosslinking, and crosslinked resin particles can be easily obtained.On the other hand, it may be difficult to achieve this in the method of crosslinking resin by melt kneading in the presence of peroxide.In addition, according to the manufacturing method of crosslinking PHA particles in an aqueous dispersion using peroxide, it is easy to control the temperature rise caused by the heat generated during the crosslinking reaction, and it is advantageous in efficiently obtaining crosslinked resin particles with a safe and stable crosslinked structure (quality).
[0064] The amount of the polyfunctional compound used may also be appropriately determined in consideration of the gel fraction of the crosslinked resin particles (B). For example, the amount is preferably 0.01 to 20 parts by weight, more preferably 0.05 to 15 parts by weight, even more preferably 0.1 to 10 parts by weight, even more preferably 0.2 to 5 parts by weight, and particularly preferably 0.3 to 3 parts by weight, relative to 100 parts by weight of the PHA particles.
[0065] In step (3), the aqueous dispersion of PHA particles impregnated with peroxide is heated to a temperature suitable for decomposing the peroxide. The heating temperature is preferably within a range of about 25°C above or below the one-hour half-life temperature of the peroxide. Specifically, the heating temperature is preferably 30 to 140°C, more preferably 50 to 135°C, and even more preferably 60 to 130°C. This method makes it possible to crosslink the PHA at a temperature lower than the melting temperature of the PHA, thereby avoiding deterioration of the PHA due to heating during the crosslinking treatment.
[0066] In the subsequent step (4), it is preferable to maintain the heating temperature. This allows the crosslinking reaction using the peroxide to proceed sufficiently. The time for maintaining the heating temperature is not particularly limited, but is preferably 1 minute to 15 hours, and more preferably 1 hour to 10 hours.
[0067] By carrying out the above steps (1) to (4), an aqueous dispersion of the crosslinked resin particles (B) can be obtained. This aqueous dispersion can be used to produce the resin powder according to this embodiment. Details will be described later.
[0068] <Thermoplastic Resin (A)> The resin powder according to this embodiment contains a thermoplastic resin (A) in addition to the crosslinked resin particles (B). By containing the thermoplastic resin (A), it is possible to form a resin powder that has good handleability despite containing the crosslinked resin particles (B).
[0069] The thermoplastic resin (A) is not particularly limited as long as it can form a resin powder together with the crosslinked resin particles (B). Specific examples include polyolefin resins such as polyethylene and polypropylene, acrylic resins such as polyvinyl chloride, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, and polymethyl methacrylic acid, AS resin, polyamide, polyacetal, polycarbonate, modified polyphenylene ether, polyester resin, and cyclic polyolefin. These thermoplastic resins may be used alone or in combination of two or more.
[0070] As the thermoplastic resin (A), polyester resins are particularly preferred due to their good compatibility with the crosslinked resin particles (B) composed of polyhydroxyalkanoate resins. Examples of such polyester resins include PHAs such as polyglycolic acid, poly(3-hydroxyalkanoate) resins, and poly(4-hydroxyalkanoate) resins; polylactic acid; aliphatic polyesters such as polyesters formed by the polycondensation of aliphatic diols and aliphatic dicarboxylic acids; and aliphatic-aromatic polyesters containing both aliphatic and aromatic compounds as monomers. Examples of aliphatic polyesters other than PHAs include polycaprolactone, polyethylene succinate, polybutylene succinate (PBS), polyhexamethylene succinate, polyethylene adipate, polybutylene adipate, polyhexamethylene adipate, polybutylene succinate adipate (PBSA), polyethylene sebacate, and polybutylene sebacate. Examples of aliphatic aromatic polyesters include poly(butylene adipate-co-butylene terephthalate) (PBAT), poly(butylene sebacate-co-butylene terephthalate), poly(butylene azelate-co-butylene terephthalate), poly(butylene succinate-co-butylene terephthalate) (PBST), polyethylene furanoate, etc. These polyester resins may be used alone or in combination of two or more.
[0071] Since the crosslinked resin particles (B) are composed of a biodegradable PHA, it is preferable that the thermoplastic resin (A) also contains a biodegradable resin, which can enhance the biodegradability of the resin powder as a whole.
[0072] Furthermore, when the crosslinked resin particles (B) are produced from plant-derived raw materials, it is preferable that the thermoplastic resin (A) is also a resin produced from plant-derived raw materials from the viewpoint of resource circulation.
[0073] When the thermoplastic resin (A) contains a biodegradable resin, the content thereof is preferably 10 to 100% by weight, more preferably 30% by weight or more, even more preferably 50% by weight or more, even more preferably 70% by weight or more, and particularly preferably 90% by weight or more, of the entire thermoplastic resin (A).
[0074] The biodegradable resin used as the thermoplastic resin (A) preferably contains the aliphatic polyester described above, and particularly preferably contains PHA and / or polylactic acid, because it has good compatibility with the crosslinked resin particles (B) and is easy to produce a resin powder with good handleability. Note that the PHA used as the thermoplastic resin (A) preferably does not have a crosslinked structure.
[0075] When the thermoplastic resin (A) contains PHA and / or polylactic acid, the content thereof is preferably 10 to 100% by weight, more preferably 30% by weight or more, even more preferably 50% by weight or more, still more preferably 70% by weight or more, and particularly preferably 90% by weight or more, of the entire thermoplastic resin (A).
[0076] The PHA that can be used as the thermoplastic resin (A) is not particularly limited, and examples thereof include polyglycolic acid, P3HA, poly(4-hydroxyalkanoate)-based resins, etc. As the PHA, one type may be used alone, or two or more types may be used in combination. Of these, P3HA is particularly preferred.
[0077] The P3HA that can be used as the thermoplastic resin (A) is the same as the P3HA related to the crosslinked resin particles (B), and the various P3HAs described above can be used. The P3HA used as the thermoplastic resin (A) is preferably different from the P3HA used for the crosslinked resin particles (B), and is more preferably a resin that is harder than the P3HA used for the crosslinked resin particles (B).
[0078] When the P3HA used as the thermoplastic resin (A) contains 3-hydroxybutanoic acid (3HB) repeating units, from the viewpoint of the balance between flexibility and strength, the composition ratio of 3HB repeating units is preferably 80 to 99 mol%, more preferably 82 to 97 mol%, of all monomer repeating units (100 mol%). When the composition ratio of 3HB repeating units is 80 mol% or more, the rigidity of the P3HA can be further improved. On the other hand, when the composition ratio of 3HB repeating units is 99 mol% or less, the flexibility of the P3HA tends to be further improved. As P3HA, two or more types having different composition ratios of 3HB repeating units may be used in combination.
[0079] The molecular weight of the PHA used as the thermoplastic resin (A) is not particularly limited, but the weight-average molecular weight is preferably 50,000 to 3,000,000, more preferably 100,000 to 2,000,000, and more preferably 150,000 to 1,500,000. By setting the weight-average molecular weight to 50,000 or more, the resin powder according to this embodiment can achieve good rigidity and strength. On the other hand, by setting the weight-average molecular weight to 3,000,000 or less, the production and handling of the PHA can be facilitated.
[0080] The polylactic acid usable as the thermoplastic resin (A) may be any conventionally known polylactic acid, and may be either crystalline or amorphous. The polylactic acid may be a homopolymer of lactic acid or a copolymer of lactic acid and another monomer. Alternatively, it may be a blend of these. Examples of the other monomer include aliphatic hydroxycarboxylic acids other than lactic acid, aliphatic polyhydric alcohols, aliphatic polycarboxylic acids, and polyfunctional polysaccharides.
[0081] The lactic acid raw material for producing polylactic acid is not particularly limited, and examples thereof include L-lactic acid, D-lactic acid, DL-lactic acid, or a mixture thereof, and L-lactide, D-lactide, meso-lactide, or a mixture thereof. Lactic acid obtained by microbial fermentation from renewable plant-derived raw materials such as starch is preferably used. The method for producing polylactic acid is not particularly limited, and known methods such as dehydration condensation polymerization and ring-opening polymerization can be used.
[0082] The molecular weight of the polylactic acid used as the thermoplastic resin (A) is not particularly limited, but the weight-average molecular weight is preferably 50,000 to 1,000,000, more preferably 70,000 to 700,000, and more preferably 100,000 to 400,000. By setting the weight-average molecular weight to 50,000 or more, the resin powder according to this embodiment can achieve good rigidity and strength. On the other hand, by setting the weight-average molecular weight to 1,000,000 or less, the production and handling of the polylactic acid can be facilitated.
[0083] <Resin Powder> As described above, the resin powder according to this embodiment contains a thermoplastic resin (A) and crosslinked resin particles (B). In the resin powder, the content of the crosslinked resin particles (B) relative to the total of the thermoplastic resin (A) and the crosslinked resin particles (B) is preferably 10% by weight or more, more preferably 20% by weight or more, and even more preferably 30% by weight or more, since this makes it easier to realize the effects of the crosslinked resin particles (B). It may even be 40% by weight or more. Furthermore, the upper limit of the content of the crosslinked resin particles (B) is preferably 90% by weight or less, more preferably 80% by weight or less, and even more preferably 70% by weight or less, since this can further improve the handleability of the resin powder. It may even be 60% by weight or less.
[0084] The resin powder according to this embodiment may be substantially composed of only a thermoplastic resin (A) and crosslinked resin particles (B), but may also contain, within the scope of the invention, one or more of the following: dispersants or emulsifiers, pH adjusters, inorganic fillers, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, UV absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, sliding property improvers, etc. Furthermore, the resin powder according to this embodiment may contain various components resulting from the manufacturing process within the scope of the invention.
[0085] The resin powder according to this embodiment is mainly composed of a thermoplastic resin (A) and crosslinked resin particles (B). Specifically, the total proportion of the thermoplastic resin (A) and crosslinked resin particles (B) in the entire resin powder may typically be 60 to 100% by weight, 80 to 100% by weight, 90 to 100% by weight, 95 to 100% by weight, or 99 to 100% by weight. The upper limit may be 99.9% by weight or less, or 99% by weight or less.
[0086] The resin powder according to this embodiment may have a median diameter in the range of 20 μm or more and 1000 μm or less, from the viewpoint of improving the handleability of the resin powder. The lower limit may be 30 μm or more. The upper limit may be 500 μm or less, 300 μm or less, 200 μm or less, or 100 μm or less. The median diameter of the resin powder is a value measured by a dry or wet laser diffraction / scattering method using, for example, an LMS-3000 manufactured by Seishin Enterprise Co., Ltd. When measuring by a wet method, it is preferable to add the resin powder to an aqueous solution to which a small amount of a surfactant has been added as a dispersant, and measure the resin powder in a state where it is not aggregated.
[0087] The resin powder according to this embodiment preferably has a low moisture content, specifically, a moisture content of preferably 5% by weight or less, more preferably 3% by weight or less, and even more preferably 1% by weight or less.
[0088] <Method for Producing Resin Powder> The method for producing the resin powder according to the present embodiment is not particularly limited, but the resin powder can be suitably produced by preparing an aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) and spray-drying the aqueous dispersion.
[0089] The aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) can be prepared by adding the thermoplastic resin (A) to the aqueous dispersion of the crosslinked resin particles (B). The aqueous dispersion of the crosslinked resin particles (B) can be produced as described above.
[0090] The thermoplastic resin (A) to be added to the aqueous dispersion of the crosslinked resin particles (B) may be in the form of a powder or an aqueous dispersion of the thermoplastic resin (A).
[0091] The volume average particle diameter of the thermoplastic resin (A) in the aqueous dispersion is preferably in the range of 0.1 μm to 10 μm. By using a thermoplastic resin (A) having such a particle diameter, a resin powder having a particle diameter within the specific range according to this embodiment can be suitably produced. The lower limit of the particle diameter is preferably 0.1 μm or more, more preferably 0.3 μm or more, and even more preferably 0.5 μm or more. The upper limit of the particle diameter is preferably 8 μm or less, more preferably 5 μm or less.
[0092] Furthermore, when powdered thermoplastic resin (A) is added to an aqueous dispersion of crosslinked resin particles (B), the volume average particle diameter of the thermoplastic resin (A) after addition is preferably in the range of 0.1 μm or more and 10 μm or less, as described above.
[0093] The aqueous dispersion of the thermoplastic resin (A) may be an emulsion. The production method thereof is not particularly limited, and may be, for example, produced by dissolving the resin in a solvent by heating, followed by crystallization, and then pulverizing the resultant by high-speed stirring with glass beads (see, for example, paragraph
[0008] of JP-A No. 9-78494), by mixing and kneading a molten resin with an aqueous solution of a surfactant (see, for example, paragraph
[0006] of JP-A No. 11-92712 and paragraph
[0006] of JP-A No. 2001-354841), or by freeze-pulverizing the resin and then dispersing it in water.
[0094] Furthermore, when the thermoplastic resin (A) is a PHA, the aqueous dispersion of the thermoplastic resin (A) may be an aqueous dispersion obtained by culturing a PHA-producing microorganism to accumulate the PHA in the cells, and then disrupting the cells in the culture solution to separate and remove the cell components, or an aqueous dispersion obtained by concentrating or diluting the aqueous dispersion.
[0095] The aqueous medium contained in the aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) may be water alone or a mixed solvent of water and a water-compatible organic solvent. In the mixed solvent, the concentration of the water-compatible organic solvent is not particularly limited as long as it is equal to or lower than the solubility in water of the organic solvent used.
[0096] The organic solvent is not particularly limited, but examples thereof include alcohols such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, pentanol, hexanol, and heptanol; ketones such as acetone and methyl ethyl ketone; ethers such as tetrahydrofuran and dioxane; nitriles such as acetonitrile and propionitrile; amides such as dimethylformamide and acetamide; dimethyl sulfoxide, pyridine, and piperidine. Among these, methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-butanol, isobutanol, acetone, methyl ethyl ketone, tetrahydrofuran, dioxane, acetonitrile, and propionitrile are preferred because they are easily removable. Furthermore, methanol, ethanol, 1-propanol, 2-propanol, butanol, and acetone are more preferred because they are easily available. Furthermore, methanol, ethanol, and acetone are particularly preferred.
[0097] The water content in the entire aqueous medium contained in the aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) is preferably 5% by weight or more, more preferably 10% by weight or more, more preferably 30% by weight or more, even more preferably 50% by weight or more, and particularly preferably 70% by weight or more. It may be 90% by weight or more, or even 95% by weight or more. There is no particular upper limit, and it may be 100% by weight or less.
[0098] The total concentration of the thermoplastic resin (A) and the crosslinked resin particles (B) in the aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) is not particularly limited, but is preferably 20% by weight or more, more preferably 30% by weight or more, and even more preferably 40% by weight or more, because this is economically advantageous in terms of drying utility and improves productivity. Furthermore, the upper limit of the total concentration is preferably 65% by weight or less, more preferably 60% by weight or less, in order to ensure the fluidity of the aqueous dispersion. The method for adjusting the total concentration is not particularly limited, and examples include adding an aqueous medium and removing a portion of the aqueous medium (for example, by centrifuging and then removing the supernatant).
[0099] The pH of the aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) is preferably adjusted to 8 or less, more preferably 7 or less, and more preferably 6 or less, as necessary, in order to suppress a decrease in the molecular weight of the resin component, for example, during spray drying and during processing steps after drying. Furthermore, the lower limit of the pH is preferably 1 or more, more preferably 2 or more, and even more preferably 3 or more, from the viewpoint of the acid resistance of the container. The method for adjusting the pH is not particularly limited, and examples thereof include a method of adding an acid. The acid is not particularly limited, and may be either an organic acid or an inorganic acid. More specifically, examples of the acid that can be used include sulfuric acid, hydrochloric acid, phosphoric acid, and acetic acid.
[0100] The aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) may contain, within the scope of the invention, one or more of the following: dispersants or emulsifiers, pH adjusters, inorganic fillers, colorants such as pigments and dyes, odor absorbers such as activated carbon and zeolite, fragrances such as vanillin and dextrin, plasticizers, antioxidants, weather resistance improvers, UV absorbers, crystal nucleating agents, lubricants, release agents, water repellents, antibacterial agents, sliding property improvers, etc. Furthermore, the aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B) may contain various components resulting from the process of the production method, within the scope of the invention.
[0101] In an aqueous dispersion containing a thermoplastic resin (A) and crosslinked resin particles (B), the thermoplastic resin (A), the crosslinked resin particles (B), and the aqueous medium are the main components. Specifically, the total proportion of the thermoplastic resin (A) and the crosslinked resin particles (B) relative to the total solid content of the aqueous dispersion may typically be 60 to 100 wt %, 80 to 100 wt %, 90 to 100 wt %, 95 to 100 wt %, or 99 to 100 wt %. The upper limit may be 99 wt % or less, or 95 wt % or less.
[0102] The resin powder according to this embodiment can be suitably produced by spray-drying the aqueous dispersion containing the thermoplastic resin (A) and crosslinked resin particles (B) described above. Examples of spray-drying methods include a method in which the aqueous dispersion is supplied as fine droplets into a dryer and dried while coming into contact with hot air in the dryer. The method for supplying the aqueous dispersion in the form of fine droplets into the dryer (atomizer) is not particularly limited, and known methods such as a method using a rotating disk or a method using a nozzle can be used. The method for contacting the droplets with the hot air in the dryer is not particularly limited, and examples include a co-current method, a counter-current method, and a combination of these.
[0103] The drying temperature during spray drying may be any temperature that can remove most of the aqueous medium from the droplets of the aqueous dispersion. The drying temperature can be appropriately set under conditions that allow drying to the desired moisture content and minimize the occurrence of quality deterioration (reduction in molecular weight, color tone, etc.), melting, etc. For example, the temperature of the hot air blown into the spray dryer can be appropriately selected within the range of 40 to 300°C. The volume of hot air blown into the dryer can also be appropriately set depending on, for example, the size of the dryer.
[0104] <Applications of Resin Powder> The applications of the resin powder according to this embodiment are not particularly limited, and the resin powder can be used in applications in which conventionally known crosslinked resin particles are used. Specific examples include, but are not limited to, resin modifiers, rheology adjusters for paints or adhesives, paint pigments, paper coating agents, matting agents, antiblocking agents, cosmetic additives, toner additives, liquid crystal spacers, coating agents, fillers for adhesive tapes, fiber processing agents, test particles for medical diagnosis, and fillers.
[0105] The resin powder according to this embodiment may be processed into articles other than the powder. Such articles are not particularly limited, but include, for example, granules and the molded articles described below. Therefore, one aspect of the present disclosure also encompasses a resin composition containing a thermoplastic resin (A) and crosslinked resin particles (B), wherein the crosslinked resin particles (B) contain a polyhydroxyalkanoate resin and have a gel fraction of 50% or more. Details of the thermoplastic resin (A) and the crosslinked resin particles (B) and the content ratios of the two components may follow the descriptions above.
[0106] The shape of the granules obtained by processing the resin composition according to the present disclosure is not particularly limited, and may be, for example, approximately spherical, flat, cubic, spindle-shaped, needle-shaped, etc. The median diameter of the granules is not particularly limited, and may be, for example, about 1 mm to 10 mm. The granules may be in the form of pellets.
[0107] When the resin powder according to the present embodiment is processed into granules, there are advantages in that it prevents classification when mixing with other thermoplastic resins described below in pellet form, and prevents clinging to the screw in a kneader. Examples of manufacturing methods for processing the resin powder according to the present embodiment into granules include, but are not limited to, a method in which the resin powder is melted and extruded using an extruder and then cut with a blade.
[0108] Furthermore, a molded article can also be produced from the resin powder according to this embodiment. The molded article is expected to have improved mechanical properties such as impact resistance due to the inclusion of crosslinked resin particles (B). A molded article may be produced using the resin powder according to this embodiment alone, or may be produced after mixing with optional additives and / or other thermoplastic resins. When mixing with optional additives and other thermoplastic resins, it is preferable to produce a molded article after obtaining a thermoplastic resin composition by a melt-kneading step.
[0109] The thermoplastic resin composition can be produced by a known method. Specifically, the resin powder according to the present embodiment, and any additives and / or other thermoplastic resins can be melt-kneaded using an extruder, kneader, Banbury mixer, kneading roll, or the like. When melt-kneading, it is preferable to mix the components while taking care to avoid a decrease in molecular weight due to thermal decomposition. Alternatively, the thermoplastic resin composition can be produced by dissolving each component in a soluble solvent and then removing the solvent.
[0110] As the other thermoplastic resin, the resins exemplified for the thermoplastic resin (A) can be used. The same resin as the thermoplastic resin (A) may be used, or a different resin may be used. In addition, the optional additive may contain the resin powder according to this embodiment, or the additives described above may be used.
[0111] When the composition is produced by melt kneading, each component may be charged separately into an extruder or the like, or each component may be mixed in advance and then charged into an extruder or the like.
[0112] When melt-kneaded using an extruder, the obtained thermoplastic resin composition may be extruded into a strand shape and then cut to be processed into particle shapes such as a bar shape, a cylindrical shape, an elliptical cylindrical shape, a sphere shape, a cube shape, a rectangular parallelepiped shape, or the like.
[0113] The resin temperature during melt-kneading cannot be generally specified because it depends on the melting point, melt viscosity, etc. of the resin used. However, from the viewpoint of uniformly dispersing the crosslinked resin particles (B) while avoiding thermal decomposition of the thermoplastic resin (A) and the other thermoplastic resins, the temperature is preferably 140 to 250°C, more preferably 150 to 230°C, and even more preferably 160 to 220°C.
[0114] The molding method is not particularly limited, and commonly used molding methods can be applied, specifically including inflation film molding, extrusion blow molding, injection blow molding, extrusion molding, calendar molding, vacuum forming, injection molding, etc. By these molding methods, for example, sheets, films, blow molded products, extrusion molded products, vacuum molded products, and injection molded products can be produced.
[0115] Molded articles formed from the resin powder according to this embodiment can be suitably used in the fields of agriculture, fisheries, forestry, horticulture, medicine, hygiene products, the food industry, clothing, non-clothing, packaging, automobiles, building materials, and other fields.
[0116] The following items list preferred embodiments of the present disclosure, but the present invention is not limited to them. [Item 1] A resin powder having a median diameter of 20 to 1000 μm, the resin powder containing a thermoplastic resin (A) and crosslinked resin particles (B), the crosslinked resin particles (B) containing a polyhydroxyalkanoate-based resin, having a gel fraction of 50% or more and a volume average particle diameter of 0.1 μm or more and 10 μm or less. [Item 2] The resin powder according to Item 1, wherein the content of the crosslinked resin particles (B) is 10 to 90 wt % of the total of the thermoplastic resin (A) and the crosslinked resin particles (B). [Item 3] The resin powder according to Item 1 or 2, wherein the polyhydroxyalkanoate-based resin is a poly(3-hydroxyalkanoate)-based resin. [Item 4] The resin powder according to any one of Items 1 to 3, wherein the crosslinked resin particles (B) are crosslinked using a peroxide. [Item 5] The resin powder according to Item 4, wherein the crosslinked resin particles (B) are further crosslinked in the presence of a polyfunctional compound. [Item 6] The resin powder according to any one of Items 1 to 5, wherein the proportion of the polyhydroxyalkanoate-based resin in the crosslinked resin particles (B) is 80% by weight or more. [Item 7] The resin powder according to any one of Items 1 to 6, wherein the thermoplastic resin (A) contains a biodegradable resin. [Item 8] The resin powder according to Item 7, wherein the biodegradable resin is a polyester-based resin. [Item 9] A method for producing the resin powder according to any one of Items 1 to 8, comprising the steps of: preparing an aqueous dispersion containing the thermoplastic resin (A) and the crosslinked resin particles (B); and spray-drying the aqueous dispersion.
[0117] The present invention will be explained in more detail below with reference to examples, but the present invention is not limited to these examples in any way.
[0118] [1] Measurement conditions 1-1. Weight average molecular weight The resin to be measured was dissolved in chloroform and heated in a hot water bath at 60°C for 30 minutes. The soluble matter was filtered through a disposable PTFE filter with a 0.45 μm pore size. The filtrate was then subjected to GPC measurement under the following conditions to determine the weight average molecular weight. GPC measurement device: High performance liquid chromatograph 20A system manufactured by Shimadzu Corporation Column: K-G 4A (1 column), K-806M (2 columns) manufactured by Showa Denko K.K. Sample concentration: 1 mg / ml Free liquid: chloroform solution Free liquid flow rate: 1.0 ml / min Sample injection amount: 100 μL Analysis time: 30 minutes Standard sample: standard polystyrene
[0119] 1-2. Volume average particle diameter The volume average particle diameter of the crosslinked resin particles or uncrosslinked resin particles was measured in the state of resin particle latex. The measuring device used was a Microtrac MT3300EXII manufactured by Nikkiso Co., Ltd.
[0120] 1-3. Gel Fraction Dried crosslinked resin particles were added to chloroform to a concentration of 0.7% by weight, and dissolved at 60°C for 30 minutes to obtain a chloroform solution. After allowing to stand at room temperature for 3 hours, the chloroform solution was filtered through a membrane filter with a pore size of 0.45 μm. Losses were prevented by pouring chloroform over the inside of the container and the filter multiple times to thoroughly wash the solution while filtering. The gel remaining on the filter was dried, and its weight was measured together with the filter, and the gel fraction was calculated using the following formula: Formula: Gel fraction = (weight of filter including dried gel - weight of filter only) / weight of crosslinked resin particles used in measurement x 100 (%)
[0121] [2] Raw materials for crosslinked resin particles 2-1. Uncrosslinked resin particles Poly(3-hydroxybutyrate-co-3-hydroxyhexanoate): (3-hydroxybutyrate) / (3-hydroxyhexanoate)=72 / 28 (mol / mol), weight average molecular weight Mw: 500,000 to 1,500,000, volume average particle size: 1.7 μm 2-2. Peroxide Di-sec-butyl peroxydicarbonate ("Luperox 225" manufactured by Arkema Yoshitomi Co., Ltd., 1-hour half-life temperature: 69°C) 2-3. Polyfunctional compound Triallyl isocyanurate
[0122] [3] Method for Preparing an Aqueous Dispersion of Crosslinked Resin Particles (B) An autoclave equipped with a stirrer, baffles, a nitrogen inlet / outlet, and a thermometer was charged with an aqueous dispersion of uncrosslinked resin particles (100 parts by weight in terms of solids), 200 parts by weight of deionized water, 2 parts by weight of peroxide, 2 parts by weight of sodium dioctyl sulfosuccinate, and 0.5 parts by weight of a polyfunctional compound. Stirring was initiated at room temperature, and the autoclave was simultaneously purged with nitrogen. The contents of the autoclave were then stirred at room temperature for 1 hour to allow the peroxide and polyfunctional compound to penetrate the uncrosslinked resin particles. The temperature was then raised to the reaction temperature of 75°C. After reaching the reaction temperature, the mixture was allowed to react at the reaction temperature for 3.5 hours, yielding an aqueous dispersion of crosslinked resin particles (B) dispersed in water. The volume average particle diameter of the crosslinked resin particles (B) in the aqueous dispersion was measured by the above-described method and found to be 1.7 μm. After adjusting the pH of the aqueous dispersion, the dispersion was dried in an oven to obtain solidified crosslinked resin particles (B). The gel fraction of the particles was measured by the above-mentioned method and found to be 95%.
[0123] [4] Method for preparing aqueous dispersion for drying (a) Aqueous dispersion of thermoplastic resin (A) (solid content concentration 50%) Thermoplastic resin (A): poly(3-hydroxybutyrate-co-3-hydroxyhexanoate) (manufactured by Kaneka Corporation, Kaneka Biodegradable Polymer PHBH (registered trademark)), (3-hydroxybutyrate) / (3-hydroxyhexanoate)=94.4 / 5.6 (mol / mol), weight average molecular weight Mw: 530,000, volume average particle size: 2.2 μm Aqueous dispersion in which 1 part by weight of ethylene oxide / propylene oxide copolymer nonionic dispersant (molecular weight of polyethylene oxide: 8000, molecular weight of polypropylene oxide: 2000, Pronon 208 manufactured by NOF Corporation) was added per 100 parts by weight of thermoplastic resin (A) (b) Aqueous dispersion of the above-mentioned crosslinked resin particles (B) (solid content concentration 25%)
[0124] The aqueous dispersion (a) and the aqueous dispersion (b) were mixed in the ratio (based on the solid content weight) shown in Table 1, and the mixture was heated to about 50 to 55°C. The pH was then adjusted to a stable pH of 3.8 to obtain a mixed aqueous dispersion.
[0125] [5] Spray Drying Method The mixed aqueous dispersion obtained as described above was spray dried using an L-8 type spray dryer manufactured by Okawara Chemical Engineering Co., Ltd. under the conditions shown in Table 1 to obtain a resin powder containing the thermoplastic resin (A) and crosslinked resin particles (B).
[0126] The median diameter of the resin powder obtained by spray drying was measured in a dry state by a laser diffraction / scattering method using an LMS-3000 manufactured by Seishin Enterprise Co., Ltd. The results are shown in Table 1.
[0127] (Oven Drying Method) The mixed aqueous dispersion obtained as described above was placed in an oven at 55° C. for 24 hours or more to thoroughly evaporate the water, and a rubber-like sheet with poor handleability was obtained.
[0128]
[0129] It can be seen from Examples 1 to 3 in Table 1 that a resin powder containing a thermoplastic resin (A) and crosslinked resin particles (B) was obtained by spray-drying an aqueous dispersion containing a thermoplastic resin (A) and crosslinked resin particles (B). The resin powder obtained in each Example had good handleability.
[0130] In Comparative Example 1 (not shown in the table), spray drying of an aqueous dispersion containing only crosslinked resin particles (B) was attempted, but the resin particles adhered to the inner wall of the spray dryer while agglomerating, making recovery difficult, and it was impossible to obtain a resin powder like that obtained in each Example. This shows that the crosslinked resin particles (B) have extremely high adhesion and agglomeration properties and are difficult to recover as a powder alone.
Claims
1. A resin powder having a median diameter of 20 to 1000 μm, the resin powder comprising a thermoplastic resin (A) and crosslinked resin particles (B), the crosslinked resin particles (B) comprising a polyhydroxyalkanoate resin, a gel fraction of 50% or more, and a volume average particle diameter of 0.1 μm or more and 10 μm or less.
2. The resin powder according to claim 1, wherein the content of the crosslinked resin particles (B) in the total of the thermoplastic resin (A) and the crosslinked resin particles (B) is 10 to 90% by weight.
3. The resin powder according to claim 1 or 2, wherein the polyhydroxyalkanoate resin is a poly(3-hydroxyalkanoate) resin.
4. The resin powder according to claim 1 or 2, wherein the crosslinked resin particles (B) are crosslinked using a peroxide.
5. The resin powder according to claim 4, wherein the crosslinked resin particles (B) are further crosslinked in the presence of a polyfunctional compound.
6. The resin powder according to claim 1 or 2, wherein the proportion of the polyhydroxyalkanoate resin in the crosslinked resin particles (B) is 80% by weight or more.
7. The resin powder according to claim 1 or 2, wherein the thermoplastic resin (A) comprises a biodegradable resin.
8. The resin powder according to claim 7, wherein the biodegradable resin is a polyester-based resin.
9. A method for producing the resin powder according to claim 1 or 2, comprising the steps of: preparing an aqueous dispersion containing a thermoplastic resin (A) and crosslinked resin particles (B); and spray-drying the aqueous dispersion.
Citation Information
Patent Citations
Composition for aqueous paper coating and coated paper obtained by coating of the same composition
JP1997078494A
Aqueous dispersion of biodegradable polyester
JP2001354841A
Vinylic crosslinked resin particle, its manufacturing method and use thereof
JP2003082191A
Matt acrylic resin film having improved design flexibility after being coated
JP2009056770A
Expanded polyhydroxyalkanoate resin bead, molded object thereof, and process for producing the expanded resin bead
WO2007049694A1
Cited By
Aqueous dispersion
JP2026134088A
Thermoplastic resin composition and use thereof
WO2025075117A1
Thermoplastic resin composition
WO2025075123A1
Molded film or molded sheet
WO2025075124A1