Glass cloth, prepreg, and printed wiring board

By regulating the blocking dispersion number in glass cloths, the issue of uneven resin impregnation in glass cloths is resolved, ensuring consistent adhesion and efficiency in prepreg production.

WO2024203751A1PCT designated stage expired Publication Date: 2024-10-03NITTO BOSEKI CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011104
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-21
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional glass cloths with warp glass strands coated with a protective agent exhibit uneven resin impregnation times, leading to reduced adhesion between the glass cloth and resin, affecting insulation reliability and manufacturing efficiency in prepreg production.

Method used

A glass cloth with a controlled blocking dispersion number between 0.027 and 0.077, achieved by optimizing the arrangement and drying of glass filaments, ensures uniform resin impregnation times and improved adhesion without compromising production efficiency.

Benefits of technology

The controlled blocking dispersion number in the glass cloth results in uniform resin impregnation, enhancing adhesion between the glass cloth and resin, thereby improving insulation reliability and maintaining manufacturing efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011104_03102024_PF_FP_ABST
    Figure JP2024011104_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The present invention addresses the problem of providing a glass cloth with which it is possible to suppress the uneven impregnation time of a resin into a glass strand for warp and obtain excellent adhesion between the glass cloth and the resin without deteriorating the production efficiency of a prepreg when producing the prepreg. This glass cloth is provided with, as warps and wefts, a glass strand 1 comprising a plurality of glass filaments 2, and the number of blocking dispersions represented by formula (1) is in the range of 0.027-0.077. Formula (1): |Bmax-Bmin| / N, where Bmax represents the maximum value of the blocking count and B min represents the minimum value of the blocking count when the glass strand for warps is divided into a left-side region, a center region, and a right-side region that have even widths in the yarn width direction of the glass strand for warps and blocking counts are measured in the respective regions, and N represents the number of glass filaments included in the glass strand for warps.
Need to check novelty before this filing date? Find Prior Art

Description

Glass cloth, prepreg and printed wiring board

[0001] The present invention relates to a glass cloth, a prepreg, and a printed wiring board.

[0002] Conventionally, warp glass strands used as the warp threads of glass cloth have been coated with a warp protective agent to prevent damage due to contact with a reed or heald during weaving (see, for example, Patent Document 1).

[0003] Japanese Unexamined Patent Publication No. 7-102483

[0004] However, glass cloth woven using warp glass strands coated with the warp protective agent has the disadvantage that the time it takes for the resin to completely penetrate the warp glass strands locally (hereinafter sometimes referred to as the impregnation time) is uneven. When producing a prepreg by impregnating a glass cloth containing warp glass strands with uneven impregnation times with resin, if the time for immersing the glass cloth in resin is matched to the portion of the warp glass strands in the glass cloth with a short impregnation time, the adhesion between the resin and the portion of the warp glass strands in the glass cloth with a long impregnation time will be reduced. Even a partial decrease in adhesion between the glass cloth and the resin is one of the factors that reduces the insulation reliability of the entire prepreg containing the glass cloth. On the other hand, if the time for immersing the glass cloth in resin is matched to the portion of the warp glass strands with a long impregnation time, the time required for prepreg production will be extended, resulting in a decrease in production efficiency.

[0005] An object of the present invention is to provide a glass cloth that can eliminate such inconveniences and can prevent the impregnation time of the warp glass strands with the resin from becoming uneven.

[0006] The present inventors investigated the reason why the resin impregnation time of the warp glass strands becomes locally non-uniform in glass cloth woven using warp glass strands coated with the warp protective agent. As a result, the present inventors discovered that, in warp glass strands coated with the warp protective agent, regions called "blocking" occur in the glass filaments constituting the warp glass strands when the strands are dried, and that there is a weak correlation, although much weaker than the effect of the silane coupling agent applied to the surface of the glass cloth, between the distribution of the number of blocking regions in the warp glass strands and the insulation reliability of prepregs containing glass cloth woven using the warp strands. The blocking regions are formed when three or four glass filaments constituting the warp glass strands are in close contact with each other on their outer peripheries, and refer to regions that are tightly closed and surrounded by the outer peripheries of three or four of the glass filaments in a cross section perpendicular to the longitudinal direction of the warp glass strand.

[0007] Here, "closed without any gaps" means that, in two contacting glass filaments, the shortest distance between the outer peripheral surface of one glass filament and the outer peripheral surface of the other glass filament is less than 0.3 μm.

[0008] The present inventors have further studied the blocking and found that by setting the number of dispersed blocks in the glass cloth within a specific range, it is possible to prevent the impregnation time of the resin into the warp glass strands of the glass cloth from becoming non-uniform.

[0009] To achieve the above object, the glass cloth of the present invention is a glass cloth having glass strands each consisting of a plurality of glass filaments as warp and weft, characterized in that the blocking dispersion number, as expressed by the following formula (1), is in the range of 0.027 to 0.077. max -B min | / N ... (1) (where B maxis the maximum value of the number of blockings when the warp glass strand is divided into three regions, a left region, a center region, and a right region, each having an equal width in the width direction of the warp glass strand, and the number of blockings is measured in each region, and B min is the minimum value of the blocking number, and N is the number of glass filaments contained in the warp glass strand).

[0010] According to the glass cloth of the present invention, since the blocking dispersion number is within the above range, when the glass cloth is impregnated with a resin, it is possible to prevent the impregnation time of the warp glass strands with the resin from becoming non-uniform throughout the glass cloth. Therefore, when the glass cloth is made into a prepreg, excellent adhesion between the glass cloth and the resin can be obtained without deteriorating the production efficiency of the prepreg.

[0011] Being able to prevent the impregnation time of the warp glass strands with the resin from becoming non-uniform means that the non-uniformity in the impregnation time of the warp glass strands with the resin measured by the method described below is 1.0 minute or less.

[0012] In the glass cloth of the present invention, if the blocking dispersion number exceeds 0.077, the impregnation time of the resin into the warp glass strands becomes locally non-uniform, and when a prepreg is made, the production efficiency of the prepreg deteriorates or excellent adhesion between the glass cloth and the resin cannot be obtained. Also, in the glass cloth of the present invention, if the blocking dispersion number is less than 0.027, the glass strands tend to stick to each other, and the occurrence of fluffing and breakage during weaving cannot be suppressed.

[0013] The prepreg and printed wiring board of the present invention are characterized by containing the glass cloth of the present invention.

[0014] 1 is a schematic diagram of an electron microscope photograph showing a cross section of a glass strand for warp used in the glass cloth of the present invention.

[0015] Next, embodiments of the present invention will be described in more detail with reference to the accompanying drawings.

[0016] The glass cloth of this embodiment has glass strands made of a plurality of glass filaments as warp and weft yarns, and the blocking dispersion number, which is expressed by the following formula (1), is in the range of 0.027 to 0.077. max -B min | / N ... (1) (where B max is the maximum value of the number of blockings when the warp glass strand is divided into three regions, a left region, a center region, and a right region, each having an equal width in the width direction of the warp glass strand, and the number of blockings is measured in each region, and B min is the minimum value of the blocking number, and N is the number of glass filaments contained in the warp glass strand.

[0017] According to the glass cloth of the present embodiment, since the blocking dispersion number is within the above range, when the glass cloth is impregnated with a resin, it is possible to prevent the impregnation time of the warp glass strands with the resin from becoming uneven throughout the glass cloth. Therefore, when the glass cloth is made into a prepreg, excellent adhesion between the glass cloth and the resin can be obtained without deteriorating the production efficiency of the prepreg.

[0018] In the glass cloth of the present embodiment, the blocking dispersion number is preferably in the range of 0.045 to 0.070, and more preferably in the range of 0.055 to 0.064.

[0019] The glass cloth of this embodiment can be produced, for example, as follows.

[0020] First, glass raw materials prepared to obtain a glass composition for glass fiber having a desired composition are melted in a glass melting furnace to obtain molten glass (a melt of the glass composition for glass fiber).

[0021] In the glass cloth of the present embodiment, the glass composition for the glass fiber is not particularly limited, and examples thereof include the most commonly used E-glass composition, a high-strength, high-elasticity glass composition, a high-elasticity, easily manufacturable glass composition, and a low-dielectric-constant, low-dielectric-loss-tangent glass composition.

[0022] The E-glass composition contains SiO in the range of 52.0 to 56.0 mass % based on the total amount of glass fibers. 2 and Al in the range of 12.0 to 16.0 mass% 2 O 3 and a total of 20.0 to 25.0 mass% of MgO and CaO, and 5.0 to 10.0 mass% of B. 2 O 3 The composition includes:

[0023] The high-strength, high-elasticity glass composition contains SiO in the range of 60.0 to 70.0 mass % based on the total amount of glass fibers. 2 and Al in the range of 20.0 to 30.0 mass% 2 O 3 and MgO in the range of 5.0 to 15.0 mass % and Fe in the range of 0 to 1.5 mass %. 2 O 3 and a total of 0 to 0.2 mass% of Na 2 O.K. 2 O and Li 2 The high strength and high modulus glass composition preferably contains 0.15 to 1.50 mass % of Fe. 2 O 3 and ZrO in the range of 0.01 to 0.10 mass %. 2 and a total of 0.02 to 0.20 mass% of Na 2 O.K. 2 O and Li 2 O.

[0024] The high elastic modulus, easily manufacturable glass composition contains SiO in the range of 57.0 to 60.0 mass % based on the total amount of glass fibers. 2 and Al in the range of 17.5 to 20.0 mass% 2 O 3 8.5 to 12.0 mass% MgO, 10.0 to 13.0 mass% CaO, and 0.5 to 1.5 mass% B 2 O 3 and a total of 98.0 mass% or more of SiO 2 , Al 2 O 3 , MgO and CaO.

[0025] The low dielectric constant and low dielectric loss tangent glass composition contains SiO in the range of 48.0 to 62.0 mass % based on the total amount of glass fibers. 2 and B in the range of 17.0 to 26.0 mass% 2 O 3 and Al in the range of 9.0 to 18.0 mass% 2 O 3 0.1 to 9.0 mass% of CaO, 0 to 6.0 mass% of MgO, and 0.05 to 0.5 mass% of Na in total. 2 O.K. 2 O and Li 2 O and TiO in the range of 0 to 5.0 mass% 2 and SrO in the range of 0 to 6.0 mass %, and F in the range of 0 to 3.0 mass % in total. 2 and Cl 2 and P in the range of 0 to 6.0 mass%. 2 O 5 The composition includes:

[0026] The content of each component of the glass composition described above can be measured using an ICP optical emission spectrometer for the light element Li, and using a wavelength dispersive X-ray fluorescence analyzer for the other elements. Specifically, the content of each component of the glass composition can be measured as follows.

[0027] First, glass cloth is cut to an appropriate size, placed in a platinum crucible, and melted in an electric furnace at a temperature of 1400 to 1650°C for 6 hours while stirring, to obtain a homogeneous molten glass. If organic matter is attached to the surface of the glass cloth or if glass fibers are contained mainly as a reinforcing material in the organic matter (resin), the glass cloth is used after removing the organic matter by, for example, heating in a muffle furnace at 300 to 650°C for 2 to 24 hours.

[0028] Next, the obtained molten glass is poured onto a carbon plate to produce glass cullet, and then the glass cullet is crushed and powdered to produce glass powder. The light element Li is quantitatively analyzed using an ICP optical emission spectrometer after the glass powder is thermally decomposed with acid. The other elements are quantitatively analyzed using a wavelength dispersive X-ray fluorescence analyzer after the glass powder is molded into a disk shape using a press. The results of these quantitative analyses are converted into oxides to calculate the content and total amount of each component, and the content (mass %) of each of the aforementioned components can be determined from these values.

[0029] The molten glass is then discharged from a vessel (bushing) having a nozzle plate with several to several thousand nozzle tips formed thereon, and is cooled and solidified while being stretched by being wound up at high speed, thereby forming a glass filament (this operation is sometimes called "spinning"). The bushing is made of a noble metal such as platinum.

[0030] Here, the glass filament discharged from one nozzle tip or hole and cooled and solidified usually has a perfectly circular cross section and a diameter in the range of 3.0 to 10.0 μm.

[0031] The elastic modulus of the glass fibers constituting the glass filaments is not particularly limited, but is, for example, in the range of 40 to 120 GPa, preferably in the range of 71 to 110 GPa. Since the impregnation time for resin into warp glass strands has traditionally tended to be long, from the viewpoint of achieving a more pronounced effect of reducing unevenness in the impregnation time according to the present invention, it is more preferably in the range of 80 to 100 GPa. Furthermore, the strength of the glass fibers constituting the glass filaments is not particularly limited, but is, for example, in the range of 1.5 to 6.0 GPa, preferably in the range of 3.5 to 5.2 GPa.

[0032] The elastic modulus and strength of the glass fibers constituting the glass filaments can be measured by the method described in the Examples below.

[0033] Next, 20 to 300 of the glass filaments formed as described above are bundled by applying a sizing agent (sometimes referred to as a primary sizing agent) with an applicator, and then wound around a collet to form a glass strand (glass fiber bundle).

[0034] In the glass strand, the glass cloth obtained by weaving the glass strand tends not to be sufficiently lightweight if the fiber diameter of the glass filaments exceeds 10 μm or the number of glass filaments exceeds 300. In addition, in the glass strand, if the fiber diameter of the glass filaments is less than 3 μm, the production efficiency decreases in order to prevent the occurrence of fluffing and breakage, and if the number of glass filaments is less than 20, it tends to be difficult to suppress the occurrence of pinholes when the glass cloth obtained by weaving the glass strand is made into a prepreg.

[0035] In the glass strand, the fiber diameter of the glass filaments is preferably in the range of 3.0 to 10.0 μm, more preferably in the range of 4.8 to 9.0 μm, and even more preferably in the range of 6.0 to 8.0 μm. In addition, in the glass strand, the number of the glass filaments is preferably in the range of 20 to 300, and more preferably in the range of 120 to 250.

[0036] Next, the formed glass strands are processed into warp glass strands and weft glass strands, and a warp protective agent (sometimes referred to as a secondary sizing agent in contrast to the primary sizing agent) is applied to the warp glass strands. Examples of the warp protective agent include starch-based or PVA (polyvinyl alcohol)-based sizing agents. The warp protective agent may contain a lubricant, an emulsifier, a softener, a preservative, an antistatic agent, an organic solvent, and the like. Examples of the warp protective agent include, but are not limited to, a warp protective agent containing 5.0% by mass of polyvinyl alcohol (PVA), 1.0% by mass of starch, 0.5% by mass of paraffin wax, and 93.5% by mass of water relative to the total amount of the warp protective agent.

[0037] The amount of the warp protective agent attached to the glass cloth is preferably 0.1 to 3.0 parts by mass, more preferably 0.5 to 1.5 parts by mass, per 100 parts by mass of the glass strands.

[0038] The warp glass strands can be coated with the warp protective agent by passing the warp glass strands through a treatment tank containing a treatment solution containing the warp protective agent while adjusting the tension, and then passing the strands through a dryer at an ambient temperature of 100 to 250°C for a time of, for example, 0.1 to 1.0 minute while adjusting the line speed so as to achieve a predetermined dry strength index. The ambient temperature of the dryer is preferably in the range of 100 to 150°C, and the passage time is preferably in the range of 0.1 to 0.35 minutes. The dry strength index is expressed as the product of the drying time (minutes) and the ambient temperature of the dryer (°C), and is, for example, in the range of 25.0 to 35.0.

[0039] The warp glass strands are coated with the warp protective agent and transported while adjusting the tension, thereby loosening the arrangement of the glass filaments inside the warp strands. The subsequent drying promotes the formation of a film of the warp protective agent, thereby fixing the arrangement of the filaments and forming the blocking locally. The tension applied to the warp strands is preferably in the range of 70 to 120 N.

[0040] The blocking refers to a region that is enclosed without gaps by the outer peripheral surfaces of three or four glass filaments in a cross section perpendicular to the longitudinal direction of the glass strand.

[0041] In the warp glass strands, the higher the dry strength index, the more rapidly the warp glass strands are dried. As a result, the formation of a film of the warp protective agent on the outer edges of the warp glass strands is accelerated, and the strand shape is fixed before the arrangement of the glass filaments inside the strands is relaxed, resulting in a large number of blocks in the central portion and a large number of dispersed blocks. On the other hand, if the dry strength index is small, the warp protective agent is not dried sufficiently, causing the warp glass strands to stick together, which can cause fuzzing or breakage when the warps are pulled apart during weaving.

[0042] The weft glass strands were only coated with the bundling agent, and were not coated with any of the warp protective agents.

[0043] Next, a first glass cloth, which is one embodiment of the glass cloth of this embodiment, can be obtained by weaving the warp glass strands as warps and the weft glass strands as wefts. The weaving can be carried out using a loom known per se, such as a jet loom (e.g., an air jet or water jet loom), a shuttle loom, or a rapier loom. Examples of weaving methods used with the loom include plain weave, satin weave, sash weave, and twill weave, with plain weave being preferred from the viewpoint of production efficiency.

[0044] Next, the first glass cloth is subjected to a deoiling treatment, a surface treatment, or a fiber-opening treatment to obtain a second glass cloth, which is one embodiment of the glass cloth of the present embodiment. The order of the deoiling treatment, surface treatment, and fiber-opening treatment is not particularly limited, and any treatment may be performed first.

[0045] In the deoiling treatment, the first glass cloth is placed in a heating furnace at an atmospheric temperature in the range of 350 to 400°C for a time in the range of 40 to 80 hours, thereby thermally decomposing the sizing agent and the warp protective agent adhering to the first glass cloth.

[0046] The surface treatment can be performed by immersing the first glass cloth in a surface treatment agent solution, squeezing out excess water, and then heating and drying the resultant at a temperature in the range of 80 to 180°C for a time in the range of 1 to 30 minutes.

[0047] The surface treatment agent solution may contain a silane coupling agent, a weak acid (for example, acetic acid, citric acid, propionic acid, etc.), and a surfactant.

[0048] Examples of the silane coupling agent include aminosilane, chlorosilane, epoxysilane, mercaptosilane, vinylsilane, and (meth)acrylicsilane. In this embodiment, the silane coupling agent may be used alone or in combination of two or more.

[0049] Examples of aminosilanes include γ-aminopropyltriethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-N'-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, and γ-anilinopropyltrimethoxysilane.

[0050] Examples of chlorosilane include γ-chloropropyltrimethoxysilane.

[0051] Examples of epoxy silanes include β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane and γ-glycidoxypropyltrimethoxysilane.

[0052] Examples of mercaptosilane include γ-mercaptotrimethoxysilane.

[0053] Examples of vinylsilanes include vinyltrimethoxysilane and N-β-(N-vinylbenzylaminoethyl)-γ-aminopropyltrimethoxysilane.

[0054] Examples of (meth)acrylic silanes include γ-methacryloxypropyltrimethoxysilane.

[0055] Examples of surfactants include nonionic surfactants, cationic surfactants, anionic surfactants, and amphoteric surfactants. In this embodiment, the surfactants may be used alone or in combination of two or more.

[0056] Examples of the opening treatment include a treatment for widening the yarn width of the warp and weft yarns by applying a tension in the range of 30 to 200 N to the warp yarns of the first glass cloth while performing opening by water jet pressure, opening by high-frequency vibration using a liquid as a medium, opening by pressure of a fluid having surface pressure, opening by pressure using a roll, or the like.

[0057] In the first glass cloth or the second glass cloth, which is one embodiment of the glass cloth of this embodiment, the weave density of the warp or weft is, for example, in the range of 20 to 160 threads / 25 mm, preferably in the range of 50 to 80 threads / 25 mm. In the first glass cloth or the second glass cloth, the yarn width of the warp or weft is, for example, in the range of 80 to 600 μm, preferably in the range of 250 to 450 μm, and more preferably in the range of 300 to 400 μm. The thickness of the first glass cloth or the second glass cloth is, for example, in the range of 8 to 200 μm, preferably in the range of 70 to 170 μm, and more preferably in the range of 91 to 140 μm. The width of the first glass cloth or the second glass cloth is, for example, in the range of 800 to 2000 mm.

[0058] Furthermore, the first glass cloth or the second glass cloth, which is one of the embodiments of the glass cloth of this embodiment, has an average number of stages, defined by (filament diameter)×(number of filaments) / (yarn width), in the range of, for example, 0.6 to 4.5, preferably 2.5 to 4.0, and more preferably 3.0 to 3.8. If the average number of stages of the first glass cloth or the second glass cloth is less than 0.6, the number of blocking dispersions tends to be too small, whereas if the average number of stages exceeds 4.5, the time required for resin impregnation into the first glass cloth or the second glass cloth tends to be long.

[0059] The blocking number can be measured as follows. First, glass cloth pieces having a size of 100 mm x 100 mm are cut out from three points: a point 200 mm inward from one end in the width direction of the glass cloth, a point 200 mm inward from the other end, and a point at the center in the width direction of the glass cloth. When the width of the glass cloth is less than 800 mm, the distance from the end and the size of the glass cloth piece may be changed in proportion to the width of the glass cloth, based on a width of 1000 mm.

[0060] Next, the cut glass cloth piece is embedded in epoxy resin and the epoxy resin is cured, and the cured epoxy resin is polished to an extent that a cross section perpendicular to the length direction of the warp yarns can be observed, to prepare a test piece for measuring the number of dispersed blocking yarns. At this time, a warp glass strand located 5 mm from one end of the test piece is selected, and the polished surface of the test piece is observed under a scanning electron microscope at a magnification of 1600x.

[0061] The blocking is maintained even after the first glass cloth after weaving is subjected to the deoiling treatment, surface treatment, or fiber-opening treatment, and therefore, the number of blocking may be measured using either the first glass cloth or the second glass cloth.

[0062] Next, the case where the blocking number is measured using the second glass cloth will be described.

[0063] 1 is a copy of an electron microscope photograph showing a part of the polished surface of the test piece, showing a cross section of the second glass cloth, in which reference numeral 1 denotes a warp glass strand and reference numeral 3 denotes a weft glass strand. The warp glass strand 1 is formed by bundling a plurality of glass filaments 2.

[0064] Next, as shown in FIG. 2, the warp glass strands 1 having a thread width L are cut in the width direction of the strand cross section to have respective widths L 1 , L 2 , L 3 is uniform (L 1 =L 2 =L 3, L 1 +L 2 +L 3 The sample is divided into three regions, a left region 1a, a center region 1b, and a right region 1c, so that the distance L is equal to the distance L. The number of blocking events in each of the regions 1a, 1b, and 1c is measured. The maximum number of blocking events in the three regions 1a, 1b, and 1c is designated as B. max , the minimum value is B min , where N is the number of glass filaments 2 contained in the warp glass strand 1, |B max -B min | / N is the blocking dispersion number of the warp glass strand.

[0065] The above measurement is carried out for five adjacent warp glass strands in each of the glass cloth pieces cut out from the three points, and the number of blocking dispersions for a total of 15 warp glass strands is measured. The average value is defined as the number of blocking dispersions for the glass cloth, and the standard deviation of the number of blocking dispersions for the 15 warp glass strands is defined as the standard deviation of the number of blocking dispersions for the glass cloth.

[0066] In the first glass cloth or the second glass cloth, which is one of the embodiments of the glass cloth of the present embodiment, the standard deviation of the blocking dispersion number is preferably in the range of 0.006 to 0.070, and more preferably in the range of 0.016 to 0.022.

[0067] The prepreg or printed wiring board of this embodiment includes the first glass cloth or the second glass cloth, and a thermoplastic resin or a thermosetting resin impregnated into the first glass cloth or the second glass cloth.

[0068] In the prepreg or printed wiring board of this embodiment, the resin impregnated into the first glass cloth or the second glass cloth is not particularly limited. Examples of such resins include thermosetting resins such as epoxy resins, phenolic resins, unsaturated polyester resins, melamine resins, modified polyimide resins, thermosetting polyphenylene ether resins, and thermosetting modified polyphenylene ether resins. Examples of thermoplastic resins include polyamide resins, polyimide resins, polybutylene terephthalate resins, polyethylene terephthalate resins, polyphenylene sulfide resins, thermoplastic polyphenylene ether resins, thermoplastic modified polyphenylene ether resins, and fluororesins.

[0069] Next, examples of the present invention and comparative examples will be described.

[0070] [Example 1] First, the glass composition shown in Table 1 (65.00 mass % of SiO relative to the total amount of glass fibers) was 2 and 25.00% by mass of Al 2 O 3 9.50% by mass of MgO, 0.05% by mass of CaO, and 0.30% by mass of Fe 2 O 3 and 0.05% by mass of ZrO 2 and a total of 0.10 mass% Li 2 O, Na 2 O and K 2 O and 0.00% by mass of B 2 O 3 and 0.00% by mass of TiO 2 and 0.00% by mass of F 2 A glass strand was prepared by bundling 196 glass filaments having a circular cross section and a filament diameter of 7.0 μm. The glass filaments were made of a high-strength, high-elasticity glass composition containing

[0071] Next, a warp protective agent treatment solution was prepared containing a warp protective agent consisting of 5.0 mass% polyvinyl alcohol (PVA), 1.0 mass% starch, 0.5 mass% paraffin wax, and 93.5 mass% water relative to the total amount.

[0072] Next, the glass strands formed as described above were used as warp glass strands and weft glass strands, and the warp protective agent was applied to the warp glass strands. The operation of applying the warp protective agent to the warp glass strands was carried out by passing the warp glass strands through a treatment tank containing the warp protective agent treatment solution, and then passing the warp glass strands through a dryer in which the atmospheric temperature was in the range of 100 to 150°C, while adjusting the line speed so that the dry strength index would be 31.5.

[0073] The weft glass strands were only coated with the bundling agent, and were not coated with any of the warp protective agents.

[0074] Next, the warp glass strands were used as warp threads and the weft glass strands were used as weft threads, and the weaving was carried out using an air jet loom to obtain a plain woven first glass cloth with a warp weave density of 65 threads / 25 mm and a weft weave density of 62 threads / 25 mm.

[0075] Next, the first glass cloth was subjected to a deoiling treatment, a surface treatment, and a fiber-opening treatment to obtain a second glass cloth as the glass cloth of this example. The deoiling treatment involved placing the first glass cloth in a heating furnace at an atmospheric temperature of 350°C to 400°C for 60 hours to thermally decompose the sizing agent and warp protective agent attached to the first glass cloth. The surface treatment involved applying a silane coupling agent to the first glass cloth and curing the silane coupling agent while continuously passing the first glass cloth through a heating furnace at 130°C. The fiber-opening treatment involved applying a tension of 50 N to the warp yarns of the first glass cloth and using a water jet pressure set at 3.0 MPa. In the fiber-opening treatment, the tension value detected by a tension detector was fed back to a guide roller conveying the first glass cloth, and the tension was adjusted by changing the position of the guide roller.

[0076] The tension applied to the warp yarns of the glass cloth in the processes other than the opening treatment is in the range of 70 to 120N.

[0077] As a result of the above treatment, the second glass cloth had warp yarns with a yarn width of 372 μm and an average number of rows of 3.7, and weft yarns with a yarn width of 365 μm and an average number of rows of 3.8, and had a thickness of 96 μm. The results are shown in Table 1.

[0078] For the second glass cloth obtained in this example, the number of dispersed blocking particles was measured and the standard deviation of the number of dispersed blocking particles was calculated, and the glass fiber elastic modulus and glass fiber strength of the glass fibers constituting the second glass cloth were measured, while the resin impregnation time for the second glass cloth was also measured, all by the following methods. The results are shown in Table 1.

[0079] [Blocking Dispersion Number and Its Standard Deviation] First, glass cloth pieces each having a size of 100 mm x 100 mm were cut out from the second glass cloth at three points: one 200 mm inward from one end in the width direction, one 200 mm inward from the other end, and the center in the width direction. The cut glass cloth pieces were then embedded in epoxy resin to harden the epoxy resin, and the hardened epoxy resin was polished to an extent that a cross section perpendicular to the length direction of the warp yarns could be observed, thereby preparing a test piece for measuring the blocking dispersion number. A warp glass strand positioned 5 mm from one end of the test piece was selected, and the polished surface of the test piece was observed with a scanning electron microscope to measure the blocking number.

[0080] The number of blockings was measured by dividing the warp glass strands 1 having a width L into 1 , L 2 , L 3 is uniform (L 1 =L 2 =L 3 , L 1 +L 2 +L 3 =L), and then each of the regions 1a, 1b, and 1c is observed at a magnification of 1600 times using a scanning electron microscope.

[0081] Then, the maximum value of the number of blockings in the three regions 1a, 1b, and 1c is defined as B max , the minimum value is B min, where N is the number of glass filaments 2 contained in the warp glass strand 1, |B max -B min | / N is the blocking dispersion number of the warp glass strand.

[0082] The measurement is carried out for five adjacent warp glass strands in each of the glass cloth pieces cut out from the three points, and the number of blocking dispersions is measured for a total of 15 warp glass strands, and the average value thereof is regarded as the number of blocking dispersions of the second glass cloth.

[0083] The standard deviation of the number of blocking dispersions of the 15 warp glass strands is taken as the standard deviation of the number of blocking dispersions of the second glass cloth.

[0084] [Glass Fiber Strength] First, glass raw materials prepared to have the same glass composition as the glass fibers of the Examples and Comparative Examples were heated in a muffle furnace at 1400 to 1650°C for 0.5 to 24 hours, and the resulting molten glass was poured onto a carbon plate to produce glass cullet. Next, the resulting glass cullet was poured into a small cylindrical platinum bushing with a single circular nozzle tip at the bottom of the container, and the bushing was heated to a predetermined temperature so that the viscosity of the poured glass cullet was 1000±150 poise, melting the glass cullet and obtaining molten glass. The molten glass discharged from the nozzle tip of the platinum bushing was wound at a predetermined speed by a winder so that the glass fiber diameter was 13±2 μm, and the glass filament was cooled and solidified while being stretched, obtaining a glass filament with a true circular cross-sectional shape. A single glass filament (monofilament) was collected between the nozzle tip of the platinum bushing and the winder, and the glass filament, with deterioration due to contact and friction minimized, was collected as a sample for tensile strength evaluation. Next, the obtained glass filament is arranged in the long side direction along a line connecting the center points of the short sides of a mount having two gripping portions and two support portions, as described below, and bonded to prepare a monofilament test piece. Next, the diameter of the obtained glass filament is measured using a scanning electron microscope (Hitachi Corporation, product name: S-3400), and the cross-sectional area of ​​the glass filament is calculated from the obtained diameter. Next, the two gripping portions in the mount are set in the upper and lower gripping tools of a tensile tester (A&D Co., Ltd., product name: benchtop material testing machine STB-1225S), with the distance between the gripping tools set to 25 mm, and the two support parts in the mount are cut off, leaving the gripping parts connected only by the glass filament, and then a tensile test is performed at a crosshead speed of 5 mm / min. Next, the tensile strength is calculated by dividing the maximum load value at which the glass filament breaks by the cross-sectional area of ​​the glass filament. The monofilament test pieces in which incomplete breakage such as thread coming off or thread breaking occurred during the measurement are excluded, and the glass fiber strength is measured by calculating the average value of the tensile strength of n=30.

[0085] The backing paper has short sides of 25 mm and long sides of 50 mm, and a cutout section with a short side of 15 mm and a long side of 25 mm in the center of its interior, with the short sides and long sides of the backing paper parallel to the short sides and long sides of the cutout, respectively.A gripping section that is set in the gripping tool of a tensile testing machine is provided between the short sides of the cutout and the short sides of the backing paper, and a support section that connects and supports the two gripping sections is provided between the long sides of the cutout and the long sides of the backing paper.

[0086] [Glass Fiber Elastic Modulus] First, a tensile test of the glass filament is carried out in exactly the same manner as in the above-mentioned method for measuring the strength of the glass fiber. Next, the strain ε between two points is measured. 1 = 0.0005 and ε 2 = 0.0025, respectively. 1 , σ 2 and the difference in stress (σ 2 -σ 1 ) to the strain difference (ε 2 -ε 1 The tensile modulus is calculated by dividing the average value of the tensile modulus of the monofilament test piece (n=15) by the average value of the tensile modulus of the monofilament test piece (n=15).

[0087] [Resin Impregnation Time] First, glass cloth pieces having a size of 60 mm x 40 mm were cut out from three points of the second glass cloth, namely, a point 200 mm inward from one end in the width direction, a point 200 mm inward from the other end, and a point at the center in the width direction, to prepare test pieces for evaluating impregnation property.

[0088] Next, the test pieces for evaluating impregnation property are immersed in benzyl alcohol, and the time from immediately after immersion until the benzyl alcohol completely penetrates the test pieces for evaluating impregnation property is measured in both the warp and weft directions. Measurements are carried out using five test pieces for evaluating impregnation property at each measurement point, and the average value is calculated for each measurement point.

[0089] The difference between the maximum and minimum values ​​of the impregnation times of the warp and weft yarns at each measurement point is taken as the unevenness of the impregnation time.

[0090] Since the refractive index of the benzyl alcohol is similar to that of the glass filaments, when the impregnation evaluation test piece is immersed in benzyl alcohol, the impregnated portion appears transparent because the benzyl alcohol has penetrated between the glass filaments of the glass strand, while the unimpregnated portion appears opaque due to a difference in refractive index between the impregnated portion and the air present between the glass filaments, making it easy to visually determine whether the impregnation has occurred.

[0091] [Example 2] In this example, a glass composition for glass fiber was prepared using the glass composition shown in Table 1 (54.60 mass % of SiO relative to the total amount of glass fiber). 2 and 14.10% by mass of Al 2 O 3 1.20% by mass of MgO, 22.40% by mass of CaO, and 0.20% by mass of Fe 2 O 3 and 0.00 mass% ZrO 2 and a total of 0.50 mass% Li 2 O, Na 2 O and K 2 O and 6.10 mass% B 2 O 3 and 0.30% by mass of TiO 2 and 0.60% by mass of F 2 A glass strand was prepared by bundling 41 glass filaments each having a filament diameter of 4.0 μm and made of an E-glass composition containing

[0092] Next, a first plain-woven glass cloth was obtained in exactly the same manner as in Example 1, except that the glass strands formed as described above were used as warp glass strands and weft glass strands, and the weaving density of the warp and weft was 95 strands / 25 mm.

[0093] Next, the first glass cloth was subjected to a deoiling treatment, a surface treatment and a fiber-opening treatment in exactly the same manner as in Example 1, except that the water pressure in the fiber-opening treatment was set to 1.0 MPa, to obtain a second glass cloth as the glass cloth of this example.

[0094] The second glass cloth of this example had warp yarns with a yarn width of 120 μm and an average number of rows of 1.4, and weft yarns with a yarn width of 185 μm and an average number of rows of 0.9, and had a thickness of 13 μm. The results are shown in Table 1.

[0095] Next, except that the second glass cloth obtained in this example was used, the number of dispersed blocking particles was measured, the standard deviation of the number of dispersed blocking particles was calculated, the glass fiber elastic modulus and glass fiber strength of the glass fibers constituting the second glass cloth were measured, and the resin impregnation time into the second glass cloth was also measured, all in the same manner as in Example 1. The results are shown in Table 1.

[0096] [Comparative Example 1] In this comparative example, a second glass cloth was obtained as the glass cloth of this comparative example in exactly the same manner as in Example 1, except that the line speed was adjusted so that the dry strength index in the operation of applying the warp protective agent to the warp glass strands was 40.9.

[0097] The second glass cloth of this comparative example had warp yarns with a yarn width of 374 μm and an average number of rows of 3.7, and weft yarns with a yarn width of 360 μm and an average number of rows of 3.8, and had a thickness of 96 μm. The results are shown in Table 1.

[0098] Next, except that the second glass cloth obtained in this comparative example was used, the number of dispersed blocking particles was measured, the standard deviation of the number of dispersed blocking particles was calculated, the glass fiber elastic modulus and glass fiber strength of the glass fibers constituting the second glass cloth were measured, and the resin impregnation time into the second glass cloth was also measured, all in the same manner as in Example 1. The results are shown in Table 1.

[0099]

[0100] From Table 1, it is clear that, according to the glass cloths of Examples 1 and 2, the blocking dispersion number was in the range of 0.027 to 0.077, so that the variation in the resin impregnation time for the warp glass strands was 1.0 minute or less, and that the non-uniformity of the impregnation time could be suppressed. On the other hand, in the glass cloth of Comparative Example 1, the impregnation times for the warp glass strands and weft glass strands at the cross ends were equivalent to those of Example 1, and the non-uniformity of the weft impregnation time was 1.0 minute or less, but the blocking dispersion number was 0.094, which is greater than 0.077, so that the non-uniformity of the resin impregnation time for the warp glass strands was 1.5, which was larger than that of the glass cloths of Examples 1 and 2, and that the non-uniformity of the impregnation time was evident.

Claims

1. A glass cloth having glass strands made of a plurality of glass filaments as warp and weft threads, characterized in that the blocking dispersion number represented by the following formula (1) is in the range of 0.027 to 0.

077. | B max -B min | / N ... (1) (where B max is the maximum value of the number of blockings when the warp glass strand is divided into three regions, a left region, a center region, and a right region, so that the regions have an equal width in the yarn width direction of the warp glass strand, and the number of blockings is measured in each region, and B is the maximum value of the number of blockings when the number of blockings is measured in each region. min is the minimum value of the blocking number, and N is the number of glass filaments contained in the warp glass strand.

2. A prepreg comprising the glass cloth according to claim 1.

3. A printed wiring board comprising the glass cloth according to claim 1.

Citation Information

Patent Citations

  • Glass cloth for laminate, and laminate

    JP1989249333A

  • Glass fiber woven fabric for laminate, its production and laminate using the same

    JP1997324340A

  • Glass cloth made from zero-twisted yarn

    JP1997503256A