Rubber composition, vulcanization molded body, and rubber roll
The rubber composition, with a focus on chloroprene-based polymers and specific additives, addresses the water and alkali resistance issues in conventional rubber compositions, providing enhanced performance for industrial applications.
Patent Information
- Application Number
- PCT/JP2024/011249
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional rubber compositions lack adequate water resistance and alkali resistance in vulcanized products, limiting their applications in harsh environments.
A rubber composition based on a laminate structure with a chloroprene rubber polymer, optimized with specific formulations and processing conditions to achieve enhanced water resistance and alkali resistance, including the use of chloroprene homopolymers or copolymers, unsaturated nitrile monomers, and selected additives, which satisfy specific hardness and heat generation relationships.
The resulting vulcanized molded products exhibit excellent water resistance and alkali resistance, enabling their use in applications such as acid and alkali cleaning lines, and other industrial settings where conventional rubber compositions fail.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure JPOXMLDOC01-APPB-T000003
Abstract
Description
Rubber composition, vulcanized molded product, and rubber roll
[0001] The present invention relates to a rubber composition, a vulcanized molded article, and a rubber roll.
[0002] Rubber products are widely used as materials for general industrial transmission belts and conveyor belts, automotive air springs, vibration-proof rubber, hoses, wipers, immersion products, sealing parts, adhesives, boots, rubber-coated fabrics, rubber rolls, etc.
[0003] For example, Patent Document 1 discloses an invention relating to a sulfur-modified chloroprene rubber composition comprising a sulfur-modified chloroprene rubber, a vulcanization accelerator, zinc oxide, and magnesium oxide, wherein the blending amount of the vulcanization accelerator is 0.1 to 5 parts by weight, and the blending amounts of zinc oxide and magnesium oxide are specified by a predetermined relationship between each blending amount and the Mooney scorch time t. Also, Patent Document 2 discloses an invention relating to a copolymer of a chloroprene monomer and an unsaturated nitrile compound, which has a Mooney viscosity ML(1+4)100°C of 20 to 80 and has a functional group with a specific structure.
[0004] Japanese Patent Application Laid-Open No. 11-209522 International Publication No. 2020 / 044899
[0005] However, conventional rubber compositions have room for improvement in the water resistance and alkali resistance of vulcanized molded articles of the compositions.
[0006] The present invention has been made in view of the above circumstances, and provides a rubber composition that can give a vulcanized molded article having excellent water resistance and alkali resistance.
[0007] According to the present invention, there is provided a rubber composition containing a rubber component, wherein test vulcanized molded articles 1 of the rubber composition are stacked to a thickness of 6.0 mm or more to form a laminate, and the hardness thereof is measured with a Type A durometer in accordance with JIS K 6253-3:2023 as X, and test vulcanized molded articles 2 of the rubber composition are evaluated in a constant strain flexometer test in accordance with JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and frequency of 1,800 vibrations per minute as Y, where X is the hardness, and Y is the heat generated by the test vulcanized molded articles 1 of the rubber composition measured with a Type A durometer in accordance with JIS K 6253-3:2023 as Y. 6299:2012, and the test vulcanized molded body 2 is a cylindrical vulcanized molded body having a diameter of 15 mm and a height of 25 mm obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes.
[0008] As a result of extensive research, the present inventors have discovered that by adjusting the formulation of a rubber composition so that a specific relationship is satisfied between the hardness X of a test vulcanized molded product 1 of the rubber composition and the heat generation Y of a test vulcanized molded product 2 of the rubber composition, a rubber composition can be obtained that can give a vulcanized molded product with excellent water resistance and alkali resistance, and have thus completed the present invention.
[0009] Various embodiments of the present invention will be described below as examples, and the embodiments shown below can be combined with each other.
[0010] [1] A rubber composition containing a rubber component, wherein test vulcanized molded articles 1 of the rubber composition are stacked to a thickness of 6.0 mm or more, and the hardness thereof is measured with a type A durometer in accordance with JIS K 6253-3:2023 as X. Test vulcanized molded articles 2 of the rubber composition are evaluated in a constant strain flexometer test in accordance with JIS K 6265:2018 under the conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and frequency of 1,800 vibrations per minute as Y. The hardness X and heat generation Y satisfy the following formula (1), and the test vulcanized molded articles 1 are obtained by stacking the rubber composition in accordance with JIS K 6299:2012, and the test vulcanization molded article 1 is a 2 mm thick sheet-like vulcanization molded article obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes in accordance with the method of the present invention. The test vulcanization molded article 2 is a cylindrical vulcanization molded article having a diameter of 15 mm and a height of 25 mm obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes. 1.4X-Y>45.0 (1) [2] The rubber composition according to [1], wherein the hardness X is 40 or more and 98 or less. [3] The rubber composition according to [1] or [2], wherein the rubber component contains a chloroprene-based polymer. [4] The rubber composition according to [3], wherein the chloroprene-based polymer contains 80 to 100% by mass of chloroprene monomer units relative to 100% by mass of the chloroprene-based polymer. [5] A vulcanization molded article of the rubber composition according to any one of [1] to [4]. [6] A rubber roll comprising a core and a surface layer provided on the peripheral surface of the core, the surface layer including the vulcanized molded article according to [5], the rubber roll being used in at least one of an acid washing line and an alkali washing line. [7] A vulcanized molded article containing a rubber component, wherein when the vulcanized molded article is made into a test vulcanized molded article 1' having a thickness of 6.0 mm or more, X' is the hardness measured with a Type A durometer in accordance with JIS K 6253-3:2023, and when the vulcanized molded article is made into a cylindrical test vulcanized molded article 2' having a diameter of 15 mm and a height of 25 mm, Y' is the heat generated by evaluation in a constant strain flexometer test in accordance with JIS K 6265:2018 under conditions of 40°C, a strain of 0.175 inches, a load of 55 pounds, and a frequency of 1,800 cycles per minute, where X' and Y' satisfy the following formula (2):1.4X'-Y'>45.0 (2).
[0011] The rubber composition according to the present invention can provide a vulcanized molded article having excellent water resistance and alkali resistance. Furthermore, since the vulcanized molded article according to the present invention has excellent water resistance and alkali resistance, these properties can be utilized to find applications in various components that require water resistance and / or alkali resistance, such as rubber rolls. The rubber roll according to one embodiment of the present invention has excellent water resistance and alkali resistance, and can be used, for example, as a rubber roll for at least one of an acid washing line and an alkali washing line.
[0012] The present invention will be described in detail below by illustrating embodiments of the present invention. The present invention is not limited by these descriptions. The features of the embodiments of the present invention described below can be combined with each other. Furthermore, each feature can be an invention independently.
[0013] 1. Rubber Composition The rubber composition according to the present invention contains a rubber component.
[0014] 1.1 Rubber Component The rubber component according to the present invention may contain at least one selected from chloroprene rubber, natural rubber (NR), hydrogenated acrylonitrile butadiene rubber (H-NBR), acrylonitrile butadiene rubber (NBR), and chlorosulfonated polyethylene (CSM). The rubber component preferably contains at least one selected from chloroprene rubber and natural rubber (NR), and the rubber composition according to one embodiment of the present invention preferably contains chloroprene rubber, i.e., preferably contains a chloroprene polymer.
[0015] 1.1.1 Chloroprene-Based Rubber The chloroprene-based rubber according to the present invention refers to a rubber containing a chloroprene-based polymer having chloroprene (2-chloro-1,3-butadiene) as a monomer unit (monomer unit = structural unit). Examples of the chloroprene-based polymer include a chloroprene homopolymer and a chloroprene copolymer (a copolymer of chloroprene and a monomer copolymerizable with chloroprene). The polymer structure of the chloroprene-based polymer is not particularly limited.
[0016] Commercially available 2-chloro-1,3-butadiene may contain a small amount of 1-chloro-1,3-butadiene as an impurity. 2-chloro-1,3-butadiene containing such a small amount of 1-chloro-1,3-butadiene can also be used as the chloroprene monomer of this embodiment.
[0017] A chloroprene-based polymer according to one embodiment of the present invention may have a monomer unit derived from a monomer other than a chloroprene monomer. The monomer other than a chloroprene monomer is not particularly limited as long as it is copolymerizable with the chloroprene monomer, and examples thereof include unsaturated nitriles, (meth)acrylic acid esters (e.g., methyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate), hydroxyalkyl (meth)acrylates (e.g., 2-hydroxymethyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate), 2,3-dichloro-1,3-butadiene, 1-chloro-1,3-butadiene, butadiene, isoprene, ethylene, styrene, and sulfur. A chloroprene-based polymer according to one embodiment of the present invention may contain at least one monomer unit selected from 2,3-dichloro-1,3-butadiene and an unsaturated nitrile monomer. The chloroprene-based polymer according to one embodiment of the present invention may include an unsaturated nitrile monomer unit.
[0018] In a chloroprene polymer according to one embodiment of the present invention, the content of unsaturated nitrile monomer units can be 25% by mass or less, preferably 20% by mass or less, and more preferably less than 20% by mass, based on 100% by mass of the chloroprene polymer. The content of unsaturated nitrile monomer units in a chloroprene rubber according to one embodiment of the present invention may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, or 25% by mass, or may be within a range between any two of the values exemplified here. By controlling the content of unsaturated nitrile monomer units in the rubber composition to the above upper limit or less, the water resistance and cold resistance of a vulcanized molded article made from the rubber composition are further improved. Furthermore, the inclusion of unsaturated nitrile monomer units improves the oil resistance of a vulcanized molded article made from the rubber composition.
[0019] Examples of unsaturated nitriles include acrylonitrile, methacrylonitrile, ethacrylonitrile, and phenylacrylonitrile. The unsaturated nitriles may be used alone or in combination of two or more. The unsaturated nitrile preferably contains acrylonitrile, from the viewpoint of easily obtaining excellent moldability and easily obtaining excellent breaking strength, breaking elongation, hardness, tear strength, and oil resistance in a vulcanized molded product.
[0020] The content of unsaturated nitrile monomer units in chloroprene-based rubber can be calculated from the content of nitrogen atoms in the chloroprene-based rubber. Specifically, the content of nitrogen atoms in 100 mg of chloroprene-based rubber can be measured using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center Co., Ltd.), and the content of structural units derived from unsaturated nitrile monomers can be calculated. Elemental analysis can be performed under the following conditions. For example, the electric furnace temperatures are set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen is flowed at 0.2 mL / min as the combustion gas and 80 mL / min as the carrier gas. A calibration curve can be prepared using aspartic acid (10.52%), which has a known nitrogen content, as a standard substance.
[0021] A chloroprene polymer according to one embodiment of the present invention preferably contains 75 to 100 mass % of chloroprene monomer units, and more preferably 80 to 100 mass %, of chloroprene monomer units, based on 100 mass % of the chloroprene polymer. The content of chloroprene monomer units in the chloroprene polymer may be, for example, 75, 80, 85, 90, 95, 99, or 100 mass %, or may be within a range between any two of the values exemplified here. By ensuring that the content of chloroprene monomer units falls within the above range, a rubber composition can be obtained that can give a molded article having an excellent balance of hardness, tensile strength, and cold resistance.
[0022] A chloroprene polymer according to one embodiment of the present invention may contain 0 to 20 mass% of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units, based on 100 mass% of the chloroprene polymer. The content of monomer units other than chloroprene monomer units and unsaturated nitrile monomer units in the chloroprene polymer may be, for example, 0, 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20 mass%, or may be within a range between any two of the values exemplified here. By adjusting the copolymerization amount of the monomer other than the chloroprene monomer and the unsaturated nitrile monomer to fall within the above range, the effects of copolymerizing these monomers can be achieved without impairing the properties of the resulting rubber composition.
[0023] The chloroprene-based rubber according to one embodiment of the present invention may contain at least one polymer selected from a chloroprene homopolymer, a copolymer containing a chloroprene monomer unit and an unsaturated nitrile monomer unit, and a copolymer containing a chloroprene monomer unit and a 2,3-dichloro-1,3-butadiene monomer unit.
[0024] The rubber component according to the present invention can use one chloroprene rubber alone or a combination of two or more chloroprene rubbers. When the rubber composition according to one embodiment of the present invention contains two or more chloroprene rubbers, it is preferable that the content based on the total amount of each monomer unit contained in the two or more chloroprene polymers be within the above-mentioned numerical range, relative to 100% by mass of the total of the two or more chloroprene polymers contained in the rubber composition.
[0025] The chloroprene polymer (e.g., chloroprene homopolymer or chloroprene copolymer) contained in the chloroprene rubber according to the present invention may be a sulfur-modified chloroprene polymer, a mercaptan-modified chloroprene polymer, a xanthogen-modified chloroprene polymer, a dithiocarbonate-based chloroprene polymer, a trithiocarbonate-based chloroprene polymer, a carbamate-based chloroprene polymer, or the like.
[0026] 1.1.2 Method for Producing Chloroprene-Based Rubber The method for producing the chloroprene-based rubber according to the present invention is not particularly limited, but the rubber can be obtained by a production method including an emulsion polymerization step in which raw material monomers including a chloroprene monomer are emulsion-polymerized. In the emulsion polymerization step according to one embodiment of the present invention, a chloroprene monomer or raw material monomers including a chloroprene monomer and other monomers are emulsion-polymerized using an appropriate emulsifier, dispersant, catalyst, chain transfer agent, etc., and a polymerization terminator is added when the target final conversion rate is reached to obtain a latex containing a chloroprene-based polymer containing chloroprene monomer units. Next, unreacted monomers can be removed from the polymerization liquid obtained by the emulsion polymerization step. The method for this removal is not particularly limited, and examples include steam stripping. Thereafter, the pH is adjusted, and the resulting mixture is subjected to conventional processes such as freeze coagulation, water washing, and hot air drying to obtain a chloroprene-based rubber containing a chloroprene-based polymer.
[0027] The polymerization initiator used in emulsion polymerization is not particularly limited, and any known polymerization initiator generally used in emulsion polymerization of chloroprene can be used. Examples of the polymerization initiator include potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and organic peroxides such as t-butyl hydroperoxide.
[0028] The emulsifier used in emulsion polymerization is not particularly limited, and any known emulsifier generally used in emulsion polymerization of chloroprene can be used. Examples of the emulsifier include alkali metal salts of saturated or unsaturated fatty acids having 6 to 22 carbon atoms, alkali metal salts of rosin acid or disproportionated rosin acid (e.g., potassium rosinate), and alkali metal salts of formalin condensates of β-naphthalenesulfonic acid (e.g., sodium salt).
[0029] The molecular weight modifier used in emulsion polymerization is not particularly limited, and any known molecular weight modifier commonly used in emulsion polymerization of chloroprene can be used, such as mercaptan compounds, xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds. Xanthogen compounds, dithiocarbonate compounds, trithiocarbonate compounds, and carbamate compounds are preferably used as molecular weight modifiers for the chloroprene rubber according to one embodiment of the present invention.
[0030] The polymerization temperature and the final conversion rate of the monomer are not particularly limited, but the polymerization temperature may be, for example, 0 to 50°C or 10 to 50°C. The polymerization may be carried out so that the final conversion rate of the monomer falls within the range of 40 to 95% by mass. In order to adjust the final conversion rate, a polymerization terminator that terminates the polymerization reaction may be added to terminate the polymerization when the desired conversion rate is reached.
[0031] The polymerization terminator is not particularly limited, and any known polymerization terminator generally used in emulsion polymerization of chloroprene can be used, such as phenothiazine (thiodiphenylamine), 4-t-butylcatechol, and 2,2-methylenebis-4-methyl-6-t-butylphenol.
[0032] The chloroprene rubber according to one embodiment of the present invention can be obtained, for example, by removing unreacted monomers by a steam stripping method, adjusting the pH of the latex, and then performing conventional steps such as freeze coagulation, water washing, and hot air drying.
[0033] Chloroprene rubbers are classified into mercaptan-modified, xanthogen-modified, sulfur-modified, dithiocarbonate-based, trithiocarbonate-based and carbamate-based types depending on the type of molecular weight modifier.
[0034] 1.2 Organic Peroxide The rubber composition according to the present invention may contain an organic peroxide. One or more organic peroxides may be freely selected and used.
[0035] Examples of organic peroxides include dicumyl peroxide, benzoyl peroxide, 1,1-bis(t-butylperoxy)-3,5,5-trimethylcyclohexane, diisobutyryl peroxide, cumyl peroxyneodecanoate, di-n-propyl peroxydicarbonate, diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, 1,1,3,3-tetramethylbutyl peroxyneodecanoate, di(4-t-butylcyclohexyl)peroxydicarbonate, and di(2-ethylhexyl)peroxydicarbonate. butylperoxyneodecanoate, t-butylperoxyneoheptanoate, t-hexylperoxypivalate, t-butylperoxypivalate, di(3,5,5-trimethylhexanoyl)peroxide, dilauroyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, disuccinic acid peroxide, 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane, t-hexylperoxy peroxy-2-ethylhexanoate, di(4-methylbenzoyl) peroxide, t-butylperoxy-2-ethylhexanoate, di(3-methylbenzoyl) peroxide, benzoyl(3-methylbenzoyl) peroxide, dibenzoyl peroxide, 1,1-di(t-butylperoxy)-2-methylcyclohexane, 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane, 1,1-di(t-hexylperoxy)cyclohexane, 1,1-di(t-butylperoxy)cyclohexane, 2, 2-di(4,4-di-(t-butylperoxy)cyclohexyl)propane, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy-3,5,5-trimethylhexanoate, t-butylperoxylaurate, t-butylperoxyisopropyl monocarbonate, t-butylperoxy-2-ethylhexyl monocarbonate, t-hexylperoxybenzoate, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, t-butylperoxyacetate, 2,Examples of such peroxides include 2-di-(t-butylperoxy)butane, t-butyl peroxybenzoate, n-butyl 4,4-di-(t-butylperoxy)valerate, 1,4-bis[(t-butylperoxy)isopropyl]benzene, di-t-hexyl peroxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, t-butylcumyl peroxide, di-t-butyl peroxide, p-menthane hydroperoxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3, diisopropylbenzene hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, cumene hydroperoxide, and t-butyl hydroperoxide. Among these, at least one selected from dicumyl peroxide, 1,4-bis[(t-butylperoxy)isopropyl]benzene, t-butyl-α-cumyl peroxide, 2,5-dimethyl-2,5-bis(t-butylperoxy)hexane, and 2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3 is preferred, and 1,4-bis[(t-butylperoxy)isopropyl]benzene is particularly preferred.
[0036] From the viewpoint of ensuring processing safety and obtaining a good vulcanized molded article, the rubber composition according to the present invention preferably contains 0 to 5 parts by mass of an organic peroxide relative to the rubber components contained in the rubber composition. The content of the organic peroxide is, for example, 0, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 2, 3, 4, or 5 parts by mass, and may be within a range between any two of the values exemplified here. Furthermore, the rubber composition according to one embodiment of the present invention does not contain an organic peroxide, and by adjusting the types and amounts of other components, it is possible to adjust the hardness X, heat generation Y, and the relationship between hardness X and heat generation Y.
[0037] 1.3 Vulcanizing Agent The rubber composition according to the present invention may contain a vulcanizing agent. The type of vulcanizing agent is not particularly limited as long as it does not impair the effects of the present invention. The vulcanizing agent is preferably a vulcanizing agent that can be used to vulcanize chloroprene-based rubber. One or more vulcanizing agents can be freely selected and used. An example of the vulcanizing agent is zinc oxide.
[0038] From the viewpoint of ensuring processing safety and obtaining a sufficiently vulcanized molded article, the rubber composition according to the present invention preferably contains 1 to 15 parts by mass of a vulcanizing agent relative to the rubber component contained in the rubber composition. The content of the vulcanizing agent is, for example, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass relative to 100 parts by mass of the rubber component contained in the rubber composition, and may be within a range between any two of the numerical values exemplified here.
[0039] 1.4 Acid Acceptor The rubber composition according to one embodiment of the present invention may contain an acid acceptor. The acid acceptor may include at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, magnesium oxide, lead oxide, trimlead tetroxide, iron trioxide, titanium dioxide, and calcium oxide, and may include at least one selected from the group consisting of hydrotalcite compounds, magnesium-aluminum solid solutions, and magnesium oxide, and preferably includes magnesium oxide. The acid acceptors may be used alone or in combination of two or more.
[0040] As the hydrotalcite, one represented by the following formula can be used: [M 2+ 1-x M 3+ x (OH) 2 ] x+ [A n-x/n ・mH 2 O] x-
[0041] In the above formula, M 2+ : Mg 2+ , Zn 2+ At least one divalent metal ion M selected from 3+ :Al 3+ , Fe 3+ At least one trivalent metal ion selected from the following: n- :CO 3 2- , Cl ― , NO 3 2-At least one n-type anion selected from the following: X: 0<X≦0.33.
[0042] As the hydrotalcite, Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 ・3.5H 2 O, Mg 4.5 Al 2 (OH) 13 CO 3 , Mg 4 Al 2 (OH) 12 CO 3 ・3.5H 2 O, Mg 6 Al 2 (OH) 16 CO 3 ・4H 2 O, Mg 5 Al 2 (OH) 14 CO 3 ・4H 2 O, Mg 3 Al 2 (OH) 10 CO 3 ・1.7H 2 O, and particularly preferably Mg 4.3 Al 2 (OH) 12.6 CO 3 ・3.5H 2 O, Mg 3 ZnAl 2 (OH) 12 CO 3 ・3H 2 It is O.
[0043] The amount of the acid acceptor added may be 0.1 to 15 parts by mass per 100 parts by mass of the rubber component contained in the rubber composition, for example, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0044] 1.5 Maleimide Compound The rubber composition according to one embodiment of the present invention may contain a maleimide compound. The maleimide compounds may be used alone or in combination of two or more.
[0045] The maleimide compound can contribute to the vulcanization of the rubber composition as a co-crosslinking agent. Examples of the maleimide compound include N,N'-o-phenylene bismaleimide, N,N'-m-phenylene bismaleimide, N,N'-p-phenylene bismaleimide, N,N'-(4,4'-diphenylmethane)bismaleimide, 2,2-bis-[4-(4-maleimidophenoxy)phenyl]propane, bis(3-ethyl-5-methyl-4-maleimidophenyl)methane, bisphenol A diphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, 4-methyl-1,3-phenylene bismaleimide, and 1,6'-bismaleimide-(2,2,4-trimethyl)hexane. From the viewpoint of improving the heat resistance of the resulting vulcanizate and vulcanized molded article, it is particularly preferable to use N,N'-m-phenylenebismaleimide (also known as m-phenylenedimaleimide).
[0046] A rubber composition according to one embodiment of the present invention may contain 0 to 10 parts by mass of a maleimide compound per 100 parts by mass of the rubber component. The content of the maleimide compound may be, for example, 0, 0.1, 0.2, 0.3, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, or may be within a range between any two of the values exemplified herein. By setting the content of the maleimide compound at or above the lower limit, vulcanization of the resulting rubber composition proceeds more sufficiently, allowing for the production of a vulcanized molded article with excellent mechanical properties and heat resistance. Furthermore, by setting the content of the maleimide compound at or below the upper limit, the rubber elasticity of the resulting vulcanized molded article can be sufficiently maintained. Furthermore, the rubber composition according to one embodiment of the present invention may not contain a maleimide compound, and instead, by adjusting the types and amounts of other components, the hardness X, heat generation Y, and the relationship between hardness X and heat generation Y can be adjusted.
[0047] 1.6 Filler The rubber composition according to one embodiment of the present invention may contain a filler, such as carbon black. Examples of carbon black include furnace carbon black such as SAF, ISAF, HAF, EPC, XCF, FEF, GPF, HMF, and SRF, modified carbon black such as hydrophilic carbon black, channel black, lamp black, thermal carbon such as FT and MT, acetylene black, and ketjen black.
[0048] The rubber composition according to the present invention may contain 0 parts by mass or more and less than 100 parts by mass of carbon black per 100 parts by mass of the rubber component. The amount of carbon black is, for example, 0, 1, 2, 3, 4, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 99 parts by mass, and may be within a range between any two of the numerical values exemplified here.
[0049] The rubber composition according to the present invention may also contain fillers other than carbon black, provided that the effects of the present invention are not impaired. Examples of fillers other than carbon black include silica, such as wet silica filler (hydrated silica), dry silica filler (anhydrous silicic acid), and colloidal silica filler, clay, talc, and calcium carbonate. These may be used alone or in combination of two or more.
[0050] In a rubber composition according to one embodiment of the present invention, the total amount of carbon black and fillers (reinforcing materials) other than carbon black contained in the rubber composition is preferably 0 to 100 parts by mass when the rubber component is taken as 100 parts by mass. In a rubber composition according to one embodiment of the present invention, the content of fillers / reinforcing materials other than carbon black can be 50% by mass or less when the total amount of carbon black and fillers (reinforcing materials) other than carbon black contained in the rubber composition is taken as 100% by mass. The content of fillers / reinforcing materials other than carbon black may be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50% by mass, and may be within a range between any two of the values exemplified here. A rubber composition according to one embodiment of the present invention may also contain no fillers (reinforcing materials) other than carbon black. Furthermore, the rubber composition according to one embodiment of the present invention does not contain carbon black and fillers other than carbon black, and the hardness X, heat generation Y, and the relationship between hardness X and heat generation Y can be adjusted by adjusting the types and amounts of other components.
[0051] 1.7 Silane Coupling Agent When the rubber composition according to one embodiment of the present invention contains silica as a filler, it may contain a silane coupling agent. There are no particular limitations on the silane coupling agent, and those used in commercially available rubber compositions can be used, such as vinyl coupling agents, epoxy coupling agents, styryl coupling agents, methacrylic coupling agents, acrylic coupling agents, amino coupling agents, polysulfide coupling agents, and mercapto coupling agents. In particular, from the perspective of scorch resistance and reinforcing effect, vinyl coupling agents, methacrylic coupling agents, and acrylic coupling agents are preferred, as they initiate reaction under high temperature conditions during crosslinking.
[0052] A rubber composition according to one embodiment of the present invention may contain 0.5 to 10 parts by mass of a silane coupling agent per 100 parts by mass of silica contained in the rubber composition. The content of the silane coupling agent may be, for example, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass per 100 parts by mass of silica, and may be within a range between any two of the values exemplified here. Silica may be used alone or in combination of two or more types. By including the above-mentioned silane coupling agent and keeping the content of the silane coupling agent within the above-mentioned range, the dispersibility of the silica filler in the rubber and the reinforcing effect between the rubber and the silica filler can be improved, and the occurrence of scorch can be suppressed.
[0053] 1.8 Lubricants and Processing Aids The rubber composition according to the present invention may further contain a lubricant and / or a processing aid. Lubricants and processing aids are added primarily to improve processability, such as by facilitating release of the rubber composition from rolls, molding dies, extruder screws, etc. Examples of lubricants and processing aids include fatty acids such as stearic acid, paraffin-based processing aids such as polyethylene, fatty acid amides, petrolatum, and factice. These may be used alone or in combination of two or more. The rubber composition according to the present invention may contain 0.1 to 15 parts by mass of lubricant and processing aid per 100 parts by mass of the rubber component, and may also contain 1 to 10 parts by mass of lubricant and processing aid. The content of the lubricant and processing aid may be, for example, 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or 15 parts by mass, or may fall within a range between any two of the values exemplified herein.
[0054] 1.9 Vulcanization Accelerator The rubber composition according to the present invention may contain a vulcanization accelerator, and may contain 0 to 5.0 parts by mass of the vulcanization accelerator when the rubber composition contained in the composition is taken as 100 parts by mass. The content of the vulcanization accelerator is, for example, 0, 0.1, 0, 2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass, and may be within a range between any two of the values exemplified here. The rubber composition according to the present invention may also be free of a vulcanization accelerator. The rubber composition according to one embodiment of the present invention may not contain a vulcanization accelerator, and the hardness X, heat generation Y, and the relationship between hardness X and heat generation Y can be adjusted by adjusting the types and amounts of other components without blending a vulcanization accelerator.
[0055] The type of vulcanization accelerator is not particularly limited as long as it does not impair the effects of the present invention. The vulcanization accelerator is preferably a vulcanization accelerator that can be used for vulcanizing chloroprene-based rubber. One or more vulcanization accelerators can be freely selected and used. Examples of vulcanization accelerators include sulfur, thiuram-based vulcanization accelerators, dithiocarbamate-based vulcanization accelerators, thiourea-based vulcanization accelerators, guanidine-based vulcanization accelerators, xanthogenate-based vulcanization accelerators, and thiazole-based vulcanization accelerators.
[0056] Examples of thiuram vulcanization accelerators include tetramethylthiuram disulfide (TMTD), tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, etc. Examples of dithiocarbamate vulcanization accelerators include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, ferric dimethyldithiocarbamate, tellurium diethyldithiocarbamate, etc. Examples of thiourea-based vulcanization accelerators include thiourea compounds such as ethylene thiourea, diethyl thiourea (N,N'-diethyl thiourea), trimethyl thiourea, diphenyl thiourea (N,N'-diphenyl thiourea), and 1,3-trimethylene-2-thiourea. Examples of guanidine-based vulcanization accelerators include 1,3-diphenyl guanidine, 1,3-di-o-tolyl guanidine, 1-o-tolyl biguanide, and di-o-tolyl guanidine salt of dicatechol borate. Examples of xanthate-based vulcanization accelerators include zinc butyl xanthogenate and zinc isopropyl xanthogenate. Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-mercaptobenzothiazole zinc salt, 2-mercaptobenzothiazole cyclohexylamine salt, 2-(4'-morpholinodithio)benzothiazole, N-cyclohexylbenzothiazole-2-sulfenamide, etc. These may be used alone or in combination of two or more.
[0057] 1.10 Others In addition to the above-mentioned components, the rubber composition according to the present invention may further contain components such as antioxidants, antioxidants, flame retardants, and vulcanization retarders, as long as the effects of the present invention are not impaired. Examples of antioxidants and antioxidants include ozone antioxidants, phenolic antioxidants, amine antioxidants, acrylate antioxidants, imidazole antioxidants, metal carbamates, waxes, phosphorus-based antioxidants, and sulfur-based antioxidants. Examples of imidazole antioxidants include 2-mercaptobenzimidazole, 2-mercaptomethylbenzimidazole, and zinc salts of 2-mercaptobenzimidazole. The rubber composition according to the present invention may contain a total of 0.1 to 10 parts by mass of antioxidants and antioxidants per 100 parts by mass of the rubber component contained in the rubber composition.
[0058] In the rubber composition according to one embodiment of the present invention, by configuring the types and contents of the components in the rubber composition in the above manner, the hardness X of the test vulcanized molded product 1 of the rubber composition and the heat generation Y of the test vulcanized molded product 2 of the rubber composition tend to satisfy the relationship of formula (1).
[0059] 2. Method for Producing Rubber Composition The rubber composition according to one embodiment of the present invention can be obtained by kneading the rubber component and other necessary components at a temperature equal to or lower than the vulcanization temperature. The method for producing the rubber composition according to one embodiment of the present invention can include a mixing step of mixing the rubber component and other necessary components at a temperature equal to or lower than the vulcanization temperature.
[0060] A manufacturing method according to one embodiment of the present invention can include a first mixing step, a standing step, and a second mixing step. In the first mixing step, raw materials including a rubber component and compounding ingredients for the first mixing step are mixed to obtain a rubber composition precursor. In the standing step, the rubber composition precursor is stood at 23° C. or less for 12 hours or more. In the second mixing step, the compounding ingredients for the second mixing step are added to the rubber composition precursor after standing and mixed to obtain a rubber composition.
[0061] In the first mixing step, raw materials including a rubber component and compounding ingredients for the first mixing step are mixed to obtain a rubber composition precursor. The compounding ingredients for the first mixing step may not contain a vulcanizing agent, a vulcanization accelerator, an organic peroxide, or a maleimide compound. The compounding ingredients for the first mixing step preferably do not contain components that contribute to vulcanization and crosslinking. The compounding ingredients for the first mixing step may include at least one, two, three, four, five, or six of carbon black, acid acceptor, lubricant, processing aid, plasticizer, and antioxidant, or may include all of these.
[0062] In the standing step, the rubber composition precursor is allowed to stand at 23°C or lower for 12 hours or more. The standing temperature can be, for example, 5 to 23°C, and may be 5, 8, 11, 14, 17, 20, or 23°C, or may be within a range between any two of the values exemplified here. The standing time can be, for example, 12 to 24 hours, and may be, for example, 12, 14, 16, 18, 20, 22, or 24 hours, or may be within a range between any two of the values exemplified here. In one embodiment of the present invention, the hardness X and heat generation Y can be adjusted by undergoing the standing step.
[0063] In the second mixing step, the compounding ingredients for the second mixing step are added to the rubber composition precursor after standing and mixed to obtain a rubber composition. The compounding ingredients for the second mixing step may include a vulcanizing agent, a vulcanization accelerator, an organic peroxide, and a maleimide compound. The compounding ingredients for the second mixing step may also include carbon black, a lubricant, a processing aid, a plasticizer, an acid acceptor, an antioxidant, etc.
[0064] In each mixing step, examples of the device for kneading the raw material components include conventionally known kneading devices such as a mixer, a Banbury mixer, a kneader mixer, and an open roll.
[0065] 3. Properties of Rubber Composition In a rubber composition according to one embodiment of the present invention, when a laminate is prepared by stacking test vulcanized molded articles 1 of the rubber composition to a thickness of 6.0 mm or more, the hardness thereof is measured with a Type A durometer in accordance with JIS K 6253-3:2023 as X, and test vulcanized molded articles 2 of the rubber composition are evaluated in a constant strain flexometer test in accordance with JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and frequency of 1,800 vibrations per minute as Y, the hardness X and heat generation Y satisfy the following formula (1): 1.4X-Y>45.0 (1)
[0066] Test vulcanized molded article 1 is a sheet-like vulcanized molded article having a thickness of 2 mm, obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes in accordance with JIS K 6299: 2012. Test vulcanized molded article 2 is a cylindrical vulcanized molded article having a diameter of 15 mm and a height of 25 mm, obtained by press-vulcanizing the rubber composition at 170°C for 20 minutes.
[0067] The rubber composition according to the present invention can produce vulcanized molded articles having excellent water resistance and alkali resistance by adjusting the hardness X and heat generation Y of the vulcanized molded article so that the hardness X and heat generation Y satisfy the relationship expressed by formula (1). The hardness X can be controlled by adjusting the manufacturing conditions described below, for example, by adjusting the amount of filler and plasticizer. The heat generation Y can also be controlled by adjusting the manufacturing conditions described below, for example, by adjusting the type and amount of filler, the crosslink density of the resulting vulcanized molded article, and the type and amount of plasticizer. It is believed that increasing the amount of filler increases the heat generation Y, increasing the crosslink density decreases the heat generation Y, and increasing the amount of plasticizer increases the heat generation Y. Here, adjusting the relationship between hardness X and heat generation Y so that formula (1) is satisfied can adjust the amount of filler, the amount of plasticizer, the crosslink density, etc. at hardness X, thereby producing a rubber composition capable of producing vulcanized molded articles having excellent water resistance and alkali resistance. The value of (1.4X-Y) can be greater than 45.0 and less than or equal to 100.0, for example, 45.5, 50.0, 55.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, 95.0, 100.0, or within a range between any two of the values exemplified here.
[0068] In the rubber composition according to one embodiment of the present invention, a laminate obtained by stacking test vulcanized molded articles 1 of the rubber composition to a thickness of 6.0 mm or more preferably has a hardness X measured with a type A durometer according to JIS K 6253-3:2023 of 40 to 98. The hardness X may be, for example, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 98, or may be within a range between any two of the values exemplified here.
[0069] The hardness X can be controlled by adjusting the manufacturing method of the rubber composition, for example, the presence or absence, type and amount of each component blended in the rubber composition, particularly the type and amount of filler and plasticizer, and the manufacturing conditions of the rubber composition (particularly the presence or absence, temperature and time of a standing step).
[0070] In a rubber composition according to one embodiment of the present invention, a test vulcanized molded article 2 of the rubber composition is preferably evaluated in a constant strain flexometer test under conditions of 40°C, a strain of 0.175 inches, a load of 55 pounds, and a frequency of 1,800 vibrations per minute in accordance with JIS K 6265:2018, and the heat generation Y is preferably 85°C or less. The heat generation Y may be, for example, 1, 2, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, and may be within a range between any two of the values exemplified here.
[0071] The heat generation Y can be controlled by adjusting the manufacturing method of the rubber composition, particularly the presence or absence, type and amount of each component blended into the rubber composition, for example, the presence or absence, type and amount of fillers and components that contribute to vulcanization and crosslinking, as well as the manufacturing conditions of the rubber composition (particularly the presence or absence, temperature and time of a standing step).
[0072] The hardness X and heat generation Y can be specifically evaluated by the method described in the Examples.
[0073] In a rubber composition according to one embodiment of the present invention, when a test vulcanization molded article 1 and / or a test vulcanization molded article 2 of the rubber composition is immersed in water at 70° C. for 144 hours, the volume change ΔV calculated in accordance with JIS K 6258 is preferably less than 9%, more preferably less than 6%. The volume change ΔV when immersed in water at 70° C. for 144 hours is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8%, or less than 9%, and may be within a range between any two of the values exemplified here.
[0074] In a rubber composition according to one embodiment of the present invention, when a test vulcanization molded article 1 and / or a test vulcanization molded article 2 of the rubber composition is immersed in 10% sodium hydroxide at 70°C for 144 hours, the volume change ΔV calculated in accordance with JIS K 6258 is preferably less than 10%, more preferably less than 7%. The volume change ΔV when immersed in water at 70°C for 144 hours is, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9%, or less than 10%, and may be within a range between any two of the values exemplified here.
[0075] The water resistance and alkali resistance of the vulcanized molded article of the rubber composition can be measured specifically by the method described in the examples.
[0076] 6. Unvulcanized molded body, vulcanized product, and vulcanized molded body The unvulcanized molded body according to one embodiment of the present invention uses the rubber composition according to one embodiment of the present invention, and is a molded body (molded article) of the rubber composition (unvulcanized state) according to one embodiment of the present invention. A method for producing an unvulcanized molded body according to one embodiment of the present invention includes a step of molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The unvulcanized molded body according to one embodiment of the present invention is made of the rubber composition (unvulcanized state) according to one embodiment of the present invention.
[0077] A vulcanizate according to one embodiment of the present invention is a vulcanizate of the rubber composition according to one embodiment of the present invention. A method for producing a vulcanizate according to one embodiment of the present invention includes a step of vulcanizing the rubber composition according to one embodiment of the present invention.
[0078] A vulcanization molded article according to one embodiment of the present invention is a vulcanization molded article of a rubber composition according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention uses a vulcanizate according to one embodiment of the present invention and is a molded article (molded product) of the vulcanizate according to one embodiment of the present invention. The vulcanization molded article according to one embodiment of the present invention is made of a vulcanizate according to one embodiment of the present invention.
[0079] The vulcanized molded article according to one embodiment of the present invention can be obtained by molding a vulcanizate obtained by vulcanizing the rubber composition (unvulcanized state) according to one embodiment of the present invention, and can also be obtained by vulcanizing a molded article obtained by molding the rubber composition (unvulcanized state) according to one embodiment of the present invention. The vulcanized molded article according to one embodiment of the present invention can be obtained by vulcanizing the rubber composition according to one embodiment of the present invention after molding or during molding. A method for producing a vulcanized molded article according to one embodiment of the present invention comprises a step of molding a vulcanized article according to one embodiment of the present invention, or a step of vulcanizing an unvulcanized molded article according to one embodiment of the present invention.
[0080] In one embodiment of the present invention, the vulcanized molded article is formed into a test vulcanized molded article 1' having a thickness of 6.0 mm or more. When the hardness of the vulcanized molded article is measured with a Type A durometer in accordance with JIS K 6253-3:2023 as X', and when the vulcanized molded article is formed into a cylindrical test vulcanized molded article 2' having a diameter of 15 mm and a height of 25 mm as Y', the heat generated is determined by evaluation in a constant strain flexometer test in accordance with JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 cycles per minute. It is preferable that the hardness X' and the heat generated Y' satisfy the following formula (2): 1.4X' - Y' > 45.0 (2) Note that the test vulcanized molded article 1' having a thickness of 6.0 mm or more may be a laminate formed by stacking multiple vulcanized molded articles having a thickness of less than 6.0 mm. The thickness of the test vulcanized molded article 1' can be set to 6.0 mm or more and 7.0 mm or less.
[0081] The value of (1.4X-Y) is greater than 45.0, for example, 45.5, 50.0, 55.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, 95.0, 100.0, and may be within a range between any two of the values exemplified here.
[0082] The hardness X' of the test vulcanized molded article 1' according to one embodiment of the present invention is, for example, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, or 98, and may be within a range between any two of the values exemplified here.
[0083] The heat generation Y' of the test vulcanized molded body 2' according to one embodiment of the present invention is, for example, 1, 2, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, or 85°C, and may be within a range between any two of the values exemplified here.
[0084] The vulcanized molded article according to one embodiment of the present invention preferably has a volume change ΔV of less than 9%, more preferably less than 6%, when immersed in water at 70° C. for 144 hours, as calculated in accordance with JIS K 6258. The volume change ΔV when immersed in water at 70° C. for 144 hours may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8%, or less than 9%, and may be within a range between any two of the values exemplified here.
[0085] The vulcanized molded article according to one embodiment of the present invention preferably has a volume change ΔV of less than 10%, more preferably less than 7%, when immersed in 10% sodium hydroxide at 70° C. for 144 hours, as calculated in accordance with JIS K 6258. The volume change ΔV when immersed in water at 70° C. for 144 hours may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9%, or less than 10%, and may be within a range between any two of the values exemplified here.
[0086] The hardness, heat generation, water resistance, and alkali resistance of the vulcanized molded article can be specifically measured by the methods described in the Examples. The hardness, heat generation, water resistance, and alkali resistance of the vulcanized molded article can also be controlled by adjusting the production method of the rubber composition, for example, the presence or absence, type, and amount of each component blended in the rubber composition, particularly the presence or absence, type, and amount of fillers and components contributing to vulcanization and crosslinking, and the production conditions of the rubber composition (particularly the presence or absence, temperature, and time of a standing step).
[0087] The unvulcanized molded article, vulcanized product, and vulcanized molded article according to one embodiment of the present invention can be used as rubber parts in various industrial fields, such as buildings, structures, ships, railways, coal mines, and automobiles. Because the rubber composition according to the present invention has excellent water resistance and alkali resistance, it can be used for various components requiring these properties. The rubber composition, vulcanized product, and vulcanized molded article according to one embodiment of the present invention can be used as rubber parts in various industrial fields, such as buildings, structures, ships, railways, coal mines, and automobiles, and can be used for rubber parts such as automotive rubber components (e.g., automotive seals), hose materials, rubber molds, gaskets, rubber rolls, industrial cables, industrial conveyor belts, and sponges. In particular, they can be used as transmission belts, conveyor belts, hoses, wipers, immersion products, sealing parts, adhesives, boots, rubber-coated fabrics, rubber rolls, vibration-proof rubber, or sponge products.
[0088] (Automotive Rubber Components) Automotive rubber components include gaskets, oil seals, and packings, which are used in machinery and equipment to prevent leaks of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets whose sealing parts are fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can enhance water resistance and alkali resistance. This makes it possible to produce automotive parts with excellent oil resistance, which was previously difficult to achieve with conventional rubber compositions.
[0089] (Hose Material) A hose material is a flexible pipe, and specific examples include high- and low-pressure hoses for water supply, oil supply, air supply, steam supply, and hydraulic applications. The rubber composition of the present invention can improve the water resistance and alkali resistance of the hose material while maintaining the processability of the unvulcanized product. This makes it possible to produce, for example, a hose material with excellent water resistance and alkali resistance, which has been difficult to achieve with conventional rubber compositions.
[0090] (Rubber molded products) Examples of rubber molded products include anti-vibration rubber, vibration-damping materials, and boots. Anti-vibration rubber and vibration-damping materials are rubbers that prevent the transmission and spread of vibrations. Specific examples include torsional dampers, engine mounts, and muffler hangers for automobiles and various other vehicles that absorb vibrations during engine operation to prevent noise. The rubber composition of the present invention can improve the water resistance and alkali resistance of anti-vibration rubber and vibration-damping materials. This makes it possible to produce anti-vibration rubber and vibration-damping materials with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions. Boots are bellows-shaped components whose outer diameter gradually increases from one end to the other. Specific examples include boots for constant velocity joint covers, boots for ball joint covers (dust cover boots), and boots for rack and pinion gears that protect drive parts such as automobile drive systems. The rubber composition of the present invention can improve water resistance and alkali resistance. This makes it possible to produce boots that can be used in harsher environments than conventional rubber compositions.
[0091] (Gaskets, etc.) Gaskets, oil seals, and packings are components in machines and equipment that prevent the leakage of liquids and gases and the intrusion of debris and foreign objects such as rainwater and dust into the interior. Specifically, there are gaskets used for fixed applications and oil seals and packings used for moving parts. Gaskets whose sealing parts are fixed with bolts or other fasteners are made of various materials depending on the purpose, as opposed to soft gaskets such as O-rings and rubber sheets. Packings are also used for rotating parts such as pump and motor shafts, moving parts of valves, reciprocating parts such as pistons, coupler connections, and water stop parts of water faucets. The rubber composition of the present invention can improve the water resistance and alkali resistance of these components. This makes it possible to produce sealing components with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions.
[0092] (Rubber Roll) A rubber roll is manufactured by adhesively coating a metal core, such as an iron core, with rubber, and is generally manufactured by spirally winding a rubber sheet around a metal iron core. Rubber materials such as NBR, EPDM, and CR are used for rubber rolls depending on the required characteristics for various applications, such as papermaking, various metal manufacturing, film manufacturing, printing, general industrial use, agricultural machinery such as rice hullers, and food processing. CR has good mechanical strength that can withstand the friction of the objects being conveyed, and is therefore used in a wide range of rubber roll applications. Furthermore, rubber rolls used to convey heavy loads have the problem of deformation under load, and improvements are needed. The rubber composition of the present invention can improve the water resistance and alkali resistance of rubber rolls. This makes it possible to manufacture embossing rubber rolls with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions. The rubber composition according to one embodiment of the present invention can be used for rubber rolls used in at least one of an acid washing line and an alkali washing line.
[0093] A rubber roll according to one embodiment of the present invention comprises a core and a surface layer provided on the circumferential surface of the core, the surface layer including the vulcanized molded article described above, and the rubber roll is used in at least one of an acid washing line and an alkali washing line.
[0094] (Industrial Cable) Industrial cables are linear components for transmitting electrical or optical signals. They are made by coating a good conductor such as copper or a copper alloy, or an optical fiber, with an insulating coating layer, and a wide variety of industrial cables are manufactured depending on their structure and installation location. The rubber composition of the present invention can improve the water resistance and alkali resistance of industrial cables. This makes it possible to manufacture industrial cables with excellent water resistance and alkali resistance, which was difficult to achieve with conventional rubber compositions.
[0095] (Industrial Conveyor Belts) Industrial conveyor belts are available in rubber, resin, and metal, and are selected to suit a wide variety of uses. Among these, rubber conveyor belts are inexpensive and widely used, but when used in environments where there is a lot of friction and collision with the conveyed materials, they have been prone to damage due to deterioration. The rubber composition of the present invention can improve the water resistance and alkali resistance of industrial conveyor belts. This makes it possible to produce industrial conveyor belts with excellent water resistance and alkali resistance that can be used in harsh environments, which has been difficult with conventional rubber compositions.
[0096] (Sponge) Sponges are porous materials with countless fine pores inside, and are specifically used in vibration-damping materials, sponge sealing parts, wetsuits, shoes, etc. The rubber composition of the present invention can improve the acid resistance and water resistance of the sponge. Furthermore, the use of chloroprene-unsaturated nitrile copolymer rubber also makes it possible to improve the flame retardancy of the sponge. This makes it possible to produce sponges with excellent water resistance and alkali resistance that can be used in harsh environments, which was difficult with conventional rubber compositions, as well as sponges with excellent flame retardancy. Furthermore, the hardness of the resulting sponge can be appropriately adjusted by adjusting the content of the foaming agent, etc.
[0097] Methods for molding the rubber composition (unvulcanized state) and vulcanized product according to one embodiment of the present invention include press molding, extrusion molding, calendar molding, etc. The temperature for vulcanizing the rubber composition may be set appropriately according to the composition of the rubber composition and can be 140 to 220°C. The vulcanization temperature may be, for example, 140, 150, 160, 170, 180, 190, 200, 210, or 220°C, and may be within a range between any two of the values exemplified here. The vulcanization time for vulcanizing the rubber composition may be set appropriately depending on the composition of the rubber composition, the shape of the unvulcanized molded product, etc., and can be 10 to 300 minutes. For example, the value may be 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, or 300 minutes, or may be within a range between any two of the values exemplified here.
[0098] The present invention will be described in more detail below based on examples, but the present invention should not be construed as being limited to these examples.
[0099] <Method for Producing Chloroprene-Based Rubber (A-2)> 24 parts by mass of chloroprene (monomer), 24 parts by mass of acrylonitrile (monomer), 0.5 parts by mass of diethylxanthogen disulfide, 200 parts by mass of pure water, 5.00 parts by mass of potassium rosinate (manufactured by Harima Chemicals Co., Ltd.), 0.40 parts by mass of sodium hydroxide, and 2.0 parts by mass of sodium salt of β-naphthalenesulfonic acid formalin condensate (manufactured by Kao Corporation) were added to a 3 L polymerization vessel equipped with a heating / cooling jacket and a stirrer. Next, 0.1 parts by mass of potassium persulfate was added as a polymerization initiator, and emulsion polymerization was carried out in a nitrogen stream at a polymerization temperature of 40°C. The chloroprene was added in portions starting 20 seconds after the start of polymerization. The portion-by-portion addition flow rate was adjusted with a solenoid valve based on the change in the heat quantity of the refrigerant over the first 10 seconds of polymerization, and the flow rate was readjusted every 10 seconds thereafter, for continuous polymerization. When the polymerization rate relative to the total amount of chloroprene and acrylonitrile reached 50%, 0.02 parts by mass of phenothiazine as a polymerization terminator was added to terminate the polymerization. Thereafter, unreacted monomers in the reaction solution were removed under reduced pressure to obtain a chloroprene-based latex containing a chloroprene-acrylonitrile copolymer.
[0100] The above-mentioned polymerization rate [%] of the chloroprene latex was calculated from the dry mass of the air-dried chloroprene latex. Specifically, it was calculated using the following formula (A). In the formula, "solid content concentration" refers to the concentration [% by mass] of the solid content obtained by heating 2 g of a sample of chloroprene latex at 130°C and removing volatile components such as the solvent (water), volatile chemicals, and raw materials. "Total charge amount" refers to the total amount [g] of raw materials, reagents, and solvent (water) charged into the polymerization vessel from the start of polymerization to a certain time. "Evaporation residue" refers to the mass [g] of chemicals and raw materials charged from the start of polymerization to a certain time that do not volatilize under conditions of 130°C and remain as solids together with the polymer. "Monomer charge amount" refers to the sum [g] of the amount of monomer initially charged into the polymerization vessel and the amount of monomer added in portions from the start of polymerization to a certain time. Note that "monomer" here refers to the total amount of chloroprene and acrylonitrile. Conversion rate = {[(total charge amount × solid content concentration / 100) - evaporation residue] / charge amount of monomer} × 100 (A)
[0101] The pH of the chloroprene latex (R-2) was adjusted to 7.0 using acetic acid or sodium hydroxide, and then the chloroprene latex was demulsified by freezing and coagulating it on a metal plate cooled to −20° C. to obtain a sheet. The sheet was washed with water and then dried at 130° C. for 15 minutes to obtain a solid chloroprene rubber (A-2).
[0102] The content of acrylonitrile monomer units contained in the chloroprene-based rubber (A-2) was calculated from the content of nitrogen atoms in the chloroprene-acrylonitrile copolymer rubber. Specifically, using an elemental analyzer (Sumigraph 220F, manufactured by Sumika Chemical Analysis Center Co., Ltd.), the content of nitrogen atoms in 100 mg of the chloroprene-based rubber (A-2) was measured, and the content of acrylonitrile monomer units was calculated. The content of acrylonitrile monomer units was 10.0 mass%.
[0103] The above elemental analysis was carried out as follows. The electric furnace temperatures were set to 900°C for the reactor, 600°C for the reduction furnace, 70°C for the column, and 100°C for the detector, and oxygen gas was flowed at 0.2 mL / min as the combustion gas and helium gas was flowed at 80 mL / min as the carrier gas. A calibration curve was prepared using aspartic acid (10.52%) with a known nitrogen content as the standard substance. The chloroprene rubber (A-2) obtained by the above production method had an acrylonitrile monomer unit content of 10.0% by mass.
[0104] <Method for producing chloroprene rubber (A-1)> The amount of acrylonitrile monomer added in the polymerization step was changed to obtain chloroprene rubber (A-1) having an acrylonitrile monomer unit content of 5.0 mass% in the chloroprene rubber.
[0105] (Examples 1 to 19, Comparative Examples 1 to 13) <Preparation of Rubber Compositions> Of the components listed in Tables 1 to 4, the components excluding the organic peroxide, vulcanization accelerator, maleimide compound, and vulcanizing agent were mixed using an 8-inch open roll to obtain a rubber composition precursor that did not contain a vulcanizing agent or the like (first mixing step). Subsequently, the obtained rubber composition precursor was allowed to stand at 23°C for 12 hours. Thereafter, the rubber composition precursor, the organic peroxide, vulcanization accelerator, maleimide compound, and vulcanizing agent were kneaded using an 8-inch open roll (second mixing step) to obtain the rubber compositions of the Examples and Comparative Examples.
[0106] (Comparative Examples 14 to 17) <Preparation of Rubber Compositions> Of the components listed in Table 4, the components excluding the organic peroxide, vulcanization accelerator, maleimide compound, and vulcanizing agent were mixed using an 8-inch open roll to obtain a rubber composition precursor that did not contain a vulcanizing agent, etc. (first mixing step). Subsequently, without a standing step, the rubber composition precursor, the organic peroxide, the vulcanization accelerator, the maleimide compound, and the vulcanizing agent were kneaded using an 8-inch open roll (second mixing step) to obtain rubber compositions of the comparative examples.
[0107] The components used to obtain the composition are as follows: Rubber components: Chloroprene rubber A-1: chloroprene-acrylonitrile copolymer AN (acrylonitrile monomer unit) content 5% by mass Chloroprene rubber A-2: chloroprene-acrylonitrile copolymer AN (acrylonitrile monomer unit) content 10% by mass Chloroprene rubber A-5: mercaptan-modified chloroprene rubber (chloroprene homopolymer), manufactured by Denka Co., Ltd., S-40V Natural rubber, manufactured by HB Chemical Co., Ltd., SMR-CV60
[0108] Carbon black: Asahi #70, HAF, manufactured by Asahi Carbon Co., Ltd. Organic peroxide: 1,4-bis[(t-butylperoxy)isopropyl]benzene, Perbutyl P-40, manufactured by Nippon Oil & Fats Co., Ltd.
[0109] Vulcanization accelerators: Nocceler TMU: trimethylthiourea, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocceler TMU Sulfur: sulfur, manufactured by Hosoi Chemical Industry Co., Ltd., fine sulfur 200 mesh Nocceler TT: tetramethylthiuram disulfide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocceler TT Nocceler CZ: N-cyclohexyl-2-benzothiazolylsulfenamide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocceler CZ
[0110] Maleimide compound: m-phenylenedimaleimide, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Valnoc PM Plasticizer: ether ester compound, manufactured by ADEKA Corporation, Adeka Cizer RS-700 Vulcanizing agent: zinc oxide, manufactured by Sakai Chemical Industry Co., Ltd., zinc oxide type 2 Acid acceptor: magnesium oxide, manufactured by Kyowa Chemical Industry Co., Ltd., Kyowa Mag 150 Antioxidants: Nocrac CD: 4,4'-bis(α,α-dimethylbenzyl)diphenylamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocrac CD Nocrac 6C: N-phenyl-N'-(1,3-dimethylbutyl)-p-phenylenediamine, manufactured by Ouchi Shinko Chemical Industry Co., Ltd., Nocrac 6C Processing aid: stearic acid, manufactured by New Japan Chemical Co., Ltd., Stearic Acid 50S
[0111] <Preparation of test vulcanized molded article 1> The obtained rubber composition was press-vulcanized at 170°C for 20 minutes in accordance with JIS K 6299:2012 to prepare a sheet-like vulcanized molded article (test vulcanized molded article 1) having a thickness of 2 mm.
[0112] (Hardness) The test vulcanized molded articles 1 were stacked to a thickness of 6.0 mm or more to form a laminate. The hardness of the laminate was measured with a Type A durometer in accordance with JIS K 6253-3:2023. The thickness of the laminate was 6.0 to 7.0 mm.
[0113] (Water resistance (volume change rate after immersion in water at 70°C for 144 hours)) A test specimen measuring 25 mm in length and 20 mm in width was punched out from the above-mentioned vulcanized molded test article 1 to obtain a test specimen. The obtained test specimen was immersed in water at 70°C for 144 hours. The volume change rate ΔV was calculated based on JIS K 6258. The obtained volume change rate ΔV was evaluated according to the following criteria: A: Less than 3% B: 3% or more but less than 6% C: 6% or more but less than 9% D: 9% or more
[0114] (Alkali Resistance (Volume Change After Immersion in 10% Sodium Hydroxide at 70°C for 144 Hours)) A test specimen measuring 25 mm in length and 20 mm in width was punched out from the above-mentioned test vulcanized molded article 1 to obtain a test specimen. The obtained test specimen was immersed in 10% sodium hydroxide at 70°C for 144 hours. The volume change ΔV was calculated based on JIS K 6258. The obtained volume change ΔV was evaluated according to the following criteria: A: Less than 4% B: 4% or more but less than 7% C: 7% or more but less than 10% D: 10% or more
[0115] (Heat Generation) The rubber composition was press-vulcanized at 170°C for 20 minutes to obtain a cylindrical vulcanized molded article (test vulcanized molded article 2) with a diameter of 15 mm and a height of 25 mm. Heat generation was evaluated by a constant strain flexometer test using a Goodrich Flexometer in accordance with JIS K 6265:2018. The constant strain flexometer test is a test method in which a dynamic repeated load is applied to a test specimen such as vulcanized rubber to evaluate fatigue characteristics due to heat generation within the test specimen. Specifically, a static initial load is applied to the test specimen under constant temperature conditions, and a constant amplitude sinusoidal vibration is then applied to measure the heat generation and creep amount of the test specimen that change over time. The test was performed in accordance with JIS K 6265:2018 under conditions of 40°C, a strain of 0.175 inches, a load of 55 pounds, and a vibration frequency of 1,800 vibrations per minute, and heat generation (°C) was measured.
[0116]
[0117]
[0118]
[0119]
Claims
1. A rubber composition comprising a rubber component, wherein X is the hardness of a laminate obtained by stacking test vulcanized moldings 1 of the rubber composition to a thickness of 6.0 mm or more, as measured with a type A durometer based on JIS K 6253-3:2023, and Y is the heat generated by evaluating test vulcanized moldings 2 of the rubber composition in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute, the hardness X and heat generation Y satisfy the following formula (1), and the test vulcanized molding 1 is a sheet-like vulcanized molding having a thickness of 2 mm obtained by press-vulcanizing the rubber composition based on JIS K 6299:2012 under conditions of 170°C and 20 minutes, The test vulcanized molded article 2 is a cylindrical vulcanized molded article having a diameter of 15 mm and a height of 25 mm, which is obtained by press-vulcanizing the rubber composition at 170° C. for 20 minutes. Rubber composition. 1.4X−Y>45.0 (1) 2. The rubber composition according to claim 1, wherein the hardness X is 40 or more and 98 or less.
3. The rubber composition according to claim 1 or 2, wherein the rubber component contains a chloroprene-based polymer.
4. The rubber composition according to claim 3, wherein the chloroprene polymer contains 80 to 100% by mass of chloroprene monomer units relative to 100% by mass of the chloroprene polymer.
5. A vulcanized molded article of the rubber composition according to claim 1 or 2.
6. A rubber roll comprising a core and a surface layer provided on the peripheral surface of the core, the surface layer including the vulcanized molded article according to claim 5, the rubber roll being used in at least one of an acid washing line and an alkali washing line.
7. A vulcanized molded article containing a rubber component, wherein when the vulcanized molded article is made into a test vulcanized molded article 1' having a thickness of 6.0 mm or more, the hardness measured with a type A durometer based on JIS K 6253-3:2023 is X', and when the vulcanized molded article is made into a cylindrical test vulcanized molded article 2' having a diameter of 15 mm and a height of 25 mm, the heat generation determined by evaluation in a constant strain flexometer test based on JIS K 6265:2018 under conditions of 40°C, strain of 0.175 inches, load of 55 pounds, and vibration frequency of 1,800 times per minute is Y', the hardness X' and heat generation Y' satisfy the following formula (2). 1.4X'-Y'>45.0 (2)
Citation Information
Patent Citations
Chloroprene-based rubber composition
JP2001342299A
Rubber composition and method for producing the same
JP2011042774A
Method of producing vinyl-cis-polybutadiene rubber and vinyl-cis-polybutadiene rubber
JP2012207052A
Rubber composition, vulcanizate thereof, and molded article
JP2020196786A
Rubber composition and vulcanized molding of the rubber composition
JP2021095493A