Hollow resin particles, production method therefor, and use thereof
Hollow resin particles with a polymer shell and a hollow core, composed of specific monomers, address the limitations of conventional particles by achieving low dielectric constants and loss tangents, along with heat resistance, for use in various electronic applications.
Patent Information
- Application Number
- PCT/JP2024/011351
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-24
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional hollow resin particles have high relative permittivity and dielectric loss tangent, insufficient heat resistance, and large particle sizes, limiting their applications in reducing the dielectric constant and dielectric loss tangent of resin layers in electronic equipment.
Development of hollow resin particles with a shell part and a hollow part, where the shell is composed of a polymer obtained by polymerizing a monomer composition containing (meth)acrylic acid ester compounds with a carboxyl group, aromatic crosslinking monomers, and hydrocarbon resins, achieving a low dielectric constant and dielectric loss tangent, along with excellent heat resistance and small particle diameters.
The resulting hollow resin particles exhibit a relative dielectric constant of less than 2.0 and a dielectric loss tangent of less than 0.004, providing effective heat resistance and enabling their use in semiconductor members, coating compositions, heat-insulating compositions, and light-diffusing compositions.
Smart Images

Figure JP2024011351_03102024_PF_FP_ABST
Abstract
Description
Hollow resin particles, their manufacturing method, and their uses
[0001] The present invention relates to hollow resin particles, a method for producing the same, and uses thereof.
[0002] In order to speed up information processing using electronic devices, attempts have been made to reduce the dielectric constant and dielectric loss tangent of the insulating layers of multilayer printed circuit boards. As part of these efforts, studies have been made to introduce airspace into the resin layer by mixing hollow particles, each having a shell portion and a hollow portion surrounded by the shell portion, into a thermosetting resin, thereby reducing the dielectric constant and dielectric loss tangent.
[0003] Furthermore, hollow resin particles used for such applications are required to have high heat resistance so that the hollow resin particles do not undergo substantial change even when heated, for example, during molding processing of a thermosetting resin containing the hollow resin particles or during use with solder.
[0004] Porous hollow polymer particles obtained by suspension polymerization of a monomer primarily composed of an acrylic polyfunctional monomer such as trimethylolpropane tri(meth)acrylate and an acrylic monofunctional monomer such as methyl methacrylate together with a hydrophobic solvent have been reported (Patent Document 1). However, acrylic resins generally have high relative permittivity and dielectric loss tangent values and insufficient heat resistance. For this reason, the porous hollow polymer particles described in Patent Document 1 are unsuitable for achieving a low dielectric constant and dielectric loss tangent of a resin layer. Furthermore, the porous hollow polymer particles described in Patent Document 1 have a large particle size, limiting the applications of resin compositions in which the hollow resin particles can be used.
[0005] Furthermore, hollow resin particles obtained by suspension polymerization of divinylbenzene together with a hydrophobic solvent have been reported (Patent Document 2). However, the hollow resin particles described in Patent Document 2 have a large particle size, so that the applications of resin compositions in which the hollow resin particles can be used are limited.
[0006] Furthermore, hollow resin particles have been reported that are obtained by reacting an isocyanate compound with an active hydrogen compound, and have a shell formed of a polymer having a urea bond and / or a urethane bond (Patent Document 3). However, hollow resin particles having a urethane composition have high values of relative permittivity and dielectric loss tangent, and therefore the hollow particles described in Patent Document 3 are unsuitable for the purpose of reducing the permittivity and dielectric loss tangent of a resin layer.
[0007] Japanese Patent No. 4445495 International Publication No. 2022-092076 Japanese Patent No. 6924533
[0008] The present invention has been made to solve the above-mentioned problems of the related art, and its main object is to provide hollow resin particles having a shell portion and a hollow portion surrounded by the shell portion, which hollow resin particles have a small particle diameter and can achieve a low dielectric constant and a low dielectric loss tangent and exhibit excellent heat resistance. It is also an object of the present invention to provide a simple method for producing such hollow resin particles. Furthermore, it is an object of the present invention to provide uses of such hollow resin particles.
[0009] [1] Hollow resin particles according to an embodiment of the present invention are hollow resin particles having a shell portion and a hollow portion surrounded by the shell portion, wherein the shell portion contains a polymer obtained by polymerizing a monomer composition containing a (meth)acrylic acid ester compound having a carboxyl group at its terminal, as represented by formula (1), and the average particle size is 0.1 μm to 10 μm. (R 1 represents H or CH3, L 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; and m L 1 , L 2 , and Q are independent of each other.)
[0010] [2] In the hollow resin particles described in [1] above, in the formula (1), L1 represents an alkanediyl group having 2 to 4 carbon atoms, L 2 represents an alkanediyl group having 2 to 4 carbon atoms, an alkenediyl group having 2 to 4 carbon atoms, or a phenylene group, and Q may represent an ester bond.
[0011] [3] In the hollow resin particles described in [1] or [2] above, the monomer composition may contain an aromatic crosslinkable monomer and at least one selected from the group consisting of a compound having an ether structure represented by formula (2) and an aromatic monofunctional monomer.
[0012] [4] In the hollow resin particles described in [3] above, when the total amount of the (meth)acrylic acid ester compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight, the aromatic crosslinkable monomer may be 1 part by weight to 60 parts by weight.
[0013] [5] In the hollow resin particles according to the above [3] or [4], the aromatic monofunctional monomer may be at least one selected from the group consisting of styrene, α-methylstyrene, ethylvinylbenzene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, vinylnaphthalene, and acenaphthylene.
[0014] [6] In the hollow resin particles according to any one of [3] to [5] above, the compound having an ether structure may be a polyphenylene ether having (meth)acryloyl groups at both ends.
[0015] [7] In the hollow resin particles according to any one of [1] to [6] above, the shell portion may contain 1 to 15 parts by weight of the hydrocarbon-based resin per 100 parts by weight of the total amount of the polymer and the hydrocarbon-based resin.
[0016] [8] The hollow resin particles according to any one of [1] to [7] above may have a 5% thermal weight loss temperature of 300°C or higher when heated at a rate of 10°C / min in a nitrogen atmosphere.
[0017] [9] The hollow resin particles according to any one of [1] to [8] above may have a relative dielectric constant of less than 2.0 and a dielectric loss tangent of less than 0.004 at a measurement frequency of 10 GHz.
[0018]
[10] The hollow resin particles according to any one of [1] to [9] above may be used in a resin composition for a semiconductor member.
[0019]
[11] The hollow resin particles according to any one of the above [1] to [9] may be used in a coating composition.
[0020]
[12] The hollow resin particles according to any one of the above [1] to [9] may be used in a heat insulating resin composition.
[0021]
[13] The hollow resin particles according to any one of the above [1] to [9] may be used in a light-diffusing resin composition.
[0022]
[14] The hollow resin particles according to any one of the above [1] to [9] may be used in a light diffusion film.
[0023]
[15] A resin composition for a semiconductor member according to an embodiment of the present invention contains the hollow resin particles according to any one of [1] to [9] above.
[0024]
[16] A coating composition according to an embodiment of the present invention contains the hollow resin particles described in any one of [1] to [9] above.
[0025]
[17] A heat insulating resin composition according to an embodiment of the present invention contains the hollow resin particles described in any one of [1] to [9] above.
[0026]
[18] A light-diffusing resin composition according to an embodiment of the present invention contains the hollow resin particles according to any one of [1] to [9] above.
[0027]
[19] A light diffusion film according to an embodiment of the present invention contains the hollow resin particles according to any one of [1] to [9] above.
[0028]
[20] A method for producing hollow resin particles according to an embodiment of the present invention is the method for producing hollow resin particles according to any one of the above items [1] to
[14] , comprising dispersing an organic mixed solution containing a monomer composition including a (meth)acrylic acid ester compound having a carboxyl group at its terminal represented by formula (1), an aromatic crosslinkable monomer, and at least one selected from the group consisting of a compound having an ether structure represented by formula (2) and an aromatic monofunctional monomer, a polymerization initiator, and an organic solvent having a boiling point of less than 100°C, in an aqueous solution containing at least one selected from the group consisting of a dispersion stabilizer and a surfactant, and performing suspension polymerization. (R 1 represents H or CH3, L 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; and m L 1 , L 2 , and Q are independent of each other.)
[0029]
[21] In the method for producing hollow resin particles according to
[20] above, when the total amount of the (meth)acrylic acid ester compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight, the aromatic crosslinkable monomer may be 1 part by weight to 60 parts by weight.
[0030]
[22] In the method for producing hollow resin particles according to
[20] or
[21] above, the organic mixed solution may contain a hydrocarbon-based resin, and the hydrocarbon-based resin may be 1 part by weight to 15 parts by weight when the total amount of the (meth)acrylic acid ester-based compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight.
[0031] According to an embodiment of the present invention, it is possible to provide hollow resin particles having a shell portion and a hollow portion surrounded by the shell portion, which can achieve a low dielectric constant and a low dielectric loss tangent, and can exhibit excellent heat resistance and have a small particle diameter. It is also possible to provide a simple method for producing such hollow resin particles. Furthermore, it is also possible to provide uses of such hollow resin particles.
[0032] FIG. 1 is a schematic cross-sectional view illustrating the structure of a hollow portion. FIG. 2 is a TEM photograph of a particle (1) obtained in Example 1. FIG. 3 is a TEM photograph of a particle (2) obtained in Example 2. FIG. 4 is a TEM photograph of a particle (3) obtained in Example 3. FIG. 5 is a TEM photograph of a particle (4) obtained in Example 4. FIG. 6 is a TEM photograph of a particle (5) obtained in Example 5. FIG. 7 is a TEM photograph of a particle (6) obtained in Example 6. FIG. 8 is a TEM photograph of a particle (7) obtained in Example 7. FIG. 9 is a TEM photograph of a particle (C1) obtained in Comparative Example 1. FIG. 10 is a TEM photograph of a particle (C2) obtained in Comparative Example 2. FIG. 11 is a TEM photograph of a particle (C3) obtained in Comparative Example 3.
[0033] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.
[0034] In this specification, the expression "(meth)acrylic" means "acrylic and / or methacrylic", and the expression "(meth)acrylate" means "acrylate and / or methacrylate".
[0035] <<1. Hollow Resin Particles>> <<1-1. Structure and Properties of Hollow Resin Particles>> The hollow resin particles according to an embodiment of the present invention are hollow resin particles having a shell portion and a hollow portion surrounded by the shell portion, and have an average particle diameter of 0.1 μm to 10 μm. Here, "hollow" means that the interior is filled with a substance other than resin, such as a gas or liquid, and preferably means that the interior is filled with a gas, in order to further exhibit the effects of the present invention.
[0036] The hollow portion may consist of a single hollow region, or may consist of multiple hollow regions or a porous structure. FIG. 1( a) is a schematic cross-sectional view of a hollow resin particle whose hollow portion consists of a single hollow region. FIG. 1( b) is a schematic cross-sectional view of a hollow resin particle whose hollow portion consists of multiple hollow regions. FIG. 1( c) is a schematic cross-sectional view of a hollow resin particle whose hollow portion consists of a porous structure. When the hollow portion consists of multiple hollow regions, it has multiple closed pores as shown in FIG. 1( b). When the hollow portion has a porous structure, it has interconnected pores like a three-dimensional network structure. When the hollow portion has a porous structure, for example, it may consist of a single hollow region (interconnected pores) or a mixture of multiple closed pores and one or more interconnected pores. From the viewpoint of preventing the resin component constituting the shell from being relatively large and penetrating into the hollow portion of the substrate, etc., it is preferable that the hollow portion consist of a single hollow region, but it may also have a porous structure.
[0037] By having an average particle diameter of 0.1 μm to 10 μm, the hollow resin particles can be used in resin compositions for a variety of applications. The average particle diameter of the hollow resin particles is preferably 0.1 μm to 5.0 μm, more preferably 0.15 μm to 1.0 μm, even more preferably 0.2 μm to 0.8 μm, and particularly preferably 0.3 μm to 0.6 μm. When the average particle diameter of the hollow resin particles is within the above range, the effects of the present invention can be more effectively achieved. If the average particle diameter of the hollow resin particles is less than 0.1 μm, the shell thickness becomes relatively thin, which may result in hollow resin particles that do not have sufficient strength. If the average particle diameter of the hollow resin particles is greater than 10 μm, phase separation between the polymer and the solvent, which occurs when the monomer component is polymerized during suspension polymerization, may be difficult to occur, which may make it difficult to form the shell. Furthermore, if the average particle diameter of the hollow resin particles is greater than 10 μm, the applications of resin compositions in which the hollow resin particles can be used are limited.
[0038] The hollow resin particles according to an embodiment of the present invention preferably have a 5% thermal weight loss temperature of 300°C or higher, more preferably 320°C or higher, even more preferably 340°C or higher, and particularly preferably 360°C or higher, when heated at a rate of 10°C / min in a nitrogen atmosphere. The upper limit of the 5% thermal weight loss temperature is preferably 500°C or lower. As long as the hollow resin particles according to an embodiment of the present invention have a 5% thermal weight loss temperature within the above range when heated at a rate of 10°C / min in a nitrogen atmosphere, the hollow resin particles according to an embodiment of the present invention can exhibit excellent heat resistance. If the hollow resin particles according to an embodiment of the present invention have a 5% thermal weight loss temperature outside the above range and too low when heated at a rate of 10°C / min in a nitrogen atmosphere, for example, when kneaded with a thermosetting resin, the hollow resin particles may be deformed by heating for the curing reaction, resulting in the loss of the hollow portion and the resulting reduced dielectric constant and dielectric loss tangent effects.
[0039] <1-2. Shell Portion> The shell portion contains a polymer (P1) obtained by polymerizing a monomer composition containing a (meth)acrylic acid ester compound having a terminal carboxyl group, represented by formula (1). (R 1 represents H or CH3, L 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; and m L 1 , L 2 , and Q are independent of each other.)
[0040] The shell portion having such a configuration can exhibit the effects of the present invention. Specifically, the (meth)acrylic acid ester-based compound having a carboxyl group at its terminal, represented by formula (1), is a hydrophilic compound. Generally, when a hydrophilic compound is incorporated into a monomer composition, it exhibits favorable dispersibility for the productivity of hollow resin particles, but it also tends to increase the dielectric constant of the polymer. In the present invention, by employing a (meth)acrylic acid ester-based compound having a carboxyl group at its terminal, represented by formula (1), it is possible to provide hollow resin particles that exhibit hydrophilicity while suppressing increases in the dielectric constant and dielectric dissipation factor of the polymer, thereby achieving low dielectric constants and low dielectric dissipation factors. This is presumably because the compound represented by formula (1) has a relatively small polarizability of the electric dipole due to its molecular weight and structure, thereby achieving low dielectric constants and low dielectric dissipation factors.
[0041] Hereinafter, the (meth)acrylic acid ester compound having a terminal carboxyl group represented by formula (1) will also be referred to as "compound A."
[0042] The content of the aromatic polymer (P1) in the shell is preferably 60% by weight to 100% by weight, more preferably 70% by weight to 100% by weight, even more preferably 80% by weight to 100% by weight, and particularly preferably 90% by weight to 100% by weight, in order to further exhibit the effects of the present invention.
[0043] <Polymer (P1)> The polymer (P1) is obtained by polymerizing a monomer composition containing compound A. That is, the polymer (P1) has structural units derived from compound A. Any appropriate polymer can be adopted as the polymer P1, as long as it is a polymer obtained by polymerizing a monomer composition containing compound A, as long as the effects of the present invention are not impaired.
[0044] In formula (1), L 1 is an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms, preferably an alkanediyl group having 2 to 6 carbon atoms, and more preferably an alkanediyl group having 2 to 4 carbon atoms.
[0045] In formula (1), L2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group, preferably an alkanediyl group having 2 to 6 carbon atoms, an alkenediyl group having 2 to 6 carbon atoms, or a phenylene group, more preferably an alkanediyl group having 2 to 4 carbon atoms, an alkenediyl group having 2 to 4 carbon atoms, or a phenylene group, and even more preferably an alkanediyl group having 2 to 4 carbon atoms.
[0046] In formula (1), Q is an ester bond, an ether bond, a carbonyl group, or a single bond, and is preferably an ester bond, an ether bond, or a carbonyl group. This configuration makes the polarizability of the electric dipole in compound A relatively small, thereby more effectively exhibiting the effects of the present invention. In formula (1), Q is more preferably an ester bond.
[0047] In formula (1), m is "-L 1 -Q-L 2 "m" represents the average number of moles of the bonding group represented by "-" (sometimes referred to as "chain length"). "m" is 1 to 5, preferably 1 to 4, more preferably 1 to 3, even more preferably 1 or 2, and particularly preferably 1.
[0048] In order to further exhibit the effects of the present invention, in formula (1), L 1 represents an alkanediyl group having 2 to 4 carbon atoms, L 2 represents an alkanediyl group having 2 to 4 carbon atoms, an alkenediyl group having 2 to 4 carbon atoms, or a phenylene group, and Q may represent an ester bond.
[0049] Examples of Compound A that can further exhibit the effects of the present invention include 2-methacryloyloxyethyl succinate, 2-methacryloyloxyethyl maleate, 2-methacryloyloxyethyl phthalate, 2-carboxyethyl acrylate, and 2-carboxyethyl acrylate oligomer.
[0050] Compound A may be 2-methacryloyloxyethyl succinate.
[0051] The compound A may be one kind or two or more kinds.
[0052] In terms of being able to more effectively exhibit the effects of the present invention, the monomer composition preferably contains compound A and another monomer that reacts with compound A. That is, polymer (P1) is preferably a polymer obtained by polymerizing a monomer composition that contains compound A and another monomer that reacts with compound A.
[0053] In order to further exhibit the effects of the present invention, the monomer composition may contain compound A, an aromatic crosslinkable monomer, and at least one selected from the group consisting of compounds having an ether structure represented by the following formula (2) and aromatic monofunctional monomers. That is, polymer (P1) may have a structural unit derived from compound A, a structural unit derived from the aromatic crosslinkable monomer, and at least one structural unit derived from a compound having an ether structure represented by the following formula (2) and aromatic monofunctional monomers.
[0054] Hereinafter, the compound having an ether structure represented by formula (2) will also be referred to as "compound B."
[0055] The total content of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer in the monomer composition is preferably 80% by weight to 100% by weight, more preferably 85% by weight to 100% by weight, even more preferably 90% by weight to 100% by weight, and particularly preferably 95% by weight to 100% by weight, in terms of being able to further exhibit the effects of the present invention.
[0056] In terms of being able to more effectively exhibit the effects of the present invention, the monomer composition preferably contains 10% by weight to 70% by weight of an aromatic crosslinkable monomer, 10% by weight to 70% by weight of at least one selected from the group consisting of compound B and aromatic monofunctional monomers, and 0.5% by weight to 30% by weight of compound A, and more preferably contains 20% by weight to 65% by weight of an aromatic crosslinkable monomer, 20% by weight to 65% by weight of at least one selected from the group consisting of compound B and aromatic monofunctional monomers, and 10% by weight of compound A. The composition preferably contains 30% to 25% by weight of an aromatic crosslinkable monomer, 30% to 60% by weight of at least one selected from the group consisting of compound B and aromatic monofunctional monomers, and 1.5% to 20% by weight of compound A, and particularly preferably contains 40% to 50% by weight of an aromatic crosslinkable monomer, 40% to 50% by weight of at least one selected from the group consisting of compound B and aromatic monofunctional monomers, and 2% to 18% by weight of compound A.
[0057] The monomer composition may contain compound A, an aromatic crosslinkable monomer, compound B, and an aromatic monofunctional monomer. That is, the polymer (P1) may have a structural unit derived from compound A, a structural unit derived from the aromatic crosslinkable monomer, a structural unit derived from compound B, and a structural unit derived from the aromatic monofunctional monomer.
[0058] The monomer composition may contain any appropriate other monomer other than compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer, as long as the effect of the present invention is not impaired. The other monomer may be one type only, or two or more types.
[0059] As the aromatic crosslinkable monomer, any appropriate aromatic crosslinkable monomer can be used as long as it is an aromatic monomer having crosslinkability and does not impair the effects of the present invention. Examples of such aromatic crosslinkable monomers include divinylbenzene, divinylnaphthalene, and diallyl phthalate, which can further demonstrate the effects of the present invention. Divinylbenzene is preferred as the aromatic crosslinkable monomer in terms of further demonstrating the effects of the present invention and reactivity.
[0060] The aromatic crosslinkable monomer may be used alone or in combination of two or more kinds.
[0061] In the monomer composition, when the total amount of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer is taken as 100 parts by weight, the aromatic crosslinkable monomer may be 1 part by weight to 60 parts by weight. Alternatively, when the total amount of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer is taken as 100 parts by weight, the aromatic crosslinkable monomer may be 10 parts by weight to 70 parts by weight, 20 parts by weight to 65 parts by weight, 30 parts by weight to 60 parts by weight, or 40 parts by weight to 50 parts by weight.
[0062] In the monomer composition, when the total amount of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer is 100 parts by weight, compound A may be 0.5 parts by weight to 30 parts by weight, 1 part by weight to 20 parts by weight, 1 part by weight to 15 parts by weight, or 1 part by weight to 10 parts by weight.
[0063] As long as the compound B has the ether structure represented by formula (2), any appropriate compound can be adopted as long as the effects of the present invention are not impaired. In terms of being able to further exhibit the effects of the present invention, such a compound is preferably polyphenylene ether. Examples of commercially available polyphenylene ethers include those under the trade name "Noryl" (manufactured by SABIC), the trade name "Iupiace" (manufactured by Mitsubishi Chemical Corporation), the trade name "Zylon" (manufactured by Asahi Kasei Corporation), and the trade name "OPE-2St" (manufactured by Mitsubishi Gas Chemical Company, Inc.).
[0064] In view of compatibility with the non-reactive solvent described below and the ease with which hollow resin particles having excellent heat resistance can be produced, the polyphenylene ether is preferably an oligomer, and preferably has a number average molecular weight (Mn) of 500 to 3,500.
[0065] Any appropriate aromatic monofunctional monomer can be used as the aromatic monofunctional monomer as long as it is a monofunctional aromatic monomer and does not impair the effects of the present invention. Examples of such aromatic monofunctional monomers include styrene, ethylvinylbenzene, α-methylstyrene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, and vinylnaphthalene, which can further exhibit the effects of the present invention. From the viewpoint of further exhibiting the effects of the present invention and reactivity, the aromatic monofunctional monomer is preferably at least one selected from the group consisting of styrene and ethylvinylbenzene.
[0066] The aromatic monofunctional monomer may be of one kind or of two or more kinds.
[0067] In the monomer composition, when the total amount of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer is taken as 100 parts by weight, the total amount of compound B and aromatic monofunctional monomer may be 10 parts by weight to 70 parts by weight, 20 parts by weight to 65 parts by weight, 30 parts by weight to 60 parts by weight, or 40 parts by weight to 50 parts by weight.
[0068] The polymer (P1) is formed by a polymerization reaction of the monomer composition, which is preferably a suspension polymerization reaction.
[0069] The shell portion may contain any appropriate other component as long as the effects of the present invention are not impaired. For example, the shell portion may contain a phase separation promoter. The phase separation promoter is, for example, a hydrocarbon-based resin. Therefore, the shell portion may contain a hydrocarbon-based resin. When the shell portion contains a hydrocarbon-based resin, it becomes easier to construct a particle structure having a shell portion and a hollow portion surrounded by the shell portion. Furthermore, when the shell portion contains a hydrocarbon-based resin, the effects of the present invention can be more effectively exhibited. The shell portion may contain 1 to 20 parts by weight of the hydrocarbon-based resin, 1 to 17 parts by weight, 1 to 15 parts by weight, or 2 to 15 parts by weight, relative to 100 parts by weight of the total amount of the polymer (P1) and the hydrocarbon-based resin.
[0070] Any appropriate compound can be used as the hydrocarbon-based resin as long as it does not impair the effects of the present invention. Examples of hydrocarbon-based resins include aliphatic / aromatic hydrocarbon resins, aromatic hydrocarbon resins, alicyclic hydrocarbon resins, and aliphatic hydrocarbon resins. The hydrocarbon-based resins may be used alone or in combination of two or more.
[0071] The aliphatic / aromatic hydrocarbon resin refers to a hydrocarbon resin in which an aliphatic hydrocarbon and an aromatic hydrocarbon are copolymerized, such as a resin polymerized using styrene, vinyltoluene, indene, piperylene, or the like as a main raw material.
[0072] The aromatic hydrocarbon resin is a resin obtained by polymerizing, for example, styrene, vinyltoluene, indene, or the like as a main raw material.
[0073] The alicyclic hydrocarbon resin is, for example, a resin obtained by hydrogenating an aliphatic / aromatic hydrocarbon resin or an aromatic hydrocarbon resin.
[0074] The aliphatic hydrocarbon resin is a hydrocarbon resin obtained by polymerizing one or more aliphatic hydrocarbons having a polymerizable unsaturated bond. In this specification, paraffin wax (for example, VYBAR manufactured by Nucera Solutions) is used. TM 260) is also included in hydrocarbon resins.
[0075] The shell portion may contain the polymer (P1) and further contain at least one non-crosslinkable polymer selected from the group consisting of polyolefins, styrene-based polymers, (meth)acrylic acid-based polymers, and styrene-(meth)acrylic acid-based polymers.
[0076] The content of the non-crosslinkable polymer in the shell portion is preferably 0% by weight to 40% by weight, more preferably 0% by weight to 30% by weight, even more preferably 0% by weight to 20% by weight, and particularly preferably 0% by weight to 10% by weight, in order to further exhibit the effects of the present invention.
[0077] Examples of polyolefins include polyethylene, polypropylene, poly-α-olefins, etc. From the viewpoint of solubility in the monomer composition, it is preferable to use a side-chain crystalline polyolefin using a long-chain α-olefin as a raw material, or a low-molecular-weight polyolefin or olefin oligomer produced using a metallocene catalyst.
[0078] Examples of styrene polymers include polystyrene, styrene-acrylonitrile copolymers, and acrylonitrile-butadiene-styrene copolymers.
[0079] Examples of the (meth)acrylic acid polymer include polymethyl(meth)acrylate, polyethyl(meth)acrylate, polybutyl(meth)acrylate, and polypropyl(meth)acrylate.
[0080] Examples of styrene-(meth)acrylic acid polymers include styrene-methyl(meth)acrylate copolymer, styrene-ethyl(meth)acrylate copolymer, styrene-butyl(meth)acrylate copolymer, and styrene-propyl(meth)acrylate copolymer.
[0081] <1-3. Dielectric Constant and Dielectric Loss Tangent of Hollow Resin Particles> In electronic devices, which are one application of hollow resin particles, the transmission loss caused by radio waves transmitted for communication being converted into heat in a dielectric is expressed as the product of the square root of the frequency, the dielectric constant, and the dielectric loss tangent. In other words, since the transmission signal is more likely to be converted into heat in proportion to the frequency, the higher the frequency band, the lower the dielectric properties required of the materials used for communication components (semiconductor components) in order to suppress transmission loss.
[0082] Therefore, the relative dielectric constant of the hollow resin particles according to an embodiment of the present invention is preferably 1.0 to 2.5, more preferably 1.0 to 2.3, and even more preferably 1.0 to 2.0, at a measurement frequency of 10 GHz.
[0083] The dielectric loss tangent of the hollow resin particles according to an embodiment of the present invention is preferably 0 to 0.005, more preferably 0 to 0.0045, and even more preferably 0 to 0.004, at a measurement frequency of 10 GHz. When the relative dielectric constant and dielectric loss tangent of the hollow resin particles according to an embodiment of the present invention are within the above ranges, the effects of the present invention can be more effectively exhibited. The hollow resin particles according to an embodiment of the present invention preferably have a relative dielectric constant of less than 2.0 and a dielectric loss tangent of less than 0.004, at a measurement frequency of 10 GHz.
[0084] When the hollow resin particles according to the embodiment of the present invention have a dielectric constant greater than 2.5 and a dielectric loss tangent greater than 0.005, even if the hollow resin particles are mixed with, for example, a thermosetting resin, a sufficient effect of lowering the dielectric constant cannot be obtained, and when used in a high frequency band, transmission loss may occur and the amount of heat generated by the component may increase. In particular, when the hollow resin particles have a dielectric constant greater than 2.05 and a dielectric loss tangent greater than 0.004, the above-mentioned problems may occur more frequently.
[0085] The values of the dielectric constant and the dielectric loss tangent of the hollow resin particles according to the embodiment of the present invention are not limited to those described above. For example, when the hollow resin particles according to the embodiment of the present invention are used for applications other than semiconductor materials, the values of the dielectric constant and the dielectric loss tangent are not limited to those described above.
[0086] <1-4. Uses of hollow resin particles> The hollow resin particles according to an embodiment of the present invention can be used in a variety of applications. Because the effects of the present invention can be more effectively utilized, the hollow resin particles according to an embodiment of the present invention are suitable for semiconductor components, and can be typically used in resin compositions for semiconductor components. In addition to the applications in the resin compositions for semiconductor components described above, the hollow resin particles according to an embodiment of the present invention can also be used in applications such as paint compositions, cosmetics, paper coating compositions, heat insulating compositions, light diffusing compositions, and light diffusing films.
[0087] <Resin Composition for Semiconductor Member> The hollow resin particles according to an embodiment of the present invention can achieve a low dielectric constant and a low dielectric loss tangent and exhibit excellent heat resistance, and therefore can be suitably used in a resin composition for a semiconductor member.
[0088] The resin composition for a semiconductor member according to an embodiment of the present invention contains hollow resin particles according to an embodiment of the present invention.
[0089] The term "semiconductor member" refers to a member that constitutes a semiconductor, such as a semiconductor package or a semiconductor module. In this specification, the term "resin composition for a semiconductor member" refers to a resin composition used for a semiconductor member.
[0090] A semiconductor package is constructed using an IC chip as an essential component and at least one member selected from a mold resin, an underfill material, a mold underfill material, a die bond material, a prepreg for a semiconductor package substrate, a metal-clad laminate for a semiconductor package substrate, and a build-up material for a printed circuit board for a semiconductor package.
[0091] A semiconductor module is constructed using a semiconductor package as an essential component and at least one member selected from a prepreg for a printed circuit board, a metal-clad laminate for a printed circuit board, a build-up material for a printed circuit board, a solder resist material, a coverlay film, an electromagnetic wave shielding film, and an adhesive sheet for a printed circuit board.
[0092] <Coating Composition> The hollow resin particles according to an embodiment of the present invention can impart an excellent appearance to a coating film containing the hollow resin particles, and therefore can be suitably used in a coating composition.
[0093] A coating composition according to an embodiment of the present invention includes hollow resin particles according to an embodiment of the present invention.
[0094] The coating composition according to an embodiment of the present invention preferably contains at least one selected from a binder resin and a UV-curable resin. The binder resin may be of only one type or may contain two or more types. The UV-curable resin may be of only one type or may contain two or more types.
[0095] Any suitable binder resin can be used as long as it does not impair the effects of the present invention. Examples of such binder resins include resins soluble in organic solvents or water, and emulsion-type aqueous resins that can be dispersed in water. Specific examples of binder resins include acrylic resins, alkyd resins, polyester resins, polyurethane resins, chlorinated polyolefin resins, and amorphous polyolefin resins.
[0096] As the UV-curable resin, any appropriate UV-curable resin can be used as long as it does not impair the effects of the present invention. Examples of such UV-curable resins include polyfunctional (meth)acrylate resins and polyfunctional urethane acrylate resins. Polyfunctional (meth)acrylate resins are preferred, and polyfunctional (meth)acrylate resins having three or more (meth)acryloyl groups in one molecule are more preferred. Specific examples of polyfunctional (meth)acrylate resins having three or more (meth)acryloyl groups in one molecule include trimethylolpropane tri(meth)acrylate, trimethylolethane tri(meth)acrylate, 1,2,4-cyclohexane tetra(meth)acrylate, pentaglycerol triacrylate, pentaerythritol tetra(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol triacrylate, dipentaerythritol pentaacrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol triacrylate, and tripentaerythritol hexaacrylate.
[0097] When the coating composition according to an embodiment of the present invention contains at least one selected from a binder resin and a UV-curable resin, any appropriate content ratio can be adopted depending on the purpose. Typically, the hollow resin particles according to an embodiment of the present invention are preferably contained in an amount of 5 to 50% by weight, more preferably 10 to 50% by weight, and even more preferably 20 to 40% by weight of the total amount of the binder resin (in terms of solids content in the case of an emulsion-type aqueous resin), the at least one selected from the UV-curable resin, and the hollow resin particles according to an embodiment of the present invention.
[0098] When a UV-curable resin is used, a photopolymerization initiator is preferably used in combination. Any appropriate photopolymerization initiator can be used as long as it does not impair the effects of the present invention. Examples of such photopolymerization initiators include acetophenones, benzoins, benzophenones, phosphine oxides, ketals, α-hydroxyalkylphenones, α-aminoalkylphenones, anthraquinones, thioxanthones, azo compounds, peroxides (described in JP 2001-139663 A, etc.), 2,3-dialkyldione compounds, disulfide compounds, fluoroamine compounds, aromatic sulfonium compounds, onium salts, borate salts, active halogen compounds, and α-acyloxime esters.
[0099] The coating composition according to the embodiment of the present invention may contain a solvent. The solvent may be one kind or two or more kinds. When the coating composition according to the embodiment of the present invention contains a solvent, any appropriate content ratio can be adopted depending on the purpose.
[0100] As the solvent, any appropriate solvent can be used as long as it does not impair the effects of the present invention. Such a solvent is preferably a solvent that can dissolve or disperse a binder resin or a UV-curable resin. Examples of such solvents include, for oil-based paints, hydrocarbon solvents such as toluene and xylene; ketone solvents such as methyl ethyl ketone and methyl isobutyl ketone; ester solvents such as ethyl acetate and butyl acetate; and ether solvents such as dioxane, ethylene glycol diethyl ether, and ethylene glycol monobutyl ether. For water-based paints, examples of such solvents include water and alcohols.
[0101] The coating composition according to the embodiment of the present invention may be diluted to adjust the viscosity as needed. Any appropriate diluent may be used depending on the purpose. Examples of such diluents include the solvents described above. The diluent may be one type or two or more types.
[0102] The coating composition according to an embodiment of the present invention may contain other components, such as a coating surface conditioner, a flowability conditioner, an ultraviolet absorber, a light stabilizer, a curing catalyst, an extender pigment, a color pigment, a metallic pigment, a mica powder pigment, or a dye, as needed.
[0103] When forming a coating film using the coating composition according to an embodiment of the present invention, any appropriate coating method can be adopted depending on the purpose, such as spray coating, roll coating, brush coating, coating reverse roll coating, gravure coating, die coating, comma coating, and spray coating.
[0104] When forming a coating film using the coating composition according to an embodiment of the present invention, any suitable method can be adopted depending on the purpose. For example, a coating film can be formed by applying the composition to any surface of a substrate, drying the coating film, and then curing the coating film as needed. Examples of substrates include metal, wood, glass, and plastics (PET (polyethylene terephthalate), PC (polycarbonate), acrylic resin, TAC (triacetyl cellulose), etc.).
[0105] The hollow resin particles according to an embodiment of the present invention can impart excellent heat insulating properties to a coating film containing the hollow resin particles, and therefore can be suitably used in a heat insulating resin composition. A coating film containing the hollow resin particles according to an embodiment of the present invention can exhibit excellent reflectance in the wavelength range from ultraviolet light to near-infrared light.
[0106] The heat insulating resin composition according to an embodiment of the present invention includes hollow resin particles according to an embodiment of the present invention.
[0107] The heat insulating resin composition according to an embodiment of the present invention preferably contains at least one selected from a binder resin and a UV-curable resin. The above-mentioned explanations regarding the coating composition can be applied to the binder resin and the UV-curable resin.
[0108] The heat insulating resin composition according to the embodiment of the present invention may contain a solvent. Regarding the solvent, the above explanation regarding the coating composition may be cited.
[0109] The heat insulating resin composition according to the embodiment of the present invention may be diluted to adjust the viscosity as needed. The above description of the coating composition can be used as the diluent.
[0110] The heat insulating resin composition according to an embodiment of the present invention may contain other components, such as a coating surface conditioner, a flowability conditioner, an ultraviolet absorber, a light stabilizer, a curing catalyst, an extender pigment, a color pigment, a metal pigment, a mica powder pigment, or a dye, as needed.
[0111] When a coating film is formed using the heat insulating resin composition according to an embodiment of the present invention, the coating method and formation method can be applied as described above for the coating composition.
[0112] <Light-diffusing resin composition> The hollow resin particles according to an embodiment of the present invention can impart excellent light-diffusing properties to a coating film containing the hollow resin particles, and therefore can be suitably used in a light-diffusing resin composition.
[0113] The light-diffusing resin composition according to an embodiment of the present invention includes hollow resin particles according to an embodiment of the present invention.
[0114] The light-diffusing resin composition according to an embodiment of the present invention preferably contains at least one selected from a binder resin and a UV-curable resin. The above-mentioned explanations regarding the coating composition can be applied to the binder resin and the UV-curable resin.
[0115] The light-diffusing resin composition according to the embodiment of the present invention may contain a solvent. Regarding the solvent, the above explanation regarding the coating composition may be cited.
[0116] The light-diffusing resin composition according to the embodiment of the present invention may be diluted to adjust the viscosity as needed. The above-mentioned description of the coating composition may be applied to the diluent.
[0117] The light-diffusing resin composition according to an embodiment of the present invention may contain other components, such as a coating surface conditioner, a flowability conditioner, an ultraviolet absorber, a light stabilizer, a curing catalyst, an extender pigment, a color pigment, a metal pigment, a mica powder pigment, or a dye, as needed.
[0118] When forming a coating film using the light-diffusing resin composition according to an embodiment of the present invention, the coating method and formation method can be applied as described above for the coating composition.
[0119] <Light Diffusion Film> The hollow resin particles according to an embodiment of the present invention can impart excellent light diffusibility to a film having a coating film containing the hollow resin particles, and therefore can also be suitably used in a light diffusing film.
[0120] The light diffusion film according to an embodiment of the present invention includes hollow resin particles according to an embodiment of the present invention.
[0121] The light diffusion film according to an embodiment of the present invention includes a light diffusion layer formed from the light-diffusing resin composition according to an embodiment of the present invention and a substrate. The light diffusion layer may or may not be the outermost layer of the light diffusion film. The light diffusion film according to an embodiment of the present invention may include any appropriate other layer depending on the purpose. Examples of such other layers include a protective layer, a hard coat layer, a planarizing layer, a high refractive index layer, an insulating layer, a conductive resin layer, a conductive metal fine particle layer, a conductive metal oxide fine particle layer, and a primer layer.
[0122] Examples of the substrate include metal, wood, glass, plastic film, plastic sheet, plastic lens, plastic panel, cathode ray tube, fluorescent display tube, and liquid crystal display panel. Examples of the plastic that constitutes the plastic film, plastic sheet, plastic lens, and plastic panel include polyethylene terephthalate (PET), polycarbonate (PC), acrylic resin, and triacetyl cellulose (TAC).
[0123] <<2. Method for Producing Hollow Resin Particles>> A method for producing hollow resin particles according to an embodiment of the present invention comprises dispersing, in an aqueous solution containing at least one selected from the group consisting of a dispersion stabilizer and a surfactant, a monomer composition including a (meth)acrylic acid ester compound having a carboxyl group at its terminal represented by formula (1), an aromatic crosslinkable monomer, and at least one selected from the group consisting of a compound having an ether structure represented by formula (2) and an aromatic monofunctional monomer, a polymerization initiator, and an organic mixed solution including an organic solvent having a boiling point of less than 100°C, and performing suspension polymerization. (R 1 represents H or CH3, L 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; and m L 1 , L2 , and Q are independent of each other.)
[0124] Dispersion of the organic mixed solution in the aqueous solution is not particularly limited, and can be carried out by any known method, as long as the organic mixed solution can be present in the aqueous solution in the form of droplets.
[0125] In the method for producing hollow resin particles according to an embodiment of the present invention, the monomer composition contained in the organic mixed solution contains at least one selected from the group consisting of a (meth)acrylic acid ester compound having a carboxyl group at its terminal, represented by formula (1), an aromatic crosslinkable monomer, and a compound having an ether structure, represented by formula (2), and an aromatic monofunctional monomer. This allows the use of an organic solvent having a boiling point of less than 100°C as the organic solvent used in suspension polymerization, making it easier to remove the solvent from the hollow portions of the obtained hollow resin particles and enabling reduction in production costs.
[0126] <2-1. Aqueous Solution (Aqueous Phase)> The aqueous solution contains an aqueous medium and at least one selected from the group consisting of a dispersion stabilizer and a surfactant.
[0127] Examples of aqueous media include water and mixed media of water and lower alcohols (methanol, ethanol, etc.).
[0128] Examples of dispersion stabilizers include polyvinyl alcohol, polycarboxylic acid, celluloses (hydroxyethyl cellulose, carboxymethyl cellulose, etc.), and polyvinylpyrrolidone. Inorganic water-soluble polymer compounds such as sodium tripolyphosphate can also be used in combination. Other examples include phosphates such as calcium phosphate, magnesium phosphate, aluminum phosphate, and zinc phosphate; pyrophosphates such as calcium pyrophosphate, magnesium pyrophosphate, aluminum pyrophosphate, and zinc pyrophosphate; and poorly water-soluble inorganic compounds such as calcium carbonate, magnesium carbonate, calcium hydroxide, magnesium hydroxide, aluminum hydroxide, calcium metasilicate, calcium sulfate, barium sulfate, and colloidal silica.
[0129] The amount of the dispersion stabilizer added is preferably 0.5 to 10 parts by weight based on 100 parts by weight of the organic mixed solution. Only one type of dispersion stabilizer may be used, or two or more types may be used.
[0130] Examples of the surfactant include anionic surfactants, cationic surfactants, zwitterionic surfactants, and nonionic surfactants.
[0131] Examples of the anionic surfactant include non-reactive anionic surfactants such as alkyl sulfate fatty acid salts, alkylbenzenesulfonates, alkylnaphthalenesulfonates, alkanesulfonates, alkyldiphenylethersulfonates, dialkylsulfosuccinates, monoalkylsulfosuccinates, and polyoxyethylene alkylphenylether phosphates; and reactive anionic surfactants such as polyoxyethylene-1-(allyloxymethyl) alkyl ether sulfate ammonium salts, polyoxyethylene alkylpropenylphenyl ether sulfate ammonium salts, and polyoxyalkylene alkenyl ether ammonium sulfate.
[0132] Examples of the cationic surfactant include alkyltrimethylammonium salts, alkyltriethylammonium salts, dialkyldimethylammonium salts, dialkyldiethylammonium salts, and N-polyoxyalkylene-N,N,N-trialkylammonium salts.
[0133] Examples of amphoteric surfactants include lauryl dimethylamine oxide, phosphate salts, and phosphite surfactants.
[0134] Examples of nonionic surfactants include polyoxyethylene alkyl ethers, polyoxyethylene alkylphenyl ethers, polyoxyethylene fatty acid esters, sorbitan fatty acid esters, polysorbitan fatty acid esters, polyoxyethylene alkylamines, glycerin fatty acid esters, and oxyethylene-oxypropylene block polymers.
[0135] The amount of surfactant added is preferably 0.01 to 1 part by weight based on 100 parts by weight of the organic mixed solution. Only one type of surfactant may be used, or two or more types may be used.
[0136] The aqueous solution may contain any other appropriate components as long as the effects of the present invention are not impaired.
[0137] <2-2. Organic Mixed Solution (Oil Phase)> The organic mixed solution contains a monomer composition including at least one selected from the group consisting of a (meth)acrylic acid ester compound (compound A) having a terminal carboxyl group represented by formula (1), an aromatic crosslinkable monomer, a compound (compound B) having an ether structure represented by formula (2) and an aromatic monofunctional monomer, a polymerization initiator, and an organic solvent having a boiling point of less than 100°C.
[0138] As for the monomer composition contained in the organic mixed solution, the explanation in the section <Polymer (P1)> in <1-2. Shell portion> of <<1. Hollow resin particles>> can be directly applied.
[0139] The content of the aromatic crosslinkable monomer in the organic mixed solution may be 1 part by weight to 60 parts by weight when the total amount of compound A, the aromatic crosslinkable monomer, compound B, and the aromatic monofunctional monomer is 100 parts by weight.
[0140] Any appropriate polymerization initiator may be used as long as it does not impair the effects of the present invention. Examples of such polymerization initiators include organic peroxides such as lauroyl peroxide, benzoyl peroxide, orthochlorobenzoyl peroxide, orthomethoxybenzoyl peroxide, 3,5,5-trimethylhexanoyl peroxide, t-butylperoxy-2-ethylhexanoate, and di-t-butyl peroxide; and azo compounds such as 2,2'-azobisisobutyronitrile, 1,1'-azobiscyclohexanecarbonitrile, and 2,2'-azobis(2,4-dimethylvaleronitrile).
[0141] The amount of the polymerization initiator added is preferably in the range of 0.1 to 5 parts by weight based on 100 parts by weight of the monomer composition. The polymerization initiator may be of one kind or two or more kinds.
[0142] Examples of organic solvents having a boiling point of less than 100°C that are suitable for use in the method for producing hollow resin particles according to an embodiment of the present invention include heptane, hexane, cyclohexane, methyl acetate, ethyl acetate, methyl ethyl ketone, chloroform, and carbon tetrachloride.
[0143] The organic solvent having a boiling point of less than 100° C. may be a mixed solvent.
[0144] The amount of the organic solvent having a boiling point of less than 100° C. to be added is preferably 20 to 250 parts by weight based on 100 parts by weight of the monomer composition.
[0145] The organic mixed solution may contain any other appropriate components as long as the effects of the present invention are not impaired. Examples of such other components include hydrocarbon resins and non-crosslinkable polymers. Regarding the hydrocarbon resins and non-crosslinkable polymers, the explanations in <Polymer (P1)> under <1-2. Shell Portion> of <<1. Hollow Resin Particles>> may be used as is.
[0146] The amount of the hydrocarbon-based resin added in the organic mixed solution may be 1 to 20 parts by weight, 1 to 17 parts by weight, 1 to 15 parts by weight, or 2 to 15 parts by weight, when the total amount of compound A, aromatic crosslinkable monomer, compound B, and aromatic monofunctional monomer is taken as 100 parts by weight.
[0147] The amount of the non-crosslinkable polymer added is preferably 0 to 67 parts by weight based on 100 parts by weight of the monomer composition. Only one type of non-crosslinkable polymer may be used, or two or more types may be used.
[0148] <2-3. Suspension Polymerization> Hollow resin particles can be obtained by dispersing an organic mixed solution in an aqueous solution, polymerizing the resulting suspension, and preferably post-heating it.
[0149] Any suitable dispersion method can be adopted for the dispersion, as long as it can cause the organic mixed solution to exist in droplets in the aqueous solution, as long as the effects of the present invention are not impaired. A typical example of such a dispersion method is a dispersion method using a homogenizer, such as an ultrasonic homogenizer or a high-pressure homogenizer.
[0150] The polymerization temperature may be any suitable temperature suitable for suspension polymerization as long as it does not impair the effects of the present invention. Such a polymerization temperature is preferably 30°C to 80°C.
[0151] The polymerization time may be any suitable time suitable for suspension polymerization as long as it does not impair the effects of the present invention. Such a polymerization time is preferably 1 hour to 20 hours.
[0152] Post-heating, which is preferably carried out after polymerization, is a treatment suitable for obtaining hollow resin particles with a high degree of perfection.
[0153] The temperature for post-heating preferably carried out after polymerization can be any appropriate temperature within a range that does not impair the effects of the present invention, and the temperature for such post-heating is preferably 70°C to 120°C.
[0154] The time for post-heating preferably carried out after polymerization can be any appropriate time within the range that does not impair the effects of the present invention, and the time for such post-heating is preferably 1 hour to 10 hours.
[0155] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "parts" means "parts by weight" and "%" means "% by weight."
[0156] <Average Particle Diameter> The Z-average particle diameter of hollow resin particles or particles was measured using dynamic light scattering, and the measured Z-average particle diameter was used as the average particle diameter of the obtained hollow resin particles or particles. First, the obtained hollow resin particles or particles were diluted with ion-exchange water, and the aqueous dispersion adjusted to 0.1 wt % was irradiated with laser light, and the scattered light intensity from the hollow resin particles or particles was measured over time in microseconds. The detected scattering intensity distribution due to the hollow resin particles or particles was then fitted to a normal distribution, and the Z-average particle diameter of the hollow resin particles or particles was calculated using cumulant analysis to calculate the average particle diameter. This Z-average particle diameter measurement can be easily performed using a commercially available particle size measurement device. In the following examples and comparative examples, the Z-average particle diameter was measured using a particle size measurement device (Malvern Zetasizer Nano ZS). Typically, commercially available particle size measurement devices are equipped with data analysis software, which automatically analyzes the measurement data to calculate the Z-average particle diameter.
[0157] <TEM Measurement: Observation of the Presence or Absence of Hollowness and Shape of Hollow Resin Particles> Hollow resin particles or particles as a dry powder were subjected to a surface treatment (10 Pa, 5 mA, 10 seconds) using an "Osmium Coater Neoc-Pro" coating device manufactured by Meiwafosis Co., Ltd. The hollow resin particles or particles were then observed with a TEM (transmission electron microscope, H-7600 manufactured by Hitachi High-Technologies Corporation) to confirm the presence or absence of hollowness and the shape of the hollow resin particles or particles. Images were taken at an acceleration voltage of 100 kV and magnifications of 10,000x, 15,000x, or 20,000x.
[0158] <Measurement of 5% Thermal Weight Loss Temperature when Heating at 10°C / min in a Nitrogen Atmosphere> The 5% thermal weight loss temperature was measured using a "NEXTA STA200RV" differential thermal thermogravimetric simultaneous analyzer manufactured by Hitachi High-Tech Science Corporation. The sampling method and temperature conditions were as follows. 10.5±0.5 mg of sample was packed tightly into the bottom of a platinum measurement vessel to prepare a measurement sample. The 5% thermal weight loss temperature was measured using alumina as the reference material under a nitrogen gas flow rate of 200 mL / min. The TG / DTA curve was obtained by heating the sample from 30°C to 800°C at a heating rate of 10°C / min. The temperature at which the 5% weight loss occurred was calculated from the obtained curve using the analysis software provided with the instrument, and was taken as the 5% thermal weight loss temperature.
[0159] <Productivity> After the completion of polymerization, the entire amount of the slurry obtained was passed through a JIS test sieve (mesh size: 75 μm) (JIS standard number: Z 8801-1:2019) while being manually shaken. The hollow resin particles remaining on the sieve (particles that did not pass through the sieve) were dried and weighed. The relative ratio to the total amount of polymer was calculated and used as a measure of productivity.
[0160] <Dielectric Properties of Hollow Resin Particles> The dielectric properties of the hollow resin particles were measured using a dielectric constant measuring device (ADMS01Nc series) manufactured by AET Co., Ltd. The relative dielectric constant and dielectric loss tangent of the hollow resin particles were calculated based on perturbation theory using a resonator at a frequency of 10 GHz under the measurement environment of 23°C and a relative humidity of 51±1%.
[0161] Example 1 66.2 g of reactive low-molecular-weight polyphenylene ether (trade name "Noryl (registered trademark) SA9000-111 resin", manufactured by SABIC Corporation) as a compound having an ether structure (compound B), 99.4 g of divinylbenzene (DVB) 810 (manufactured by Nippon Steel Chemical & Material Co., Ltd., 81% content, 19% is ethylvinylbenzene (EVB)), 60 g of heptane, VYBAR TMAn oil phase was prepared by mixing 9.0 g of 260 (paraffin wax, manufactured by Nucera Solutions), 5.4 g of 2-methacryloyloxyethyl succinate (Light Ester HO-MS(N), manufactured by Kyoeisha Chemical Co., Ltd.) as Compound A, and 3.0 g of lauroyl peroxide (Perloyl L, manufactured by NOF Corporation). Next, 1,360 g of ion-exchanged water and 1.09 g of a surfactant (Aqualon AR-10, manufactured by Dai-ichi Kogyo Seiyaku Co., Ltd.) were mixed to prepare an aqueous phase. The oil phase was added to the aqueous phase, and the mixture was dispersed at 7,000 rpm for 5 minutes using a Polytron homogenizer "PT10-35" (manufactured by Central Scientific Trading Co., Ltd.), followed by emulsification at a processing pressure of 20 MPa using a high-pressure emulsifier NVL-AS200 (manufactured by Yoshida Kikai Kogyo Co., Ltd.) to prepare a suspension. The resulting suspension was heated at 70°C for 5 hours to polymerize, yielding a slurry. The obtained slurry was heated and dried to obtain particles (1) as a dry powder. The average particle diameter of the obtained particles (1) was 373 nm. The TEM observation results of the obtained hollow resin particles (1) are shown in Figure 2. It was confirmed that the particles (1) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (1) when heated at a rate of 10°C / min under a nitrogen atmosphere was 396.0°C. The relative dielectric constant of the obtained particles was 1.69, and the dielectric loss tangent was 0.0029. The blending amounts and various measurement results are shown in Table 1.
[0162] Example 2 Particles (2) were obtained in the same manner as in Example 1, except that the amount of reactive low-molecular-weight polyphenylene ether (trade name "Noryl (registered trademark) SA9000-111 resin", manufactured by SABIC Corporation) used was changed to 53.6 g, and the amount of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), manufactured by Kyoeisha Chemical Co., Ltd.) used as Compound A was changed to 18.0 g. The average particle diameter of the obtained particles (2) was 423 nm. The TEM observation results of the obtained particles (2) are shown in FIG. 3 . It was confirmed that the particles (2) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (2) when heated at a rate of 10°C / min under a nitrogen atmosphere was 369.1°C. The relative dielectric constant of the obtained particles was 1.72, and the dielectric loss tangent was 0.0033. The blending amounts and various measurement results are shown in Table 1.
[0163] Example 3 Particles (3) were obtained in the same manner as in Example 1, except that 66.2 g of styrene was used instead of 66.2 g of reactive low-molecular-weight polyphenylene ether (trade name "Noryl (registered trademark) SA9000-111 resin", manufactured by SABIC Corporation). The average particle diameter of the obtained particles (3) was 392 nm. The TEM observation results of the obtained particles (3) are shown in FIG. 4. It was confirmed that the particles (3) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (3) when heated at a rate of 10°C / min under a nitrogen atmosphere was 373.1°C. The relative dielectric constant of the obtained particles was 1.83, and the dielectric loss tangent was 0.0033. The blending amounts and various measurement results are shown in Table 1.
[0164] Example 4: 52.9 g of reactive low-molecular-weight polyphenylene ether (trade name "Noryl (registered trademark) SA9000-111 resin", manufactured by SABIC Corporation), 79.4 g of divinylbenzene (DVB) 810 (manufactured by Nippon Steel Chemical & Material Co., Ltd., 81% content, 19% is ethylvinylbenzene (EVB)), 96 g of heptane, and 100 g of VYBAR TMParticles (4) were obtained in the same manner as in Example 1, except that the amount of 260 (paraffin wax, manufactured by Nucera Solutions) used was changed to 7.2 g, the amount of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS(N), manufactured by Kyoeisha Chemical Co., Ltd.) used was changed to 4.5 g, and the amount of lauroyl peroxide (Perloyl L, manufactured by NOF Corporation) used was changed to 2.4 g. The average particle diameter of the obtained particles (4) was 396 nm. The TEM observation results of the obtained particles (4) are shown in FIG. 5. It was confirmed that the hollow resin particles (4) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (4) when heated at a rate of 10°C / min under a nitrogen atmosphere was 392.4°C. The relative dielectric constant of the obtained particles was 1.48, and the dielectric dissipation factor was 0.0023. The blending amounts and various measurement results are shown in Table 1.
[0165] Example 5 Particles (5) were obtained in the same manner as in Example 1, except that the amount of divinylbenzene (DVB) 810 (manufactured by Nippon Steel Chemical & Material Co., Ltd., 81% content, 19% ethylvinylbenzene (EVB)) used was changed to 72.0 g and 27.0 g of styrene was used. The average particle diameter of the obtained particles (5) was 417 nm. The TEM observation result of the obtained particles (5) is shown in FIG. 6 . It was confirmed that the particles (5) were hollow resin particles with an internally porous structure surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (5) when heated at a rate of 10°C / min under a nitrogen atmosphere was 392.2°C. The relative dielectric constant of the obtained particles was 1.62 and the dielectric loss tangent was 0.0025. The blending amounts and various measurement results are shown in Table 1.
[0166] Example 6 Particles (6) were obtained in the same manner as in Example 1, except that the amount of divinylbenzene (DVB) 810 (manufactured by Nippon Steel Chemical & Material Co., Ltd., 81% content, 19% ethylvinylbenzene (EVB)) used was changed to 54.0 g and 45.0 g of styrene was used. The average particle diameter of the obtained particles (6) was 399 nm. The TEM observation result of the obtained particles (6) is shown in FIG. 7 . It was confirmed that the particles (6) were hollow resin particles with an internally porous structure surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (6) when heated at a rate of 10°C / min under a nitrogen atmosphere was 391.7°C. The relative dielectric constant of the obtained particles was 1.63 and the dielectric loss tangent was 0.0027. The blending amounts and various measurement results are shown in Table 1.
[0167] Example 7 Particles (7) were obtained in the same manner as in Example 1, except that the amount of reactive low-molecular-weight polyphenylene ether (trade name "Noryl (registered trademark) SA9000-111 resin", manufactured by SABIC) used was changed to 32.3 g and the amount of divinylbenzene (DVB) 810 (manufactured by Nippon Steel Chemical & Material Co., Ltd., 81% content, 19% ethylvinylbenzene (EVB)) used was changed to 133.3 g. The average particle diameter of the obtained particles (7) was 411 nm. The TEM observation result of the obtained particles (6) is shown in FIG. 8 . It was confirmed that the particles (7) were hollow resin particles with an internal porous structure surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (7) when heated at a rate of 10°C / min in a nitrogen atmosphere was 409.7°C. The relative dielectric constant of the obtained particles was 1.79 and the dielectric loss tangent was 0.0033. The blending amounts and various measurement results are shown in Table 1.
[0168] Comparative Example 1 Particles (C1) were obtained in the same manner as in Example 1, except that 5.4 g of polyethylene glycol propylene glycol monomethacrylate (BLEMMER 50PEP-300, NOF Corporation) was used instead of 5.4 g of 2-methacryloyloxyethyl succinate (Light Ester HO-MS (N), Kyoeisha Chemical Co., Ltd.). The average particle diameter of the obtained particles (C1) was 403 nm. The TEM observation results of the obtained particles (C1) are shown in FIG. 9 . It was confirmed that the hollow resin particles (C1) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (C1) when heated at a rate of 10°C / min under a nitrogen atmosphere was 387.7°C. The relative dielectric constant of the obtained particles was 1.77, and the dielectric loss tangent was 0.0050. The blending amounts and various measurement results are shown in Table 1.
[0169] Comparative Example 2 Particles (C2) were obtained in the same manner as in Example 1, except that 5.4 g of methoxypolyethylene glycol methacrylate (BLEMMER PME-100, NOF Corporation) was used instead of 5.4 g of 2-methacryloyloxyethyl succinic acid (Light Ester HO-MS (N), Kyoeisha Chemical Co., Ltd.). The average particle diameter of the obtained particles (C2) was 416 nm. The TEM observation results of the obtained particles (C2) are shown in FIG. 10 . It was confirmed that the particles (C2) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (C2) when heated at a rate of 10°C / min under a nitrogen atmosphere was 406.0°C. The relative dielectric constant of the obtained particles was 1.72, and the dielectric dissipation factor was 0.0051. The blending amounts and various measurement results are shown in Table 1.
[0170] Comparative Example 3 69.6 g of methyl methacrylate (MMA), 69.6 g of dipentaerythritol hexaacrylate (ADPH) (manufactured by Shin-Nakamura Chemical Co., Ltd.), 96 g of toluene, 5.0 g of polystyrene (non-crosslinked, weight-average molecular weight of 300,000), and 4.2 g of Perloyl L (polymerization initiator, manufactured by NOF Corporation) were mixed to prepare an oil phase. Next, 1,360 g of ion-exchanged water and 1.36 g of Rapisol A-80 (surfactant, manufactured by NOF Corporation) were mixed to prepare an aqueous phase. Except for the above, the same procedure as in Example 1 was repeated to obtain particles (C3) as a dry powder. The average particle diameter of the obtained particles (C3) was 476 nm. The TEM observation results of the obtained particles (C3) are shown in FIG. 11 . It was confirmed that particles (C3) were hollow resin particles having a single void surrounded by a shell. The 5% thermal weight loss temperature of the obtained particles (C3) when heated at a rate of 10°C / min under a nitrogen atmosphere was 325.0°C. The relative dielectric constant of the obtained particles was 1.88, and the dielectric loss tangent was 0.0143. The blending amounts and various measurement results are shown in Table 1.
[0171]
[0172] <Performance Evaluation: Evaluation of Relative Dielectric Constant and Dielectric Loss Tangent of Particle-Added Films> 0.425 g of the particles obtained in the Examples and Comparative Examples, 8.3 g of ethyl acetate, and 1.7 g of solvent-soluble polyimide KPI-MX300F (manufactured by Kawamura Sangyo Co., Ltd.) were degassed and stirred using a planetary stirring defoamer (manufactured by KURABO Corporation, "Mazerustar KK-250") to prepare a mixture for evaluation. The mixture for evaluation was applied to a 5 mm-thick glass plate using an applicator set to a wet thickness of 250 μm, and then heated at 60°C for 30 minutes, 90°C for 10 minutes, 150°C for 30 minutes, and 200°C for 30 minutes to remove ethyl acetate. Film samples containing each particle were then cooled to room temperature to obtain them. The relative dielectric constant and dielectric loss tangent of the resulting films were evaluated using a cavity resonance method (measurement frequency: 5.8 GHz). The measurement results were expressed as a relative percentage (%), with the measured value for a film containing no particles being 100%. The results are shown in Table 2.
[0173]
[0174] From the results in Table 2, it can be confirmed that the hollow resin particles provided by the present invention have the effect of lowering the relative dielectric constant and dielectric loss tangent of the substrate, and are therefore effective for the purpose of lowering the dielectric constant and dielectric loss tangent of semiconductor materials.
[0175] The hollow resin particles according to the embodiment of the present invention and the hollow resin particles obtained by the production method according to the embodiment of the present invention can be used as semiconductor materials and the like.
Claims
1. Hollow resin particles having a shell portion and a hollow portion surrounded by the shell portion, the shell portion comprising a polymer obtained by polymerizing a monomer composition containing a (meth)acrylic acid ester compound having a carboxyl group at its terminal, represented by formula (1), and having an average particle size of 0.1 μm to 10 μm. (R 1 is H or CH 3 represents 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; 1 , L 2 , and Q are independent of each other.) 2. In the formula (1), L 1 represents an alkanediyl group having 2 to 4 carbon atoms; L 2 2. The hollow resin particle according to claim 1, wherein represents an alkanediyl group having 2 to 4 carbon atoms, an alkenediyl group having 2 to 4 carbon atoms, or a phenylene group, and Q represents an ester bond.
3. The hollow resin particle according to claim 1, wherein the monomer composition comprises an aromatic crosslinkable monomer and at least one selected from the group consisting of a compound having an ether structure represented by formula (2) and an aromatic monofunctional monomer.
4. The hollow resin particles according to claim 3, wherein the amount of the aromatic crosslinkable monomer is 1 part by weight to 60 parts by weight when the total amount of the (meth)acrylic acid ester compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight.
5. The hollow resin particles according to claim 3, wherein the aromatic monofunctional monomer is at least one selected from the group consisting of styrene, α-methylstyrene, ethylvinylbenzene, vinyltoluene, o-chlorostyrene, m-chlorostyrene, p-chlorostyrene, vinylbiphenyl, vinylnaphthalene, and acenaphthylene.
6. The hollow resin particle according to claim 3, wherein the compound having an ether structure is a polyphenylene ether having (meth)acryloyl groups at both ends.
7. The hollow resin particle according to claim 1, wherein the shell portion contains 1 to 15 parts by weight of the hydrocarbon resin per 100 parts by weight of the total amount of the polymer and the hydrocarbon resin.
8. The hollow resin particles according to claim 1, wherein the 5% thermal weight loss temperature of said hollow resin particles when heated at a rate of 10° C. / min in a nitrogen atmosphere is 300° C. or higher.
9. The hollow resin particle according to claim 1, which has a relative dielectric constant of less than 2.0 and a dielectric loss tangent of less than 0.004 at a measurement frequency of 10 GHz.
10. The hollow resin particles according to claim 1, which are used in a resin composition for semiconductor members.
11. The hollow resin particles according to claim 1, which are used in a coating composition.
12. The hollow resin particles according to claim 1, which are used in a heat insulating resin composition.
13. The hollow resin particles according to claim 1, which are used in a light-diffusing resin composition.
14. The hollow resin particles according to claim 1, which are used in a light diffusing film.
15. A resin composition for semiconductor members, comprising the hollow resin particles according to any one of claims 1 to 9.
16. A coating composition comprising the hollow resin particles according to any one of claims 1 to 9.
17. A heat insulating resin composition comprising the hollow resin particles according to any one of claims 1 to 9.
18. A light-diffusing resin composition comprising the hollow resin particles according to any one of claims 1 to 9.
19. A light-diffusing film comprising the hollow resin particles according to any one of claims 1 to 9.
20. A method for producing hollow resin particles according to any one of claims 1 to 14, comprising dispersing a monomer composition containing a (meth)acrylic acid ester compound having a carboxyl group at its terminal as represented by formula (1), an aromatic crosslinkable monomer, and at least one selected from the group consisting of a compound having an ether structure as represented by formula (2) and an aromatic monofunctional monomer, a polymerization initiator, and an organic mixed solution containing an organic solvent having a boiling point of less than 100°C, in an aqueous solution containing at least one selected from the group consisting of a dispersion stabilizer and a surfactant, and carrying out suspension polymerization. (R 1 is H or CH 3 represents L 1 represents an alkanediyl group having 1 to 10 carbon atoms or an alkenediyl group having 2 to 10 carbon atoms; L 2 represents a single bond, an alkanediyl group having 1 to 10 carbon atoms, an alkenediyl group having 2 to 10 carbon atoms, or a phenylene group; Q represents an ester bond, an ether bond, a carbonyl group, or a single bond; m represents a number from 1 to 5; 1 , L 2 , and Q are independent of each other.) 21. A method for producing hollow resin particles according to claim 20, wherein the amount of the aromatic crosslinkable monomer is 1 part by weight to 60 parts by weight when the total amount of the (meth)acrylic acid ester compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight.
22. The method for producing hollow resin particles according to claim 20, wherein the organic mixed solution contains a hydrocarbon-based resin, and when the total amount of the (meth)acrylic acid ester compound, the aromatic crosslinkable monomer, the compound having an ether structure, and the aromatic monofunctional monomer is 100 parts by weight, the amount of the hydrocarbon-based resin is 1 part by weight to 15 parts by weight.
Citation Information
Patent Citations
Reaction mixture, porous particles, and production method
JP2016519199A
Hollow particle and use therefor
JP2020176266A
Resin particle
JP2021088641A
Hollow resin particles for semiconductor member resin composition
JP2022096299A
Hollow resin particles, their manufacturing method, and their uses
JP2023021971A
Cited By
Hollow resin particle and use thereof
WO2026034577A1
Hollow resin particle, resin composition for semiconductor member, and dispersion
WO2026141026A1
Hollow resin particles and resin composition for semiconductor member
WO2026196936A1
Particle, colored particle, sensitization particle, measurement reagent, and measurement method
WO2026205121A1