Method for controlling injection molding machine and method for producing injection-molded article
By adjusting cylinder and mold temperatures based on reference product pressure values, the method stabilizes injection molding conditions, addressing resin material variations and temperature fluctuations to enhance product quality and consistency.
Patent Information
- Application Number
- PCT/JP2024/011358
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional injection molding control methods fail to stabilize product dimensions and quality due to variations in resin material viscosity and solidification rate, especially when temperature fluctuations occur, leading to inconsistent mold pressure and poor product quality.
A method for controlling injection molding machines by using a reference product to adjust cylinder and mold temperatures based on peak pressure and pressure integral values, ensuring that the peak pressure and pressure reduction time or integral value match those of the reference product, thereby stabilizing the molding process despite temperature fluctuations.
This approach effectively reduces variations in injection molded product quality, particularly dimensional changes and appearance issues, by aligning the molding conditions with those of a reference product, even under temperature fluctuations.
Smart Images

Figure JP2024011358_03102024_PF_FP_ABST
Abstract
Description
Injection molding machine control method and injection molded product manufacturing method
[0001] The present invention relates to a method for controlling an injection molding machine and a method for manufacturing an injection-molded product.
[0002] In injection molding using thermoplastic resins, the dwell pressure and dwell time are adjusted to stabilize the dimensions and quality of the molded product. However, variations in viscosity and solidification rate due to the quality of the resin material can cause fluctuations in the pressure inside the mold (cavity pressure) during injection molding. This can result in variations in physical properties, dimensions, and appearance, resulting in quality problems. To address these variations in cavity pressure caused by variations in the quality of the resin material (viscosity, solidification rate, etc.), a conventional technique is to feed back the cavity pressure and reflect it in the screw forward pressure. Specifically, the peak cavity pressure can be controlled by detecting the peak cavity pressure using a cavity pressure sensor and correcting the error by reflecting it in the screw forward pressure.
[0003] In addition, Patent Document 1 describes an injection hold pressure control device that divides the control mode of injection hold pressure into an early process and a late process, controls the injection hold pressure using mold internal pressure for the early process and controls the injection hold pressure using hydraulic pressure in the injection cylinder for the late process, and has the function of continuing pressure control. Patent Document 2 describes a method for controlling resin pressure in an injection molding machine that performs injection molding by providing a strain gauge for detecting mold distortion near the resin passage or cavity of the injection mold and an internal mold pressure control unit that converts this mold distortion into resin pressure in the mold and controls the resin pressure, measuring mold distortion from the time molten resin is injected into the cavity until it is cooled and solidified, and controlling the internal mold resin pressure by the internal mold pressure control unit within a predetermined necessary and sufficient range of resin pressure in the mold.
[0004] JP-A No. 62-261419 JP-A No. 8-112842
[0005] However, the conventional control method based on correction of mold internal pressure described above is based on the assumption that there is no temperature fluctuation, and there is a problem in that when temperature fluctuation occurs, variations occur in the quality of the injection-molded product.
[0006] The present invention has been made in consideration of the above-mentioned problems of the conventional art, and an object of the present invention is to provide a control method for an injection molding machine that can adjust variations in injection-molded products caused by the quality of the resin material, even when temperature fluctuations occur, and a manufacturing method for resin-molded products that obtains injection-molded products using the control method for the injection molding machine.
[0007] One aspect of the present invention that solves the above-mentioned problems is as follows: (1) A control method for an injection molding machine that injects molten resin in a cylinder into a mold to produce an injection-molded product, comprising: setting an injection-molded product that is previously evaluated as a suitable product as a reference product; acquiring, in one injection molding of the reference product, the peak pressure in the mold and the pressure drop time from the start of injection to the time the pressure in the mold becomes zero or the pressure integrated value from the start of injection to the time the pressure in the mold becomes zero; and, in injection molding of a product to be manufactured, adjusting the cylinder temperature so that the peak pressure in the mold becomes the peak pressure in the mold of the reference product, and adjusting the temperature in the mold so that the pressure drop time or the pressure integrated value becomes the pressure drop time or the pressure integrated value of the reference product.
[0008] (2) A control method for an injection molding machine described in (1), wherein, during injection molding of the product to be manufactured, if the peak pressure in the mold is greater than the peak pressure in the mold for the reference product, the cylinder temperature is lowered, and if the peak pressure in the mold is less than the peak pressure in the mold for the reference product, the cylinder temperature is raised.
[0009] (3) A control method for an injection molding machine according to (1) or (2), wherein, in the injection molding of the product to be manufactured, if the pressure drop time in the mold is longer than the pressure drop time in the mold for the reference product, the mold temperature is lowered, and if the pressure drop time in the mold is shorter than the pressure drop time in the mold for the reference product, the mold temperature is raised.
[0010] (4) A control method for an injection molding machine described in any one of (1) to (3), wherein, during injection molding of the product to be manufactured, if the pressure integral value within the mold is greater than the pressure integral value within the mold of the reference product, the mold temperature is lowered, and if the pressure integral value within the mold is smaller than the pressure integral value within the mold of the reference product, the mold temperature is raised.
[0011] (5) A method for producing an injection-molded product, comprising controlling an injection molding machine by the method for controlling an injection molding machine according to any one of (1) to (4) above to produce an injection-molded product.
[0012] According to the present invention, it is possible to provide a control method for an injection molding machine that can adjust variations in injection-molded products caused by the quality of the resin material even when temperature fluctuations occur, and a manufacturing method for resin-molded products that obtains injection-molded products using the control method for the injection molding machine.
[0013] 1 is a diagram (master curve) showing pressure changes over time within a mold during injection molding. It is a diagram showing measurement positions for dimensions of dumbbell test specimens molded by injection molding in the examples. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained by injection molding under the same conditions using two types of resins with different melt viscosities. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained in Example 1-1. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained in Example 1-2. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained in Comparative Example 1-1. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained in Comparative Example 1-2. It is a graph showing dimensions at positions a, b, and c of dumbbell test specimens obtained in Comparative Example 3.
[0014] <Injection Molding Machine Control Method> The injection molding machine control method of this embodiment is a control method for an injection molding machine that injects molten resin in a cylinder into a mold to produce an injection-molded product. An injection-molded product that is evaluated as a suitable product is used as a reference product in advance. In one injection molding of the reference product, the peak pressure in the mold and the pressure drop time from the start of injection until the pressure in the mold reaches zero or the pressure integral value from the start of injection until the pressure in the mold reaches zero are obtained. Next, in injection molding of a product to be manufactured, the cylinder temperature is adjusted so that the peak pressure in the mold matches the peak pressure in the mold of the reference product, and the mold temperature is adjusted so that the pressure drop time or pressure integral value matches the pressure drop time or pressure integral value of the reference product.
[0015] In the control method for an injection molding machine according to this embodiment, an injection-molded product that is evaluated as being good, with minimal dimensional change and visual defects, is designated as a suitable product, and this suitable product is designated as a reference product. Then, when the reference product is injection-molded, the peak pressure in the mold during one injection molding cycle and the pressure drop time from the start of injection until the pressure in the mold reaches zero, or the pressure integral value from the start of injection until the pressure reaches zero, are acquired. It is believed that a suitable product can be obtained by setting the peak pressure in the mold, the pressure drop time, or the pressure integral value during injection molding of the reference product during injection molding of the target product. Therefore, during injection molding of the target product, the cylinder temperature is adjusted so that the peak pressure in the mold matches that of the reference product, and the mold temperature is adjusted so that the pressure drop time or the pressure integral value matches that of the reference product. Controlling the injection molding machine in this manner can suppress quality variations in injection-molded products, particularly dimensional change and visual defects, even when temperature fluctuations occur.
[0016] In the control method for an injection molding machine of this embodiment, first, an injection-molded product evaluated as a suitable product is determined as a reference product. Here, "suitable product" means an injection-molded product having desired properties, such as minimal dimensional change and visual defects. The suitable product can be determined by performing injection molding once or preferably multiple times in advance and selecting the injection-molded product with the best quality or the molded product that achieves the desired quality.
[0017] Next, in one injection molding of the reference product, the peak pressure in the mold and the pressure drop time from the start of injection to the time the pressure in the mold reaches zero, or the pressure integral value from the start of injection to the time the pressure in the mold reaches zero, are obtained. This will be explained with reference to the master curve shown in Figure 1. Figure 1 shows the change in pressure in the mold over time in one injection molding. The solid line is the master curve for the reference product, and the dashed line is the master curve for injection molding using a resin material with a higher melt viscosity than the reference product. The horizontal axis represents time, and the vertical axis represents the pressure in the mold. As shown in Figure 1, the pressure reaches its maximum in the circled region A. In other words, this maximum pressure is the peak pressure. The pressure then drops and finally reaches zero. The "pressure drop time" is the time from the start of injection to the time the pressure in the mold reaches zero. In Figure 1, the pressure drop time begins at the start of injection (0 seconds), reaches the peak pressure in approximately 3 seconds, and reaches zero in approximately 25 seconds, so the pressure drop time is approximately 25 seconds. On the other hand, the "pressure integral value" is the time integral value of pressure from the start of injection to the time when the pressure inside the mold becomes zero, and in FIG. 1, it is the area of the region surrounded by the master curve and the horizontal axis (the straight line where pressure = 0 MPa). Note that the "injection start time" in the pressure drop time and pressure integral value refers to the time when the injection of resin material into the mold begins in the injection molding machine. As described above, in this embodiment, the peak pressure inside the mold and the pressure drop time or pressure integral value are obtained in advance for a reference product.
[0018] The injection molding of the product to be manufactured is performed using the peak pressure in the mold and the pressure drop time or pressure integral value of the reference product obtained as described above. Specifically, the cylinder temperature is adjusted so that the peak pressure in the mold is the same as that of the reference product, and the temperature in the mold is adjusted so that the pressure drop time or pressure integral value is the same as that of the reference product. In other words, changes in the pressure in the mold due to variations in the resin material are corrected using the cylinder temperature and the temperature in the mold so that it is equivalent to that of the reference product. More specifically, (1) changes in the peak pressure in the mold due to variations in the melt viscosity of the resin material are corrected using the cylinder temperature, and (2) changes in the pressure drop time or pressure integral value in the mold due to variations in the solidification rate of the resin material are corrected using the mold temperature. Below, (1) and (2) are explained.
[0019] (1) Fluctuations in the peak pressure inside the mold due to variations in the melt viscosity of the resin material. Possible factors that cause changes in the pressure inside the mold include variations in the quality of the resin material and external disturbances (such as the temperature inside the mold and the cylinder temperature). The "melt viscosity," one of the characteristics of the resin material, is corrected using the "cylinder temperature." Specifically, the pressure value obtained from the injection molding machine's sensor is fed back to adjust the cylinder temperature so that the peak pressure inside the mold is the same as that of a reference product of appropriate quality. For example, if the peak pressure inside the mold during injection molding of the target product is higher than that of the reference product, the cylinder temperature is lowered. Conversely, if the peak pressure inside the mold is lower than that of the reference product, the cylinder temperature is raised. The cylinder temperature can be adjusted using temperature adjustment, PID control, or the like, as described in the examples below.
[0020] (2) Fluctuations in the pressure drop time or pressure integral value in the mold due to fluctuations in the solidification rate of the resin material. As described above, possible factors that cause changes in the pressure in the mold include variations in the quality of the resin material and external disturbances. The "solidification rate," one of the characteristics of the resin material, is corrected using the "mold temperature." That is, the mold temperature is adjusted so that the pressure drop time or pressure integral value in the mold is the same as that of a reference product of appropriate quality. For example, if the pressure drop time in the mold during injection molding of the target product is longer than that of the reference product, the mold temperature is lowered. Conversely, if the pressure drop time in the mold during injection molding of the target product is shorter than that of the reference product, the mold temperature is raised. Similarly, if the pressure integral value in the mold during injection molding of the target product is greater than that of the reference product, the mold temperature is lowered. Conversely, if the pressure integral value in the mold during injection molding of the target product is smaller than that of the reference product, the mold temperature is raised. The mold temperature can be adjusted using temperature adjustment, PID control, or the like, as described in the examples below.
[0021] In injection molding of a product to be manufactured, the timing for setting the peak pressure in the mold and the pressure drop time or pressure integral value to match the values of the reference product can be set for every arbitrary shot, for example, every 5 shots or every 10 shots.
[0022] The above-described adjustment of the mold temperature and cylinder temperature is controlled within the injection molding machine as follows. First, the deviation between the output value (peak pressure and fall time or pressure integral value) detected by the pressure sensor installed in the mold and the reference value (peak pressure and fall time or pressure integral value) of a reference product obtained in advance is determined. Next, the mold temperature and cylinder temperature are adjusted so that the deviation between the measured output value (peak pressure and fall time or pressure integral value) and the reference value (target value) of the master curve of the reference product is minimized. Furthermore, the above control can be performed by sequence control using a PLC (programmable logic controller) installed outside the injection molding machine. That is, correction based on the cylinder temperature and mold temperature is performed by sending a signal from the PLC to the injection molding machine. The signal transmission from the PLC to the injection molding machine can be performed, for example, by a program that adjusts the cylinder temperature and mold temperature based on the difference between the measured peak pressure output value and the reference value.
[0023] In the method for controlling an injection molding machine according to this embodiment, the resin material used for injection molding is not particularly limited as long as it is a thermoplastic resin, and various materials can be used.
[0024] <Method for manufacturing injection-molded products> The method for manufacturing injection-molded products of this embodiment controls an injection molding machine using the above-described injection molding machine control method to manufacture injection-molded products. Therefore, even when temperature fluctuations occur, it is possible to adjust for variations in the injection-molded products caused by the quality of the resin material, and to manufacture injection-molded products with little variation in quality.
[0025] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to the following examples.
[0026] <<Preparation of Injection-Molded Articles>> The following resin materials 1 and 2, which have different melt viscosities, were used and injection molded under the following molding conditions to obtain dumbbell test pieces (test piece type: 1A). Resin material 1: Polyacetal resin (DURACON (registered trademark) (standard product (MI = 9 g / 10 min)) manufactured by Polyplastics Co., Ltd.) Resin material 2: Polyacetal resin (DURACON (registered trademark) (high flow product (MI = 14 g / 10 min)) manufactured by Polyplastics Co., Ltd.) (Molding conditions) Cylinder temperature: 200°C Mold temperature: 80°C Injection speed: 17 mm / sec Dwell pressure: 80 MPa Injection dwell time: 30 sec Cooling time: 10 sec Sampling period: 1 / 1000 sec During injection molding, the pressure in the mold was monitored using a pressure sensor (Futaba Corporation, pressure sensor SSE (φ3)).
[0027] The state of the mold and dumbbell test specimen during injection molding is shown in Figure 2. As shown in Figure 2, molten resin flows into the mold 10 from the gate 12, reaches the other end, and is molded into the shape of a dumbbell test specimen 14. Inside the mold 10, the width of each of positions a, b, and c is 10 mm, and the pitch between positions a, b, and c is 30 mm.
[0028] The widths of a dumbbell test piece molded using resin material 1 (hereinafter referred to as the "reference product") and a dumbbell test piece molded using resin material 2 (hereinafter referred to as the "high flow product") were measured at positions a, b, and c. The measurement results are shown in Figure 3. In Figure 3, the dashed line shows the measurement results for the reference product, and the solid line shows the measurement results for the high flow product (the same applies to Figures 4 to 8).
[0029] On the other hand, for the reference product, a master curve similar to that shown in Figure 1 was created for the pressure change during injection molding, and the peak pressure inside the mold and the pressure integral value from the start of injection to the point when the pressure inside the mold becomes zero were calculated.
[0030] As shown in Figure 3, there is a difference in width between the reference product and the high-flow product at positions a, b, and c. This is thought to be due to the high-flow product's lower melt viscosity compared to the reference product, which increases the pressure and therefore the dimensions. As described above, when two resins with different melt viscosities are used and injection molded in the same manner, a difference in width dimension occurs. Therefore, in the following examples, to reduce such a difference in dimension, injection molding was performed by controlling the injection molding machine. Specifically, the injection molding machine was controlled to bring the high-flow product closer to the dimensions of the reference product. That is, the reference product was evaluated as the appropriate product, and the peak pressure in the mold during one injection molding of the reference product and the pressure integral value from the start of injection to the time when the pressure reached zero were obtained. Control was performed based on these values to bring the high-flow product closer to the reference product.
[0031] [Example 1-1] Dumbbell test specimens were obtained in the same manner as in the above "Preparation of Injection-Molded Products." However, in the injection molding of the high-flow product, the cylinder temperature was adjusted so that the peak pressure in the mold was the same as that in the injection molding of the reference product. Additionally, the mold temperature was adjusted so that the pressure was the integrated value from the start of injection to the point where the pressure became zero during the injection molding of the reference product. The widths of the dumbbell test specimens at positions a, b, and c for both the reference product and the high-flow product were then measured. The measurement results are shown in Figure 4. As can be seen from Figure 4, the difference in width between the dumbbell test specimens at positions a, b, and c was suppressed for both the reference product and the high-flow product.
[0032] [Example 1-2] Dumbbell test pieces for the reference product and the high flow product were obtained in the same manner as in Example 1-1, except that the mold temperature was set 5°C higher for both the reference product and the high flow product. The widths of the dumbbell test pieces at positions a, b, and c were then measured for both the reference product and the high flow product. The measurement results are shown in Figure 5. As shown in Figure 5, the deviation in width at positions a, b, and c of the dumbbell test pieces was suppressed for both the reference product and the high flow product. In other words, it can be seen that even when temperature fluctuations occurred, the deviation in width at positions a, b, and c of the dumbbell test pieces was suppressed for both the reference product and the high flow product. It was confirmed that the appearance of the injection-molded products in Examples 1-1 and 1-2 was equivalent for both the reference product and the high flow product.
[0033] [Comparative Example 1-1] Dumbbell test specimens were obtained in the same manner as in the above "Preparation of Injection-Molded Product." However, the injection molding of the high-flow product was adjusted so that the peak pressure in the mold was the same as that during injection molding of the reference product. The widths of the dumbbell test specimens at positions a, b, and c for both the reference product and the high-flow product were then measured. The measurement results are shown in Figure 6. As shown in Figure 6, the difference in width between the dumbbell test specimens at positions a, b, and c for both the reference product and the high-flow product was reduced.
[0034] [Comparative Example 1-2] Dumbbell test pieces for the reference product and the high flow product were obtained in the same manner as in Comparative Example 1-1, except that the mold temperature was set 5°C higher for both the reference product and the high flow product. The widths of the dumbbell test pieces for the reference product and the high flow product were then measured at positions a, b, and c. The measurement results are shown in Figure 7. As shown in Figure 7, there is a difference in width between the reference product and the high flow product at positions a, b, and c. That is, in Comparative Example 1-1, the difference in width dimension of the dumbbell test pieces was suppressed, whereas in Comparative Example 1-2, the rise in mold temperature meant that the difference in width dimension could no longer be suppressed. That is, if temperature fluctuations occur in the mold, simply adjusting the peak pressure in the mold will result in variations in the quality of the molded products.
[0035] [Comparative Example 3] Dumbbell test specimens for the reference product and the high flow product were obtained in the same manner as in Example 1-2, except that the mold temperature for the high flow product was not adjusted so that it was the pressure integral value from the start of injection to the point where the pressure became zero during injection molding of the reference product. That is, during injection molding of the high flow product, temperature control was performed only on the cylinder temperature. Then, the widths of the dumbbell test specimens for the reference product and the high flow product at positions a, b, and c were measured. The measurement results are shown in Figure 8. As shown in Figure 8, there is a difference in the widths at positions a, b, and c between the reference product and the high flow product. This result shows that temperature control is required for both the mold and the cylinder.
[0036] (1) Dimensional Change The dimensions of the injection-molded dumbbell test pieces in each Example and Comparative Example were measured at positions a to c, and a maximum difference from the standard was evaluated as good if it was 0.005 mm or less, and as bad if it was more than 0.005 mm. The evaluation results are shown in Table 1.
[0037]
[0038] From Table 1, it can be seen that in Examples 1-1 and 1-2, all evaluation results were good, and that variations in the injection-molded products due to the quality of the resin material were able to be adjusted even when temperature changes occurred in the mold. In contrast, in Comparative Examples 1-1 and 1-2, good evaluation results were obtained when there was no temperature change, but poor results were obtained when temperature changes occurred. On the other hand, in Comparative Example 3, in which the mold temperature was not adjusted, good evaluation results were not obtained, and it can be seen that adjusting both the mold temperature and the cylinder temperature is necessary to adjust variations in the injection-molded products due to the quality of the resin material.
[0039] 10 mold 12 gate 14 dumbbell test piece
Claims
1. A control method for an injection molding machine which injects molten resin in a cylinder into a mold to produce an injection-molded product, comprising the steps of: setting an injection-molded product which is previously evaluated as being suitable as a reference product; obtaining, in a single injection molding of the reference product, the peak pressure in the mold and the pressure drop time from the start of injection to the time when the pressure in the mold becomes zero or the pressure integral value from the start of injection to the time when the pressure in the mold becomes zero; adjusting, in injection molding of a product to be manufactured, the cylinder temperature so that the peak pressure in the mold becomes the peak pressure in the mold of the reference product, and adjusting the temperature in the mold so that the pressure drop time or the pressure integral value becomes the pressure drop time or pressure integral value of the reference product.
2. A control method for an injection molding machine as described in claim 1, wherein, during injection molding of the product to be manufactured, if the peak pressure in the mold is greater than the peak pressure in the mold for the reference product, the cylinder temperature is lowered, and if the peak pressure in the mold is less than the peak pressure in the mold for the reference product, the cylinder temperature is raised.
3. A control method for an injection molding machine as described in claim 1 or 2, wherein, during injection molding of the product to be manufactured, if the pressure drop time in the mold is longer than the pressure drop time in the mold for the reference product, the mold temperature is reduced, and if the pressure drop time in the mold is shorter than the pressure drop time in the mold for the reference product, the mold temperature is increased.
4. A control method for an injection molding machine as described in claim 1 or 2, wherein, during injection molding of the product to be manufactured, if the pressure integral value in the mold is greater than the pressure integral value in the mold of the reference product, the mold temperature is lowered, and if the pressure integral value in the mold is smaller than the pressure integral value in the mold of the reference product, the mold temperature is raised.
5. A method for producing an injection molded product, comprising controlling an injection molding machine by the method for controlling an injection molding machine according to claim 1 or 2 to produce an injection molded product.
Citation Information
Patent Citations
Controlling method for injection molding machine
JP1995290543A
Method and apparatus for injection molding
JP2001300997A