Optical member and method for manufacturing optical member
The two-step polymerization method for optical materials improves photochromic function and color density by incorporating a photochromic compound, addressing the limitations of conventional methods in enhancing optical properties and productivity.
Patent Information
- Application Number
- PCT/JP2024/011384
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional optical materials with photochromic compounds exhibit suboptimal color density and productivity, with existing manufacturing methods not effectively enhancing optical properties.
A method involving a two-step polymerization process using a hydroxyl group-containing polyether compound and a bifunctional or more functional iso(thio)cyanate compound, followed by mixing with a bifunctional or more active hydrogen compound and a catalyst, to create a prepolymer and subsequently cure it, incorporating a photochromic compound to improve photochromic function and color density.
The method enhances the photochromic function and color density of optical members by controlling the haze value within a specific range, allowing for effective exhibition of the photochromic compound's function while maintaining good moldability and optical properties.
Smart Images

Figure JPOXMLDOC01-APPB-M000002 
Figure JPOXMLDOC01-APPB-M000003 
Figure JPOXMLDOC01-APPB-M000004
Abstract
Description
Optical member and method for manufacturing the same
[0001] The present invention relates to an optical member and a method for manufacturing an optical member.
[0002] Plastic lenses are lightweight, shatter-resistant, and dyeable, and therefore have rapidly become widespread as optical materials for eyeglass lenses, camera lenses, and the like. Lens molded articles using various plastic materials have been developed and are now in use.
[0003] Typical examples include allyl resins obtained from diethylene glycol bisallyl carbonate or diallyl isophthalate, (meth)acrylic resins obtained from (meth)acrylates, and polythiourethane resins obtained from isocyanates and thiols.
[0004] In recent years, high-performance plastic lenses endowed with various functions have been developed by applying functional compounds to the above-mentioned plastic materials. Examples include lenses that block harmful wavelengths of light, lenses that are resistant to surface scratches, lenses that are resistant to fogging caused by temperature differences, and plastic lenses with photochromic properties. In particular, by using plastic lenses with photochromic properties in eyeglasses, the lenses function as normal clear eyeglasses indoors, but can be colored gray, brown, etc. in response to sunlight (ultraviolet rays) outdoors, thereby providing eye protection from glare. Furthermore, unlike sunglasses, these eyeglasses do not require changing glasses indoors and outdoors, and a single pair of glasses can be used both indoors and outdoors.
[0005] On the other hand, when a functional compound is applied to a plastic material, it is important that the function of the functional compound is effectively exhibited. For example, a plastic lens obtained using a plastic material to which a photochromic compound is applied is required to have a fast response time for coloring and decoloring, and to exhibit good coloring performance.
[0006] Therefore, Patent Document 1 discloses that by using a specific aliphatic or alicyclic isocyanate, a urethane resin-based optical material or a thiourethane resin-based optical material and a plastic lens containing a photochromic compound can be obtained without causing a decrease in the performance of the photochromic compound.Furthermore, Patent Document 2 discloses that by using an optical material containing a specific polyol compound, a polyurethane-based optical material or a polythiourethane-based optical material containing a photochromic compound can be obtained that exhibits excellent photochromic performance without causing a decrease in the performance of the photochromic compound and is also excellent in physical properties such as mechanical strength.
[0007] Polyroxitane has also been used in photochromic compositions for photochromic eyeglasses. For example, Patent Document 3 discloses a curable resin composition incorporating the property of polyroxitane, in which cyclic molecules move within the axial molecule, in the cured product (polymer). It also discloses that the use of a polypseudoroxitane monomer (prepolymer) obtained in a previous process, rather than polyroxitane, in the production process of the curable resin composition simplifies the production process and improves productivity.
[0008] International Publication No. 2014 / 002844 International Publication No. 2015 / 115648 International Publication No. 2020 / 032056
[0009] The present inventors have found that there is room for improvement in the color density of conventional optical materials employing photochromic compounds such as those described in Patent Documents 1 and 2. Furthermore, the technology disclosed in Patent Document 3 aims to improve productivity while retaining the properties of polyoxane monomers, but does not address the improvement of optical properties.
[0010] In view of the above circumstances, an object of the present invention is to enable an optical member to which a functional compound is applied to exhibit its functions more effectively.
[0011] The present inventors have conducted extensive research to solve the above problems and have found that it is effective to manufacture optical members using a new manufacturing method, thereby completing the present invention (first invention). Furthermore, the present inventors have conducted extensive research to solve the above problems and have found, unexpectedly, that good photochromic function of optical members can be obtained by controlling the haze value, thereby completing the present invention (second invention).
[0012] That is, the present invention can be shown as follows.
[0013] [1] A method for producing an optical member, comprising: a first polymerization step of reacting a hydroxyl group-containing polyether compound (A) with a difunctional or higher functional iso(thio)cyanate compound (B) to obtain a prepolymer; and a second polymerization step of mixing the obtained prepolymer with a difunctional or higher functional active hydrogen compound (C) and a catalyst (D) and polymerizing and curing the mixture. [2] The method for producing an optical member according to [1], wherein in the first polymerization step, the hydroxyl group-containing polyether compound (A) and the difunctional or higher functional iso(thio)cyanate compound (B) are mixed and heated to 20°C or higher and 150°C or lower to cause the reaction. [3] The method for producing an optical member according to [1] or [2], wherein in the first polymerization step, the hydroxyl group-containing polyether compound (A) is present in an amount of 0.5% by mass or higher and 50% by mass or lower, when the total amount of the hydroxyl group-containing polyether compound (A) and the difunctional or higher functional iso(thio)cyanate compound (B) is taken as 100% by mass. [4] The method for producing an optical member according to any one of [1] to [3], wherein in the first polymerization step, the ratio of the number of hydroxyl group equivalents of the hydroxyl group-containing polyether compound (A) to the number of iso(thio)cyanate group equivalents of the difunctional or higher iso(thio)cyanate compound (B) (hydroxyl groups / iso(thio)cyanate groups) is 10 to 100,000. [5] The method for producing an optical member according to any one of [1] to [4], wherein in the second polymerization step, a difunctional or higher iso(thio)cyanate compound (B) is further added. [6] The method for producing an optical member according to any one of [1] to [5], wherein in the second polymerization step, the reaction is carried out by heating to a maximum temperature of 100°C to 150°C. [7] The method for producing an optical member according to any one of [1] to [6], further comprising a mixing step of mixing a hydroxyl group-containing polyether compound (A), a di- or higher functional iso(thio)cyanate compound (B), and a functional compound (E) before the first polymerization step. [8] The method for producing an optical member according to [7], wherein the functional compound (E) is a photochromic compound (e). [9] The method for producing an optical member according to [8], wherein the photochromic compound (e) is a naphthopyran-based compound having no active hydrogen.
[0014]
[10] An optical element comprising a cured product obtained by curing a polymerizable composition for optical materials, the cured product comprising a hydroxyl group-containing polyether compound (A), a difunctional or higher iso(thio)cyanate compound (B), a difunctional or higher active hydrogen compound (C), a catalyst (D), and a functional compound (E), wherein the cured product contains spherical domains comprising the hydroxyl group-containing polyether compound (A), the difunctional or higher iso(thio)cyanate compound (B), and the functional compound (E), and the optical element has a haze (%) relative to the thickness (mm) at the center of the optical element of 0.58% / mm or more and 30% / mm or less.
[11] The optical element according to
[10] , wherein the maximum major axis of the spherical domains obtained by SAXS (small-angle X-ray scattering) analysis is 1 nm or more and 300 nm or less.
[12] The optical element according to
[10] or
[11] , wherein the number-average molecular weight of the hydroxyl group-containing polyether compound (A) is 500 to 50,000.
[13] The optical member according to any one of
[10] to
[12] , wherein the number of hydroxyl groups per molecule of the hydroxyl-containing polyether compound (A) is 1 to 10.
[14] The optical member according to any one of
[10] to
[13] , wherein the hydroxyl-containing polyether compound (A) contains one or two compounds selected from polyethylene glycol and polypropylene glycol.
[15] The optical member according to any one of
[10] to
[14] , wherein the bifunctional or higher functional iso(thio)cyanate compound (B) is one or two or more compounds selected from alicyclic polyiso(thio)cyanate compounds, aromatic polyiso(thio)cyanate compounds, and modified products thereof.
[16] The optical member according to any one of
[10] to
[15] , wherein the difunctional or higher iso(thio)cyanate compound (B) is one or more selected from xylylene diisocyanate, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and phenylene diisocyanate.
[17] The optical member according to any one of
[10] to
[16] , wherein the bifunctional or higher functional active hydrogen compound (C) has one or more functional groups selected from a hydroxy group, a mercapto group, an amino group, and a carboxyl group.
[18] The bifunctional or higher active hydrogen compound (C) is 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 2,5-bis(mercaptomethyl)-1,4-dithiane, bis(mercapto The optical member according to any one of
[10] to
[17] , comprising one or more polythiols selected from the group consisting of 1,1,3,3-tetrakis(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithietane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 3-mercaptomethyl-1,5-dimercapto-2,4-dithiapentane, tris(mercaptomethylthio)methane, and ethylene glycol bis(3-mercaptopropionate).
[19] The optical member according to any one of
[10] to
[18] , wherein the functional compound (E) is a photochromic compound (e).
[20] The optical member according to
[19] , wherein the photochromic compound (e) is a naphthopyran-based compound having no active hydrogen.
[21] The optical member according to
[20] , wherein the photochromic compound (e) is one or more compounds selected from naphthopyran-based compounds and spiropyran-based compounds.
[22] An optical device comprising the optical member according to any one of
[10] to
[21] and an electronic substrate.
[23] An optical lens comprising the optical member according to any one of
[10] to
[21] .
[0015] According to the present invention, there are provided optical members to which functional compounds are applied, which can more effectively exhibit their functions, and methods for producing the same.
[0016] The optical member of the present invention and its manufacturing method will be described based on the following embodiments. Note that the explanation of the constituent elements described below may be based on representative embodiments of the present disclosure, but the present disclosure is not limited to such embodiments. Furthermore, the symbol "a to b" indicating a numerical range represents a to b, unless otherwise specified.
[0017] <Optical Member> The optical member of the present embodiment comprises a cured product obtained by curing a polymerizable composition for optical materials, the cured product comprising a hydroxyl group-containing polyether compound (A), a difunctional or higher functional iso(thio)cyanate compound (B), a difunctional or higher functional active hydrogen compound (C), a catalyst (D), and a functional compound (E), and the cured product contains spherical domains containing the hydroxyl group-containing polyether compound (A), the difunctional or higher functional iso(thio)cyanate compound (B), and the functional compound (E), and the optical member has a haze (%) relative to the thickness (mm) at the center (hereinafter also referred to as "haze H (% / mm)") of 0.58% / mm or more and 30% / mm or less.
[0018] This allows the function of the functional compound (E) to be more effectively exhibited in the optical component. Specifically, when the functional compound (E) is a photochromic compound (e), the photochromic function can be improved, and in particular, the color density can be improved. Hereinafter, a case where the functional compound (E) is a photochromic compound (e) will be described, but the functional compound (E) of this embodiment is not limited thereto.
[0019] Although the details of why the optical member of this embodiment can improve the photochromic function are not clear, it is speculated as follows. First, the hydroxyl group-containing polyether compound (A) forms domains due to a microphase separation structure. It is speculated that, when mixed with the iso(thio)cyanate compound (B), spherical domains are formed, and the photochromic compound (e) can be incorporated into the domains. It is also speculated that the photochromic compound (e) is more likely to exhibit its function when incorporated into the spherical domains. Therefore, by polymerizing and curing the hydroxyl group-containing polyether compound (A), the iso(thio)cyanate compound (B), and the active hydrogen compound (C) to form an optical member, the photochromic compound (e) is dispersed within the optical member, and as a result, the photochromic function of the photochromic compound (e) is more likely to be exhibited. In the optical member of this embodiment, the photochromic compound (e) can be incorporated into the hydroxyl group-containing polyether compound (A) at a higher concentration than in the past, and it is speculated that the photochromic function, particularly the color density, can be improved. It is presumed that the presence of a high concentration of the photochromic compound (e) in the optical element makes light diffusion more likely, resulting in fluctuations in haze. Therefore, in this embodiment, it is presumed that the function of the photochromic compound (e) is effectively exerted by controlling the optical element so that the haze H (% / mm) falls within a predetermined numerical range. The microphase separation structure is described in International Publication No. 2018 / 070383.
[0020] In this embodiment, the haze H (% / mm) is 0.58% / mm or more, preferably 0.59% / mm or more, more preferably 0.60% / mm or more. This allows the photochromic compound (e) to be incorporated at a higher concentration, improving the photochromic function and improving the photochromic performance. On the other hand, the upper limit of the haze H (% / mm) is 30% / mm or less. From the viewpoint of maintaining good moldability of the optical component, it is preferably 20% / mm or less, more preferably 15% / mm or less, and even more preferably 10% / mm or less. From the viewpoint of reducing the light transmittance and improving the color density, it is particularly preferably 8.0% / mm or less.
[0021] The haze H (% / mm) is preferably set according to the number-average molecular weight of the hydroxyl group-containing polyether compound (A1). For example, when the number-average molecular weight of the hydroxyl group-containing polyether compound (A1) is 500 to 10,000, the haze H (% / mm) is preferably 0.58 to 10% / mm, more preferably 0.58 to 8.0% / mm, and even more preferably 0.58 to 5.0% / mm. When the number-average molecular weight of the hydroxyl group-containing polyether compound (A1) is 10,000 to 50,000, the haze H (% / mm) is preferably 1 to 10% / mm, more preferably 3 to 10% / mm, and even more preferably 5 to 10% / mm. This allows for increased photochromic function, particularly color density.
[0022] In this embodiment, the spherical domains are formed from a hydroxyl group-containing polyether compound (A) and a difunctional or higher functional iso(thio)cyanate compound (B), and can incorporate a functional compound (E) into the interior. The spherical domains can be observed by small-angle X-ray scattering measurement using a Spring-8 BL03XU.
[0023] The maximum major axis of the spherical domains is preferably 1 nm or more, more preferably 3 nm or more, and even more preferably 5 nm or more. This allows the concentration of the functional compound (E) to be increased, making it possible to impart the desired function to the optical component. On the other hand, the maximum major axis of the spherical domains is preferably 300 nm or less, more preferably 100 nm or less, and even more preferably 70 nm or less. This allows the optical component to maintain its optical properties while also obtaining the function of the functional compound (E).
[0024] The center of the optical member refers to the central portion of the optical member in a planar view. For example, if the optical member is convexly curved, the center refers to the central portion in a planar view (top view of the convex portion) when the convex portion is in the thickness direction.
[0025] The thickness is measured by a dial thickness gauge SM-130LW manufactured by TECLOCK.
[0026] The haze value (%) is measured using a haze meter. The lower the haze value (%), the higher the transparency of the optical lens.
[0027] Optical components satisfying the above-mentioned haze H (% / mm) can be realized, for example, by selecting the type and number-average molecular weight of the hydroxyl group-containing polyether compound (A), combining the hydroxyl group-containing polyether compound (A) with the difunctional or higher iso(thio)cyanate compound (B), and devising a manufacturing method for the optical component. Specifically, for example, a method can be used in which the hydroxyl group-containing polyether compound (A) and the difunctional or higher iso(thio)cyanate compound (B) are reacted to polymerize a prepolymer, and then the prepolymer is mixed with the difunctional or higher active hydrogen compound (C) and the catalyst (D) to polymerize and harden the prepolymer. In this case, the photochromic compound (e) may be mixed with the hydroxyl group-containing polyether compound (A) and the difunctional or higher iso(thio)cyanate compound (B) before polymerizing the prepolymer.
[0028] [Polymerizable composition] The optical member of this embodiment is composed of a cured product of a polymerizable composition for optical materials (hereinafter also referred to as "polymerizable composition"). Each component contained in the optical member (polymerizable composition) will be described below. The cured product refers to a polymerizable composition that has been polymerized and cured by heat or light.
[0029] (Hydroxyl Group-Containing Polyether Compound (A)) The hydroxyl group-containing polyether compound (A) of this embodiment is a polyether compound containing at least one hydroxyl group and includes at least one polyether segment. The hydroxyl group-containing polyether compound (A) of this embodiment is preferably a block copolymer that may be combined with at least one segment of polyester, polycarbonate, poly(meth)acrylate, polyamide, polyethyleneimine, polysiloxane, polysulfide, polyolefin, or polystyrene, in addition to polyether.
[0030] Another embodiment of the hydroxyl group-containing polyether compound (A) of this embodiment is a linear polyether block copolymer having at least two different segments, such as a segment structure having a divalent organic group derived from ethylene glycolate, propylene glycolate, butylene glycolate, or the like, or a segment structure having a divalent organic group derived from ethanedithiol, propanedithiol, or the like.
[0031] The polyether is not particularly limited, but examples thereof include polyethylene glycol, polypropylene glycol, polybutylene glycol, etc. The hydroxyl group-containing polyether compound (A) preferably contains one or two selected from polyethylene glycol and polypropylene glycol.
[0032] The polyesters include, but are not limited to, those obtained by condensation of dicarboxylic acids and diols.
[0033] The dicarboxylic acid may include adipic acid, succinic acid, or a combination thereof.
[0034] Examples of the diol include ethylene-1,2-diol, butane-1,4-diol, hexane-1,6-diol, propane-1,2-diol, 3-methylpentane-1,5-diol, 2-methylpropane-1,3-diol, 2,2-dimethylpropane-1,3-diol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, pentane-1,5-diol, heptane-1,7-diol, and the like, or combinations thereof.
[0035] The polyester may also include polycaprolactone, polybutyrolactone, polyvalerolactone, polylactic acid, polyglycolic acid, or combinations thereof.
[0036] The polycarbonate is not particularly limited, but examples thereof include those obtained by condensation of carbonate and diol.
[0037] Examples of the diol include ethylene-1,2-diol, butane-1,4-diol, hexane-1,6-diol, propane-1,2-diol, 3-methylpentane-1,5-diol, 2-methylpropane-1,3-diol, 2,2-dimethylpropane-1,3-diol, pentane-1,5-diol, heptane-1,7-diol, diethylene glycol, triethylene glycol, dipropylene glycol, tripropylene glycol, and the like, or combinations thereof.
[0038] The poly(meth)acrylate is not particularly limited, but examples thereof include methyl (meth)acrylate, butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, benzyl (meth)acrylate, phenyl (meth)acrylate, and the like, or combinations thereof.
[0039] The polyamide is not particularly limited, but examples thereof include those obtained by condensation of dicarboxylic acid and diamine.
[0040] The dicarboxylic acid may be adipic acid, succinic acid, or a combination thereof. The diamine may be hexamethylenediamine.
[0041] The polyamides may also include lactams such as polycaprolactam.
[0042] The polyethyleneimine may be a polyethyleneimine chain, which is a polymer chain, such as a polyethyleneimine chain, a polypropionylaziridine chain, a polyacetylaziridine chain, or a polyformylaziridine chain.
[0043] The polysiloxane may be a polysiloxane chain, which is a polymer chain, such as a polydimethylsiloxane chain or a polymethylphenylsiloxane chain.
[0044] The polysulfide may contain a polyethylene sulfide chain or the like.
[0045] The polyolefin may include polyethylene, polypropylene, and the like, or a combination thereof.
[0046] The polystyrene may include polystyrene, polystyrene sulfonate, and the like, or a combination thereof.
[0047] The hydroxyl group-containing polyether compound (A) of this embodiment forms a domain structure. Specifically, it preferably forms micelles by microphase separation, and can provide uniformly dispersed nano-sized structures. The micellar structure can effectively disperse the functional compound (E), such as a photochromic dye, in the optical component of this embodiment while maintaining the mechanical and optical properties.
[0048] The number of hydroxyl groups per molecule of the hydroxyl group-containing polyether compound (A) is preferably 1 to 10, more preferably 1 to 8, and even more preferably 1 to 6. By setting the number of hydroxyl groups per molecule of the hydroxyl group-containing polyether compound (A) within the above numerical range, the function of the functional compound (E) can be more easily exhibited, and performance such as the color development density and color development / fading speed of the photochromic compound can be improved, for example.
[0049] The number-average molecular weight of the hydroxyl group-containing polyether compound (A) is preferably 500 to 50,000, more preferably 1,000 to 30,000, and even more preferably 2,000 to 20,000. By setting the number-average molecular weight of the hydroxyl group-containing polyether compound (A) to the above-mentioned lower limit or more, the functionality of the functional compound is easily improved, and for example, photochromic performance is easily improved. On the other hand, by setting the number-average molecular weight of the hydroxyl group-containing polyether compound (A) to the above-mentioned upper limit or less, the functionality of the functional compound is well maintained while opacity of the optical component can be suppressed.
[0050] (Iso(thio)cyanate Compound (B)) The iso(thio)cyanate compound (B) of this embodiment is an iso(thio)cyanate compound having two or more iso(thio)cyanato groups. Here, the iso(thio)cyanate compound refers to an isocyanate compound or an isothiocyanate compound. Examples of the iso(thio)cyanate compound (B) of this embodiment include alicyclic polyiso(thio)cyanate compounds, aromatic polyiso(thio)cyanate compounds, and modified products thereof.
[0051] More specifically, the isocyanate compound includes isophorone diisocyanate, bis(isocyanatomethyl)cyclohexane, dicyclohexylmethane-4,4'-diisocyanate, cyclohexane diisocyanate, methylcyclohexane diisocyanate, dicyclohexyldimethylmethane isocyanate, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 3,8-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, alicyclic polyisocyanate compounds such as 3,9-bis(isocyanatomethyl)tricyclodecane, 3,9-bis(isocyanatomethyl)tricyclodecane, 4,8-bis(isocyanatomethyl)tricyclodecane, and 4,9-bis(isocyanatomethyl)tricyclodecane; and aromatic polyisocyanate compounds such as phenylene diisocyanate, 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and diphenyl sulfide-4,4'-diisocyanate.
[0052] Examples of the isothiocyanate compound include isophorone diisothiocyanate, bis(isothiocyanatomethyl)cyclohexane, dicyclohexylmethane diisothiocyanate, cyclohexane diisothiocyanate, methylcyclohexane diisothiocyanate, 2,5-bis(isothiocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isothiocyanatomethyl)bicyclo-[2.2.1]-heptane, 3,8-bis(isothiocyanatomethyl)bicyclo-[2.2.1]-heptane, alicyclic polyisothiocyanate compounds such as 3,9-bis(isothiocyanatomethyl)tricyclodecane, 3,9-bis(isothiocyanatomethyl)tricyclodecane, 4,8-bis(isothiocyanatomethyl)tricyclodecane, and 4,9-bis(isothiocyanatomethyl)tricyclodecane; and aromatic polyisothiocyanate compounds such as tolylene diisothiocyanate, 4,4'-diphenylmethane diisothiocyanate, and diphenyl disulfide-4,4'-diisothiocyanate.
[0053] The iso(thio)cyanate compound (B) may also be a halogen-substituted compound such as a chlorine-substituted compound or a bromine-substituted compound, an alkyl-substituted compound, an alkoxy-substituted compound, a nitro-substituted compound, a prepolymer-type modified compound with a polyhydric alcohol, a carbodiimide-modified compound, a urea-modified compound, a biuret-modified compound, a dimerization or trimerization reaction product, etc. The iso(thio)cyanate compound (B) may also be used alone or in combination of two or more selected from these.
[0054] [Active Hydrogen Compound (C)] The active hydrogen compound (C) of this embodiment has two or more functional groups. Examples of functional groups include hydroxyl groups, mercapto groups, amino groups, and carboxyl groups. Examples of the active hydrogen compound (C) include poly(thiol) compounds having two or more hydroxyl or mercapto groups, polyamine compounds having two or more primary or secondary amino groups, and polycarboxylic acid compounds having two or more carboxyl groups. Also included are compounds having two or more active hydrogen groups selected from hydroxyl groups, mercapto groups, primary amino groups, secondary amino groups, and carboxyl groups in one molecule. The two or more active hydrogen groups may be the same or different.
[0055] For example, bifunctional or higher active hydrogen compounds having a hydroxy group, such as ethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, glycerin, polyglycerin, and thioglycerin; trithioglycerin, pentaerythritol tetrakis(thioglycolate), trimethylolpropane(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptopropionate), dipentaerythritol hexa(3-mercaptopropionate), bis(2-mercaptoethyl)sulfide, 4-mercaptomethyl-3,6-dithiaoctane-1,8-dithiol, and 4,8-bis(mercaptomethyl)-3,6,9-trithiaundecane- difunctional or higher active hydrogen compounds having a mercapto group, such as 1,11-dithiol, 4,7-bis(mercaptomethyl)-3,6,9-trithiaundecane-1,11-dithiol, 5,7-bis(mercaptomethyl)-3,6,9-trithiaundecane-1,11-dithiol, 1,1,3,3-tetrakis(mercaptomethyl)-2-thiapropane, 1,4-dithiane-2,5-dithiol, 2,5-bis(mercaptomethyl)-1,4-dithiane, and xylylenedithiol; Examples of such an active hydrogen compound include bifunctional or higher functional compounds having an amino group, such as xylylenediamine, α,α,α',α'-tetramethyl-xylylenediamine, 1,5-diaminopentane, 1,6-diaminohexane, diaminopolypropylene, diaminopolyethylene, isophoronediamine, bis(aminocyclohexyl)methane, bis(aminomethyl)cyclohexane, and bis(aminomethyl)norbornane.
[0056] [Catalyst (D)] The catalyst (D) of the present embodiment may be one or more selected from Lewis acids, tertiary amines, organic acids, amine-organic acid salts, etc. Among these, Lewis acids, amines, and amine-organic acid salts are preferred, and dimethyltin chloride, dibutyltin dichloride, and dibutyltin laurate are more preferred.
[0057] [Photochromic Compound (e)] The photochromic compound (e) may be a compound whose absorption characteristics (absorption spectrum) change with respect to light of a specific wavelength. As the photochromic compound (e) of this embodiment, known compounds can be used, and for example, they can be obtained by the methods described in International Publication No. 2009 / 146509, International Publication No. 2010 / 20770, International Publication No. 2012 / 149599, and International Publication No. 2012 / 162725. Specific examples include spiropyran compounds, spirooxazine compounds, fulgide compounds, naphthopyran compounds, and bisimidazole compounds. Among these, naphthopyran compounds and spiropyran compounds are preferred, and naphthopyran compounds having no active hydrogen are more preferred.
[0058] [Others] The polymerizable composition of the present embodiment may further contain additives such as an internal mold release agent, a resin modifier, a light stabilizer, an antioxidant, and a color inhibitor, depending on the properties desired for the application.
[0059] (Internal Mold Release Agent) The polymerizable composition of the present embodiment may contain an internal mold release agent for the purpose of improving releasability from the mold after molding. An acidic phosphate ester can be used as the internal mold release agent. Examples of acidic phosphate esters include monophosphate esters and diphosphate esters, each of which can be used alone or in combination of two or more. Examples of commercially available internal mold release agents include ZelecUN manufactured by STEPAN Corporation, MR internal mold release agents manufactured by Mitsui Chemicals, Inc., the JP series manufactured by Johoku Chemical Industry Co., Ltd., the Phosphanol series manufactured by Toho Chemical Industry Co., Ltd., and the AP and DP series manufactured by Daihachi Chemical Industry Co., Ltd.
[0060] (Resin Modifier) The optical member of this embodiment may contain a resin modifier for the purpose of adjusting various physical properties such as optical properties, impact resistance, specific gravity, etc., and adjusting the viscosity and pot life of the polymerizable composition. Examples of the resin modifier include episulfide compounds, alcohol compounds other than the above-mentioned polyol compounds, amine compounds other than the above-mentioned amine compounds, epoxy compounds, organic acids and anhydrides thereof, and olefin compounds including (meth)acrylate compounds.
[0061] (Light Stabilizer) As the light stabilizer, a hindered amine compound, which is a compound having a 2,2,6,6-tetramethylpiperidine skeleton or a 1,2,2,6,6-pentamethylpiperidine skeleton, can be used. Commercially available hindered amine compounds include Lowilite 76 and Lowilite 92 manufactured by Chemtura Corporation, Tinuvin 144, Tinuvin 292, and Tinuvin 765 manufactured by BASF Corporation, Adekastab LA-52 and LA-72 manufactured by ADEKA Corporation, JF-95 manufactured by Johoku Chemical Industry Co., Ltd., and Hostavin PR-25 manufactured by Clariant Chemicals.
[0062] <Method for Manufacturing Optical Member> Next, an example of a method for manufacturing the optical member of this embodiment will be described.
[0063] The method for producing an optical member according to this embodiment includes the following steps: Step 1 (mixing step): A mixing step of mixing a hydroxyl group-containing polyether compound (A), a difunctional or higher functional iso(thio)cyanate compound (B), and a functional compound (E). Step 2 (first polymerization step): A first polymerization step of reacting the hydroxyl group-containing polyether compound (A) with the difunctional or higher functional iso(thio)cyanate compound (B) to obtain a prepolymer. Step 3 (second polymerization step): A second polymerization step of mixing the obtained prepolymer with a difunctional or higher functional active hydrogen compound (C) and a catalyst (D), followed by polymerization and curing.
[0064] This allows the functions of the functional compound (E) to be effectively exhibited in the optical member obtained by applying the functional compound. Furthermore, the haze H (% / mm) of the optical member can be increased to 0.58% / mm or more. In this embodiment, the photochromic performance of the photochromic compound (e) as the functional compound (E) can be improved. Examples of photochromic performance include high color density and fast color development / decolorization speed.
[0065] Although the details of how this effect is achieved are unclear, it is speculated as follows. Conventionally, a hydroxyl-containing polyether compound (A), an iso(thio)cyanate compound (B), and an active hydrogen compound (C) are mixed together and polymerized and cured. In the method for producing an optical component of this embodiment, prior to polymerization and curing, the hydroxyl-containing polyether compound (A) and the iso(thio)cyanate compound (B) are reacted in step 1 to obtain a prepolymer. This is speculated to make it easier than ever to incorporate the functional compound (E) into the spherical domains formed from the hydroxyl-containing polyether compound (A). As a result, it is thought that a higher concentration of the functional compound (E) can be applied, or the proportion of the functional compound (E) incorporated into the spherical domains can be increased, making it easier for the functional compound (E) to exert its function.
[0066] In this embodiment, an example including Step 1 (mixing step) will be described, but the present invention is not limited to the example including Step 1 (mixing step). In addition, an example using a photochromic compound (e) as the functional compound (E) will be described, but the functional compound (E) is not limited thereto.
[0067] Each step will be described in detail below.
[0068] [Step 1 (Mixing Step)] First, the hydroxyl group-containing polyether compound (A), the iso(thio)cyanate compound (B), and the photochromic compound (e) are mixed.
[0069] This makes it possible to obtain an optical member having a photochromic function.
[0070] The mixing method is not particularly limited, and any conventionally known method can be used, and a method of stirring by known means can be adopted. The stirring rotation speed is preferably adjusted appropriately depending on the stirring means and scale used, but is about 100 to 250 rpm. The temperature during mixing is preferably kept lower than room temperature (25°C).
[0071] The hydroxyl group-containing polyether compound (A), the iso(thio)cyanate compound (B), and the photochromic compound (e) may be added to a mixing vessel simultaneously or separately, and the order of addition is not particularly limited.
[0072] [Step 2 (First Polymerization Step)] Next, the hydroxyl group-containing polyether compound (A) and the iso(thio)cyanate compound (B) are reacted to obtain a prepolymer.
[0073] As a reaction method, a mixed liquid containing the hydroxyl group-containing polyether compound (A) and the iso(thio)cyanate compound (B) is preferably heated to react the hydroxyl groups of the hydroxyl group-containing polyether compound (A) with the iso(thio)cyanato groups of the iso(thio)cyanate compound (B). The heating temperature is preferably 20°C or higher and 150°C or lower, more preferably 40°C or higher and 120°C or lower, and even more preferably 50°C or higher and 100°C or lower. The heating time is adjusted as appropriate and can be, for example, 10 to 24 hours.
[0074] During heating, it is preferable to continue stirring in order to ensure that the reaction proceeds uniformly. The stirring speed is not particularly limited, but is, for example, about 100 to 250 rpm.
[0075] The production of the prepolymer can be confirmed by differential scanning calorimetry (DSC) when heat generation caused by the reaction between the hydroxyl groups of the hydroxyl group-containing polyether compound (A) and the iso(thio)cyanato groups of the iso(thio)cyanate compound (B) is completed.
[0076] After the prepolymer is obtained, it is preferable to cool the mixture to room temperature (25° C.) or below.
[0077] The amount of the hydroxyl group-containing polyether compound (A) blended is preferably 0.5% by mass or more and 50% by mass or less, and more preferably 1 to 25% by mass, when the total amount of the hydroxyl group-containing polyether compound (A) and the iso(thio)cyanate compound (B) is taken as 100% by mass.
[0078] The ratio of the number of hydroxyl group equivalents of the hydroxyl group-containing polyether compound (A) to the number of iso(thio)cyanate group equivalents of the iso(thio)cyanate compound (B) (iso(thio)cyanate groups / hydroxyl groups) is preferably 10 to 100,000, more preferably 1 to 10,000, and even more preferably 10 to 5,000.
[0079] [Second Polymerization Step] The prepolymer obtained in the first polymerization step is mixed with an active hydrogen compound (C) and a catalyst (D) and polymerized and cured. That is, a polymerizable composition containing the prepolymer, the active hydrogen compound (C), and the catalyst (D) is obtained, and then the polymerizable composition is polymerized and cured to obtain an optical element.
[0080] The mixing method is not particularly limited, and mixing can be performed by a conventionally known method, and a method of stirring by a known means can be adopted. The stirring rotation speed is preferably adjusted appropriately depending on the stirring means and scale used, but is about 100 to 250 rpm.
[0081] The active hydrogen compound (C) and the catalyst (D) are mixed preferably at room temperature or below, more preferably at 15 to 20°C.
[0082] The active hydrogen compound (C) and the catalyst (D) may be mixed with the prepolymer all at once or separately, and the order of mixing them is not important.
[0083] In the second polymerization step, the polymerizable composition may further contain the other additives described above (such as an internal mold release agent, a resin modifier, a light stabilizer, and a bluing agent). However, if the solubility of the additives such as the catalyst (D) and the internal mold release agent is poor, the composition may be heated before mixing.
[0084] In the second polymerization step, an iso(thio)cyanate compound (B) may be further added, thereby increasing the polymerization rate of the polymerization curing.
[0085] The polymerizable composition is then polymerized to obtain the optical member of this embodiment. The polymerization method may be a conventionally known method, and the conditions for the polymerization are not particularly limited.
[0086] Optical components can be obtained in various shapes depending on the shape of the mold. The method for molding optical components is not particularly limited, but cast polymerization is preferred. Specifically, a polymerizable composition is first poured into a mold space held together by a gasket, tape, or the like. Depending on the physical properties required for the resulting optical component, it may be preferable to perform a degassing treatment under reduced pressure or a filtration treatment under pressure or reduced pressure, as needed.
[0087] The polymerization conditions are not limited because they vary depending on the composition of the polymerization composition, the type and amount of catalyst used, the shape of the mold, etc., but are generally carried out for 1 to 50 hours at a temperature of approximately −50 to 150° C. In some cases, it is preferable to maintain or gradually increase the temperature within a temperature range of 10 to 150° C. and cure for 1 to 25 hours.
[0088] The optical member of this embodiment may be subjected to a treatment such as annealing, if necessary. The treatment temperature is usually between 50 and 150°C, preferably between 90 and 140°C, and more preferably between 100 and 130°C.
[0089] The optical member of this embodiment is colorless and transparent, has an excellent appearance, and contains the photochromic compound (e), thereby imparting photochromic functionality.
[0090] The above has described the case where the photochromic compound (e) is used as the functional compound (E) of this embodiment, but functional compounds (E) other than the photochromic compound (e) will be described below.
[0091] [Functional Compound (E)] The functional compound (E) is used to impart a new function to the optical component of this embodiment. Examples of the functional compound (E) include, in addition to the photochromic compound (e), dyes, ultraviolet absorbers, blooming agents, visible light absorbing pigments, and the like. According to the optical component of this embodiment, when a dye is used, the dyeability is improved, when an ultraviolet absorber is used, the ultraviolet blocking rate can be increased, and when a blooming agent is used, the hue of a specific wavelength can be changed.
[0092] (Ultraviolet Absorber) Examples of the ultraviolet absorber include benzophenone-based compounds, triazine-based compounds, and benzotriazole-based compounds.
[0093] Examples of the benzophenone-based ultraviolet absorber include 2,2'-dihydroxy-4-methoxybenzophenone, 2-hydroxy-4-acryloyloxybenzophenone, 2-hydroxy-4-acryloyloxy-5-tert-butylbenzophenone, and 2-hydroxy-4-acryloyloxy-2',4'-dichlorobenzophenone.
[0094] Examples of triazine-based ultraviolet absorbers include 2-[4-[(2-hydroxy-3-dodecyloxypropyl)oxy]-2-hydroxyphenyl]4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-(2-hydroxy-3-tridecyloxypropyl)oxy]-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-[(2-hydroxy-3-(2'-ethyl) 2,4-bis(2-hydroxy-4-butyloxyphenyl)-6-(2,4-bis-butyloxyphenyl)-1,3,5-triazine, 2-[2-hydroxy-4-(1-octyloxycarbonylethoxy)phenyl]-4,6-bis(4-phenylphenyl)-1,3,5-triazine, and the like.
[0095] Examples of benzotriazole-based ultraviolet absorbers include 2-(2H-benzotriazol-2-yl)-4-methylphenol, 2-(2H-benzotriazol-2-yl)-4-tert-octylphenol, 2-(2H-benzotriazol-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol, 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol, 2-(5-chloro-2H-benzotriazol-2-yl)-4-methyl-6-tert-butylphenol, 2-(5-chloro-2H-benzotriazol-2-yl)-2,4-tert-butylphenol, and 2,2'-methylenebis[6-(2H-benzotriazol-2-yl)-4-(1,1,3,3-tetramethylbutyl)phenol]. These ultraviolet absorbents may be used alone or in combination of two or more.
[0096] (Bluing Agent) Examples of bluing agents include those that have an absorption band in the orange to yellow wavelength region of the visible light range and have the function of adjusting the hue of an optical component made of a resin. More specifically, the bluing agent includes a substance that exhibits a blue to purple color.
[0097] (Visible Light Absorbing Dye) As the visible light absorbing dye, commercially available products may be used, and organic dye compounds are preferred. Specific examples include porphyrin compounds and tetraazaporphyrin compounds. A more specific example of a visible light absorbing dye is PD-311S (manufactured by Yamamoto Chemical Industry Co., Ltd.).
[0098] [Uses] Examples of uses of the optical member of this embodiment include plastic lenses, camera lenses, light-emitting diode lenses, light-emitting diode lens cases, prisms, optical fibers, information recording substrates, and filters. In particular, optical materials or optical elements such as plastic lenses, camera lenses, light-emitting diode lenses, and light-emitting diode lens cases are suitable. Alternatively, the optical member of this embodiment may be an optical device including an electronic substrate on which electronic components are mounted. Examples of optical devices include AR (Augmented Reality) glasses and smart glasses.
[0099] The above-mentioned plastic lens including the optical member of this embodiment may be used as a laminated plastic lens by applying a coating layer to one or both sides of the lens substrate made of the optical member, as needed. Examples of the coating layer include a primer layer, a hard coat layer, an anti-reflection film layer, an anti-fogging film layer, an anti-fouling layer, and a water-repellent layer. Each of these coating layers may be used alone, or multiple coating layers may be used in a multilayer configuration. When applying coating layers to both sides, the same coating layer may be applied to each side, or different coating layers may be applied to each side.
[0100] These coating layers may each contain an infrared absorber to protect the eyes from infrared rays, a light stabilizer or antioxidant to improve the weather resistance of the lens, a dye or pigment to enhance the fashionability of the lens, a photochromic dye or photochromic pigment, an antistatic agent, or other known additives to improve lens performance. A coating layer such as a hard coat layer or an antireflection coat, or a primer layer may also be provided.
[0101] The plastic lens of the present embodiment may be dyed using a dye according to the purpose, for the purpose of imparting fashionability, photochromic properties, etc. The lens can be dyed by a known dyeing method.
[0102] Although the present disclosure has been described above based on the present embodiment, various configurations can be adopted within the scope that does not impair the effects of the present disclosure.
[0103] EXAMPLES The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to these. First, the evaluation items and evaluation methods for the molded articles in the examples of the present invention are shown below.
[0104] <Experiment 1> (1) Evaluation Method [Evaluation of Light Control Performance] Using a xenon lamp (180 W) light source device, each molded product sample obtained in (3) below was allowed to develop color for 15 minutes under conditions of a temperature of 23°C and an ultraviolet intensity of 50,000 lux (lx) measured with an integrating actinometer. In this state, the transmittance (%) of a molded product sample 0.7 mm thick was measured to confirm the color density. A lower transmittance indicates a higher color density. Light source: MS-35AAF / FB, manufactured by Ushio Electric Co., Ltd. Instant multi-photometering system: MSPD-7700, manufactured by Otsuka Electronics Co., Ltd.
[0105] (2) Raw Materials (Part) [Hydroxyl Group-Containing Polyether Compound (A)] Hydroxyl group-containing polyether compound (A1): polyethylene glycol, polypropylene glycol, polyethylene glycol (ADEKA PLURONIC (registered trademark) L-64 manufactured by ADEKA CORPORATION), number average molecular weight: 2900, number of hydroxyl groups per molecule: 2 Hydroxyl group-containing polyether compound (A2): polyoxyethylene polyoxypropylene glycol, (Pluronic F127 manufactured by BASF), number average molecular weight: 12600, number of hydroxyl groups per molecule: 2
[0106] [Photochromic compound (e)] Photochromic compound (e1): Reversacol Wembley Grey (R1966): 500 ppm Photochromic compound (e2): Reversacol Jalapeño Red (R1950): 500 ppm
[0107] (3) Preparation of Optical Members / Photochromic Lenses (Molded Products) <Comparative Example 1-1> A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e2) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. To 41.3 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 10 parts by weight of the resulting master solution was added and stirred, to which 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Kyoeisha Chemical Co., Ltd., Polyflow KL-100), and 0.1 parts by weight of an acidic phosphate ester (Johoku Chemical Industry Co., Ltd., JP-506H) were added, and the mixture was stirred for 30 minutes at 15°C to 20°C (mixing step). Meanwhile, 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance, and a solution was prepared by uniformly dissolving the mixture. This solution was added to the mixed liquid obtained in the mixing step and stirred at 15°C to 20°C for 15 minutes to obtain a polymerizable composition (mixing step). The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15°C to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The obtained polymerizable composition was cast into a glass mold and heated from 10°C to 130°C over 24 hours (polymerization step). The resulting lens was cooled to room temperature and removed from the glass mold to obtain a photochromic lens. The obtained photochromic lens (molded sample) was evaluated and measured as described in Experiment 1(1) above. The results are shown in Table 1.
[0108] Example 1-1 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e2) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 20.78 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto and stirred at 60°C for 14 hours or more (first polymerization step). In the first polymerization step, the total weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) (30.78 parts by weight) was divided by the final amount used (51.3), thereby defining a prepolymer ratio of 60%. To the solution after the first polymerization step, 20.52 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane was added, and the mixture was stirred at 15°C to 20°C for 5 minutes to obtain a second solution. Separately, a solution was prepared by adding 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride to the second solution and dissolving them uniformly. This solution was then added to the second solution and stirred for 15 minutes at 15 to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was poured into the space enclosed between the glass molds and heated from 10 to 130°C over 24 hours (second polymerization step). The distance between the glass molds at the center of the lens was 0.8 mm.The lens was then cooled to room temperature and removed from the glass mold to obtain a photochromic lens having a thickness of 0.7 mm. The obtained photochromic lens (molded sample) was subjected to the evaluation and measurement described in Experiment 1(1) above. The results are shown in Table 1.
[0109] Example 1-2 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e2) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 41.3 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto and stirred at 60°C for 14 hours or more (first polymerization step). In the first polymerization step, the combined weight of 51.3 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) was divided by the final amount used, 51.3, to define the prepolymer ratio as 100%. Meanwhile, 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance and dissolved uniformly to prepare a solution. This solution was added to the mixture obtained in the first polymerization step and stirred for 15 minutes at a temperature between 15°C and 20°C, yielding a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at a temperature between 15°C and 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was cast into a glass mold and heated from 10°C to 130°C over 24 hours (second polymerization step). The composition was cooled to room temperature and removed from the glass mold to obtain a photochromic lens. The resulting photochromic lens (molded sample) was evaluated and measured as in Experiment 1(1) above. The results are shown in Table 1.
[0110] Comparative Example 1-2 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e1) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. To 43.33 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 10 parts by weight of the resulting master solution was added and stirred, followed by 2.5 parts by weight of a hydroxyl group-containing polyether compound (A2), 0.4 parts by weight of a polyether-modified siloxane compound (Kyoeisha Chemical Co., Ltd., Polyflow KL-100), and 0.1 parts by weight of an acidic phosphate ester (Johoku Chemical Co., Ltd., JP-506H), and the mixture was stirred at 15°C to 20°C for 30 minutes (first polymerization step). 44.17 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance and dissolved uniformly to prepare a solution. This solution was added to the mixed solution obtained in the first polymerization step and stirred at 15°C to 20°C for 15 minutes to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15°C to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was cast into a glass mold and heated from 10°C to 130°C over 24 hours (second polymerization step). The resulting lens was cooled to room temperature and removed from the glass mold to obtain a photochromic lens. The resulting photochromic lens (molded sample) was evaluated and measured as described in Experiment 1(1). The results are shown in Table 1.
[0111] Example 1-3 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e1) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 21.98 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 2.5 parts by weight of a hydroxyl group-containing polyether compound (A2), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto, and the mixture was stirred at 60°C for 14 hours or more (first polymerization step). The total amount of 31.98 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and Reversacol Wembley Grey manufactured by Vivimed, Inc. used in the first polymerization step, was divided by the final amount of 53.3, thereby defining a prepolymer ratio of 60%. 21.32 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane was added to the solution after the first polymerization step, and the mixture was stirred at 15°C to 20°C for 5 minutes to obtain a second solution. Separately, a solution was prepared in advance by adding 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride and dissolving them uniformly. This solution was added to the second solution and stirred for 15 minutes at 15 to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was cast into a glass mold and heated from 10 to 130°C over 24 hours (second polymerization step). The resulting mixture was cooled to room temperature and removed from the glass mold to obtain a photochromic lens.The obtained photochromic lenses (molded samples) were subjected to the evaluation and measurement described in Experiment 1(1). The results are shown in Table 1.
[0112] Example 1-4 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e1) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 41.3 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 2.5 parts by weight of a hydroxyl group-containing polyether compound (A2), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 part by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto, and the mixture was stirred at 60°C for 14 hours or more (first polymerization step). In the first polymerization step, the combined weight of 51.3 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) was divided by the final amount used, 51.3, to define the prepolymer ratio as 100%. Meanwhile, 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance and dissolved uniformly to prepare a solution. This solution was added to the mixture obtained in the first polymerization step and stirred for 15 minutes at a temperature between 15°C and 20°C, yielding a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at a temperature between 15°C and 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was cast into a glass mold and heated from 10°C to 130°C over 24 hours (second polymerization step). The composition was cooled to room temperature and removed from the glass mold to obtain a photochromic lens. The resulting photochromic lens (molded sample) was evaluated and measured as in Experiment 1(1) above. The results are shown in Table 1.
[0113] Comparative Example 1-3 A polymerizable composition and a photochromic lens (molded sample) were obtained in the same manner as in Comparative Example 2, except that the photochromic compound (e1) was changed to the photochromic compound (e2). The obtained photochromic lens (molded sample) was subjected to the evaluation and measurement in Experiment 1(1) above. The results are shown in Table 1.
[0114] Example 1-5 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e2) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 31.04 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 2.5 parts by weight of a hydroxyl group-containing polyether compound (A2), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto, and the mixture was stirred at 60°C for 14 hours or more (first polymerization step). The total weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) used in the first polymerization step (41.04 parts by weight) was divided by the final amount used (51.3), thereby defining a prepolymer ratio of 80%. To the solution after the first polymerization step (10.26 parts by weight) of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane was added, and the mixture was stirred at 15°C to 20°C for 5 minutes to obtain a second solution. Separately, a solution was prepared in advance by adding 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride and dissolving them uniformly. This solution was added to the second solution and stirred for 15 minutes at 15 to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was cast into a glass mold and heated from 10 to 130°C over 24 hours (second polymerization step). The resulting mixture was cooled to room temperature and removed from the glass mold to obtain a photochromic lens.The obtained photochromic lenses (molded samples) were subjected to the evaluation and measurement described in Experiment 1(1). The results are shown in Table 1.
[0115] Example 1-6 A polymerizable composition and a photochromic lens (molded sample) were obtained in the same manner as in Example 1-4, except that the photochromic compound (e1) was changed to the photochromic compound (e2). The obtained photochromic lens (molded sample) was subjected to the evaluation and measurement in Experiment 1(1) above. The results are shown in Table 1.
[0116]
[0117] (4) Confirmation of Spherical Domains (Small-Angle X-ray Scattering Measurement) Next, to observe the aggregation structure of the block copolymer, small-angle X-ray scattering measurement was performed under the following conditions. For background processing, the two-dimensional scattering intensity obtained from the sample was divided by the X-ray transmittance, and then the two-dimensional scattering intensity obtained from a measurement without a sample was subtracted. The one-dimensional scattering intensity I(q) obtained by circularly averaging the two-dimensional scattering intensity after background processing was subjected to fitting using the least squares method. Here, q is the magnitude of the scattering vector, q = 4π sin θ / λ (π is the circumference constant, 2θ is the scattering angle, and λ is the incident X-ray wavelength). The fitting function used was Equation 1, into which Equations 2 to 5, which represent a core-shell spherical structure in which the core particle size follows a Gaussian distribution, and Equations 6 to 10 (Percus-Yevick approximation), which represent the interference between particles, were substituted. Igor Pro 9 was used as the analysis software. The fitting range was 0.07<q<2 nm. -1 It was decided.
[0118] <Measurement conditions> Sample thickness: 0.8 mm to 1.1 mm Equipment: SPring-8 / BL03XU Camera length: 2316 mm Detector: PILATUS 1M manufactured by DECTRIS Incident X-ray wavelength: 1 Å Attenuator: 10 μm thick gold plate Exposure time: 1 s
[0119]
[0120]
[0121]
[0122]
[0123]
[0124]
[0125]
[0126]
[0127]
[0128]
[0129] ρ c , ρ m The X-ray scattering length densities of PPO and thiourethane resin (9.41 × 10 10 cm -2 , 10.8 x 10 10 cm -2 ) and K, B, < R c >,ρ c , t, ρ s、 D PY , φ PY was used as a fitting parameter.
[0130] Results In Examples 1-1 to 1-6, all parameters converged, which indicated that the block copolymers in the photochromic lenses of each Example formed core-shell type spherical domains.
[0131] <Experiment 2> (1) Evaluation Method [Evaluation of Light Control Performance] Using a xenon lamp (180 W) light source device, each molded product sample obtained in (3) below was allowed to develop color for 15 minutes under conditions of a temperature of 23°C and an ultraviolet intensity of 50,000 lux (lx) measured with an integrating actinometer. In this state, the transmittance (%) of a molded product sample 0.7 mm thick was measured to confirm the color density. A lower transmittance indicates a higher color density. Light source: MS-35AAF / FB, manufactured by Ushio Electric Co., Ltd. Instant multi-photometering system: MSPD-7700, manufactured by Otsuka Electronics Co., Ltd.
[0132] [Measurement of Haze Value (%)] The haze value (%) was measured using a haze meter (model number: NDH 2000) manufactured by Nippon Denshoku Industries Co., Ltd.
[0133] (2) Raw Materials (Part) [Hydroxyl Group-Containing Polyether Compound (A)] Hydroxyl group-containing polyether compound (A1): polyethylene glycol, polypropylene glycol, polyethylene glycol (ADEKA PLURONIC (registered trademark) L-64 manufactured by ADEKA CORPORATION), number average molecular weight: 2900, number of hydroxyl groups per molecule: 2 Hydroxyl group-containing polyether compound (A2): polyoxyethylene polyoxypropylene glycol, (Pluronic F127 manufactured by BASF), number average molecular weight: 12600, number of hydroxyl groups per molecule: 2
[0134] [Photochromic compound (e)] Photochromic compound (e); Reversacol Wembley Grey (R1966): 500 ppm
[0135] (3) Preparation of Optical Members and Photochromic Lenses (Molded Samples) Example 2-1 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 20.78 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto and stirred at 60°C for 14 hours or more (first polymerization step). In the first polymerization step, the total weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) (30.78 parts by weight) was divided by the final amount used (51.3), thereby defining a prepolymer ratio of 60%. To the solution after the first polymerization step, 20.52 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane was added, and the mixture was stirred at 15°C to 20°C for 5 minutes to obtain a second solution. Separately, a solution was prepared in advance by adding 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride to the second solution and dissolving them uniformly. This solution was added to the second solution and stirred for 15 minutes at 15 to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was poured into the space enclosed between glass molds and then heated from 10 to 130°C over 24 hours (second polymerization step).The distance between the glass molds at the center of the lens was 0.8 mm. The lens was then cooled to room temperature and removed from the glass mold to obtain a photochromic lens with a thickness of 0.7 mm. The obtained photochromic lens (molded sample) was evaluated and measured as in Experiment 2(1) above. The results are shown in Table 2.
[0136] Example 2-2 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 41.3 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto and stirred at 60°C for 14 hours or more (first polymerization step). In the first polymerization step, the combined weight of 51.3 parts by weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) was divided by the final amount used, 51.3, to define the prepolymer ratio as 100%. Meanwhile, 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance and dissolved uniformly to prepare a solution. This solution was added to the solution after the first polymerization step and stirred for 15 minutes at a temperature between 15°C and 20°C, yielding a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was poured into the space enclosed between the glass molds and heated from 10 to 130°C over 24 hours (second polymerization step). The distance between the glass molds at the center of the lens was 0.8 mm. The lens was then cooled to room temperature and removed from the glass mold to obtain a photochromic lens with a thickness of 0.7 mm. The resulting photochromic lens (molded sample) was evaluated and measured as described in Experiment 2(1) above. The results are shown in Table 2.
[0137] Example 2-3 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. 10 parts by weight of the obtained master liquid was added to 31.04 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and stirred, and then 2.5 parts by weight of a hydroxyl group-containing polyether compound (A2), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added thereto, and the mixture was stirred at 60°C for 14 hours or more (first polymerization step). The total weight of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and the photochromic compound (e2) used in the first polymerization step (41.04 parts by weight) was divided by the final amount used (51.3), thereby defining a prepolymer ratio of 80%. To the solution after the first polymerization step (10.26 parts by weight) of the composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane was added, and the mixture was stirred at 15°C to 20°C for 5 minutes to obtain a second solution. Separately, a solution was prepared by adding 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride to the second solution and dissolving them uniformly. This solution was then added to the second solution and stirred for 15 minutes at 15 to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15 to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was poured into the space enclosed between the glass molds and heated from 10 to 130°C over 24 hours (second polymerization step). The distance between the glass molds at the center of the lens was 0.8 mm.The lens was then cooled to room temperature and removed from the glass mold to obtain a 0.7 mm thick photochromic lens. The obtained photochromic lens (molded sample) was subjected to the evaluation and measurement described in Experiment 2(1) above. The results are shown in Table 2.
[0138] Comparative Example 2-1 A master liquid was prepared in advance by dissolving 0.05 parts by weight of photochromic compound (e) in 9.95 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane. To 41.3 parts by weight of a composition containing 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane and 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 10 parts by weight of the resulting master liquid was added and stirred, and then 8.6 parts by weight of a hydroxyl group-containing polyether compound (A1), 0.4 parts by weight of a polyether-modified siloxane compound (Polyflow KL-100 manufactured by Kyoeisha Chemical Co., Ltd.), and 0.1 parts by weight of an acidic phosphate ester (JP-506H manufactured by Johoku Chemical Industry Co., Ltd.) were added and stirred. (First Solution) Meanwhile, 40.1 parts by weight of 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane and 0.015 parts by weight of dimethyltin dichloride were added in advance and dissolved uniformly to prepare a solution. This solution was added to the first solution and stirred for 15 minutes at 15°C to 20°C to obtain a polymerizable composition. The polymerizable composition was then stirred and degassed for 1 hour and 30 minutes at 15°C to 20°C under a reduced pressure of 400 Pa or less, and then filtered using a 1.0 μm PTFE filter. The resulting polymerizable composition was poured into the space enclosed between the glass molds and heated from 10°C to 130°C over 24 hours (second polymerization step). The distance between the glass molds at the center of the lens was 0.8 mm. The lens was then cooled to room temperature and removed from the glass mold to obtain a 0.7 mm thick photochromic lens. The resulting photochromic lens (molded sample) was evaluated and measured as described in Experiment 2(1). The results are shown in Table 2.
[0139]
[0140] For Examples 2-1 to 2-3, when "(4) Confirmation of spherical domains (small-angle X-ray scattering measurement)" in Experiment 1 above was performed, all parameters converged, indicating that the block copolymers in the photochromic lenses of these Examples also formed core-shell type spherical domains.
[0141] This application claims priority based on Japanese Patent Application Nos. 2023-052882 and 2023-052885, filed on March 29, 2023, the disclosures of which are incorporated herein in their entireties.
Claims
1. A method for producing an optical member, comprising: a first polymerization step of reacting a hydroxyl group-containing polyether compound (A) with a di- or higher functional iso(thio)cyanate compound (B) to obtain a prepolymer; and a second polymerization step of mixing the obtained prepolymer with a di- or higher functional active hydrogen compound (C) and a catalyst (D) to polymerize and harden the mixture.
2. The method for producing an optical member according to claim 1, wherein in the first polymerization step, the hydroxyl group-containing polyether compound (A) and the difunctional or higher iso(thio)cyanate compound (B) are mixed and reacted by heating at 20°C or higher and 150°C or lower.
3. The method for producing an optical member according to claim 1 or 2, wherein in the first polymerization step, when the total amount of the hydroxyl group-containing polyether compound (A) and the difunctional or higher iso(thio)cyanate compound (B) is taken as 100 mass%, the hydroxyl group-containing polyether compound (A) is 0.5 mass% or more and 50 mass% or less.
4. The method for producing an optical member according to claim 1 or 2, wherein in the first polymerization step, the ratio of the number of hydroxyl group equivalents of the hydroxyl group-containing polyether compound (A) to the number of iso(thio)cyanate group equivalents of the difunctional or higher iso(thio)cyanate compound (B) (hydroxyl group / iso(thio)cyanate group) is 10 to 100,000.
5. The method for producing an optical member according to claim 1 or 2, wherein a di- or higher functional iso(thio)cyanate compound (B) is further added in the second polymerization step.
6. The method for producing an optical member according to claim 1 or 2, wherein in the second polymerization step, the reaction is carried out by heating to a maximum temperature of 100°C to 150°C.
7. A method for producing an optical member according to claim 1 or 2, further comprising a mixing step of mixing a hydroxyl group-containing polyether compound (A), a di- or higher functional iso(thio)cyanate compound (B), and a functional compound (E) prior to the first polymerization step.
8. The method for producing an optical member according to claim 7, wherein the functional compound (E) is a photochromic compound (e).
9. The method for producing an optical member according to claim 8, wherein the photochromic compound (e) is a naphthopyran-based compound having no active hydrogen.
10. An optical component comprising a cured product obtained by curing a polymerizable composition for optical materials, the cured product comprising a hydroxyl-containing polyether compound (A), a difunctional or higher iso(thio)cyanate compound (B), a difunctional or higher active hydrogen compound (C), a catalyst (D), and a functional compound (E), wherein the cured product comprises spherical domains comprising the hydroxyl-containing polyether compound (A), the difunctional or higher iso(thio)cyanate compound (B), and the functional compound (E), and the haze (%) relative to the thickness (mm) at the center of the optical component is 0.58% / mm or more and 30% / mm or less.
11. The optical member according to claim 10, wherein the maximum major axis of the spherical domains obtained by SAXS (small angle X-ray scattering) analysis is 1 nm or more and 300 nm or less.
12. The optical member according to claim 10 or 11, wherein the hydroxyl group-containing polyether compound (A) has a number average molecular weight of 500 to 50,000.
13. The optical member according to claim 10 or 11, wherein the hydroxyl-containing polyether compound (A) has 1 to 10 hydroxyl groups per molecule.
14. The optical member according to claim 10 or 11, wherein the hydroxyl group-containing polyether compound (A) comprises one or two compounds selected from the group consisting of polyethylene glycol and polypropylene glycol.
15. The optical member according to claim 10 or 11, wherein the di- or higher functional iso(thio)cyanate compound (B) is one or more compounds selected from the group consisting of alicyclic polyiso(thio)cyanate compounds, aromatic polyiso(thio)cyanate compounds, and modified compounds thereof.
16. The optical member according to claim 10 or 11, wherein the di- or higher functional iso(thio)cyanate compound (B) is one or more selected from the group consisting of xylylene diisocyanate, 2,5-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, 2,6-bis(isocyanatomethyl)bicyclo-[2.2.1]-heptane, tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, and phenylene diisocyanate.
17. The optical member according to claim 10 or 11, wherein the bifunctional or higher functional active hydrogen compound (C) has one or more functional groups selected from the group consisting of a hydroxy group, a mercapto group, an amino group, and a carboxyl group.
18. The bifunctional or higher active hydrogen compound (C) is 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, pentaerythritol tetrakis(2-mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), 2,5-bis(mercaptomethyl)-1,4-dithiane, bis(mercaptomethyl)-1,5-dithiane, 12. The optical member according to claim 10, comprising one or more polythiols selected from the group consisting of 1,1,3,3-tetrakis(mercaptomethylthio)propane, 4,6-bis(mercaptomethylthio)-1,3-dithiane, 2-(2,2-bis(mercaptomethylthio)ethyl)-1,3-dithietane, 1,1,2,2-tetrakis(mercaptomethylthio)ethane, 3-mercaptomethyl-1,5-dimercapto-2,4-dithiapentane, tris(mercaptomethylthio)methane, and ethylene glycol bis(3-mercaptopropionate).
19. The optical member according to claim 10 or 11, wherein the functional compound (E) is a photochromic compound (e).
20. The optical member according to claim 19, wherein the photochromic compound (e) is a naphthopyran-based compound having no active hydrogen.
21. The optical member according to claim 20, wherein the photochromic compound (e) is one or more compounds selected from the group consisting of naphthopyran compounds and spiropyran compounds.
22. An optical device comprising the optical member according to claim 10 or 11 and an electronic substrate.
23. An optical lens comprising the optical member according to claim 10 or 11.
Citation Information
Patent Citations
High impact poly(urethane urea) polysulfide
JP2005509703A
Polymerizable composition for optical material, molding, optical material, plastic lens, and laminated plastic lens
JP2020164839A
Method for producing resin composition and adhesive composition
JP2021080391A
Polymerizable composition for optical material, optical material obtained from said composition, and method for producing said composition
WO2018079518A1
Polymerizable composition for optical material, method of producing polymerizable composition for optical material, and method of producing optical article
WO2019177141A1