Method for manufacturing lithium hydroxide
The method of mixing lithium carbonate with a calcium compound and using an electrochemical device with a lithium selectively permeable membrane effectively addresses impurity issues and cost concerns in lithium hydroxide production, achieving high purity and efficiency.
Patent Information
- Application Number
- PCT/JP2024/011385
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional methods for producing lithium hydroxide from low-grade lithium carbonate suffer from impurity issues, particularly due to residual calcium ions, which reduce the purity of the lithium compound and are costly due to the use of expensive reagents like acetic acid.
A method involving the mixing of lithium carbonate with a calcium compound to form calcium carbonate, followed by solid-liquid separation and the use of an electrochemical device with a lithium selectively permeable membrane to recover lithium ions, maintaining a concentration above 3000 mass ppm to achieve high-purity lithium hydroxide production.
This method efficiently produces high-purity lithium hydroxide by selectively recovering lithium ions, even under conditions with residual calcium ions, and reduces production costs by avoiding expensive reagents.
Smart Images

Figure JP2024011385_03102024_PF_FP_ABST
Abstract
Description
How to manufacture lithium hydroxide
[0001] The present invention relates to a method for producing lithium hydroxide.
[0002] In recent years, lithium secondary batteries and the like have been used in fields such as information-related devices and communication devices, such as personal computers, video cameras, and mobile phones, and their use in hybrid cars and electric vehicles, which have been developed in response to carbon dioxide emission regulations, has also been considered. As a result, securing lithium sources has become more urgent than ever, and as part of this effort, technologies for recovering lithium by recycling lithium secondary batteries have been developed (see, for example, Patent Document 1).
[0003] Known lithium recovery technologies include a recovery method that involves contacting battery powder obtained by processing lithium-ion battery scrap with a leachate consisting of water, adding calcium hydroxide to the leachate, and leaching the powder as lithium hydroxide (see, for example, Patent Document 2), and a lithium hydroxide purification method that involves adding an alkali hydroxide to a solution in which lithium carbonate has been dissolved, performing solid-liquid separation, and drying the resulting lithium hydroxide under specified conditions (see, for example, Patent Document 3). Another proposed method involves reacting lithium carbonate with an acid containing acetic acid to produce lithium acetate, and then reacting the lithium acetate with a metal hydroxide to produce lithium hydroxide (see, for example, Patent Document 4).
[0004] JP 2019-81953 A JP 2019-178395 A JP 2012-106874 A JP 2019-131448 A
[0005] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a method for producing lithium hydroxide that can efficiently produce high-purity lithium hydroxide from low-grade lithium carbonate containing impurities such as brine.
[0006] A method for producing lithium hydroxide according to the present invention includes: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove a solid component containing calcium carbonate; recovering lithium ions from the lithium ion aqueous solution obtained by the solid-liquid separation into a recovered liquid using an electrochemical device equipped with a lithium permselective membrane; and obtaining lithium hydroxide from the recovered liquid, wherein a lithium ion concentration in the lithium ion aqueous solution is 3000 ppm by mass or more.
[0007] According to the present invention, it is possible to provide a method for producing lithium hydroxide that can efficiently produce high-purity lithium hydroxide from low-grade lithium carbonate containing impurities such as brine.
[0008] 1 is a flow diagram showing a preferred embodiment of the method for producing lithium hydroxide according to the present embodiment. 2 is a schematic diagram showing a preferred embodiment of an electrochemical device equipped with a lithium permselective membrane that can be used in the method for producing lithium hydroxide according to the present embodiment.
[0009] Hereinafter, a method for producing lithium hydroxide according to one embodiment of the present invention (hereinafter referred to as "this embodiment") will be described. In this specification, the upper and lower limit values of the ranges of "greater than or equal to," "less than or equal to," and "to" can be arbitrarily combined, and the numerical values in the examples can also be used as the upper and lower limit values. Furthermore, preferred specifications can be arbitrarily adopted. In other words, one preferred specification can be adopted in combination with one or more other preferred specifications. It can be said that a combination of preferred specifications is more preferable.
[0010] Furthermore, the method for producing lithium hydroxide according to one embodiment of the present invention is merely one embodiment of the method for producing lithium hydroxide according to one embodiment of the present invention, and the present invention is not limited to the method for producing lithium hydroxide according to one embodiment of the present invention. Furthermore, in this specification, lithium means both lithium and lithium ions, and should be interpreted appropriately unless technical contradiction arises.
[0011] (Findings Obtained by the Inventors to Achieve the Present Invention) The inventors conducted extensive research to solve the above-mentioned problems, and as a result, discovered the following and completed the present invention. The technology described in Patent Document 1 uses a lithium ion conductor to recover lithium ions from a source solution containing lithium ions, and a lithium permselective membrane is an extremely useful technology. However, with the recent increase in demand for lithium, there is a greater need than ever to improve the efficiency of lithium recovery. The inventors found that there is room for improvement in the overall efficiency of the production method for obtaining lithium hydroxide. Furthermore, the technology described in Patent Document 4 uses acetic acid, but acetic acid is expensive and volatile, resulting in high equipment costs, and therefore the inventors found that there are issues with reducing costs.
[0012] The technology described in Patent Document 2 involves contacting battery powder with a leachate consisting of water, reacting lithium carbonate in the leachate with calcium hydroxide to produce lithium hydroxide through a leaching process, and then obtaining lithium carbonate through a solid-liquid separation process and a Li-carbonation process. However, after the leaching process, only the solid-liquid separation process and the Li-carbonation process are assumed to produce lithium carbonate, and no attention is paid to obtaining lithium hydroxide contained in the leachate. Therefore, Patent Document 2 does not present or even suggest the problem of obtaining high-purity lithium hydroxide. Furthermore, Patent Document 2 only includes a solid-liquid separation process after the leaching process, and it is believed that the leachate produced in the leaching process contains residual calcium ions and the like. Therefore, there is a problem of a decrease in the purity of the lithium carbonate to be obtained, but no mention is made of this issue.
[0013] Furthermore, the technology described in Patent Document 3 involves adding an alkali hydroxide to a lithium carbonate solution, followed by solid-liquid separation to obtain lithium hydroxide, which is then dried under specified conditions to purify it. The invention described in Patent Document 3 aims to prevent deviations in the composition of water of crystallization in the resulting lithium hydroxide, and employs drying under specified conditions to solve this problem. However, since Patent Document 3 simply dries the filtrate containing lithium hydroxide obtained by solid-liquid separation, it is believed that the filtrate contains residues such as calcium ions. Therefore, there is also the issue of a decrease in the purity of the lithium hydroxide to be obtained, but no mention is made of this issue.
[0014] As described above, conventional lithium recovery technologies have a problem in that when lithium hydroxide is obtained by reacting lithium carbonate with calcium hydroxide, impurities derived from residual calcium ions are generated, resulting in a decrease in the purity of the lithium compound to be obtained. Based on the finding that the purity of the lithium compound decreases due to the presence of residual calcium ions in conventional technologies, the present inventors conducted studies focusing on whether the residual calcium ions can be reduced and whether the decrease in purity can be suppressed even if calcium ions remain. During the course of their studies, the present inventors adopted a lithium permselective membrane and found that highly pure lithium hydroxide could be obtained.
[0015] (Various aspects of the present embodiment) Hereinafter, a method for producing lithium hydroxide according to the first to sixteenth aspects of the present embodiment, an electrochemical device according to the seventeenth aspect, a method for producing a lithium-containing material according to the eighteenth aspect, and a method for producing a lithium-ion battery according to the nineteenth aspect will be described.
[0016] A method for producing lithium hydroxide according to a first aspect of the present embodiment includes: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove a solid component containing calcium carbonate; recovering lithium ions from the lithium ion aqueous solution obtained by the solid-liquid separation into a recovered liquid using an electrochemical device equipped with a lithium permselective membrane; and obtaining lithium hydroxide from the recovered liquid, wherein a lithium ion concentration in the lithium ion aqueous solution is 3000 ppm by mass or more.
[0017] To recover lithium from a solid raw material containing lithium carbonate and produce lithium hydroxide, it is effective to react lithium carbonate with a calcium compound to produce calcium carbonate and then recover lithium. However, the use of calcium compounds results in residual calcium ions, which reduces the purity of lithium compounds such as lithium hydroxide. After further investigation, the inventors discovered that using an electrochemical device equipped with a lithium permselective membrane makes it possible to recover only lithium ions. Furthermore, even under less favorable conditions, such as when calcium compounds are used and calcium ions remain, high-purity lithium hydroxide can be obtained by using an electrochemical device equipped with a lithium permselective membrane and maintaining a lithium ion concentration above a predetermined level, i.e., 3000 ppm by mass. Thus, the lithium hydroxide production method of this embodiment enables the efficient production of high-purity lithium hydroxide from low-grade lithium carbonate containing impurities, such as brine.
[0018] In the production method of this embodiment, a solid raw material containing lithium carbonate is first mixed with a calcium compound in a medium, whereby the lithium carbonate and the calcium compound react to produce calcium carbonate. This reaction allows lithium to be recovered from the lithium carbonate, and the resulting calcium carbonate can be easily separated by solid-liquid separation, yielding a lithium ion aqueous solution rich in lithium ions. Next, the lithium ion aqueous solution containing lithium ions at a predetermined concentration or higher is supplied to an electrochemical device equipped with a lithium permselective membrane, whereby only lithium can be efficiently recovered, enabling the efficient production of high-purity lithium hydroxide.
[0019] A method for producing lithium hydroxide according to a second aspect of the present embodiment is the same as that of the first aspect, except that the calcium compound is at least one selected from calcium hydroxide and calcium chloride. A method for producing lithium hydroxide according to a third aspect is the same as that of the second aspect, except that the calcium compound is calcium hydroxide.
[0020] By using calcium hydroxide alone, calcium chloride alone, or a combination of calcium hydroxide and calcium chloride as the calcium compound, it is possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide. In particular, by using calcium hydroxide, it is possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide.
[0021] A method for producing lithium hydroxide according to a fourth aspect of the present embodiment is any one of the first to third aspects, wherein a calcium ion concentration contained in the aqueous lithium ion solution is 20 ppm by mass or less.
[0022] According to the production method of this embodiment, even if calcium ions remain, it is possible to efficiently recover only lithium and efficiently produce high-purity lithium hydroxide. The lower the calcium ion concentration in the lithium ion aqueous solution, the more efficiently it is possible to recover only lithium and efficiently produce high-purity lithium hydroxide.
[0023] A method for producing lithium hydroxide according to a fifth aspect of the present embodiment is any one of the first to fourth aspects, further comprising subjecting the aqueous lithium ion solution to a chelate treatment. A method for producing lithium hydroxide according to a sixth aspect is the fifth aspect, further comprising subjecting the aqueous lithium ion solution after the chelate treatment to a calcium ion concentration of 10 ppm by mass or less.
[0024] The chelate treatment makes it easier to reduce the calcium ion concentration in the aqueous lithium ion solution, preferably to an extremely low concentration of 10 ppm by mass or less, which allows for more efficient recovery of lithium alone and more efficient production of high-purity lithium hydroxide.
[0025] A method for producing lithium hydroxide according to a seventh aspect of the present embodiment is any one of the first to sixth aspects, further comprising washing the solid content with a washing fluid and subjecting a washed material produced by the washing to solid-liquid separation. A method for producing lithium hydroxide according to an eighth aspect is the seventh aspect, further comprising mixing a liquid obtained by solid-liquid separation of the washed material with the aqueous lithium ion solution.
[0026] By subjecting the calcium carbonate-containing liquid to solid-liquid separation, it is possible to remove solids containing calcium carbonate. The removed solids containing calcium carbonate are accompanied by and contain an aqueous solution containing lithium hydroxide. By washing the solids with a washing fluid, it is possible to wash away the calcium carbonate and to incorporate the lithium hydroxide accompanying the solids into the washing fluid.
[0027] In this way, the washed material produced by washing contains washed calcium carbonate as a solid content and also contains a liquid containing lithium hydroxide. Therefore, by subjecting the washed material to solid-liquid separation, it is possible to separate the washed calcium carbonate from a liquid containing lithium hydroxide. Furthermore, since the crystallized product is a liquid containing lithium hydroxide, by mixing this with an aqueous lithium ion solution, it is possible to recover more lithium.
[0028] A liquid obtained by solid-liquid separation of the washed substance. A method for producing lithium hydroxide according to a ninth aspect of the present embodiment is any one of the first to eighth aspects, wherein the amount of the calcium compound used per 1.0 mol of the lithium carbonate is 1.0 mol or more and 2.0 mol or less.
[0029] By setting the amount of the calcium compound used relative to the lithium carbonate contained in the solid raw material within the above range, it is possible to more easily achieve a lithium ion concentration of 3000 mass ppm or more in the aqueous lithium ion solution, thereby more efficiently recovering lithium alone and more efficiently producing high-purity lithium hydroxide.
[0030] A method for producing lithium hydroxide according to a tenth aspect of the present embodiment is any one of the first to ninth aspects, wherein recovering the lithium hydroxide in the recovery solution is carried out while adjusting the temperature to 50°C or higher.
[0031] In an electrochemical device equipped with a lithium permselective membrane, efficient recovery of lithium ions requires that the lithium ion concentration in the lithium ion aqueous solution be a predetermined concentration or higher, and it is preferable to lower the calcium ion concentration. In addition, adjusting the temperature condition during recovery into a recovery solution to 50°C or higher is also effective for efficient recovery of lithium ions. That is, by adjusting the temperature during recovery into a recovery solution to 50°C or higher, only lithium can be recovered more efficiently, and high-purity lithium hydroxide can be produced more efficiently.
[0032] A method for producing lithium hydroxide according to an eleventh aspect of the present embodiment is any one of the first to tenth aspects, wherein, in recovering the lithium ion in the recovery liquid, the pH of the aqueous lithium ion solution is adjusted to 11 or more and 14 or less.
[0033] In addition to the above temperature conditions, by adjusting the pH of the aqueous lithium ion solution to 11 or more and 14 or less, it is possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide.
[0034] A lithium hydroxide production method according to a twelfth aspect of the present embodiment is any one of the first to eleventh aspects, wherein obtaining lithium hydroxide from the recovered solution comprises crystallizing the recovered solution and performing solid-liquid separation.
[0035] In an electrochemical device equipped with a lithium permselective membrane, when lithium hydroxide is obtained from a recovered solution from which lithium ions have been recovered, the recovered solution is crystallized and subjected to solid-liquid separation, whereby lithium hydroxide with a high purity can be produced more easily.
[0036] A thirteenth aspect of this embodiment relates to the method for producing lithium hydroxide of any one of the first to twelfth aspects, wherein the solid raw material contains at least one atom selected from a sodium atom, a potassium atom, a magnesium atom, a calcium atom, an iron atom, a cobalt atom, a nickel atom, a zinc atom, an aluminum atom, a silicon atom, a lead atom, a boron atom, a phosphorus atom, a sulfur atom, a fluorine atom, a chlorine atom, and a bromine atom.
[0037] The solid raw material used in the production method of this embodiment contains lithium carbonate, that is, contains lithium element, carbon element, and oxygen element, and in addition to these elements, contains iron element and at least one element selected from the above-mentioned elements. The production method of this embodiment can use a solid raw material containing such miscellaneous elements, for example, low-grade lithium carbonate containing impurities such as brine, as a solid raw material, and can efficiently produce high-purity lithium hydroxide.
[0038] A method for producing lithium hydroxide according to a fourteenth aspect of the present embodiment is any one of the first to thirteenth aspects, wherein the lithium hydroxide obtained in obtaining the lithium hydroxide is at least one selected from lithium hydroxide monohydrate and lithium hydroxide anhydrate.
[0039] According to the production method of this embodiment, either a monohydrate or anhydrous lithium hydroxide can be produced. For example, when lithium hydroxide is recovered from the recovered solution by the above-mentioned crystallization, a monohydrate is obtained. To produce an anhydrous lithium hydroxide, the monohydrate may be dried by heating, for example.
[0040] A method for producing lithium hydroxide according to a fifteenth aspect of the present embodiment is the method for producing lithium hydroxide according to the fourteenth aspect, wherein the purity of the lithium hydroxide is 98% or more. According to the production method of the present embodiment, lithium hydroxide with a high purity of 98% or more can be obtained.
[0041] A method for producing lithium hydroxide according to a sixteenth aspect of the present embodiment is any one of the first to fifteenth aspects, wherein the solid raw material containing lithium carbonate is a solid raw material containing lithium carbonate derived from recycled batteries selected from lithium ion batteries and all-solid-state lithium ion batteries.
[0042] According to the production method of this embodiment, a lithium ion battery and an all-solid-state lithium ion battery can be suitably used as a solid raw material source containing lithium carbonate.
[0043] An electrochemical device according to a seventeenth aspect of the present embodiment includes a lithium permselective membrane, and includes mixing a solid raw material containing lithium carbonate with a calcium compound in a medium, performing solid-liquid separation on the resulting calcium carbonate-containing liquid, and removing the solid content containing calcium carbonate to obtain an aqueous lithium ion solution, from which lithium ions are recovered into a recovered liquid.
[0044] The electrochemical device of this embodiment is provided with a lithium permselective membrane, which allows for efficient recovery of only lithium. Therefore, by using the electrochemical device, high-purity lithium hydroxide can be efficiently produced.
[0045] A method for producing a lithium-containing material according to an eighteenth aspect of the present embodiment includes: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove a solid content containing calcium carbonate; recovering lithium ions from an aqueous lithium ion solution having a lithium ion concentration of 3000 ppm by mass or more obtained by the solid-liquid separation, into a recovered liquid using an electrochemical device equipped with a lithium permselective membrane; obtaining lithium hydroxide from the recovered liquid; and producing a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide.
[0046] The method for producing a lithium-containing material of this embodiment is a method for producing a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material, using lithium hydroxide obtained by the method for producing lithium hydroxide of this embodiment. As described above, the method for producing lithium hydroxide of this embodiment makes it possible to efficiently produce high-purity lithium hydroxide, and as a result, the method for producing a lithium-containing material of this embodiment makes it possible to efficiently produce the lithium-containing material.
[0047] A method for producing a lithium ion battery according to a nineteenth aspect of the present embodiment includes: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation and removing a solid content containing calcium carbonate; recovering lithium ions from an aqueous lithium ion solution having a lithium ion concentration of 3000 ppm by mass or more obtained by the solid-liquid separation, into a recovered liquid using an electrochemical device equipped with a lithium permselective membrane; obtaining lithium hydroxide from the recovered liquid; obtaining a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide; and using a material selected from the lithium-containing materials.
[0048] The method for producing a lithium ion battery of this embodiment is a method for producing a lithium ion battery by mixing lithium-containing materials selected from the lithium-containing materials obtained by the method for producing a lithium-containing material of this embodiment. As described above, the method for producing a lithium-containing material of this embodiment makes it possible to efficiently produce a lithium-containing material, and as a result, the method for producing a lithium ion battery of this embodiment makes it possible to efficiently produce a lithium ion battery.
[0049] [Method for producing lithium hydroxide] The method for producing lithium hydroxide of this embodiment includes: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid, subjecting the calcium carbonate-containing liquid to solid-liquid separation and removing a solid component containing calcium carbonate, recovering lithium ions from the lithium ion aqueous solution obtained by the solid-liquid separation using an electrochemical device equipped with a lithium permselective membrane, and obtaining lithium hydroxide from the recovered solution, wherein the lithium ion concentration in the lithium ion aqueous solution is 3000 ppm by mass or more. Hereinafter, the method for producing lithium hydroxide of this embodiment will be described in more detail with reference to the flow chart shown in FIG.
[0050] The flow diagram shown in Fig. 1 is a flow diagram showing a preferred embodiment of the method for producing lithium hydroxide according to this embodiment. In the flow diagram shown in Fig. 1, a solid raw material containing lithium carbonate and a calcium compound are mixed in a medium, a calcium carbonate-containing liquid is obtained by the mixing, and the calcium carbonate-containing liquid is separated into a solid and a liquid by solid-liquid separation. The liquid is supplied as an aqueous lithium ion solution to an electrochemical device equipped with a lithium permselective membrane. The recovered liquid from which lithium ions have been recovered in the electrochemical device is subjected to a process such as evaporation to obtain lithium hydroxide.
[0051] The flow diagram shown in FIG. 1 also shows processes that are preferably included in the manufacturing method of this embodiment.
[0052] The chelate treatment shown in Figure 1 is a preferred treatment, and it is shown that the lithium ion aqueous solution is supplied to the electrochemical device after undergoing the chelate treatment. One preferred embodiment is to wash the solid fraction obtained by the solid-liquid separation using a cleaning fluid. The washed material obtained by washing with the cleaning fluid is further subjected to solid-liquid separation, and since the liquid contains lithium ions, it is mixed with the lithium ion aqueous solution and supplied to the electrochemical device. Furthermore, since the solid fraction has been washed, it becomes calcium carbonate with high purity.
[0053] FIG. 1 also shows that after lithium ions are recovered in the electrochemical device, the aqueous solution from which lithium ions have been recovered is reused when the solid raw material is mixed with the calcium compound.
[0054] [Mixing] The production method of the present embodiment includes obtaining a calcium carbonate-containing liquid by mixing a solid raw material containing lithium carbonate and a calcium compound in a medium.
[0055] (Medium) The medium used when mixing a solid raw material containing lithium carbonate with a calcium compound is preferably a liquid, taking into consideration the removal of solids that occurs after mixing and the recovery of lithium ions in a recovery solution using an electrochemical device, among other things. A liquid capable of dissolving lithium carbonate, a calcium compound, and their reaction products, particularly water, is preferred. This facilitates the production of an aqueous lithium ion solution, promotes the reaction between lithium carbonate contained in the solid raw material and the calcium compound, and allows for more efficient recovery of lithium alone, resulting in more efficient production of high-purity lithium hydroxide. Furthermore, the medium is easy to handle.
[0056] (Solid Raw Material) The solid raw material used in the production method of the present embodiment is not particularly limited as long as it contains lithium carbonate. Examples of the solid raw material containing lithium carbonate include solid raw materials obtained by concentrating seawater, salt lake brine, mining wastewater, geothermal water, or a combination of any of these solid raw material sources by means of evaporation or the like.
[0057] The production method of this embodiment can use, as a solid raw material, a variety of solid raw material sources, for example, low-grade lithium carbonate containing impurities obtained from lithium ion batteries, all-solid-state lithium ion batteries, etc. Therefore, the solid raw material used in the production method of this embodiment may contain, in addition to the lithium atoms, carbon atoms, and oxygen atoms contained in lithium carbonate, at least one atom selected from, for example, sodium atoms, potassium atoms, magnesium atoms, calcium atoms, iron atoms, cobalt atoms, nickel atoms, zinc atoms, aluminum atoms, silicon atoms, lead atoms, boron atoms, phosphorus atoms, sulfur atoms, fluorine atoms, chlorine atoms, and bromine atoms.
[0058] The atoms contained in the solid raw material other than the lithium atoms, carbon atoms, and oxygen atoms contained in lithium carbonate cannot be generally specified because they depend on the source of the solid raw material from which the solid raw material was obtained. Furthermore, although the content of atoms other than lithium atoms, carbon atoms, and oxygen atoms contained in the solid raw material cannot be generally specified either, the content of atoms other than lithium atoms, carbon atoms, and oxygen atoms contained in the solid raw material is usually 5,000 to 300,000 ppm by mass, and representative preferred ranges include 10 to 200 ppm by mass, 300 to 2,000 ppm by mass, 100 to 800 ppm by mass, 200 to 1,500 ppm by mass, and 1,500 to 4,500 ppm by mass.
[0059] The low-grade lithium carbonate that can be used in the production method of this embodiment contains moisture resulting from moisture absorption, brine, etc., as well as various other impurities. For example, low-grade lithium carbonate usually contains lithium atoms, boron atoms, sodium atoms, potassium atoms, magnesium atoms, calcium atoms, etc., and the content of these atoms, expressed as metal atoms, is usually 5,000 to 300,000 ppm by mass, with typical preferred ranges being 10 to 200 ppm by mass, 300 to 2,000 ppm by mass, 100 to 800 ppm by mass, 200 to 1,500 ppm by mass, and 1,500 to 4,500 ppm by mass.
[0060] In addition to the above, low-grade lithium carbonate may contain chlorine atoms, zinc atoms, aluminum atoms, lead atoms, etc. In such cases, the content of chlorine atoms is usually 300 to 2,000 mass ppm, and the contents of zinc atoms, aluminum atoms, and lead atoms are usually 0.5 to 50 mass ppm as metal atoms, with ranges of 0.1 to 10 mass ppm and 0.1 to 20 mass ppm being representatively preferred. 4 It may be contained at a content of 50 to 1,000 ppm by mass.
[0061] Furthermore, low-grade lithium carbonate derived from recycled batteries, particularly those selected from lithium ion batteries and all-solid-state lithium ion batteries, may contain cobalt atoms, nickel atoms, silicon atoms, phosphorus atoms, fluorine atoms, and bromine atoms. The low-grade lithium carbonate used in the production method of this embodiment varies depending on the properties of the brine and the types of lithium ion batteries and all-solid-state lithium ion batteries to be recycled. Therefore, the above-mentioned low-grade lithium carbonate is described as an example of a lithium carbonate having typical properties, and it goes without saying that the low-grade lithium carbonate is not limited to the above-mentioned one.
[0062] (Calcium Compound) The calcium compound can be any compound that can react with lithium carbonate to produce calcium carbonate, and calcium hydroxide and calcium chloride are preferred, with calcium hydroxide being particularly preferred. These calcium compounds react easily with lithium carbonate, allowing for more efficient recovery of lithium alone, and enabling more efficient production of high-purity lithium hydroxide. They are also easy to prepare into an aqueous solution and are easy to handle. These calcium compounds can be used alone or in combination.
[0063] The content of the calcium compound is preferably 0.3 mol / L or more, more preferably 0.5 mol / L or more, even more preferably 0.75 mol / L or more, and still more preferably 1.0 mol / L or more, based on the total amount of the calcium carbonate-containing liquid, and the upper limit is preferably 3.0 mol / L or less, more preferably 2.5 mol / L or less, even more preferably 2.0 mol / L or less, and still more preferably 1.7 mol / L or less. Here, the content of the calcium compound can also be considered as the amount (mol) of the calcium compound used per 1 L of the medium used. The numerical range can be any combination of the above upper and lower limits, and preferably includes 0.3 to 3.0 mol / L, 0.3 to 2.5 mol / L, 0.3 to 2.0 mol / L, 0.3 to 1.6 mol / L, 0.5 to 3.0 mol / L, 0.5 to 2.5 mol / L, 0.5 to 2.0 mol / L, 0.5 to 1.6 mol / L, 0.75 to 3.0 mol / L, 0.75 to 2.5 mol / L, 0.75 to 2.0 mol / L, 0.75 to 1.6 mol / L, 1.0 to 3.0 mol / L, 1.0 to 2.5 mol / L, 1.0 to 2.0 mol / L, and 1.0 to 1.6 mol / L. When the concentration is within the above range, calcium carbonate can be produced more efficiently by the reaction of lithium carbonate with a calcium compound, and as a result, only lithium can be recovered more efficiently, and high-purity lithium hydroxide can be produced more efficiently.
[0064] Furthermore, with regard to the amount of calcium compound used, the amount of calcium compound used per 1.0 mole of lithium carbonate is preferably 1.0 mole or more, with the upper limit being preferably 2.0 moles or less, more preferably 1.8 moles or less, even more preferably 1.5 moles or less, and even more preferably 1.2 moles or less. In particular, it is preferable to use 1.0 mole, i.e., the same number of moles of calcium compound as lithium carbonate. Within the above range, calcium carbonate can be produced more efficiently by the reaction between lithium carbonate and the calcium compound, and the concentration of calcium ions contained in the aqueous lithium ion solution can be reduced. As a result, lithium alone can be recovered more efficiently, and high-purity lithium hydroxide can be produced more efficiently.
[0065] (Mixing) The mixing of the solid raw material containing lithium carbonate and the calcium compound in a medium may be carried out to an extent that calcium carbonate is produced by a reaction between the lithium carbonate and the calcium compound, and may be carried out using a device generally called a stirrer or a mixer.
[0066] The mixing of the solid raw material containing lithium carbonate and the calcium compound in the medium may be carried out by supplying the solid raw material containing lithium carbonate and the calcium compound to a medium such as water and mixing them, or by mixing a mixture obtained by previously mixing the solid raw material containing lithium carbonate with water and the calcium compound, or by mixing a mixture obtained by previously mixing the calcium compound and water with the solid raw material containing lithium carbonate, or by mixing a mixture obtained by previously mixing the solid raw material containing lithium carbonate with water and a mixture obtained by previously mixing the calcium compound and water. Considering ease of operation, it is preferable to supply the solid raw material containing lithium carbonate and the calcium compound to the medium and mix them.
[0067] Examples of the stirrer or mixer include a mechanical stirring mixer that is equipped with a stirrer or stirring blades in a reaction vessel and is capable of stirring (also referred to as mixing by stirring or stirring and mixing). Examples of the mechanical stirring mixer include a high-speed stirring mixer and a double-arm mixer, and examples of the high-speed stirring mixer include a vertical-axis rotary mixer and a horizontal-axis rotary mixer. In the production method of this embodiment, any type of mixer may be used, and the type may be determined depending on the processing amount, etc.
[0068] The mixing time is not particularly limited as long as it is long enough to produce calcium carbonate by the reaction between lithium carbonate and the calcium compound, but is usually 1 minute or more, preferably 10 minutes or more, more preferably 30 minutes or more, even more preferably 1 hour or more, and still more preferably 3 hours or more. The upper limit is usually 10 hours or less, preferably 8 hours or less, more preferably 6 hours or less, and even more preferably 5 hours or less.
[0069] The temperature conditions during mixing are not particularly limited as long as they are such that calcium carbonate is produced by the reaction between lithium carbonate and the calcium compound, but are usually 10°C or higher, preferably 15°C or higher, and more preferably 20°C or higher. The upper limit is a temperature at which the calcium carbonate-containing liquid does not boil, and is usually 98°C or lower, and preferably 95°C or lower. Since the production efficiency of lithium hydroxide tends to increase slightly when mixed while heating, when considering reducing energy consumption, it is also preferable to use room temperature (23°C±3°C) without any particular adjustment of the temperature conditions. When production efficiency is particularly taken into consideration, mixing while heating may be performed within the above-mentioned upper limit temperature range.
[0070] [Removing Solid Content] The production method of the present embodiment includes subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove solid content containing calcium carbonate. By the solid-liquid separation, the solid content containing calcium carbonate contained in the calcium carbonate-containing liquid is removed, and at the same time, the separated liquid becomes an aqueous lithium ion solution.
[0071] (Solid-Liquid Separation) The method for solid-liquid separation is not particularly limited as long as it can separate a solid component containing calcium carbonate from a liquid contained in a calcium carbonate-containing liquid and remove the solid component containing calcium carbonate. For example, the solid-liquid separation may be performed using a solid-liquid separator that is generally used for solid-liquid separation, and examples of the solid-liquid separator that can be used include a vacuum filter, a pressure filter, a centrifuge, a belt press, and a screw press.
[0072] (Lithium ion aqueous solution) The lithium ion aqueous solution obtained by solid-liquid separation contains lithium ions at a concentration of 3000 ppm by mass or more. Since the lithium ion concentration is 3000 ppm by mass or more, even if the lithium ion aqueous solution contains calcium ions, high-purity lithium hydroxide can be efficiently obtained by using an electrochemical device equipped with a lithium permselective membrane.
[0073] The lithium ion concentration in the lithium ion aqueous solution is preferably 4000 ppm by mass or more, more preferably 6000 ppm by mass or more, even more preferably 8000 ppm by mass or more, and even more preferably 10000 ppm by mass or more. The upper limit of the lithium ion concentration is not particularly limited, and the higher the lithium ion concentration, the better. However, it is usually 15000 ppm by mass or less, preferably 12000 ppm by mass or less. When the lithium ion concentration is within the above range, only lithium can be recovered more efficiently, and highly pure lithium hydroxide can be obtained more efficiently.
[0074] The calcium ion concentration in the lithium ion aqueous solution is usually 20 ppm by mass or less. The calcium ion concentration is preferably 18 ppm by mass or less, more preferably 15 ppm by mass or less, and even more preferably 10 ppm by mass or less. The lower limit of the calcium ion concentration is preferably as low as possible, but there is no particular limitation, and in practice it is about 0.1 ppm by mass. When the calcium ion concentration is within the above range, lithium alone can be recovered more efficiently, and lithium hydroxide with high purity can be obtained more efficiently. Furthermore, as will be described later, a chelate treatment can be performed to reduce the calcium ion concentration.
[0075] (Solid Content and Washing) A solid content containing calcium carbonate is obtained by the solid-liquid separation. The solid content is obtained by performing solid-liquid separation on a calcium carbonate-containing liquid containing a solid content and a liquid, and therefore may contain an entrained liquid, i.e., an aqueous lithium ion solution. In order to obtain calcium carbonate with high purity, the production method of this embodiment preferably includes washing the solid content with a washing fluid, as shown in FIG. 1 . Furthermore, washing allows the aqueous lithium ion solution entrained in the solid content to be recovered, thereby making it possible to recover a larger amount of lithium.
[0076] The washing fluid is not particularly limited as long as it can wash calcium carbonate and recover the aqueous lithium ion solution entrained in the solids, but it is preferable to use water. By using water, the aqueous lithium ion solution entrained in the solids can be supplied to the liquid separated by the solid-liquid separation, and the lithium ions contained in the aqueous lithium ion solution entrained in the solids can be easily recovered.
[0077] In washing solids, the amount of washing fluid used is preferably 2 times or more, more preferably 3 times or more, and even more preferably 4 times or more, the mass of the solids. There is no particular upper limit, and the amount may be 10 times or less. In consideration of more efficient washing, the amount is preferably 8 times or less, more preferably 6 times or less, and even more preferably 5 times or less.
[0078] When the solid content is washed using a washing fluid, it is preferable to include solid-liquid separation of the washed product produced by washing, as shown in Fig. 1. The washed product produced by washing contains washed calcium carbonate with high purity as a solid content and a liquid containing an aqueous lithium ion solution. By subjecting the washed product to solid-liquid separation, washed calcium carbonate with high purity and a liquid containing an aqueous lithium ion solution are obtained.
[0079] The liquid obtained by solid-liquid separation of the washed object contains a lithium ion aqueous solution entrained in the solid content and a cleaning fluid, and if the cleaning fluid is water, it can be called a lithium ion aqueous solution. In the production method of this embodiment, it is preferable to mix the liquid obtained by solid-liquid separation of the washed object with the lithium ion aqueous solution obtained by solid-liquid separation of the calcium carbonate-containing liquid. This allows lithium ions contained in the lithium ion aqueous solution entrained in the solid content containing calcium carbonate to be supplied to an electrochemical device equipped with a lithium permselective membrane, thereby allowing a larger amount of lithium to be recovered.
[0080] (Chelate Treatment) The production method of the present embodiment preferably further includes chelate treating the aqueous lithium ion solution, as shown in Fig. 1. By chelate treating the aqueous lithium ion solution, calcium ions contained in the aqueous lithium ion solution can be more easily reduced, making it possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide.
[0081] The chelate treatment may be carried out according to a known method, for example, using a chelating adsorbent such as a chelating resin. A chelating adsorbent is generally a water-insoluble polymer substrate having a ligand that coordinates with metal ions to form a complex, and has the function of selectively adsorbing and separating specific metal ions. In the production method of this embodiment, a chelating adsorbent that selectively adsorbs and separates calcium is used.
[0082] Preferred examples of the chelating adsorbent include chelating resins having a sulfonic acid group, a phosphonic acid group, an iminodiacetic acid group, an aminophosphate group, an amidoxime group, a polyamino group, or a quaternary ammonium group as a functional group, and among these, chelating resins having an iminodiacetic acid group are preferred. The ionic type of the chelating resin may be a hydrogen type, a sodium type, or a calcium type, and among these, a sodium type is preferred.
[0083] The method of chelating treatment is not particularly limited, and either a continuous flow method (e.g., a method in which chelating treatment is performed using multiple chelating adsorption towers while switching between an adsorption process and an elution process) or a batch method (e.g., a method in which chelating treatment is performed by stirring in a chelating treatment tank storing a chelating adsorbent) can be used.
[0084] The calcium ion concentration in the lithium ion aqueous solution after the chelate treatment becomes extremely low, for example, 10 mass ppm or less, 8 mass ppm or less, 6 mass ppm or less, or 4 mass ppm or less.
[0085] [Recovering in a recovery solution] The production method of this embodiment includes recovering lithium ions from the lithium ion aqueous solution obtained by the solid-liquid separation into a recovery solution using an electrochemical device equipped with a lithium permselective membrane. By using an electrochemical device equipped with a lithium permselective membrane, it is possible to efficiently recover only the lithium ions contained in the lithium ion aqueous solution. Here, "only lithium ions" means that the solution is substantially free of ions other than Li ions, and the content of such other ions is 0.5 mass% or less.
[0086] (Electrochemical Device Comprising a Lithium Permselective Membrane) In the production method of this embodiment, lithium ions contained in the lithium ion aqueous solution are recovered into a recovery solution using an electrochemical device comprising a lithium permselective membrane. As described above, the lithium ion aqueous solution is obtained by mixing a solid raw material containing lithium carbonate with a calcium compound in a medium, subjecting the resulting calcium carbonate-containing liquid to solid-liquid separation, and removing the solids containing calcium carbonate. The electrochemical device is not particularly limited in terms of its type as long as it is equipped with a lithium permselective membrane. For example, the simplest configuration is an apparatus in which a water tank is partitioned by a lithium permselective membrane, with one tank serving as a lithium ion aqueous solution tank and the other as a recovery solution tank. A preferred example of an electrochemical device comprising a lithium permselective membrane, which is used in the production method of this embodiment, is described with reference to FIG. 2 .
[0087] 2 includes an aqueous lithium ion solution tank 10a for storing an aqueous lithium ion solution, a recovery solution tank 10b for storing a recovery solution, and a lithium permselective membrane 10c. The lithium permselective membrane 10c includes a first electrode 10d (anode) on one main surface side (the lithium ion aqueous solution tank 10a side) and a second electrode 10e (cathode) on the other main surface side (the recovery solution tank 10b side). By applying a voltage between the first electrode and the second electrode, lithium ions migrate from the aqueous lithium ion solution to the recovery solution via the lithium permselective membrane 10c, and are recovered by the recovery solution.
[0088] The lithium ion aqueous solution obtained by removing the solid content is supplied to a lithium ion aqueous solution tank 10a, and after the lithium ions are recovered, it is discharged from the lithium ion aqueous solution tank 10a. The lithium ion-recovered aqueous solution after the discharged lithium ions have been recovered can be discarded as is, or, as shown in Figure 1, may be reused when mixing the solid raw material with the calcium compound in the medium. By reusing the aqueous solution, it is no longer necessary to use a new solvent such as water, and lithium hydroxide can be produced more efficiently.
[0089] The recovered liquid from which lithium ions have been recovered is evaporated and dried to obtain lithium hydroxide, as shown in Fig. 1. Fig. 2 also shows that when the amount of recovered liquid stored in the recovered liquid tank 10b decreases, a recovered liquid not containing lithium ions (e.g., pure water) is supplied.
[0090] The electrochemical device 10 may have a configuration in which a single tank is divided into a lithium ion aqueous solution tank 10a and a recovery liquid tank 10b by a lithium permselective membrane 10c, or may have a configuration in which the two tanks, the lithium ion aqueous solution tank 10a and the recovery liquid tank 10b, are connected via the lithium permselective membrane 10c.
[0091] (Lithium Permselective Membrane) A lithium permselective membrane functions to transfer lithium ions from a lithium ion aqueous solution to a recovery solution. It is typically installed to separate the lithium ion aqueous solution from the recovery solution. The lithium permselective membrane preferably comprises a lithium permselective membrane body made of a superlithium ion conductor (ion conductor) with particularly high ionic conductivity, and a thin lithium adsorption layer formed on the lithium ion aqueous solution side. Using a superlithium ion conductor as the lithium permselective membrane body increases the ionic current of lithium ions flowing between the electrodes, thereby improving the lithium ion recovery efficiency. Here, lithium ions contained in the lithium ion aqueous solution exist as lithium hydrate ions, with water molecules coordinating around them. Therefore, to further increase the ionic current, it is effective to create a condition where water molecules can be easily removed from the surface of the lithium permselective membrane (the interface between the lithium permselective membrane and the lithium ion aqueous solution). Therefore, a lithium adsorption layer that adsorbs lithium ions (excluding hydrates) from the lithium ion aqueous solution is preferably formed on the surface of the lithium permselective membrane. That is, the lithium permselective membrane is preferably subjected to a surface lithium adsorption treatment. As a lithium adsorption layer, as will be described later, a layer formed by modifying the surface of the material constituting the lithium permselective membrane is preferred.
[0092] As the material constituting the lithium permselective membrane body, for example, the following oxides, oxynitrides, etc. containing lithium can be preferably mentioned. That is, the lithium permselective membrane preferably contains the following oxides, oxynitrides, etc. containing lithium. As the oxides containing lithium, for example, lithium lanthanum titanate: (Li x , La y ) TiO z (wherein x=3a-2b, y=2 / 3-a, z=3-b, 0<a≦1 / 6, 0≦b≦0.06, x>0) (hereinafter also referred to as "LLTO"), lithium lanthanum zirconate: Li 7 La 3 Zr 2 O 12(hereinafter also referred to as "LLZO"), lithium lanthanum niobate: Li 5 La 3 Nb 2 O 12 , lithium lanthanum tantalate: Li 5 La 3 Ta 2 O 12 The LLTO may more specifically be Li 0.29 La 0.57 TiO 3 (a≈0.1, b≈0) can be used.
[0093] These materials can be obtained as sintered bodies by, for example, mixing particles made of these materials with a sintering aid or the like and sintering the mixture at high temperatures (1000°C or higher). In this case, the surface of the lithium permselective membrane can be configured as a porous body in which fine particles made of LLTO are bonded (sintered), thereby increasing the effective surface area of the lithium permselective membrane body. This is true not only for LLTO, but also for other oxides containing Li and oxynitrides, which will be described later.
[0094] As a super lithium ion conductor that can be used as a material for constituting the lithium permselective membrane body, in addition to the above-mentioned LLTO, LLZO, etc. as an oxide containing lithium, for example, Li substituted NASICON (Na Super Ionic Conductor) type crystal, Li 1+x+y Al x (Ti, Ge) 2-x Si y P 3-y O 12 (where 0≦x≦0.6, 0≦y≦0.6) (Li 2 O-Al 2 O 3 -SiO 2 -P 2 O 5 -TiO 2 -GeO 2 system, hereinafter also referred to as "LASiPTiGeO").
[0095] Furthermore, examples of oxynitrides containing lithium include lithium phosphate oxynitride (Li 3Preferred examples of the nitride include PON (also referred to as "LiPON"), nitride of LLTO (LLTON), nitride of LLZO (LLZON), nitride of LASiPTiGeO (LASiPTiGeON), and the like.
[0096] The super lithium ion conductors such as the above-mentioned lithium-containing oxides and oxynitrides contain lithium as one of their constituent elements, and exhibit ionic conductivity by the movement of lithium ions outside the crystal between lithium sites in the crystal. Lithium ions flow through the lithium permselective membrane itself, but sodium ions cannot flow through the lithium permselective membrane. At this time, it is the lithium ions (Li + ) and lithium hydrate ions present in the lithium ion aqueous solution together with lithium ions cannot enter the lithium sites and therefore do not conduct through the crystal. In this respect, it is the same as the lithium permselective membrane described in WO2015 / 020121.
[0097] Here, if a large amount of lithium ions in particular are adsorbed onto the surface of the lithium permselective membrane body by the lithium adsorption layer, the water molecules of the lithium hydrated ions are removed during adsorption, leaving only lithium ions, and the lithium ion conduction efficiency (ionic current flowing through the lithium permselective membrane body) from the lithium ion aqueous solution side (one main surface side) of the lithium permselective membrane body to the recovery liquid side (the other main surface side) can be increased.
[0098] The lithium permselective membrane preferably has an anode and a cathode bonded thereto, with the anode being bonded to the lithium ion aqueous solution side (one main surface) of the lithium permselective membrane and the cathode being bonded to the recovered solution side (the other main surface). With this configuration, the one main surface of the lithium permselective membrane on the lithium ion aqueous solution side and the other main surface on the recovered solution side are maintained at a constant positive potential and a constant negative potential, respectively. As materials for the anode and cathode, metal materials that do not undergo electrochemical reactions in the lithium ion aqueous solution and the recovered solution can be used as appropriate. Examples of such metal materials include SUS, Ti, and Ti—Ir alloys.
[0099] Although the above-mentioned materials used as lithium permselective membranes are solids, they are known to exhibit electrical conductivity due to the flow of Li ions in the crystal in a form similar to free electrons. Therefore, when the anode is at a positive potential and the cathode is at a negative potential, lithium ions (positive ions) in the lithium ion aqueous solution on the anode side that reach the cathode side of the lithium permselective membrane flow by ionic conduction from the anode side (lithium ion aqueous solution) of the lithium permselective membrane to the cathode side (recovery solution). The lithium ions that reach the cathode side of the lithium permselective membrane are recovered in the recovery solution. Therefore, after a predetermined time has passed, the lithium ion concentration in the lithium ion aqueous solution decreases, while the lithium ion concentration in the recovery solution increases.
[0100] The lithium adsorption layer is formed as a thin layer on the surface of the lithium selective permeable membrane body by chemically treating the lithium selective permeable membrane body. Specifically, it is formed by acid treating one main surface of the lithium selective permeable membrane body (e.g., LLTO), for example by exposing this surface to hydrochloric acid or nitric acid for 5 days. This treatment causes lithium, which is particularly susceptible to oxidation among the constituent elements of the lithium selective permeable membrane body (e.g., LLTO), to be replaced with hydrogen in the acid, resulting in the formation of H 0.29 La 0.57 TiO 3 It is presumed that a substance layer (HLTO) having a composition similar to that of the lithium permselective membrane itself (e.g., LLTO) is formed. The formation of the thin surface layer (HLTO) is supported by the X-ray diffraction results in WO 2017 / 131051, which show the presence of a peak different from that of the lithium permselective membrane itself (e.g., LLTO).
[0101] The H sites in HLTO were originally intended for lithium ions, so H is particularly susceptible to substitution by lithium ions, but is difficult to substitute by other ions (such as sodium ions). Therefore, HLTO functions as a lithium adsorption layer. Furthermore, because HLTO is produced by a reaction with acid, it is formed only on the outermost surface of the lithium permselective membrane itself.
[0102] (Recovery Liquid) The recovery liquid used in this embodiment is not particularly limited as long as it can dissolve lithium ions, and can be appropriately selected depending on the form of lithium to be finally obtained. For example, pure water such as distilled water or ion-exchanged water is preferably used as the recovery liquid. The recovery liquid is supplied as water such as pure water or ion-exchanged water, and by transferring lithium ions from an aqueous lithium ion solution and recovering the lithium ions, a recovery liquid containing lithium ions (corresponding to the "recovery liquid (containing lithium ions)" in FIG. 2) is obtained. After obtaining lithium hydroxide by evaporation, drying, crystallization, or the like, the recovery liquid containing lithium ions becomes a recovery liquid substantially free of lithium ions. The recovery liquid substantially free of lithium ions can be reused as, for example, the "recovery liquid (not containing lithium ions)" shown in FIG. 2, instead of pure water such as distilled water or ion-exchanged water.
[0103] (Temperature Conditions) The recovery of lithium ions into the recovery solution is preferably carried out while adjusting the temperature to 50° C. or higher. By adjusting the temperature to 50° C. or higher, the recovery of lithium ions into the recovery solution is promoted, making it possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide.
[0104] There are no particular limitations on the method for adjusting the temperature, and it is preferable to adjust the temperature at least in the recovery liquid tank 10b to 50°C or higher, and it is also possible to adjust the temperatures in the recovery liquid tank 10b and the lithium ion aqueous solution tank 10a to 50°C or higher.
[0105] As a means for adjusting the temperature, for example, a heat exchanger such as a jacket type or heater type using electricity or a heat medium may be provided in the tank, or a method may be adopted in which the aqueous lithium ion solution and the recovery liquid are extracted from each tank, heated using a heat exchanger or the like, and then returned to each tank.
[0106] (pH Adjustment) The recovery of lithium ions into a recovery solution is preferably carried out while adjusting the pH of the lithium ion aqueous solution. By adjusting the pH, lithium ions can be efficiently recovered into the recovery solution. In this case, it is preferable to adjust the pH to a range of 11 to 14. Here, a pH of 11 to 14 is an adjustment target. Regarding the pH of the lithium ion aqueous solution, pH 11 includes a value of 10.5 to less than 11.5, and pH 14 includes a value of 13.5 to less than 14.5, and essentially means a range of 10.5 to less than 14.5.
[0107] When adjusting the pH of the lithium ion aqueous solution, there are no particular limitations on the means for doing so, and it may be done, for example, by adding an alkaline aqueous solution to the lithium ion aqueous solution. Furthermore, the adjustment of the pH of the lithium ion aqueous solution may be done when recovering lithium ions into the recovery liquid, i.e., the lithium ions may be recovered into the recovery liquid while adjusting the pH of the lithium ion aqueous solution, or it may be done in advance before recovering lithium ions into the recovery liquid. It goes without saying that if the pH of the lithium ion aqueous solution obtained by solid-liquid separation is within the above range, it is not necessary to adjust the pH.
[0108] Preferred examples of alkaline components of the alkaline aqueous solution used to adjust the pH of the lithium ion aqueous solution include sodium hydroxide, lithium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, tetramethylammonium hydroxide, tetraethylammonium hydroxide, calcium hydroxide, barium hydroxide, europium(II) hydroxide, thallium(I) hydroxide, and guanidine. These alkaline components may be used alone or in combination of two or more. Among these, sodium hydroxide is more preferred in view of its ability to rapidly adjust the pH.
[0109] [Obtaining lithium hydroxide from recovered solution] The method for producing lithium hydroxide according to this embodiment includes obtaining lithium hydroxide from the recovered solution. The method for obtaining lithium hydroxide from the recovered solution is not particularly limited as long as lithium hydroxide can be obtained, and examples thereof include evaporation by heating and drying, as shown in FIG. 1 . Methods for separating lithium hydroxide from the recovered solution are also included. More specifically, preferred examples include crystallization methods such as cooling crystallization and evaporation crystallization. According to crystallization methods, lithium hydroxide can be obtained without the need for a dehydration step such as heating and concentration, thereby reducing the energy consumption required for the dehydration step and making it possible to more efficiently produce lithium hydroxide with high purity.
[0110] In cooling crystallization, the recovery liquid is heated in a stage prior to crystallization, thereby increasing the Li ion content in the recovery liquid and creating a temperature difference, thereby enabling more efficient recovery of Li ions. In the case of cooling crystallization, the specific method is not particularly limited as long as it is carried out by a conventional cooling crystallization technique, and for example, it is preferable to carry out the crystallization while maintaining a positive pressure by blowing an inert gas into the Li ion-containing recovery liquid. Blowing in an inert gas can suppress the production of lithium carbonate and further promote the production of lithium hydroxide by cooling crystallization, allowing for more efficient production of high-purity lithium hydroxide.
[0111] In evaporative crystallization, the recovered liquid is heated in the stage prior to crystallization, so that the energy required for evaporation can be reduced. In the case of evaporative crystallization, the specific method is not particularly limited as long as it is carried out by a normal evaporative crystallization technique, and for example, it is preferable to carry out the evaporative crystallization while adjusting the temperature preferably to 80°C or higher and 100°C or lower. From the viewpoint of carrying out evaporative crystallization more efficiently, the adjusted temperature is more preferably 85°C or higher, and even more preferably 90°C or higher.
[0112] When lithium hydroxide is obtained by crystallization, the filtrate produced by crystallization can be reused as a recovered liquid. Because lithium ions are recovered from the recovered liquid by crystallization as lithium hydroxide anhydride or lithium hydroxide hydrate, the recovered liquid after lithium ions have been removed is used as part of the pure water newly supplied as the recovered liquid. By adding the filtrate to the recovered liquid and reusing it, it is possible to reduce the amount of lithium discharged from the filtrate and the amount of discharge of the filtrate itself, which is a major advantage. Furthermore, the amount of new pure water used to supply as the recovered liquid can be reduced, allowing for more efficient production of lithium hydroxide.
[0113] Furthermore, a heat exchanger can be provided that can utilize the waste heat from cooling crystallization and excess heat generated by evaporation crystallization to heat the recovered liquid. This makes it easier to adjust the temperature of the recovered liquid to 50°C or higher, promoting the recovery of lithium ions into the recovered liquid. This makes it possible to more efficiently recover only lithium and more efficiently produce high-purity lithium hydroxide. It also makes it possible to further increase thermal efficiency.
[0114] The lithium hydroxide obtained by crystallization is usually in the form of monohydrate (LiOH·H 2 O). The lithium hydroxide obtained by the production method of this embodiment can be used as is depending on the application, or can be further dehydrated before use. That is, according to the production method of lithium hydroxide of this embodiment, lithium hydroxide is obtained in the form of at least one of lithium hydroxide monohydrate and lithium hydroxide anhydride. When lithium hydroxide monohydrate is dehydrated, it may be dehydrated by drying, which is typically performed by heating, reducing pressure, or the like.
[0115] The purity of the lithium hydroxide obtained by the production method of this embodiment is, for example, 98% or more, 98.5% or more, or 99% or more. Thus, the lithium hydroxide obtained by the production method of this embodiment has an extremely high purity.
[0116] [Method for Producing Lithium-Containing Material] The method for producing a lithium-containing material of this embodiment includes mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid, subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove solids containing calcium carbonate, recovering lithium ions from a lithium ion aqueous solution having a lithium ion concentration of 3000 ppm by mass or more obtained by the solid-liquid separation using an electrochemical device equipped with a lithium permselective membrane, and producing lithium hydroxide from the recovered liquid. The lithium hydroxide is then used to produce a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material. That is, the method for producing a lithium-containing material of this embodiment uses the lithium hydroxide obtained by the method for producing lithium hydroxide of this embodiment. The method for producing lithium hydroxide employed in the method for producing a lithium-containing material of this embodiment is as described above.
[0117] (Lithium-containing material: lithium sulfide) The lithium-containing material obtained by the method for producing a lithium-containing material of the present embodiment is a material containing lithium selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material. Lithium sulfide can be produced, for example, by reacting lithium hydroxide with hydrogen sulfide.
[0118] (Lithium-Containing Material: Sulfide Solid Electrolyte) A sulfide solid electrolyte can be produced by using, for example, lithium hydroxide or lithium sulfide obtained using lithium hydroxide as a solid electrolyte raw material, and reacting raw material-containing materials including other solid electrolyte raw materials by mixing, etc. Other solid electrolyte raw materials that can be used in combination with lithium hydroxide or lithium sulfide obtained using lithium hydroxide are not particularly limited as long as they can produce a sulfide solid electrolyte, and preferred examples include substances containing at least one atom selected from a lithium atom, a phosphorus atom, and a sulfur atom, and more preferred examples include substances containing at least one atom selected from a lithium atom, a phosphorus atom, a sulfur atom, and a halogen atom.
[0119] Such a solid electrolyte raw material is, for example, diphosphorus trisulfide (P 2S 3 ), diphosphorus pentasulfide (P 2 S 5 Representative examples of suitable raw materials include raw materials containing at least two types of atoms selected from the above-mentioned atoms, such as phosphorus element, sulfur element, and the like. Among these, lithium sulfide and diphosphorus trisulfide (P 2 S 3 ), diphosphorus pentasulfide (P 2 S 5 Among phosphorus sulfides, phosphorus pentasulfide (P 2 S 5 ) is preferred.
[0120] The raw material may further contain a halogen atom, and examples of the raw material include substances containing a halogen atom. For example, lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; fluorine (F 2 ), chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ) and other simple halogen atoms are typically preferred.
[0121] The above solid electrolyte raw materials may be blended in a blending ratio that matches the composition of the sulfide solid electrolyte having the desired crystal structure. Examples of the blending ratio of lithium sulfide and other solid electrolyte raw materials contained in the raw material inclusions include those described in International Publication No. 2020 / 105737 (see paragraphs
[0024] to
[0028] ). Furthermore, the solid electrolyte raw material may be appropriately selected from the materials exemplified in International Publication No. 2020 / 105737 (see paragraphs
[0020] to
[0022] ).
[0122] The reaction of the raw material components can be carried out, for example, by mixing (i) or by heat treatment in a pressure vessel or by heat treatment in a solvent under reflux (ii). First, the process (i) will be described.
[0123] (Regarding Production Method (i)) The method for mixing the solid electrolyte raw materials containing lithium sulfide is not particularly limited as long as it can mix the solid electrolyte raw materials. For example, the method can be performed using a pulverizer, a mixer, an agitator, or the like. When a pulverizer is used, the raw materials are pulverized, but mixing also occurs at the same time. Mixing of the raw materials can also occur when a mixer or an agitator is used. Therefore, it can be said that the sulfide solid electrolyte obtained by the production method for a lithium-containing material of this embodiment can be preferably produced by stirring, mixing, pulverizing, or a combination of any of these processes, using two or more raw materials selected from substances containing at least one atom of a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom.
[0124] The equipment used to mix the raw material components, such as a grinder, mixer, or agitator, is not particularly limited and any commonly available equipment can be used.
[0125] In the above mixing, a solvent can be added to the above raw materials and mixed. As the solvent, various solvents widely known as organic solvents can be used. As the solvent, a wide range of solvents that have conventionally been used in the production of solid electrolytes can be used, and examples thereof include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents.
[0126] In addition to the hydrocarbon solvents, examples of the solvent include solvents containing heteroatoms such as nitrogen, oxygen, sulfur, and halogen atoms, and the like, in addition to carbon and hydrogen atoms. Such solvents have the property of readily forming complexes (which can also be referred to as "electrolyte precursors" because a sulfide solid electrolyte can be obtained by removing the complexing agent from the "complex") with raw materials containing lithium, phosphorus, sulfur, oxygen, and halogen atoms (hereinafter, such solvents are also referred to as "complexing agents"). These solvents facilitate the retention of halogen atoms within the structure of the sulfide solid electrolyte, making them useful in terms of achieving higher ionic conductivity. Furthermore, the use of a complexing agent is useful because it allows the solid electrolyte raw materials to be mixed using equipment such as a mixer or agitator, i.e., without the need for a pulverizer, to proceed with the reaction of the solid electrolyte raw materials.
[0127] As the complexing agent and the hydrocarbon solvent that can be employed, for example, the complexing agents and hydrocarbon solvents exemplified in International Publication No. 2020 / 105737 can be used. Among these solvents containing heteroatoms, it is preferable to use a solvent containing a nitrogen atom as the complexing agent, more preferably an amine solvent having an amino group, and even more preferably a diamine solvent having two amino groups.
[0128] (Drying) When producing a sulfide solid electrolyte and mixing is performed using a solvent, the method may include drying the fluid (usually a slurry) obtained by mixing. When a complexing agent is used as a solvent, the sulfide solid electrolyte is obtained by removing the complexing agent from a complex containing the complexing agent. When a complexing agent and a solvent are used in combination, the complexing agent is removed from a complex containing the complexing agent and the solvent is removed. When a solvent other than a complexing agent is used, the solvent is removed to obtain the sulfide solid electrolyte.
[0129] The drying method can be any method that can remove the solvent, and can be selected from solid-liquid separation, drying by heating, drying under reduced pressure (vacuum drying), and a combination of these. When a complexing agent is used as the solvent and the complexing agent is removed from the complex (electrolyte precursor), drying by heating is preferred, and it is preferably performed using a dryer such as a flow-type heater. This is because the complexing agent can be quickly removed from the complex (electrolyte precursor), and the generation of impurities can be more efficiently suppressed, resulting in a high-quality sulfide solid electrolyte. Preferred examples of the flow-type heater include a flash dryer, a spray dryer, and a fluidized dryer using a medium, with a flash dryer being particularly preferred.
[0130] (Heating) When producing a sulfide solid electrolyte, heating may be further included. If an amorphous sulfide solid electrolyte (glass component) is obtained by the above mixing, a crystalline sulfide solid electrolyte can be obtained by heating. Also, if a crystalline sulfide solid electrolyte is obtained, a crystalline sulfide solid electrolyte with improved crystallinity can be obtained. In either case, heating can make the resulting sulfide solid electrolyte a crystalline sulfide solid electrolyte, and can improve ionic conductivity. In other words, the heating can be considered an operation performed for crystallization.
[0131] When a complexing agent is used as a solvent during mixing, a complex containing the complexing agent is formed. However, the complexing agent can be removed from the complex by heating without performing the drying process, and a sulfide solid electrolyte can be obtained. Depending on the heating conditions, the sulfide solid electrolyte can be made amorphous or crystalline.
[0132] (Regarding Production Method (ii)) Production method (ii) is a production method in which the reaction of raw material contents is carried out by heat-treating in a solvent while heat-treating or refluxing in a pressure-resistant vessel. When the heat treatment using a pressure-resistant vessel is adopted as the production method for the sulfide solid electrolyte of this embodiment, it is a suitable method for producing a sulfide solid electrolyte having an argyrodite-type crystal structure, which will be described later. Details of the heat treatment in a solvent while heat-treating or refluxing in a pressure-resistant vessel in production method (ii) are explained in JP 2020-095953 A and the like, and these may be followed.
[0133] By the above-mentioned production methods (i) and (ii), an amorphous sulfide solid electrolyte and a crystalline sulfide solid electrolyte can be obtained as the sulfide solid electrolyte. The amorphous sulfide solid electrolyte contains lithium atoms, sulfur atoms, and phosphorus atoms, and preferably further contains halogen atoms. Representative examples include Li, 2 S-P 2 S 5 , and Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P 2 S 5 - LiBr, Li 2 S-P 2 S 5 -LiI-LiBr, etc., solid electrolytes composed of lithium sulfide, phosphorus sulfide, and lithium halide; and solid electrolytes further containing other atoms such as oxygen atoms and silicon atoms, for example, Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 -P 2 S 5 In order to obtain higher ionic conductivity, a solid electrolyte such as Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P2 S 5 - LiBr, Li 2 S-P 2 S 5 A solid electrolyte composed of lithium sulfide, phosphorus sulfide, and lithium halide, such as LiI-LiBr, is preferred. The types of atoms constituting the amorphous sulfide solid electrolyte can be confirmed, for example, by an ICP emission spectrometer.
[0134] In the amorphous sulfide solid electrolyte, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.6, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.05 to 0.5, and even more preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.08 to 0.4. Further, when bromine and iodine are used in combination as halogen atoms, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, bromine, and iodine is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.3: 0.01 to 0.3, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.02 to 0.25: 0.02 to 0.25, more preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.03 to 0.2: 0.03 to 0.2, and even more preferably 1.35 to 1.45: 1.4 to 1.7: 0.3 to 0.45: 0.04 to 0.18: 0.04 to 0.18. By setting the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms within the above range, it becomes easier to obtain a solid electrolyte with higher ionic conductivity having a thiolisiconregion II type crystal structure, an argyrodite type crystal structure, or the like, which will be described later.
[0135] The crystalline sulfide solid electrolyte may be a so-called glass ceramic obtained by heating an amorphous sulfide solid electrolyte to a crystallization temperature or higher, and its crystalline structure may be Li 3 P.S. 4 Crystal structure, Li 4 P 2 S 6 Crystal structure, Li 7 P.S. 6 Crystal structure, Li 7 P3 S 11 Examples of such structures include a crystal structure having peaks at 2θ=approximately 20.2° and 23.6° (for example, JP 2013-16423 A).
[0136] Preferred examples of the crystal structure include a thiosilicon region II crystal structure and an argyrodite crystal structure. Details of these crystal structures are described, for example, in International Publication Nos. 2024 / 010078 and 2024 / 010079. The atomic composition ratio of the crystalline sulfide solid electrolyte is determined by a composition formula corresponding to the various crystal structures, and is preferably within the range of the atomic composition ratio of the amorphous sulfide solid electrolyte. When the atomic composition ratio is within this range, it is easier to form a thiosilicon region II crystal structure or an argyrodite crystal structure, among the above crystal structures.
[0137] The sulfide solid electrolyte thus obtained can be used as it is in the solid electrolyte layer (separator layer) of a lithium ion battery, or can be mixed with an electrode active material described later to form an electrode mixture for use in a positive electrode or a negative electrode.
[0138] (Lithium-containing material: electrode active material) The electrode active material can be produced by using, for example, lithium hydroxide or lithium sulfide obtained using lithium hydroxide as a raw material, wet mixing or dry mixing with other raw materials such as hydroxide salts, halide salts, carbonates, and oxides containing atoms such as cobalt, nickel, manganese, iron, and phosphorus, followed by firing.
[0139] Examples of the electrode active material obtained in this way include LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminate), LNCO (lithium nickel cobalt oxide), and olivine-type compounds (LiMeNPO 4, Me=Fe, Co, Ni, Mn), LFP (lithium iron phosphate), NM (lithium nickel manganese oxide), etc. These lithium-containing transition metal composite oxides are also called oxide positive electrode active materials, and are mainly used as positive electrode active materials.
[0140] The electrode active material obtained by the method for producing a lithium-containing material of this embodiment can be used as an electrode mixture by mixing it with a sulfide solid electrolyte also obtained by the method for producing a lithium-containing material of this embodiment.
[0141] When preparing an electrode mixture, the blending ratio (mass ratio) of the electrode active material to the sulfide solid electrolyte is preferably 99.5:0.5 to 40:60, more preferably 99:1 to 50:50, and even more preferably 98:2 to 60:40, in consideration of improving battery performance and production efficiency.
[0142] Furthermore, when an electrode mixture is used, components that can be used other than the electrode active material and sulfide solid electrolyte include conductive materials that are carbon-based materials such as artificial graphite, graphite carbon fiber, resin-baked carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads, furfuryl alcohol resin-baked carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon; fluorine-based polymers such as polytetrafluoroethylene and polyvinylidene fluoride, thermoplastic elastomers such as butylene rubber and styrene-butadiene rubber, and various resin binders such as acrylic resins, acrylic polyol resins, polyvinyl acetal resins, polyvinyl butyral resins, and silicone resins.
[0143] When a conductive material is contained, the content of the conductive material in the electrode mixture is not particularly limited, but in consideration of improving battery performance and manufacturing efficiency, it is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more, with the upper limit being preferably 10% by mass or less, preferably 8% by mass or less, and even more preferably 5% by mass or less. Furthermore, when a binder is contained, the content of the binder in the electrode mixture is not particularly limited, but in consideration of improving battery performance and manufacturing efficiency, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, with the upper limit being preferably 20% by mass or less, preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0144] The electrode active material can be used as an electrode mixture, and the electrode mixture can be used as a positive electrode layer or a negative electrode layer of a lithium ion battery.
[0145] [Method for Manufacturing Lithium-Ion Battery] The method for manufacturing a lithium-ion battery of this embodiment includes mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid, subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove solids containing calcium carbonate, recovering lithium ions from a lithium ion aqueous solution having a lithium ion concentration of 3000 ppm by mass or more obtained by the solid-liquid separation using an electrochemical device equipped with a lithium permselective membrane, and obtaining lithium hydroxide from the recovered liquid, using the lithium hydroxide to obtain a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material, and using the material selected from the lithium-containing materials. That is, the method for manufacturing a lithium-ion battery of this embodiment uses the lithium-containing material obtained by the method for manufacturing a lithium-containing material of this embodiment. The method for manufacturing a lithium-containing material employed in the method for manufacturing a lithium-ion battery of this embodiment is as described above.
[0146] The material selected from the lithium-containing materials used in the manufacturing method of this embodiment is a material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material, and preferably a sulfide solid electrolyte and an electrode active material are used. As already described, the sulfide solid electrolyte is preferably used as is in the solid electrolyte layer of a lithium ion battery, and is also preferably mixed with an electrode active material to form an electrode composite for the positive or negative electrode of a lithium ion battery. Furthermore, the electrode active material is preferably mixed with a solid electrolyte such as a sulfide solid electrolyte to form an electrode composite for the positive or negative electrode of a lithium ion battery.
[0147] The lithium ion battery obtained by the manufacturing method of this embodiment preferably includes, for example, a positive electrode layer, a negative electrode layer, an electrolyte layer, and a current collector. The positive electrode layer and the negative electrode layer preferably use the above-mentioned electrode mixture, and the electrolyte layer preferably uses the sulfide solid electrolyte obtained by the manufacturing method of the lithium-containing material of this embodiment. Furthermore, a known current collector may be used. For example, a layer in which a material that reacts with the above-mentioned solid electrolyte, such as Au, Pt, Al, Ti, or Cu, is coated with Au or the like can be used.
[0148] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.
[0149] (Lithium hydroxide production apparatus) An apparatus having the configuration shown in the flow diagram of Fig. 1 was used. As an electrochemical apparatus equipped with a lithium permselective membrane, an apparatus having the configuration shown in Fig. 2 was used.
[0150] (Preparation of lithium permselective membrane) The lithium permselective membrane was prepared as follows. 0.29 La 0.57 TiO 3 One main surface of the lithium permselective membrane body was exposed to hydrochloric acid at 60°C for 5 days, thereby obtaining a lithium permselective membrane in which a lithium adsorption layer (HLTO) was formed on one main surface of the lithium permselective membrane body (LLTO).
[0151] (Measurement of Yield and Purity of Lithium Hydroxide) The solid (also referred to as "cake") obtained by filtration using the solid-liquid separation device of the lithium hydroxide manufacturing apparatus was transferred to a petri dish and dried at 40°C for 2 hours in a vacuum dryer (corresponding to a "drying device") to obtain a dried cake. The dried cake was weighed and used as the yield of lithium hydroxide monohydrate in each Example and Comparative Example, and the purity was measured by neutralization titration.
[0152] Example 1: 16.6 g of lithium carbonate (manufactured by Tokyo Chemical Industry Co., Ltd., purity 99.5%) and 16.7 g of calcium hydroxide were placed in an Erlenmeyer flask (volume: 300 mL), and 150 g of ion-exchanged water was poured in. The concentrations of lithium carbonate and calcium hydroxide were each 1.5 mol / L. A stirrer was placed in the Erlenmeyer flask, and mixing was performed for 4 hours using the stirrer at room temperature (23°C) (stirring speed: 500 rpm). The resulting calcium carbonate-containing solution was subjected to solid-liquid separation by vacuum filtration (filter paper: Type 5A equivalent as specified in JIS P3810:1995 was used), and solids including calcium carbonate were removed. The resulting liquid lithium ion aqueous solution was then supplied to a lithium ion aqueous solution tank of an electrochemical device equipped with a lithium permselective membrane. A voltage of 5 V was applied between the electrodes (first and second electrodes) on both sides of the lithium permselective membrane, and lithium ions were recovered in the recovery solution. The current value was 31 mA one hour after the start of voltage application. The current value is a numerical value that serves as an index of the recovery efficiency of lithium ions, and a larger current value means a higher recovery efficiency of lithium ions.
[0153] After 70 hours of voltage application, a portion (50.0 mL) of the recovered solution from which lithium ions had been recovered was heated to obtain 0.19 g of lithium hydroxide monohydrate, with a purity of 99.9%.
[0154] The solid content containing calcium carbonate after the solid-liquid separation (calcium carbonate concentration in the solid: 62.1 mass%) was dissolved in hydrochloric acid and then subjected to ion chromatography analysis. The measurement results are shown in Table 1 (lithium concentration and calcium concentration of the solid content containing calcium carbonate). In addition, the lithium ion aqueous solution after the solid-liquid separation was also subjected to ion chromatography analysis. The measurement results are shown in Table 1.
[0155] Example 2 Lithium hydroxide was obtained in the same manner as in Example 1, except that the lithium carbonate, calcium hydroxide, and ion-exchanged water were mixed at 90° C. The measurement results are shown in Table 1.
[0156] Example 3 The same operations as in Example 1 were performed up to solid-liquid separation of a calcium carbonate-containing liquid. 10 g of a calcium carbonate-containing solid obtained by solid-liquid separation was mixed with 40 g of ion-exchanged water as a washing fluid in a separately prepared Erlenmeyer flask, and the mixture was mixed for 10 minutes using a stirrer (stirring speed: 300 rpm). The washed product was subjected to solid-liquid separation by vacuum filtration (filter paper: equivalent to Type 5A as specified in JIS P3810:1995). The liquid obtained by solid-liquid separation was analyzed by ion chromatography. The obtained solid (washed calcium carbonate, calcium carbonate concentration in the solid: 94.0 mass%) was dissolved in hydrochloric acid and then analyzed by ion chromatography. The measurement results are shown in Table 1 (lithium concentration and calcium concentration of the calcium carbonate-containing solid).
[0157] Example 4 The same operations as in Example 1 were performed up to solid-liquid separation of the calcium carbonate-containing liquid, except that an Erlenmeyer flask (volume: 500 mL) was used, 33.2 g of lithium carbonate and 33.4 g of calcium hydroxide were added, and 300 g of ion-exchanged water was poured. 250 g of the lithium ion aqueous solution obtained by solid-liquid separation was poured into an Erlenmeyer flask (volume: 300 mL) containing 1.8 g of a chelating absorbent ("Lewatit Monoplus TP208 (trade name)" manufactured by AMP Ionex Co., Ltd.), and the mixture was mixed using a stirrer for 3 hours (stirring speed: 500 rpm) to perform a chelate treatment. Next, solid-liquid separation was performed, and the resulting liquid lithium ion aqueous solution was subjected to ion chromatography analysis. The measurement results are shown in Table 1. Furthermore, lithium ions were recovered from the lithium ion aqueous solution obtained by solid-liquid separation in the same manner as in Example 1. The current value 1 hour after the start of voltage application was 53 mA.
[0158] Comparative Example 1 Lithium hydroxide was obtained in the same manner as in Example 1, except that the amount of lithium carbonate used was 14.2 g, calcium hydroxide was not used, and the amount of ion-exchanged water used was 993.5 g. One hour after the start of voltage application, the current value was 10 mA.
[0159] Note: In Table 1, lithium ion aqueous solution 1 refers to the lithium ion aqueous solution obtained by mixing and solid-liquid separation, lithium ion aqueous solution 2 refers to the liquid obtained after washing the solid content containing calcium carbonate and performing solid-liquid separation on the washed matter, and lithium ion aqueous solution 3 refers to the lithium ion aqueous solution supplied to the electrochemical device.
[0160] In Examples 1 and 4, the current values one hour after the start of voltage application in the electrochemical device were 31 mA and 53 mA, respectively, which were greater than the current value of 10 mA in Comparative Example 1. This confirmed that the lithium ion recovery efficiency in the Examples was extremely high compared to Comparative Example 1, in which no calcium compound was used. Furthermore, the results of Example 1 also confirmed that the production method of this embodiment can obtain high-purity lithium hydroxide in high yield. Thus, it was confirmed that the production method of this embodiment can efficiently obtain high-purity lithium hydroxide. Note that, for convenience, lithium carbonate with a relatively high purity was used in the Examples. However, considering that the purity of the obtained lithium hydroxide was further improved as shown in Example 1, it is clear that even if low-grade lithium carbonate is used, lithium hydroxide with high purity can be obtained by improving the purity.
[0161] The lithium ion concentration in the lithium ion aqueous solution in Comparative Example 1 was 2643 ppm by mass, which is significantly lower than the lithium ion concentration of 11022 ppm by mass in Examples 1 and 4. The lithium carbonate content in Comparative Example 1 was 0.19 mol / L, and if the amount of lithium carbonate used was increased beyond this, the lithium carbonate would not dissolve but would precipitate. In other words, if a calcium compound is not used, the lithium ion concentration in the lithium ion aqueous solution cannot be increased to 2643 ppm by mass or more. According to the production method of this embodiment, by using lithium carbonate in combination with a calcium compound, it is possible to increase the lithium ion concentration in the lithium ion aqueous solution, and it can also be said that high-purity lithium hydroxide can be produced more efficiently.
[0162] The results of Example 4 confirmed that when chelate treatment was performed, the calcium concentration in the aqueous lithium ion solution supplied to the electrochemical device was 3.2 ppm by mass (see lithium ion aqueous solution 3 of Example 4 in Table 1), which was reduced to about one-fourth of the 12.3 ppm by mass in Example 1, in which chelate treatment was not performed. As a result, the current value one hour after the start of voltage application in the electrochemical device increased from 31 mA to 53 mA, indicating a further improvement in the recovery efficiency of lithium ions.
[0163] From the results of Example 2, it was confirmed that the lithium ion concentration and calcium ion concentration in the lithium ion aqueous solution increased slightly when the temperature condition for mixing was 90° C. If more efficient recovery of lithium ions is desired, mixing can be performed while heating, and if further reduction in energy consumption is desired, mixing can be performed at room temperature.
[0164] The results of Example 1 showed that the calcium carbonate-containing solid fraction removed by solid-liquid separation was accompanied by an aqueous lithium ion solution, and lithium ions resulting from this were detected. The results of Example 3 confirmed that washing the calcium carbonate-containing solid fraction could reduce the lithium content, based on the total amount of metal atoms contained in the solid fraction, from 12.5 mass % to 1.5 mass %. Furthermore, the liquid obtained by solid-liquid separation of the washed material contains the lithium ions that had accompanied the calcium carbonate-containing solid fraction. By mixing this liquid with an aqueous lithium ion solution, the lithium ions that had accompanied the calcium carbonate-containing solid fraction could be recovered, demonstrating that lithium ions could be recovered more efficiently.
[0165] 10. Electrochemical device with lithium permselective membrane 10a. Lithium ion aqueous solution tank 10b. Recovery liquid tank 10c. Lithium permselective membrane 10d. First electrode 10e. Second electrode
Claims
1. A method for producing lithium hydroxide, comprising: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation to remove a solid component containing calcium carbonate; recovering lithium ions from an aqueous lithium ion solution obtained by the solid-liquid separation using an electrochemical device equipped with a lithium permselective membrane, into a recovered liquid; and obtaining lithium hydroxide from the recovered liquid, wherein a lithium ion concentration in the aqueous lithium ion solution is 3000 ppm by mass or more.
2. The method for producing lithium hydroxide according to claim 1, wherein the calcium compound is at least one selected from calcium hydroxide and calcium chloride.
3. The method for producing lithium hydroxide according to claim 2, wherein the calcium compound is calcium hydroxide.
4. The method for producing lithium hydroxide according to any one of claims 1 to 3, wherein the calcium ion concentration in the aqueous lithium ion solution is 20 ppm by mass or less.
5. The method for producing lithium hydroxide according to any one of claims 1 to 4, further comprising subjecting the aqueous lithium ion solution to a chelate treatment.
6. The method for producing lithium hydroxide according to claim 5, wherein the concentration of calcium ions contained in the aqueous lithium ion solution after the chelate treatment is 10 ppm by mass or less.
7. A method for producing lithium hydroxide according to any one of claims 1 to 6, comprising washing the solids with a washing fluid, and subjecting a washed product produced by the washing to solid-liquid separation.
8. The method for producing lithium hydroxide according to claim 7, wherein the liquid obtained by solid-liquid separation of the washed matter is mixed with the aqueous lithium ion solution.
9. A method for producing lithium hydroxide according to any one of claims 1 to 8, wherein the amount of the calcium compound used per 1.0 mole of the lithium carbonate is 1.0 mole or more and 2.0 moles or less.
10. The method for producing lithium hydroxide according to any one of claims 1 to 9, wherein the recovery in the recovery liquid is carried out while adjusting the temperature to 50°C or higher.
11. The method for producing lithium hydroxide according to any one of claims 1 to 10, wherein the pH of the aqueous lithium ion solution is adjusted to 11 or more and 14 or less during recovery in the recovery liquid.
12. The method for producing lithium hydroxide according to any one of claims 1 to 11, wherein in obtaining lithium hydroxide from the recovered liquid, the recovered liquid is crystallized and subjected to solid-liquid separation.
13. A method for producing lithium hydroxide according to any one of claims 1 to 12, wherein the solid raw material contains at least one atom selected from the group consisting of sodium atoms, potassium atoms, magnesium atoms, calcium atoms, iron atoms, cobalt atoms, nickel atoms, zinc atoms, aluminum atoms, silicon atoms, lead atoms, boron atoms, phosphorus atoms, sulfur atoms, fluorine atoms, chlorine atoms, and bromine atoms.
14. A method for producing lithium hydroxide according to any one of claims 1 to 13, wherein the lithium hydroxide obtained in obtaining the lithium hydroxide is at least one selected from the group consisting of lithium hydroxide monohydrate and lithium hydroxide anhydride.
15. The method for producing lithium hydroxide according to claim 14, wherein the purity of the lithium hydroxide is 98% or more.
16. A method for producing lithium hydroxide according to any one of claims 1 to 15, wherein the solid raw material containing lithium carbonate is a solid raw material containing lithium carbonate derived from recycled batteries selected from lithium ion batteries and all-solid-state lithium ion batteries.
17. An electrochemical device having a lithium selective permeable membrane, which comprises mixing a solid raw material containing lithium carbonate with a calcium compound in a medium, performing solid-liquid separation of the resulting calcium carbonate-containing liquid, and removing the solids containing calcium carbonate to obtain an aqueous lithium ion solution from which lithium ions are recovered into a recovered liquid.
18. A method for producing a lithium-containing material, comprising: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation and removing a solid component containing calcium carbonate; recovering lithium ions from an aqueous lithium ion solution having a lithium ion concentration of 3000 ppm by mass or more obtained by the solid-liquid separation using an electrochemical device equipped with a lithium permselective membrane, into a recovered liquid; and obtaining lithium hydroxide from the recovered liquid; and using the lithium hydroxide to produce a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material.
19. A method for manufacturing a lithium ion battery, comprising: mixing a solid raw material containing lithium carbonate and a calcium compound in a medium to obtain a calcium carbonate-containing liquid; subjecting the calcium carbonate-containing liquid to solid-liquid separation and removing a solid component containing calcium carbonate; recovering lithium ions from an aqueous lithium ion solution obtained by the solid-liquid separation, the aqueous lithium ion solution having a lithium ion concentration of 3000 ppm by mass or more, into a recovered liquid using an electrochemical device equipped with a lithium permselective membrane; obtaining lithium hydroxide from the recovered liquid; obtaining a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide; and using a material selected from the lithium-containing materials.
Citation Information
Patent Citations
Lithium recovery apparatus and lithium recovery method
JP2019081953A
Method for producing lithium hydroxide
JP2021172537A
Method for producing lithium hydroxide
JP2022075619A
Method for recovering lithium from lithium ion secondary battery
JP2022164547A