Ion permeable membrane
Patent Information
- Application Number
- PCT/JP2024/011386
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-22
- Publication Date
- 2024-10-03
AI Technical Summary
Lithium ion permeable membranes used in lithium recovery face challenges with handling larger sizes, prone to cracking and distortion, and require weight reduction, while existing membranes with organic polymer ceramics suffer from pinhole generation and reduced quality.
An ion permeable membrane combining a solid electrolyte with alkalinity and a resin containing a carboxyl group, which enhances binding properties and suppresses pinhole formation, allowing for larger sizes, improved yield, and reduced weight.
The membrane achieves high-quality ion permeation, improved handling, and weight reduction, enabling efficient lithium recovery and production of lithium-containing materials for batteries.
Smart Images

Figure JP2024011386_03102024_PF_FP_ABST
Abstract
Description
ion-permeable membrane
[0001] The present invention relates to an ion-permeable membrane.
[0002] In recent years, lithium secondary batteries and the like have been used in fields such as information-related devices and communication devices, such as personal computers, video cameras, and mobile phones, and their use in hybrid cars and electric vehicles, which have been developed in response to carbon dioxide emission regulations, has also been considered. As a result, securing lithium sources has become more urgent than ever, and as part of this effort, technologies for recovering lithium by recycling lithium secondary batteries have been developed (see, for example, Patent Document 1).
[0003] Furthermore, as an ion-permeable membrane used for recovering ions such as lithium, in addition to the lithium-selective permeable membrane described in Patent Document 1, Patent Document 2, for example, proposes a membrane for separating target ions, which contains a material containing a target ion-permeable ceramic and a target ion-permeable organic polymer that is bonded to the permeable ceramic.
[0004] Japanese Patent Application Laid-Open No. 2019-81953 Japanese Patent Application Laid-Open No. 2022-543897
[0005] The present invention has been made in view of the above circumstances, and aims to provide an ion-permeable membrane that has high quality as a permeable membrane, is adaptable to larger sizes, has improved yields, is easier to handle, and is lightweight.
[0006] The ion-permeable membrane according to the present invention comprises an alkaline solid electrolyte and a resin containing a carboxy group, and has an acid value of more than 0 mgKOH / g.
[0007] According to the present invention, it is possible to provide an ion-permeable membrane that has high quality as a permeable membrane, is adaptable to large sizes, and has improved yield, improved handleability, and is lightweight.
[0008] 1 is a schematic diagram showing an example of a preferred configuration of an ion recovery device using the ion permeable membrane of the present embodiment. 2 is a schematic diagram showing an electrodeposition device used in a Li selectivity test in Examples. 3 is a scanning electron microscope (SEM) image (magnification: 1000x) of a cross section of the ion permeable membrane prepared in Example 4. 4 is an SEM image (magnification: 1000x) of a cross section of the ion permeable membrane prepared in Comparative Example 2.
[0009] Hereinafter, an embodiment of the present invention (hereinafter, sometimes referred to as "the present embodiment") will be described. In this specification, the upper and lower limit values of a range expressed as "greater than or equal to," "less than or equal to," and "to" can be arbitrarily combined, and the numerical values in the examples can also be used as the upper and lower limit values.
[0010] (Insights Gained by the Inventor to Achieve the Present Invention) Meanwhile, with the recent increase in demand for lithium, there has been a greater demand than ever before for larger devices and improved lithium recovery efficiency. The technology described in Patent Document 1 uses a lithium ion conductor to recover lithium ions from a source solution containing lithium ions, and the lithium permselective membrane used therein is an extremely useful technology. However, lithium permselective membranes using lithium ion conductors are prone to cracking and distortion during fabrication, and there is room for improvement in terms of handling, yield improvement, and handling ease, as they are prone to cracking during transportation. Furthermore, due to their heavy weight, weight reduction is also required to accommodate larger devices.
[0011] The membrane for separating target ions described in Patent Document 2 contains a target ion-permeable organic polymer bonded to a permeable ceramic, and therefore is more adaptable to larger sizes than the permeable membrane described in Patent Document 1, and is less susceptible to cracking and distortion during fabrication and transportation. However, pinholes are likely to cause a decrease in the membrane's functionality, posing a significant challenge for improving its quality. Thus, permeable membranes that allow specific atoms (ions) to pass through not only have high permeable quality, but also room for improvement in terms of adaptability to larger sizes, yield, ease of handling, and weight reduction.
[0012] In view of the problems with the permeable membranes described in Patent Documents 1 and 2, the present inventors focused on the resins used in the permeable membranes and conducted studies to improve them. During the course of their studies, they discovered that the use of a resin containing carboxyl groups provides excellent binding with ion-permeable substances, such as lithium ion conductors. It is believed that the excellent binding between the ion-permeable substance and the resin suppresses the occurrence of pinholes at the interface between them, resulting in a permeable membrane of high quality. It is also believed that improvements can be made in terms of adaptability to larger sizes, yield, ease of handling, and weight reduction.
[0013] In this way, the present inventors have been able to obtain a permeable membrane that can solve the above-mentioned problems by combining a substance having ion permeability with a resin containing a carboxyl group.
[0014] (Various Forms of the Present Embodiment) The ion-permeable membrane according to a first embodiment of the present embodiment is an ion-permeable membrane that includes an alkaline solid electrolyte and a resin containing carboxy groups and has an acid value exceeding 0 mgKOH / g. The ion-permeable membrane according to the present embodiment selectively permeates ions to be recovered, substantially permeating only ions, such as metal ions to be recovered in a treatment solution containing metal ions such as lithium ions, while blocking other ions and water. In this specification, "solid electrolyte" refers to an electrolyte that remains solid at 25°C under a nitrogen atmosphere. Furthermore, "alkaline" refers to a solution in which the solid electrolyte is dispersed, with a pH of 7.0 or higher. The ion-permeable membrane according to the present embodiment includes a resin having a carboxy group as an acidic group, thereby resulting in an acid value exceeding 0 mgKOH / g. By combining such a resin having an acidic group with an alkaline solid electrolyte, excellent binding properties can be achieved, as described above, and it is believed that the occurrence of pinholes is suppressed. Furthermore, the membrane can be made larger, is less prone to cracking and distortion during fabrication, has good yield and handleability, and is lightweight.
[0015] The ion-permeable membrane according to a second aspect of the present embodiment is the same as the first aspect, except that the alkaline solid electrolyte is an oxide solid electrolyte. The oxide solid electrolyte used in this embodiment is alkaline and can improve the recovery efficiency of lithium ions.
[0016] The ion-permeable membrane according to a third aspect of the present embodiment is the membrane according to the first or second aspect, wherein the resin containing a carboxy group is selected from a block copolymer containing a monomer having a carboxy group and an acid-modified resin graft-modified with a compound having a carboxy group. From the viewpoint of achieving better binding properties with an alkaline solid electrolyte, the resin containing a carboxy group is preferably a resin selected from a block copolymer containing a monomer having a carboxy group and an acid-modified resin graft-modified with a compound having a carboxy group.
[0017] The ion-permeable membrane according to a fourth aspect of the present embodiment is the same as that of the third aspect, except that the block copolymer is a block copolymer of a monomer having a carboxy group and an olefin monomer. From the viewpoint of achieving better binding properties with an alkaline solid electrolyte, the block copolymer is preferably a block copolymer of a monomer having a carboxy group and an olefin monomer.
[0018] The ion-permeable membrane according to a fifth aspect of the present embodiment is the same as that of the third aspect, except that the main chain of the acid-modified resin is formed from an olefin monomer. From the viewpoint of achieving better binding strength with an alkaline solid electrolyte, the main chain of the acid-modified resin is preferably formed from an olefin monomer.
[0019] The ion-permeable membrane according to a sixth aspect of the present embodiment is the third or fourth aspect, wherein the monomer having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof. When the monomer having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof, the ion-permeable membrane has better binding properties with an alkaline solid electrolyte.
[0020] The ion-permeable membrane according to a seventh aspect of the present embodiment is the third or fifth aspect, wherein the compound having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof. When the compound having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof, the binding strength with the alkaline solid electrolyte is improved.
[0021] The ion-permeable membrane according to an eighth aspect of the present embodiment is the sixth or seventh aspect, wherein the monomer having a carboxy group and the compound having a carboxy group are compounds selected from acrylic acid, methacrylic acid, maleic acid, and derivatives thereof. When the monomer having a carboxy group and the compound having a carboxy group are compounds selected from acrylic acid, methacrylic acid, maleic acid, and derivatives thereof, the ion-permeable membrane has better binding strength with an alkaline solid electrolyte.
[0022] The ion-permeable membrane according to a ninth aspect of the present embodiment is the membrane of any one of the first to seventh aspects, further comprising a resin that does not contain a carboxy group. By further comprising the resin that does not contain a carboxy group, the ion-permeable membrane of the present embodiment has a more uniform distribution of the resin and the solid electrolyte, thereby improving adhesion and, as a result, making it more impervious to water permeation.
[0023] The ion-permeable membrane according to a tenth aspect of the present embodiment is the ion-permeable membrane of the ninth aspect, wherein the resin not containing a carboxy group is an olefin resin. From the viewpoints of binding ability with the resin containing a carboxy group and making it more impervious to water permeation, the resin not containing a carboxy group is preferably an olefin resin.
[0024] The ion-permeable membrane according to an eleventh aspect of the present embodiment is the membrane of any one of the first to tenth aspects, wherein the content of the carboxyl group-containing resin is 1% by mass or more and 30% by mass or less. In the ion-permeable membrane of this embodiment, the content of the carboxyl group-containing resin is preferably within the above range, from the viewpoint of achieving better binding strength with an alkaline solid electrolyte.
[0025] The ion-permeable membrane according to a twelfth aspect of the present embodiment is the ion-permeable membrane of any one of the first to eleventh aspects, wherein the acid value is more than 0 mgKOH / g and not more than 20 mgKOH / g. From the viewpoint of further exhibiting the effects of the present disclosure, the ion-permeable membrane of the present embodiment preferably has an acid value within the above range.
[0026] The ion-permeable membrane according to a thirteenth aspect of the present embodiment is the membrane of any one of the first to twelfth aspects, which allows lithium ions to permeate, and the ion-permeable membrane according to a fourteenth aspect of the present embodiment is the membrane of any one of the first to thirteenth aspects, which is for recovering lithium ions. The ion-permeable membrane of the present embodiment can be suitably used for recovering lithium ions.
[0027] A lithium recovery device according to a fifteenth aspect of the present embodiment includes an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g.
[0028] The ion-permeable membrane employed in the lithium recovery device of this embodiment has high quality as a permeable membrane, while also being adaptable to larger sizes, improved yield, improved handleability, and reduced weight. Therefore, the lithium recovery device of this embodiment equipped with this membrane can efficiently recover lithium and can easily be adapted to larger sizes.
[0029] A method for producing lithium hydroxide according to a sixteenth aspect of the present embodiment involves recovering lithium hydroxide from a lithium ion-containing liquid using an ion-permeable membrane that includes a solid electrolyte exhibiting alkaline properties and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g.
[0030] The ion-permeable membrane employed in the lithium recovery device of this embodiment has high quality as a permeable membrane, while also being adaptable to larger sizes, improving yield, improving handleability, and reducing weight. Therefore, the lithium hydroxide production method of this embodiment using this membrane can efficiently produce lithium hydroxide.
[0031] A method for producing a lithium-containing material according to a seventeenth aspect of the present embodiment comprises recovering lithium hydroxide from a lithium ion-containing solution using an ion-permeable membrane that includes a solid electrolyte exhibiting alkaline properties and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g, and producing a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide.
[0032] The method for producing a lithium-containing material of this embodiment is a method for producing a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material, using lithium hydroxide obtained by the method for producing lithium hydroxide of this embodiment. As described above, the method for producing lithium hydroxide of this embodiment makes it possible to efficiently produce lithium hydroxide, and as a result, the method for producing a lithium-containing material of this embodiment makes it possible to efficiently produce the lithium-containing material.
[0033] A method for manufacturing a lithium ion battery according to an eighteenth aspect of the present embodiment includes recovering lithium hydroxide from a lithium ion-containing solution using an ion-permeable membrane that includes an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g, obtaining a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide, and using a material selected from the lithium-containing materials.
[0034] The method for producing a lithium ion battery of this embodiment is a method for producing a lithium ion battery by mixing lithium-containing materials selected from the lithium-containing materials obtained by the method for producing a lithium-containing material of this embodiment. As described above, the method for producing a lithium-containing material of this embodiment makes it possible to efficiently produce a lithium-containing material, and as a result, the method for producing a lithium ion battery of this embodiment makes it possible to efficiently produce a lithium ion battery.
[0035] (Ion-permeable membrane) The ion-permeable membrane of this embodiment includes an alkaline solid electrolyte and a carboxyl group-containing resin, and has an acid value of greater than 0 mgKOH / g. As described above, the carboxyl group-containing resin of this embodiment results in an acid value of greater than 0 mgKOH / g, thereby improving the adhesion to the alkaline solid electrolyte and suppressing the occurrence of pinholes, resulting in a high-quality membrane. The acid value of the ion-permeable membrane is preferably greater than 0 mgKOH / g and not greater than 20 mgKOH / g, more preferably 1 mgKOH / g or more and 18 mgKOH / g or less, and even more preferably 2 mgKOH / g or more and 15 mgKOH / g or less. In this specification, the acid value can be measured in accordance with JIS K0070:1992, specifically, by the method described in the Examples. The acid value of the ion-permeable membrane can be appropriately adjusted by changing the type and content of the carboxyl group-containing resin.
[0036] The ion-permeable membrane of this embodiment may be a single layer or a multi-layer structure consisting of two or more layers. From the viewpoint of ion selectivity, the thickness of the ion-permeable membrane is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 10 μm or more, and even more preferably 50 μm or more. On the other hand, from the viewpoint of further suppressing cracking and improving ion recovery efficiency, the thickness is preferably 1 mm or less, more preferably 500 μm or less, even more preferably 300 μm or less, and even more preferably 200 μm or less. When the ion-permeable membrane is a multi-layer membrane, the thickness of the ion-permeable membrane is the total thickness of the layers.
[0037] The ions selectively permeable by the ion-permeable membrane of this embodiment are preferably metal ions that are cations in which the metal atom has lost an electron, preferably ions of typical metals or transition metals, more preferably alkali metal ions, alkaline earth metal ions, magnesium group metal ions, aluminum group metal ions, rare earth group metal ions, iron group metal ions, chromium group metal ions, manganese group metal ions, noble metal ions, platinum group metal ions, lanthanoid metal ions, or actinoid metal ions, even more preferably alkali metal ions, alkaline earth metal ions, noble metal ions, platinum group metal ions, lanthanoid metal ions, or actinoid metal ions, even more preferably alkali metal ions, even more preferably lithium ions or sodium ions, and particularly preferably lithium ions. Thus, the ion-permeable membrane of this embodiment is preferably used for recovering metal ions. As the metal ion, the above-mentioned metal ions are preferably used, and among them, it is preferable to use it for recovering lithium ions or sodium ions, and it is particularly preferable to use it for recovering lithium ions.
[0038] (Solid electrolyte exhibiting alkaline properties) The solid electrolyte used in the present embodiment is not particularly limited as long as it exhibits alkaline properties. However, from the viewpoint of further increasing the ion recovery efficiency, an oxide solid electrolyte is preferable. As the oxide solid electrolyte, for example, a NASICON (sodium super ionic conductor) type oxide (for example, Li 3.5 Zn 0.25 GeO 4 ), LISICON (Lithium super ionic conductor) type oxides (e.g., Li 3.5 Zn 0.25 GeO 4 ), garnet-type oxides (e.g., Li 7 La 3 Zr 2 O 12 , LLZO), perovskite-type oxides (e.g., La 0.55 Li 0.35 TiO 3 ) and the like. More specifically, lithium lanthanum titanate: (Li x , La y ) TiO z (where x = 3a - 2b, y = 2 / 3 - a, z = 3 - b, 0 < a ≤ 1 / 6, 0 ≤ b ≤ 0.06, x > 0) (hereinafter referred to as LLTO) can be used, and more specifically, Li 0.29 La 0.57 TiO 3 (a ≒ 0.1, b ≒ 0) can be used. These materials can be obtained as sintered bodies by mixing particles made of these materials with sintering aids and the like and sintering the mixture at high temperatures (1000°C or higher).
[0039] The shape of the alkaline solid electrolyte is not particularly limited, and may be, for example, particulate. From the viewpoint of further reducing the resistance of the ion-permeable membrane, the median diameter of the particles of the alkaline solid electrolyte is preferably 100 μm or less, more preferably 10 μm or less. On the other hand, from the viewpoint of suppressing an increase in interfacial resistance between particles and between the particles and the resin containing a carboxy group, the median diameter of the particles of the alkaline solid electrolyte is preferably 1 nm or more, more preferably 10 nm or more. In this specification, the median diameter of the particles of the alkaline solid electrolyte is the volume-based median diameter measured using a laser diffraction / scattering particle size distribution analyzer.
[0040] The content of the alkaline solid electrolyte contained in the ion-permeable membrane is preferably 70% by mass or more and 99% by mass or less, more preferably 75% by mass or more and 99% by mass or less, and even more preferably 80% by mass or more and 99% by mass or less. When the content of the alkaline solid electrolyte is 70% by mass or more, the ion recovery efficiency can be further improved, and when it is 99% by mass or less, cracks and distortions during production are less likely to occur, and the yield and handleability are improved.
[0041] (Carboxy group-containing resin) The carboxy group-containing resin used in this embodiment is not particularly limited as long as it has one or more carboxy groups in one molecule, but from the viewpoint of improving the binding ability with the alkaline solid electrolyte, it is preferable that the resin is selected from a block copolymer containing a monomer having a carboxy group and an acid-modified resin graft-modified with a compound having a carboxy group. One type of carboxy group-containing resin may be used, or two or more types may be used in combination.
[0042] (Block copolymer containing a monomer having a carboxy group) The block copolymer containing a monomer having a carboxy group (hereinafter also simply referred to as "block copolymer") is preferably a block copolymer of a monomer having a carboxy group and an olefin monomer. When the block copolymer is used together with a resin not containing a carboxy group, which will be described later, the affinity between the resin containing a carboxy group and the resin not containing a carboxy group is increased, thereby obtaining an ion-permeable membrane of higher quality.
[0043] From the viewpoint of achieving superior binding properties with the alkaline solid electrolyte, the carboxyl group-containing monomer is preferably a compound selected from unsaturated carboxylic acids and their derivatives. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, fumaric acid, itaconic acid, crotonic acid, citraconic acid, sorbic acid, mesaconic acid, and angelic acid. Derivatives thereof include acid anhydrides, esters, amides, imides, and metal salts, such as maleic anhydride, itaconic anhydride, citraconic anhydride, methyl acrylate, methyl methacrylate, ethyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, maleic acid monoethyl ester, acrylamide, maleic acid monoamide, maleimide, N-butylmaleimide, sodium acrylate, and sodium methacrylate. From the viewpoint of achieving superior binding properties with the alkaline solid electrolyte, the carboxyl group-containing monomer is preferably a compound selected from acrylic acid, methacrylic acid, maleic acid, and derivatives thereof, and more preferably acrylic acid or maleic anhydride, which may be used alone or in combination of two or more.
[0044] The content of the monomer having a carboxy group contained in the block copolymer is preferably 0.1 to 50 mass %, more preferably 1 to 20 mass %, and even more preferably 1.5 to 15 mass %, from the viewpoint of improving the binding property with the alkaline solid electrolyte.
[0045] As the olefin monomer, for example, one or more types selected from α-olefins having 2 to 30 carbon atoms can be used. Specific examples include linear olefins such as ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, and 1-decene; and branched olefins such as isobutene and 4-methyl-1-pentene. These olefin monomers may be used alone or in combination of two or more types. Among them, ethylene and propylene are preferred, and propylene is more preferred, from the viewpoint of improving alkali resistance.
[0046] The mass ratio of the monomer having a carboxy group to the olefin monomer [monomer having a carboxy group / olefin monomer] is preferably 0.1 / 99.9 to 50 / 50, more preferably 1 / 99 to 20 / 80, and even more preferably 1.5 / 98.5 to 15 / 85, from the viewpoint of achieving better binding properties with the alkaline solid electrolyte.
[0047] The method for producing the block copolymer is not particularly limited, and the block copolymer can be produced by a known polymerization method such as an ionic polymerization method such as anionic polymerization or cationic polymerization, or a radical polymerization method.
[0048] (Acid-modified resin graft-modified with a compound having a carboxy group) In the acid-modified resin graft-modified with a compound having a carboxy group (hereinafter also simply referred to as "acid-modified resin"), the main chain of the acid-modified resin is preferably formed from an olefin monomer. When the acid-modified resin is used together with a resin not containing a carboxy group, which will be described later, the affinity between the resin containing a carboxy group and the resin not containing a carboxy group is increased, thereby resulting in an ion-permeable membrane of higher quality.
[0049] Examples of the olefin monomer forming the main chain of the acid-modified resin include those exemplified as the olefin monomer in the section (Block copolymer containing a monomer having a carboxy group). As the olefin monomer, from the viewpoint of improving alkali resistance, ethylene and propylene are preferred, and propylene is more preferred. These may be used alone or in combination of two or more.
[0050] The resin constituting the main chain of the acid-modified resin is preferably polypropylene, and the polypropylene may be a specific polypropylene exemplified below as a resin not containing a carboxy group. Examples of polypropylene include propylene homopolymers and propylene-olefin copolymers, with propylene homopolymers being preferred.
[0051] The acid-modified resin is obtained by grafting a compound having a carboxy group onto a resin constituting the main chain. The compound having a carboxy group is preferably a compound selected from unsaturated carboxylic acids and their derivatives, from the viewpoint of improving the binding ability with alkaline solid electrolytes. Examples of unsaturated carboxylic acids and their derivatives include those exemplified as unsaturated carboxylic acids and their derivatives in the section (Block copolymer containing a monomer having a carboxy group). The compound having a carboxy group is preferably a compound selected from acrylic acid, methacrylic acid, maleic acid, and their derivatives, more preferably acrylic acid and maleic anhydride, from the viewpoint of improving the binding ability with alkaline solid electrolytes. These may be used alone or in combination of two or more.
[0052] The acid-modified amount of the acid-modified resin is preferably 0.5 to 20.0 mass %, more preferably 0.8 to 18.0 mass %, and even more preferably 1.0 to 15.0 mass %, from the viewpoint of further enhancing the binding strength with the alkaline solid electrolyte. The acid-modified amount can be determined by infrared absorption (IR) spectroscopy, specifically, by the method described in the Examples.
[0053] The method for producing the acid-modified resin is not particularly limited, and examples thereof include a radical graft reaction, i.e., a reaction in which radical species are generated in a resin constituting the main chain, and a compound having a carboxy group is graft-polymerized using the radical species as a polymerization initiation point.
[0054] The radical generator is not particularly limited, but is preferably an organic peroxide. Examples of the organic peroxide include peroxides such as di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, dicumyl peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butylperoxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, and lauroyl peroxide; and azonitriles such as azobisisobutyronitrile and azobisisopropionitrile.
[0055] From the viewpoint of further enhancing the binding strength with the alkaline solid electrolyte, the carboxyl group-containing resin has an acid value of more than 0 mgKOH / g, preferably 1 mgKOH / g or more and 100 mgKOH / g or less, and more preferably 5 mgKOH / g or more and 80 mgKOH / g or less.
[0056] From the viewpoint of ease of mixing with the solid electrolyte, the carboxyl group-containing resin preferably has a weight average molecular weight (Mw) of 20,000 to 150,000, more preferably 25,000 to 100,000, and even more preferably 30,000 to 50,000. Easier mixing allows the solid electrolyte and resin to be more uniformly present, thereby increasing adhesion and, as a result, making it more impervious to water permeation.
[0057] From the viewpoint of ease of mixing with the solid electrolyte, the carboxyl group-containing resin preferably has a molecular weight distribution (Mw / Mn) of 1.5 to 4.0, more preferably 1.6 to 3.0, even more preferably 1.7 to 2.8, and even more preferably 1.8 to 2.5. Easier mixing allows the solid electrolyte and resin to be more uniformly present, thereby increasing adhesion and, as a result, making it more impervious to water permeation.
[0058] In this specification, the weight average molecular weight (Mw) and molecular weight distribution (Mw / Mn) are determined by gel permeation chromatography (GPC). The weight average molecular weight is a weight average molecular weight measured in terms of polystyrene using the following apparatus and conditions, and the molecular weight distribution is a value calculated from the number average molecular weight (Mn) measured in the same manner and the above weight average molecular weight (Mw).
[0059] <GPC measurement device> Column: "TOSO GMHHR-H(S)HT" manufactured by Tosoh Corporation Detector: RI detection for liquid chromatogram, "WATERS 150C" manufactured by Waters Corporation
[0060] <Measurement conditions> Solvent: 1,2,4-trichlorobenzene Measurement temperature: 145°C Flow rate: 1.0 mL / min Sample concentration: 5 mg / 10 mL Injection volume: 300 μL Calibration curve: Universal Calibration Analysis program: HT-GPC (Ver. 1.0)
[0061] The content of the carboxyl group-containing resin in the ion-permeable membrane is preferably 1% by mass or more and 30% by mass or less, more preferably 1% by mass or more and 25% by mass or less, and even more preferably 1% by mass or more and 20% by mass or less. When the content of the carboxyl group-containing resin is 1% by mass or more, cracks and distortions during fabrication are less likely to occur, and the yield and handling properties are improved. When the content is 30% by mass or less, the ion recovery efficiency can be further improved.
[0062] (Carboxy-free resin) The ion-permeable membrane of this embodiment preferably further contains a resin that does not contain a carboxy group. By including a resin that does not contain a carboxy group in the ion-permeable membrane, the viscosity of the resin decreases during mixing, and the resin and the solid electrolyte are well mixed, thereby increasing adhesion, and as a result, water permeability can be further reduced. The resin that does not contain a carboxy group may exist in the form of a mixture of a resin that contains a carboxy group and a separate resin, or may exist in the form of a copolymer, but the former is preferred.
[0063] As the resin not containing a carboxy group, from the viewpoint of binding ability with the resin containing a carboxy group and making it more impervious to water permeation, an olefin resin is preferred, and for example, polyethylene, polypropylene, etc. can be used. The olefin resin may be a homopolymer or a copolymer.
[0064] The copolymer may be a copolymer of ethylene or propylene with a monomer copolymerizable therewith. Examples of monomers copolymerizable with ethylene or propylene include α-olefins, styrenes, dienes, and cyclic compounds. The α-olefin is preferably an α-olefin having 4 to 30 carbon atoms. Specific examples include linear olefins such as 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, and 1-decene, and branched olefins such as isobutene and 4-methyl-1-pentene. Examples of styrenes include styrene, 4-methylstyrene, and 4-dimethylaminostyrene. Examples of dienes include 1,3-butadiene, 1,5-hexadiene, 1,4-hexadiene, and 1,7-octadiene. Examples of cyclic compounds include norbornene and cyclopentene. These copolymerizable monomers may be used alone or in combination of two or more. A copolymer of ethylene and propylene may also be used. The copolymer may be an alternating copolymer, a random copolymer, or a block copolymer.
[0065] As the resin not containing a carboxy group, polypropylene is preferred, and propylene homopolymer is more preferred, from the viewpoint of further improving the binding strength with the resin containing a carboxy group and from the viewpoint of making it more difficult for water to permeate. From the viewpoint of further improving flexibility, the polypropylene has a melting endotherm (ΔH-D) obtained from a melting endotherm curve obtained by using a differential scanning calorimeter (DSC) to hold a sample at -10 ° C. for 5 minutes under a nitrogen atmosphere and then raising the temperature at 10 ° C. / min. It is preferably 0 J / g or more and 80 J / g or less, more preferably 5 J / g or more and 70 J / g or less, even more preferably 10 J / g or more and 60 J / g or less, and even more preferably 15 J / g or more and 50 J / g or less. Improved flexibility makes it less likely to crack or warp during production, improving yield and handleability.
[0066] The melting endotherm (ΔH-D) is calculated by determining the area enclosed by a line including the highest peak observed on the high-temperature side of the melting endotherm curve obtained by DSC measurement and the line connecting the low-temperature side point where there is no change in heat quantity and the high-temperature side point where there is no change in heat quantity as a baseline. The melting endotherm (ΔH-D) can be controlled by appropriately adjusting the monomer concentration and reaction pressure.
[0067] From the viewpoint of further enhancing flexibility, the polypropylene preferably does not exhibit a melting point (Tm-D), which is defined as the peak top observed on the highest temperature side of a melting endothermic curve obtained by holding a sample at −10° C. for 5 minutes under a nitrogen atmosphere and then raising the temperature at a rate of 10° C. / min using a differential scanning calorimeter (DSC), or is preferably not observed or is 0° C. or higher and 120° C. or lower. If a melting point is observed, it is more preferably 20° C. or higher and 110° C. or lower, and even more preferably 30° C. or higher and 100° C. or lower. The melting point can be controlled by appropriately adjusting the monomer concentration and reaction pressure. Improved flexibility makes the polypropylene less susceptible to cracking and distortion during production, improving yield and handleability.
[0068] From the viewpoint of further enhancing the binding property with the carboxyl group-containing resin, the softening point of the polypropylene is preferably 90° C. or higher and 165° C. or lower, more preferably 100° C. or higher and 160° C. or lower, and even more preferably 115° C. or higher and 150° C. or lower. The softening point can be measured by the Ring and Ball method in accordance with JAI7-1991.
[0069] From the viewpoint of reducing the viscosity during mixing, the polypropylene preferably has a weight average molecular weight (Mw) of 20,000 to 500,000, more preferably 25,000 to 300,000, and even more preferably 30,000 to 150,000.
[0070] From the viewpoint of further enhancing the binding strength with the carboxyl group-containing resin, the molecular weight distribution (Mw / Mn) of the carboxyl group-containing resin is preferably 1.5 to 4.0, more preferably 1.6 to 3.0, even more preferably 1.7 to 2.8, and still more preferably 1.8 to 2.5.
[0071] Commercially available polypropylenes can be used. Specific examples include "S400," "S410," "S401," "S600," and "S901" under the "L-MODU" (registered trademark) brand (manufactured by Idemitsu Kosan Co., Ltd.). Commercially available amorphous poly-α-olefins include "REXtac" manufactured by REXtac, LLC, "Vestoplast" manufactured by Evonik, and "Eastoflex" and "Aerafin" manufactured by Eastman (all trade names). Commercially available propylene-based elastomers include "Tafmer XM," "Tafmer PN," and "Tafmer SN" manufactured by Mitsui Chemicals, Inc.; "Tafthren" manufactured by Sumitomo Chemical Co., Ltd.; "Prime TPO" manufactured by Prime Polymer Co., Ltd.; "Versify" manufactured by The Dow Chemical Company; "Vistamaxx" and "Linxar" manufactured by ExxonMobil Corporation; "Licocene" manufactured by Clariant; and "Adflex" manufactured by Basell (all of which are trade names).
[0072] Polypropylene can be obtained by polymerizing monomers in the presence of a polymerization catalyst such as a Ziegler-Natta catalyst or a metallocene catalyst. Among them, polypropylene obtained using a metallocene catalyst is preferred. A metallocene catalyst is a type of homogeneous catalyst, and the resulting polymer is a uniform polymer with a narrow molecular weight distribution and a narrow composition distribution.
[0073] When the ion-permeable membrane of this embodiment contains a resin that does not contain a carboxy group, the content of the resin that does not contain a carboxy group is preferably 3% by mass or more and 30% by mass or less, more preferably 5% by mass or more and 25% by mass or less, and even more preferably 6% by mass or more and 20% by mass or less. When the content of the resin that does not contain a carboxy group is 3% by mass or more, the binding strength with the resin that contains a carboxy group can be further improved, and when it is 30% by mass or less, the lithium selectivity can be further improved.
[0074] From the viewpoint of binding properties, the mass ratio of the resin not containing a carboxy group to the resin containing a carboxy group [resin not containing a carboxy group / resin containing a carboxy group] is preferably 40 / 60 to 95 / 5, more preferably 45 / 55 to 95 / 5, and even more preferably 50 / 50 to 90 / 10.
[0075] (Production of ion-permeable membrane) The ion-permeable membrane of the present embodiment can be obtained, for example, by adding the above-mentioned alkaline solid electrolyte, a resin containing a carboxy group, and an optional resin not containing a carboxy group to a solvent, stirring and mixing to prepare a slurry, applying the obtained slurry to a release film to form a coating film, and then drying the coating film.
[0076] Examples of the agitator used for the above stirring and mixing include a ball mill, a sand mill, a bead mill, an ultrasonic disperser, a homogenizer, a planetary mixer, and a filmix.
[0077] The solvent is not particularly limited, and examples thereof include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, aromatic hydrocarbon solvents, etc. Examples of aliphatic hydrocarbons include hexane, pentane, 2-ethylhexane, heptane, octane, decane, undecane, dodecane, tridecane, etc. Examples of alicyclic hydrocarbons include cyclohexane, methylcyclohexane, etc. Examples of aromatic hydrocarbon solvents include benzene, toluene, xylene, mesitylene, ethylbenzene, tert-butylbenzene, trifluoromethylbenzene, nitrobenzene, etc.
[0078] From the viewpoint of the coatability of the slurry, the solid content concentration of the slurry is preferably 60.0 to 99.0 mass %, more preferably 65.0 to 95.0 mass %, and even more preferably 70.0 to 90.0 mass %, based on the total amount (100 mass %) of the slurry. In this specification, the term "solid content concentration" refers to the content (concentration) of components other than the solvent.
[0079] The method for applying the slurry onto the release film is not particularly limited, and examples thereof include a doctor blade method, a dipping method, a reverse roll method, a direct roll method, a gravure method, an extrusion method, brush coating, etc. The amount of the slurry to be applied is not particularly limited, and can be appropriately set depending on the desired thickness of the ion-permeable membrane, etc.
[0080] The method for drying the slurry on the release film is not particularly limited, and examples include drying with warm air, hot air, or low-humidity air, vacuum drying, and drying by irradiation with (far) infrared rays, electron beams, etc. Drying conditions can be set appropriately, and the drying temperature is preferably 50 to 200°C, more preferably 60 to 150°C. Drying time is not particularly limited, and is usually carried out in the range of 5 minutes to 20 hours, preferably 5 minutes to 18 hours. Drying may be carried out in one stage or two stages.
[0081] The dried ion-permeable membrane may be compacted by pressing, which may be performed using a die press, a roll press, a calendar press, or the like, but is not limited thereto.
[0082] [Ion recovery device] The ion recovery device of this embodiment is a device equipped with an ion-permeable membrane that includes an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g. That is, the ion recovery device of this embodiment is a device equipped with the ion-permeable membrane of this embodiment described above. The ion-permeable membrane of this embodiment that is equipped in the recovery device of this embodiment is as described above.
[0083] A schematic diagram of a preferred example of the configuration of an ion recovery device using the ion permeable membrane of this embodiment is shown in Figure 1. The ion recovery device 10 can recover lithium ions in a recovery solution, which is an aqueous solution, by transferring lithium ions from a treatment solution containing lithium ions extracted from, for example, a treatment component of a lithium secondary battery. This ion recovery device 10 recovers target metal ions, metal ion derivatives, or metals from target metal ions 4 and non-target ions 5 contained in a treatment solution 2.
[0084] The ion recovery device 10 has an ion permeable membrane 1 that selectively allows metal ions to be recovered into a treatment tank 11. The ion permeable membrane 1 is installed in the treatment tank 11 so as to separate the treatment liquid from the recovery liquid, with the treatment liquid on one main surface and the recovery liquid on the other main surface. The ion recovery device 10 preferably has an electrode, which allows the metal ions to be recovered to selectively permeate the ion permeable membrane 1 and move to the recovery liquid 3 (shown as A) more quickly and efficiently, thereby recovering the target ions. The ion recovery device 10 may further have a storage tank for storing the recovery liquid and a recovery tank for recovering lithium ions from the recovery liquid, as needed, and a liquid transfer pipe connecting them.
[0085] [Method for producing lithium hydroxide] The method for producing lithium hydroxide of this embodiment involves recovering lithium hydroxide from a lithium ion-containing liquid using an ion-permeable membrane that includes an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g. That is, the method for producing lithium hydroxide of this embodiment uses the ion-permeable membrane of this embodiment described above. The ion-permeable membrane of this embodiment used in the method for producing lithium hydroxide of this embodiment is as described above.
[0086] In the method for producing lithium hydroxide of this embodiment, the production of lithium hydroxide is not particularly limited as long as the ion-permeable membrane of this embodiment is used, but can be carried out, for example, by recovering lithium ions from a lithium ion-containing liquid and obtaining lithium hydroxide from the recovered liquid from which the lithium ions have been recovered. Here, when recovering lithium ions from a lithium ion-containing liquid, this can be done using an electrochemical device equipped with the ion-permeable membrane of this embodiment, and as such an electrochemical device, for example, the above-mentioned ion recovery device of this embodiment can be used.
[0087] There are no particular limitations on the method for obtaining lithium hydroxide from a recovered solution obtained by recovering lithium ions from a lithium ion-containing solution, but examples include evaporation by heating and drying. Other examples include a method for separating lithium hydroxide from the recovered solution. More specifically, preferred examples include crystallization methods such as cooling crystallization and evaporation crystallization. According to the crystallization method, lithium hydroxide can be obtained without the need for a dehydration step such as heating and concentration, thereby reducing the energy consumption required for the dehydration step and enabling more efficient production of high-purity lithium hydroxide.
[0088] [Method for producing lithium-containing material] The method for producing a lithium-containing material of this embodiment is a method for recovering lithium hydroxide from a lithium ion-containing solution using an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g, and for producing a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide. That is, the method for producing a lithium-containing material of this embodiment uses the lithium hydroxide obtained by the method for producing lithium hydroxide of this embodiment described above. The method for producing lithium hydroxide employed in the method for producing a lithium-containing material of this embodiment is as described above.
[0089] (Lithium-containing material: lithium sulfide) The lithium-containing material obtained by the method for producing a lithium-containing material of the present embodiment is a material containing lithium selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material. Lithium sulfide can be produced, for example, by reacting lithium hydroxide with hydrogen sulfide.
[0090] (Lithium-Containing Material: Sulfide Solid Electrolyte) A sulfide solid electrolyte can be produced by using, for example, lithium hydroxide or lithium sulfide obtained using lithium hydroxide as a solid electrolyte raw material, and reacting raw material-containing materials including other solid electrolyte raw materials by mixing, etc. Other solid electrolyte raw materials that can be used in combination with lithium hydroxide or lithium sulfide obtained using lithium hydroxide are not particularly limited as long as they can produce a sulfide solid electrolyte, and preferred examples include substances containing at least one atom selected from a lithium atom, a phosphorus atom, and a sulfur atom, and more preferred examples include substances containing at least one atom selected from a lithium atom, a phosphorus atom, a sulfur atom, and a halogen atom.
[0091] Such a solid electrolyte raw material is, for example, diphosphorus trisulfide (P 2 S 3 ), diphosphorus pentasulfide (P 2 S 5Representative examples of suitable raw materials include raw materials containing at least two types of atoms selected from the above-mentioned atoms, such as phosphorus element, sulfur element, and the like. Among these, lithium sulfide and diphosphorus trisulfide (P 2 S 3 ), diphosphorus pentasulfide (P 2 S 5 Among phosphorus sulfides, phosphorus pentasulfide (P 2 S 5 ) is preferred.
[0092] The raw material may further contain a halogen atom, and examples of the raw material include substances containing a halogen atom. For example, lithium halides such as lithium fluoride, lithium chloride, lithium bromide, and lithium iodide; fluorine (F 2 ), chlorine (Cl 2 ), bromine (Br 2 ), iodine (I 2 ) and other simple halogen atoms are typically preferred.
[0093] The above solid electrolyte raw materials may be blended in a blending ratio that matches the composition of the sulfide solid electrolyte having the desired crystal structure. Examples of the blending ratio of lithium sulfide and other solid electrolyte raw materials contained in the raw material inclusions include those described in International Publication No. 2020 / 105737 (see paragraphs
[0024] to
[0028] ). Furthermore, the solid electrolyte raw material may be appropriately selected from the materials exemplified in International Publication No. 2020 / 105737 (see paragraphs
[0020] to
[0022] ).
[0094] The reaction of the raw material components can be carried out, for example, by mixing (i) or by heat treatment in a pressure vessel or by heat treatment in a solvent under reflux (ii). First, the process (i) will be described.
[0095] (Regarding Production Method (i)) The method for mixing the solid electrolyte raw materials containing lithium sulfide is not particularly limited as long as it can mix the solid electrolyte raw materials. For example, the method can be performed using a pulverizer, a mixer, an agitator, or the like. When a pulverizer is used, the raw materials are pulverized, but mixing also occurs at the same time. Mixing of the raw materials can also occur when a mixer or an agitator is used. Therefore, it can be said that the sulfide solid electrolyte obtained by the production method for a lithium-containing material of this embodiment can be preferably produced by stirring, mixing, pulverizing, or a combination of any of these processes, using two or more raw materials selected from substances containing at least one atom of a lithium atom, a sulfur atom, a phosphorus atom, and a halogen atom.
[0096] The equipment used to mix the raw material components, such as a grinder, mixer, or agitator, is not particularly limited and any commonly available equipment can be used.
[0097] In the above mixing, a solvent can be added to the above raw materials and mixed. As the solvent, various solvents widely called organic solvents can be used. As the solvent, a wide range of solvents that have been conventionally used in the production of solid electrolytes can be used, and examples thereof include hydrocarbon solvents such as aliphatic hydrocarbon solvents, alicyclic hydrocarbon solvents, and aromatic hydrocarbon solvents.
[0098] In addition to the hydrocarbon solvents, examples of the solvent include solvents containing heteroatoms such as nitrogen, oxygen, sulfur, and halogen atoms, and the like, in addition to carbon and hydrogen atoms. Such solvents have the property of readily forming complexes (which can also be referred to as "electrolyte precursors" because a sulfide solid electrolyte can be obtained by removing the complexing agent from the "complex") with raw materials containing lithium, phosphorus, sulfur, oxygen, and halogen atoms (hereinafter, such solvents are also referred to as "complexing agents"). These solvents facilitate the retention of halogen atoms within the structure of the sulfide solid electrolyte, making them useful in terms of achieving higher ionic conductivity. Furthermore, the use of a complexing agent is useful because it allows the solid electrolyte raw materials to be mixed using equipment such as a mixer or agitator, i.e., without the need for a pulverizer, to proceed with the reaction of the solid electrolyte raw materials.
[0099] As the complexing agent and the hydrocarbon solvent that can be employed, for example, the complexing agents and hydrocarbon solvents exemplified in International Publication No. 2020 / 105737 can be used. Among these solvents containing heteroatoms, it is preferable to use a solvent containing a nitrogen atom as the complexing agent, more preferably an amine solvent having an amino group, and even more preferably a diamine solvent having two amino groups.
[0100] (Drying) When producing a sulfide solid electrolyte and mixing is performed using a solvent, the method may include drying the fluid (usually a slurry) obtained by mixing. When a complexing agent is used as a solvent, the sulfide solid electrolyte is obtained by removing the complexing agent from a complex containing the complexing agent. When a complexing agent and a solvent are used in combination, the complexing agent is removed from a complex containing the complexing agent and the solvent is removed. When a solvent other than a complexing agent is used, the solvent is removed to obtain the sulfide solid electrolyte.
[0101] The drying method can be any method that can remove the solvent, and can be selected from solid-liquid separation, drying by heating, drying under reduced pressure (vacuum drying), and a combination of these. When a complexing agent is used as the solvent and the complexing agent is removed from the complex (electrolyte precursor), drying by heating is preferred as the drying method, and it is preferably performed using a dryer such as a flow-type heater. This is because the complexing agent can be quickly removed from the complex (electrolyte precursor), and the generation of impurities can be more efficiently suppressed, resulting in a high-quality sulfide solid electrolyte. Preferred flow-type heaters include flash dryers, spray dryers, and fluidized dryers using a medium, with flash dryers being particularly preferred.
[0102] (Heating) When producing a sulfide solid electrolyte, heating may be further included. If an amorphous sulfide solid electrolyte (glass component) is obtained by the above mixing, a crystalline sulfide solid electrolyte can be obtained by heating. Also, if a crystalline sulfide solid electrolyte is obtained, a crystalline sulfide solid electrolyte with improved crystallinity can be obtained. In either case, heating can make the resulting sulfide solid electrolyte a crystalline sulfide solid electrolyte, and can improve ionic conductivity. In other words, the heating can be considered an operation performed for crystallization.
[0103] When a complexing agent is used as a solvent during mixing, a complex containing the complexing agent is formed. However, the complexing agent can be removed from the complex by heating without performing the drying process, and a sulfide solid electrolyte can be obtained. Depending on the heating conditions, the sulfide solid electrolyte can be made amorphous or crystalline.
[0104] (Regarding Production Method (ii)) Production method (ii) is a production method in which the reaction of raw material contents is carried out by heat-treating in a solvent while heat-treating or refluxing in a pressure-resistant vessel. When the heat treatment using a pressure-resistant vessel is adopted as the production method for the sulfide solid electrolyte of this embodiment, it is a suitable method for producing a sulfide solid electrolyte having an argyrodite-type crystal structure, which will be described later. Details of the heat treatment in a solvent while heat-treating or refluxing in a pressure-resistant vessel in production method (ii) are explained in JP 2020-095953 A and the like, and these may be followed.
[0105] By the above-mentioned production methods (i) and (ii), an amorphous sulfide solid electrolyte and a crystalline sulfide solid electrolyte can be obtained as the sulfide solid electrolyte. The amorphous sulfide solid electrolyte contains lithium atoms, sulfur atoms, and phosphorus atoms, and preferably further contains halogen atoms. Representative examples include Li, 2 S-P 2 S 5 , and Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P 2 S 5 - LiBr, Li 2 S-P 2 S 5 -LiI-LiBr, etc., solid electrolytes composed of lithium sulfide, phosphorus sulfide, and lithium halide; and solid electrolytes further containing other atoms such as oxygen atoms and silicon atoms, for example, Li 2 S-P 2 S 5 -Li 2 O-LiI, Li 2 S-SiS 2 -P 2 S 5 In order to obtain higher ionic conductivity, a solid electrolyte such as Li 2 S-P 2 S 5 - LiI, Li 2 S-P 2 S 5 -LiCl, Li 2 S-P2 S 5 - LiBr, Li 2 S-P 2 S 5 A solid electrolyte composed of lithium sulfide, phosphorus sulfide, and lithium halide, such as LiI-LiBr, is preferred. The types of atoms constituting the amorphous sulfide solid electrolyte can be confirmed, for example, by an ICP emission spectrometer.
[0106] In the amorphous sulfide solid electrolyte, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.6, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.05 to 0.5, and even more preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.08 to 0.4. Further, when bromine and iodine are used in combination as halogen atoms, the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, bromine, and iodine is preferably 1.0 to 1.8: 1.0 to 2.0: 0.1 to 0.8: 0.01 to 0.3: 0.01 to 0.3, more preferably 1.1 to 1.7: 1.2 to 1.8: 0.2 to 0.6: 0.02 to 0.25: 0.02 to 0.25, more preferably 1.2 to 1.6: 1.3 to 1.7: 0.25 to 0.5: 0.03 to 0.2: 0.03 to 0.2, and even more preferably 1.35 to 1.45: 1.4 to 1.7: 0.3 to 0.45: 0.04 to 0.18: 0.04 to 0.18. By setting the compounding ratio (molar ratio) of lithium atoms, sulfur atoms, phosphorus atoms, and halogen atoms within the above range, it becomes easier to obtain a solid electrolyte with higher ionic conductivity having a thiolisiconregion II type crystal structure, an argyrodite type crystal structure, or the like, which will be described later.
[0107] The crystalline sulfide solid electrolyte may be a so-called glass ceramic obtained by heating an amorphous sulfide solid electrolyte to a crystallization temperature or higher, and its crystalline structure may be Li 3 P.S. 4 Crystal structure, Li 4 P 2 S 6 Crystal structure, Li 7 P.S. 6 Crystal structure, Li 7 P3 S 11 Examples of such a crystal structure include a crystal structure having peaks at 2θ=approximately 20.2° and 23.6° (for example, JP 2013-16423 A).
[0108] Preferred examples of the crystal structure include a thiosilicon region II crystal structure and an argyrodite crystal structure. Details of these crystal structures are described, for example, in International Publication Nos. 2024 / 010078 and 2024 / 010079. The atomic composition ratio of the crystalline sulfide solid electrolyte is determined by a composition formula corresponding to the various crystal structures, and is preferably within the range of the atomic composition ratio of the amorphous sulfide solid electrolyte. When the atomic composition ratio is within this range, it is easier to form a thiosilicon region II crystal structure or an argyrodite crystal structure, among the above crystal structures.
[0109] The sulfide solid electrolyte thus obtained can be used as it is in the solid electrolyte layer (separator layer) of a lithium ion battery, or can be mixed with an electrode active material described later to form an electrode mixture for use in a positive electrode or a negative electrode.
[0110] (Lithium-containing material: electrode active material) The electrode active material can be produced by using, for example, lithium hydroxide or lithium sulfide obtained using lithium hydroxide as a raw material, wet mixing or dry mixing with other raw materials such as hydroxide salts, halide salts, carbonates, and oxides containing atoms such as cobalt, nickel, manganese, iron, and phosphorus, followed by firing.
[0111] Examples of the electrode active material obtained in this way include LMO (lithium manganese oxide), LCO (lithium cobalt oxide), NMC (lithium nickel manganese cobalt oxide), NCA (lithium nickel cobalt aluminate), LNCO (lithium nickel cobalt oxide), and olivine-type compounds (LiMeNPO 4, Me=Fe, Co, Ni, Mn), LFP (lithium iron phosphate), NM (lithium nickel manganese oxide), etc. These lithium-containing transition metal composite oxides are also called oxide positive electrode active materials, and are mainly used as positive electrode active materials.
[0112] The electrode active material obtained by the method for producing a lithium-containing material of this embodiment can be used as an electrode mixture by mixing it with a sulfide solid electrolyte also obtained by the method for producing a lithium-containing material of this embodiment.
[0113] When preparing an electrode mixture, the blending ratio (mass ratio) of the electrode active material to the sulfide solid electrolyte is preferably 99.5:0.5 to 40:60, more preferably 99:1 to 50:50, and even more preferably 98:2 to 60:40, in consideration of improving battery performance and production efficiency.
[0114] Furthermore, when an electrode mixture is used, components that can be used other than the electrode active material and sulfide solid electrolyte include conductive materials that are carbon-based materials such as artificial graphite, graphite carbon fiber, resin-baked carbon, pyrolytic vapor-grown carbon, coke, mesocarbon microbeads, furfuryl alcohol resin-baked carbon, polyacene, pitch-based carbon fiber, vapor-grown carbon fiber, natural graphite, and non-graphitizable carbon; fluorine-based polymers such as polytetrafluoroethylene and polyvinylidene fluoride, thermoplastic elastomers such as butylene rubber and styrene-butadiene rubber, and various resin binders such as acrylic resin, acrylic polyol resin, polyvinyl acetal resin, polyvinyl butyral resin, and silicone resin; and the like.
[0115] When a conductive material is contained, the content of the conductive material in the electrode mixture is not particularly limited, but in consideration of improving battery performance and manufacturing efficiency, it is preferably 0.5% by mass or more, more preferably 1% by mass or more, and even more preferably 1.5% by mass or more, with the upper limit being preferably 10% by mass or less, preferably 8% by mass or less, and even more preferably 5% by mass or less. Furthermore, when a binder is contained, the content of the binder in the electrode mixture is not particularly limited, but in consideration of improving battery performance and manufacturing efficiency, it is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, with the upper limit being preferably 20% by mass or less, preferably 15% by mass or less, and even more preferably 10% by mass or less.
[0116] The electrode active material can be used as an electrode mixture, and the electrode mixture can be used as a positive electrode layer or a negative electrode layer of a lithium ion battery.
[0117] [Method for manufacturing lithium-ion battery] The method for manufacturing a lithium-ion battery of this embodiment includes recovering lithium hydroxide from a lithium-ion-containing solution using an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g, obtaining a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide, and using a material selected from the lithium-containing materials. That is, the method for manufacturing a lithium-ion battery of this embodiment uses the lithium-containing material obtained by the method for manufacturing a lithium-containing material of this embodiment. The method for manufacturing a lithium-containing material employed in the method for manufacturing a lithium-ion battery of this embodiment is as described above.
[0118] The material selected from the lithium-containing materials used in the manufacturing method of this embodiment is a material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material, and preferably a sulfide solid electrolyte and an electrode active material are used. As already described, the sulfide solid electrolyte is preferably used as is in the solid electrolyte layer of a lithium ion battery, and is also preferably mixed with an electrode active material to form an electrode composite for the positive or negative electrode of a lithium ion battery. Furthermore, the electrode active material is preferably mixed with a solid electrolyte such as a sulfide solid electrolyte to form an electrode composite for the positive or negative electrode of a lithium ion battery.
[0119] The lithium ion battery obtained by the manufacturing method of this embodiment preferably includes, for example, a positive electrode layer, a negative electrode layer, an electrolyte layer, and a current collector. The positive electrode layer and the negative electrode layer preferably use the above-mentioned electrode mixture, and the electrolyte layer preferably uses the sulfide solid electrolyte obtained by the manufacturing method of the lithium-containing material of this embodiment. Furthermore, a known current collector may be used. For example, a layer in which a material that reacts with the above-mentioned solid electrolyte, such as Au, Pt, Al, Ti, or Cu, is coated with Au or the like can be used.
[0120] The present invention will now be described in detail with reference to examples, but the present invention is not limited to these examples in any way.
[0121] Details of the raw material compounds used in the synthesis examples and working examples are as follows: Polypropylene (1): L-MODU (registered trademark) S400, manufactured by Idemitsu Kosan Co., Ltd., melting endotherm (ΔH-D) = 36 J / g, melting point (Tm-D) = 80°C, weight average molecular weight (Mw) = 45,000, molecular weight distribution (Mw / Mn) = 2.0, polypropylene obtained using a metallocene catalyst Polypropylene (2): L-MODU (registered trademark) S901, manufactured by Idemitsu Kosan Co., Ltd., melting endotherm (ΔH-D) = 40 J / g, melting point (Tm-D) = 80°C, weight average molecular weight (Mw) = 130,000, molecular weight distribution (Mw / Mn) = 2.0, polypropylene obtained using a metallocene catalyst LLTO (1): A mixture of "TP-02N (fired at 1300°C in air), manufactured by Toho Titanium Co., Ltd., average particle size: 20 μm" and "TP-02F, manufactured by Toho Titanium Co., Ltd., average particle size: 1 μm" in a mass ratio of TP-02N:TP-02F = 80:20
[0122] The melting endotherm (ΔH-D), melting point (Tm-D), weight average molecular weight (Mw), and molecular weight distribution of polypropylenes (1) and (2) were measured by the following methods.
[0123] [DSC Measurement] Using a differential scanning calorimeter (manufactured by Perkin-Elmer, "DSC-7"), 10 mg of a sample was held at -10°C for 5 minutes under a nitrogen atmosphere, and then heated at a rate of 10°C / min to obtain a melting endothermic curve, from which the melting endothermic amount (ΔH-D) was determined. The melting point (Tm-D) was determined from the peak top of the peak observed on the highest temperature side of the obtained melting endothermic curve. The melting endothermic amount (ΔH-D) was calculated by determining the area enclosed by the line connecting the low-temperature point where there is no change in calorific value and the high-temperature point where there is no change in calorific value as the baseline, and the line including the peak of the melting endothermic curve obtained by DSC measurement using a differential scanning calorimeter (manufactured by Perkin-Elmer, "DSC-7"), and the baseline.
[0124] [Measurement of Weight Average Molecular Weight (Mw) and Molecular Weight Distribution (Mw / Mn)] The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by gel permeation chromatography (GPC) to determine the molecular weight distribution (Mw / Mn). The following apparatus and conditions were used for the measurement, and the polystyrene-equivalent weight average molecular weight and number average molecular weight were obtained. The molecular weight distribution (Mw / Mn) was a value calculated from the weight average molecular weight (Mw) and number average molecular weight (Mn). <GPC measurement device> Column: "TOSO GMHHR-H(S)HT" manufactured by Tosoh Corporation Detector: RI detection for liquid chromatography, "WATERS 150C" manufactured by Waters Corporation <Measurement conditions> Solvent: 1,2,4-trichlorobenzene Measurement temperature: 145°C Flow rate: 1.0 mL / min Sample concentration: 5 mg / 10 mL Injection volume: 300 μL Calibration curve: Universal Calibration Analysis program: HT-GPC (Ver. 1.0)
[0125] (Acid-Modified Polypropylene) Acid-modified polypropylenes (1) to (3) were prepared by varying the mixing ratio of polypropylene (1) and maleic anhydride. Acid-modified polypropylene (1) had an acid value of 15.3 mg KOH / g and an acid-modified amount of 1.8 mass%, acid-modified polypropylene (2) had an acid value of 42.7 mg KOH / g and an acid-modified amount of 6.3 mass%, and acid-modified polypropylene (3) had an acid value of 71.2 mg KOH / g and an acid-modified amount of 10.9 mass%. The acid value and acid-modified amount of each were measured by the following method.
[0126] [Acid Value] The acid values of the acid-modified polypropylenes (1) to (3) were measured in accordance with JIS K0070: 1992. The acid values of the ion-permeable membranes obtained in the examples were calculated from the acid value and content of the acid-modified polypropylene contained in the ion-permeable membrane.
[0127] [Amount of Acid Modification] A mixture of polypropylene and maleic anhydride before modification was pressed using a 0.1 mm spacer, and then IR was measured to determine the characteristic carbonyl (1600 to 1900 cm -1A calibration curve was created from the absorption amount of the acid-modified polypropylene and the amount of maleic anhydride added, and IR measurement of the acid-modified polypropylene press plate was performed to measure the amount of acid modification. IR measurement equipment: "Nicolet 8700" manufactured by Thermo Fisher Scientific
[0128] Example 1 To a rotation-revolution mixer (THINKY MIXER AR310, manufactured by THINKY CORPORATION), 80 parts by mass of "TP-02N, manufactured by Toho Titanium Co., Ltd., average particle size: 20 μm" and 20 parts by mass of "TP-02F, manufactured by Toho Titanium Co., Ltd., average particle size: 1 μm" were added as alkaline solid electrolytes, and the mixture was stirred and mixed at 2000 rpm for 1 minute, allowed to cool at room temperature (25° C.) for 1 minute, and then further stirred and mixed at 2000 rpm for 1 minute to obtain LLTO (1) (a mixture of TP-02N and TP-02F). Next, 50 parts by mass of polypropylene (2) as a resin not containing a carboxyl group and 50 parts by mass of acid-modified polypropylene (1) as a resin containing a carboxyl group were added to a rotation / revolution mixer (Thinky Corporation) containing 40 parts by mass of xylene as a solvent, and the mixture was stirred and mixed at 2000 rpm for 10 minutes. The LLTO (1) was then added so that the mass ratio of the resin in the slurry was LLTO (1):resin = 80:20. The mixture was stirred and mixed at 2000 rpm for 5 minutes, and then ice-cooled for 5 minutes. This procedure was repeated twice to prepare a slurry with a solids concentration of 75% by mass. The slurry was vacuum degassed at 45°C for 3 minutes, and half of the slurry was applied to a PTFE film using a tabletop coater to form a coating film with a thickness of 500 μm. The coating was dried at 50°C for 20 minutes using a hot plate, and the remaining slurry was applied to the coating to a film thickness of 500 μm. The coating was then dried at 50°C for 20 minutes and further vacuum dried at 120°C for 6 hours to obtain an ion-permeable membrane. The resulting ion-permeable membrane was subjected to a water leakage test (solution isolation test) and a Li selectivity test, which will be described later. The results are shown in Tables 1 and 2.
[0129] (Examples 2 to 5 and Comparative Examples 1 and 2) Ion-permeable membranes were obtained in the same manner as in Example 1, except that the components and blending amounts were changed as shown in Table 1. The produced ion-permeable membranes were subjected to a water leakage test (solution isolation test) described below. The results are shown in Table 1. FIG. 3 shows an SEM image (magnification: 1000x) of a cross section of the ion-permeable membrane produced in Example 4, and FIG. 4 shows an SEM image (magnification: 1000x) of a cross section of the ion-permeable membrane produced in Comparative Example 2.
[0130] [Water Leakage Test (Solution Isolation Test)] An ion permeable membrane cut to a size of 25 mm x 25 mm was set in the acrylic ion recovery device shown in Figure 1, with 15 mL of a 1.0 mol / L aqueous potassium hydroxide solution as the treatment liquid set on one side and 15 mL of ion-exchanged water as the recovery liquid set on the other side. After leaving the device at room temperature (25°C) for 24 hours, 0.5 mL of the recovery liquid was sampled at 0 hours, 2 hours, and 4 hours, and the potassium ion concentration was measured using ion chromatography (IC-8100, manufactured by Tosoh Corporation).
[0131] [Li Selectivity Test] An ion-permeable membrane cut to a size of 25 mm x 25 mm was set in an acrylic electrodeposition apparatus shown in Figure 2, and an electrode (IrO 2 50 mL of a 1.0 mol / L aqueous potassium hydroxide solution was placed in the tank on the electrode (Sns) side as a treatment liquid, and 100 mL of ion-exchanged water was placed in the tank on the electrode (Sns) side as a recovery liquid, and a voltage of 5 V was applied for 24 hours. After 1 hour, the electrode (IrO 2 50 mL of a 1.0 mol / L aqueous solution of lithium hydroxide was added as a treatment liquid to the tank on the side of the reactor. 0.5 mL of the recovery liquid was sampled after 0 minutes, 30 minutes, and 60 minutes, and the potassium ion concentration and lithium ion concentration were measured by ion chromatography (IC-8100, manufactured by Tosoh Corporation).
[0132]
[0133]
[0134] As shown in Table 1, the ion-permeable membranes of Examples 1 to 5 all exhibited high quality as permeable membranes, preventing water from passing through. Furthermore, as shown in Table 2, the ion-permeable membrane of Example 1 was confirmed to have lithium selectivity. Furthermore, in the ion-permeable membrane of Example 4 shown in FIG. 3, it can be seen that both the solid electrolyte with an average particle size of 20 μm and the solid electrolyte with an average particle size of 1 μm are in close contact with the resin. In contrast, the ion-permeable membrane of Comparative Example 2 shown in FIG. 4 shows many gaps around the solid electrolyte with an average particle size of 20 μm, and the solid electrolyte with an average particle size of 1 μm is seen floating between the resin and the solid electrolyte. This suggests that the adhesion between the solid electrolyte and the resin is low, resulting in water permeation through the ion-permeable membrane.
[0135] 1. Ion-permeable membrane 2. Treatment liquid 3. Recovery liquid 4. Metal ions to be recovered 5. Ions other than those to be recovered 10. Ion recovery device 11. Treatment tank 12. Electrode (IrO 2 ) 13. Electrodes (Sns) 14. Power Supply A. Transport of ions for collection purposes
Claims
1. An ion-permeable membrane comprising an alkaline solid electrolyte and a resin containing a carboxyl group, the acid value of which is greater than 0 mgKOH / g.
2. The ion-permeable membrane according to claim 1, wherein the solid electrolyte exhibiting alkalinity is an oxide solid electrolyte.
3. The ion-permeable membrane according to claim 1 or 2, wherein the resin containing a carboxy group is a resin selected from a block copolymer containing a monomer having a carboxy group and an acid-modified resin graft-modified with a compound having a carboxy group.
4. The ion-permeable membrane according to claim 3, wherein the block copolymer is a block copolymer of a monomer having a carboxy group and an olefin monomer.
5. The ion-permeable membrane according to claim 3, wherein the main chain of the acid-modified resin is formed from an olefin monomer.
6. The ion-permeable membrane according to claim 3 or 4, wherein the monomer having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof.
7. The ion-permeable membrane according to claim 3 or 5, wherein the compound having a carboxy group is a compound selected from unsaturated carboxylic acids and derivatives thereof.
8. The ion-permeable membrane according to claim 6 or 7, wherein the monomer having a carboxy group and the compound having a carboxy group are compounds selected from the group consisting of acrylic acid, methacrylic acid, maleic acid and derivatives thereof.
9. The ion-permeable membrane according to any one of claims 1 to 7, further comprising a resin containing no carboxyl groups.
10. The ion-permeable membrane according to claim 9, wherein the resin not containing a carboxy group is an olefin resin.
11. The ion-permeable membrane according to any one of claims 1 to 10, wherein the content of the resin containing a carboxy group is from 1% by mass to 30% by mass.
12. The ion-permeable membrane according to any one of claims 1 to 11, wherein the acid value is greater than 0 mgKOH / g and not greater than 20 mgKOH / g.
13. The ion-permeable membrane according to any one of claims 1 to 12, which allows lithium ions to permeate.
14. The ion-permeable membrane according to any one of claims 1 to 13, which is used for recovering lithium ions.
15. A lithium recovery device comprising an ion-permeable membrane that includes an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mgKOH / g.
16. A method for producing lithium hydroxide, comprising recovering lithium hydroxide from a lithium ion-containing liquid using an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mg KOH / g.
17. A method for producing a lithium-containing material, comprising recovering lithium hydroxide from a lithium ion-containing liquid using an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mg KOH / g, and using the lithium hydroxide to produce a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material.
18. A method for producing a lithium ion battery, comprising: recovering lithium hydroxide from a lithium ion-containing liquid using an ion-permeable membrane that contains an alkaline solid electrolyte and a resin containing a carboxy group and has an acid value of more than 0 mg KOH / g; obtaining a lithium-containing material selected from lithium sulfide, a sulfide solid electrolyte, and an electrode active material using the lithium hydroxide; and using a material selected from the lithium-containing materials.
Citation Information
Patent Citations
Apparatus and method for collecting lithium
JP2022075618A
Method for producing lithium hydroxide
JP2022075619A
Aqueous electrolyte bipolar secondary battery, battery pack, vehicle and stationary power source
JP2022143728A