Metal powder for molding, and molded article

The use of a metal powder with a controlled composition and solidification molding process addresses the challenge of achieving high strength and machinability in age-hardening austenitic tool steel by refining the microstructure, resulting in improved mechanical properties and reduced defects in shaped objects.

WO2024203945A1PCT designated stage expired Publication Date: 2024-10-03PROTERIAL LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011470
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-22
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Age-hardening austenitic tool steel manufactured through traditional melting processes struggles to achieve both high strength and machinability due to the difficulty in refining carbides and MnS, which leads to coarse structures and reduced mechanical properties.

Method used

A metal powder with a controlled composition (C: 0.40-0.70%, Si: 1.40% or less, Mn: 5.00-15.00%, Ni: 2.00-10.00%, Cr: 7.00-14.00%, Mo: 0.80-5.00%, V: 1.00-2.50%, Cu: 0.60-4.00%, Al: 0.60-4.00%, S: 0.0500-0.1500%) is used for shaping, employing solidification and molding processes to refine the microstructure and produce shaped objects with improved strength and machinability.

Benefits of technology

The refined microstructure results in shaped objects with enhanced high strength, machinability, and reduced internal defects, such as cracks and decreased toughness, while maintaining optimal hardness and wear resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024011470_03102024_PF_FP_ABST
    Figure JP2024011470_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided are: a metal powder for molding from which a molded article having both high strength and machinability can be produced; and a molded article molded by using the same. Provided are: a metal powder for molding which contains 0.40-0.70 mass% of C, at most 1.40 mass% of Si, 5.00-15.00 mass% of Mn, 2.00-10.00 mass% of Ni, 7.00-14.00 mass% of Cr, 0.80-5.00 mass% of Mo, 1.00-2.50 mass% of V, 0.60-4.00 mass% of Cu, 0.60-4.00 mass% of Al, and 0.0500-0.1500 mass% of S, with the balance being Fe and inevitable impurities; and a molded article molded by using the same.
Need to check novelty before this filing date? Find Prior Art

Description

Metal powders for molding and molded objects

[0001] The present invention relates to a metal powder for molding and a molded object using the same.

[0002] Due to their non-magnetic and high hardness characteristics, age-hardenable austenitic tool steels are utilized in plastic-magnet forming dies and jigs that require non-magnetic properties. An example of an age-hardenable austenitic tool steel is proposed in Patent Document 1. Machinability is also required for age-hardenable austenitic tool steels, and Patent Document 1 optimizes high strength and machinability through chemical composition design. Such age-hardenable austenitic tool steels are manufactured by a so-called ingot manufacturing process, in which a steel material is obtained by hot plastic working of a steel ingot obtained by an ingot-making process such as conventional casting or remelting casting.

[0003] Japanese Unexamined Patent Publication No. 63-203753

[0004] The age-hardenable austenitic tool steel of Patent Document 1 has a chemical composition that allows the formation of carbides and MnS in order to obtain high strength and machinability. When this steel is produced by an ingot process, the carbides and MnS crystallized from the molten metal during normal casting or remelting casting are deformed by hot plastic working to form the steel into the final shape. These carbides and MnS remain in the subsequent heat treatment process, making it difficult to refine them in the steel state.

[0005] An object of the present invention is to provide a metal powder for molding that can be used to produce a molded product that has both high strength and machinability, and a molded product made using the same.

[0006] The inventors have investigated methods for controlling the structure of age-hardenable austenitic tool steels, and have discovered that by adopting a process of solidifying and molding metal powder for molding, it is possible to obtain molded products that combine high strength and machinability by refining the structure morphology, thereby arriving at the present invention.

[0007] The present invention provides a metal powder for molding containing, by mass%, C = 0.40 to 0.70%, Si = 1.40% or less, Mn = 5.00 to 15.00%, Ni = 2.00 to 10.00%, Cr = 7.00 to 14.00%, Mo = 0.80 to 5.00%, V = 1.00 to 2.50%, Cu = 0.60 to 4.00%, Al = 0.60 to 4.00%, S = 0.0500 to 0.1500%, and the balance being Fe and unavoidable impurities.

[0008] The present invention also provides a shaped article containing, by mass%, C = 0.40 to 0.70%, Si = 1.40% or less, Mn = 5.00 to 15.00%, Ni = 2.00 to 10.00%, Cr = 7.00 to 14.00%, Mo = 0.80 to 5.00%, V = 1.00 to 2.50%, Cu = 0.60 to 4.00%, Al = 0.60 to 4.00%, S = 0.0500 to 0.1500%, and the balance being Fe and unavoidable impurities, wherein the maximum length of MnS is less than 1 μm in a cross section parallel to the stacking direction.

[0009] The present invention provides a useful technique for producing shaped articles that combine high strength and machinability by refining the microstructure of age-hardenable austenitic tool steel.

[0010] FIG. 1 shows an elemental mapping image of S when a cross section of a metal powder for molding according to an example of the present invention is analyzed by EPMA (electron probe microanalyzer). FIG. 2 shows an elemental mapping image of S when a cross section parallel to the stacking direction of a molded object according to an example of the present invention is analyzed by EPMA. FIG. 3 shows an elemental mapping image of S when a cross section of a steel material according to a comparative example is analyzed by EPMA. FIG. 4 shows an optical microscope photograph of a molded object according to an example of the present invention after solution treatment. FIG. 5 shows an optical microscope photograph of a steel material according to a comparative example after solution treatment.

[0011] The metal powder for molding (hereinafter also referred to simply as "metal powder") and molded article of the present invention contain, by mass%, C = 0.40 to 0.70%, Si = 1.40% or less, Mn = 5.00 to 15.00%, Ni = 2.00 to 10.00%, Cr = 7.00 to 14.00%, Mo = 0.80 to 5.00%, V = 1.00 to 2.50%, Cu = 0.60 to 4.00%, Al = 0.60 to 4.00%, S = 0.0500 to 0.1500%, and the balance consisting of Fe and unavoidable impurities.

[0012] C = 0.40 to 0.70 mass% Carbon (C) is an austenite-forming element, along with Mn and Ni, and is necessary for maintaining the structure of the shaped article of the present invention as austenite. Furthermore, C is also necessary for improving hardness and wear resistance by forming carbides together with Cr, Mo, and V. From the viewpoint of obtaining hardness of the shaped article, the C content is set to 0.40 mass% or more. For the same reasons as above, the C content is preferably set to 0.45 mass% or more, more preferably 0.50 mass% or more. On the other hand, if the C content is too high, coarse carbides may be formed, potentially resulting in a decrease in toughness. Therefore, the C content is set to 0.70 mass% or less. For the same reasons as above, the C content is preferably set to 0.65 mass% or less, more preferably 0.60 mass% or less.

[0013] Si = 1.40 mass% or less Si is an element necessary for improving oxidation resistance. However, if the Si content is too high, segregation may occur inside the shaped object, resulting in a decrease in strength. Therefore, the Si content is set to 1.40 mass% or less. For the same reasons as above, in the present invention, the Si content is preferably set to 1.00 mass% or less, and more preferably 0.60 mass% or less. Note that, in consideration of industrial mass productivity, the Si content is preferably set to 0.1 mass ppm or more, and more preferably 0.5 mass ppm or more.

[0014] Mn = 5.00 to 15.00% by mass Mn, together with C and Ni, is an austenite-forming element and is necessary for maintaining the structure of the shaped article of the present invention as austenite. If the Mn content is too low, ferrite may be generated, which may reduce the maximum hardness in aging treatment. Therefore, the Mn content is set to 5.00% by mass or more. For the same reasons as above, in the present invention, the Mn content is preferably set to 5.50% by mass or more, and more preferably 6.00% by mass or more. On the other hand, if the Mn content is too high, there is a risk of reducing machinability. Therefore, the Mn content is set to 15.00% by mass or less. For the same reasons as above, in the present invention, the Mn content is preferably set to 10.00% by mass or less.

[0015] Ni = 2.00 to 10.00 mass% Ni, together with C and Mn, is an element necessary for maintaining the structure of the shaped article of the present invention as austenite. Furthermore, Ni is an element necessary for forming fine intermetallic compounds with Al during aging treatment after solution treatment, thereby obtaining the hardness required for age-hardenable austenitic tool steel. For this reason, the Ni content is set to 2.00 mass% or more. For the same reasons as above, in the present invention, the Ni content is preferably set to 3.00 mass% or more, and more preferably 5.00 mass% or more. On the other hand, if the Ni content is too high, non-metallic inclusions may increase in the structure of the shaped article, potentially reducing toughness. For this reason, the Ni content is set to 10.00 mass% or less. For the same reasons as above, in the present invention, the Ni content is preferably set to 9.00 mass% or less, and more preferably 8.00 mass% or less.

[0016] Cr = 7.00 to 14.00 mass% Cr is an element necessary for improving the corrosion resistance and oxidation resistance of steel materials and for forming carbides to suppress coarsening of crystal grains during solution treatment. Therefore, the Cr content is set to 7.00 mass% or more. In the present invention, for the same reasons as above, the Cr content is preferably set to 8.00 mass% or more, more preferably 9.00 mass% or more. On the other hand, if the Cr content is too high, it may promote the formation of coarse carbides, resulting in a decrease in toughness. Furthermore, if the Cr content is too high, it may result in a decrease in high-temperature strength and the formation of ferrite. Therefore, the Cr content is set to 14.00 mass% or less. In the present invention, for the same reasons as above, the Cr content is preferably set to 13.00 mass% or less, more preferably 12.00 mass% or less.

[0017] Mo = 0.80 to 5.00 mass% Mo is an element necessary for forming carbides to suppress coarsening of crystal grains during solution treatment and precipitating fine carbides during aging treatment, thereby achieving high aging hardness and high-temperature strength. Therefore, the Mo content is set to 0.80 mass% or more. For the same reasons as above, the Mo content is preferably set to 1.30 mass% or more, more preferably 1.80 mass% or more. On the other hand, if the Mo content is too high, coarse carbides may be formed, potentially reducing toughness. Therefore, the Mo content is set to 5.00 mass% or less. For the same reasons as above, the Mo content is preferably set to 4.00 mass% or less, more preferably 3.00 mass% or less.

[0018] V = 1.00 to 2.50 mass% V (vanadium) is an element necessary for forming carbides and suppressing coarsening of crystal grains during solution treatment. Furthermore, V is an element necessary for precipitating fine carbides during aging treatment and obtaining particularly high aging hardness. Therefore, the V content is set to 1.00 mass% or more. In the present invention, for the same reasons as above, the V content is preferably set to 1.20 mass%. On the other hand, if the V content is too high, coarse carbides may be formed, which may reduce toughness. Therefore, the V content is set to 2.50 mass% or less. In the present invention, for the same reasons as above, the V content is preferably set to 2.00 mass% or less, and more preferably 1.50 mass% or less.

[0019] Cu = 0.60 to 4.00 mass% Cu is an element necessary for forming fine intermetallic compounds with Fe during aging treatment after solution treatment, thereby obtaining the hardness required for age-hardenable austenitic tool steel. Cu is also an element that has the effect of improving corrosion resistance. For this reason, the Cu content is set to 0.60 mass% or more. For the same reasons as above, in the present invention, the Cu content is preferably set to 0.80 mass% or more, and more preferably 1.00 mass% or more. On the other hand, if the Cu content is too high, there is a concern that the hardness may decrease. For this reason, the Cu content is set to 4.00 mass% or less. For the same reasons as above, in the present invention, the Cu content is preferably set to 3.50 mass% or less, and more preferably 3.00 mass% or less.

[0020] Al = 0.60 to 4.00 mass% Al is an element necessary for forming fine intermetallic compounds with Ni during aging treatment after solution treatment and for obtaining the hardness required for age-hardenable austenitic tool steel. Therefore, the Al content is set to 0.60 mass% or more. In the present invention, for the same reasons as above, it is preferable that the Al content be 0.90 mass% or more. On the other hand, if the Al content is too high, it will lead to the formation of ferrite. Therefore, the Al content is set to 4.00 mass% or less. In the present invention, for the same reasons as above, it is preferable that the Al content be 3.00 mass% or less, and more preferably 2.00 mass% or less.

[0021] S = 0.0500 to 0.1500 mass% S (sulfur) is an element necessary for forming sulfides with Mn and improving machinability. If the S content is too high, the toughness of the resulting shaped product will decrease. For this reason, the S content is set to 0.0500 to 0.1500 mass%. In the present invention, for the same reasons as above, it is preferable that the S content be set to 0.0500 to 0.1000 mass%.

[0022] The metal powder of the present invention can be produced by, for example, gas atomization, water atomization, disk atomization, plasma atomization, rotating electrode atomization, etc. Among these production methods, gas atomization allows scrap metal, raw metal raw materials, etc. to be used as the melting raw material, and enables production at a lower cost than plasma atomization, rotating electrode atomization, etc., which require the preparation of raw materials with the desired composition and shape in advance. For this reason, gas atomization is preferred as a production method for obtaining the metal powder of the present invention.

[0023] The metal powder of the present invention preferably has a 50% particle size (hereinafter referred to as "D50") of the cumulative particle size distribution on a volume basis of 10 to 250 μm. By making the metal powder of the present invention have a D50 of 250 μm or less, the powder can be easily melted, and the formation of defects in the molded product can be suppressed. Furthermore, by making the metal powder of the present invention have a D50 of 10 μm or more, the powder is less susceptible to the effects of atmospheric moisture and the like, and good fluidity can be ensured. The cumulative particle size distribution of the metal powder of the present invention is expressed as a cumulative volume particle size distribution, and the D50 is expressed as a measurement value obtained by the laser diffraction scattering method specified in JIS Z 8825.

[0024] The metal powder of the present invention is preferably adjusted in particle size by mesh sieving or airflow classification, depending on the molding method. For example, metal powders used in powder bed fusion using a laser beam are melted by the laser beam, which serves as the heat source, but coarse powder that is difficult to melt must be removed to minimize the area of ​​thermal influence. Furthermore, highly adhesive fine powder must also be removed to obtain optimal fluidity for ensuring the laying of the metal powder. Therefore, when applying the metal powder of the present invention to powder bed fusion, it is preferable to adjust the D50 to the range of 10 to 53 μm.

[0025] In the shaped product of the present invention, the maximum length of MnS included in the observation field in a cross section parallel to the stacking direction is less than 1 μm. Here, a cross section parallel to the stacking direction refers to, for example, a cross section parallel to the filling direction of the metal powder in the case of a shaped product obtained by pressure sintering, or a cross section parallel to the direction in which multiple solidified layers are formed in the case of a shaped product obtained by additive manufacturing. Figure 2 shows an example of an elemental mapping image of S obtained by EPMA analysis of MnS observed in a cross section parallel to the stacking direction of the shaped product. In Figure 2, the dot-like inclusions shown in gray in the matrix shown in black are MnS. By limiting the maximum length of MnS to less than 1 μm in the shaped product of the present invention, internal defects such as cracks can be reduced, and deterioration of mechanical properties such as ductility and toughness can be suppressed.

[0026] To measure whether the maximum length of MnS is less than 1 μm, the S concentration distribution in a cross section parallel to the stacking direction can be analyzed by, for example, EPMA. First, a cross section parallel to the stacking direction of the shaped object is taken from an arbitrary position on the shaped object. Then, an arbitrary region can be analyzed with EPMA at, for example, 5000x magnification to obtain the S distribution.

[0027] Furthermore, from the viewpoint of improving machinability, the shaped article of the present invention has an S content of 0.0500 to 0.1500 mass %. In the present invention, for the same reasons as above, it is preferable that the S content be 0.0500 to 0.1000 mass %.

[0028] The shaped object of the present invention can be obtained, for example, by a powder sintering method. Specifically, it can be obtained by pressure sintering the above-mentioned metal powder. The pressure sintering can be performed using, for example, a HIP method, a hot pressing method, or an electric current sintering method. The shaped object of the present invention can also be obtained by an additive manufacturing method in which a plurality of solidified layers are formed by repeating a process of spreading metal powder in layers and a process of successively melting and solidifying the spread metal powder using a scanning heat source to form solidified layers. Here, for example, a laser or an electron beam can be used as the scanning heat source. It is preferable to make the diameter of the scanning heat source larger than the average diameter of the metal powder, since this allows for uniform melting of the metal powder aggregates.

[0029] If the laser power is too high, the molten metal will be deep during laser irradiation, making it more likely that strong segregation will form during solidification. However, if the laser power is too low, the metal powder will not be melted sufficiently, and many voids will form in the solidified object due to the gaps between the metal powder. For this reason, it is preferable to set the laser power to 50 to 350 W.

[0030] If the laser scanning speed is too fast, the metal powder will not receive enough heat, making it difficult to melt the powder for shaping, and many voids will likely form in the solidified component. On the other hand, if the laser scanning speed is too slow, the molten metal will become deeper during laser irradiation, making it more likely to form segregation. Furthermore, if the laser scanning speed is too slow, excessive heat will be applied to the metal powder, causing the molten metal to flow more actively, which will entrain gas and lead to the inclusion of air bubbles in the solidified component. For this reason, the scanning speed is preferably set to 200 to 2000 mm / sec.

[0031] If the scanning pitch is too large, it becomes difficult to melt the entire surface of the spread metal powder during laser irradiation, which may result in the formation of voids inside the solidified component. The scanning pitch refers to the distance between the scanning beams. If the scanning pitch is too small, the molten metal portion becomes deep during laser irradiation, making it more likely to form segregation. Therefore, the scanning pitch is preferably set to 0.02 to 0.20 mm.

[0032] If the layer thickness per scan is too large, heat is not easily transferred to the entire spread metal powder during laser irradiation, making it difficult to achieve the melting required for shaping. The "layer thickness per scan" refers to the "thickness of each metal powder layer" laid out when shaping each layer. If the layer thickness per scan is too small, the number of layers required to achieve the desired size of the shaped object increases, lengthening the time required for shaping. For this reason, it is preferable that the layer thickness per scan be 10 to 200 μm.

[0033] The shaped article of the present invention is preferably further subjected to a heat treatment process including a solution treatment and an aging treatment. The age-hardenable austenitic tool steel is used as a product after undergoing solution treatment and aging treatment on the member. The solution treatment brings into solution the intermetallic compounds precipitated by the heat during shaping, and further recrystallizes the anisotropic structure formed by pressure sintering or the anisotropic structure formed by the molten pool or solidification structure formed by additive manufacturing, thereby forming a structure with equiaxed crystal grains and suppressing the anisotropy of the mechanical properties.

[0034] The solution treatment temperature is preferably 1100°C or higher, and more preferably 1150°C or higher. Increasing the solution treatment temperature improves the effect of eliminating segregation formed during shaping. However, if the solution treatment temperature is too high, the main body of the shaped object will melt, resulting in a decrease in the strength and toughness of the shaped object. Therefore, the solution treatment temperature is preferably 1250°C or lower, and more preferably 1200°C or lower. The solution treatment time (the time maintained at the solution treatment temperature) is preferably 10 minutes or longer, and more preferably 15 minutes or longer. Increasing the solution treatment time improves the effect of eliminating segregation formed during shaping. However, if the solution treatment time is too long, the prior austenite grain size will coarsen. Therefore, the solution treatment time is preferably 120 minutes or shorter, and more preferably 90 minutes or shorter.

[0035] Then, by subjecting this member to aging treatment, various intermetallic compounds are precipitated in the structure, and the hardness can be adjusted to, for example, 20 to 50 HRC, thereby achieving superior high strength and high toughness. The aging treatment temperature is preferably 400°C or higher, more preferably 450°C or higher, and even more preferably 500°C or higher. The aging treatment temperature is particularly preferably 550°C or higher. Increasing the aging treatment temperature further enhances the effect of improving strength. However, if the aging treatment temperature is too high, the intermetallic compounds become coarse, and sufficient strength commensurate with the amount of intermetallic compounds precipitated cannot be obtained. For this reason, the aging treatment temperature is preferably 900°C or lower, more preferably 800°C or lower. The aging treatment time (maintenance time at the aging treatment temperature) is preferably 30 minutes or higher, more preferably 60 minutes or higher. Increasing the aging treatment time increases the amount of intermetallic compounds formed. However, if the aging treatment time is too long, the intermetallic compounds become coarse and the strength decreases, so the aging treatment time is preferably 600 minutes or less, and more preferably 400 minutes or less.

[0036] Each metal raw material was prepared so as to have the composition of Sample No. 1-1 in Table 1, then charged into a high-frequency induction melting furnace and melted. The molten metal was pulverized with argon gas to obtain an atomized powder. The obtained atomized powder was subjected to mesh sieving and air classification to adjust the powder particle size, resulting in a metal powder serving as an example of the present invention with a D50 of 28.8 μm. A shaped object was then produced using this metal powder. The shaped object was produced using an EOS-M290 manufactured by EOS under the shaping conditions shown in Table 2. The results of the component analysis of the obtained shaped object serving as an example of the present invention are shown in Table 1 as Sample No. 1-2. As a comparative example, a steel material was prepared by subjecting a molten metal having the composition of Sample No. 2 in Table 1 to an ingot casting process and hot plastic working.

[0037] The state of existence of carbides and MnS was confirmed. Figure 1 shows elemental mapping images of S when a cross section of a metal powder according to an example of the present invention, a shaped product according to an example of the present invention, and a steel material according to a comparative example were analyzed by EPMA. In the comparative steel material obtained by the so-called ingot manufacturing method, as shown in the gray areas in Figure 3, many MnS particles with a maximum length exceeding 10 μm were observed. In contrast, in the metal powder according to an example of the present invention and a shaped product manufactured using the same, as shown in the gray areas in Figures 1 and 2, all MnS particles had a maximum length of less than 1 μm, confirming that they were finely dispersed.

[0038] The shaped article obtained above was subjected to solution treatment at 1180°C for 1 hour, and the microstructure was confirmed. Fig. 4 shows the optical micrographs of the shaped article of the present invention, and Fig. 5 shows the optical micrographs of the steel material of the comparative example. In the steel material of the comparative example, numerous MnS particles with a maximum length exceeding 10 μm were observed. In contrast, in the shaped article of the present invention, all MnS particles had a maximum length of less than 1 μm, confirming that they were finely dispersed. Such fine dispersion of MnS and carbides is expected to have a favorable effect on the mechanical properties and machinability required for tool steel.

[0039]

[0040]

Claims

1. Metal powder for manufacturing containing, by mass, C = 0.40-0.70%, Si = 1.40% or less, Mn = 5.00-15.00%, Ni = 2.00-10.00%, Cr = 7.00-14.00%, Mo = 0.80-5.00%, V = 1.00-2.50%, Cu = 0.60-4.00%, Al = 0.60-4.00%, S = 0.0500-0.1500%, and the remainder being Fe and unavoidable impurities.

2. A shaped object containing, by mass, C = 0.40-0.70%, Si = 1.40% or less, Mn = 5.00-15.00%, Ni = 2.00-10.00%, Cr = 7.00-14.00%, Mo = 0.80-5.00%, V = 1.00-2.50%, Cu = 0.60-4.00%, Al = 0.60-4.00%, S = 0.0500-0.1500%, with the remainder being Fe and unavoidable impurities, and in which the maximum length of MnS in a cross section parallel to the lamination direction is less than 1 μm.

Citation Information

Patent Citations

  • Age hardening type austenitic tool steel

    JP1993302149A

  • Metal powder and sintered compact

    JP2010222661A

  • Powder for lamination molding, lamination molded object and manufacturing method of lamination molded object

    JP2020172674A