Chlorosulfonated polyolefin latex

The chlorosulfonated polyolefin latex composition, featuring specific surfactants, allows for solvent-free dip molding of gloves with enhanced strength and chemical resistance, addressing the limitations of existing methods by eliminating sodium alginate and organic solvents.

WO2024203978A1PCT designated stage expired Publication Date: 2024-10-03SUMITOMO SEIKA CHEM CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011541
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-05
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing methods for manufacturing chlorosulfonated polyolefin rubber gloves require organic solvents and often use sodium alginate, which limits control over viscosity and desirability of solvent-free processes.

Method used

A chlorosulfonated polyolefin latex composition comprising chlorosulfonated polyolefin, surfactants with anionic and nonionic moieties, and an aqueous dispersion medium, specifically using surfactants like amino acid, alkylaryl sulfonic acid, and sulfosuccinic acid surfactants to facilitate dip molding without sodium alginate.

Benefits of technology

Enables the production of dip-molded articles with excellent strength and chemical resistance, particularly suitable for gloves, without the need for organic solvents and sodium alginate, promoting environmental protection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided is a means for producing a dip molded body comprising a chlorosulfonated polyolefin, without using sodium alginate or the like. More specifically provided is a chlorosulfonated polyolefin latex containing: (A) a chlorosulfonated polyolefin; (B) a surfactant having an anionic portion and a nonionic portion, wherein the nonionic portion contains a polyoxyalkylene chain, and the anionic portion contains a carboxylate, a sulfonate, a carbonate ester salt, a sulfate ester salt, or a phosphate ester salt; (C) at least one surfactant selected from the group consisting of an amino acid surfactant, an alkyl aryl sulfonic acid surfactant, an alkyl sulfate surfactant, and a sulfosuccinic acid surfactant; and (D) an aqueous dispersion medium.
Need to check novelty before this filing date? Find Prior Art

Description

Chlorosulfonated polyolefin latex

[0001] The present disclosure relates to a chlorosulfonated polyolefin latex, more particularly to a chlorosulfonated polyolefin latex for dip molding, and also to a dip-molded article produced using the chlorosulfonated polyolefin latex.

[0002] Rubber gloves are widely used, for example, for housework, in various industrial applications such as the food industry and electronic component manufacturing industry, and in medical applications. A widely used method for manufacturing rubber gloves is the coagulation dipping method using latex. For example, Patent Document 1 discloses a method for manufacturing gloves, in which a hand mold corresponding to the three-dimensional shape of the glove is prepared, the surface of the mold is treated with a coagulant such as a calcium nitrate aqueous solution, the treated hand mold is then immersed in a dip solution containing nitrile rubber latex, and then pulled out, allowing rubber particles to adhere to the surface of the mold, followed by drying and crosslinking.

[0003] Chlorosulfonated polyolefins have excellent resistance to strong acids and strong alkalis, and are therefore used as materials for protective gloves for use in processes involving the heavy use of hazardous chemicals, such as plating processes, semiconductor manufacturing processes, and dyeing processes. Generally, chlorosulfonated polyolefin rubber gloves are manufactured by immersing a glove former in an organic solvent solution of rubber, followed by drying and vulcanization (see, for example, Patent Document 2). However, from the viewpoint of environmental protection, a method for manufacturing gloves using rubber latex, which does not require the use of organic solvents, is desired.

[0004] As a method for manufacturing a glove using chlorosulfonated polyolefin latex, for example, Patent Document 3 discloses a method for manufacturing a dip-molded product by dipping a mold to which calcium ions are attached into chlorosulfonated polyethylene latex blended with sodium alginate, κ-carrageenan and pectin.

[0005] International Publication No. 2015 / 146974 Japanese Patent Application Laid-Open No. 05-230702 Japanese Patent No. 7033242 International Publication No. 2012 / 141020

[0006] However, sodium alginate and the like also have a thickening effect, and from the viewpoint of freely controlling the viscosity, it is preferable to be able to produce a dip-molded article using a latex that does not contain sodium alginate, etc. One aspect of the present disclosure aims to provide a method for producing a dip-molded article made of a chlorosulfonated polyolefin without using sodium alginate, etc., a latex that can be used in the method, and a dip-molded article made of a chlorosulfonated polyolefin that does not need to contain sodium alginate, etc.

[0007] The present disclosure includes, for example, the subject matter described in the following items. <Item 1> A chlorosulfonated polyolefin latex containing: (A) a chlorosulfonated polyolefin; (B) a surfactant having an anionic moiety and a nonionic moiety, wherein the nonionic moiety contains a polyoxyalkylene chain and the anionic moiety contains a carboxylate, sulfonate, carbonate ester salt, sulfate ester salt, or phosphate ester salt; (C) at least one surfactant selected from the group consisting of amino acid surfactants, alkylarylsulfonic acid surfactants, alkyl sulfate surfactants, and sulfosuccinic acid surfactants; and (D) an aqueous dispersion medium. <Item 2> The latex according to Item 1, which is used for dip molding. <Item 3-1> The latex according to Item 1 or 2, wherein the content of (C) is 1 to 10 parts by mass per 100 parts by mass of (A). <Item 3-2> The latex according to Item 1, 2, or 3-1, wherein the content of (B) is 0.3 to 12 parts by mass per 100 parts by mass of (A). <Item 4-1> The latex according to any one of Items 1 to 2, 3-1 and 3-2, wherein the amino acid surfactant is at least one amino acid surfactant selected from the group consisting of glutamic acid surfactants, alanine surfactants, sarcosine surfactants, glycine surfactants, aspartic acid surfactants and taurine surfactants; the alkylarylsulfonic acid surfactant is an alkylarylsulfonic acid surfactant in which the alkyl group in the active agent is a linear or branched C8 to C18 alkyl and the aryl group is a phenylene group or a naphthylene group; the alkyl sulfate surfactant is at least one alkyl sulfate surfactant selected from the group consisting of alkyl sulfate surfactants and polyoxyalkylenesulfonic acid surfactants; and the sulfosuccinic acid surfactant is at least one sulfosuccinic acid surfactant selected from the group consisting of monoalkylsulfosuccinic acid surfactants, dialkylsulfosuccinic acid surfactants and alkylalkenylsulfosuccinic acid surfactants.<Item 4-2> The latex according to any one of Items 1 to 2, 3-1 and 3-2, wherein the surfactant (C) is at least one selected from the group consisting of alanine-based surfactants, taurine-based surfactants, alkylbenzenesulfonic acid-based surfactants, alkyl sulfate-based surfactants, polyoxyalkylenesulfonate-based surfactants, monoalkyl sulfosuccinate-based surfactants, dialkyl sulfosuccinate-based surfactants and alkylalkenyl sulfosuccinate-based surfactants. <Item 4-3> The latex according to any one of Items 1 to 2, 3-1 and 3-2, wherein the surfactant (C) is at least one surfactant selected from the group consisting of N-C8 to C18 aliphatic acyl methyl alanine salts and N-C8 to C18 aliphatic acyl methyl taurine salts, linear alkylbenzenesulfonates having a C8 to C18 alkyl group, alkyl sulfates wherein the alkyl group is a linear or branched C8 to C18 alkyl group and polyoxyalkylenesulfonates, and mono-C8 to C18 alkyl sulfosuccinates, di-C8 to C18 alkyl sulfosuccinates and C8 to C18 alkyl C2 to C6 alkenyl sulfosuccinates. <Item 5> The latex according to any one of Items 1 to 2, 3-1 to 3-2 and 4-1 to 4-3, wherein the chlorosulfonated polyolefin is chlorosulfonated polyethylene. <Item 6-1> The surfactant (B) is represented by the formula (I): R. 1 -O-(CH 2 CHR 2 -O) n -R 3 (I) (wherein, R 1 is R 1a - or R 1a -R 1b represents a group represented by -, and R 1a - represents an alkyl group having 6 to 20 carbon atoms, and -R 1b - represents a phenylene group, n represents an integer of 2 to 40, and R 2 are the same or different and represent hydrogen or a methyl group; R 3 Ha-SO 3The latex according to any one of items 1 to 2, 3-1 to 3-2, 4-1 to 4-3, and 5, wherein the latex is a compound represented by the formula: (I) -COOM or -COOM, where M represents an alkali metal. <Item 7> A dip-formed article obtained by dip-forming the latex according to any one of items 1 to 2, 3-1 to 3-2, 4-1 to 4-3, and 5 to 6, using a polyvalent metal salt as a coagulant. <Item 8> The dip-formed article according to item 7, which has a thickness of 0.1 mm or more. <Item 9> The dip-formed article according to item 7, which is a glove. Item 10: A method for producing a dip-molded article, comprising the steps of: preparing a dip-molding composition by mixing (C) at least one surfactant selected from the group consisting of amino acid-based surfactants, alkylarylsulfonic acid-based surfactants, alkylsulfonic acid-based surfactants, and sulfosuccinic acid-based surfactants with a latex containing (A) a chlorosulfonated polyolefin, (B) a surfactant having an anionic moiety and a nonionic moiety, the nonionic moiety containing a polyoxyalkylene chain and the anionic moiety containing a carboxylate, sulfonate, carbonate ester salt, sulfate ester salt, or phosphate ester salt, and (D) an aqueous dispersion medium; adhering a coagulant to the surface of a mold having a desired shape; and immersing the mold with the coagulant adhered thereto in the dip-molding composition to form a coagulated coating. Item 11: A method for producing a dip-molded article according to Item 10, further comprising the steps of removing the mold from the dip-molding composition, washing the coagulated coating, and heating the coagulated coating.

[0008] The present invention provides a method for producing a dip-molded article made of a chlorosulfonated polyolefin without using sodium alginate, a latex that can be used in the method, and a dip-molded article made of a chlorosulfonated polyolefin that does not need to contain sodium alginate, which allows for the convenient production of a dip-molded article that is preferably excellent in strength and chemical resistance.

[0009] Each embodiment included in the present disclosure will be described in more detail below. The present disclosure preferably includes, but is not limited to, a chlorosulfonated polyolefin latex, its uses, and a production method thereof, and the like. The present disclosure includes all that is disclosed in the present specification and that can be recognized by a person skilled in the art.

[0010] The chlorosulfonated polyolefin latex encompassed by the present disclosure contains (A) a chlorosulfonated polyolefin, (B) a surfactant having an anionic moiety and a nonionic moiety, the nonionic moiety containing a polyoxyalkylene chain and the anionic moiety containing a carboxylate, sulfonate, carbonate ester salt, sulfate ester salt, or phosphate ester salt, (C) at least one surfactant selected from the group consisting of amino acid surfactants, alkylarylsulfonate surfactants, alkyl sulfate surfactants, and sulfosuccinate surfactants, and (D) an aqueous dispersion medium. The chlorosulfonated polyolefin latex encompassed by the present disclosure may be referred to as the "latex of the present disclosure." These components may also be referred to as components (A) to (D), respectively.

[0011] The chlorosulfonated polyolefin (component (A)) is obtained by chlorinating and chlorosulfonating a polyolefin. Examples of polyolefins include polymers or copolymers of α-olefins, and copolymers of α-olefins and other polymerizable components.

[0012] Examples of α-olefins include ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, etc. Other polymerizable components include chain dienes such as isoprene, 1,3-butadiene, 1,4-hexadiene, 1,6-octadiene, and 2-methyl-1,5-hexadiene; cyclic dienes such as 1,4-cyclohexadiene, dicyclopentadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, 5-methylene-2-norbornene, 5-isopropylidene-2-norbornene, and 6-chloromethyl-5-isopropenyl-2-norbornene; and vinyl compounds such as vinyl acetate, vinyl chloride, acrylonitrile, styrene, methyl acrylate, and methyl methacrylate.

[0013] The chlorosulfonated polyolefin is preferably a chlorosulfonated α-olefin polymer. In the chlorosulfonated α-olefin polymer, one α-olefin may be used alone or two or more α-olefins may be used. When two or more α-olefins are used, one of them is preferably ethylene.

[0014] More specific examples of chlorosulfonated polyolefins include chlorosulfonated polyethylene, chlorosulfonated ethylene-α-olefin copolymers, and chlorosulfonated α-olefin polymers. Note that the "α-olefin" in chlorosulfonated ethylene-α-olefin copolymers and chlorosulfonated α-olefin polymers refers to α-olefins other than ethylene. A preferred example of the α-olefin other than ethylene here is propylene. That is, a preferred example of the chlorosulfonated ethylene-α-olefin copolymer is chlorosulfonated ethylene-propylene copolymer, and a preferred example of the chlorosulfonated α-olefin polymer is chlorosulfonated propylene polymer.

[0015] The chlorosulfonated polyolefins may be used alone or in combination of two or more.

[0016] The sulfur content in the chlorosulfonated polyolefin is preferably 0.5% by mass or more, more preferably 0.8% by mass or more, preferably 2.0% by mass or less, more preferably 1.5% by mass or less, and preferably 0.5 to 2.0% by mass, more preferably 0.8 to 1.5% by mass.

[0017] The chlorine content in the chlorosulfonated polyolefin of the present disclosure is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more. It is also preferably 50% by mass or less, more preferably 40% by mass or less. It is also preferably 10 to 50% by mass, more preferably 20 to 40% by mass.

[0018] The sulfur content and chlorine content of the chlorosulfonated polyolefin are the contents of sulfur atoms and chlorine atoms contained in the chlorosulfonated polyolefin, respectively, and can be measured by the oxygen flask combustion method.

[0019] Methods for chlorinating and chlorosulfonating polyolefins include a solution method in which the polyolefin is dissolved in an organic solvent and the reaction is carried out in a homogeneous system, a suspension method in which the polyolefin is suspended in a solvent and the reaction is carried out, a melt method in which the polyolefin is reacted in a molten state, and a gas-phase method in which the polyolefin is suspended in a gas phase and the reaction is carried out. Among these, the solution method is preferred from the viewpoint of uniform chlorination and chlorosulfonation. Examples of the chlorinating agent and chlorosulfonating agent that can be used include a combination of chlorine gas and sulfurous acid gas, a combination of chlorine gas and sulfuryl chloride, and sulfuryl chloride alone. The chlorosulfonation reaction can be carried out by using a chlorinating agent, a chlorosulfonating agent, a radical generator, and, if necessary, a co-catalyst such as pyridine.

[0020] Commercially available chlorosulfonated polyolefins may be used, examples of which include those available from Tosoh Corporation under the trade names "TOSO-CSM" and "extos" (chlorosulfonated polyethylene).

[0021] The content of (A) in the latex of the present disclosure is, for example, preferably about 20 to 60 mass%, more preferably about 25 to 55 mass%, and even more preferably about 30 to 50 mass%.

[0022] The surfactant of component (B) is a surfactant having an anionic moiety and a nonionic moiety, the nonionic moiety containing a polyoxyalkylene chain, and the anionic moiety containing a carboxylate, sulfonate, carbonate, sulfate, or phosphate salt (preferably a carbonate or sulfate). Examples of such salts include alkali metal salts (particularly sodium salts and potassium salts), ammonium salts, and amine salts, with alkali metal salts being preferred.

[0023] The polyoxyalkylene is preferably polyoxyethylene, polyoxypropylene, or polyoxyethylene polyoxypropylene, with polyoxyethylene being particularly preferred. The number of moles of alkylene oxide added (repeated) is preferably an integer of 2 to 40 (2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, or 40).

[0024] As the component (B), a surfactant having a polyoxyalkylene alkyl ether structure or a polyoxyalkylene alkyl phenyl ether structure is more preferred.

[0025] The "alkyl ether" in the polyoxyalkylene alkyl ether structure is preferably an alkyl ether having 6 to 20 carbon atoms (6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20). Furthermore, the "alkyl phenyl ether" in the polyoxyalkylene alkyl phenyl ether structure is preferably an alkyl ether in which a phenylene group (particularly a 1,4-phenylene group) exists between the alkyl group and the oxygen atom.

[0026] More specifically, the compound represented by the following formula (I) is particularly preferred as the component (B): 1 -O-(CH 2 CHR 2 -O) n -R 3 (I)

[0027] In formula (I), R 1 is R 1a - or R 1a -R 1b represents a group represented by -. 1a - represents an alkyl group having 6 to 20 carbon atoms (6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20). 1b - represents a phenylene group (preferably a 1,4-phenylene group).

[0028] R 2 represents a hydrogen atom or a methyl group, and n is the number of moles of alkylene oxide added, and is an integer of 2 to 40, preferably an integer of 2 to 35, and more preferably an integer of 2 to 20.

[0029] R 3 is -SO 3 M or -COOM. M represents an alkali metal, preferably sodium (Na) or potassium (K).

[0030] In formula (I), (CH 2 CHR 2 The polyoxyalkylene unit represented by —O)n is R 2 Two types of polyoxyalkylenes with different structures, namely, polyoxyethylene ((CH 2 CH 2 -O)x) and polyoxypropylene ((CH 2 CH (CH 3 )-O)y) such that the sum of x and y is n.

[0031] In formula (I), R 1 is R 1a represents a group represented by -, and R 3 Ga-SO 3When M is present, formula (I) represents a polyoxyalkylene alkyl ether sulfate. Specific examples of the polyoxyalkylene alkyl ether sulfate include polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene myristyl ether sulfate, and sodium polyoxyethylene oleyl ether sulfate; polyoxypropylene alkyl ether sulfates such as sodium polyoxypropylene lauryl ether sulfate, sodium polyoxypropylene tridecyl ether sulfate, sodium polyoxypropylene myristyl ether sulfate, and sodium polyoxypropylene oleyl ether sulfate; and polyoxyethylene polyoxypropylene alkyl ether sulfates such as sodium polyoxyethylene polyoxypropylene lauryl ether sulfate and sodium polyoxyethylene polyoxypropylene tridecyl ether sulfate. Among these, sodium polyoxyethylene lauryl ether sulfate, sodium polyoxyethylene tridecyl ether sulfate, sodium polyoxyethylene myristyl ether sulfate, sodium polyoxypropylene lauryl ether sulfate, sodium polyoxypropylene tridecyl ether sulfate, sodium polyoxyethylene polyoxypropylene lauryl ether sulfate, and sodium polyoxyethylene polyoxypropylene tridecyl ether sulfate are preferred. These may be used alone or in combination of two or more.

[0032] The polyoxyalkylene alkyl ether sulfate represented by formula (I) may be used singly or in combination of two or more. When using one type of polyoxyalkylene alkyl ether sulfate, it is particularly preferable to use a polyoxyalkylene alkyl ether sulfate in which n in formula (I) is an integer of 2 to 20. On the other hand, when using two or more types in combination, it is preferable to use a polyoxyalkylene alkyl ether sulfate containing a polyoxyalkylene alkyl ether sulfate (IA) in formula (I) where n is an integer of 9 to 35 and a polyoxyalkylene alkyl ether sulfate (IB) in formula (I) where n is an integer of 2 to 8. The polyoxyalkylene alkyl ether sulfate (IA) and the polyoxyalkylene alkyl ether sulfate (IB) are preferably selected so that the difference in n in formula (I) is 8 to 30, more preferably 10 to 20.

[0033] When the polyoxyalkylene alkyl ether sulfate (IA) and the polyoxyalkylene alkyl ether sulfate (IB) are used in combination, the polyoxyalkylene alkyl ether sulfate preferably contains 0.1 to 5 parts by mass, and more preferably 0.3 to 3 parts by mass, of the polyoxyalkylene alkyl ether sulfate (IB) per 1 part by mass of the polyoxyalkylene alkyl ether sulfate (IA).

[0034] In the latex of the present disclosure, the content of component (B) is preferably set to 0.3 to 12 parts by mass per 100 parts by mass of chlorosulfonated polyolefin (A). If the amount of component (B) used is less than 0.3 parts by mass, the static stability and mechanical stability of the resulting latex may be reduced. The range of parts by mass (0.3 to 12 parts by mass) is more preferably 0.5 to 10 parts by mass, and even more preferably 1 to 5 parts by mass.

[0035] As described above, the surfactant of component (C) is at least one surfactant selected from the group consisting of amino acid surfactants, alkylarylsulfonic acid surfactants, alkyl sulfate surfactants, and sulfosuccinic acid surfactants.

[0036] Preferred amino acid surfactants are compounds having an amide bond between a fatty acid and an amino acid salt. Preferred fatty acids include coconut oil fatty acids and C8 to C18 (C8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18) straight-chain or branched-chain fatty acids. Preferred amino acids include glutamic acid, aspartic acid, glycine, alanine, methylalanine, sarcosine, and methyltaurine. Preferred salts are alkali metal salts, more preferably sodium or potassium salts, and even more preferably sodium salts.

[0037] More specific examples of amino acid surfactants include glutamic acid surfactants such as N-coconut oil fatty acid glutamate, N-lauroyl glutamate, and N-myristoyl glutamate; alanine surfactants such as N-coconut oil fatty acid alanine salt, N-lauroyl alanine salt, N-coconut oil fatty acid methyl alanine salt, and N-lauroyl methyl alanine salt; sarcosine surfactants such as N-coconut oil fatty acid sarcosine salt and N-lauroyl sarcosine salt; glycine surfactants such as N-coconut oil fatty acid glycine salt and N-lauroyl glycine salt; aspartic acid surfactants such as N-coconut oil fatty acid aspartate, N-lauroyl aspartate, and N-myristoyl aspartate; and taurine surfactants such as N-coconut oil fatty acid methyl taurine salt, N-lauroyl methyl taurine salt, N-myristoyl methyl taurine salt, and N-stearoyl methyl taurine salt. The salt is preferably an alkali metal salt, more preferably a sodium salt or potassium salt, and even more preferably a sodium salt. Among them, from the viewpoint of coagulation efficiency, at least one selected from the group consisting of an alanine-based surfactant and a taurine-based surfactant is preferred, and at least one selected from the group consisting of N-C8 to C18 aliphatic acylmethylalanine sodium and N-C8 to C18 aliphatic acylmethyltaurine sodium is particularly preferred.

[0038] The alkylaryl sulfonic acid surfactant is preferably an alkylaryl sulfonic acid surfactant having a C8 to C18 (C8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18) linear or branched (preferably linear) alkyl group. The aryl is preferably benzene or naphthalene (i.e., a phenylene group or a naphthylene group is preferred, with 1,4-phenylene being more preferred as the phenylene group and 1,4-naphthylene being more preferred as the naphthylene group). More specific examples include linear or branched alkylbenzene sulfonic acid surfactants such as octylbenzene sulfonate, decylbenzene sulfonate, undecylbenzene sulfonate, dodecylbenzene sulfonate, and tetradecylbenzene sulfonate; and linear or branched alkylnaphthalene sulfonate surfactants such as butylnaphthalene sulfonate, octylnaphthalene sulfonate, decylnaphthalene sulfonate, and dodecylnaphthalene sulfonate. The salt is preferably an alkali metal salt, more preferably a sodium salt or potassium salt, and even more preferably a sodium salt. Among these, from the viewpoint of coagulation efficiency, a linear alkylbenzenesulfonate having an alkyl group of C8 to C18 is preferred, and a linear alkylbenzenesulfonate having an alkyl group of C10 to C16 is particularly preferred.

[0039] The alkyl sulfate surfactant may be an alkyl sulfate surfactant, preferably an alkyl sulfate having a C8 to C18 (C8, 9, 10, 11, 12, 13, 14, 15, 16, 17, or 18) linear or branched alkyl group, more preferably an alkyl sulfate having a linear alkyl group. More specific examples include linear alkyl sulfate surfactants such as octyl sulfate, decyl sulfate, undecyl sulfate, dodecyl sulfate (lauryl sulfate), α-olefin (C12 to C14) sulfate, α-olefin (C14 to C16) sulfate, and stearyl sulfate; and branched alkyl sulfate surfactants such as 2-ethylhexyl sulfate and isostearyl sulfate. The salt is preferably an alkali metal salt, more preferably a sodium or potassium salt, and even more preferably a sodium salt. From the viewpoint of coagulation efficiency, C8 to C18 linear alkyl sulfates are preferred, and C10 to C14 linear alkyl sulfates are particularly preferred. The alkyl sulfate surfactant may have some of the methylene groups in the alkyl chain replaced with an ether bond (—O—), and includes, for example, those in which the alkyl chain is a polyoxyalkylene chain. The alkyl sulfate surfactant also includes a polyoxyalkylene sulfonic acid surfactant, and may be a polyoxyalkylene sulfonate surfactant, and among these, polyoxyalkylene sulfonates (particularly polyoxyalkylene monosulfonates and polyoxyalkylene disulfonates) are preferred.

[0040] The sulfosuccinic acid surfactant may be a monoalkyl sulfosuccinic acid surfactant, a dialkyl sulfosuccinic acid surfactant, or an alkyl alkenyl sulfosuccinic acid surfactant, and examples thereof include monoalkyl sulfosuccinic acid surfactants such as monolauryl sulfosuccinate and monococonut oil fatty acid sulfosuccinate; dialkyl sulfosuccinic acid surfactants such as diisobutyl sulfosuccinate, dihexyl sulfosuccinate, dioctyl sulfosuccinate, di(2-ethylhexyl) sulfosuccinate and dinonyl sulfosuccinate; and alkyl alkenyl sulfosuccinic acid surfactants such as octyl allyl sulfosuccinate, 2-ethylhexyl allyl sulfosuccinate, nonyl allyl sulfosuccinate and dodecyl allyl sulfosuccinate. The salt is preferably an alkali metal salt, more preferably a sodium salt or potassium salt, and even more preferably a sodium salt. Among these, from the viewpoint of coagulation efficiency, at least one selected from the group consisting of mono C8 to C18 alkyl sulfosuccinates, di C8 to C18 alkyl sulfosuccinates, and C8 to C18 alkyl C2 to C6 alkenyl sulfosuccinates is particularly preferred.

[0041] The surfactant of component (C) may be appropriately synthesized or a commercially available product may be used. As described above, the surfactant of component (C) may be used alone or in combination of two or more types.

[0042] As the component (C), at least one selected from the group consisting of taurine-based surfactants, alkylbenzenesulfonic acid-based surfactants, and dialkylsulfosuccinic acid-based surfactants is more preferred.

[0043] The latex of the present disclosure may contain surfactants other than component (B) and component (C) within a range that does not impair the effects of the present invention. Examples of such other surfactants include alkylsulfonic acid surfactants such as nonanesulfonate and dodecanesulfonate; fatty acid surfactants such as oleate, stearate, and myristate; alkylenedisulfonic acid surfactants such as polyoxypropylene disulfonate and polyoxypropylene disulfonate; rosin surfactants such as rosinate, hydrogenated rosinate, and disproportionated rosinate; and sulfated oil-based surfactants such as sulfated castor oil, sulfated beef tallow, and sulfated rapeseed oil.

[0044] In the latex of the present disclosure, the content of the component (C) is preferably 0.5 to 12 parts by mass relative to 100 parts by mass of the component (A). The upper or lower limit of this range may be, for example, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10, 10.5, 11, or 11.5. For example, the range is more preferably 1 to 10 parts by mass, and even more preferably 2 to 8 parts by mass.

[0045] As the aqueous dispersion medium for component (D), for example, water is preferred. The content of component (D) in the latex of the present disclosure can be appropriately set depending on the degree of emulsification and viscosity of the latex. For example, in the latex of the present disclosure, it can be contained preferably in an amount of 60% by mass or more, more preferably 65% ​​by mass or more or 70% by mass or more. It can also be used as the balance of components other than component (D) to adjust the content ratio of each component while making the total latex 100% by mass.

[0046] As described above, the latex of the present disclosure can be preferably used to prepare a dip-molded article made of chlorosulfonated polyolefin even if it does not contain sodium alginate or the like. However, this does not exclude the further blending of sodium alginate or the like with the above components (A) to (D). In other words, the latex of the present disclosure preferably includes one that does not contain sodium alginate or the like. More specifically, the latex of the present disclosure preferably does not contain alginic acid or a salt thereof (particularly a sodium salt), carrageenan (particularly κ-carrageenan), or pectin.

[0047] As a method for producing the latex of the present disclosure, for example, there is a method in which a latex containing components (A), (B), and (D) is prepared, and then component (C) is added to the prepared latex. Here, the latex containing components (A), (B), and (D) before the addition of component (C) is sometimes referred to as a precursor latex for convenience.

[0048] Examples of methods for producing a precursor latex include melting component (A) and dispersing it in an aqueous dispersion medium containing component (B), or dissolving component (A) in an organic solvent and dispersing it in an aqueous dispersion medium containing component (B), followed by removing the organic solvent. The removed organic solvent can be easily recovered and reused. Component (B) can function as an emulsifier. The latter method is preferred from the viewpoint of easily controlling the particle size of component (A) in the resulting latex.

[0049] Examples of methods for dispersing component (A) in an aqueous dispersion medium using an organic solvent include a phase inversion emulsification method in which an aqueous dispersion medium is added to component (A) dissolved in an organic solvent to form a water-in-oil (W / O) emulsion, and then water is added to invert the phase to form an oil-in-water (O / W) emulsion, and a forced emulsification method in which component (A) dissolved in an organic solvent is mechanically dispersed in water in the presence of component (B) using an emulsifier. These methods may be used alone or in combination.

[0050] The organic solvent is not particularly limited as long as it is capable of dissolving component (A) and is immiscible with water, and examples thereof include aliphatic hydrocarbon solvents such as hexane, heptane, cyclohexane, etc.; aromatic hydrocarbon solvents such as benzene, toluene, xylene, etc.; chlorinated hydrocarbon solvents such as chloroform, 1,2-dichloroethane, etc.; alcohol solvents such as 1-butanol, isobutanol, etc.; ester solvents such as ethyl acetate, isopropyl acetate, n-butyl acetate, etc.; ketone solvents such as methyl ethyl ketone, methyl isobutyl ketone, etc.; ether solvents such as diisopropyl ether, dibutyl ether, anisole, etc. These organic solvents may be used alone or in combination of two or more.

[0051] The amount of organic solvent used here is not particularly limited, but is preferably set so that the concentration of component (A) in a composition obtained by dissolving component (A) in an organic solvent is 5 to 25% by mass, and more preferably 8 to 20% by mass.

[0052] The amount of component (B) used is not particularly limited, but is preferably 0.3 to 12 parts by mass, more preferably 0.5 to 10 parts by mass, and particularly preferably 1 to 5 parts by mass, per 100 parts by mass of component (A).

[0053] As the emulsifying apparatus, a known apparatus can be used, for example, a paddle mixer, a planetary mixer, a homomixer, a homogenizer, a disperser mixer, etc. The emulsifying apparatus may be of a batch type or a continuous type.

[0054] The temperature during emulsification cannot be determined in general because it depends on the type of organic solvent used, but it is usually about 5 to 70°C.

[0055] The organic solvent can be removed from the emulsion obtained by the above method by, for example, distillation under normal pressure, reduced pressure, or increased pressure. At this time, water can be removed at the same time, if necessary, to adjust the concentration of component (A) in the latex. In this organic solvent removal operation, an antifoaming agent may be used to suppress foaming caused by the emulsifier. Examples of antifoaming agents include mineral oil-based antifoaming agents, silicone-based antifoaming agents, acetylene-based antifoaming agents, metal soap-based antifoaming agents, acrylic antifoaming agents, and fluorine-based antifoaming agents. Of these, acetylene-based antifoaming agents are preferred. These may be used alone or in combination of two or more types. The amount of antifoaming agent used depends on the amount of component (B) used, but is generally 100 to 2,000 ppmwt (100 x 10) per 100 parts by mass of component (A). -6 ~2000 x 10 -6 The defoaming agent may be added to the emulsion before the removal operation or may be added appropriately during the removal operation. The addition method may be a method of adding all at once, a method of adding dropwise, a method of spraying, or the like. After removing the organic solvent, if water is to be further removed to adjust the concentration, it can be removed by a method such as distillation, centrifugation, membrane separation, or filtration.

[0056] The precursor latex may be commercially available, for example, "Seporex CSM-N" manufactured by Sumitomo Seika Chemicals Co., Ltd.

[0057] The latex of the present disclosure can be prepared, for example, by adding component (C) to a precursor latex.

[0058] The amount of component (C) added is preferably 0.5 to 12 parts by mass, more preferably 1 to 10 parts by mass, and even more preferably 2 to 8 parts by mass, per 100 parts by mass of component (A) in the precursor latex.

[0059] The latex of the present disclosure may further contain known additives such as a rheology modifier, an antioxidant, an antifoaming agent, a pH adjuster, a chelating agent, a vulcanizing agent, a vulcanization accelerator, a vulcanization accelerator aid, an acid acceptor, a film-forming aid, a plasticizer, a filler, a pigment, a thickener, etc., within a range that does not impair the effects of the present disclosure.

[0060] Examples of rheology modifiers include polysaccharides such as cellulose, cellulose nanofiber, cellulose nanocrystal, hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxypropylmethyl cellulose, carboxymethyl cellulose, chitin, chitosan, guar gum, and xanthan gum; water-soluble vinyl polymers such as polyacrylic acid, sodium polyacrylate, crosslinked polyacrylic acid, polyacrylamide, polyvinyl alcohol, polyvinyl methyl ether, and polyvinylpyrrolidone; and clay minerals such as montmorillonite, nontronite, saponite, beidellite, and hectorite.

[0061] Examples of the antioxidant include phenol-based antioxidants such as dibutylhydroxytoluene, 2,2′-methylenebis(4-ethyl-6-tert-butylphenol), and 2,5-di-tert-butylhydroquinone; amine-based antioxidants such as N-phenyl-1-naphthylamine and di(4-octylphenyl)amine; phosphorus-based antioxidants such as tris(nonylphenyl)phosphite; sulfur-based antioxidants such as dilauryl thiodipropionate, 2-mercaptobenzimidazole, and nickel dibutyldithiocarbamate; and bisphenol A-type epoxy resins.

[0062] Examples of the defoaming agent include oil-based defoaming agents, mineral oil-based defoaming agents, silicone-based defoaming agents, and polyether-based defoaming agents.

[0063] Examples of pH adjusters include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, trimethylamine, triethanolamine, hydrochloric acid, sulfuric acid, phosphoric acid, citric acid, and acetic acid.

[0064] Examples of the chelating agent include ethylenediaminetetraacetic acid, nitrilotriacetic acid, trans-1,2-diaminocyclohexanetetraacetic acid, diethylenetriaminepentaacetic acid, bis(aminoethyl)glycol ether-N,N,N',N'-tetraacetic acid, N-(2-hydroxyethyl)ethylenediamine-N,N',N'-triacetic acid, dihydroxyethylglycine, 1-hydroxyethane-1,1-diphosphonic acid, gluconic acid, citric acid, malic acid, and tartaric acid.

[0065] Examples of the vulcanizing agent include sulfur such as powdered sulfur, sulfur flowers, precipitated sulfur, and colloidal sulfur; organic peroxides such as di-tert-butyl peroxide and dicumyl peroxide; maleimide compounds such as N,N'-m-phenylene bismaleimide; quinoid compounds such as p-quinone dioxime and p,p'-dibenzoylquinone dioxime; metal compounds such as magnesium oxide and lead oxide; and polyhydric alcohol compounds such as pentaerythritol, dipentaerythritol, sorbitol, and trimethylolpropane.

[0066] Examples of the vulcanization accelerator include diethyldithiocarbamic acid, dibutyldithiocarbamic acid, diphenyldithiocarbamic acid, sodium diethyldithiocarbamate, sodium dibutyldithiocarbamate, sodium diphenyldithiocarbamate, zinc diethyldithiocarbamate, zinc dibutyldithiocarbamate, zinc diphenyldithiocarbamate, 2-mercaptobenzothiazole, zinc 2-mercaptobenzothiazole, di-2-benzothiazolyl disulfide, 2-(4'-morpholino) dithio)benzothiazole, trimethylthiourea, N,N'-diethylthiourea, 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, N-cyclohexyl-2-benzothiazolylsulfenamide, N-oxydiethylene-2-benzothiazolylsulfenamide, tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetramethylthiuram monosulfide, dipentamethylenethiuram tetrasulfide, zinc isopropyl xanthogenate, and the like.

[0067] Examples of the vulcanization accelerator include metal oxides such as zinc oxide and magnesium oxide, and fatty acids such as stearic acid and palmitic acid.

[0068] Examples of the acid acceptor include metal oxides such as lead oxide, magnesium oxide, zinc oxide, and calcium oxide; metal hydroxides such as magnesium hydroxide, calcium hydroxide, and aluminum hydroxide; clay minerals such as hydrotalcite; and epoxy compounds such as phenyl glycidyl ether, bisphenol A diglycidyl ether, epoxidized soybean oil, epoxidized linseed oil, epoxidized polybutadiene, and polyglycidyl methacrylate.

[0069] Examples of the film-forming aid include propylene glycol, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, ethylene glycol monoisopropyl ether, ethylene glycol mono-n-butyl ether, ethylene glycol monoiso-butyl ether, ethylene glycol mono-tert-butyl ether, ethylene glycol monophenyl ether, diethylene glycol monoethyl ether, diethylene glycol monopropyl ether, diethylene glycol monoisopropyl ether, diethylene glycol mono-n-butyl ether, diethylene glycol monoiso-butyl ether, diethylene glycol mono-tert-butyl ether, diethylene glycol monophenyl ether, diethylene glycol dimethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol monobutyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, dipropylene glycol mono-n-butyl ether, dipropylene glycol dimethyl ether, tripropylene glycol monomethyl ether, and 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate.

[0070] Examples of the plasticizer include phthalate esters, adipic acid esters, glycerin fatty acid esters, polyether polyols, and polyester polyols.

[0071] Examples of fillers include carbon fiber, cellulose fiber, carbon black, silica, talc, clay, calcium carbonate, titanium oxide, and barium sulfate.

[0072] Examples of pigments include carbon black, titanium oxide, chromium oxide, iron blue, amber, nickel titanium yellow, viridian, cobalt blue, phthalocyanine blue, phthalocyanine green, molybdenum orange, chrome yellow, anthraquinone, and quinacridone.

[0073] When an additive is contained, the amount of the additive contained in the latex of the present disclosure is not particularly limited, but is preferably 5 to 30 parts by mass per 100 parts by mass of the solid content in the latex composition (i.e., component (A)).

[0074] The method for preparing the latex of the present disclosure is not particularly limited, and examples thereof include a method of mixing a precursor latex with the component (C) and, if necessary, various other additives using a dispersing machine such as a ball mill, a bead mill, a kneader, or a disper; a method of preparing an aqueous dispersion containing the component (C) and, if necessary, various other additives using a dispersing machine in advance, and then mixing the aqueous dispersion with the precursor latex; a method of mixing a precursor latex with the component (C) and some of the additives, and then mixing it with an aqueous dispersion of the other additives; and a method of mixing a precursor latex with some of the additives, and then mixing it with an aqueous dispersion of the component (C) and other additives.

[0075] The pH of the latex of the present disclosure is preferably 5 or higher, and more preferably in the range of 7 to 12, from the viewpoint of facilitating coagulation.

[0076] The solid content concentration of the latex of the present disclosure is preferably 20 to 60% by mass, more preferably 25 to 50% by mass.

[0077] The viscosity of the latex of the present disclosure at 25°C is preferably 20 to 300 mPa·s, more preferably 30 to 200 mPa·s, and particularly preferably 50 to 100 mPa·s. When the viscosity is within this range, a film with a uniform thickness is easily obtained during dip molding. The viscosity in the present disclosure is measured using a Brookfield viscometer with rotor No. 1 or No. 2 at a rotation speed of 60 rpm, and is the viscosity measured 1 minute after the start of measurement.

[0078] The latex of the present disclosure can be preferably used for dip molding. In other words, the latex of the present disclosure can be preferably used as a dip molding composition.

[0079] The latex of the present disclosure may be aged (also referred to as pre-vulcanization) before being subjected to dip molding. The aging time can be appropriately set depending on the type of additives and the aging temperature, and is, for example, preferably 1 to 7 days, more preferably 1 to 3 days. The aging temperature is preferably 10 to 50°C, more preferably 20 to 40°C.

[0080] After aging, it is preferably stored at a temperature of 30° C. or less until it is subjected to dip molding.

[0081] The particle size of component (A) contained in the latex of the present disclosure is not particularly limited, but the volume-based median particle size measured with a laser diffraction particle size analyzer is preferably 0.1 to 10 μm, more preferably 0.3 to 5 μm, and particularly preferably 0.5 to 2.0 μm. Particle sizes within this range make it easier to obtain a dense film upon coagulation. The particle size can be adjusted, for example, by the type and amount of organic solvent and emulsifier used in preparing the precursor latex, the amount of water used, and the operating conditions of the emulsification apparatus. Alternatively, the particle size can be adjusted by the amount of component (C) used in preparing the latex of the present disclosure from the precursor latex, the type and amount of known additives that can be used as needed, and the preparation method.

[0082] To enhance the stability of the latex of the present disclosure, additives such as dispersion stabilizers such as polyvinyl alcohol, polyvinylpyrrolidone, and hydroxyethyl cellulose, and stabilizers such as dibutylhydroxytoluene, 2,5-di-tert-butylhydroquinone, and bisphenol A epoxy resin may be added. Such additives may be added to the precursor latex, or, depending on the type of additive, may be added to the organic solvent solution or water used for emulsification during the preparation of the precursor latex. Alternatively, they may be added in advance to the raw material (A) component. The additives are typically preferably added as an individual or mixed aqueous solution or aqueous dispersion. When the additives are added, a total amount of 0.1 to 10 parts by mass per 100 parts by mass of component (A) is preferred.

[0083] The present disclosure also encompasses a dip-molded article obtained by using the latex of the present disclosure as a dip-molding composition.

[0084] Dip molding is a method in which a mold (molding mold) is immersed in a dip-molding composition, the composition is deposited on the surface of the mold, the mold is then lifted from the composition, and the composition deposited on the surface of the mold is then dried. Below, methods that can be used to prepare the dip-molded article of the present disclosure are described in more detail.

[0085] The mold used for dip molding can be a mold that corresponds to the desired three-dimensional shape and is integrally formed from ceramic, metal, glass, plastic, etc. The surface of the mold may be finished with a matte finish or may be provided with other materials such as fibers or other types of rubber coatings, depending on the purpose of the dip-molded article. In addition, the mold may be preheated before being immersed in the dip-molding composition.

[0086] Before immersing the mold in the dip-molding composition or after removing the mold from the dip-molding composition, a coagulant is preferably used to aggregate the solid component (sometimes referred to as the rubber component) mainly composed of chlorosulfonated polyolefin. Examples of methods for using the coagulant include immersing the mold before immersion in the dip-molding composition in a coagulant solution (hereinafter also referred to as a coagulant liquid) to adhere the coagulant to the mold, and immersing the mold on which the dip-molding composition has been deposited in a coagulant liquid. From the viewpoint of obtaining a dip-molded article with minimal thickness unevenness, a method of immersing the mold before immersion in the dip-molding composition in a coagulant solution to adhere the coagulant to the mold is preferred.

[0087] Examples of coagulants include metal salts, with water-soluble metal salts being more preferred. Among metal salts, polyvalent metal salts that generate polyvalent metal ions are preferred from the viewpoint of high coagulation power, with water-soluble polyvalent metal salts being more preferred. Examples of water-soluble metal salts include metal halides such as sodium chloride, potassium chloride, barium chloride, calcium chloride, magnesium chloride, zinc chloride, and aluminum chloride; metal nitrates such as sodium nitrate, potassium nitrate, barium nitrate, calcium nitrate, zinc nitrate, and aluminum nitrate; metal acetates such as sodium acetate, potassium acetate, barium acetate, calcium acetate, zinc acetate, and aluminum acetate; and metal sulfates such as sodium sulfate, potassium sulfate, calcium sulfate, magnesium sulfate, and aluminum sulfate. As the polyvalent metal, alkaline earth metals are preferred, with calcium, barium, and magnesium being more preferred, and calcium being particularly preferred. Furthermore, as the coagulant, calcium chloride and calcium nitrate are particularly preferred from the viewpoint of high solubility in water. These coagulants may be used alone or in combination of two or more.

[0088] The coagulant is preferably used in the form of an aqueous solution. This aqueous solution may further contain a water-soluble organic solvent such as methyl alcohol or ethyl alcohol, or a nonionic surfactant. The concentration of the coagulation liquid is not particularly limited, but is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, and particularly preferably 15 to 35% by mass. The immersion time of the casting mold in the coagulation liquid is not particularly limited, but is usually preferably 5 to 300 seconds, and more preferably 10 to 100 seconds.

[0089] After the casting mold is immersed in the coagulation liquid to adhere the coagulation liquid to the surface, the solvent of the coagulation liquid may be removed by drying. The drying temperature can be set appropriately depending on the type of solvent and salt used, and is preferably 60 to 150°C, and more preferably 80 to 120°C. The drying time is not particularly limited, but is preferably 1 to 600 seconds, and more preferably 5 to 300 seconds. Drying the coagulation liquid on the surface of the casting mold makes it easier to create a state in which the salt is uniformly adhered to the surface of the casting mold.

[0090] The time for immersing the mold in the latex (dip-molding composition) of the present disclosure may be appropriately set depending on the desired thickness (film thickness), but is preferably 5 to 600 seconds, more preferably 10 to 300 seconds.

[0091] After the mold is removed from the dip-molding composition, the solidified coating formed on the mold surface is typically dried by heating. The drying method is not particularly limited, and drying can be performed using a hot air heater, infrared heater, microwave heater, high-frequency heater, or the like. The drying temperature is not particularly limited, but is preferably 50 to 160°C, more preferably 60 to 140°C, and particularly preferably 70 to 120°C. The drying time is also not particularly limited, but is preferably 1 to 120 minutes, more preferably 10 to 100 minutes, and particularly preferably 20 to 60 minutes.

[0092] Furthermore, if necessary, further heating may be performed to vulcanize the solidified coating formed on the mold surface. The heating conditions during vulcanization are not particularly limited, but 60 to 200°C is preferred, 80 to 180°C is more preferred, and 100 to 160°C is particularly preferred. By setting the heating temperature within this range, it is possible to achieve an appropriate vulcanization rate and suppress deterioration of the rubber component due to excessive heating. The heating time for vulcanization may be selected appropriately depending on the heating temperature, and is usually 5 to 120 minutes. The heating method can be, for example, the same method as the heating method described above.

[0093] Before or after heating the mold onto which the dip-molding composition has been deposited, it is preferable to wash the mold with water or warm water to remove water-soluble impurities (e.g., excess emulsifier, surfactant, coagulant, uncoagulated latex, etc.). The temperature of the water or warm water used is preferably 20 to 80°C, more preferably 30 to 70°C. The washing time is preferably about 0.5 to 60 minutes.

[0094] The dip-molded article after drying (and further vulcanization, if necessary) is removed from the mold. Removal methods include peeling from the mold by hand, peeling from the mold using a peeling roller, and peeling using water pressure or compressed air pressure. After being removed from the mold, the dip-molded article may be further washed with water. Furthermore, if necessary, to prevent adhesion at the contact surfaces between dip-molded articles and to improve slippage during attachment and detachment, inorganic fine particles such as talc or calcium carbonate or organic fine particles such as cornstarch may be applied to the surface, an elastomer layer containing fine particles may be further formed on the surface, or the surface layer may be chlorinated.

[0095] The thickness of the dip-molded article thus obtained is preferably 0.1 to 2 mm, more preferably 0.2 to 1.5 mm, and particularly preferably 0.3 to 1.0 mm. The thickness can be appropriately set by the immersion time, etc., as described above.

[0096] In this specification, the term "comprising" includes "consisting essentially of" and "consisting of." In addition, the present disclosure includes any and all combinations of the constituent elements described in this specification.

[0097] Furthermore, the various characteristics (properties, structures, functions, etc.) described in each embodiment of the present disclosure above may be combined in any way to identify the subject matter encompassed by the present disclosure, i.e., the present disclosure encompasses all subject matter consisting of any combination of the combinable characteristics described herein.

[0098] The present disclosure will be specifically described below with reference to examples and comparative examples, but the present disclosure is not limited to these examples or the like.

[0099] The surfactants used in the examples and comparative examples are listed below. A: Sodium alkyl (C10-16) benzenesulfonate (manufactured by NOF Corporation, trade name "Newlex R", solid content concentration 50% by mass) B: Sodium di-2-ethylhexyl sulfosuccinate (manufactured by NOF Corporation, trade name "Rapisol A-80", solid content concentration 80% by mass) C: Sodium N-acylmethyl taurate (manufactured by NOF Corporation, trade name "Diapon S", solid content concentration 13% by mass) D: Sodium alkylaryl sulfosuccinate (manufactured by Sanyo Chemical Industries, Ltd., trade name "Eleminol JS-20", solid content concentration 40% by mass) E: Sodium lauryl sulfate (manufactured by Tokyo Chemical Industry Co., Ltd., reagent, solid content concentration 97% by mass) F: Sodium polyoxyalkylene disulfonate (manufactured by Nippon Nyukazai Co., Ltd., trade name "Newcol 240", solid content concentration 30% by mass) G: disodium lauryl sulfosuccinate (manufactured by Sanyo Chemical Industries, Ltd., trade name "Viewlite SSS", solid content concentration 40% by mass); H: sodium N-lauroylmethylalanine (manufactured by NOF Corporation, trade name "Softilt AS-L", solid content concentration 30% by mass); I: potassium oleate (manufactured by NOF Corporation, trade name "NonSal OK-1", solid content concentration 80% by mass); J: β-naphthalenesulfonic acid formalin condensate sodium salt (manufactured by Kao Corporation, trade name "Demol N", solid content concentration 100% by mass); K: lauryl dimethylaminoacetic acid betaine (manufactured by NOF Corporation, trade name "Nissan Anon BL", solid content concentration 35% by mass); L: potassium rosinate (manufactured by Arakawa Chemical Industries, Ltd., trade name "Londis K-25", solid content concentration 25% by mass); The parts by mass of each surfactant in each example and comparative example is a value relative to 100 parts by mass of chlorosulfonated polyolefin in chlorosulfonated polyolefin latex (specifically, manufactured by Sumitomo Seika Chemicals Co., Ltd., trade name "Sepolex CSM-N" (chlorosulfonated polyethylene), solid content concentration 40% by mass). The number of parts added [phr] (per hundred rubber) in Table 1 indicates this value.

[0100] The surfactant concentrations (solids concentrations) of the above surfactant products A to L vary, and the parts by mass values ​​for each surfactant in the examples are calculated based on the converted surfactant amounts. For example, as described below, in Example 1, a chlorosulfonated polyethylene latex (Sepolex CSM-N) with a solids concentration of approximately 40% by mass was used, and 2.5 parts by mass of a sodium alkyl (C10-16) benzenesulfonate product (Newrex R) with a solids concentration of 50% by mass was used. In this case, if the amount of Sepolex CSM-N used is α parts by mass, the amount of chlorosulfonated polyethylene is 0.4α parts by mass, and the amount of sodium alkyl (C10-16) benzenesulfonate is 0.4α × 2.5 / 100 = 0.01α parts by mass. In addition, the amount of Newrex R used is 0.01α ÷ 0.5 = 0.02α parts by mass. In other words, the number of added parts [phr] in Table 1 indicates the mass parts of the surfactant contained in the surfactant product used relative to 100 mass parts of chlorosulfonated polyolefin contained in the chlorosulfonated polyolefin latex used.

[0101] Seporex CSM-N is a latex composition containing 40% by mass of chlorosulfonated polyethylene, approximately 60% by mass of water, and a small amount (approximately 0.1 to 2% by mass) of polyoxyalkylene alkyl ether sulfate as an emulsifier.

[0102] Evaluation Method <Evaluation of Coagulation Possibility> The coagulation possibility was evaluated as ◯ when the film thickness was 0.1 mm or more, indicating that coagulation occurred, and × when the film thickness was less than 0.1 mm, indicating that coagulation did not occur. <Film Strength> A test piece was punched out from the obtained film into the shape of a JIS No. 4 dumbbell, and a tensile test was performed using an autograph (Shimadzu Corporation, product name "AGS-X") at a measurement temperature of 25°C and a pulling rate of 300 mm / min to measure the breaking strength and breaking elongation. <Chemical Resistance of Film> A test piece was cut into a square 1 cm from the obtained film. A pH test paper (WATT MANN CO., LTD., pH test paper, SR type) was attached to the back of the test piece, and one drop of 95% sulfuric acid (reagent, Fujifilm Wako Pure Chemical Industries, Ltd.) was dropped on the front side of the film and left to stand for 1 hour. The change in the pH test paper after 1 hour was observed, and if there was no change in color of the pH test paper, it was evaluated as ◯, indicating that sulfuric acid had not permeated, and if there was a change in color of the pH test paper, it was evaluated as ×, indicating that sulfuric acid had permeated.

[0103] Example 1 Preparation of Dip-Forming Composition Chlorosulfonated polyethylene latex (manufactured by Sumitomo Seika Chemicals Co., Ltd., trade name "Sepolex CSM-N," solids concentration 40% by mass) was mixed with 2.5 parts by mass of sodium alkyl (C10-16) benzenesulfonate (manufactured by NOF Corporation, trade name "Newlex R") per 100 parts by mass of chlorosulfonated polyethylene contained in the latex, and the mixture was stirred until completely dissolved, to obtain a dip-forming composition. The viscosity of the obtained dip-forming composition at 25°C was 56 mPa s.

[0104] <Production of Dip-Molded Article> A ceramic mold was immersed in a 35% by mass aqueous solution of calcium nitrate for 5 seconds and dried in a 120°C air dryer for 5 minutes. The ceramic mold was then immersed in the dip-molding composition for 30 seconds to adhere a rubber component to the ceramic mold, and then removed from the dip-molding composition. The ceramic mold with the adhered rubber component was dried in a 70°C air dryer for 4 hours and then immersed in 60°C hot water for 1 hour to remove water-soluble components. It was then dried at 70°C for 1 hour and further heated at 120°C for 20 minutes. After cooling to room temperature, the coating was peeled from the ceramic mold to obtain a dip-molded article. The obtained dip-molded article was evaluated according to the following criteria. The ceramic mold used was boat-shaped, measuring 10 cm x 1.5 cm x 1 cm (length x width x depth), and a coating (dip-molded article) was obtained using the above-mentioned procedure.

[0105] (Examples 2 to 15) Dip-molded articles were obtained in the same manner as in Example 1, except that the compounding ingredients, compounding amounts, and immersion time in Example 1 were changed to those shown in Table 1. In Examples 11 to 15, surfactant 1 was added to chlorosulfonated polyethylene latex, and then surfactant 2 was further added, followed by stirring until completely dissolved, to obtain dip-molding compositions.

[0106] Comparative Example 1 A dip-molding composition was prepared by adding nothing to chlorosulfonated polyethylene latex (manufactured by Sumitomo Seika Chemicals Co., Ltd., trade name "Sepolex CSM-N", solid content concentration 40% by mass).

[0107] Comparative Examples 2 to 5 Dip-molded articles were obtained in the same manner as in Example 1, except that the ingredients, amounts thereof, and immersion time were changed to those shown in Table 1.

[0108]

[0109] (Examples 16 and 17) <Preparation of Dip-forming Composition> 7.5 parts by mass of a surfactant having the formulation shown in Table 2 was added to chlorosulfonated polyethylene latex (manufactured by Sumitomo Seika Chemicals Co., Ltd., trade name "Sepolex CSM-N," solid content concentration 40% by mass), and the mixture was stirred until completely dissolved or dispersed. Note that, like the number of added parts [phr] in Table 1, this "7.5 parts by mass" indicates the parts by mass of the surfactant contained in the surfactant product used relative to 100 parts by mass of chlorosulfonated polyolefin contained in the chlorosulfonated polyolefin latex used.

[0110] Thereafter, 3 parts by mass, calculated as solid content, of an aqueous sodium dibutyldithiocarbamate solution (manufactured by Ouchi Shinko Chemical Industry Co., Ltd., trade name "Noccela TP") and 10 parts by mass of triethylene glycol monobutyl ether (manufactured by Nippon Nyukazai Co., Ltd., trade name "Butyl Triglycol") were added, and the mixture was stirred until homogeneous, thereby obtaining a dip-forming composition. The viscosity of the obtained dip-forming composition at 25°C was 121 mPa s.

[0111] <Production of Dip-Molded Article> A ceramic mold was immersed in a 35% by mass aqueous solution of calcium nitrate for 5 seconds and dried in a 120°C air dryer for 5 minutes. The ceramic mold was then immersed in the dip-molding composition for 5 minutes, a rubber component was attached to the ceramic mold, and the ceramic mold was then removed from the dip-molding composition. The ceramic mold with the attached rubber component was dried in a 70°C air dryer for 4 hours and then heated at 120°C for 20 minutes. After cooling to room temperature, the coating was peeled off from the ceramic mold to obtain a dip-molded article. The obtained dip-molded article was evaluated according to the above criteria. The ceramic mold used was a rectangle measuring 20 cm x 8 cm, and a coating (dip-molded article) was obtained using the above-described procedure.

[0112]

[0113] From the above results, it was found that the addition of a specific surfactant to chlorosulfonated polyolefin latex enables coagulation, and a dip-molded product with excellent strength and chemical resistance can be obtained.

[0114] The present invention provides a method for producing a dip-molded article made of a chlorosulfonated polyolefin without using sodium alginate, a latex that can be used in the method, and a dip-molded article made of a chlorosulfonated polyolefin that does not need to contain sodium alginate. This method allows for the convenient production of dip-molded articles that are preferably excellent in strength and chemical resistance, and is also useful for protecting the environment, as it allows for the production of dip-molded articles such as gloves without using organic solvents during dip-molding.

Claims

1. A chlorosulfonated polyolefin latex comprising: (A) a chlorosulfonated polyolefin; (B) a surfactant having an anionic portion and a nonionic portion, the nonionic portion containing a polyoxyalkylene chain and the anionic portion containing a carboxylate, a sulfonate, a carbonate ester salt, a sulfate ester salt, or a phosphate ester salt; (C) at least one surfactant selected from the group consisting of amino acid-based surfactants, alkylarylsulfonate-based surfactants, alkylsulfate-based surfactants, and sulfosuccinate-based surfactants; and (D) an aqueous dispersion medium.

2. The latex according to claim 1, which is for dip molding.

3. The latex according to claim 1 or 2, wherein the content of (C) is 1 to 10 parts by mass per 100 parts by mass of (A).

4. The latex according to claim 1 or 2, wherein the amino acid surfactant is at least one amino acid surfactant selected from the group consisting of glutamic acid surfactants, alanine surfactants, sarcosine surfactants, glycine surfactants, aspartic acid surfactants, and taurine surfactants; the alkylarylsulfonic acid surfactant is an alkylarylsulfonic acid surfactant in which the alkyl group in the active agent is a linear or branched C8-C18 alkyl and the aryl group is a phenylene group or a naphthylene group; the alkyl sulfate surfactant is at least one alkyl sulfate surfactant selected from the group consisting of alkyl sulfate salt surfactants and polyoxyalkylenesulfonic acid surfactants; and the sulfosuccinic acid surfactant is at least one sulfosuccinic acid surfactant selected from the group consisting of monoalkylsulfosuccinic acid surfactants, dialkylsulfosuccinic acid surfactants, and alkylalkenylsulfosuccinic acid surfactants.

5. The latex according to claim 1 or 2, wherein the chlorosulfonated polyolefin is a chlorosulfonated polyethylene.

6. The surfactant of (B) is represented by the formula (I): 1 -O-(CH 2 CHR 2 -O) n -R 3 (I) (wherein, R 1 is R 1a -, or R 1a -R 1b R represents a group represented by -; 1a - represents an alkyl group having 6 to 20 carbon atoms; -R 1b - represents a phenylene group, n represents an integer of 2 to 40, and R 2 are the same or different and represent a hydrogen atom or a methyl group; R 3 Ha-SO 3 The latex according to claim 1 or 2, wherein the compound is represented by the following formula:

7. A dip-molded product obtained by dip-molding the latex according to claim 1 or 2 using a polyvalent metal salt as a coagulant.

8. The dip-formed article according to claim 7, having a thickness of 0.1 mm or more.

9. The dip-formed article according to claim 7, which is a glove.

10. A method for producing a dip-molded body, comprising the steps of: preparing a dip-molding composition by mixing (C) at least one surfactant selected from the group consisting of amino acid-based surfactants, alkylarylsulfonic acid-based surfactants, alkylsulfuric acid-based surfactants, and sulfosuccinic acid-based surfactants with a latex containing (A) a chlorosulfonated polyolefin, (B) a surfactant having an anionic moiety and a nonionic moiety, the nonionic moiety containing a polyoxyalkylene chain and the anionic moiety containing a carboxylate, a sulfonate, a carbonate ester salt, a sulfate ester salt, or a phosphate ester salt, and (D) an aqueous dispersion medium; adhering a coagulant to the surface of a mold having a desired shape; and immersing the mold with the coagulant adhered thereto in the dip-molding composition to form a coagulated coating.

Citation Information

Patent Citations

  • Chemical-resistant glove

    JP1993230702A

  • Method for manufacturing film-molded body

    JP7033242B1

  • Dip molded article and method for manufacturing dip molded article

    WO2015146974A1

  • JP1975037885A

  • Production of powderd rubber

    JP1982000147A