Bismaleimide-based resin molded body containing pitch-based carbon fibers and method for producing the same
The pitch-based carbon fiber-containing bismaleimide resin molded article addresses the warping and cost issues of polyimide resin-based articles by maintaining shape stability and mechanical strength at lower curing temperatures, enhancing economic efficiency and sliding performance.
Patent Information
- Application Number
- PCT/JP2024/011569
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-27
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Fiber-reinforced resin molded articles using addition reaction polyimide resins exhibit excellent mechanical strength and heat resistance but often warp, making them unsuitable for slidable applications, and the high curing temperature requirements increase equipment and energy costs, posing economic inefficiencies.
A pitch-based carbon fiber-containing bismaleimide resin molded article is developed, with a specific fiber content and processing method that maintains shape stability and mechanical strength while reducing curing temperatures, allowing for uniform carbon fiber dispersion and lower equipment costs.
The bismaleimide resin molded article achieves excellent shape stability, heat resistance, and sliding performance comparable to polyimide resin-based articles but with reduced warpage and lower energy costs, making it economically viable for use in sliding members.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000018_0000
Abstract
Description
Pitch-based carbon fiber-containing bismaleimide resin molding and its manufacturing method
[0001] The present invention relates to a pitch-based carbon fiber-containing bismaleimide resin molded article and a method for producing the same, and more specifically to a pitch-based carbon fiber-containing bismaleimide resin molded article that is effectively prevented from warping, has excellent shape stability during molding, and is also economical, and a method for producing the same.
[0002] Conventionally, molded articles made of fiber-reinforced resins obtained by blending functional fibers such as carbon fibers with resins have been widely used in applications such as transportation equipment (e.g., automobiles and aircraft), civil engineering and construction materials, and sporting goods due to their excellent properties such as weather resistance, mechanical strength, and durability. For example, Patent Document 1 listed below describes a carbon fiber-reinforced resin molded article made of a specific pitch-based short carbon fiber mixture and a matrix resin, and states that it is suitable for use in various electronic components. Patent Document 2 listed below also proposes a friction material made of a friction material resin composition using a specific aromatic polyimide oligomer as a binder for carbon fibers, etc., and states that this friction material has superior heat resistance and mechanical properties of the binder itself and good moldability compared to when phenolic resins, which have traditionally been used as suitable binders for friction materials, are used.
[0003] When such fiber-reinforced resin molded articles are used as sliding members such as bearings, they are required to have properties such as high mechanical strength (e.g., strength and rigidity), a small coefficient of dynamic friction (i.e., low wear), and a high limiting PV value. Therefore, it is desirable to use an addition-reaction polyimide resin as the matrix resin, which has excellent mechanical strength, heat resistance, and durability, as well as excellent resin impregnation. High-performance addition-reaction polyimide resins that can be used to produce carbon fiber-reinforced composites by transfer molding (RTM) and resin injection (RI) have also been proposed (Patent Document 3). However, when an addition-reaction polyimide resin is used as the matrix resin for a fiber-reinforced resin molded article, even though excellent heat resistance, durability, and mechanical strength can be obtained, the resulting molded article tends to warp, making it unsuitable for practical use as a sliding member.
[0004] To solve these problems, the present inventors have proposed a molding precursor comprising a functional fiber impregnated with an addition-reaction-type polyimide resin, which has a melt viscosity of 300 to 3,200 kPa s when maintained at a temperature 5 to 20°C lower than the viscosity increase starting temperature of the addition-reaction-type polyimide resin for 1 to 10 minutes, and a method for producing the molding precursor (Patent Document 4).
[0005] Japanese Patent No. 4538502 Japanese Patent Laid-Open No. 2009-242656 Japanese Patent Publication No. 2003-526704 International Publication No. 2020 / 116658
[0006] According to Patent Document 4, it is possible to mold a functional fiber-reinforced resin precursor in which functional fibers are uniformly dispersed in an addition-reaction polyimide resin, and a resin molded article molded from this resin precursor has excellent shape stability without distortion such as warping, and also has excellent heat resistance, mechanical strength, and sliding performance. However, since addition-reaction polyimide resins have a high curing temperature, it is necessary to increase the molding temperature. Therefore, the compression molding machine used for molding also needs to have high heat resistance, which increases equipment costs and the energy costs required for molding, making it unsatisfactory from an economic standpoint.
[0007] Therefore, an object of the present invention is to provide a fiber-reinforced resin molding that has shape stability, heat resistance, mechanical strength, sliding performance, etc. similar to those of a molding using an addition reaction type polyimide resin as a matrix resin, while also being economical, and a method for producing the same.
[0008] According to the present invention, there is provided a resin molding characterized in that pitch-based carbon fibers are contained in a bismaleimide-based resin.
[0009] The resin molded product of the present invention preferably has the following characteristics: 1. The pitch-based carbon fiber is contained in an amount ranging from 17 to 43 parts by mass relative to 100 parts by mass of the bismaleimide resin; 2. The ratio of the amount of warpage t (mm) of the resin molded product to the longest dimension D (mm) of the resin molded product in the planar direction {(t / D) x 100} is less than 0.25%; 3. The pitch-based carbon fiber has an average fiber length ranging from 50 to 6000 μm and an average fiber diameter ranging from 5 to 20 μm; and 4. The pitch-based carbon fiber is a mesophase pitch-based carbon fiber.
[0010] According to the present invention, there is also provided an impregnation step in which a prepolymer of a bismaleimide resin is mixed with pitch-based carbon fiber, the mixture is maintained at a temperature above the melting point of the bismaleimide resin and below the viscosity initiation temperature, and the pitch-based carbon fiber is impregnated with the bismaleimide resin; the impregnated product is maintained at a temperature above the viscosity initiation temperature of the bismaleimide resin, and 0.5 g of the pulverized product obtained in this manner is pressed into a tablet having a diameter of 12 mm. The tablet is placed between parallel flat plates on the pressure axis, heated to 120°C under a load of 60 N and maintained for 3 minutes, and then heated to 160°C and maintained for 5 minutes, and the area of the impregnated product is 200 to 2000 mm. 2 a pre-curing step of increasing the viscosity of the impregnated product to a temperature equal to or higher than the thermal curing initiation temperature of the bismaleimide resin; a pulverizing and mixing step of pulverizing the pulverized product at a temperature equal to or higher than the thermal curing initiation temperature of the bismaleimide resin;
[0011] In the method for producing a resin molded product of the present invention, it is preferable that: 1. in the pre-curing step, the impregnated product is held at a temperature range of 160 to 180°C for 15 to 70 minutes; 2. the shaping step is performed by compression molding; and 3. the content of the pitch-based carbon fiber is 17 to 43 parts by mass relative to 100 parts by mass of the bismaleimide-based resin.
[0012] In the resin molded article of the present invention, by using a bismaleimide resin as the matrix resin, it is possible to obtain excellent shape stability, heat resistance, mechanical strength, and sliding performance comparable to those obtained when an addition reaction type polyimide resin is used. Furthermore, since the curing temperature of the bismaleimide resin is lower than that of the addition reaction type polyimide resin and high heat resistance is not required for the molding equipment, it is possible to reduce equipment costs. It is also possible to reduce the energy costs required for molding. Furthermore, by containing pitch-based carbon fiber in the above range, the resin molded article of the present invention can reduce the amount of wear in a sliding wear test. This, combined with the resin molded article having excellent shape stability without distortion such as warping, makes it suitable for use as a sliding member with excellent durability. Furthermore, in the method for producing a resin molded body of the present invention, the bismaleimide resin is crosslinked and cured to an appropriate extent in a pre-curing step prior to the shaping step, forming a pre-cured product in which the carbon fibers are uniformly present in the matrix resin without settling, and in the shaping step, the carbon fibers are crosslinked and cured while maintaining this dispersed state, and shaping is then performed.This makes it possible to mold resin molded bodies with excellent shape stability, in which the carbon fibers are uniformly dispersed and free of distortion such as warping, with good yield.
[0013] 1A is a diagram illustrating a measurement position of the amount of warpage t of a resin molded body, and FIG. 1B is a diagram illustrating a longest dimension in a planar direction of the resin molded body.
[0014] (Bismaleimide Resin) The bismaleimide resin used as the matrix resin of the resin molded article of the present invention is excellent in properties such as heat resistance, mechanical strength, and sliding performance, similar to addition reaction polyimide resins, while having a lower curing temperature than addition reaction polyimide resins, making it possible to reduce the molding temperature compared to when addition reaction polyimide resins are used, and as mentioned above, is also excellent in terms of economy. As the bismaleimide resin used in the present invention, it is preferable to use a bismaleimide compound having at least two maleimide groups in the molecule.
[0015] Examples of bismaleimide compounds include, but are not limited to, bismaleimide compounds having two maleimide groups in the molecule, such as 4,4'-diphenylmethane bismaleimide, m-phenylene bismaleimide, p-phenylene bismaleimide, 2,2-bis[4-(4-maleimidophenoxy)phenyl]propane, bis-(3-ethyl-5-methyl-4-maleimidophenyl)methane, 4-methyl-1,3-phenylene bismaleimide, N,N'-ethylene dimaleimide, N,N'-hexamethylene dimaleimide, bis(4-maleimidophenyl)ether, bis(4-maleimidophenyl)sulfone, 3,3-dimethyl-5,5-diethyl-4,4-diphenylmethane bismaleimide, and bisphenol A diphenyl ether bismaleimide; as well as polymaleimide compounds having three or more maleimide groups in the molecule, such as biphenylaralkyl maleimide and polyphenylmethane maleimide. In the present invention, polymaleimide compounds such as polyphenylmethanemaleimide can be particularly suitably used.
[0016] The bismaleimide resin used in the present invention may contain other thermosetting resins, curing agents, etc., as needed, along with the bismaleimide compound, thereby allowing adjustment of the mechanical strength, heat resistance, etc., of the resin molded product. Examples of such thermosetting resins include those conventionally used in bismaleimide resins, including, but not limited to, epoxy resins, polyimide resins, phenolic resins, and benzoxazine compounds. In the present invention, it is particularly preferred that the resin contains an epoxy resin and a benzoxazine compound. The epoxy resin is preferably contained in an amount of 5 to 100 parts by weight per 100 parts by weight of the bismaleimide compound, and the benzoxazine compound is preferably contained in an amount of 10 to 100 parts by weight per 100 parts by weight of the bismaleimide compound. An example of such a bismaleimide resin is HR3070 manufactured by Printec Co., Ltd.
[0017] [Carbon Fiber] In the present invention, the carbon fibers dispersed in the bismaleimide-based resin described above are preferably pitch-based carbon fibers (hereinafter sometimes simply referred to as "carbon fibers"). In particular, mesophase pitch-based carbon fibers are preferably used. Compared to PAN-based carbon fibers, pitch-based carbon fibers have a higher elastic modulus and superior wear resistance, making them particularly advantageous when resin molded articles are used as sliding members. Carbon fibers having an average fiber length of 50 to 6,000 μm and an average fiber diameter of 5 to 20 μm are preferably used. If the average fiber length is shorter than the above range, the carbon fiber's effectiveness as a reinforcing material cannot be fully achieved. On the other hand, if the average fiber length is longer than the above range, the carbon fiber's dispersibility in the bismaleimide-based resin becomes poor. Furthermore, if the average fiber diameter is smaller than the above range, the carbon fiber is difficult to handle and expensive. On the other hand, if the average fiber diameter is larger than the above range, the sedimentation rate of the carbon fiber increases, which may lead to uneven distribution of the carbon fiber and a decrease in the strength of the carbon fiber, which may result in an insufficient effect as a reinforcing material.
[0018] The carbon fiber content has a significant effect on the sliding performance of the resin molded body and the occurrence of warpage during molding. In the present invention, the carbon fiber content is 17 to 43 parts by mass, particularly 25 to 33 parts by mass, per 100 parts by mass of the bismaleimide resin. This is preferable for obtaining a molded body that has excellent wear resistance, excellent sliding performance over a long period of time, and excellent shape stability without warpage. That is, not only when the pitch-based carbon fiber content is low, but also when it is high, the wear resistance is lower than when the carbon fiber content is within the above range. Furthermore, if the carbon fiber content is lower than the above range, the occurrence of warpage of the resin molded body may increase. On the other hand, if the carbon fiber content is higher than the above range, excessive viscosity may occur, making it impossible to shape the molded body.
[0019] In the present invention, the composition may further contain at least one inorganic material, such as fine carbon materials (e.g., graphite, PTFE, molybdenum disulfide, carbon black), or metal powders (e.g., aluminum powder, copper powder), in addition to the carbon fibers. The inorganic material is preferably contained in an amount of 5 to 40 parts by mass, particularly 5 to 30 parts by mass, per 100 parts by mass of the bismaleimide resin. If the amount of inorganic material is less than the above range, the effects of blending the inorganic material cannot be fully achieved. On the other hand, if the amount of inorganic material is greater than the above range, the coefficient of friction may increase, wear resistance may decrease, or sliding performance may be impaired.
[0020] (Method for producing resin molded body) The method for producing a resin molded body of the present invention includes an impregnation step of mixing a prepolymer of a bismaleimide resin with pitch-based carbon fiber, maintaining the mixture at a temperature equal to or higher than the melting point and equal to or lower than the viscosity initiation temperature of the bismaleimide resin, and impregnating the pitch-based carbon fiber with the bismaleimide resin; an impregnated product is maintained at a temperature equal to or higher than the viscosity initiation temperature of the bismaleimide resin, and 0.5 g of the pulverized product thus obtained is pressed into a φ12 mm tablet, which is placed between parallel flat plates on the pressure axis, heated to 120°C under a load of 60 N and maintained for 3 minutes, and then heated to 160°C and maintained for 5 minutes, and the area of the impregnated product is 200 to 2000 mm 2the pre-curing step of increasing the viscosity of the impregnated product to the temperature below the initiation temperature of thermal curing of the bismaleimide resin; the step of pulverizing and mixing the pre-cured product; and the step of shaping the pulverized product at a temperature equal to or higher than the initiation temperature of thermal curing of the bismaleimide resin.
[0021] The viscosity increase onset temperature is defined as follows. Using a parallel plate rheometer, the temperature is raised at 4°C / min at an angular frequency of 100 rad / s. After reaching a predetermined target temperature, the target temperature is maintained for a certain period of time, and the viscosity of the unreacted bismaleimide resin is measured under these conditions. The temperature increases, causing the resin to melt and decrease in viscosity. The lowest viscosity during measurement is defined as the minimum melt viscosity, and the melt viscosity is measured for 120 minutes after reaching the target temperature. The target temperatures are set in multiples of 5, from low to high, and the melt viscosity is measured for each temperature. The time at which the minimum melt viscosity is measured is set to 0 minutes, and the horizontal axis is time (min) and the vertical axis is melt viscosity (Pa s). The exponential approximation is calculated using spreadsheet software. The viscosity increase onset temperature is determined by the temperature at which the value of B in the approximation formula (1) first exceeds 0.041: Y = Aexp(Bx) (1), where Y is melt viscosity (Pa s), x is time (min), and A and B are constants.
[0022] Since bismaleimide resins have low viscosity in the prepolymer state before crosslinking and curing, if the viscosity is not increased in the shaping step, the carbon fibers will settle, resulting in an inhomogeneous dispersion of the carbon fibers in the prepolymer, which may result in warping of the resulting resin molded product. On the other hand, if the viscosity of the prepolymer is increased in the shaping step of the resin molded product, the prepolymer will thermally decompose, foam, and expand. The subsequent pressure application in compression molding causes the bubbles to collapse, causing the resin to flow and orienting the carbon fibers, resulting in warping of the resin molded product. In the present invention, after the impregnation step, the viscosity of the impregnated product is increased in the pre-curing step. 0.5 g of pulverized material of the impregnated product is pressed into a φ12 mm tablet, which is then placed between parallel plates on the pressure axis. The tablet is heated to 120°C under a load of 60 N and maintained for 3 minutes, and then heated to 160°C and maintained for 5 minutes. The area of the impregnated product is 200 to 2000 mm. 2By pre-curing the carbon fibers as described below, the carbon fibers are maintained in a uniformly dispersed state, complete curing is not required in the shaping process, and a molded body can be formed in which the carbon fibers are uniformly dispersed and shrink evenly, resulting in no warping.
[0023] [Impregnation Step] In the impregnation step, a bismaleimide resin prepolymer is first mixed with carbon fiber, and the mixture is then held at a temperature above the melting point and below the viscosity increase onset temperature of the bismaleimide resin prepolymer, specifically, at a temperature range of 5 to 20°C lower than the viscosity increase onset temperature, for a certain period of time, thereby melting the prepolymer and impregnating it into the carbon fiber. As described above, the carbon fiber is used in an amount of 17 to 43 parts by mass, particularly 25 to 33 parts by mass, per 100 parts by mass of the bismaleimide resin. The inorganic materials described above can also be blended in the amounts described above. The prepolymer and carbon fiber can be mixed using a conventional mixer such as a Henschel mixer, a tumbler mixer, or a ribbon blender. However, because it is important to prevent breakage of the carbon fiber and disperse it, a batch-type pressure kneader is particularly preferred.
[0024] [Preliminary Curing Step] In the preliminary curing step, it is important to partially crosslink and cure the prepolymer to a desired viscosity range without completely crosslinking and curing it by holding the impregnated product, obtained by impregnating the carbon fiber with the prepolymer that has undergone the above-mentioned impregnation step, for a certain period of time at a temperature equal to or higher than the viscosity increase onset temperature of the bismaleimide resin. Specifically, by holding the temperature at a temperature range 30 to 50°C higher than the viscosity increase onset temperature for 19 to 93 minutes, 0.5 g of pulverized material of the impregnated product is pressed into a φ12 mm tablet, which is placed between parallel flat plates on the pressure axis, heated to 120°C under a load of 60 N and held for 3 minutes, and then heated to 160°C and held for 5 minutes, so that the area of the impregnated product is 200 to 2000 mm 2A pre-cured product is obtained by crosslinking and curing as follows. Note that although the pre-curing conditions vary depending on the type of bismaleimide resin used, by ensuring that the viscosity of the bismaleimide resin in the impregnated product is within the above range, sedimentation of the carbon fibers is prevented, making it possible to form a pre-cured product in which the carbon fibers are uniformly dispersed. Specifically, as shown in the examples described below, for bismaleimide resins whose main component is polyphenylmethane maleimide, it is preferable to hold the resin at a temperature in the range of 160 to 180°C for 15 to 70 minutes.
[0025] [Pulverization Step] The pre-cured product obtained by cooling (including natural cooling) and solidifying after the pre-curing step is a bulk mold compound (BMC) in the form of chunks of a predetermined size in which the carbon fibers are uniformly dispersed in the prepolymer. Therefore, it is possible to store the BMC in this state over time, but it is also possible to pulverize and mix the BMC using a pulverizer such as a roll mill or grinder to produce a powder having a particle size of 0.1 to 1000 μm.
[0026] [Shaping step] The powdery pre-cured product pulverized in the pulverization step is introduced into a mold, and, if necessary, in a slightly melted state in the mold, is shaped at a temperature equal to or higher than the thermosetting initiation temperature of the bismaleimide resin used, to form a desired resin molded product. In this case, in the present invention, the viscosity of the mixture of bismaleimide resin and pitch-based carbon fiber is such that 0.5 g of the pulverized mixture is pressed into a φ12 mm tablet, which is placed between parallel flat plates on the pressure axis, heated to 120°C under a load of 60 N and held for 3 minutes, and then heated to 160°C and held for 5 minutes, so that the area of the impregnated product is 200 to 2000 mm. 2Since the resin is pre-cured to the following temperature range, even when compressed under pressure by compression molding or the like, the flow of the resin is reduced and the orientation of the carbon fibers is also reduced, effectively suppressing the occurrence of warping due to heat curing. Furthermore, since pressure is applied from the room temperature stage before heating, uniform heating during heat compression is achieved, the curing reaction proceeds uniformly, and the occurrence of residual stress and strain is reduced, thereby suppressing the occurrence of warping. Specifically, for the bismaleimide resin containing polyphenylmethane maleimide as the main component used in the examples described below, it is preferable to hold a pre-cured product having a viscosity within the above range at a temperature range of 230 to 250°C for 60 to 240 minutes to form it. Note that shaping is preferably performed by compression molding or transfer molding, in which a mixture introduced into a mold is compressed under pressure to form it, but molding can also be performed by injection molding or extrusion molding.
[0027] (Resin Molded Article) As described above, the resin molded article of the present invention, which is obtained by undergoing the preliminary curing process and then molding in the shaping process, has a bismaleimide resin matrix in which pitch-based carbon fibers are uniformly dispersed, and has little distortion such as warping. This can be expressed by the following formula (2): R(%) = (t / D) × 100 ... (2), where t represents the amount of warping t (mm) of the resin molded article as shown in FIG. 1(A), and D represents the dimension D (mm) of the longest part in the planar direction of the resin molded article as shown in FIG. 1(B). The resin molded article of the present invention, in which the ratio of the amount of warping of the resin molded article to the longest part in the planar direction, as shown by R(%), to the longest part in the planar direction, is less than 0.25%, effectively prevents warping, and therefore has good yield, excellent productivity, and excellent economy. It can be molded into shapes suitable for various applications, such as disks and rings. It also has excellent heat resistance, durability, and mechanical strength, as well as excellent sliding performance.
[0028] (Melt Viscosity Measurement of Pre-Cured Product) The melt viscosity of the pre-cured product of bismaleimide resin and pitch-based carbon fiber was confirmed by measuring the area of the fluid obtained by holding a certain amount of pre-cured product between parallel plates under desired pressure and temperature conditions for a certain period of time. 0.5 g of the pulverized pre-cured product was pressed into a φ12 mm tablet. The tablet was placed between parallel plates so that it was on the pressure axis. The mixture was heated to 120°C under a load of 60 N and held for 3 minutes, then heated to 160°C and held for 5 minutes, after which it was rapidly cooled and the fluidized mixture was removed. The fluidized mixture was photographed, and the area was measured using software (ImageJ). The pass / fail criteria were the absence of leakage or bubble inclusions during molding, and a warpage / diameter ratio [%] of less than 0.25.
[0029] (Measurement of Viscosity Initiation Temperature) The viscosity initiation temperature was measured using a rheometer. Under the temperature conditions of a rate of reaching the target temperature of 4°C / min and a temperature retention time of 120 minutes after reaching the target temperature, the melt viscosity was measured using parallel plates at an angular frequency of 100 rad / s and a strain of 10%. The time showing the minimum melt viscosity was set to 0 minutes, and the values were plotted on a semi-logarithmic graph with the horizontal axis representing time (min) and the vertical axis representing melt viscosity (Pa s). The coefficient B of the formula (1) was calculated using an exponential approximation equation. For a bismaleimide resin (HR3070 manufactured by Printec Co., Ltd.), the B value was 0.033 when the target temperature was 125°C, and the B value was 0.0413 when the target temperature was 130°C, and the viscosity initiation temperature was determined to be 130°C.
[0030] (Measurement of Wear Volume) Using a thrust type wear tester (friction wear tester EFM-III-F manufactured by A&D Co., Ltd.) conforming to JIS K 7218 (sliding wear test method for plastics), a sliding wear test was performed using the ring-on-disk method as shown in FIG. 2 under the conditions of a load (W) of 300 N, a speed of 0.5 m / s, a sliding distance (L) of 108 km (test time 60 hours), and a mating material S45C (surface roughness Ra = 0.8 μm). The cross-sectional area S of the groove of the test piece was measured using a three-dimensional contour measuring instrument (Surfcom 2000SD3 manufactured by Tokyo Seimitsu Co., Ltd.), and the wear volume V was calculated from the following formula (3): V = 2πg x s...(3) In the formula, g xrepresents the midpoint between the outer and inner ring diameters.
[0031] (Example 1) 100 parts by mass of bismaleimide resin (HR3070 manufactured by Printec Co., Ltd.) was mixed with 17.6 parts by mass of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics Co., Ltd.) having an average fiber length of 200 μm, dry blended, and held at 120 ° C. for 20 minutes in an electric furnace, followed by 160 ° C. for 70 minutes. Then, the mixture was quenched and cooled to room temperature to obtain a mixture (bulk molding compound, hereinafter referred to as BMC). The obtained BMC was pulverized and mixed in a pulverizer and then fed into a compression molding mold. At room temperature, the temperature was increased to 150 ° C. at a rate of 4.3 ° C. / min while pressurizing to 3.0 MPa, and then the temperature was increased to 230 ° C. at 2.7 ° C. / min. The temperature was held for 10 minutes, and then slowly cooled to obtain a plate having a diameter of 200 mm and a thickness of 3 mm.
[0032] Example 2 The same procedure as in Example 1 was repeated except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 25 parts by mass and the holding time at 160° C. was changed to 60 minutes.
[0033] Example 3 The same procedure as in Example 2 was carried out except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 33.3 parts by mass.
[0034] Example 4 The procedure was the same as Example 2, except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 42.9 parts by mass.
[0035] Example 5 The same procedure as in Example 1 was repeated except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 42.9 parts by mass and the holding time at 160° C. was changed to 50 minutes.
[0036] Example 6 The same procedure as in Example 1 was repeated except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 42.9 parts by mass.
[0037] Comparative Example 1 The procedure was the same as in Example 1, except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 11.1 parts by mass.
[0038] Comparative Example 2 The procedure was the same as Example 1, except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 66.7 parts by mass, and the holding time at 160° C. was changed to 50 minutes.
[0039] Comparative Example 3 The procedure was the same as Example 1, except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 42.9 parts by mass, and the holding time at 160° C. was changed to 40 minutes.
[0040] Comparative Example 4 was the same as Example 1, except that the blending amount of mesophase pitch-based carbon fiber (K223HM manufactured by Mitsubishi Plastics) having an average fiber length of 200 μm was changed to 42.9 parts by mass and the holding time at 160° C. was changed to 80 minutes. Furthermore, the resin viscosity was high, and voids occurred in the resin molded body.
[0041] The results of evaluation of the wear volume, warpage / diameter ratio, and formability of the resin molded articles obtained in Examples 1 to 6 and Comparative Examples 1 to 4 are shown in Tables 1 and 2. In the tables, the wear volume of the resin molded article was 29 mm 3 If it is less than 29 mm, mark it as "〇" 3 A warpage / diameter ratio of less than 0.25% is indicated by "Good", and a warpage / diameter ratio of 0.25% or more is indicated by "Poor".
[0042]
[0043]
[0044] The resin molded article of the present invention has excellent heat resistance, durability, mechanical strength, and sliding performance equivalent to those of resin molded articles made using addition-reaction polyimide resins that have been suitably used in applications such as sliding members, and therefore can be used in a variety of applications such as sliding members in the automotive, electrical, and electronic fields. Furthermore, since the curing temperature of the bismaleimide resin used as the matrix resin is lower than that of addition-reaction polyimide resins, high heat resistance is not required in the molding equipment, which is advantageous in terms of energy costs, and the resin molded article can also be suitably used in sliding members that require high economic efficiency.
Claims
1. A resin molding comprising a bismaleimide resin containing pitch-based carbon fiber.
2. The resin molding according to claim 1, wherein the pitch-based carbon fiber is contained in an amount ranging from 17 to 43 parts by mass per 100 parts by mass of the bismaleimide-based resin.
3. A resin molding according to claim 1 or 2, in which the ratio of the amount of warping t (mm) of the resin molding to the longest dimension D (mm) of the resin molding in the planar direction {(t / D) x 100} is less than 0.25%.
4. The resin molding according to claim 1 or 2, wherein the pitch-based carbon fibers have an average fiber length in the range of 50 to 6000 μm and an average fiber diameter in the range of 5 to 20 μm.
5. The resin molding according to claim 1 or 2, wherein the pitch-based carbon fiber is a mesophase type pitch-based carbon fiber.
6. An impregnation process in which a bismaleimide resin prepolymer is mixed with pitch-based carbon fiber, the mixture is maintained at a temperature above the melting point of the bismaleimide resin and below the viscosity increase starting temperature, and the pitch-based carbon fiber is impregnated with the bismaleimide resin; the impregnated product is maintained at a temperature above the viscosity increase starting temperature of the bismaleimide resin, and 0.5 g of the pulverized product obtained is pressed into a tablet of φ12 mm, which is placed between parallel flat plates on the pressure axis, heated to 120° C. under a load of 60 N and maintained for 3 minutes, and then heated to 160° C. and maintained for 5 minutes, and the area of the impregnated product is 200 to 2000 mm 2 a pre-curing step of increasing the viscosity of the impregnated product to a viscosity of at least 1000° C. or less, a pulverizing and mixing step of the pre-cured product, and a shaping step of shaping the pulverized product at a temperature condition equal to or higher than a thermal curing initiation temperature of the bismaleimide resin.
7. The method for producing a resin molded article according to claim 6, wherein in the pre-curing step, the impregnated material is held at a temperature in the range of 160 to 180° C. for 15 to 70 minutes.
8. The method for producing a resin molded article according to claim 6 or 7, wherein the shaping step is performed by compression molding.
9. The method for producing a resin molded article according to claim 6 or 7, wherein the content of said pitch-based carbon fiber is 17 to 43 parts by mass per 100 parts by mass of said bismaleimide-based resin.
Citation Information
Patent Citations
Pitch-based carbon fiber composite material with heat-conducting interface as well as preparation method and application thereof
CN115838526A
Composition for molding sliding material
JP1983001747A
Prepreg
JP1996127663A
Synthetic resin-made seal ring
JP1998061777A
Member for conveyance made of fiber-reinforced composite material having resistance to ultraviolet light, and manufacturing method therefor
JP2001322198A