Electret nonwoven fabric, method for producing same, filter material, and air filter
The electret nonwoven fabric with strategically incorporated metal compounds addresses the dual challenge of antiviral and collection performance by optimizing metal distribution, achieving effective virus capture and particle collection with balanced efficiency and pressure loss.
Patent Information
- Application Number
- PCT/JP2024/011579
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing electret nonwoven fabrics face challenges in achieving both high antiviral performance and high collection performance, as antiviral agents applied to the fibers can impede particle collection due to surface coverage, particularly in electret fabrics with electrically charged fibers.
An electret nonwoven fabric composed of thermoplastic resin fibers with specific metal compounds (copper, cobalt, aluminum, nickel, zinc, palladium, molybdenum, and tungsten) within specific mass and area ratios, ensuring both antiviral and collection efficiencies are enhanced by optimizing the distribution and proportion of these metals on the fabric surface.
The fabric achieves high antiviral performance while maintaining high collection efficiency, effectively capturing particles and viruses without compromising on pressure loss or charging performance.
Smart Images

Figure JP2024011579_03102024_PF_FP_ABST
Abstract
Description
Electret nonwoven fabric, its manufacturing method, filter medium, and air filter
[0001] The present invention relates to an electret nonwoven fabric.
[0002] In recent years, growing interest in environmental hygiene, influenza epidemics, and the outbreak of new infectious diseases such as coronavirus infections have led to the active development of various antiviral materials and antiviral articles using such materials. Among these, various articles using antiviral nonwoven fabrics have been proposed because of their low cost and ease of processing.
[0003] In particular, it has long been known that certain metal ions have antiviral activity, and inorganic antiviral agents using these metal ions are not prone to volatilization or decomposition, and therefore not only are they highly safe, but also have properties such as long-lasting antiviral activity and excellent heat resistance.
[0004] As such a technique, for example, Patent Document 1 proposes a filter containing an inorganic antiviral agent, which comprises a porous inorganic powder having countless micropores on its surface and a monovalent copper compound supported on at least one of the surface of the porous inorganic powder and the inside of the countless micropores.It is described that this can provide a component using an inorganic antiviral agent that can quickly adsorb and inactivate viruses floating in the air or water.In addition, Patent Document 2 proposes a filter medium in which a thin film layer of a functional agent is dispersed between the fibers of the outermost layer of a nonwoven fabric on at least one side of a charge-retentive nonwoven fabric having a specific range of air permeability, and the area ratio of the thin film layer of the functional agent in the outermost layer of the nonwoven fabric is within a specific range.It is described that this can provide a filter medium that has high filter medium properties (high collection efficiency and low pressure loss) together with electret performance, and at least one of antiallergenic, antibacterial, antiviral, and fungal resistance.
[0005] JP 2011-178720 A JP 2013-121556 A
[0006] As proposed in Patent Documents 1 and 2 above, it is possible to impart a certain degree of antiviral performance to a nonwoven fabric by attaching or applying a chemical containing an antiviral agent to the nonwoven fabric. However, simply attaching or applying an antiviral agent to a nonwoven fabric results in the agent covering the fiber surface, preventing contact between the target particles and the fibers. This can hinder the capture of target particles when used as a component of a filter. This effect is particularly pronounced in the case of electret nonwoven fabrics in which the fiber surfaces have been subjected to an electrostatic charging process, making it difficult to achieve both antiviral performance and high collection performance (high collection efficiency and low pressure loss).
[0007] Even if a layer with antiviral properties and a layer with high collection performance are laminated separately and used as a component of a filter, droplet nuclei containing viruses will be mainly captured on the layer with high collection performance, and the current situation is that sufficient antiviral performance cannot be obtained as a filter.
[0008] Therefore, an object of the present invention is to address the above-mentioned problems and to provide an electret nonwoven fabric that combines high antiviral performance and high collection performance.
[0009] As a result of extensive research to achieve the above object, the inventors have discovered that the antiviral performance and collection performance of an electret nonwoven fabric can both be increased to high levels by including particles containing specific metal atoms and by having the specific metal atoms present at a specific area ratio on the surface of the electret nonwoven fabric.
[0010] The present invention has been completed based on these findings, and provides the following inventions.
[0011] [1] An electret nonwoven fabric composed of fibers made of a thermoplastic resin, wherein the fibers have an average fiber diameter of 0.1 μm or more and 30.0 μm or less, and the electret nonwoven fabric contains one or more inorganic particles containing one or more selected from the group consisting of copper compounds, cobalt compounds, aluminum compounds, nickel compounds, zinc compounds, palladium compounds, molybdenum compounds, and tungsten compounds, and the electret nonwoven fabric satisfies the following formulas (1) and (2).
[0012] 0.01≦a Cu +a Co +a Al +a Ni +a Zn +a Pd +a Mo +a W ≦0.50 (1) 40≦S Cu +S Co +S Al +S Ni +S Zn +S Pd +S Mo +S W ≦60 (2) where a Cu , a Co , a Al , a Ni , a Zn , a Pd , a Mo , a W are the mass proportions (mass%) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms in the electret nonwoven fabric, respectively, and S Cu , S Co , S Al , S Ni , S Zn , S Pd , S Mo , S W are the area percentages (area %) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms measured and calculated by SEM-EDX analysis of the surface of the electret nonwoven fabric.
[0013] [2] The electret nonwoven fabric according to [1], wherein the electret nonwoven fabric is a melt-blown nonwoven fabric.
[0014] [3] The electret nonwoven fabric according to [1] or [2], wherein the thermoplastic resin is a polyolefin resin.
[0015] [4] The electret nonwoven fabric according to [3], wherein the thermoplastic resin is a polypropylene-based resin.
[0016] [5] The electret nonwoven fabric according to any one of [1] to [4], wherein the content of the hindered amine compound in the thermoplastic resin is 0.1% by mass or more and 5.0% by mass or less.
[0017] [6] A filter medium using the electret nonwoven fabric according to any one of [1] to [5].
[0018] [7] An air filter using the filter medium according to [6] above.
[0019] [8] A method for producing an electret nonwoven fabric according to any one of [1] to [5] above, comprising the steps of: melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; collecting the spun yarn with a collecting device below to obtain a fiber web; and electretizing the fiber web.
[0020] [9] A method for producing an electret nonwoven fabric according to any one of [1] to [5] above, comprising: a step of melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; a step of spraying water onto the spun yarn between the spinneret and a collecting device to obtain an electret spun yarn; and a step of collecting the electret spun yarn in a collecting device below.
[0021] According to the present invention, an electret nonwoven fabric that combines high antiviral performance and high collection performance can be obtained.
[0022] FIG. 2 is a schematic side view showing an example of a measurement device for collection efficiency and pressure loss.
[0023] The electret nonwoven fabric of the present invention is an electret nonwoven fabric composed of fibers made of a thermoplastic resin, wherein the fibers have an average fiber diameter of 0.1 μm or more and 30.0 μm or less, and the electret nonwoven fabric contains one or more inorganic particles containing one or more compounds selected from the group consisting of copper compounds, cobalt compounds, aluminum compounds, nickel compounds, zinc compounds, palladium compounds, molybdenum compounds, and tungsten compounds, and the following formulas (1) and (2) are satisfied: 0.01≦a Cu +a Co +a Al +a Ni +a Zn +a Pd +a Mo +a W ≦0.50 (1) 40≦S Cu +S Co +S Al +S Ni +S Zn +S Pd +S Mo +S W ≦60 (2) where a Cu , a Co , a Al , a Ni , a Zn , a Pd , a Mo , a W are the mass percentages (mass%) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms (hereinafter sometimes referred to as specific metal atoms) in the electret nonwoven fabric, and S Cu , S Co , S Al , S Ni , S Zn , S Pd , S Mo , S W are the area percentages (area %) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms on the surface of the electret nonwoven fabric, respectively.
[0024] The components will be described in detail below, but the present invention is not limited to the scope of the following description as long as it does not deviate from the gist of the present invention.
[0025] [Thermoplastic Resin] First, the electret nonwoven fabric of the present invention is made of fibers made of a thermoplastic resin.
[0026] In the present invention, examples of thermoplastic resins include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate and polylactic acid, polycarbonate resins, polystyrene resins, polyphenylene sulfide resins, fluorine-containing resins, elastomers such as polystyrene elastomers, polyolefin elastomers, polyester elastomers, polyamide elastomers and polyurethane elastomers, etc. Furthermore, copolymers in which different components are copolymerized with these homopolymers, and resins such as blends of two or more different polymers can also be used.
[0027] Among these, polyolefin resins are preferred, and polypropylene resins are more preferred, because they have high volume resistivity and excellent chargeability and charge retention properties when electretized, resulting in an electret nonwoven fabric with high collection efficiency.
[0028] The thermoplastic resin used in the electret nonwoven fabric of the present invention preferably has a melt flow rate (MFR) of 50 g / 10 min or more and 2500 g / 10 min or less, measured at a temperature of 230°C, a load of 2.16 kg, and a measurement time of 10 minutes in accordance with "8A Method: Mass Measurement" in JIS K7210-1:2014, "Plastics - Determination of Melt Mass Flow Rate (MFR) and Melt Volume Flow Rate (MVR) of Thermoplastic Plastics - Part 1: Standard Test Methods." The melt flow rate of the thermoplastic resin is preferably 200 g / 10 min or more, more preferably 500 g / 10 min or more, so that the constituent fibers become ultrafine fibers, resulting in an electret nonwoven fabric with high collection efficiency. On the other hand, a melt flow rate of the thermoplastic resin is preferably 2000 g / 10 min or less, more preferably 1500 g / 10 min or less, resulting in an electret nonwoven fabric with excellent strength.
[0029] The thermoplastic resin used in the present invention may contain additives such as heat stabilizers, weathering agents, crystal nucleating agents, lubricants, and polymerization inhibitors, as long as the effects of the present invention are not impaired.
[0030] In the present invention, the content of the hindered amine compound in the thermoplastic resin is preferably 0.1% by mass or more and 5.0% by mass. When the content of the hindered amine compound is 0.1% by mass or more, preferably 0.7% by mass or more, an electret nonwoven fabric having excellent chargeability and charge retention properties is obtained. On the other hand, when the content of the hindered amine compound is 5.0% by mass or less, preferably 3.0% by mass or less, an electret nonwoven fabric having excellent chargeability and charge retention properties is obtained.
[0031] The content of hindered amine compounds refers to a value measured and calculated by the following method: (i) Five 50 mg test pieces are randomly taken from the electret nonwoven fabric. (ii) The test pieces are subjected to Soxhlet extraction with a methanol / chloroform mixed solution, and the extract is repeatedly fractionated by HPLC. Each fraction is subjected to IR measurement, GC measurement, GC / MS measurement, and MALDI-MS measurement. 1 H-NMR measurement, and 13The structure is confirmed by C-NMR measurement. (iii) The masses of the fractions are summed up, and the percentage relative to the total nonwoven fabric is measured and calculated. (iv) Steps (ii) to (iii) are repeated for all test pieces, and the content (mass%) is measured and calculated, and the arithmetic mean value (mass%) is rounded to one decimal place.
[0032] The hindered amine compound used in the present invention is a compound having a structural unit represented by the following general formula (1).
[0033]
[0034] Here, in general formula (1), R 1 represents a hydrogen atom or a methyl group, and * represents a bond.
[0035] Examples of hindered amine compounds having this structure include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (manufactured by BASF Japan Ltd., "Chimassorb" (registered trademark) 944LD), dimethyl succinate- Examples include 1-(2-hydroxyethyl)-4-hydroxy-2,2,6,6-tetramethylpiperidine polycondensate (manufactured by BASF Japan Ltd., "TINUVIN" (registered trademark) 622LD), and bis(1,2,2,6,6-pentamethyl-4-piperidyl) 2-(3,5-di-t-butyl-4-hydroxybenzyl)-2-n-butylmalonate (manufactured by BASF Japan Ltd., "TINUVIN" (registered trademark) 144).
[0036] Furthermore, in the present invention, it is also preferable that the content of the triazine-based compound in the thermoplastic resin is 0.1% by mass or more and 5.0% by mass or less. When the content of the triazine-based compound is 0.1% by mass or more, more preferably 0.7% by mass or more, an electret nonwoven fabric having superior chargeability and charge retention properties is obtained. On the other hand, when the content of the triazine-based compound is 5.0% by mass or less, preferably 3.0% by mass or less, an electret nonwoven fabric having superior chargeability and charge retention properties is obtained.
[0037] In the present invention, the content of the triazine-based compound can be measured and calculated in the same manner as in the case of the hindered amine-based compound.
[0038] The triazine compound used in the present invention is a compound having a triazine ring structure represented by the following general formula (2).
[0039]
[0040] In the general formula (2), * represents a bond.
[0041] Examples of triazine compounds having a triazine ring structure include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (manufactured by BASF Japan Ltd., "Chimassorb" (registered trademark) 944LD), and 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-((hexyl)oxy)-phenol (manufactured by BASF Japan Ltd., "Tinuvin" (registered trademark) 1577FF).
[0042] Among these hindered amine compounds and triazine compounds, it is more preferable to use a compound having both structures of general formulas (1) and (2), that is, the hindered amine compound is also a compound having a triazine ring structure represented by general formula (2), because this allows the amount of compound to be added to the thermoplastic resin to be reduced, and results in an electret nonwoven fabric that is more excellent in chargeability and charge retention properties.
[0043] Examples of such compounds include poly[(6-(1,1,3,3-tetramethylbutyl)imino-1,3,5-triazine-2,4-diyl)((2,2,6,6-tetramethyl-4-piperidyl)imino)hexamethylene((2,2,6,6-tetramethyl-4-piperidyl)imino)] (manufactured by BASF Japan Ltd., "Chimassorb" (registered trademark) 944LD).
[0044] [Fibers] Next, the electret nonwoven fabric of the present invention is composed of fibers made of the thermoplastic resin. The average fiber diameter of these fibers is 0.1 μm or more and 30.0 μm or less. When the average fiber diameter is 0.1 μm or more, preferably 1.0 μm or more, and more preferably 5.0 μm or more, the nonwoven fabric has excellent strength. On the other hand, when the average fiber diameter is 30.0 μm or less, preferably 20.0 μm or less, and more preferably 15.0 μm or less, the fiber surface area of the electret nonwoven fabric is increased, resulting in an electret nonwoven fabric with excellent antiviral performance and collection performance.
[0045] The average fiber diameter of the thermoplastic resin fibers used in the electret nonwoven fabric of the present invention refers to a value measured and calculated by the following method. (i) Measurement samples of 3 mm x 3 mm are taken from three points in the width direction of the electret nonwoven fabric (two side edge points and one central point), plus five points spaced 5 cm apart in the longitudinal direction, for a total of 15 points. (ii) Using a scanning electron microscope (SEM, for example, the "VHX-D500" manufactured by Keyence Corporation) at a magnification of 3000x, one fiber surface photograph is taken from each of the taken measurement samples, for a total of 15 photographs. (iii) The single fiber diameter is measured for fibers whose fiber diameter (single fiber diameter) can be clearly identified in the photograph. (iv) For all measurement samples, (iii) is performed, and the arithmetic mean value (μm) of the single fiber diameters of all fibers is rounded to one decimal place.
[0046] Furthermore, the fibers made of thermoplastic resin may be composite fibers, and may take the form of composite fibers such as core-sheath type, eccentric core-sheath type, side-by-side type, split type, sea-island type, and alloy type.
[0047] [Electret Nonwoven Fabric] The electret nonwoven fabric of the present invention is composed of the above-described fibers. In the present invention, the term "electret nonwoven fabric" refers to an electretized nonwoven fabric. Electretization can be confirmed by exposing the nonwoven fabric to isopropyl alcohol vapor at room temperature (25°C) for 24 hours and measuring the collection efficiency by the method described below. That is, an electret nonwoven fabric charged by electretization is neutralized by exposure to isopropyl alcohol vapor, and therefore, if a decrease in collection efficiency is observed after exposure, it can be determined to be an electret nonwoven fabric.
[0048] Examples of the electret nonwoven fabric include nonwoven fabrics manufactured by combining web formation methods such as a dry method, a wet method, a spunbond method, a melt-blowing method, and an air-laid method with fiber bonding methods such as a chemical bond method, a thermal bond method, a needle punch method, and a spunlace method. Among these, the spunbond method and the melt-blowing method are preferably used because the spinning (forming yarn) step and the fabrication (forming nonwoven fabric) step are continuous, which provides excellent productivity and cost, and because the fabric is made of continuous fibers, which provides excellent strength.
[0049] Among these, the electret nonwoven fabric is preferably a nonwoven fabric obtained by a melt-blowing method, i.e., a melt-blown nonwoven fabric. By using this melt-blown nonwoven fabric, the constituent fibers become ultrafine fibers, resulting in an electret nonwoven fabric with high collection efficiency.
[0050] The electret nonwoven fabric of the present invention contains one or more inorganic particles containing one or more compounds selected from the group consisting of copper compounds, cobalt compounds, aluminum compounds, nickel compounds, zinc compounds, palladium compounds, molybdenum compounds, and tungsten compounds. Specific examples of the above compounds used in the present invention include the following.
[0051] That is, examples of copper compounds include copper(I) hydroxide, copper(II) hydroxide, copper(I) oxide, copper(II) oxide, copper(I) chloride, copper(II) chloride, copper(I) sulfide, copper(II) sulfide, copper(I) iodide, copper(II) iodide, copper(I) fluoride, copper(II) fluoride, copper(I) bromide, and copper(II) bromide.
[0052] Examples of the cobalt compound include cobalt(II) hydroxide, cobalt(II) oxide, cobalt(II, III) oxide, cobalt(II) chloride, and cobalt(II) sulfide.
[0053] Examples of aluminum compounds include aluminum(III) hydroxide, aluminum(III) oxide, aluminum(III) chloride, aluminum(III) iodide, aluminum(III) fluoride, and aluminum(III) bromide.
[0054] Examples of nickel compounds include nickel(II) hydroxide, nickel(II) oxide, nickel(II) chloride, and nickel(II) sulfide.
[0055] Examples of zinc compounds include zinc hydroxide(II), zinc oxide(II), zinc chloride(II), zinc sulfide(II), zinc iodide(II), zinc fluoride(II), and zinc bromide(II).
[0056] Examples of palladium compounds include palladium(II) hydroxide, palladium(II) oxide, palladium(II) chloride, palladium(II) sulfide, palladium(II) iodide, palladium(II) fluoride, and palladium(II) bromide.
[0057] The molybdenum compound may include molybdenum (VI) oxide.
[0058] Examples of tungsten compounds include tungsten (III) oxide, tungsten (IV) oxide, and tungsten (VI) oxide.
[0059] There are various theories about the mechanism of the antiviral properties of these compounds, but it is speculated that the metal ions dissolved in the moisture in the air bind to the lipid membrane or protein membrane of the virus, inhibiting its function and denaturing the protein, and furthermore, generate active oxygen species (hydroxyl radicals, etc.), which promote the denaturation of proteins, etc. Among the above metal compounds, copper compounds or zinc compounds are preferred, and copper iodide, copper sulfide, and zinc oxide are particularly preferred, from the viewpoint of excellent antiviral properties and small influence on charging performance during electretization.
[0060] In addition, the electret nonwoven fabric of the present invention satisfies the following formulas (1) and (2).
[0061] 0.01≦a Cu +a Co +a Al +a Ni +a Zn +a Pd +a Mo +a W ≦0.50 (1) 40≦S Cu +S Co +S Al +S Ni +S Zn +S Pd +S Mo +S W ≦60 (2) where a Cu , a Co , a Al , a Ni , a Zn , a Pd , a Mo , a W are the mass proportions (mass%) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms in the electret nonwoven fabric, respectively, and S Cu , S Co , S Al , S Ni , S Zn , S Pd , S Mo , S Ware the area percentages (area %) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms on the surface of the electret nonwoven fabric, respectively. Satisfying both formulas (1) and (2) results in an electret nonwoven fabric that maintains high collection efficiency and has excellent antiviral properties. Note that formulas (1) and (2) do not mean that all of the above metal atoms are included, but it is sufficient that at least one of the above metal atoms is included.
[0062] First, with respect to formula (1), the total mass proportion (% by mass) of the specific metal atoms in the electret nonwoven fabric is 0.01% by mass or more and 0.50% by mass or less. When the lower limit of this total mass proportion range is 0.01% by mass or more, preferably 0.05% by mass or more, the electret nonwoven fabric has excellent antiviral properties. On the other hand, when the upper limit of the total mass proportion range is 0.50% by mass or less, preferably 0.30% by mass or less, the electret nonwoven fabric has excellent collection efficiency.
[0063] The mass percentage (mass%) of the specific metal atoms in the electret nonwoven fabric can be determined using analytical techniques such as X-ray fluorescence analysis, atomic absorption spectrometry (FLAAS), and inductively coupled plasma-atomic emission spectroscopy (ICP-AES). For example, X-ray fluorescence analysis is a method in which X-rays are irradiated onto a nonwoven fabric and the generated fluorescent X-rays are detected. Since these fluorescent X-rays have an energy specific to the element, qualitative analysis using Mosley's law and quantitative analysis based on the fluorescent X-ray intensity are possible. In quantitative analysis, the relationship between the concentration of the element to be analyzed and the fluorescent X-rays (calibration curve) is created in advance, and an unknown sample is measured based on the results to determine the concentration from the fluorescent X-ray intensity obtained. As a method for adjusting the total mass proportion (mass%) of the specific metal atoms in the electret nonwoven fabric to fall within the above range, for example, the mass proportion (mass%) of the specific metal atoms contained in the inorganic particles is calculated from the atomic weights of the atoms constituting the inorganic particles, and the amount of inorganic particles added may be adjusted so that the total mass proportion (mass%) of the specific metal atoms in the electret nonwoven fabric falls within the range of 0.01 mass% or more and 0.50 mass% or less.
[0064] Next, with regard to formula (2), the total area ratio (area %) of the specific metal atoms on the surface of the electret nonwoven fabric is 40 area % or more and 60 area % or less. When the lower limit of this total area ratio range is 40 area % or more, preferably 45 area % or more, the electret nonwoven fabric has excellent antiviral properties. On the other hand, when the upper limit of the total area ratio range is 60 area % or less, preferably 55 area % or less, the electret nonwoven fabric has excellent collection efficiency.
[0065] The area percentage (area %) of specific metal atoms on the surface of the electret nonwoven fabric refers to a value measured and calculated by the following method. (i) In SEM-EDX analysis, the electret nonwoven fabric is irradiated with an electron beam and the specific X-rays generated are analyzed to identify the constituent elements. In this case, for example, a cold cathode field emission scanning electron microscope "FE-SEM S-4800" manufactured by Hitachi High-Tech Corporation can be used as the observation device, and for example, a "QUANTAX FlatQUAD Xflash 5060FQ" manufactured by BRUKER AXS can be used as the analyzer. (ii) Based on the detected information, element mapping is performed to visualize the metal atoms constituting the inorganic particles in the fibers constituting the electret nonwoven fabric in an image. For example, with the above-mentioned "QUANTAX FlatQUAD Xflash 5060FQ" manufactured by BRUKER AXS, element mapping can be performed by displaying copper atoms in green and zinc atoms in yellow, etc. (iii) The image in which the metal atoms are visualized is binarized using image processing software (for example, "ImageJ"), and the area ratio (area %) of each metal atom on the surface of the electret nonwoven fabric is calculated. When "ImageJ" is used as the image processing software, the binarization process involves converting the captured image into the "Lab" color system, and using the above-mentioned "QUANTAX FlatQUAD Xflash 5060FQ" manufactured by BRUKER AXS, when element mapping is performed in green, the threshold value for the a-axis is set to -40 (green: -60 to achromatic color: 0 to red: +60), and when element mapping is performed in yellow, the threshold value for the b-axis is set to +40 (blue: -60 to achromatic color: 0 to yellow: +60). When other software is used, the binarization process is performed under similar conditions. (iv) The above operations (i) to (iii) are performed on one surface (first surface) of a nonwoven fabric and the other surface (second surface) opposite thereto, respectively, to determine the area ratio (area %) of the specific metal atoms on the surface of the electret nonwoven fabric. In the electret nonwoven fabric that achieves both antiviral properties and collection efficiency, the total area ratio (area %) of the specific metal atoms on both the first surface and the second surface is 40 area % or more and 60 area % or less.
[0066] In the present invention, it is important that the mass proportion (mass%) and area proportion (area%) of the specific metal atoms simultaneously satisfy formula (1) and formula (2). When formula (1) alone is satisfied, if the surface proportion (area%) of the specific metal atoms on the fiber surface is small, the antiviral properties are poor, and when it is large, the collection efficiency is poor. On the other hand, when formula (2) alone is satisfied, if the mass proportion (mass%) of the specific metal atoms is small, the durability of the antiviral properties is poor, and when it is large, the charging performance is reduced due to the discharge action of the metal atoms.
[0067] Furthermore, examples of a method for adjusting the total area ratio (area %) of the specific metal atoms on the surface of the electret nonwoven fabric to fall within the above range include adjusting the content of metal atoms, the average fiber diameter, the spinning temperature, the discharge amount of resin, and the diameter of the discharge holes in the spinneret.
[0068] The electret nonwoven fabric of the present invention has a basis weight of 3 g / m 2 More than 100g / m 2 The basis weight of the electret nonwoven fabric is preferably 3 g / m or less. 2 More preferably, 5 g / m 2 More preferably, 10 g / m 2 By setting the density to 100 g / m or more, the antiviral performance of the electret nonwoven fabric can be improved. 2 More preferably, 80 g / m 2 More preferably 60 g / m or less 2 By setting the thickness as follows, the thickness of the electret nonwoven fabric can be reduced and the processability can be improved.
[0069] The basis weight of the electret nonwoven fabric in the present invention is determined by taking a sample of 15 cm x 15 cm length x width from the electret nonwoven fabric, measuring the mass of the sample, and calculating the value obtained by dividing the mass by 1 m 2 The value is converted to the unit weight per unit area and rounded off to the nearest tenth to obtain the unit weight per unit area of the nonwoven fabric (g / m 2 ) will be calculated.
[0070] The electret nonwoven fabric of the present invention has a bulk density of 0.05 g / cm 30.30g / cm or more 3 The bulk density of the electret nonwoven fabric is preferably 0.05 g / cm or less. 3 More preferably, 0.07 g / cm 3 By satisfying the above conditions, when pleating is performed for use as an air filter, the electret nonwoven fabric can be prevented from bending between the peaks of the peaks and the peaks of the valleys, which would otherwise increase pressure loss. 3 or less, more preferably 0.28 g / cm 3 When the above condition is satisfied, the electret nonwoven fabric has excellent breathability.
[0071] The bulk density of the electret nonwoven fabric in the present invention can be calculated from the basis weight of the electret nonwoven fabric and the thickness described later by the following formula, and the value is rounded to two decimal places to obtain the bulk density (g / cm 3 ) is calculated. Bulk density (g / cm 3 ) = basis weight (g / m 2 ) / (thickness (mm) × 1000) ... (formula).
[0072] The thickness of the electret nonwoven fabric in the present invention is measured at 10 equally spaced points, and the average value is rounded to two decimal places to calculate the thickness (mm) of the nonwoven fabric. As a thickness meter, for example, "TECLOCK (registered trademark) SM-114" manufactured by Teclock Corporation can be used.
[0073] [Method for Producing Electret Nonwoven Fabric] Next, two preferred embodiments of the method for producing the electret nonwoven fabric of the present invention will be exemplified.
[0074] (i) First embodiment This preferred embodiment has the following steps: (ia) a step of melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; (ib) a step of collecting the spun yarn with a collecting device below to obtain a fiber web; and (ic) a step of electretizing the fiber web. In this first embodiment, a fiber web is obtained once and then electretized, and compared to the second embodiment described below, an electret nonwoven fabric having superior strength due to self-fusion of the fibers can be obtained. Further details will be explained below.
[0075] (ia) Step of Obtaining Spun Yarn First, in this step, the molten thermoplastic resin is melt-spun from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn.
[0076] In this step, as a method for preparing a thermoplastic resin containing inorganic particles, inorganic particles may be mixed into a thermoplastic resin while extruding using a twin-screw extruder or the like to prepare thermoplastic resin A, and then thermoplastic resin B may be mixed therewith, or a chip blend may be prepared using a masterbatch and then extruded. When a masterbatch is used, for example, a masterbatch of thermoplastic resin A kneaded with inorganic particles is prepared, and thermoplastic resin B is chip-blended with this and kneaded in an extruder to prepare a polyolefin resin composition containing inorganic particles.
[0077] Next, a method for obtaining spun yarn will be described using the melt-blowing method as an example. In the melt-blowing method, a thermoplastic resin is extruded from a melt-blowing nozzle having a predetermined hole diameter to form a thread. The diameter of the thread is reduced by spraying hot air at a certain angle onto the extrusion. The hole diameter of the melt-blowing nozzle is usually 0.05 mm or more and 1.0 mm or less. The temperature at which the thermoplastic resin is extruded can be adjusted appropriately depending on the type of thermoplastic resin.
[0078] (ib) Step of Obtaining a Fiber Web Next, the spun yarn is collected by a collecting device below to obtain a fiber web.
[0079] In this step, the collector is a device that has a suction device underneath or inside a porous support (e.g., a belt conveyor, a drum, a roll, etc.) and prevents the collected fiber web from being blown away. The surface of the porous support does not need to be flat, and may be three-dimensional, such as curved.
[0080] (ic) Step of Converting a Fiber Web to an Electret In this step, the fiber web obtained in the previous step is converted to an electret. Specifically, the fiber web is immersed in water, passed over a nozzle with a slit, and the water is sucked through the nozzle to penetrate the fiber web, and then dehydrated and dried to obtain an electret nonwoven fabric.
[0081] The water used for electretization is preferably as clean as possible, with dirt removed using a liquid filter or the like. In particular, pure water such as ion-exchanged water, distilled water, and filtered water passed through a reverse osmosis membrane is preferably used. The level of pure water is such that the conductivity is 10 3 It is preferable that the conductivity is 10 μS / m or less, and more preferably 10 2 Pure water with a viscosity of μS / m or less is preferably used. Furthermore, in order to increase the water permeability into the fiber web, a water-soluble organic solvent such as isopropyl alcohol, ethyl alcohol, or acetone can be mixed with the water to the extent that the collection properties are not affected. Furthermore, any conventionally known method can be used to dry the fiber web after water permeation. For example, hot air drying, vacuum drying, natural drying, etc. can be applied. Among these, hot air drying is preferred because it allows continuous processing. In the case of hot air drying, the drying temperature must be set to a temperature that does not deactivate the electret. It is preferably 120°C or less, more preferably 100°C or less, and even more preferably 80°C or less. Furthermore, it is even more preferable to perform pre-drying before hot air drying by removing excess moisture using a nip roll, a water-absorbing roll, suction, or the like.
[0082] (ii) Second embodiment This preferred embodiment has the following steps: (ii-a) A step of melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; (ii-b) A step of spraying water onto the spun yarn between the spinneret and a collector to obtain an electretized spun yarn; and (ii-c) A step of collecting the electretized spun yarn in a collector below, and a step of collecting the electretized spun yarn in a collector below. This second embodiment involves spraying water onto the spun yarn to obtain an electretized spun yarn, which is then formed into a fiber web and an electret nonwoven fabric. Compared to the first embodiment, self-fusion between fibers can be suppressed, making it possible to obtain an electret nonwoven fabric that is bulkier and more breathable. Further details will be explained below.
[0083] (ii-a) Step of Obtaining Spun Yarn This step is the same as the above (ia) step of obtaining spun yarn.
[0084] (ii-b) Step of spraying water to obtain electret spun yarn: In this step, water is sprayed onto the spun yarn between the spinneret and the collector to obtain electret spun yarn. As a droplet spraying device, a single-hole spray nozzle that sprays water droplets in a conical or fan shape from a single hole, or a slit-type spray nozzle that sprays water droplets in a band shape from a slit-shaped outlet can be used. Among these, in terms of being able to uniformly apply even a small amount of water in the width direction, it is more preferable to use a spray nozzle that has multiple water outlets arranged in the width direction and a pair of air outlets that open continuously or intermittently across the width direction and are arranged opposite each other so as to sandwich the multiple water outlets, and that causes air ejected from the air outlet to collide with water ejected from the multiple water outlets.
[0085] The position where the droplets are sprayed or sprayed may be anywhere between the position where the hot air is sprayed and the collection net, but is preferably at a position at least 7.5 cm below the spinneret. More preferably, it is at least 8 cm, and even more preferably, it is at least 9 cm. In the region less than 7.5 cm from the spinneret, the temperature is high due to heat radiation from the spinneret, and the spun yarn itself is also at a high temperature, so some of the sprayed or sprayed water may evaporate. Therefore, by spraying or spraying the droplets at a position at least 7.5 cm below the spinneret, the spun yarn is sufficiently solidified into a yarn, and the sprayed or sprayed droplets can be sufficiently distributed until the yarn is formed into a nonwoven fabric.
[0086] (ii-c) Step of collecting the electretized spun yarn in a lower collecting device. Subsequently, the electretized spun yarn is collected in a lower collecting device. This is substantially the same as the step (ib) of obtaining a fiber web.
[0087] <Other Steps> The sheet that has been subjected to step (ic) or step (ii-c) may be used as an electret nonwoven fabric as is, but it is also preferable to subject the sheet to heat treatment processing such as embossing and pressure bonding, air-through, or pin tentering to form an electret nonwoven fabric with improved shape stability.
[0088] [Filter media, air filters, and other uses] The electret nonwoven fabric of the present invention is preferably used as a filter media in order to take advantage of the high collection efficiency and antiviral properties. In other words, the filter media according to the present invention is preferably made using the electret nonwoven fabric.
[0089] As a method for obtaining the filter medium of the present invention from the electret nonwoven fabric of the present invention, a method in which the electret nonwoven fabric and an aggregate sheet having higher rigidity are bonded together by spraying a moisture-curing urethane resin or the like using a spray method, or a method in which a thermoplastic resin or heat-fusible fiber is sprayed between the electret nonwoven fabric and an aggregate sheet having higher rigidity and then bonded together through a heat path can be used.
[0090] The aggregate sheet is intended to capture relatively large dust particles and to provide the necessary rigidity as a filter medium by being bonded to the electret nonwoven fabric. Examples of the aggregate sheet that can be used include nonwoven fabrics, woven and knitted fabrics, etc. made of polyester fiber, polypropylene fiber, rayon fiber, glass fiber, natural pulp, etc.
[0091] Furthermore, the air filter of the present invention preferably uses the filter medium described above. Specifically, it preferably includes an air filter unit in which the filter medium described above is incorporated into a frame material, or an air filter unit in which the pleated filter medium described above (the filter medium described above pleated with repeated mountain and valley folds) is incorporated into a frame material.
[0092] More preferably, the air filter is an air conditioner filter, an air purifier filter, or an automobile cabin filter. In summary, the electret nonwoven fabric or filter medium of the present invention can be suitably used in air filters for these high-performance applications.
[0093] In addition to the above-mentioned air filters, the composition can also be suitably used in products requiring antiviral properties, such as sanitary materials for disposable diapers, including top sheets, back sheets, and side gathers, as well as incontinence pads, sanitary napkins, and breast pads, and components for medical supplies, including surgical masks, gauze, bandages, medical gowns, and medical drapes.
[0094] The present invention will now be described in detail with reference to examples, although the present invention is not limited to these examples.
[0095] [Measurement Methods] The evaluation methods and measurement conditions used in the examples are described below. In the measurement of each physical property, unless otherwise specified, the measurement and calculation were carried out based on the above-mentioned methods.
[0096] (1) Spinnability: The spinnability of the fiber is 1 m wide x 1 m long (1 m 2The formation of the electret nonwoven fabric was observed, and the nonwoven fabrics were evaluated as follows: those with 0 or more but less than 10 shots (portions where the thermoplastic resin was not in a fibrous state but was in a resin mass); those with 10 or more but less than 30 shots; and those with 30 or more shots.
[0097] (2) Average fiber diameter (μm) of fibers: Measurement and calculation were carried out using a scanning electron microscope (SEM) "VHX-D500" manufactured by Keyence Corporation according to the above-mentioned method.
[0098] (3) Mass ratio (mass%) of specific metal atoms in electret nonwoven fabric: The mass ratio of specific metal atoms in electret nonwoven fabric was calculated assuming that the mass ratio of specific metal atoms contained in the raw material thermoplastic resin is the same as the mass ratio of the electret nonwoven fabric (the mass ratio does not change during the manufacturing process). Note that the mass ratio of the specific metal atoms (a Cu +a Co +a Al +a Ni +a Zn +a Pd +a Mo +a W ) are listed in Tables 1 and 2 as the total mass percentage (mass %) of specific metal atoms.
[0099] (4) Area ratio (area %) of metal atoms on the surface of electret nonwoven fabric: As the observation device for SEM-EDX analysis, a cold cathode field emission scanning electron microscope "FE-SEM S-4800" manufactured by Hitachi High-Tech Corporation was used, as the analyzer, a "QUANTAX FlatQUAD Xflash 5060FQ" manufactured by BRUKER AXS, and "ImageJ" were used as the image processing software. The respective measurement conditions were as follows. Observation equipment (cold cathode field emission scanning electron microscope "FE-SEM S-4800" manufactured by Hitachi High-Tech Corporation) a) Acceleration voltage: 5.0 kV b) Detection signal: secondary electrons c) Pretreatment: carbon deposition on sample Analyzer (BRUKER AXS "QUANTAX FlatQUAD Xflash 5060FQ") Xflash 5060FQ a) Acceleration voltage: 5.0 kV b) Measurement time: 10 min c) Pretreatment: carbon deposition on sample Then, the copper atoms were displayed in green and the zinc atoms in yellow by the analyzer, and the element mapping was carried out in "ImageJ." When the element mapping was in green, the threshold value for the a-axis was set to -40 (green: -60 to achromatic: 0 to red: +60), and when the element mapping was in yellow, the threshold value for the b-axis was set to +40 (blue: -60 to achromatic: 0 to yellow: +60). Measurements and calculations other than these were carried out using the methods described above.
[0100] The above operation was performed on one side (first side) of the nonwoven fabric and the other side (second side) opposite thereto, and each was taken as the area ratio (area %) of the specific metal atoms on the surface of the electret nonwoven fabric. The total area ratio (S Cu +S Co +S Al +S Ni +S Zn +S Pd +S Mo +S W ) are listed in Tables 1 and 2 as the sum of the area percentages (area %) of specific metal atoms.
[0101] (5) Electret nonwoven fabric basis weight (g / m 2 ), thickness (mm), bulk density (g / cm3 ): A "TECLOCK (registered trademark) SM-114" manufactured by Teclock Corporation was used as a thickness gauge, and measurements and calculations were carried out according to the above-mentioned method.
[0102] (6) Pressure loss (Pa), collection efficiency (%), and QF value (Pa) of the electret nonwoven fabric -1 ): The pressure loss, collection efficiency, and QF value of the electret nonwoven fabric were measured and calculated using the following methods. (a) Measurement samples M, each measuring 15 cm x 15 cm in length x width (five samples in total), were collected at five locations across the width of the electret nonwoven fabric. (b) A collection efficiency measurement device, shown in the schematic side view of Figure 1, was prepared. This collection efficiency measurement device has a dust storage box 2 connected upstream of a sample holder 1 in which the measurement sample M is set, and a flow meter 3, a flow control valve 4, and a blower 5 connected downstream. A particle counter 6 is also attached to the sample holder 1, and the number of dust particles on the upstream and downstream sides of the measurement sample M can be measured via a selector cock 7. (c) A 10% aqueous solution of polystyrene particles ("OptiBind", manufactured by ThermoScientific, product number: 9100079710290) was diluted 200 times with distilled water and filled into a dust storage box 2. (d) A measurement sample M was set in a sample holder 1, and the air flow rate was adjusted with a flow control valve 4 so that the air passing through the filter would be 4.5 m / min, and the dust concentration was adjusted to 10,000 particles / 2.83 × 10 -4 m 3 (0.01 ft 3 )~40,000 pieces / 2.83×10 -4 m 3 (0.01 ft 3) and stabilized within the range. (e) The number of dust particles D upstream and the number of dust particles d downstream of measurement sample M were measured three times per measurement sample using a particle counter 6 ("KC-01D" manufactured by Rion Co., Ltd.), and the collection efficiency (%) of 0.3 to 0.5 μm particles was calculated using the following calculation formula based on JIS K0901:1991 "Test methods for shape, dimensions and performance of filter media for collecting dust samples in gas": Collection efficiency (%) = [1 - (d / D)] x 100 ... (formula) (where d represents the total number of downstream dust particles measured three times, and D represents the total number of upstream dust particles measured three times.) (f) Additionally, the static pressure difference between the upstream and downstream of measurement sample M was read using a pressure gauge 8, and the pressure loss (Pa) of measurement sample M was calculated. (g) The average value of the collection efficiency (%) for the five measurement samples M was calculated, and the value obtained by rounding off to the fourth decimal place was designated as the collection efficiency (%) of the electret nonwoven fabric. (h) The average value of the pressure loss (Pa) for the five measurement samples M was calculated, and the value obtained by rounding off to the first decimal place was designated as the pressure loss (Pa) of the electret melt-blown nonwoven fabric. (i) Finally, the QF value (Pa) was calculated as an index of collection performance. -1 ) was calculated using the following formula: QF value (Pa -1 ) = - [ln (1 - (collection efficiency (%)) / 100)] / (pressure loss (Pa)) ... (formula) In addition, the QF value (Pa -1 ) shows the relationship between collection efficiency and pressure loss, and the QF value (Pa -1 ) indicates that the higher the collection efficiency and the lower the pressure loss, that is, the better the collection performance.
[0103] (7) Antiviral activity value of electret nonwoven fabric (-): The antiviral activity value of the electret nonwoven fabric was evaluated under the following conditions in accordance with JIS L1922:2016 “Antiviral test method for textile products”.
[0104] a) Test virus: Influenza A virus (H3N2) b) Host cells: MDCK cells (canine kidney-derived cell line) c) Reaction conditions: 25°C d) Washout solution: SCDLP medium e) Infectivity titer measurement method: Plaque method Note that an antiviral activity value of 3.0 or more, which is the certification standard for the SEK mark, a certification system implemented by the Japan Textile Evaluation Technology Council, a general incorporated association, was evaluated as having antiviral activity.
[0105] Example 1 (a) Step of Obtaining Spun Yarn A thermoplastic resin P was used, which contained polypropylene as the thermoplastic resin, 0.54 mass% of copper (I) iodide particles (particle diameter (primary particle diameter): 5 nm to 1000 nm) as inorganic particles, and 1.0 mass% of "Chimasorb" (registered trademark) 944 (manufactured by BASF Japan Ltd., referred to as "C944" in Tables 1 and 2) as a hindered amine compound. This thermoplastic resin P was charged into the raw material hopper of an extruder, melted and kneaded in the extruder, and then fed to a gear pump. The thermoplastic resin P measured by the gear pump was then sprayed using a die with 0.4 mm diameter nozzles arranged in a straight line by a melt-blowing method under the following conditions: a discharge rate of 27 g / min, a nozzle temperature of 270°C, and an air pressure of 0.17 MPa, to obtain a spun yarn.
[0106] (b) Step of Obtaining a Fiber Web The obtained spun yarn is spun into a fiber web having a basis weight of 20 g / m by adjusting the conveyor speed of the collecting device below. 2 A fiber web of
[0107] (c) Step of converting the fiber web into an electret Next, the obtained fiber web was immersed in water, passed over a nozzle with a slit, and the water was sucked through the nozzle to penetrate the fiber web, and the web was dehydrated and dried to convert it into an electret nonwoven fabric. The obtained electret nonwoven fabric is shown in Table 1.
[0108] [Example 2] (a) In the step of obtaining spun yarn, an electret nonwoven fabric was obtained in the same manner as in Example 1, except that the content of copper iodide particles (I) contained in the thermoplastic resin P was changed from 0.54% by mass to 0.27% by mass. The obtained electret nonwoven fabric is shown in Table 1.
[0109] [Example 3] (a) In the step of obtaining spun yarn, the inorganic particles of the thermoplastic resin P were copper (I) iodide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was 0.54 mass %. However, the inorganic particles were changed to copper (II) sulfide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was changed to 0.60 mass %. An electret nonwoven fabric was obtained in the same manner as in Example 1. The obtained electret nonwoven fabric is shown in Table 1.
[0110] [Example 4] (a) In the step of obtaining spun yarn, the inorganic particles of the thermoplastic resin P were copper (I) iodide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was 0.54 mass %. However, the inorganic particles were changed to zinc (II) oxide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was changed to 0.59 mass %. An electret nonwoven fabric was obtained in the same manner as in Example 1, except that. The obtained electret nonwoven fabric is shown in Table 1.
[0111] [Comparative Example 1] (a) In the step of obtaining spun yarn, an electret nonwoven fabric was obtained in the same manner as in Example 1, except that the content of copper iodide particles (I) contained in the thermoplastic resin P was changed from 0.54% by mass to 0.12% by mass. The obtained electret nonwoven fabric is shown in Table 2.
[0112] [Comparative Example 2] (a) In the step of obtaining spun yarn, an electret nonwoven fabric was obtained in the same manner as in Example 1, except that the content of copper iodide particles (I) contained in the thermoplastic resin P was changed from 0.54% by mass to 1.80% by mass. The obtained electret nonwoven fabric is shown in Table 2.
[0113] [Comparative Example 3] (a) In the step of obtaining spun yarn, an electret nonwoven fabric was obtained in the same manner as in Example 1, except that the content of copper iodide particles (I) in the thermoplastic resin P was changed from 0.54% by mass to 0.21% by mass. The obtained electret nonwoven fabric is shown in Table 2.
[0114] Comparative Example 4 (a) An electret nonwoven fabric was obtained in the same manner as in Example 1, except that the thermoplastic resin P did not contain copper iodide particles (I) in the step of obtaining spun yarn.
[0115] (d) Furthermore, an aqueous solution S in which copper (II) sulfide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) were dispersed in a 58 mass % ethanol aqueous solution was applied to both sides of the obtained electret nonwoven fabric by a spray method.
[0116] (e) The electret nonwoven fabric was dried for 5 minutes at 95° C. using a hot air dryer. The properties of the obtained electret nonwoven fabric are shown in Table 2.
[0117] [Comparative Example 5] (a) In the step of obtaining spun yarn, the inorganic particles of the thermoplastic resin P were copper (I) iodide particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was 0.54 mass %. However, the inorganic particles were changed to silver octadecanoate particles (particle diameter (primary particle diameter): 5 nm or more and 1000 nm or less) and the content was changed to 0.40 mass %. An electret nonwoven fabric was obtained in the same manner as in Example 1, except that. The obtained electret nonwoven fabric is shown in Table 2.
[0118]
[0119]
[0120] As is clear from Table 1, the electret nonwoven fabrics described in Examples 1 to 4 of the present invention achieved high antiviral activity values and high collection performance, and it can be seen that excellent electret nonwoven fabrics that combine antiviral performance and high collection performance were obtained.
[0121] In contrast, as shown in Table 2, the electret nonwoven fabrics described in Comparative Examples 1 and 3, in which the area ratio of metal atoms on the surface of the electret nonwoven fabric was less than 40%, had lower antiviral activity values than the electret nonwoven fabrics described in Examples 1 to 4.
[0122] Next, the electret nonwoven fabric described in Comparative Example 2, in which the area ratio of metal atoms on the surface of the electret nonwoven fabric exceeded 60%, showed lower collection performance than the electret nonwoven fabrics described in Examples 1 to 4.
[0123] Furthermore, the electret nonwoven fabric described in Comparative Example 4, in which the aqueous solution S was applied to the surface of the electret nonwoven fabric, had an area ratio of metal atoms on the surface of the electret nonwoven fabric of more than 60%, and as a result, the collection performance was lower than that of the electret nonwoven fabrics described in Examples 1 to 4.
[0124] Furthermore, the electret nonwoven fabric described in Comparative Example 5, in which the inorganic particles were changed to silver octadecanoate particles, had a lower antiviral activity value than the electret nonwoven fabrics described in Examples 1 to 4.
[0125] 1: Sample holder 2: Dust storage box 3: Flow meter 4: Flow control valve 5: Blower 6: Particle counter 7: Switch cock 8: Pressure gauge M: Measurement sample
Claims
1. An electret nonwoven fabric made of fibers made of a thermoplastic resin, the fibers having an average fiber diameter of 0.1 μm or more and 30.0 μm or less, the electret nonwoven fabric contains one or more inorganic particles containing one or more compounds selected from the group consisting of copper compounds, cobalt compounds, aluminum compounds, nickel compounds, zinc compounds, palladium compounds, molybdenum compounds, and tungsten compounds, and the electret nonwoven fabric satisfies the following formulas (1) and (2). Cu +a Co +a Al +a Ni +a Zn +a Pd +a Mo +a W ≦0.50 (1) 40≦S Cu +S Co +S Al +S Ni +S Zn +S Pd +S Mo +S W ≦60 (2) where a Cu , a Co , a Al , a Ni , a Zn , a Pd , a Mo , a W are the mass percentages (mass%) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms, and tungsten atoms in the electret nonwoven fabric, respectively, and S Cu , S Co , S Al , S Ni , S Zn , S Pd , S Mo , S W are the area percentages (area %) of copper atoms, cobalt atoms, aluminum atoms, nickel atoms, zinc atoms, palladium atoms, molybdenum atoms and tungsten atoms measured and calculated by SEM-EDX analysis of the electret nonwoven fabric surface.
2. The electret nonwoven fabric according to claim 1, wherein the electret nonwoven fabric is a meltblown nonwoven fabric.
3. The electret nonwoven fabric according to claim 1 or 2, wherein the thermoplastic resin is a polyolefin resin.
4. The electret nonwoven fabric according to claim 3, wherein the thermoplastic resin is a polypropylene-based resin.
5. The electret nonwoven fabric according to claim 1 or 2, wherein the content of the hindered amine compound in the thermoplastic resin is 0.1% by mass or more and 5.0% by mass or less.
6. A filter medium comprising the electret nonwoven fabric according to claim 1 or 2.
7. An air filter comprising the filter medium according to claim 6.
8. A method for producing an electret nonwoven fabric according to claim 1 or 2, comprising the steps of: melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; collecting the spun yarn with a collecting device below to obtain a fiber web; and converting the fiber web into an electret.
9. A method for producing an electret nonwoven fabric according to claim 1 or 2, comprising the steps of: melt-spinning the thermoplastic resin from a spinneret having a plurality of spinning holes in the width direction to obtain a spun yarn; spraying water onto the spun yarn between the spinneret and a collecting device to obtain an electret spun yarn; and collecting the electret spun yarn in a collecting device below.
Citation Information
Patent Citations
Antibacterial melt-blown cloth and preparation method thereof
CN112796038A
Antibacterial nonwoven fabric as well as sanitary materials, medical articles, clothing articles and food packaging material which are produced by using antibacterial nonwoven fabric
JP2021116483A
Electret melt-blown non-woven fabric, filter material and air filter obtained using same, and method for producing electret melt-blown non-woven fabric
WO2021149606A1
Electret and electret filter
WO2023095800A1