Carbon fiber sheet, gas diffusion electrode base material, fuel cell, and method for manufacturing carbon fiber sheet

The carbon fiber sheet with a resin and fibrous carbon binding material addresses the challenges of thermal conductivity and gas diffusivity in polymer electrolyte fuel cells, enhancing power generation performance in high current density and high-temperature conditions by optimizing pore size distribution and composition.

WO2024204020A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC

Patent Information

Application Number
PCT/JP2024/011611
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-18
Filing Date
2024-03-25
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing gas diffusion electrode base materials for polymer electrolyte fuel cells face challenges in achieving high thermal conductivity and gas diffusivity, leading to voltage drops and reduced power generation performance, especially in high current density regions and high-temperature conditions.

Method used

A carbon fiber sheet is developed with a binding material containing resin and fibrous carbon, featuring a specific pore size distribution and composition that enhances both thermal conductivity and gas diffusivity, including a pore diameter range of 0.3 μm to 1.0 μm and 20 μm to 100 μm, with a fibrous carbon content of 25% or more, to improve drainage and heat dissipation.

Benefits of technology

The carbon fiber sheet effectively suppresses electrolyte membrane dry-up and maintains high power generation performance in high current density regions and high-temperature environments by ensuring efficient gas diffusion and heat dissipation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a carbon fiber sheet exhibiting high gas diffusibility even in a high current density region while suppressing dry-up of an electrolyte membrane through high thermal conductivity. The present invention pertains to a carbon fiber sheet in which carbon fiber structures are bonded with a binder containing at least a resin and fibrous carbon. The content of the fibrous carbon is 25 mass% or more with respect to 100 mass% of the carbon fiber sheet. In the pore diameter distribution of the carbon fiber sheet, peaks exist at a pore diameter of 0.3-1.0 μm and at a pore diameter of 20-100 μm.
Need to check novelty before this filing date? Find Prior Art

Description

Carbon fiber sheet, gas diffusion electrode substrate, fuel cell, and method for producing carbon fiber sheet

[0001] The present invention relates to a carbon fiber sheet suitable for use in electrodes of fuel cells, particularly polymer electrolyte fuel cells, a method for producing the same, and a gas diffusion electrode substrate and fuel cell using the same.

[0002] The electrodes used in polymer electrolyte fuel cells are sandwiched between two separators in the polymer electrolyte fuel cell and are constructed of a catalyst layer formed on the surface of the electrolyte membrane on both sides and a gas diffusion electrode substrate formed on the outside of this catalyst layer. The performance required of this gas diffusion electrode substrate includes, for example, gas diffusivity, electrical conductivity for collecting electricity generated in the catalyst layer, drainage for efficiently removing moisture generated on the surface of the catalyst layer, and thermal conductivity for dissipating heat generated by the reaction from the catalyst layer to the outside of the system.

[0003] The drainage properties of gas diffusion electrode substrates are particularly important in high current density regions where large amounts of water are generated, in order to prevent a sudden voltage drop (flooding). To improve drainage, carbon fiber sheets made of carbon fibers are typically treated to enhance water repellency. Gas diffusion electrode substrates are also designed with a controlled pore size distribution, which allows for the formation of pores of different sizes within the substrate, ensuring that gas diffusion pathways are maintained even if water accumulates in some pores.

[0004] Furthermore, fuel cells used as a power source for automobiles will be required to exhibit high power generation performance under high-temperature conditions where the cell temperature exceeds 90°C. At high temperatures, the electrolyte membrane dries out, reducing the ionic conductivity of the electrolyte membrane and making it prone to a decline in power generation performance (this phenomenon is called "dry-up"). Therefore, gas diffusion electrode substrates are required to have high thermal conductivity to dissipate heat generated in the catalyst layer so that the electrolyte membrane does not become too hot.

[0005] In Patent Document 1, fibrillated synthetic pulp is added to a carbon fiber sheet to form pores of 5 μm or more and less than 20 μm and pores of 20 μm or more and 50 μm or less, thereby achieving both gas diffusion and drainage properties.

[0006] In Patent Document 2, pores of different sizes are formed in a carbon fiber sheet containing pulp by using carbon fibers with a fiber length of 1 mm or more and short carbon fibers with a fiber length of less than 1 mm, thereby improving gas diffusion properties.

[0007] Patent Document 3 proposes a porous member that contains vapor grown carbon fiber (VGCF) and is supported only by conductive particles and resin in order to ensure thermal conductivity.

[0008] JP 2011-181511 A JP 2013-218951 A International Publication No. 2010 / 050219

[0009] In Patent Document 1, pulp with a low degree of graphitization was used, and thus high thermal conductivity was not achieved. Furthermore, pores with a size of 5 μm or more but less than 20 μm tended to retain generated water and did not function effectively as gas diffusion paths, resulting in a tendency for voltage to decrease due to flooding in high current density regions. Patent Document 2 adds PAN- or pitch-based milled carbon fibers, but the thermal conductivity was insufficient to suppress dry-up. Furthermore, the pore diameter formed by the short carbon fibers was only a few μm, and did not function effectively as gas diffusion paths under power generation conditions in which large amounts of water were generated. Patent Document 3 does not use carbon fibers as a skeleton, and therefore does not have pore diameters of 20 μm or more, and therefore does not have drainage paths of sufficient size, resulting in the problem of flooding occurring easily in high current density regions.

[0010] An object of the present invention is to provide a carbon fiber sheet that has high thermal conductivity, which suppresses dry-up of an electrolyte membrane, and exhibits high gas diffusivity even in a high current density region.

[0011] The present inventors have discovered a carbon fiber sheet that achieves both thermal conductivity and gas diffusivity by binding carbon fibers with a mixture containing fibrous carbon. The present invention addresses the above-mentioned problems as follows: (1) A carbon fiber sheet in which carbon fibrous structures are bound with a binder containing at least a resin and fibrous carbon, wherein the fibrous carbon content is 25 mass% or more relative to 100 mass% of the carbon fiber sheet, and the pore size distribution of the carbon fiber sheet has peaks between 0.3 μm and 1.0 μm and between 20 μm and 100 μm. (2) A carbon fiber sheet in which carbon fibrous structures are bound with a binder containing at least a resin and fibrous carbon, wherein the pore size distribution of the carbon fiber sheet has peaks between 0.3 μm and 1.0 μm and between 20 μm and 100 μm, and the pore volume of pores with diameters of 0.3 μm to 1.0 μm is 0.40 mL / g or more. (3) The carbon fiber sheet according to (1), wherein the pore volume of pores with diameters of 0.3 μm to 1.0 μm is 0.40 mL / g or more. (4) The carbon fiber sheet according to any one of (1) to (3), wherein the content of the resin is 5% by mass or more and 25% by mass or less, based on 100% by mass of the carbon fiber sheet. (5) The carbon fiber sheet according to any one of (1) to (4), wherein the content of the fibrous carbon is 40% by mass or more, based on 100% by mass of the carbon fiber sheet. (6) The carbon fiber sheet according to any one of (1) to (5), wherein the aspect ratio of the fibrous carbon is 10 or more and 400 or less. (7) The carbon fiber sheet according to any one of (1) to (6), wherein the fiber diameter of the fibrous carbon is 100 nm or more and 1 μm or less. (8) The carbon fiber sheet according to any one of (1) to (7), wherein the X-ray diffraction pattern has a peak with a half-width of 0.3° or more and 1.0° or less in the range of 25° to 28°. (9) The carbon fiber sheet according to any one of (1) to (8), wherein the decrease in tensile stress when pulled an additional 0.2 mm after break is 1 N / cm or more and 6 N / cm or less. (10) The carbon fiber sheet according to any one of (1) to (9), wherein the carbon fibrous structure is a carbon fiber paper sheet. (11) The carbon fiber sheet according to any one of (1) to (10), wherein the resin is a fluororesin. (12) A gas diffusion electrode substrate comprising the carbon fiber sheet according to any one of (1) to (11), and a microporous layer formed on one side thereof.(13) A fuel cell using the carbon fiber sheet according to any one of (1) to (11) as a gas diffusion electrode. (14) A fuel cell using the gas diffusion electrode substrate according to (12) as a gas diffusion electrode. (15) Transportation equipment using the fuel cell according to (13) or (14) as a power supply source. (16) A method for producing a carbon fiber sheet according to any one of (1) to (12), comprising the steps of: impregnating carbon fibrous structures with a liquid composition containing a resin as a binder and fibrous carbon; and heat-treating the carbon fiber sheet according to any one of (1) to (12) to melt the resin contained in the liquid composition impregnated in the impregnation step.

[0012] By using the carbon fiber sheet of the present invention in a gas diffusion electrode, it is possible to achieve both thermal conductivity and gas diffusivity, and to produce a polymer electrolyte fuel cell that exhibits high power generation performance in high temperature environments and high current density regions.

[0013] <Carbon Fiber Sheet> In the present invention, carbon fiber sheets are particularly suitable for use as gas diffusion electrode substrates for polymer electrolyte fuel cells. Hereinafter, the effects of using a carbon fiber sheet as a gas diffusion electrode substrate may be described as the effects of a specific embodiment of the carbon fiber sheet. A "carbon fiber sheet" is a structure having a network structure essentially composed of carbon fibers and a porous structure consisting of voids between the carbon fibers. Specific examples of the carbon fiber sheet of the present invention include carbon fiber sheets formed by binding carbon fiber structures such as carbon fiber paper sheets, woven fabrics, and nonwoven fabrics with a binder. Among these, it is particularly preferable to use a carbon fiber paper sheet as the carbon fiber structure because of its excellent "springiness," i.e., its ability to absorb dimensional changes in the direction perpendicular to the electrolyte membrane. Here, the term "carbon fiber paper sheet" refers to a structure in which carbon fibers are randomly dispersed in a two-dimensional plane.

[0014] The carbon fiber paper sheet can be produced by a wet papermaking method in which carbon fibers are dispersed in a liquid, or a dry papermaking method in which carbon fibers are dispersed in air. Among these, the wet papermaking method is preferred due to its superior productivity. The carbon fiber paper sheet may be produced by mixing carbon powder or organic fibers to improve the electrical conductivity and drainage of the gas diffusion electrode substrate. Furthermore, the carbon fibers may be bonded together with organic polymers such as polyvinyl alcohol, polyvinyl acetate, polyacrylonitrile, and cellulose, which facilitates improved shape retention and handling.

[0015] Examples of carbon fibers that constitute the carbon fiber sheet include polyacrylonitrile (PAN)-based, pitch-based, and rayon-based carbon fibers. Among these, PAN-based carbon fibers are preferably used because of their excellent mechanical strength.

[0016] The carbon fibers constituting the carbon fiber sheet preferably have an average single fiber diameter (hereinafter referred to as "carbon fiber diameter") in the range of 3 to 20 μm, more preferably in the range of 5 to 12 μm. When the carbon fiber diameter is 3 μm or more, more preferably 5 μm or more, the pore size becomes large, improving drainage and making it easier to suppress flooding. On the other hand, when the carbon fiber diameter is 20 μm or less, more preferably 12 μm or less, thickness unevenness becomes small, making it easier to control the thickness of the carbon fiber sheet within the preferred thickness range described below. Here, the carbon fiber diameter is determined by taking a photograph of the carbon fiber at 1,000x magnification using a microscope such as a scanning electron microscope (SEM), randomly selecting 30 different single fibers, measuring their diameters, and calculating the average value.

[0017] Furthermore, when a carbon fiber paper sheet is used as the carbon fiber structure, the carbon fibers constituting the carbon fiber paper sheet preferably have an average single fiber length (hereinafter referred to as "carbon fiber length") in the range of 3 to 20 mm, more preferably in the range of 5 to 15 mm. When the carbon fiber length is 3 mm or more, more preferably 5 mm or more, the resulting carbon fiber sheet is likely to have excellent mechanical strength, electrical conductivity, and thermal conductivity. On the other hand, when the carbon fiber length is 20 mm or less, more preferably 15 mm or less, the carbon fiber dispersion during papermaking is excellent, making it easier to obtain a homogeneous carbon fiber sheet. Carbon fibers having such a carbon fiber length can be obtained by, for example, cutting continuous carbon fibers to the desired length. The carbon fiber length was determined by photographing the carbon fibers at 50x magnification using a microscope such as an SEM, randomly selecting 30 different single fibers, and measuring their lengths to determine the average value.

[0018] The thickness of the carbon fiber sheet is preferably 50 to 230 μm, and more preferably 70 to 180 μm. By making the thickness of the carbon fiber sheet 230 μm or less, more preferably 180 μm or less, gas diffusibility is likely to be increased and generated water is also likely to be discharged more easily. Furthermore, the overall size of the fuel cell can be made smaller. On the other hand, by making the thickness of the carbon fiber sheet 50 μm or more, more preferably 70 μm or more, gas diffusion in the in-plane direction within the carbon fiber sheet is efficient, and power generation performance is likely to be improved.

[0019] The pore size distribution of the carbon fiber sheet of the present invention has at least two peaks between 0.3 μm to 1.0 μm and between 20 μm to 100 μm. The pores of 0.3 μm to 1.0 μm are formed by a binder containing at least a resin and fibrous carbon. Even under power generation conditions in which a large amount of water is generated during power generation, the generated water does not stagnate and functions as a gas diffusion path, thereby effectively suppressing flooding. Furthermore, the volume of pores of 0.3 μm to 1.0 μm is preferably 0.40 mL / g or more, more preferably 0.50 mL / g to 1.5 mL / g. If the pore volume of 0.3 μm to 1.0 μm is less than 0.40 mL / g, flooding may occur due to the small number of gas diffusion paths. If the pore volume of 0.3 μm to 1.0 μm is greater than 1.5 mL / g, the volume of pores with pore diameters of 20 μm to 100 μm decreases, tending to reduce gas diffusivity. The pores of 20 μm or more and 100 μm or less originate from the pores formed by the carbon fibers bound together by the binder, and serve as the main gas diffusion paths and the discharge paths of the generated water. The pore size distribution can be measured by pore measurement using a mercury porosimeter such as an Autopore 9520 manufactured by Shimadzu Corporation.

[0020] The decrease in tensile stress when the carbon fiber sheet of the present invention is pulled an additional 0.2 mm after breakage is preferably 1 N / cm or more and 6 N / cm or less, more preferably 1 N / cm or more and 4 N / cm or less. By having a tensile stress of 6 N / cm or less per 0.2 mm, even if excessive tensile stress is applied to the carbon fiber sheet and the carbon fiber sheet breaks in a subsequent process using the carbon fiber sheet, such as the process of producing a membrane-electrode assembly, the decrease in tensile stress immediately after breakage is small, making it easy to restore the process. The smaller the decrease in tensile stress of the carbon fiber sheet immediately after breakage, the more preferable it is. However, in the case of a carbon fiber paper sheet, it is not easy to achieve a decrease of less than 1 N / cm per 0.2 mm, so the lower limit is about 1 N / cm per 0.2 mm. The decrease in tensile stress of the carbon fiber sheet immediately after breakage can be controlled by the type and amount of resin used as a binder. The decrease in tensile stress when the carbon fiber sheet is pulled an additional 0.2 mm after breaking can be determined by measuring the difference between the tensile stress at the breaking point and the tensile stress after pulling an additional 0.2 mm immediately after breaking, in a tensile test using an Autograph (registered trademark) manufactured by Shimadzu Corporation, etc. The tensile stress is calculated by dividing the tensile force by the width of the test piece.

[0021] The binder used to bind the carbon fibers in the carbon fiber sheet of the present invention is a mixture containing at least a resin and fibrous carbon. In a structure in which carbon fibers are bound with a binder containing a resin and fibrous carbon, pores of 0.3 μm to 1.0 μm are likely to be formed in the binder. When carbon fibers are bound with a binder containing only a resin, and fibrous carbon is contained in the carbon fiber sheet but not in the binder, the binder often lacks pores, and the binder spreads out like a web, inhibiting gas diffusion. Furthermore, since fibrous carbon has superior thermal conductivity compared to resin, the presence of fibrous carbon in the binder functions as a heat conduction path, improving the thermal conductivity of the entire carbon fiber sheet. Whether the carbon fibers are bound with a binder containing a resin and fibrous carbon can be confirmed by magnifying and photographing the web-like binder portions formed at the intersections of the carbon fibers using an SEM or the like, and determining whether pores are formed within the binder by the fibrous carbon and resin.

[0022] The resin contained in the binder can be a carbonized resin or an uncarbonized resin, but one primarily composed of an uncarbonized resin is preferred. Using an uncarbonized resin eliminates the need for a high-temperature treatment process under an inert atmosphere, significantly reducing manufacturing costs. Phenol resin, epoxy resin, fluororesin, and the like are preferred as the resin, with fluororesin being particularly preferred. Examples of fluororesins that can be used include polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA). PTFE or FEP is more preferred due to its high water repellency. Mixing PTFE or FEP with fibrous carbon forms pores with a water-repellent surface, which reduces water retention within the pores, resulting in a carbon fiber sheet with high drainage properties. Using an uncarbonized phenolic resin, epoxy resin, or fluororesin as the resin softens the carbon fiber sheet, making it easier to wind it onto a roll. Furthermore, the decrease in tensile stress when the carbon fiber sheet is pulled an additional 0.2 mm after breaking can be 6 N / cm or less. Furthermore, by not including a thermosetting resin as the binder, there is an advantage that the carbon fibers can be easily separated, recovered, and reused after the binder is burned off from the carbon fiber sheet.

[0023] The use of a fluororesin as the resin contained in the binder can be determined by observation with SEM-EDX. If the shape of the binder binding the carbon fibers together observed with SEM matches the shape of the F element mapped in the same field of view by EDX, it can be determined that a fluororesin is used as the binder.

[0024] The carbon fiber sheet of the present invention preferably contains 5% by mass or more of the resin per 100% by mass of the carbon fiber sheet. Furthermore, the upper limit of the resin content is preferably 25% by mass or less per 100% by mass of the carbon fiber sheet. When the resin content is 5% by mass or more relative to the carbon fiber sheet, the mechanical strength of the carbon fiber sheet is increased, and the risk of breakage during the manufacturing process can be reduced. When the resin content is 25% by mass or less relative to the carbon fiber sheet, the ratio of materials that inhibit conductivity in the carbon fiber sheet is reduced, and the carbon fiber sheet can achieve both mechanical strength and conductivity.

[0025] As the fibrous carbon contained in the binder, it is preferable to use carbon nanofibers because they have high thermal conductivity and a shape that makes it easy to form pores of 0.3 μm to 1.0 μm. Fibrous carbon acts as a heat conduction path, and the higher the degree of graphitization, the better the thermal conductivity. The degree of graphitization can be evaluated using an X-ray diffraction pattern, and the narrower the half-width of the peak, the higher the degree of graphitization. Therefore, the X-ray diffraction pattern of the carbon fiber sheet preferably has a peak in the range of 25° to 28° with a half-width of 0.3° to 1.0°, and more preferably has a peak with a half-width of 0.3° to 0.6°. The half-width can be controlled by the manufacturing method of the fibrous carbon and the heat treatment temperature. If the half-width of the peak in this range is 1.0° or less, the degree of graphitization is high. If it is 0.6° or less, the degree of graphitization is even higher. Since a material with high thermal conductivity is included, the thermal conductivity of the entire carbon fiber sheet is excellent. The narrower the half-value width of the peak in this range, the higher the degree of graphitization, which is preferable, but the smaller the fiber diameter of the fibrous carbon, the lower the degree of graphitization, so when fibrous carbon having a fiber diameter that forms pores of 0.3 μm or more and 1.0 μm or less is attached to a carbon fiber sheet, it is not easy to make the half-value width less than 0.3°, and the lower limit is about 0.3°. The half-value width of the carbon fiber sheet can be calculated by measuring the X-ray diffraction pattern of the carbon fiber sheet using an X-ray diffractometer (D8 ADVANCE, manufactured by Bruker).

[0026] The aspect ratio of the fibrous carbon is preferably 10 or more, more preferably 10 to 400, and even more preferably 20 to 150. When the aspect ratio is 10 or more, more preferably 20 or more, pores of 0.3 μm to 1.0 μm are easily formed in the binder, and even a small amount of fibrous carbon easily forms a heat conduction path in the binder, thereby improving the thermal conductivity of the carbon fiber sheet. When the aspect ratio is greater than 400, entanglement of the fibrous carbon is easily generated, which may increase the viscosity of the liquid composition in which the fibrous carbon is dispersed in a solvent. When the aspect ratio is 150 or less, the viscosity can be kept low even when the fibrous carbon in the liquid composition is at a high concentration.

[0027] When a carbon fiber sheet is produced by impregnating the carbon fiber sheet with a highly viscous liquid composition, the fibrous carbon adheres to the outside of the carbon fiber sheet and the amount of fibrous carbon adhered to the inside of the carbon fiber sheet is reduced, making it difficult for the fibrous carbon to adhere uniformly in the thickness direction of the carbon fiber sheet. If the fibrous carbon is not adhered uniformly in the thickness direction, there will be areas in the carbon fiber sheet with few heat conduction paths, which may significantly reduce the thermal conductivity of the entire carbon fiber sheet. Therefore, it is preferable that the fibrous carbon adheres uniformly in the thickness direction of the carbon fiber sheet.

[0028] The fiber diameter of the fibrous carbon is preferably 100 nm or more and 1 μm or less. If it is 100 nm or more, pores of 0.3 μm or more are likely to be formed in the binder. If it is less than 100 nm, the pores in the binder become small, which may reduce gas diffusibility. If it is 1 μm or less, a heat conduction path can be formed with a small content, thereby improving thermal conductivity while maintaining gas diffusibility. The fiber diameter can be measured, for example, by magnifying and observing the fibrous carbon using an SEM. In a photograph of the fibrous carbon taken, 30 different pieces of fibrous carbon were randomly selected, and the diameters perpendicular to the fiber length were measured and the average value was calculated. Similarly, for the aspect ratio, 30 different pieces of fibrous carbon were randomly selected in a SEM photograph of the fibrous carbon taken, and the fiber lengths were measured and the average value was calculated. The fiber length relative to the fiber diameter was used as the aspect ratio.

[0029] The carbon fiber sheet of the present invention preferably contains 25% by mass or more, and more preferably 40% by mass or more, of fibrous carbon per 100% by mass of the carbon fiber sheet. The upper limit of the fibrous carbon content is preferably 60% by mass or less per 100% by mass of the carbon fiber sheet. When the carbon fiber sheet contains 25% by mass or more, preferably 40% by mass or more, of fibrous carbon, pores with diameters of 0.3 μm or more and 1.0 μm or less can be formed in the carbon fiber sheet. When the carbon fiber sheet contains 60% by mass or less of fibrous carbon, a sufficient volume of pores of 20 μm or more and 100 μm or less can be secured, resulting in high drainage and gas diffusion properties. When the method for producing a carbon fiber sheet includes a heat treatment step, it is preferable that the carbon fiber sheet after the heat treatment step satisfy the above ranges.

[0030] <Method for Producing Carbon Fiber Sheet> A method for producing a carbon fiber sheet of the present invention will now be exemplified, but the carbon fiber sheet of the present invention is not limited to the following method for producing the carbon fiber sheet.

[0031] The method for producing a carbon fiber sheet of the present invention preferably comprises an impregnation step of impregnating a carbon fiber structure with a liquid composition containing at least a resin and fibrous carbon, a molding step of controlling the thickness of the carbon fiber sheet by hot pressing, and a heat treatment step of melting the resin contained in the liquid composition impregnated in the impregnation step.

[0032] [Impregnation Step] The method for producing a carbon fiber sheet of the present invention preferably includes a step of forming carbon fibers into a carbon fiber structure having a certain shape, such as a paper sheet, and then impregnating the carbon fibers with a liquid composition containing a resin and fibrous carbon.

[0033] Methods for impregnating a carbon fiber sheet with a liquid composition include immersion in the liquid composition and application of the liquid composition. When application is used, the resin and fibrous carbon contained in the liquid composition tend to be greater on the coated surface and less on the other surface. Although it is possible to melt the resin and move it to some extent from the coated surface to the other surface using a heating treatment such as hot pressing after application, the fibrous carbon does not melt even when heated and is therefore less likely to move, making it difficult to ensure that the fibrous carbon is uniformly distributed throughout the carbon fiber sheet. Therefore, the method of immersing the carbon fiber sheet in the liquid composition is particularly preferred because it allows the fibrous carbon to be uniformly distributed from both sides of the carbon fiber sheet to the inside and is also highly productive. Furthermore, when a fluororesin is used as the resin, the viscosity of the liquid composition can be reduced by using a fluororesin microparticle dispersion as the fluororesin source of the liquid composition, which is preferred because the viscosity of the liquid composition is less likely to increase even when the fibrous carbon is mixed at a high concentration. By making the liquid composition low in viscosity, it is possible to adhere a sufficient amount of fibrous carbon to the inside of the carbon fiber sheet in one impregnation to ensure thermal conductivity.

[0034] The amount of fibrous carbon attached to the carbon fiber sheet can be controlled by adjusting the content of fibrous carbon in the liquid composition.

[0035] The impregnation step is preferably carried out before the molding step described below. Because the carbon fiber sheet before molding has a low density, the resin and fibrous carbon tend to adhere to the inside of the carbon fiber sheet when immersed in the liquid composition.

[0036] [Forming Step] The carbon fiber sheet manufacturing method of the present invention preferably includes a forming step in which the carbon fiber structure impregnated with the liquid composition is heated and pressurized at a temperature of 100°C or higher after the impregnation step and before the heat treatment step described below. This forming step allows for more accurate control of the thickness and porosity of the resulting carbon fiber sheet, and also smooths the surface of the carbon fiber sheet by applying pressure while partially melting the resin on the surface of the carbon fiber sheet. When an electrolyte membrane is sandwiched between carbon fiber sheets to assemble a fuel cell, binders containing resin and fibrous carbon may form protrusions that break through the electrolyte membrane and cause a short circuit. Smoothing the surface of the carbon fiber sheet can significantly reduce such short circuits. In the forming step, the heating temperature is preferably 100 to 250°C. The applied pressure is preferably 0.01 to 5 MPa.

[0037] [Heat Treatment Step] The carbon fiber sheet that has been immersed in a liquid composition containing a resin and fibrous carbon and, if necessary, has been subjected to a molding step is then subjected to a heat treatment step. The heat treatment temperature in the heat treatment step is preferably 300°C or higher and 400°C or lower. By performing heat treatment at a temperature of 300°C or higher, the resin contained in the impregnated liquid composition melts and wets and spreads. Furthermore, by setting the temperature to 400°C or lower, a large-scale heating furnace is not required, and the production cost of the carbon fiber sheet can be significantly reduced.

[0038] Generally, the content of fibrous carbon hardly decreases during the heat treatment process, whereas the content of resin decreases significantly during the heat treatment process. Therefore, by determining the resin content in the liquid composition taking into account the decrease in resin due to the heat treatment, the resin content in the carbon fiber sheet after the heat treatment process can be controlled. Since the degree of decrease in resin during the heat treatment process varies depending on the heat treatment conditions, the resin content in the liquid composition is appropriately adjusted according to the heat treatment conditions.

[0039] [Water-repellent Step] The method may include a step of subjecting the carbon fiber sheet to a water-repellent treatment using a water-repellent treatment liquid in which a water-repellent agent containing a fluororesin is dispersed.

[0040] Examples of the water-repellent treatment method include a method of immersing a carbon fiber sheet in a water-repellent treatment liquid, and a method of applying the water-repellent treatment liquid to a carbon fiber sheet by die coating or the like. From the viewpoint of uniformly distributing the fluororesin in the carbon fiber sheet in the direction perpendicular to the surface, the method of immersing a carbon fiber sheet in a water-repellent treatment liquid is preferred. After the water-repellent treatment, it is preferred to carry out a heat-drying step or a sintering step.

[0041] However, if the water-repellent treatment is performed after forming a binder having pores, the water-repellent agent will adhere to cover the already formed pores, blocking the pores and reducing gas diffusibility. Therefore, it is preferable to apply the water-repellent agent in the impregnation step.

[0042] <Method for producing carbon fiber sheet having a microporous layer> [Coating step] The above-mentioned carbon fiber sheet can be used as a gas diffusion electrode substrate, but a microporous layer may be formed on one side of the carbon fiber sheet to be used as a gas diffusion electrode substrate. The microporous layer is a porous layer that usually contains carbon powder and a water repellent agent and has pores with a diameter of 0.01 μm to 1 μm.

[0043] Examples of carbon powder contained in the microporous layer include carbon black, graphite particles, carbon nanotubes, carbon nanofibers, etc. Among these, carbon black is preferably used.

[0044] As the water repellent agent contained in the microporous layer, fluororesins such as polytetrafluoroethylene (PTFE), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and tetrafluoroethylene-perfluoroalkylvinyl ether copolymer (PFA) are preferably used.

[0045] The basis weight of the microporous layer is not particularly limited, but is preferably 10 to 50 g / m 2 It is preferable that the range is 14 to 30 g / m 2 It is more preferable that the basis weight of the microporous layer is 10 g / m 2 More preferably, 14 g / m 2When the microporous layer has a mass per unit area of ​​50 g / m or more, one surface of the carbon fiber sheet can be covered with the microporous layer, which further promotes the back diffusion of generated water and further suppresses the drying of the electrolyte membrane. 2 or less, more preferably 30 g / m 2 When the water content is less than 100%, the drainage property is further improved and flooding can be further suppressed.

[0046] The microporous layer is obtained by applying a coating liquid containing the above-mentioned carbon powder and water repellent agent to a carbon fiber sheet. Coating methods such as screen printing, rotary screen printing, spray atomization, intaglio printing, gravure printing, die coater coating, bar coating, and blade coating can be used for the coating. The coating is then preferably dried at a temperature of 80 to 180°C. After drying, the sheet is preferably heated to a temperature of about 300 to 400°C, more preferably 340 to 390°C, to melt the water repellent agent.

[0047] [Membrane Electrode Assembly] In the present invention, a membrane electrode assembly can be formed by bonding the above-mentioned carbon fiber sheet or gas diffusion electrode substrate to at least one side of an electrolyte membrane having catalyst layers on both sides. When using a gas diffusion electrode substrate having a microporous layer, it is preferable to place the microporous layer of the gas diffusion electrode substrate on the catalyst layer side, as this not only facilitates back diffusion of generated water but also increases the contact area between the catalyst layer and the gas diffusion electrode substrate, thereby reducing contact electrical resistance. Platinum is usually used as the catalyst for the catalyst layer. The electrolyte membrane is preferably made of a perfluorosulfonic acid-based polymer material, which has high proton conductivity, oxidation resistance, and heat resistance.

[0048] [Fuel Cell] The fuel cell of the present invention comprises the carbon fiber sheet or gas diffusion electrode substrate of the present invention. That is, it has separators on both sides of the above-mentioned membrane electrode assembly. That is, a fuel cell is constructed by disposing separators on both sides of the above-mentioned membrane electrode assembly. Typically, a solid polymer fuel cell is constructed by stacking multiple such membrane electrode assemblies, each sandwiched between separators on both sides. The catalyst layer is composed of a layer containing a solid polymer electrolyte and catalyst-supporting carbon. The configuration of such a fuel cell unit and a fuel cell itself is well known.

[0049] The fuel cell of the present invention can be used as a power supply source for transportation equipment such as automobiles, ships, and trains.

[0050] In particular, when used as a power source for automobiles, they must be used under high-temperature conditions. Current fuel cells installed in automobiles typically operate at 60 to 70°C, but large radiators are used to cool the heat generated by power generation. By increasing the operating temperature to around 90°C, the radiators required for exhaust heat can be made smaller, and so active development is underway for fuel cells with higher operating temperatures. Since it is necessary to prevent the electrolyte from drying out in order to operate fuel cells at high temperatures, the carbon fiber sheet with enhanced thermal conductivity of the present invention, which promotes heat dissipation from the electrolyte membrane, is preferably used.

[0051] Next, the carbon fiber sheet of the present invention will be specifically described with reference to examples. The materials used in the examples, the methods for producing and evaluating the carbon fiber sheet, and the method for evaluating the cell performance of the fuel cell are described below.

[0052] <Pore size distribution> The carbon fiber sheet is placed in a 6 cm square measuring 2 cm x 3 cm. 2 Five measurement samples cut into 1 / 4" pieces were prepared, and measurements were performed by mercury intrusion porosimetry at a measurement pressure range of 6 kPa to 123 MPa (pore diameters of 10 nm to 200 μm). The peak pore diameter was determined from the average value of the pore diameter distribution obtained. The measurement device used was an Autopore 9520 manufactured by Shimadzu Corporation. The pore diameter peak was determined by taking the maximum point in the target region of the curve of the logarithmic differential pore volume distribution graph obtained by pore measurement using a mercury porosimeter.

[0053] The pore volume of pores with diameters of 0.3 μm to 1.0 μm was calculated by subtracting the cumulative pore volume of pores with diameters of 1.0 μm or more from the cumulative pore volume of pores with diameters of 0.3 μm or more.

[0054] <Weight per unit area of ​​carbon fiber sheet> Ten test pieces of 10 cm x 10 cm were prepared from the carbon fiber sheet, and the mass of each test piece was measured to determine the average weight per unit area of ​​the ten test pieces.

[0055] <Thickness and Density of Carbon Fiber Sheet> The thickness of the carbon fiber sheet was measured using a digital thickness meter Digimicro manufactured by Nikon Corporation while applying a load of 0.15 MPa to the carbon fiber sheet. The density was calculated from the basis weight of the carbon fiber sheet.

[0056] <Thermal Resistance> Ten test pieces were prepared by cutting the carbon fiber sheet into 30 mm diameter circles, and each test piece was set in a thermal conductivity measuring device (IE-1230 (manufactured by Iwatsu Measurement Co., Ltd.)) and the thermal resistance (K / W) was measured when a pressure of 1.0 MPa was applied. The thermal resistance (K cm) in the direction perpendicular to the surface of the carbon fiber sheet was calculated by multiplying the thermal resistance by the area of ​​the carbon fiber sheet. 2 / W) and the average of the ten test pieces was calculated.

[0057] <Half-width in X-ray diffraction pattern> A carbon fiber sheet was cut to a diameter of 47 mm to prepare a sample. Using an X-ray diffractometer (D8 ADVANCE, manufactured by Bruker), measurements were taken over a range of 15 to 40° in 0.02° steps while rotating the sample stage at a speed of 30 rpm, and the peak with the maximum diffraction intensity was obtained. The half-width of this peak was used.

[0058] <Decrease in tensile stress when pulled an additional 0.2 mm after break> The tensile properties of the carbon fiber sheet were measured using the tensile test mode of an Autograph (registered trademark) AGS-X manufactured by Shimadzu Corporation. A carbon fiber sheet test piece cut to a size of 15 cm in length and 1.5 cm in width was attached to two upper and lower sample mounting jigs attached to the tensile tester, and the carbon fiber sheet was pulled in the longitudinal direction at a rate of 2 mm / min to obtain a stress-displacement curve. The maximum stress in this curve was taken as the break point of the carbon fiber sheet, and the difference between the tensile stress at the break point and the tensile stress after pulling an additional 0.2 mm from immediately after break was measured. The tensile stress was calculated by dividing the tensile force by the width of the test piece. This measurement was performed five times using different test pieces, and the average value was used as the decrease in tensile stress when pulled an additional 0.2 mm from break.

[0059] <Gas Diffusivity> Using a gas / water vapor diffusivity measuring device (MVDP-200C) manufactured by Seika Sangyo Co., Ltd., a gas for which diffusivity was to be measured was flowed on one side (primary side) of a carbon fiber sheet, and nitrogen gas was flowed on the other side (secondary side). The differential pressure between the primary and secondary sides was controlled to approximately 0 Pa (0±3 Pa) (i.e., a state was created in which there was almost no gas flow due to the pressure difference and gas movement occurred only by molecular diffusion), and the gas concentration when equilibrium was reached was measured using a gas concentration meter on the secondary side, and this value (%) was used as an index of gas diffusivity in the thickness direction.

[0060] <Power Generation Performance of Polymer Electrolyte Fuel Cell> A catalyst solution was prepared by sequentially adding 1.00 g of platinum-loaded carbon (manufactured by Tanaka Kikinzoku Kogyo K.K., platinum loading: 50% by mass), 1.00 g of purified water, 8.00 g of Nafion (registered trademark) solution (5.0% by mass of Nafion (registered trademark) manufactured by Aldrich), and 18.00 g of isopropyl alcohol (manufactured by Nacalai Tesque, Inc.).

[0061] Next, the catalyst solution was sprayed onto a piece of "Naflon (registered trademark)" PTFE tape "TOMBO (registered trademark)" No. 9001 (manufactured by Nichias Corporation) cut to a size of 5 cm x 5 cm, and the tape was dried at room temperature to obtain a platinum content of 0.3 mg / cm. 2A PTFE sheet with a catalyst layer was produced. Subsequently, a solid polymer electrolyte membrane "Nafion (registered trademark)" NRE-211CS (manufactured by DuPont) cut to 8 cm x 8 cm was sandwiched between two PTFE sheets with a catalyst layer, and pressed at 5 MPa with a flat plate press at a temperature of 130°C for 5 minutes to transfer the catalyst layer to the electrolyte membrane. After pressing, the PTFE sheets were peeled off to produce an electrolyte membrane with a catalyst layer.

[0062] Next, the catalyst layer-equipped electrolyte membrane was sandwiched between two gas diffusion electrode substrates prepared in each Example and Comparative Example, each cut to a size of 5 cm x 5 cm, and pressed at 3 MPa using a flat press at 130°C for 5 minutes to prepare a membrane electrode assembly.

[0063] The resulting membrane electrode assembly was assembled into a single cell for fuel cell evaluation. A single-channel serpentine separator with a groove width, groove depth, and rib width of 1.0 mm was used as the separator. Unpressurized hydrogen was supplied to the anode side, and unpressurized air was supplied to the cathode side, with the relative humidity set at 30%.

[0064] The measurements were carried out as follows: the utilization rates of hydrogen and oxygen in the air were 70 mol% and 40 mol%, respectively, and the cell temperature was 90°C. Under these conditions, the current density was 1.9 A / cm 2 The output voltage was measured and used as an index of power generation performance.

[0065] Example 1 Toray Industries, Inc.'s polyacrylonitrile carbon fiber "TORAYCA (registered trademark)" T300 was cut to a length of 7 mm, dispersed in water, and made into paper. The paper was then immersed in a 10% by mass aqueous dispersion of polyvinyl alcohol and dried to obtain a carbon fiber sheet having a basis weight of about 20 g / m. 2 A long carbon fiber paper sheet was obtained and wound into a roll.

[0066] A liquid composition was prepared by mixing an aqueous dispersion of PTFE resin (Polyflon (registered trademark) PTFE Dispersion D-210C (manufactured by Daikin Industries, Ltd.)), vapor-grown carbon fiber "VGCF (registered trademark)" (fibrous carbon, aspect ratio: 53, fiber diameter: 0.15 μm, manufactured by Resonac Co., Ltd.) as fibrous carbon, a nonionic surfactant as a dispersant, and water in a ratio (mass ratio) of aqueous dispersion of PTFE resin: fibrous carbon: dispersant: water = 7:13:4:76. The carbon fiber sheet cut to 10 cm x 10 cm was immersed in the liquid composition and pulled out. After heat treatment, the sheet was squeezed with a mangle to remove excess liquid so that the fibrous carbon accounted for 48 mass% and the resin for 17 mass% of 100 mass% of the carbon fiber sheet. The sheet was then dried at 100°C for 10 minutes.

[0067] Next, the carbon fiber paper sheet after immersion in the liquid composition was subjected to a heat and pressure treatment at 180°C for 5 minutes while being pressed at 3 MPa using a platen press, to obtain a carbon fiber sheet. A heat treatment was further performed at 360°C for 10 minutes to obtain a carbon fiber sheet. The obtained carbon fiber sheet was measured using the various measurement methods described above, and the results are shown in Table 1.

[0068] (Example 2) A carbon fiber sheet was obtained in the same manner as in Example 1, except that a carbon fiber sheet was immersed in a liquid composition prepared by mixing an aqueous dispersion of PTFE resin, fibrous carbon, dispersant, and water in a ratio (mass ratio) of 4:7:2:87, and excess liquid was removed with a mangle so that after heat treatment, the fibrous carbon accounted for 36 mass% and the resin for 13 mass% of 100 mass% of the carbon fiber sheet.

[0069] (Comparative Example 1) The weight of the carbon fiber is about 30 g / m 2 A long carbon fiber sheet was prepared, and the carbon fiber sheet was immersed in a liquid composition prepared by mixing an aqueous dispersion of PTFE resin, fibrous carbon, dispersant, and water in a ratio (mass ratio) of 7:4:1:88. After heat treatment, excess liquid was removed with a mangle so that the fibrous carbon accounted for 22 mass% and the resin accounted for 26 mass% of 100 mass% of the carbon fiber sheet. A carbon fiber sheet was obtained in the same manner as in Example 1.

[0070] Comparative Example 2 A carbon fiber sheet was obtained in the same manner as in Example 1, except that CNT paste (fibrous carbon, aspect ratio: 500, fiber diameter: 0.02 μm, manufactured by Cnano Corporation) was used instead of vapor-grown carbon fiber, and a liquid composition was prepared by mixing an aqueous dispersion of PTFE resin: fibrous carbon: dispersant: water = 4:7:2:87 (mass ratio). The carbon fiber sheet was immersed in this liquid composition, dried, and then immersed again in the same liquid composition. After heat treatment, the carbon fiber sheet was immersed again in the same liquid composition, and excess liquid was removed with a mangle so that the fibrous carbon accounted for 49 mass% and the resin for 17 mass% of 100 mass% of the carbon fiber sheet.

[0071] Comparative Example 3 A carbon fiber sheet was obtained in the same manner as in Example 1, except that "Denka Black (registered trademark)" (acetylene black, aspect ratio: 1, manufactured by Denka Co., Ltd.) was used instead of the vapor-grown carbon fiber, and excess liquid was removed with a mangle so that the resin content was 18 mass %.

[0072] (Example 3) A carbon fiber sheet was obtained in the same manner as in Example 1, except that a carbon fiber sheet was immersed in a liquid composition prepared by mixing an aqueous dispersion of PTFE resin, fibrous carbon, dispersant, and water in a ratio (mass ratio) of 4:4:1:91, and excess liquid was removed with a mangle so that after heat treatment, the fibrous carbon accounted for 26 mass% and the resin for 100 mass% of the carbon fiber sheet.

[0073] (Example 4) A carbon fiber sheet was obtained in the same manner as in Example 1, except that a carbon fiber sheet was immersed in a liquid composition prepared by mixing an aqueous dispersion of PTFE resin, fibrous carbon, dispersant, and water in a ratio (mass ratio) of 3:17:5:75, and excess liquid was removed with a mangle so that after heat treatment, the fibrous carbon accounted for 61 mass% and the resin for 7 mass% of 100 mass% of the carbon fiber sheet.

[0074] Comparative Example 4 A carbon fiber sheet was obtained in the same manner as in Example 1, except that carbon nanofibers (aspect ratio: 7, fiber diameter: 0.7 μm) were used as the fibrous carbon instead of vapor-grown carbon fiber, and a carbon fiber sheet was immersed in a liquid composition prepared by mixing an aqueous dispersion of PTFE resin: fibrous carbon: dispersant: water in a ratio (mass ratio) of 7:13:5:75, and after drying, the sheet was immersed again in the same liquid composition, and excess liquid was removed with a mangle so that after heat treatment, the fibrous carbon accounted for 50 mass% and the resin for 16 mass% of 100 mass% of the carbon fiber sheet.

[0075]

[0076] The carbon fiber sheet of the present invention and the gas diffusion electrode substrate using the same can be suitably used for fuel cells, particularly gas diffusion electrodes of polymer electrolyte fuel cells. Furthermore, the gas diffusion electrode substrate using the carbon fiber sheet of the present invention achieves both thermal conductivity and gas diffusivity, suppresses dry-up of the electrolyte membrane, and exhibits high gas diffusivity even in a high current density range, making it possible to produce high-performance polymer electrolyte fuel cells.

Claims

1. A carbon fiber sheet in which carbon fiber structures are bound with a binder containing at least a resin and fibrous carbon, the content of the fibrous carbon being 25 mass% or more in 100 mass% of the carbon fiber sheet, and the pore size distribution of the carbon fiber sheet has peaks between 0.3 μm and 1.0 μm and between 20 μm and 100 μm.

2. A carbon fiber sheet in which carbon fiber structures are bound with a binder containing at least a resin and fibrous carbon, the pore size distribution of the carbon fiber sheet has peaks between pore sizes of 0.3 μm to 1.0 μm and between 20 μm to 100 μm, and the pore volume of pores with diameters of 0.3 μm to 1.0 μm is 0.40 mL / g or more.

3. The carbon fiber sheet according to claim 1, wherein the volume of pores having a pore diameter of 0.3 μm to 1.0 μm is 0.40 mL / g or more.

4. A carbon fiber sheet according to claim 1 or 2, wherein the resin content is 5% by mass or more and 25% by mass or less based on 100% by mass of the carbon fiber sheet.

5. A carbon fiber sheet according to claim 1 or 2, wherein the content of the fibrous carbon is 40 mass% or more based on 100 mass% of the carbon fiber sheet.

6. The carbon fiber sheet according to claim 1 or 2, wherein the aspect ratio of the fibrous carbon is 10 or more and 400 or less.

7. The carbon fiber sheet according to claim 1 or 2, wherein the fiber diameter of the fibrous carbon is 100 nm or more and 1 μm or less.

8. The carbon fiber sheet according to claim 1 or 2, which has a peak with a half-width of 0.3° or more and 1.0° or less in the range of 25° to 28° in an X-ray diffraction pattern.

9. The carbon fiber sheet according to claim 1 or 2, wherein the drop in tensile stress when pulled an additional 0.2 mm from break is 1 N / cm or more and 6 N / cm or less.

10. The carbon fiber sheet according to claim 1 or 2, wherein the carbon fiber structure is a carbon fiber paper body.

11. The carbon fiber sheet according to claim 1 or 2, wherein the resin is a fluororesin.

12. A gas diffusion electrode substrate comprising the carbon fiber sheet according to claim 1 or 2 and a microporous layer formed on one side thereof.

13. A fuel cell using the carbon fiber sheet according to claim 1 or 2 as a gas diffusion electrode.

14. A fuel cell using the gas diffusion electrode substrate according to claim 12 as a gas diffusion electrode.

15. A transportation device using the fuel cell according to claim 13 as a power source.

16. A transportation device using the fuel cell according to claim 14 as a power source.

17. A method for producing a carbon fiber sheet according to claim 1 or 2, comprising the steps of: impregnating a carbon fiber structure with a liquid composition containing a resin as a binder and fibrous carbon; and a heat treatment step for melting the resin contained in the liquid composition impregnated in the impregnation step.

Citation Information

Patent Citations

  • Porous electrode substrate for polymer electrolyte fuel cell

    JP2011181511A

  • Porous conductive sheet, manufacturing method thereof, electrode material, and fuel battery

    JP2013218951A

  • Gas diffusion layer for fuel cell, manufacturing method therefor, membrane electrode assembly, and fuel cell

    WO2010050219A1

  • Fuel cell electrode, manufacture thereof and fuel cell

    JP2000182626A

  • Method of manufacturing carbon fiber sheet

    JP2008214120A

Cited By

  • Conductive sheets, membrane electrode assemblies, and fuel cells

    JP2026113171A

  • Conductive sheets, membrane electrode assemblies, and fuel cells

    JP7909013B2

  • Conductive sheet, membrane electrode assembly, and fuel cell

    WO2026141060A1

  • Electroconductive sheet, membrane electrode assembly, and fuel cell

    WO2026141061A1

  • Porous transport layer, membrane electrode assembly, water electrolysis device, composition for microporous layer, and method for producing porous transport layer

    WO2026141265A1