Resin needle
The resin needle composition, featuring polylactic acid and non-fibrous inorganic particles, addresses the heat resistance and puncturing performance challenges of conventional medical needles by enhancing moldability and stability, ensuring effective puncturing in high-temperature conditions.
Patent Information
- Application Number
- PCT/JP2024/011654
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional medical needles made from polylactic acid suffer from poor heat resistance and brittleness, leading to compromised puncturing performance, especially in high-temperature environments, and require time for crystallization, which hampers productivity.
A resin needle composition incorporating polylactic acid with a weight average molecular weight of 20,000 to 400,000 and a D-isomer ratio of 15% to 85% combined with non-fibrous inorganic particles, such as talc, to enhance heat resistance and moldability, with a crystallinity of 1 to 60% and a crystallization temperature above 80°C, ensuring improved puncturing properties and stability.
The resin needle exhibits excellent micro-moldability, puncturing properties, and heat resistance, maintaining performance even in high-temperature environments, while avoiding the brittleness and productivity issues of conventional polylactic acid-based needles.
Smart Images

Figure JP2024011654_03102024_PF_FP_ABST
Abstract
Description
Resin needle
[0001] The present invention relates to a resin needle made of a resin composition.
[0002] Patent Document 1 discloses a medical needle having a microstructure.
[0003] Patent No. 4065906
[0004] Patent Document 1 cites polylactic acid as an example of a polymer that can be used to make medical needles. Polylactic acid has a glass transition temperature of approximately 60°C, which means it has poor heat resistance. Its microstructure collapses in high-temperature environments, making it impossible to maintain its puncture performance. While crystallizing polylactic acid improves its heat resistance, it also becomes brittle and requires a long time for crystallization, reducing productivity.
[0005] The present invention has been made in view of the above circumstances, and aims to provide a resin needle that is excellent in fine moldability, puncture property, and heat resistance.
[0006] According to the present invention, the following inventions are provided. [1] A resin needle made of a resin composition, the resin composition containing polylactic acid and non-fibrous inorganic particles, the polylactic acid having a weight-average molecular weight of 20,000 to 400,000 and a D-form ratio of 15% by mass or less or 85% by mass or more, the non-fibrous inorganic particles having an average particle size of 0.05 to 20 μm, and the content of the non-fibrous inorganic particles being 5 to 70 parts by mass per 100 parts by mass of the polylactic acid. [2] The resin needle according to [1], the resin composition containing a biocompatible resin other than the polylactic acid, the content of the biocompatible resin being 50 parts by mass or less per 100 parts by mass of the polylactic acid. [3] The resin needle according to [1] or [2], the polylactic acid component of the resin needle having a crystallinity of 1 to 60%. [4] The resin needle according to any one of [1] to [3], wherein the crystallization temperature of the polylactic acid component of the resin needle is above 80° C. [5] The resin needle according to any one of [1] to [4], wherein the resin composition is extruded at a melting temperature of 220° C. to a length of 50 mm, a cross-sectional area of 3 mm 2[6] A resin needle according to any one of [1] to [5], wherein the resin composition is extruded at a melting temperature of 220°C to form a resin needle having a length of 50 mm, a cross-sectional area of 3 mm, and a modulus of elasticity at 80°C measured by preheating the strand of the resin composition in an 80°C environment for 5 minutes and performing a tensile test at 1 mm / min. 2 A resin needle having an elongation at 23°C of 1% or more as measured by subjecting a strand of the resin needle to a tensile test at 1 mm / min in an environment of 23°C. [7] The resin needle according to any one of [1] to [6], wherein the non-fibrous inorganic particles are layered minerals. [8] The resin needle according to [7], wherein the layered mineral is talc. [9] The resin needle according to any one of [1] to [8], wherein the resin needle is a medical needle.
[0007] As a result of extensive research, the present inventors have found that the resin needle of the present invention has excellent micro-moldability, puncture properties and heat resistance, which has led to the completion of the present invention.
[0008] 2A shows the shape of the resin needle 1 manufactured in the examples and comparative examples. FIG. 2B shows a detailed structure of the puncture part 10 of the resin needle 1 in FIG. 1, with FIG. 2A being a perspective view, FIG. 2B being a front view, and FIG. 2C being a plan view.
[0009] The following describes embodiments of the present invention. The various features shown in the following embodiments can be combined with each other. Furthermore, each feature can be an independent invention.
[0010] 1. Uses, Structure, and Manufacturing Method of Resin Needle A resin needle according to one embodiment of the present invention can be used for any purpose involving puncturing a target, and the target may be a living body or a non-living body. The resin needle is preferably a medical needle used in medical applications.
[0011] The shape of the resin needle is not particularly limited as long as it has a puncturing portion with puncture properties, and it may have a hollow structure or a solid structure. The puncturing portion of the resin needle may have a simple structure that tapers toward the tip, or may have a complex shape as disclosed in Patent Document 1. The resin needle preferably has a holder shaped to fit the casing of the puncture tool that holds the resin needle.
[0012] The radius of curvature of the tip of the puncture part is, for example, preferably 100 μm or less, more preferably 50 μm or less, and even more preferably 10 μm or less. This radius of curvature is, for example, 0.1 to 100 μm, specifically, for example, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 50, or 100 μm, and may be in a range between any two of the values exemplified here.
[0013] In order to achieve excellent puncture performance, resin needles must be molded to have a sharp tip, and it is desirable for them to have excellent micro-moldability. Furthermore, resin needles may be exposed to high-temperature environments during storage, sterilization, etc., and it is desirable that their puncture performance not be impaired even in high-temperature environments. The resin needle of this embodiment can solve these problems by being made of a resin composition having the composition shown below.
[0014] The resin needle can be produced by molding the resin composition shown below by a method such as injection molding.
[0015] 2. Composition of the Resin Needle The resin needle is made of a resin composition containing polylactic acid and non-fibrous inorganic particles.
[0016] Polylactic acid is a polymer containing components derived from lactic acid. The polylactic acid used in the resin composition of this embodiment has a weight-average molecular weight of 20,000 to 400,000, preferably 50,000 to 300,000, and more preferably 100,000 to 250,000. If the weight-average molecular weight is too small, puncture resistance tends to be poor, while if the weight-average molecular weight is too large, micro-moldability tends to be poor. Specific examples of this weight-average molecular weight are 20,000, 50,000, 100,000, 150,000, 200,000, 250,000, 300,000, 350,000, and 400,000, and may be in a range between any two of the values exemplified here. The weight-average molecular weight can be measured by gel permeation chromatography (GPC).
[0017] Lactic acid includes L-lactic acid and D-lactic acid, and polylactic acid contains one or both of an L-component, which is a component derived from L-lactic acid, and a D-component, which is a component derived from D-lactic acid. The polylactic acid used in the resin composition of this embodiment has a D-component ratio of 15% by mass or less or 85% by mass or more, more preferably 12% by mass or less or 90% by mass or more, and even more preferably 10% by mass or less or 95% by mass or more. The D-component ratio is the proportion of the D-component when the total of the L-component and the D-component is taken as 100% by mass. The closer the D-component ratio is to 50% by mass, the more difficult the polylactic acid is to crystallize. If the D-component ratio is more than 15% by mass or less than 85% by mass, the degree of crystallization may be too low. Specific examples of the D-isomer ratio are 0, 0.1, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, and 15% by mass, and may be between any two of the values exemplified herein or any value less than the range. Specific examples of the D-isomer ratio are 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 99.5, 99.9, and 100% by mass, and may be between any two of the values exemplified herein or any value greater than the range. The D-isomer ratio of a polylactic acid resin can be determined according to the method for measuring the D-isomer content described in "Voluntary Standards for Food Containers and Packaging Made of Polyolefins and Other Synthetic Resins, Third Edition, Revised Edition, June 2004 Supplement, Part 3, Hygiene Test Method, P12-13." Specifically, the method for measuring the D-form ratio of polylactic acid resin is as follows.
[0018] First, sodium hydroxide / methanol is added to precisely weighed polylactic acid, and the mixture is placed in a water bath shaker set to 65°C. Hydrolysis is continued until the resin content becomes a homogeneous solution. After hydrolysis is completed, dilute hydrochloric acid is added to the alkaline solution to neutralize it. The decomposed solution is dissolved in pure water, and a certain volume is then transferred to a measuring flask and diluted with a high-performance liquid chromatography (HPLC) mobile phase solution. The pH is adjusted to a range of 3 to 7, and the volumetric flask is metered and filtered through a membrane filter (0.45 μm). The D-lactic acid and L-lactic acid content of this adjusted solution can be determined by HPLC.
[0019] Non-fibrous inorganic particles are inorganic particles that are not fibrous. When fibrous inorganic particles are incorporated into a resin composition, if the fibrous inorganic particles remain on the skin, there is a risk of causing tumors, so the inorganic particles incorporated into the resin composition are non-fibrous. Examples of non-fibrous inorganic particles include layered minerals having a layered structure, such as talc and mica, and non-layered minerals not having a layered structure, such as calcium carbonate and hydroxyapatite. When the non-fibrous inorganic particles contain a layered mineral, the heat resistance tends to be good, so it is preferable that the non-fibrous inorganic particles contain a layered mineral. Furthermore, when the layered mineral is talc, the heat resistance tends to be particularly high, so it is preferable that the layered mineral is talc.
[0020] The non-fibrous inorganic particles have an average particle size of 0.05 to 20 μm, preferably 0.1 to 10 μm, and more preferably 0.2 to 8 μm. If the average particle size is too small, heat resistance tends to deteriorate, while if the average particle size is too large, micro-molding tends to deteriorate. Specifically, the average particle size may be, for example, 0.05, 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 μm, or may be within a range between any two of the values exemplified here. The average particle size refers to the particle size at 50% of the cumulative value in the particle size distribution determined by laser diffraction / scattering, and can be measured according to JIS R1629 "Method for measuring particle size distribution of fine ceramic raw materials by laser diffraction / scattering method."
[0021] The content of non-fibrous inorganic particles is 5 to 70 parts by weight per 100 parts by weight of polylactic acid. If this content is too low, the heat resistance of the resin needles tends to deteriorate, while if this content is too high, the micro-moldability tends to deteriorate. The content of non-fibrous inorganic particles per 100 parts by weight of polylactic acid is preferably 8 parts by weight or more, more preferably 15 parts by weight or more, and even more preferably 20 parts by weight or more. Furthermore, this content is preferably 60 parts by weight or less, more preferably 43 parts by weight or less, and even more preferably 35 parts by weight or less. Specific examples of this content include 5, 8, 10, 15, 20, 25, 30, 35, 40, 43, 45, 50, 55, 60, 65, and 70 parts by weight, and may be in a range between any two of the values exemplified here.
[0022] The resin composition of the present embodiment may contain a biocompatible resin other than polylactic acid. The biocompatible resin means a resin that has low toxicity to cells and high affinity with living organisms (human bodies and animals). Examples of such resins include polycarbonate, poly(meth)acrylic ester, polyvinyl chloride, polyethylene glycol, parylene, polyethylene, polypropylene, silicone, polyisoprene, fluororesin, polyetherimide, polyethylene oxide, polyethylene terephthalate, polyethylene succinate, polybutylene terephthalate, polybutylene succinate, polybutylene succinate carbonate, polyphenylene oxide, polyphenylene sulfide, polyformaldehyde, polyanhydride, polyamide (nylon 6, nylon 66), polybutadiene, polyvinyl acetate, polyvinyl alcohol, polyvinylpyrrolidone, polyesteramide, polyacrylonitrile, polysulfone, polyethersulfone, ABS resin, polyurethane (polyetherurethane, polyesterurethane, polyetherurethaneurea), polyvinylidene chloride, polystyrene, polyacetal, polybutadiene, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer polymers, ethylene propylene copolymers, polyhydroxyethyl methacrylate, polyhydrobutyrate, polyorthoesters, polyglycols, polycaprolactone, polylactic acid copolymers, polyglycolic acid-glycol copolymers, polycapronolactone copolymers, polydioxanone, perfluoroethylene-propylene copolymers, cyanoacrylate polymers, polybutyl cyanoacrylate, polyaryl ether ketone, epoxy resins, polyester resins, polyimides, phenolic resins), cellulose Examples of suitable sugars include starch, chitin / chitosan, agar, carrageenan, alginic acid, agarose, pullulan, mannan, curdlan, xanthan gum, gellan gum, pectin, xyloglucan, guar gum, lignin, oligosaccharides, hyaluronic acid, schizophyllan, lentinan, collagen, gelatin, keratin, fibroin, glue, sericin, vegetable proteins, milk proteins, orchid proteins, synthetic proteins, heparin, nucleic acids, sugars, candy, glucose, maltose, sucrose, and polymer alloys thereof.However, from the viewpoint of heat resistance, a resin with a softening point exceeding 80°C is preferable. Examples of poly(meth)acrylic acid esters include polymethyl methacrylate. The content of the biocompatible resin is preferably 50 parts by mass or less per 100 parts by mass of polylactic acid. If the content of the biocompatible resin is too high, micromolding properties tend to deteriorate. The content of the biocompatible resin per 100 parts by mass of polylactic acid is, for example, 1 to 50 parts by mass, specifically, for example, 1, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, and may be within a range between any two of the values exemplified here, or any of the values less than or equal to the range.
[0023] 3. Physical Properties of Resin Needles and Resin Compositions The resin needle has a crystallinity of 1 to 60%, preferably 3 to 55%, and more preferably 5 to 45% for the polylactic acid component. If the crystallinity is too low, heat resistance tends to be insufficient. If the crystallinity is too high, the resin needle tends to break easily, resulting in insufficient puncture performance. Specific examples of the crystallinity are 1, 3, 5, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, and 60%, and may be in a range between any two of the values exemplified here.
[0024] The crystallization temperature of the polylactic acid component of the resin needle is preferably above 80°C. In this case, the crystallization temperature is prevented from unintentionally increasing the crystallinity of the resin needle and impairing the flexibility of the resin needle. This crystallization temperature is, for example, 81 to 105°C, specifically, for example, 81, 82, 83, 84, 85, 86, 87, 88, 89, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100, 101, 102, 103, 104, or 105°C, and may be in a range between any two of the values exemplified here.
[0025] The degree of crystallinity and crystallization temperature of the polylactic acid component of the resin needle can be measured by differential scanning calorimetry, as will be described in detail in the Examples.
[0026] The resin composition of this embodiment preferably has an 80°C elastic modulus of 10 MPa or more. If this value is too small, the heat resistance decreases, the resin needle is easily deformed in a high-temperature environment, and the puncture ability when returned to room temperature is likely to be poor. The 80°C elastic modulus is, for example, 10 to 140 MPa, specifically, for example, 10, 15, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95, 100, 105, 110, 115, 120, 125, 130, 135, or 140 MPa, and may be in a range between any two of the values exemplified here.
[0027] The resin composition of this embodiment preferably has an elongation at 23°C of 1% or more. If this value is too small, puncture resistance is likely to be poor. The elongation at 23°C is, for example, 1 to 20%, and specifically, for example, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, 7.0, 7.5, 8.0, 8.5, 9.0, 9.5, 10, 11, 12, 12.5, 15, or 20%, and may be in a range between any two of the values exemplified here.
[0028] The 80°C elastic modulus and 23°C elongation can be measured by the method shown in the examples.
[0029] 1. Preparation of Materials The materials shown in Tables 1 to 3 were prepared for use in manufacturing resin needles.
[0030] <Polylactic Acid> PLLA (poly-L-lactic acid) and PDLA (poly-D-lactic acid) shown in Table 1 were prepared according to the following Production Examples. [Production Example 1-1] 100 parts by weight of L-lactide was charged into a reactor equipped with a stirrer, a nitrogen gas inlet tube, a thermometer, and a pressure reducer. The contents were heated to 190°C while introducing nitrogen gas into the reactor. 0.15 parts by weight of stearyl alcohol and 0.005 parts by weight of tin octoate were added, and polymerization was carried out at 190°C for 2 hours. Finally, the pressure was reduced to below 10 Pa, the monomer was removed, and the mixture was pelletized to obtain poly-L-lactic acid (PL-1). [Production Example 1-2] Poly-L-lactic acid (PL-2) was obtained by the same procedure as in Production Example 1-1, except that the amount of stearyl alcohol in Production Example 1-1 was changed to 0.1 parts by weight. [Production Example 1-3] Poly-L-lactic acid (PL-3) was obtained by the same procedure as in Production Example 1-1, except that the amount of stearyl alcohol in Production Example 1-1 was changed to 0.6 parts by weight. [Production Example 1-4] Poly-L-lactic acid (PL-4) was obtained by the same procedure as in Production Example 1-1, except that the amount of L-lactide and D-lactide in Production Example 1-1 were changed to 88 parts by weight and 12 parts by weight, respectively. [Production Example 1-5] Poly-L-lactic acid (PL-5) was obtained by the same procedure as in Production Example 1-1, except that the amount of stearyl alcohol in Production Example 1-1 was changed to 3 parts by weight. [Production Example 1-6] Poly-L-lactic acid (PL-6) was obtained by the same procedure as in Production Example 1-1, except that the amount of stearyl alcohol in Production Example 1-1 was changed to 0.07 parts by weight. [Production Example 1-7] Poly-L-lactic acid (PL-7) was obtained by the same procedure as in Production Example 1-1, except that the L-lactide and D-lactide were changed to 80 parts by weight and 20 parts by weight, respectively. [Production Example 1-8] Poly-D-lactic acid (PL-8) was obtained by the same procedure as in Production Example 1-1, except that the L-lactide was changed to 100 parts by weight of D-lactide.
[0031] <Non-fibrous inorganic particles> Talc (hydrated magnesium silicate) [Production Example 2-1] Talc ore was coarsely crushed using a jaw crusher to a particle size of 1 cm or less, and then finely crushed and classified using a pulverizer, an impact crusher with a built-in classifier. Subsequently, the resulting powder was classified using an air elutriation classifier to obtain talc (T-1). [Production Example 2-2] The talc powder from Production Example 2-1 before classification using the air elutriation classifier was recovered to obtain talc (T-2). [Production Example 2-3] Talc (T-1) obtained in Production Example 2-2 was crushed by dry jet crushing to obtain talc (T-3). [Production Example 2-4] Talc (T-1) obtained in Production Example 2-1 was crushed by dry jet crushing to obtain talc (T-4). [Production Example 2-5] Talc ore was roughly crushed to a particle size of 1 cm or less using a jaw crusher, and then finely crushed using a VX mill to obtain talc (T-5).
[0032] Mica M-1: San-esu Ointment Co., Ltd., model SJ-005 Calcium carbonate C-1: Asahikomatsu Co., Ltd., model MC-140 Hydroxyapatite A-1: Taihei Chemical Industry Co., Ltd., model HAP-200
[0033] <Other biocompatible resins> Polycarbonate PC-1: Mitsubishi Engineering Plastics, model S-3000 PMMA PM-1: Polymethyl methacrylate, Kuraray, model Parapet HR
[0034]
[0035]
[0036]
[0037] 2. Manufacturing of Resin Needles Resin needles 1 of the examples and comparative examples were manufactured in the shapes shown in Figures 1 and 2 using the method described below. The resin needle 1 includes a puncturing portion 10 that punctures a living body, and a holder 20. The holder 20 includes a main body 21, a pair of arms 22, 22 provided on both sides of the main body 21, and a rod 23 extending toward the base end of the main body 21. The holder 20 specifically had a shape that was compatible with the casing of the "Pinnix Light" puncturing device manufactured by Lightnix. The puncturing portion 10 had a shape that was compatible with embodiment 3 of Patent Document 1. Specifically, the total length L was 0.4 mm, the width W was 0.9 mm, the height H was 0.2 mm, the radius of curvature of the tip 11 was 3 μm, and the ridge angle θ was 18.3°.
[0038] <Examples and Comparative Examples Other Than Examples 14 and 15> The resin needles of the Examples and Comparative Examples other than Examples 14 and 15 were manufactured by pre-drying a resin composition obtained by blending the materials shown in Tables 1 to 3 in the proportions shown in Tables 4 to 6 at 80°C for 5 hours, then completely melting it at 220°C, which is a temperature above the melting point of polylactic acid, injecting it into a mold at 23°C, and cooling it for 10 seconds. The resin needles were not annealed.
[0039] Examples 14 and 15 The resin needles of Examples 14 and 15 were produced by pre-drying a resin composition obtained by blending the materials shown in Tables 1 to 3 in the proportions shown in Table 5 at 80°C for 5 hours, melting it at 220°C, injecting it into a mold at 100°C, holding it there for 300 seconds, and then cooling it to 23°C and cooling it for 10 seconds.
[0040]
[0041]
[0042]
[0043] 3. Measurement of physical properties of resin needles and resin compositions Physical properties of resin needles and resin compositions were measured by the methods described below.
[0044] <Crystallization degree and crystallization temperature of polylactic acid component of resin needle> Resin needles of the examples and comparative examples were cut into approximately 5 mg pieces to prepare measurement samples. Next, using a differential scanning calorimeter (Hitachi High-Tech Science, DSC7000X), the measurement samples were heated to 300 °C at 10 °C / min in a nitrogen atmosphere. The point at which the resin changes to a rubber-like state was measured as the glass transition point (Tg), the peak of the crystallization peak as the crystallization temperature (Tc), its crystallization energy (ΔHc), and the peak of the crystallization melting peak as the melting point (Tm) and its melting energy (ΔHm). The crystallization degree was calculated using the values of ΔHm and ΔHc according to the following formula 1. In formula (1), "93" refers to the melting energy (93 mJ / mg) of polylactic acid with 100% crystallinity, and "WtP" refers to the weight ratio of polylactic acid to the entire resin composition (weight of PLA / weight of the entire resin composition). Note that ΔHm and ΔHc derived from PLA are used in the calculation. It is preferable to know the Tc and Tm derived from PLA in advance, for example by measuring only PLA. Furthermore, the output values of ΔHm and ΔHc are output as energy per unit weight of the entire measurement sample, so they are calculated based on a weight including components other than PLA. Therefore, in order to calculate the crystallinity of the PLA component in the measurement sample, it is necessary to divide (ΔHm - ΔHc) by WtP. (Equation 1) Crystallinity (%) = [{(ΔHm - ΔHc) / WtP} / 93}] x 100
[0045] <Elastic modulus at 80°C> The resin compositions of the Examples and Comparative Examples were extruded at a melting temperature of 220°C to form a sample having a length of 50 mm and a cross-sectional area of 3 mm. 2 The strand was preheated in an 80°C environment for 5 minutes, and subjected to a tensile test at 1 mm / min to measure the modulus of elasticity, which was taken as the 80°C modulus of elasticity.
[0046] <23°C elongation> The resin compositions of the Examples and Comparative Examples were extruded at a melting temperature of 220°C to form a sample having a length of 50 mm and a cross-sectional area of 3 mm. 2 The strand was subjected to a tensile test at 1 mm / min in an environment of 23°C, and the elongation obtained by measuring the elongation was defined as the 23°C elongation.
[0047] 4. Evaluation The Examples and Comparative Examples were evaluated using the following methods. The resin needles of the Examples obtained good results in all evaluation items. On the other hand, the resin needles of the Comparative Examples obtained poor results in at least one evaluation item.
[0048] <Micro-moldability> Micro-moldability was evaluated according to the following criteria based on the presence or absence of shape defects when the resin needles of the Examples and Comparative Examples were visually observed. ◎: Details such as the needle tip are molded into the specified shape, and there are no problems with releasability when released from the mold. ○: Details such as the needle tip are molded into the specified shape, but adhesion to the mold is somewhat strong, and releasability is somewhat poor, but this does not pose a major problem in practical use. △: Details such as the needle tip are molded into the specified shape, but adhesion to the mold is strong, and damage may occur occasionally when releasing, but the needle can be used in practice. ×: Details such as the needle tip are not molded into the specified shape, and the needle cannot be used in practical use.
[0049] <Punctureability before heating / Punctureability after heating> A 1.0 mm thick silicone rubber with a rubber hardness of 50, an 8 μm thick aluminum foil, and a 1.5 mm thick silicone rubber with a rubber hardness of 50 were laminated in this order to produce a laminate. Next, the resin needles of the Examples and Comparative Examples were placed in the casing of a "Pinnix Lite" manufactured by Lightnix Co., Ltd., and the Pinnix Lite was pressed against the 1.0 mm silicone rubber side of the laminate. Based on whether puncture was possible, the puncture ability before heating was evaluated according to the following criteria. In addition, the resin needles of the Examples and Comparative Examples were left standing at 80°C for one week, and then a similar test was performed to evaluate the puncture ability after heating according to the following criteria. ⊚: Puncture of 1.0 mm or more was possible, and no needle deformation was observed. ○: Minor needle deformation was observed, but puncture of 1.0 mm or more was possible, and there was no problem in practical use. △: Significant needle deformation was observed, but puncture of 1.0 mm or more was possible, and practical use was possible. ×: Unable to puncture more than 1.0 mm, and therefore not suitable for practical use.
[0050] 1: resin needle, 10: puncture part, 11: tip part, 20: holder, 21: main body, 22: arm, 23: rod, H: height, W: width, L: total length, θ: ridge angle
Claims
1. A resin needle made of a resin composition, the resin composition containing polylactic acid and non-fibrous inorganic particles, the polylactic acid having a weight average molecular weight of 20,000 to 400,000 and a D-form ratio of 15 mass % or less or 85 mass % or more, the non-fibrous inorganic particles having an average particle size of 0.05 to 20 μm, and the content of the non-fibrous inorganic particles being 5 to 70 mass parts per 100 mass parts of the polylactic acid.
2. A resin needle as described in claim 1, wherein the resin composition contains a biocompatible resin other than the polylactic acid, and the content of the biocompatible resin is 50 parts by mass or less per 100 parts by mass of the polylactic acid.
3. A resin needle according to claim 1, wherein the crystallinity of the polylactic acid component of the resin needle is 1 to 60%.
4. A resin needle according to claim 1, wherein the crystallization temperature of the polylactic acid component of the resin needle is above 80°C.
5. The resin needle according to claim 1, wherein the resin composition is extruded at a melting temperature of 220° C. to have a length of 50 mm and a cross-sectional area of 3 mm 2 The resin needle has an 80°C elastic modulus of 10 MPa or more as measured by preheating a strand of the above in an 80°C environment for 5 minutes and carrying out a tensile test at 1 mm / min.
6. The resin needle according to claim 1, wherein the resin composition is extruded at a melting temperature of 220° C. to have a length of 50 mm and a cross-sectional area of 3 mm 2 A resin needle having a tensile test of a strand of the above described resin needle at 1 mm / min in a 23°C environment, the 23°C elongation measured being 1% or more.
7. A resin needle according to claim 1, wherein the non-fibrous inorganic particles are layered minerals.
8. A resin needle according to claim 7, wherein the layered mineral is talc.
9. A resin needle according to any one of claims 1 to 8, wherein the resin needle is a medical needle.
Citation Information
Patent Citations
Resin composition and medical tubular body
JP2017179234A
Synthetic resin needles and synthetic resin composition for needles
WO2007037164A1
Sensor with fine needle having channel formed therein
WO2010013598A1