Coating film and article
The coated film, utilizing urethane acrylate and a surface conditioner with low organic solvent content and antibacterial/antiviral agents, addresses the challenges of durability and protection in touch panels and other applications, offering superior optical and mechanical properties and antibacterial/antiviral functionality.
Patent Information
- Application Number
- PCT/JP2024/011656
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional water-based coating agents for touch panels and other applications struggle to achieve durability and optical clarity, mechanical strength, and antibacterial/antiviral properties, while also minimizing organic solvent use for environmental and health considerations.
A coated film with a base layer and a coat layer formed using a urethane acrylate material and a surface conditioner, with a residual organic solvent content of 50 ppm or less, and incorporating a particulate antibacterial/antiviral agent, which provides excellent optical and mechanical properties and antibacterial/antiviral functionality.
The coated film achieves optical and mechanical properties comparable to those using conventional organic solvents, while ensuring a low organic solvent residue and effective antibacterial and antiviral protection, making it suitable for various applications including touch panels and surface protection.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Coated films and articles
[0001] The present invention relates to a coated film having a substrate layer and a coating layer, and an article including the coated film.
[0002] In recent years, touch panels and the like that serve as both a display device and an input means have come into widespread use in various electronic devices. A coated film having a coating layer is often provided on the surface of these touch panels to prevent scratches and other damage. In addition to touch panels, coated films are often provided on the surfaces of interior and exterior components of vehicles (automobiles, railroad cars, etc.), transport aircraft (passenger planes, cargo planes, etc.), ships, and buildings to prevent scratches and other damage. Furthermore, coated films are often provided on surface protection films that are used to protect the surface of an object to which they are attached until they are peeled off during use.
[0003] Conventionally, the coating layer of such a coated film has generally been formed using a coating layer-forming composition (coating agent) containing a large amount of organic solvent. However, in recent years, from the viewpoints of promoting the SDGs, consideration for the environment, and promoting the health of workers, there has been a social demand for reducing the amount of organic solvent used. As a coating agent using a reduced amount of organic solvent, for example, a coating agent (aqueous coating agent) using water or a mixed solvent (aqueous solvent) consisting of water and a water-compatible organic solvent as the solvent is known.
[0004] However, when using conventional water-based coating agents, it has sometimes been difficult to form a coating layer having the durability required for optical applications such as display devices, transportation equipment applications such as vehicles, transport aircraft, and ships, architectural applications, surface protection applications for various articles, etc. Furthermore, since there are only a limited number of polymerization initiators and leveling agents that can be used in water-based coating agents, thermosetting water-based coating agents have become mainstream, and it has often been difficult to form a coating layer having excellent optical properties and mechanical strength.
[0005] Therefore, there has been a demand for a coated film obtained using an environmentally friendly water-based coating agent that has optical and mechanical properties equivalent to those of a coating layer obtained using a coating agent containing an organic solvent.
[0006] In relation to the present invention, Patent Documents 1 to 3 describe laminates having a hydrophilic coating layer formed using a coating agent containing an aqueous solvent as the solvent. However, these documents do not state that the resulting laminates have excellent interlayer adhesion even after being placed in a harsh environment, or that they have excellent transmission clarity. Furthermore, it is difficult to say that the optical properties and mechanical properties of these laminates are excellent enough to be used suitably in optical displays such as touch panels.
[0007] Meanwhile, the threat of viral infections, such as the COVID-19 pandemic caused by the novel coronavirus (SARS-CoV-2), has become a major global issue. In this situation, for example, if a virus adheres to the surface of a touch panel, touching the surface of the touch panel with a finger could result in the virus entering the body through the finger and causing infection. Therefore, it is desirable to impart high antiviral properties (the ability to inactivate viruses adhering to the film surface and inhibit viral proliferation) in addition to antibacterial properties to the surface of touch panels that are touched by human fingers, etc.
[0008] JP 2018-180099 A (WO2018 / 185590A1) JP 2020-104499 A JP 2020-168764 A (US2022 / 0145029A1)
[0009] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide an environmentally friendly coated film that has a coating layer with a small amount of residual organic solvent and excellent optical properties and mechanical properties, a coated film that also has excellent antibacterial and antiviral properties, and an article including the coated film.
[0010] In order to solve the above-mentioned problems, the present inventors conducted extensive research into coated films having a substrate layer and a coating layer. As a result, they discovered that a coated film in which (α) the coating layer is formed from a coating layer-forming composition containing a urethane acrylate material and a surface modifier, (β) the coating layer has a residual organic solvent content of 50 ppm or less, and (γ) the transmission clarity is 50 or more, has excellent coatability of the coating layer-forming composition, and has optical and mechanical properties equivalent to those of coated films obtained using conventional organic solvents. Furthermore, they discovered that adding a water-soluble antibacterial / antiviral agent can produce a coated film with excellent antibacterial and antiviral properties, leading to the completion of the present invention.
[0011] Thus, according to the present invention, the following coated films [1] to [9] and articles
[10] and
[11] are provided.
[0012] [1] A coated film having a base layer and a coating layer, characterized in that the transmitted light clarity is 50 or more, the coating layer is formed from a coating layer-forming composition containing the following components (A) and (B), and the amount of residual organic solvent in the coating layer is 50 ppm or less: Component (A): urethane acrylate-based material Component (B): surface conditioner
[0013] [2] The coated film according to [1], wherein the component (A) is an emulsion containing emulsified particles of a urethane acrylate having an average particle size of 300 nm or less and 5 or more active energy ray-polymerizable functional groups.
[0014] [3] The coated film according to [1], wherein the component (B) is a water-soluble leveling agent and / or surfactant.
[0015] [4] The coated film according to [1], wherein the content of the component (B) in the composition for forming the coating layer is 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the component (A).
[0016] [5] The coated film according to [1], wherein the surface of the coating layer opposite to the substrate layer has a water contact angle of 70° or more.
[0017] [6] The coated film according to [1], wherein the composition for forming the coating layer further contains a filler as component (C).
[0018] [7] The coated film according to [1], wherein the composition for forming the coating layer further contains a particulate antibacterial and antiviral agent as component (D).
[0019] [8] The coated film according to [7], wherein the particulate antibacterial and antiviral agent has an average particle size of 0.5 μm or more and 5 μm or less, and the coating layer has a thickness of 5 μm or less.
[0020] [9] The coated film according to [7], which has an antibacterial activity value of 2.0 or more in an antibacterial test in accordance with JIS Z2801:2010, and an antiviral activity value of 2.0 or more in an antiviral test in accordance with ISO 21702.
[0021]
[10] An article comprising the coated film according to any one of [1] to [9].
[0022]
[11] The article according to
[10] , which is any one of an optical display, a vehicle, a transport aircraft, a ship, a building, and a surface protection film.
[0023] According to the present invention, an environmentally friendly coated film is provided, which has a coating layer with a small amount of residual organic solvent and excellent optical and mechanical properties. Furthermore, according to the present invention, a film having a coating layer obtained using an environmentally friendly aqueous coating agent is provided, which has coatability equivalent to that obtained when produced using an organic solvent, and has optical and mechanical properties equivalent to those of a coated film having a coating layer formed using a conventional organic solvent. Furthermore, according to the present invention, by optionally adding a particulate antibacterial and antiviral agent, a coated film is provided that has excellent antibacterial and antiviral properties in addition to excellent optical and mechanical properties.
[0024] The coated film of the present invention can be suitably used in various articles such as optical displays, vehicles, transport aircraft, ships, buildings, and surface protection films. In optical displays, it can be particularly suitably used for touch panels. In vehicles, transport aircraft, and ships, it can be particularly suitably used for windows, license plates, exteriors, and the like. In buildings, it can be suitably used on the surfaces of interior and exterior members. Furthermore, in the case of surface protection films, it can suitably protect the surfaces of various objects to be protected until use.
[0025] The present invention will be described in detail below, divided into the following sections: 1) a coated film, and 2) an article including a coated film.
[0026] 1) Coated Film The coated film of the present invention is a coated film having a base layer and a coating layer, and has a transmission clarity of 50 or more, and the coating layer is preferably formed from a coating layer-forming composition containing component (A): a urethane acrylate material and component (B): a surface conditioner, and the amount of residual organic solvent in the coating layer is preferably 50 ppm or less. The coated film of the present invention has excellent optical properties and mechanical properties, and is an environmentally friendly coated film with an extremely small amount of residual organic solvent.
[0027] 1. Substrate Layer The coated film of the present invention has a substrate layer. As the substrate layer, a film appropriately selected from known resin films conventionally used as optical films can be used.
[0028] Examples of resin materials constituting the resin film include polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene, polypropylene, viscose, diacetyl cellulose, triacetyl cellulose, acetyl cellulose butyrate, polyvinyl chloride, polyvinylidene chloride, polyvinyl alcohol, ethylene-vinyl acetate copolymer, polystyrene, polycarbonate, polymethylpentene, polysulfone, polyether ether ketone, polyether sulfone, polyetherimide, polyimide, fluororesin, polyamide, acrylic resin, norbornene-based resin, and cycloolefin resin. Among these, polyethylene terephthalate (PET), polycarbonate, triacetyl cellulose, and cycloolefin resin are preferred, with polyethylene terephthalate and triacetyl cellulose being more preferred, from the viewpoint of excellent transparency and adhesion, excellent heat resistance, and mechanical strength, and from the viewpoint of easily satisfying the optical properties described below. Furthermore, from the viewpoint of the SDGs, materials with a high biomass content may be used as the material constituting the resin film, and materials that can be recycled or reused, or recycled or reused materials may also be used.
[0029] The substrate layer may be a single-layer or two or more-layer resin film. When forming a coating layer or the like on the substrate layer, the surface of the substrate layer may be subjected to a physical treatment such as a corona discharge treatment or an oxidation treatment in order to improve adhesion.
[0030] The thickness of the substrate layer can be selected as desired depending on the purpose and is not particularly limited, but is preferably 25 to 500 μm, more preferably 40 to 400 μm, particularly preferably 60 to 300 μm, even more preferably 80 to 250 μm, and most preferably 120 to 220 μm, and most preferably 130 to 200 μm. This tends to increase the scratch resistance and hardness of the coated film. In addition, the handleability of the resulting coated film is improved, resulting in an excellent usability when applied.
[0031] 2. Coating Layer The coated film of the present invention has a coating layer in addition to the base layer. This coating layer (sometimes referred to herein as the "coating layer according to the present invention") is preferably a layer formed from a coating layer-forming composition (sometimes referred to herein as the "coating layer-forming composition according to the present invention") containing component (A): a urethane acrylate-based material and component (B): a surface conditioner.
[0032] (1) Component (A) The coating layer-forming composition according to the present invention preferably contains a urethane acrylate material as component (A). Examples of urethane acrylates include those obtained by reacting a hydroxyl group-containing (meth)acrylate compound with a polyvalent isocyanate compound, and those obtained by reacting an isocyanate group-containing (meth)acrylate compound with a polyol compound. Among these, oligomers having urethane bonds formed by reacting an isocyanate group with a hydroxy group and an acrylic group are preferred. For example, they can be obtained by esterifying a polyurethane oligomer obtained by reacting a polyether polyol or polyester polyol with a polyisocyanate with (meth)acrylic acid. In this specification, (meth)acrylic refers to both acrylic and methacrylic. The same applies to other similar terms.
[0033] The urethane acrylate used in the present invention has an active energy ray-polymerizable functional group. The active energy ray-polymerizable functional group is a group that has the property of crosslinking and curing when irradiated with active energy rays such as ultraviolet rays and electron beams. Examples of the active energy ray-polymerizable functional group include functional groups containing a vinyl group, a (meth)acryloyl group, an epoxy group, an oxetane group, an isocyanate group, and the like.
[0034] The number of active energy ray-polymerizable functional groups possessed by the urethane acrylate is preferably 5 or more, more preferably 6 to 20, even more preferably 8 to 16, and particularly preferably 9 to 12. This makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below.
[0035] The urethane acrylate material of component (A) is not particularly limited in its form, etc., as long as it contains a urethane acrylate, preferably a urethane acrylate having five or more active energy ray-polymerizable functional groups, and is capable of forming a coating layer having an amount of residual organic solvent of 50 ppm or less using a coating layer-forming composition containing component (A).
[0036] In the present invention, the urethane acrylate material of component (A) is preferably an emulsion containing emulsified particles of urethane acrylate, more preferably an emulsion containing emulsified particles of urethane acrylate having five or more active energy ray-polymerizable functional groups. The emulsion containing emulsified particles of urethane acrylate is preferably a so-called oil-in-water emulsion in which an acrylic component lacking hydrophilic groups is emulsified in a state where it is surrounded by a urethane component having hydrophilic groups. Emulsions containing emulsified particles of urethane acrylate have good stability over time, can be diluted with water without using organic solvents that are harmful to the human body and the environment, and also have good coatability to resin substrates, etc. By using such a material as component (A), it is possible to form a coating layer using an environmentally friendly aqueous solvent without using an organic solvent, as described below. Furthermore, the resulting coating layer is likely to have optical and mechanical properties equivalent to those of coating layers obtained using conventional organic solvents.
[0037] The average particle size of the emulsified particles contained in the emulsion is preferably 300 nm or less. This makes it easier to obtain a coating layer having optical and mechanical properties equivalent to those formed using a coating layer-forming composition containing a large amount of organic solvent, even when the amount of organic solvent used is reduced. Furthermore, the resulting coating layer (and coated film) is more likely to satisfy the physical properties described below. From this perspective, the average particle size is preferably 5 to 260 nm, more preferably 10 to 220 nm, even more preferably 20 to 200 nm, and particularly preferably 30 to 180 nm. The average particle size of the emulsified particles can be measured by dynamic light scattering.
[0038] An emulsion containing emulsified particles of urethane acrylate can be produced by a conventionally known method, for example, by emulsifying and dispersing a mixture obtained by mixing an oil-soluble substance, urethane acrylate, with a water-soluble substance containing an aqueous solvent and an emulsifier in a predetermined ratio using a high-speed agitator such as a homomixer or a sand mill or a microfluidizer, or by passing the mixture through a porous membrane (see, for example, JP-A-5-320283, JP-A-2005-247884, and Japanese Patent No. 7033232).
[0039] In the present invention, commercially available urethane acrylate emulsions can also be used. Examples of commercially available products include ART RESIN WEH-1 (manufactured by Negami Chemical Industrial Co., Ltd.), BEAMSET EM-94 (manufactured by Arakawa Chemical Industries, Ltd.), and BEAMSET EM-90 (manufactured by Arakawa Chemical Industries, Ltd.). The urethane acrylate materials can be used alone or in combination of two or more.
[0040] (2) Component (B) The coating layer-forming composition according to the present invention preferably contains a surface conditioner as component (B). This makes it easier to form a coating layer with excellent appearance. In the present invention, as described below, an aqueous solvent is preferably used in accordance with the object of the present invention, and therefore the surface conditioner used is preferably water-soluble.
[0041] The content of component (B) in the coating layer (coating layer-forming composition) is preferably 0.1 to 20 parts by mass, more preferably 0.3 to 10 parts by mass, even more preferably 0.6 to 7 parts by mass, particularly preferably 0.8 to 4 parts by mass, and even more preferably 1 to 3 parts by mass, per 100 parts by mass of component (A). This makes it easier to obtain a coating layer with excellent mechanical properties and to satisfy the physical properties described below.
[0042] Examples of the surface conditioner include a leveling agent, a surfactant, etc. The surface conditioner may be used alone or in combination of two or more.
[0043] <Leveling Agent> It is preferable to include a leveling agent as a surface conditioner in the coating layer-forming composition. This effectively suppresses the occurrence of repelling, streaks, etc. when the coating layer-forming composition is applied to a substrate, and allows the formation of a coating layer with a uniform film thickness and good appearance. In addition, the use of a leveling agent makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below.
[0044] The leveling agent is preferably a water-soluble leveling agent. Here, the water-soluble leveling agent refers to one that does not produce any visible cloudiness or separation when mixed with water in a 1:1 mass ratio at 25°C.
[0045] Preferred examples of the leveling agent include water-soluble polyether-modified silicone leveling agents, acrylic leveling agents, and fluorine-based leveling agents. The polyether-modified silicone leveling agent is a compound in which a portion of the substituents bonded to silicon atoms in the siloxane structure is substituted with an organic group having an alkylene oxide. The acrylic leveling agent is, for example, a compound obtained by copolymerizing a monomer having a (meth)acryloyl group. The fluorine-based leveling agent is a compound having a perfluoroalkyl group or a fluorinated alkenyl group in the main chain or side chain.
[0046] As the leveling agent, commercially available products can be suitably used. Commercially available polyether-modified silicone leveling agents include BYK-348 and BYK-3530 (both manufactured by BYK Japan). Commercially available acrylic leveling agents include BYK-381 and BYK-3441 (both manufactured by BYK Japan). Commercially available fluorine-based leveling agents include Megafac F-477, Megafac F-553, Megafac F-555-A, Megafac F-557, Megafac F-559, Megafac F-569 (all manufactured by DIC Corporation). The leveling agents can be used alone or in combination of two or more.
[0047] When a leveling agent is used as the surface conditioner, the blending ratio thereof is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 8 parts by mass, even more preferably 0.3 to 5 parts by mass, and particularly preferably 0.4 to 3 parts by mass, per 100 parts by mass of component (A). This allows for a sufficient leveling effect to be obtained. In particular, this makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below.
[0048] <Surfactant> It is also preferable to include a surfactant as a surface conditioner in the coating layer-forming composition. The surfactant is suitably used, for example, when a filler described later is used. Specifically, when a filler with low water affinity is used in an aqueous solvent described later, the use of a surfactant improves the dispersibility of the filler, thereby improving the transmission clarity and antiglare properties of the resulting coating layer.
[0049] Examples of the surfactant include known surfactants such as anionic surfactants, cationic surfactants, nonionic surfactants, amphoteric surfactants, silicone surfactants, fluorine-based surfactants, etc. Among these, nonionic surfactants are preferred from the viewpoint of easily achieving the effects of the present invention.
[0050] Examples of nonionic surfactants include ether-based surfactants such as polyoxyethylene nonylphenyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene oleyl ether, and polyoxyethylene alkyl ether; ester-based surfactants such as polyoxyethylene oleate, polyoxyethylene distearate, sorbitan laurate, sorbitan monostearate, sorbitan monooleate, and polyoxyethylene stearate; acetylene glycol-based or acetylene alcohol-based surfactants such as 2,4,7,9-tetramethyl-5-decyne-4,7-diol, 3,6-dimethyl-4-octyne-3,6-diol, and 3,5-dimethyl-1-hexyn-3-ol; and polyglycol ether-based surfactants. Among these, acetylene glycol-based or acetylene alcohol-based surfactants are preferred. Commercially available products of these surfactants include Olfine PD-201, Olfine PD-003, Olfine PD-301, and Olfine AF103 (all manufactured by Nissin Chemical Industry Co., Ltd.). The surfactants can be used alone or in combination of two or more.
[0051] When a surfactant is used, the blending ratio thereof is preferably 0.1 to 10 parts by mass, more preferably 0.2 to 4 parts by mass, even more preferably 0.3 to 3 parts by mass, and particularly preferably 0.4 to 2 parts by mass, per 100 parts by mass of component (A). This allows the surfactant's effects to be fully obtained. In particular, this makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below.
[0052] (3) Component (C) The coating layer-forming composition according to the present invention preferably contains a filler as component (C) in addition to the components (A) and (B). By containing a filler, it becomes easier to adjust the optical properties of the coating layer, such as the haze value, to desired values. In addition, the resulting coating layer (and coated film) is more likely to satisfy the physical properties described below, and in particular, antiglare properties can be imparted to the resulting coated film.
[0053] Examples of fillers include inorganic fillers such as silica, calcium carbonate, aluminum hydroxide, magnesium hydroxide, clay, talc, and titanium dioxide; organic fillers made of resins such as acrylic resin, polystyrene resin, polyethylene resin, and epoxy resin; and organic-inorganic fillers made of silicon-containing compounds having an intermediate structure between inorganic and organic.
[0054] The shape of the filler may be regular, such as spherical, or may be irregular, with no particular shape. From the viewpoint of easily obtaining desired optical properties, the average particle size of the filler is preferably 0.1 to 10 μm, more preferably 0.5 to 7 μm, particularly preferably 0.8 to 5 μm, even more preferably 1.0 to 4 μm, and of these, preferably 1.2 to 3 μm.
[0055] As the filler, commercially available products such as Seahoster KE-P250 and Seahoster KE-S150 (both manufactured by Nippon Shokubai Co., Ltd.), and Sylysia 530 (manufactured by Fuji Silysia Chemical Ltd.) can also be used. These fillers may be used alone or in combination of two or more.
[0056] When a filler is used, the content thereof is preferably 0.1 to 60 parts by mass, more preferably 0.5 to 45 parts by mass, even more preferably 1 to 30 parts by mass, particularly preferably 3 to 20 parts by mass, and of these, preferably 4 to 15 parts by mass, per 100 parts by mass of component (A). This makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below, and in particular, makes it easier for the optical properties, such as antiglare properties, to be exhibited.
[0057] (4) Component (D) The coating layer-forming composition according to the present invention preferably contains an antibacterial / antiviral agent as component (D) in addition to components (A) and (B). This allows the resulting coated film to exhibit antibacterial / antiviral properties. Here, the term "antibacterial / antiviral agent" refers to an agent that exhibits antibacterial and / or antiviral properties. Antibacterial properties refer to the ability to kill or eliminate bacteria and fungi, or to inhibit their occurrence, growth, and proliferation. Antiviral properties refer to the ability to inactivate viruses and inhibit their proliferation. In the present invention, the antibacterial / antiviral agent preferably has both antibacterial and antiviral properties.
[0058] The shape of component (D) is not particularly limited, and may be regular or irregular. From the viewpoint of easily exhibiting antibacterial and antiviral properties, a regular shape is preferred, and particulate shape is particularly preferred. Particulate shape includes any shape, such as spherical, polyhedral, confetti-like, cocoon-like, and flat. When the antibacterial and antiviral agent is particulate, its average particle size is preferably 0.1 to 5 μm, more preferably 0.4 to 3 μm, and even more preferably 0.8 to 2 μm. The average particle size can be measured by laser diffraction. By setting the average particle size within this range and setting the coating layer thickness to 5 μm or less, as described below, antibacterial and antiviral properties can be better expressed.
[0059] Bacteria targeted by the antibacterial / antiviral agent are not particularly limited, and examples thereof include Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, etc. Viruses targeted by the antibacterial / antiviral agent may be enveloped or non-enveloped viruses. Examples of enveloped viruses include influenza virus, SARS-CoV-2, herpes virus, rubella virus, hepatitis B virus, hepatitis C virus, AIDS virus, human immunodeficiency virus, etc. Examples of non-enveloped viruses include norovirus, rotavirus, poliovirus, adenovirus, feline calicivirus, etc.
[0060] Examples of antibacterial and antiviral agents include organic antibacterial and antiviral agents and inorganic antibacterial and antiviral agents. Among these, it is preferable to use antibacterial and antiviral agents with high water dispersibility. Examples of organic antibacterial and antiviral agents include those comprising a resin base and a group having antibacterial and antiviral properties, such as an anionic group, a cationic group, or an ether group. Examples of anionic groups include sulfonic acid groups, phosphate groups, carboxyl groups, hydroxyl groups, and nitro groups. Examples of cationic groups include quaternary amino groups. Examples of ether groups include alkyl ether groups such as ethyl ether groups and propyl ether groups. The resin base is preferably a polymer of a monomer having a vinyl group. Examples of monomers having a vinyl group include styrene, (meth)acrylic acid esters, divinylbenzene, and trivinylbenzene.
[0061] The inorganic antiviral agent is preferably an inorganic particle containing at least one selected from the group consisting of antibacterial and antiviral metal oxides, metal salts (including double salts; the same applies hereinafter), and metal ion carriers. Examples of metal oxides include silver oxide, zinc oxide, copper oxide, iron oxide, titanium oxide, tin oxide, tungsten oxide, chromium oxide, zirconium oxide, and molybdenum oxide. Among these, silver oxide, zinc oxide, copper(I) oxide, and copper(II) oxide are preferred.
[0062] The metal salt is preferably a salt of a Group 11 element such as silver or copper, a Group 12 element such as zinc, or a Group 6 element such as molybdenum, and more preferably a salt of silver, copper, zinc, or molybdenum. Preferred metal salts include silver salts such as silver nitrate, silver acetate, and silver sulfate; copper salts such as copper nitrate, copper acetate, and copper sulfate; zinc salts such as zinc nitrate, zinc acetate, and zinc sulfate; alkali metal salts of molybdenum oxoacids such as sodium molybdate, potassium molybdate, lithium molybdate, sodium polymolybdate, and sodium isopolymolybdate; ammonium molybdate; and the like.
[0063] Examples of metal ions in the metal ion carrier include silver ions, copper ions, zinc ions, etc. Examples of carriers that can support these metal ions include ion exchangers such as zeolite, silica gel, clay minerals, zirconium phosphate, calcium phosphate, calcium apatite, calcium silicate, magnesium aluminosilicate, titanium oxide, potassium titanate, silica-alumina, soluble glass, thiosulfite, and metals. One type of antibacterial and antiviral agent may be used alone, or two or more types may be used in combination.
[0064] These antibacterial and antiviral agents may be commercially available products, such as Novalon AG1100 (manufactured by Toagosei Co., Ltd.), Ion Pure (manufactured by Ishizuka Glass Co., Ltd.), and Willtaker VM (manufactured by Sekisui Material Co., Ltd.).
[0065] The content of component (D) in the coating layer (coating layer-forming composition) is preferably 0.1 to 40 parts by mass, more preferably 0.5 to 30 parts by mass, even more preferably 1 to 25 parts by mass, particularly preferably 2 to 20 parts by mass, and of these, preferably 3 to 15 parts by mass, relative to 100 parts by mass of component (A). This makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below and, in particular, makes it easier for them to exhibit excellent antibacterial and antiviral properties.
[0066] (4) Other Components [Component (E)] The coating layer-forming composition according to the present invention may contain another component [component (E)] in addition to the components (A) to (D). Preferred examples of component (E) include a photopolymerization initiator.
[0067] The use of a photopolymerization initiator can reduce the amount of light irradiation and the polymerization and curing time when forming a coating layer. In particular, when crosslinking is carried out by irradiation with active light such as ultraviolet light as the active energy ray, the presence of a photopolymerization initiator is preferred.
[0068] The photopolymerization initiator used is preferably one that can exist stably in an emulsion of a urethane acrylate having an active energy ray-polymerizable functional group and that initiates polymerization of the urethane acrylate having an active energy ray-polymerizable functional group upon irradiation with active energy rays.
[0069] Examples of the photopolymerization initiator include benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, benzophenone, p-phenylbenzophenone, 2-methylanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, benzyl dimethyl ketal, p-dimethylaminobenzoic acid ester, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinopropan-1-one, lithium phenyl-2,4,6-trimethylbenzoylphosphinate, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone, eosin Y, N-vinylpyrrolidone, triethanolamine, and 1-hydroxycyclohexyl phenyl ketone.
[0070] Among these, it is preferable to use a water-soluble photopolymerization initiator such as 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone. Commercially available products include OMNIRAD2959 (manufactured by IGM RESINS) and H1361 (manufactured by Tokyo Chemical Industry Co., Ltd.). The photopolymerization initiator may be used alone or in combination of two or more.
[0071] When a photopolymerization initiator is used, the blending ratio thereof is preferably 0.1 to 20 parts by mass, more preferably 0.2 to 10 parts by mass, and even more preferably 1.0 to 7 parts by mass, per 100 parts by mass of component (A), which makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties (particularly scratch resistance and hardness) described below.
[0072] The coating layer-forming composition according to the present invention may further contain other additives such as antioxidants, ultraviolet absorbers, silane coupling agents, light stabilizers, antifoaming agents, infrared absorbers, colorants, and antistatic agents, as long as they do not affect the effects of the present invention.
[0073] (5) Formation of Coating Layer The coating layer can be formed by applying (coating) a composition for forming a coating layer onto the surface of the substrate layer or another layer laminated on the substrate layer, and irradiating the resulting coating film with active energy rays to cure the coating film.
[0074] The coating layer-forming composition can be prepared by adding the above-mentioned essential components (A) and (B), and, if desired, the components (C), (D), and other components, to a solvent and dissolving or dispersing these components.
[0075] In the present invention, from the viewpoints of promoting the SDGs, reducing the environmental load, and managing the health of workers, the solvent used is preferably an aqueous solvent with a reduced content of organic solvent, and more preferably water.
[0076] Examples of the aqueous solvent include water and a mixed solvent of water and a water-compatible organic solvent. Examples of the water-compatible organic solvent include alcohols such as methanol, ethanol, and isopropanol; ketones such as acetone and methyl ethyl ketone; cellosolves such as methyl cellosolve; amides such as N,N-dimethylformamide; and ethers such as tetrahydrofuran.
[0077] The amount of solvent used can be determined appropriately so that the coating layer-forming composition according to the present invention has a concentration and viscosity suitable for forming a coating film. Typically, the amount is 10 to 500 parts by mass, preferably 30 to 300 parts by mass, and more preferably 50 to 200 parts by mass, per 100 parts by mass of component (A).
[0078] The method for applying the coating layer-forming composition to the surface of the substrate layer or another layer laminated on the substrate layer is not particularly limited, and any conventionally known method can be used, such as bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, etc. The coating film is preferably dried at 40 to 120°C for about 30 seconds to 5 minutes.
[0079] The coating layer-forming composition according to the present invention has excellent coatability, i.e., it is possible to form a coating film of uniform thickness without causing cissing or streaky or dot-like defects during coating.
[0080] The coating film can then be cured by irradiating it with active energy rays to form a coating layer. Examples of active energy rays used to cure the coating film include ultraviolet rays; electron beams; laser light such as semiconductor lasers, argon lasers, and He—Cd lasers; and ionizing radiation such as α rays, β rays, γ rays, neutron beams, X-rays, and accelerated electron beams. Among these, ultraviolet rays and electron beams are preferred as active energy rays, as they can be generated using a relatively simple device, and ultraviolet rays are more preferred.
[0081] When ultraviolet rays are used as the active energy rays, the ultraviolet light source may be an ultra-high pressure mercury lamp, a high pressure mercury lamp, a low pressure mercury lamp, a carbon arc, a black light lamp, a metal halide lamp, or the like.
[0082] The amount of ultraviolet light is 50 to 1,000 mJ / cm 2 is preferably 100 to 700 mJ / cm 2 The illuminance of the ultraviolet light is usually 100 to 1000 mW / cm. 2 is preferably 200 to 700 mW / cm 2 The irradiation time is usually from 1 second to 1 hour, and the irradiation temperature is usually from 20 to 100°C.
[0083] The electron beam irradiation can be carried out by an electron beam accelerator, etc. The irradiation dose of the electron beam is preferably 10 to 1000 krad.
[0084] The irradiation with active energy rays can be carried out in an air atmosphere or an inert gas atmosphere, such as nitrogen, argon, or helium.
[0085] The thickness of the resulting coating layer can be selected as desired depending on the purpose and application, but is typically 0.1 to 50 μm, preferably 0.5 to 30 μm, more preferably 1 to 20 μm, even more preferably 2 to 10 μm, and most preferably 3 to 7 μm. This makes it easier for the resulting coating layer (and coated film) to satisfy the physical properties described below. When the coating layer contains the above-mentioned component (C), having such a thickness makes it easy to adjust the coating layer so that it exhibits the desired antiglare properties. Note that if the coating layer thickness is less than 0.1 μm, it may be difficult to obtain the hardness required for practical use.
[0086] From the viewpoint of environmental considerations, the amount of residual organic solvent in the coating layer according to the present invention is preferably 50 ppm or less, preferably 30 ppm or less, more preferably 10 ppm or less, and particularly preferably 1 ppm or less. In order to keep the amount of residual organic solvent within the above range, it is preferable to use an aqueous solvent with a low organic solvent content, preferably water, as the solvent when forming the coating layer. The amount of residual organic solvent can be calculated by cutting the coated film (coating layer) into a size of 4 cm x 5 cm, heating it at 120°C for 20 minutes, and measuring the amount of vaporized solvent by gas chromatography (apparatus name "GC-2010" manufactured by Shimadzu Corporation).
[0087] (6) Other Layers The coated film of the present invention may be provided with other layers such as a primer layer, an anti-reflection layer, and an adhesive layer depending on the purpose.
[0088] In the coated film of the present invention, a primer layer may be provided between the substrate layer and the coating layer. This serves to enhance the adhesion between the substrate layer and the coating layer. The primer layer is formed, for example, by applying a reactive coating liquid containing a polyester polyol or polyether polyol and a polyisocyanate to the surface of the substrate layer at a rate of 0.5 to 2 g / m. 2It can be formed by coating.
[0089] In the coated film of the present invention, the antireflection layer may be provided at a position where it can exhibit the desired performance, such as the side of the coating layer opposite the substrate layer side. This serves to eliminate screen glare caused by reflection from sunlight, fluorescent lights, etc., and to improve transparency by suppressing surface reflectance. Depending on the type of antireflection layer, it may also be possible to improve antistatic properties.
[0090] In the coated film of the present invention, the adhesive layer may be provided on the side of the substrate layer opposite to the side having the coating layer. This allows the adhesive layer to be well attached to the surface of the touch panel. The adhesive constituting the adhesive layer is not particularly limited, and known adhesives having a predetermined transparency, such as acrylic adhesives, rubber adhesives, silicone adhesives, urethane adhesives, and polyester adhesives, can be used.
[0091] When the coated film of the present invention has a pressure-sensitive adhesive layer, a release film may be laminated on the surface of the pressure-sensitive adhesive layer. The release film has a role of protecting the surface of the pressure-sensitive adhesive layer and is peeled off and removed when used. The release film is not particularly limited as long as it has the desired releasability on its release surface (the surface in contact with the pressure-sensitive adhesive layer), and any known release film can be used.
[0092] (7) Surface Protective Sheet The coated film of the present invention may have a surface protective sheet on the coating layer for the purpose of protecting the surface of the coating layer until use. The surface protective sheet is peeled off and removed when used. As the surface protective sheet, a conventionally known resin film is preferably used.
[0093] (8) Layer Structure Examples of the layer structure of the coated film of the present invention include, but are not limited to, the following. In the following, the following symbols are used: BL: base layer, AVC: coating layer, PL: primer layer, SP: surface protection sheet, RF: release film, AL: adhesive layer, AR: anti-reflection layer
[0094] BL / AVC, BL / AVC / SP, BL / AVC / AR, BL / AVC / AR / SP, AVC / BL / AVC, SP / AVC / BL / AVC / SP, BL / PL / AVC, BL / PL / AVC / SP, RF / AL / BL / AVC, RF / AL / BL / AVC / SP, RF / AL / BL / AVC / AR / SP, RF / AL / BL / PL / AVC / AR / SP
[0095] 3. Properties of the Coated Film (1) Total Light Transmittance From the viewpoint of transparency, the total light transmittance of the coated film of the present invention is preferably 85% or more, more preferably 88% or more, and even more preferably 90% or more. The upper limit of the total light transmittance is usually 100%. This results in excellent visibility of the displayed image on the display. The film can also be suitably used in applications other than displays where transparency is required (for example, windows of vehicles, transport aircraft, ships, etc., windows of buildings, etc.). Furthermore, application of the coated film tends to result in an excellent appearance. The total light transmittance can be measured using a haze meter in accordance with JIS K 7361-1.
[0096] (2) Haze Value From the viewpoint of easily maintaining visibility, the haze value of the coated film of the present invention is preferably 50% or less, more preferably 25% or less, even more preferably 15% or less, particularly preferably 5% or less, and especially preferably 1% or less. When the coated film is used in a display, the displayed image has excellent transparency, making it easier to maintain visibility. The coated film can also be suitably used in articles other than displays that require transparency, such as windows for vehicles, transport aircraft, ships, etc., and windows for buildings. The lower limit of the haze value is usually 0% or more, and from the viewpoint of achieving both transparency, visibility, and scratch resistance, it is preferably 0.01% or more. From the viewpoint of providing antiglare properties, the haze value of the coated film of the present invention is preferably 0.1% or more, preferably 1% or more, more preferably 3% or more, particularly preferably 5% or more, and especially preferably 10% to 50%. This enables both visibility of the displayed image and antiglare properties to be achieved. In addition, when used in windows of vehicles, transport aircraft, ships, etc., or windows of buildings, it is possible to impart desired light scattering properties and crime prevention properties. Furthermore, when used in surface protection films, it produces a cloudy appearance, which is useful as an indicator for preventing forgetting to peel off the surface protection film. The haze value can be measured using a haze meter in accordance with JIS K 7136:2000.
[0097] (3) Transmission Clarity The transmission clarity of the coated film of the present invention is preferably 50 or more, more preferably 100 or more, even more preferably 140 or more, particularly preferably 180 or more, and most preferably 250 or more. The upper limit of the transmission clarity is not particularly limited, but is usually 500 or less. This facilitates good visibility in displays and the like. This is particularly suitable for high-definition displays. It can also be suitably used in applications other than displays that require transparency (e.g., windows for vehicles, transport aircraft, ships, etc., and windows for buildings). The application of the coated film also facilitates excellent appearance. Transmission clarity can be determined in accordance with JIS K 7374 by using an image clarity tester in transmission mode, irradiating light from the coating layer side, and calculating the total image clarity value for five combs (comb widths: 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm).
[0098] (4) 60° Gloss In the coated film of the present invention, the 60° gloss (glossiness) value of the coating layer surface is preferably 30 or more, more preferably 60 or more, even more preferably 90 or more, particularly preferably 120 or more, and even more preferably 150 or more, from the viewpoint of easily satisfying the above-mentioned optical properties. The 60° gloss value is preferably 180 or less, from the viewpoint of easily obtaining an excellent appearance. Furthermore, from the viewpoint of antiglare properties, it is preferably 160 or less, more preferably 150 or less, particularly preferably 130 or less, and from the viewpoint of achieving both antibacterial and antiviral properties, it is preferably 120 or less. The 60° gloss can be measured using a gloss meter in accordance with JIS Z 8741:1997.
[0099] (5) Scratch Resistance In the coated film of the present invention, the surface of the coating layer preferably has excellent scratch resistance. Excellent scratch resistance can be confirmed by the absence of any change in appearance in a scratch resistance test using steel wool. Specifically, the surface of the coating layer is scratched at 250 g / cm using #0000 steel wool in accordance with JIS K5600-5-10. 2 This can be confirmed by the fact that no scratches are produced on the surface after rubbing 10 times back and forth over a distance of 10 cm under a load of 1000 psi. As a result, when used on the surface of an object to be adhered, such as a display, the film exhibits excellent surface protection properties and can maintain the aesthetic appearance of the object to be adhered.
[0100] (6) Pencil Hardness In the coated film of the present invention, the pencil hardness of the coating layer surface is preferably H or higher, more preferably 2H or higher. The upper limit of the pencil hardness is not particularly limited, but is usually preferably 9H or lower, more preferably 7H or lower, even more preferably 5H or lower, and particularly preferably 3H or lower. This provides excellent scratch resistance and excellent surface protection when used on the surface of an object to be adhered, such as a display. Since the surface is particularly scratch-resistant, the aesthetic appearance of the object to be adhered can be well maintained. Furthermore, since the film has a moderate hardness and its rigidity tends to provide good handling, it is likely to be suitable for application to displays; windows of vehicles, transport aircraft, ships, etc.; windows of buildings, etc. The pencil hardness can be measured in accordance with JIS K 5600 by the method described in the examples.
[0101] (7) Water Contact Angle and Oleic Acid Contact Angle In the coated film of the present invention, the water contact angle of the coating layer surface is preferably 60 to 110°, more preferably 65 to 100°, even more preferably 70 to 95°, and particularly preferably 72 to 90°. The oleic acid contact angle is preferably 10 to 80°, more preferably 15 to 60°, even more preferably 20 to 50°, and particularly preferably 25 to 40°. By keeping the water contact angle and oleic acid contact angle within the above ranges, fingerprints and dirt are less likely to adhere, and even if fingerprints or dirt do adhere, they blend easily into the coating layer surface and are less noticeable, thereby maintaining the beauty of the layer surface. The contact angle can be measured by the method described in the Examples.
[0102] (8) Antiglare Properties The coated film of the present invention, which has a coating layer formed using the coating layer-forming composition containing the component (C): filler, has excellent antiglare properties. The excellent antiglare properties can be confirmed by the evaluation method described in the examples.
[0103] (9) Adhesion The coated film of the present invention has excellent adhesion between the substrate layer and the coating layer. Excellent adhesion can be confirmed by a checkerboard adhesion method in accordance with JIS K5400. That is, a 10 x 10 grid (100 grids in total) is drawn at 1 mm intervals on the surface of the coating layer with a cutter, and cellophane tape manufactured by Nichiban Co., Ltd. is applied to the grid (i) immediately thereafter, (ii) after 1000 hours at 85°C, (iii) after 1000 hours at 60°C and 90% humidity, and (iv) after 1000 hours at -40°C. When the tape is peeled off, it is visually observed whether the coating layer peels off from the substrate layer. Absence of peeling in any grid indicates excellent adhesion.
[0104] (10) Antibacterial and Antiviral Activity The coated film of the present invention, having a coating layer formed using a coating layer-forming composition containing the component (D): an antibacterial and antiviral agent, has antibacterial and antiviral properties. The antibacterial activity value of the coating layer surface in an antibacterial test in accordance with JIS Z2801:2010 is preferably 2.0 or higher, more preferably 2.4 or higher, and even more preferably 2.7 or higher. Furthermore, the antiviral activity value of the coating layer surface in an antiviral test in accordance with ISO 21702 is preferably 0.4 or higher, more preferably 2.0 or higher, and even more preferably 2.7 or higher. The antibacterial and antiviral activity values can be determined by the test methods described in the examples.
[0105] 4. Use of the Coated Film The coated film of the present invention can be produced using an aqueous solvent, is environmentally friendly, has a residual organic solvent content of 50 ppm or less, and has optical and mechanical properties equivalent to those of coated films produced using conventional organic solvents. Therefore, it can be safely and securely used in various displays, such as liquid crystal displays, organic electroluminescence (EL) displays, and light-emitting diode (LED) displays. Furthermore, a coating layer containing an antibacterial or antiviral agent can be suitably used as the surface layer of a touch panel that is touched by human hands. Specifically, it is preferably used by laminating it on a cover material in a display having a display module such as a liquid crystal display module, a light-emitting diode (LED) module, or an organic EL module. The coated film is preferably laminated to the cover material by adhering it via the aforementioned adhesive layer. It can also be suitably used in articles such as vehicles, transportation aircraft, ships, buildings, and surface protection films.
[0106] 2) Articles Comprising a Coated Film The article of the present invention comprises the coated film of the present invention. The type of article is not particularly limited as long as it comprises the coated film of the present invention. Examples of the article include optical displays, vehicles, transport aircraft, ships, buildings, and surface protection films.
[0107] The optical display of the present invention can be obtained, for example, by bonding (laminating) a display body and the coated film of the present invention, with the display surface side of the display body being bonded to the substrate layer (or adhesive layer) of the coated film. The coated film of the present invention may be laminated directly onto the display surface of the display body, or may be laminated onto the display surface side of the display body via another member or layer (such as a cover material).
[0108] Examples of vehicles include automobiles, railway vehicles, etc. Examples of transport aircraft include passenger planes, cargo planes, etc. The coated film is preferably used by being attached to the surfaces of interior and exterior members of these vehicles, transport aircraft, ships, etc., particularly to the surfaces of license plates, windows, etc.
[0109] In buildings, coated films are preferably used on the surfaces of exterior and interior components, particularly windows.
[0110] The surface protection film is attached to the surface of an object to be protected until use, and is peeled off from the object to be protected at the time of use. The object to be protected is not particularly limited, and examples thereof include various optical films, electronic devices, electrical products, etc.
[0111] The above-described embodiments have been described to facilitate understanding of the present invention, and are not intended to limit the present invention. Therefore, each element disclosed in the above embodiments is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.
[0112] In this specification, when it is stated that "α to β" (α and β are any numerical values), it means "not less than α and not more than β" and also means "preferably greater than α" or "preferably smaller than β" unless otherwise specified. Furthermore, when it is stated that "not less than α" (α is any numerical value), it also means "preferably greater than α" unless otherwise specified, and when it is stated that "not more than β" (β is any numerical value), it also means "preferably smaller than β" unless otherwise specified.
[0113] The present invention will be explained in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.
[0114] Example 1 A coating layer-forming composition was prepared by uniformly mixing 100 parts by mass of a cationic urethane acrylate material as the component (A) [trade name: ART RESIN WEH-1, molecular weight: 2000, average particle size: 50-100 nm, number of functional groups: 10, manufactured by Negami Chemical Industrial Co., Ltd.] (referred to as "A1" in Table 1 below), 1.0 part by mass of an acrylic group-containing polyether-modified siloxane (leveling agent) as the component (B) [trade name: BYK-3530, manufactured by BYK Corporation] (referred to as "B1-1" in Table 1 below), 5.0 parts by mass of a photopolymerization initiator as the component (E) [1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-methylpropanone] (referred to as "E1" in Table 1 below), and water as a solvent.
[0115] The composition for forming a coating layer was applied with a Mayer bar onto a polyethylene terephthalate (PET) film (trade name "Lumirror U40", thickness: 188 μm, manufactured by Toray Industries, Inc.) as a base layer to form a coating film, which was then placed in an oven maintained at 110°C for 1 minute to dry. Next, under a nitrogen atmosphere, an ultraviolet irradiation device (Eigrantage ECS-401GX, manufactured by Eye Graphics Co., Ltd.) was used, and a high-pressure mercury lamp was used as a light source to irradiate the coating layer at an illuminance of 200 mW / cm. 2 , light intensity: 200mJ / cm 2 The coating film was cured by ultraviolet irradiation under the irradiation conditions of 100 to 200, thereby preparing a coated film (coated film 1) having a coating layer with a thickness of 4 μm.
[0116] (Examples 2 and 3) Coated films 2 and 3 were prepared in the same manner as in Example 1, except that B1-2 and B1-3 (listed in Table 1 below) shown below were used instead of B1-1 as component (B) in Example 1.
[0117] Example 4 A coating layer-forming composition was prepared in the same manner as in Example 1, except that 0.8 parts by mass of B2-1 was used in addition to B1-1 as the component (B), and 8.0 parts by mass of C1 was used as the component (C). A coated film 4 was produced in the same manner as in Example 1. B2-1 and C1 are as shown below.
[0118] (Examples 5 to 9, Comparative Examples 1 to 3) In Example 4, a coating layer-forming composition was prepared in the same manner as in Example 4, except that the types of components (A) to (E) shown in Table 1 below were used in the amounts shown in Table 1, and coated films 5 to 9 and 1r to 3r having the film thicknesses shown in Table 1 were produced in the same manner as in Example 4. However, in Comparative Example 3, when forming the coating film, instead of drying in an oven maintained at 110°C for 1 minute, drying was carried out in an oven maintained at 70°C for 1 minute. The types of components (A) to (E) in Table 1 below are shown below.
[0119] A2: NK Ester A-DPH (dipentaerythritol polyacrylate), manufactured by Shin-Nakamura Chemical Co., Ltd. B1-2: F-477 (oligomer containing fluorine-containing groups, hydrophilic groups, and lipophilic groups), manufactured by DIC Corporation B1-3: F-553 (oligomer containing fluorine-containing groups, hydrophilic groups, and lipophilic groups), manufactured by DIC Corporation B1-4: SH28 (silicone-based leveling agent), manufactured by Dow-Toray Industries, Inc. B2-1: PD-201 (acetylene alcohol-based surfactant), manufactured by Nissin Chemical Industry Co., Ltd. C1: Seahoster KE-P250 (spherical silica, particle size: 2.5 μm), manufactured by Nippon Shokubai Co., Ltd. C2: KE-S150 (spherical silica, particle size: 1.5 μm), manufactured by Nippon Shokubai Co., Ltd. C3: SYLYSIA530 (irregular silica, particle size: 2.7 μm), manufactured by Fuji Silysia Chemical Industries, Ltd. D1: Novalon AG1100 (silver-supported hexagonal zirconium phosphate, average particle size: 1 μm), manufactured by Toagosei Co., Ltd. D2: Ion Pure (metal ion-containing water-soluble glass), manufactured by Ishizuka Glass Co., Ltd. D3: Virustaker VM (organic anionic antibacterial and antiviral agent), manufactured by Sekisui Material Co., Ltd. E2: 1-hydroxycyclohexyl phenyl ketone
[0120]
[0121] The coated films 1 to 9 and 1r to 3r obtained in Examples 1 to 9 and Comparative Examples 1 to 3 were subjected to the following tests.
[0122] [Measurement of residual organic solvent amount] Each of the coated films 1 to 9 and 1r to 3r was cut into a size of 4 cm x 5 cm and heated at 120°C for 20 minutes, and the amount of vaporized solvent was measured by gas chromatography (apparatus name "GC-2010", manufactured by Shimadzu Corporation) to measure the amount of residual organic solvent. The results are shown in Table 2. "nd" in the table indicates that no residual organic solvent was detected.
[0123] [Coatability] The surface of the coating layer of each of the coated films 1 to 9 and 1r to 3r was visually inspected. A rating of ◯ was given when no cissing marks and no streaks or point-like defects were observed on the coating layer surface. A rating of NG1 was given when cissing marks were observed on the coating layer surface, and a rating of NG2 was given when streaks, point-like defects, or the like were observed. The results are shown in Table 2.
[0124] [Total Light Transmittance] For each of the coated films 1 to 9 and 1r to 3r, the total light transmittance (%) was measured in accordance with JIS K 7361-1 using a haze meter ("NDH-5000", manufactured by Nippon Denshoku Industries Co., Ltd.) by irradiating light from the coating layer side after blank correction. The results are shown in Table 2.
[0125] [Haze] For Coated Films 1 to 9 and 1r to 3r, the haze value (%) of the coating layer surface was measured in accordance with JIS K 7136: 2000 using a haze meter ("NDH-5000", manufactured by Nippon Denshoku Industries Co., Ltd.) by irradiating light from the coating layer side after blank correction. The results are shown in Table 2.
[0126] [Transmission clarity] For each of the coated films 1 to 9 and 1r to 3r, light was irradiated from the coating layer side in transmission mode using an image clarity tester ("ICM-1T", manufactured by Suga Test Instruments Co., Ltd.) in accordance with JIS K 7374, and the total image clarity value for five combs (comb widths: 0.125 mm, 0.25 mm, 0.5 mm, 1.0 mm, and 2.0 mm) was calculated, and this calculated value was taken as the transmission clarity value. The results are shown in Table 2.
[0127] [60° Gloss (Glossiness)] For each of the coated films 1 to 9 and 1r to 3r, the 60° gloss of the coating layer surface was measured using a gloss meter (VG7000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with JIS Z 8741: 1997. The results are shown in Table 2.
[0128] [Abrasion Resistance] The abrasion resistance of the coating layer surface of each of the coated films 1 to 9 and 1r to 3r was evaluated. That is, the coating layer surface was subjected to abrasion resistance of 250 g / cm using #0000 steel wool in accordance with JIS K5600-5-10. 2 The coating layer was rubbed back and forth 10 times with a load of 0.015 and a sliding distance of 10 cm. The presence or absence of scratches on the surface of the coating layer was then visually inspected under a three-wavelength fluorescent lamp and evaluated according to the following criteria. The results are shown in Table 2. ○: 3 or fewer scratches were observed △: 4 to 10 scratches were observed ×: 11 or more scratches were observed
[0129] [Pencil Hardness] The pencil hardness of the coating layer surface of each of the coated films 1 to 9 and 1r to 3r was measured in accordance with JIS K 5600. That is, pencils with different pencil lead hardnesses ("Mitsubishi Pencil UNI," manufactured by Mitsubishi Pencil Co., Ltd.) were used to observe the degree of surface damage when moved at a 45° angle for 7 mm or more while applying a load of 750 g. This was repeated five times for each sample, and the hardness of the hardest pencil lead that did not damage the surface four or more times was recorded as the pencil hardness. The results are shown in Table 2.
[0130] [Water Contact Angle and Oleic Acid Contact Angle] The water contact angle and oleic acid contact angle on the coating layer surface of the coated films 1 to 9 and 1r to 3r were measured. That is, a glass plate was attached to the substrate layer side surface of the coated film, and then the coated film with the glass plate was placed on the test stand of a contact angle meter (DH350 test stand, manufactured by Kyowa Corporation) with the glass plate side facing down. Next, 2 μL of water (or oleic acid) was dropped on the coating layer surface of the coated film with the glass plate, and the contact angle (°) immediately after dropping was measured with the contact angle meter. The measured value was taken as the water contact angle (or oleic acid contact angle) (°). The results are shown in Table 2.
[0131] [Anti-glare properties] The coated films 1 to 9 and 1r to 3r were placed on a black board with the coating surface facing up, and the light reflected from the coating surface under a three-wavelength fluorescent lamp was visually observed at an angle of 70 to 80 degrees from the surface, and the anti-glare properties were evaluated based on the shape of the fluorescent lamp in the reflected light. The evaluation was made with a circle when the fluorescent lamp did not appear straight, and with an x when the fluorescent lamp appeared straight. The results are shown in Table 2.
[0132] [Cross-Cut Adhesion Test (Adhesion)] The adhesion of the coated films 1 to 9 and 1r to 3r was evaluated by the cross-cut adhesion method according to JIS K5400. That is, a 10 x 10 grid (100 grids in total) was drawn at 1 mm intervals on the surface of the coating layer with a cutter, and after initially leaving the film at 85 ° C for 1000 hours, after leaving it in an environment of 60 ° C and 90% relative humidity for 1000 hours, and after leaving it at -40 ° C for 1000 hours, cellophane tape manufactured by Nichiban Co., Ltd. was applied, and when the tape was peeled off, it was confirmed whether the coating layer peeled off from the base layer, and the number of grids that did not peel off was evaluated. The results are shown in Table 2.
[0133] [Antibacterial test] The coated films 7 to 9 obtained in Examples 7 to 9 using the antibacterial and antiviral agent were subjected to an antibacterial test in accordance with JIS Z 2801:2010 "Antibacterial processed products - Antibacterial product test, antibacterial effect." The results are shown in Table 2.
[0134] Test Method: Test bacterial solution A containing Staphylococcus aureus (a gram-positive bacterium) at a predetermined concentration and test bacterial solution B containing Escherichia coli (a gram-negative bacterium) at a predetermined concentration were prepared using 1 / 500 nutrient medium. 0.4 ml of each of test bacterial solutions A and B was dropped onto the surface of the coating layer of a coated film cut to a size of 5 cm x 5 cm, covered with a polyethylene film cut to a size of 4 cm x 4 cm, and left for 24 hours at 35°C and a relative humidity of 90% or higher. Subsequently, bacteria adhering to the surface of the coating layer were thoroughly washed into a petri dish, and the viable cell count in 1 ml of this solution was measured. Furthermore, a substrate without a coating layer (PET film: standard sample) was placed instead of the coated film, and the viable cell count was measured in the same manner as above. The antibacterial activity value was calculated from the measured viable cell count of the standard sample and the viable cell count of the measurement sample.
[0135] [Antiviral Test] The coated films 7 to 9 obtained in Examples 7 to 9 using the antibacterial / antiviral agent were subjected to an antiviral test using seasonal influenza A virus (enveloped) and feline calicivirus (non-enveloped) in accordance with ISO 21702 by the following method. The results are shown in Table 2.
[0136] Test Method: A virus suspension of a predetermined concentration was prepared by infecting and culturing host cells with the virus. A coated film (5 cm x 5 cm; measurement sample) was placed in a Petri dish with the coating layer surface facing up, and 0.4 mL of the virus suspension was placed on the coating layer surface of the coated film. The coated film was then covered with a polyethylene film (4 cm x 4 cm) so that the virus suspension was distributed over the entire surface of the coated film. After storing the Petri dish in a thermo-hygrostat for a predetermined time, the virus suspension was washed out with SCDLP (Soybean-Casein Digest Broth with Lecithin & Polysorbate 80) medium, and the washed solution was serially diluted with EMEM (Eagle's minimal essential medium) medium. The virus infectivity of these diluted solutions was then measured by plaque assay. A polyethylene film (5 cm × 5 cm; standard sample) was used instead of the coated film, and the virus infectivity was measured in the same manner as above. The difference between the measured virus infectivity of the standard sample and the virus infectivity of the measurement sample was calculated as a log value, and this was used as the antiviral activity value.
[0137]
[0138] Table 2 shows that coated films 1 to 9 of the present invention have high total light transmittance, high transmitted light clarity, excellent hardness, and excellent scratch resistance and adhesion. Furthermore, coated films 4 to 9, which use a filler in the coating layer, also have excellent antiglare properties, and coated films 7 to 9, which use an antibacterial and antiviral agent, also have excellent antibacterial and antiviral properties.
[0139] On the other hand, in Comparative Example 1, which used a coating layer-forming composition that did not contain component (B), repelling occurred during coating layer production, resulting in poor coatability. The coated film 2r of Comparative Example 2 had low transmittance clarity. Furthermore, numerous dot-like defects occurred during coating, resulting in poor coatability. Furthermore, in Comparative Example 3, which did not use a urethane acrylate-based material as component (A), the residual organic solvent exceeded 50 ppm, making it unfriendly to the environment.
[0140] As described above in detail, the coated film of the present invention is environmentally friendly, has excellent coatability of the coating layer, and is also excellent in optical and mechanical properties. Furthermore, since it can also be imparted with antibacterial and antiviral properties, it is expected to be suitably used in products such as touch panels amid the current epidemic of infectious diseases.
Claims
1. A coated film having a base layer and a coating layer, characterized in that the transmitted light clarity is 50 or more, the coating layer is a layer formed from a coating layer forming composition containing the following components (A) and (B), and the amount of residual organic solvent in the coating layer is 50 ppm or less. Component (A): urethane acrylate-based material Component (B): surface conditioner 2. The coated film according to claim 1, wherein the component (A) is an emulsion containing emulsified particles of a urethane acrylate having an average particle size of 300 nm or less and having 5 or more active energy ray-polymerizable functional groups.
3. The coated film according to claim 1, wherein the component (B) is a water-soluble leveling agent and / or surfactant.
4. The coated film according to claim 1, wherein the content of the component (B) in the composition for forming the coating layer is 0.1 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the component (A).
5. The coated film according to claim 1, wherein the surface of the coating layer opposite the substrate layer has a water contact angle of 70° or more.
6. The coated film according to claim 1, wherein the composition for forming the coating layer further contains a filler as component (C).
7. The coated film according to claim 1, wherein the composition for forming the coating layer further contains a particulate antibacterial and antiviral agent as component (D).
8. The coated film according to claim 7, wherein the particulate antibacterial and antiviral agent has an average particle size of 0.5 μm or more and 5 μm or less, and the coating layer has a thickness of 5 μm or less.
9. The coated film according to claim 7, which has an antibacterial activity value of 2.0 or more in an antibacterial test in accordance with JIS Z2801:2010, and an antiviral activity value of 2.0 or more in an antiviral test in accordance with ISO 21702.
10. An article comprising the coated film according to any one of claims 1 to 9.
11. The article according to claim 10, which is any one of an optical display, a vehicle, a transportation aircraft, a ship, a building, and a surface protection film.
Citation Information
Patent Citations
Energy ray-curable oil-in-water emulsion and aqueous hard coat agent
JP2005247884A
Anti-glaring hard coat film
JP2008119867A
Hard coat film
JP2013037323A
Optical film, polarizing plate, liquid crystal panel, and image displaying device
JP2014059334A
Hard coat film
JP2022131260A