Thiol compound
A multifunctional thiol compound with specific structural features addresses the adhesion and performance issues of existing thiol compounds in epoxy resin curing, offering tack-free, high-elongation, low-elasticity, and impact-resistant cured products.
Patent Information
- Application Number
- PCT/JP2024/011677
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Existing thiol compounds used for curing epoxy resins often result in cured products that adhere to fingers, compromising their tack-free performance, while also lacking high elongation and low elasticity.
A multifunctional thiol compound with a specific structure, featuring multiple thiol groups, is developed to provide excellent tack-free performance, high elongation, and low elasticity, along with rapid curing and improved impact resistance.
The thiol compound effectively prevents adhesion to fingers, achieves high elongation and low elasticity, and enhances the impact resistance and hydrolysis resistance of cured epoxy resins, making it suitable for various applications.
Smart Images

Figure JPOXMLDOC01-APPB-I000001 
Figure JPOXMLDOC01-APPB-I000002 
Figure JPOXMLDOC01-APPB-I000003
Abstract
Description
thiol compounds
[0001] The present invention relates to a novel thiol compound used for curing epoxy resins, etc. More specifically, the novel thiol compound can be used as a curing agent for epoxy resins.
[0002] Compositions using compounds containing thiol groups (also known as sulfanyl groups or mercapto groups, or -SH groups) as curing agents for epoxy resins have been extensively studied due to their excellent low-temperature curing properties. In particular, various studies have been conducted on compounds containing multiple thiol groups in the molecule (Patent Documents 1 to 3).
[0003] Japanese Patent Application Laid-Open No. 2012-153794 Japanese Patent Application Laid-Open No. 2016-164134 International Publication No. 2014 / 084292 Pamphlet
[0004] Generally, when curing an epoxy resin, the use of a bifunctional thiol compound with a long molecular chain can produce a cured product with high elongation, low elasticity, and excellent impact resistance. However, when a finger or other object touches the surface of a cured product after curing has progressed, uncured cured material may adhere to the finger or other object, affecting the surface condition of the cured product. Therefore, there has been a demand for a thiol compound that does not adhere to fingers or other objects, that is, has so-called tack-free properties, and can exhibit high elongation and low elasticity.
[0005] The present inventors have conducted extensive research to solve the above-mentioned problems. As a result, the present inventors have discovered that a compound having a specific thiol group is a polyfunctional thiol compound that exhibits high elongation and low elasticity, yet is effective as a curing agent that gives a cured resin product with good tack-free properties, and have arrived at the present invention. That is, the present invention can include the following aspects.
[0006] [1] General formula (I): (I) A compound represented by formula (I), wherein X's are each independently a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, or a C1-C6 alkoxy group, and n's are each independently an integer of 1 to 5. [2] The compound according to the above item [1], wherein X's are each independently a hydrogen atom, a methyl group, or an ethyl group, and n's are each an integer of 1 to 3. [3] The compound according to the above item [1], wherein X's are each independently a hydrogen atom or a methyl group, and n's is 1. [4] The compound shown below. or [5] An epoxy resin composition containing an epoxy resin and the compound described in any one of [1] to [4]. [6] An epoxy resin curing agent containing the compound described in any one of [1] to [4]. [7] A cured epoxy resin obtained by thermally curing an epoxy resin and the compound described in any one of [1] to [4].
[0007] The present invention provides an epoxy resin curing agent that can exhibit high elongation and low elasticity while providing a cured product with good tack-free properties. By using the compound having a thiol group of the present invention, the curing of the epoxy resin proceeds rapidly, and a cured epoxy resin with good tack-free properties can be provided.
[0008] NMR data of the thiol compound (1) prepared in Example 1 is shown below.
[0009] [Thiol Compound] One embodiment of the present invention is a thiol compound represented by the following general formula (I). (I)
[0010] In formula (I), each X is independently a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, or a C1-C6 alkoxy group, preferably a hydrogen atom or a C1-C6 alkyl group, more preferably a hydrogen atom, a methyl group, or an ethyl group, and even more preferably a hydrogen atom or a methyl group. Each n is independently an integer of 1 to 5, preferably an integer of 1 to 3, and more preferably 1.
[0011] Another embodiment of the present invention is a thiol compound represented by the following general formula (Ib): (Ib) In formula (Ib), the definitions of X and n are the same as those in formula (I).
[0012] More specific embodiments of the thiol compound of the present invention include the following thiol compounds (1) and (2).
[0013] Thiol Compound (1)
[0014] Thiol Compound (2)
[0015] [Method for Preparing Thiol Compound] The thiol compound can be produced by known methods, but can also be prepared, for example, as follows. The following describes the thiol compound (1) as an example. First, tetraallyloxyethane is used as a starting material, and an organic solvent such as toluene and azobisisobutyronitrile are added. Thioacetic acid is then added, and the reaction is carried out, for example, at 50 to 200°C, preferably 60 to 150°C, and more preferably 80°C ± 10 to 20°C, for 30 minutes to 12 hours, preferably 1 to 5 hours, and more preferably 3 hours ± 1 hour. The organic solvent such as toluene is removed from the resulting reaction product, yielding tetraallyloxyethane (thioester). The resulting thioester is then reacted with an alcohol such as methanol and a base such as sodium hydroxide, for example, at 50 to 200°C, preferably 60 to 150°C, and more preferably 70°C ± 10 to 20°C, for 30 minutes to 12 hours, preferably 1 to 5 hours, and more preferably 1.5 hours ± 1 to 2 hours. The resulting reaction product is neutralized with hydrochloric acid or the like, and extracted with an organic solvent such as toluene 1 to 5 times, preferably about 3 times, from the resulting organic solvent layer, and the organic solvent such as toluene is removed to obtain thiol compound (1) from the organic solvent layer.
[0016] [Uses of Thiol Compounds] The thiol compounds described above are polyfunctional thiol compounds with long molecular chains and four or more thiol groups. When used as curing agents for epoxy resins, they can produce cured products with high elongation, low elasticity, and excellent impact resistance. Furthermore, these thiol compounds are useful as curing agents for epoxy resins because they exhibit excellent low-temperature curing properties and superior hydrolysis resistance compared to other thiol compounds containing ester groups. Furthermore, these thiol compounds can also be used as crosslinkers or curing aids for compounds containing carbon-carbon double bonds (ene compounds). The reaction between a thiol compound and a carbon-carbon double bond is known as the thiol-ene reaction, and these thiol compounds can be used in the reaction (thiol-ene reaction) between the thiol compounds and resins containing carbon-carbon double bonds, such as (meth)acrylate compounds, allyl compounds, vinyl compounds, unsaturated polyesters, and polybutadiene. By using the thiol compound as a crosslinking agent or curing aid, the thiol compound is less susceptible to oxygen inhibition during the reaction and has excellent reactivity with compounds having a carbon-carbon double bond, allowing the crosslinking of compounds having a carbon-carbon double bond to proceed quickly. Note that, in each application, the thiol compound of the present invention may be used alone or in combination of multiple types.
[0017] [Epoxy Resin Composition] One aspect of the present invention is an epoxy resin composition containing an epoxy resin and the above-described thiol compound. Examples of epoxy resins include epoxy resin compounds having, on average, two or more epoxy groups per molecule. Examples of epoxy resins include polyglycidyl ethers obtained by reacting epichlorohydrin with polyhydric phenols such as bisphenol A, bisphenol F, bisphenol AD, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol; polyglycidyl ether esters obtained by reacting epichlorohydrin with hydroxy acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid; polyglycidyl esters obtained by reacting epichlorohydrin with polycarboxylic acids such as phthalic acid and terephthalic acid; and epoxidized phenol novolac resins, epoxidized cresol novolac resins, epoxidized polyolefins, alicyclic epoxy resins, and other urethane-modified epoxy resins. From the viewpoint of maintaining high heat resistance and low moisture permeability, preferred epoxy resins include bisphenol A type epoxy resins, bisphenol F type epoxy resins, phenol novolac type epoxy resins, biphenyl aralkyl type epoxy resins, phenol aralkyl type epoxy resins, aromatic glycidylamine type epoxy resins, and epoxy resins having a dicyclopentadiene structure, with bisphenol A type epoxy resins and bisphenol F type epoxy resins being more preferred, and bisphenol A type epoxy resins being even more preferred.
[0018] The epoxy resin may be liquid or solid. The epoxy resin used herein may be a mixture of liquid and solid epoxy resins. Here, "liquid" and "solid" refer to the state of the epoxy resin at room temperature (25°C). Specific examples of liquid epoxy resins include liquid bisphenol A epoxy resins ("jER (registered trademark) Epoxy Resin 828" and "jER (registered trademark) Epoxy Resin 827" manufactured by Mitsubishi Chemical Corporation), liquid bisphenol F epoxy resins ("jER (registered trademark) Epoxy Resin 807" manufactured by Mitsubishi Chemical Corporation), naphthalene-type bifunctional epoxy resins ("HP4032" and "HP4032D" manufactured by DIC Corporation), liquid bisphenol AF epoxy resins ("ZX1 O59" manufactured by Nippon Steel Epoxy Manufacturing Co., Ltd.), and hydrogenated epoxy resins ("jER (registered trademark) Epoxy Resin YX8000" manufactured by Mitsubishi Chemical Corporation). Among these, "jER (registered trademark) Epoxy Resin 828," "jER (registered trademark) Epoxy Resin 827," and "jER (registered trademark) Epoxy Resin 807," manufactured by Mitsubishi Chemical Corporation, which have high heat resistance and low viscosity, are preferred, with "jER (registered trademark) Epoxy Resin 828" being more preferred. Specific examples of solid epoxy resins include naphthalene-type tetrafunctional epoxy resins ("HP4700" manufactured by DIC Corporation), dicyclopentadiene-type multifunctional epoxy resins ("HP7200" manufactured by DIC Corporation), naphthol-type epoxy resins ("ESN-475V" manufactured by Nippon Steel Epoxy Manufacturing Co., Ltd. (Tohto Kasei Co., Ltd.)), epoxy resins having a butadiene structure ("PB-3600" manufactured by Daicel Corporation), and epoxy resins having a biphenyl structure ("NC3000H" and "NC3000L" manufactured by Nippon Kayaku Co., Ltd., and "YX4000" manufactured by Mitsubishi Chemical Corporation).
[0019] From the viewpoints of coatability, processability, and adhesiveness, it is preferable that at least 10% by mass of the total epoxy resin used be a liquid epoxy resin, more preferably 30% by mass or more, and even more preferably 50% by mass or more. In the epoxy resin composition of the present invention, the content of the thiol compound of the present invention per 100 parts by mass of epoxy resin varies depending on the number of thiol groups. For example, when the thiol compound of the present invention is a tetrafunctional thiol compound having four thiol groups (thiol equivalent = 4), it is preferably 1 part by mass or more, more preferably 5 parts by mass or more, even more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, particularly preferably 20 parts by mass or more, and especially preferably 25 parts by mass or more. Furthermore, the content of the thiol compound of the present invention per 100 parts by mass of the epoxy resin of the present invention is preferably 95 parts by mass or less, more preferably 90 parts by mass or less, even more preferably 85 parts by mass or less, even more preferably 80 parts by mass or less, especially preferably 75 parts by mass or less, and especially preferably 70 parts by mass or less. The preferred content of the thiol compound of the present invention may be within a range selected from the upper limit, the lower limit, and any of the values in the examples. When the number of thiol groups contained in the thiol compound of the present invention is greater than 4, the content may be proportional to the above content or the thiol equivalent. That is, for example, when the number of thiol groups is 8 (thiol equivalent = 8), the above "preferably 5 parts by mass or more" may be read as "preferably 2.5 parts by mass or more," and "preferably 300 parts by mass or less" may be read as "preferably 150 parts by mass or less."
[0020] Other components that can be added to the epoxy resin composition of the present invention include curing accelerators, solvents, storage stabilizers, other curing agents, thixotropy-imparting agents, fillers, diluents, dispersants, flexibility-imparting agents, coupling agents, antioxidants, etc. Examples of curing accelerators include latent curing accelerators. A latent curing accelerator is a compound that is insoluble in epoxy resins at room temperature (25°C) but becomes soluble upon heating and functions as a curing accelerator for the epoxy resin. Examples include, but are not limited to, imidazole compounds that are solid at room temperature (25°C) and amine adduct latent curing accelerators. Of these, amine adduct latent curing accelerators are preferred. Examples of amine adduct latent curing accelerators include reaction products of amine compounds and epoxy compounds (amine-epoxy adduct latent curing accelerators) and reaction products of amine compounds and isocyanate compounds (amine-isocyanate latent curing accelerators).
[0021] Examples of the imidazole compound that is solid at room temperature (25° C.) include 2-heptadecylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2-undecylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4-benzyl-5-hydroxymethylimidazole, 2,4-diamino-6-(2-methylimidazolyl-(1))-ethyl-S-triazine, 2,4-diamino-6- Examples include (2'-methylimidazolyl-(1)')-ethyl-S-triazine isocyanuric acid adduct, 2-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-methylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazole trimellitate, and N-(2-methylimidazolyl-1-ethyl)-urea.
[0022] Examples of epoxy compounds used as one of the raw materials for producing the amine-epoxy adduct latent curing accelerator include polyglycidyl ethers obtained by reacting epichlorohydrin with polyhydric phenols such as bisphenol A, bisphenol F, catechol, and resorcinol, or polyhydric alcohols such as glycerin and polyethylene glycol; glycidyl ether esters obtained by reacting epichlorohydrin with hydroxy acids such as p-hydroxybenzoic acid and β-hydroxynaphthoic acid; polyglycidyl esters obtained by reacting epichlorohydrin with polycarboxylic acids such as phthalic acid and terephthalic acid; glycidyl amine compounds obtained by reacting epichlorohydrin with 4,4'-diaminodiphenylmethane or m-aminophenol; and polyfunctional epoxy compounds such as epoxidized phenol novolac resins, epoxidized cresol novolac resins, and epoxidized polyolefins; and monofunctional epoxy compounds such as butyl glycidyl ether, phenyl glycidyl ether, and glycidyl methacrylate.
[0023] The amine compound used as a raw material for producing the amine adduct latent curing accelerator may be any compound having one or more active hydrogen atoms in the molecule capable of addition reacting with an epoxy group or an isocyanate group (also known as an isocyanato group) and one or more amino groups (at least one of a primary amino group, a secondary amino group, and a tertiary amino group) in the molecule. Examples of such amine compounds include aliphatic amine compounds such as diethylenetriamine, triethylenetetramine, propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane; aromatic amine compounds such as 4,4'-diaminodiphenylmethane and 2-methylaniline; and nitrogen-containing heterocyclic compounds such as 2-ethyl-4-methylimidazole, 2-ethyl-4-methylimidazoline, 2,4-dimethylimidazoline, piperidine, and piperazine.
[0024] Furthermore, among the above-mentioned raw materials, if a compound having a tertiary amino group in the molecule is used, a latent curing accelerator having excellent curing acceleration ability can be produced. Examples of the compound having a tertiary amino group in the molecule include amines having a tertiary amino group in the molecule, such as dimethylaminopropylamine, diethylaminopropylamine, dipropylaminopropylamine, dibutylaminopropylamine, dimethylaminoethylamine, diethylaminoethylamine, N-methylpiperazine, 2-methylimidazole, 2-ethylimidazole, 2-ethyl-4-methylimidazole, and 2-phenylimidazole; 2-dimethylaminoethanol, 1-methyl-2-dimethylaminoethanol, 1-phenoxymethyl-2-dimethylaminoethanol, 2-diethylaminoethanol, 1-butoxymethyl-2-dimethylaminoethanol, 1-(2-hydroxy-3-phenoxypropyl)-2-methylimidazole, 1-(2-hydroxy-3-phenoxypropyl)-2-ethyl-4-methylimidazole, 1-(2-hydroxy-3-butoxypropyl)-2 ... 1-(2-hydroxy-3-phenoxypropyl)-2-phenylimidazoline, 1-(2-hydroxy-3-butoxypropyl)-2-methylimidazoline, 2-(dimethylaminomethyl)phenol, 2,4,6-tris(dimethylaminomethyl)phenol, N-β-hydroxyethylmorpholine, 2-dimethylaminoethanethiol, 2-mercaptopyridine, 2-benzimidazole, 2-methyl and alcohols, phenols, thiols, carboxylic acids and hydrazides having a tertiary amino group in the molecule such as mercaptobenzimidazole, 2-mercaptobenzothiazole, 4-mercaptopyridine, N,N-dimethylaminobenzoic acid, N,N-dimethylglycine, nicotinic acid, isonicotinic acid, picolinic acid, N,N-dimethylglycine hydrazide, N,N-dimethylpropionic acid hydrazide, nicotinic acid hydrazide and isonicotinic acid hydrazide.
[0025] When the epoxy compound and the amine compound are subjected to an addition reaction to produce the amine adduct-based latent curing accelerator, an active hydrogen compound having two or more active hydrogen atoms in the molecule can also be added. Examples of such active hydrogen compounds include polyhydric phenols such as bisphenol A, bisphenol F, bisphenol S, hydroquinone, catechol, resorcinol, pyrogallol, and phenol novolac resin, polyhydric alcohols such as trimethylolpropane, polycarboxylic acids such as adipic acid and phthalic acid, 1,2-dimercaptoethane, 2-mercaptoethanol, 1-mercapto-3-phenoxy-2-propanol, mercaptoacetic acid, anthranilic acid, and lactic acid.
[0026] Examples of the isocyanate compound used as a raw material for producing the amine adduct-based latent curing accelerator include monofunctional isocyanate compounds such as butyl isocyanate, isopropyl isocyanate, phenyl isocyanate, and benzyl isocyanate; polyfunctional isocyanate compounds such as hexamethylene diisocyanate, tolylene diisocyanate (e.g., 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate), 1,5-naphthalene diisocyanate, diphenylmethane-4,4'-diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, 1,3,6-hexamethylene triisocyanate, and bicycloheptane triisocyanate; and terminal isocyanate group-containing compounds obtained by reacting these polyfunctional isocyanate compounds with active hydrogen compounds. Examples of such a terminal isocyanate group-containing compound include an addition compound having a terminal isocyanate group obtained by reacting tolylene diisocyanate with trimethylolpropane, and an addition compound having a terminal isocyanate group obtained by reacting tolylene diisocyanate with pentaerythritol.
[0027] The curing accelerator can be easily obtained, for example, by appropriately mixing the above-mentioned production raw materials, reacting them at room temperature (25°C) to 200°C, cooling them to solidify them, and then pulverizing them; or by reacting the above-mentioned production raw materials in a solvent such as methyl ethyl ketone, dioxane, or tetrahydrofuran, removing the solvent, and then pulverizing the solid content.
[0028] The curing accelerator may be a commercially available product. Examples of the amine-epoxy adduct latent curing accelerator include "Amicure (registered trademark) PN-23" (Ajinomoto Fine-Techno Co., Ltd.), "Amicure (registered trademark) PN-H" (Ajinomoto Fine-Techno Co., Ltd.), "Hardener X-3661S" (ACR Corporation), "Hardener X-3670S" (ACR Corporation), "Novacure (registered trademark) HX-3742" (Asahi Kasei Corporation), and "Novacure (registered trademark) HX-3721" (Asahi Kasei Corporation). Examples of the amine-isocyanate latent curing accelerator include "Fujicure FXE-1000" (Fuji Kasei Co., Ltd.), and "Fujicure FXR-1030" (Fuji Kasei Co., Ltd.).
[0029] In the epoxy resin composition of the present invention, the content of the curing accelerator per 100 parts by mass of the epoxy resin is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, and especially preferably 2 parts by mass or more. Furthermore, the content of the curing accelerator per 100 parts by mass of the epoxy resin of the present invention is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, even more preferably 30 parts by mass or less, even more preferably 25 parts by mass or less, and especially preferably 20 parts by mass or less. A preferred content of the curing accelerator may be within a range selected from the upper limit, lower limit, and values in the examples.
[0030] Examples of the solvent include water and organic solvents that are commonly used in the art. Examples of the organic solvent include toluene, tetrahydrofuran, methyl ethyl ketone, methyl isobutyl ketone, and dioxane. Although the solvent may be present, it is preferably finally removed from the epoxy resin composition.
[0031] The storage stabilizer is used to impart excellent storage stability to the epoxy resin composition, and preferably further contains at least one storage stabilizer selected from, for example, borate compounds, titanate compounds, aluminate compounds, zirconate compounds, isocyanate compounds, carboxylic acids, acid anhydrides, and mercapto organic acids. Examples of the borate compound include trimethyl borate, triethyl borate, tripropyl borate, triisopropyl borate, tributyl borate, tripentyl borate, triallyl borate, trihexyl borate, tricyclohexyl borate, trioctyl borate, trinonyl borate, tridecyl borate, tridodecyl borate, trihexadecyl borate, trioctadecyl borate, tris(2-ethylhexyloxy)borane, bis(1,4,7,10-tetraoxaundecyl)(1,4,7,10,13-pentaoxatetradecyl)(1,4,7-trioxaundecyl)borane, tribenzyl borate, triphenyl borate, tri-o-tolyl borate, tri-m-tolyl borate, and triethanolamine borate.
[0032] Examples of the titanate compounds include tetraethyl titanate, tetrapropyl titanate, tetraisopropyl titanate, tetrabutyl titanate, and tetraoctyl titanate. Examples of the aluminate compounds include triethyl aluminate, tripropyl aluminate, triisopropyl aluminate, tributyl aluminate, and trioctyl aluminate. Examples of the zirconate compounds include tetraethyl zirconate, tetrapropyl zirconate, tetraisopropyl zirconate, and tetrabutyl zirconate. Examples of the isocyanate compound include butyl isocyanate, isopropyl isocyanate, 2-chloroethyl isocyanate, phenyl isocyanate, p-chlorophenyl isocyanate, benzyl isocyanate, hexamethylene diisocyanate, 2-ethylphenyl isocyanate, 2,6-dimethylphenyl isocyanate, tolylene diisocyanate (e.g., 2,4-tolylene diisocyanate, 2,6-tolylene diisocyanate), 1,5-naphthalene diisocyanate, diphenylmethane-4,4′-diisocyanate, tolidine diisocyanate, isophorone diisocyanate, xylylene diisocyanate, paraphenylene diisocyanate, and bicycloheptane triisocyanate.
[0033] Examples of the carboxylic acid include saturated aliphatic monobasic acids such as formic acid, acetic acid, propionic acid, butyric acid, caproic acid, and caprylic acid; unsaturated aliphatic monobasic acids such as acrylic acid, methacrylic acid, and crotonic acid; halogenated fatty acids such as monochloroacetic acid and dichloroacetic acid; monobasic hydroxy acids such as glycolic acid, lactic acid, and acetic acid; aliphatic aldehyde acids and ketone acids such as glyoxylic acid; aliphatic polybasic acids such as oxalic acid, malonic acid, succinic acid, and maleic acid; aromatic monobasic acids such as benzoic acid, halogenated benzoic acids, toluic acid, phenylacetic acid, cinnamic acid, and mandelic acid; and aromatic polybasic acids such as phthalic acid and trimesic acid. Examples of the acid anhydride include aliphatic polybasic acid anhydrides such as succinic anhydride, dodecynylsuccinic anhydride, maleic anhydride, an adduct of methylcyclopentadiene and maleic anhydride, hexahydrophthalic anhydride, and methyltetrahydrophthalic anhydride; and aromatic polybasic acid anhydrides such as phthalic anhydride, trimellitic anhydride, and pyrrolimellitic anhydride. Examples of the mercapto organic acid include mercaptoaliphatic monocarboxylic acids such as mercaptoacetic acid, mercaptopropionic acid (e.g., 3-mercaptopropionic acid), and mercaptobutyric acid (e.g., 3-mercaptobutyric acid, 4-mercaptobutyric acid); esters containing a thiol group and a carboxy group obtained by an esterification reaction between a hydroxy acid and a mercapto organic acid; mercaptoaliphatic dicarboxylic acids such as mercaptosuccinic acid and dimercaptosuccinic acid (e.g., 2,3-dimercaptosuccinic acid); and mercaptoaromatic monocarboxylic acids such as mercaptobenzoic acid (e.g., 4-mercaptobenzoic acid).
[0034] As the storage stabilizer, from the viewpoints of versatility, high safety, and improving storage stability, borate compounds are preferred, triethyl borate, tripropyl borate, triisopropyl borate, and tributyl borate are more preferred, and triethyl borate is even more preferred. The content of the storage stabilizer in the epoxy resin composition of the present invention is not particularly limited as long as the storage stability of the composition is improved, but the content is preferably 0.001 to 50 parts by mass, more preferably 0.05 to 30 parts by mass, and even more preferably 0.1 to 10 parts by mass of the storage stabilizer per 100 parts by mass of the epoxy resin.
[0035] The other curing agent may be any compound other than the thiol compound of the present invention, as long as it can be used as a curing agent for epoxy resins. Examples of other curing agents include complete esters of polyols and mercapto organic acids. Here, complete esters refer to esters of polyols and carboxylic acids, in which all of the hydroxyl groups of the polyol form ester bonds. Examples of the polyols include ethylene glycol, trimethylolpropane, pentaerythritol, and dipentaerythritol. Examples of the mercapto organic acid include mercaptoaliphatic monocarboxylic acids such as mercaptoacetic acid, mercaptopropionic acid (e.g., 3-mercaptopropionic acid), and mercaptobutyric acid (e.g., 3-mercaptobutyric acid, 4-mercaptobutyric acid); esters containing a thiol group and a carboxy group obtained by an esterification reaction between a hydroxy acid and a mercapto organic acid; mercaptoaliphatic dicarboxylic acids such as mercaptosuccinic acid and dimercaptosuccinic acid (e.g., 2,3-dimercaptosuccinic acid); and mercaptoaromatic monocarboxylic acids such as mercaptobenzoic acid (e.g., 4-mercaptobenzoic acid). The number of carbon atoms in the mercaptoaliphatic monocarboxylic acid is preferably 2 to 8, more preferably 2 to 6, even more preferably 2 to 4, and particularly preferably 3. Among the mercapto organic acids, mercapto aliphatic monocarboxylic acids having 2 to 8 carbon atoms are preferred, mercaptoacetic acid, 3-mercaptopropionic acid, 3-mercaptobutyric acid, and 4-mercaptobutyric acid are more preferred, and 3-mercaptopropionic acid is even more preferred.
[0036] Specific examples of complete esters of polyols and mercapto organic acids include ethylene glycol bis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptobutyrate), ethylene glycol bis(4-mercaptobutyrate), trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane tris(4-mercaptobutyrate), pentaerythritol tetrakis(mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(4-mercaptobutyrate), and dipentaerythritol Examples of the complete ester include hexakis(mercaptoacetate), dipentaerythritol hexakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptobutyrate), and dipentaerythritol hexakis(4-mercaptobutyrate). From the viewpoint of storage stability, the complete ester preferably has as little basic impurity content as possible, and more preferably does not require the use of a basic substance in its production.
[0037] Other curing agents that can be used include polythiol compounds produced using a basic substance as a reaction catalyst in the production process, such as alkyl polythiol compounds such as 1,4-butanedithiol, 1,6-hexaneedithiol, and 1,10-decanedithiol; terminal thiol group-containing polyethers; terminal thiol group-containing polythioethers; polythiol compounds obtained by reacting an epoxy compound with hydrogen sulfide; and polythiol compounds having terminal thiol groups obtained by reacting a polythiol compound with an epoxy compound. Polythiol compounds produced using a basic substance are preferably subjected to a dealkalization treatment to reduce the alkali metal ion concentration to 50 ppm by weight or less before use. Examples of dealkalization treatments for polythiol compounds produced using a basic substance include dissolving the polythiol compound in an organic solvent such as acetone or methanol, neutralizing it by adding an acid such as dilute hydrochloric acid or dilute sulfuric acid, and then desalting it by extraction and washing, etc.; adsorption using an ion exchange resin; and purification by distillation.
[0038] Other curing agents that can be used include, for example, tris[(3-mercaptopropionyloxy)-ethyl]-isocyanurate and 1,3,5-tris(3-mercaptobutyloxyethyl)-1,3,5-triazine-2,4,6(1H,3H,5H)-trione. Preferably, it is one or more complete esters of ethylene glycol, trimethylolpropane, pentaerythritol, or dipentaerythritol with a mercaptoaliphatic monocarboxylic acid having 2 to 8 carbon atoms; more preferably, ethylene glycol bis(mercaptoacetate), ethylene glycol bis(3-mercaptopropionate), ethylene glycol bis(3-mercaptobutyrate), ethylene glycol bis(4-mercaptobutyrate), trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), trimethylolpropane tris(4-mercaptobutyrate), pentaerythritol tetrakis(mercaptoacetate), pentaerythritol tetrakis(3-mercaptopropionate), and pentaerythritol At least one selected from tetrakis(3-mercaptobutyrate), pentaerythritol tetrakis(4-mercaptobutyrate), dipentaerythritol hexakis(mercaptoacetate), dipentaerythritol hexakis(3-mercaptopropionate), dipentaerythritol hexakis(3-mercaptobutyrate), and dipentaerythritol hexakis(4-mercaptobutyrate); more preferably at least one selected from trimethylolpropane tris(mercaptoacetate), trimethylolpropane tris(3-mercaptopropionate), trimethylolpropane tris(3-mercaptobutyrate), and trimethylolpropane tris(4-mercaptobutyrate); particularly preferably trimethylolpropane tris(3-mercaptopropionate).
[0039] When another curing agent is used in the epoxy resin composition, it is preferably used in an amount that does not affect the curing of the thiol compound of the present invention. Preferably, the amount of the other curing agent is 0.001 to 50 parts by mass, more preferably 0.05 to 30 parts by mass, and even more preferably 0.1 to 10 parts by mass per 100 parts by mass of the epoxy resin. The ratio of the thiol compound of the present invention to the other curing agent, [mass of the thiol compound of the present invention] / [total mass of the thiol compound of the present invention and the other curing agent], is preferably, for example, 0.001 to 0.8. The lower limit of this ratio is more preferably 0.01, even more preferably 0.03, and particularly preferably 0.1. The upper limit of this ratio is not particularly limited, but is more preferably 0.6, even more preferably 0.4, and particularly preferably 0.2.
[0040] The ratio of the total equivalent of thiol groups contained in the thiol compound of the present invention and / or other curing agents to the equivalent of epoxy groups contained in the epoxy resin, i.e., [total number of thiol groups contained in the thiol compound of the present invention and / or other curing agents] / [number of epoxy groups contained in the epoxy resin], is preferably 0.2 to 2.0, more preferably 0.6 to 1.2.
[0041] Examples of the thixotropy-imparting agent include precipitated silica, calcined silica, and fumed silica, and among these, fumed silica is preferred. The specific surface area of the thixotropy-imparting agent measured by the BET method (hereinafter referred to as the BET specific surface area) is preferably 50 m 2 / g or more, more preferably 50 to 600m 2 / g, more preferably 100 to 400m 2 When a thixotropy-imparting agent is used, the content of the thixotropy-imparting agent in the epoxy resin composition is preferably 5 to 200 parts by mass, more preferably 10 to 100 parts by mass, per 100 parts by mass of the epoxy resin.
[0042] The epoxy resin composition may be a one-component epoxy resin composition or a two-component epoxy resin composition. In the case of a two-component epoxy resin composition, for example, an epoxy resin may be component A, and a thiol compound and other additives may be component B, and the two components may be used as a kit. The epoxy resin composition may contain one or more of the above-mentioned components such as the thiol compound.
[0043] [Cured Epoxy Resin Product] One embodiment of the present invention may be a cured epoxy resin product obtained by curing the above-described epoxy resin in the presence of the above-described thiol compound. The curing method may be a thermal curing method typically used for epoxy resins. For example, an epoxy resin, a thiol compound, and other optional additives may be mixed to prepare an epoxy resin composition, and the epoxy resin composition may be maintained at a temperature of, for example, 50 to 250°C, preferably 80 to 200°C, and more preferably 120°C ± 10 to 20°C, for, for example, 10 minutes to 3 hours, preferably 30 minutes to 2 hours, and more preferably 1 hour ± 10 to 20 minutes, to obtain a cured product. When preparing the epoxy resin composition, it is preferable to degas the components using a defoamer or the like.
[0044] The epoxy resin cured product of the present invention can be used for applications such as adhesives, casting agents, sealing agents, encapsulants, fiber-reinforcing resins, coating agents, and paints.
[0045] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples. [Method for measuring high-performance liquid chromatography and mass spectrometry (LC / MS measurement)] (Measurement conditions for high-performance liquid chromatography and mass spectrometry) A sample was diluted to 1 mg / mL with tetrahydrofuran (THF), and measurement by high-performance liquid chromatography and mass spectrometry (LC / MS) was performed under the following conditions. High-performance liquid chromatography (HPLC): ACQUITY UPLC (Nihon Waters) Mass spectrum (MS): SQ Detector 2 (Nihon Waters) Column: ACQUITY UPLC BEH C8 1.7 μm, 2.1 mm × 50 mm (Nihon Waters) Mobile phase A: 2 mmol ammonium acetate aqueous solution Mobile phase B: 2-propanol / acetonitrile (50:50) Mobile phase mixing time and mixing ratio (A%): 0-0.5 min (95%) → 1 min-8.5 min (75%) → 9-11 min (5%) → 11.1 min (95%) → 13 min (95%) Flow rate: 0.30 mL / min Analysis time: 13 min Column temperature: 40°C, ion mode: ESI (electrospray ionization) positive Ion polarity: Positive detection mode Desolvation gas flow rate: 700 L / hr, 250°C Cone gas: 70 L / hr Ion source heater: 150°C
[0046] [NMR Measurement Method] NMR data of the thiol compounds (1) and (2) prepared in Examples 1 and 2 were collected using a JEOL A-500 (manufactured by JEOL Corporation).
[0047] Example 1 Synthesis of Thiol Compound (1) (1) Synthesis of Thioester A Tetraallyloxyethane (below, 20 g, 0.078 mol, 1.0 eq), toluene (100 mL), and azobisisobutyronitrile (AIBN, 1.29 g, 0.008 mol, 0.1 eq) were charged into a 200 mL four-neck flask, and thioacetic acid (26.34 g, 0.346 mol, 4.4 eq) was added dropwise under a nitrogen atmosphere, followed by a reaction at 80° C. for 3 hours. The toluene was then removed by concentration under reduced pressure, yielding 45.0 g of thioester A (below) as a yellow liquid.
[0048] Tetraallyloxyethane
[0049] Thioester A
[0050] (2) Synthesis of Thiol Compound Next, a 500 mL four-neck flask was charged with thioester A (40 g) obtained in (1) above, methanol (200 g), and 20% NaOH (20.2 g), and the mixture was reacted at 70°C under a nitrogen atmosphere for 1.5 hours. Next, 2.5 N HCl (30 mL) was added to neutralize the mixture, followed by extraction three times with toluene (50 mL). The extracted organic layer was washed with saturated brine, dehydrated over magnesium sulfate, and insoluble matter was removed by filtration. The toluene was removed from the organic layer of the filtrate by vacuum concentration, yielding 27.2 g of a yellow liquid thiol compound (LC purity 58.3%, yield 97.3%). The resulting thiol compound was analyzed using the LC / MS method described above, and spectral peaks corresponding to the proton adduct at m / z = 391 and the ammonium adduct at m / z = 408 were detected. From the analytical data and the NMR spectrum results shown in FIG. 1, the obtained thiol compound was confirmed to be thiol compound (1) having the following structure.
[0051] Thiol Compound (1)
[0052] Example 2 Synthesis of Thiol Compound (2) (1) Synthesis of Thioester B The following thioester B was obtained in the same manner as in Example 1, except that 20 g (0.078 mol) of tetraallyloxyethane in Example 1 was changed to 24.2 g (0.078 mol) of tetra(2-methylallyl)oxyethane (described below).
[0053] Tetra(2-methylallyl)oxyethane
[0054] Thioester B
[0055] (2) Synthesis of Thiol Compound The thioester B obtained in (1) above was reacted in the same manner as in Example 1 (2) to obtain 28 g of a yellow liquid thiol compound. The obtained thiol compound was measured according to the LC / MS measurement method described above, and a spectral peak of m / z = 447 corresponding to a proton adduct and a spectral peak of m / z = 464 corresponding to an ammonium adduct were detected. From the analytical data, the obtained thiol compound was confirmed to be thiol compound (2) having the following structure:
[0056] Thiol Compound (2)
[0057] [Evaluation Test] The cured state of epoxy resins cured using the thiol compounds obtained in Examples 1 and 2 above was evaluated. Specifically, the epoxy resin, thiol compound, and curing accelerator (Amicure (registered trademark) PN-H, manufactured by Ajinomoto Fine-Techno Co., Ltd.) were weighed and mixed in the amounts shown in Table 1 below (component amounts in Table 1 are in parts by mass). The mixture was then degassed in a revolution-type agitator / defoamer (HM-200W, manufactured by Kyoritsu Seiki Co., Ltd.) at 900 rpm for 2 minutes under vacuum to obtain the desired resin composition. The resulting resin composition was cured in a heat circulation oven at 120°C for 1 hour to obtain a cured product. The surface of the resulting cured product was touched with a finger to confirm whether any residue remained on the finger. jER (registered trademark) 828 (manufactured by Mitsubishi Chemical Corporation) was used as the epoxy resin. PE-1 (pentaerythritol tetrakis(3-mercaptobutyrate), manufactured by Resonac Co., Ltd.) was used as the thiol curing agent in Comparative Example 1.
[0058] PE-1 (Pentaerythritol tetrakis(3-mercaptobutyrate))
[0059] Table 1
[0060] As shown in Table 1, flexible cured products without tack were obtained in Examples 1 and 2. On the other hand, in Comparative Example 1, a cured product without tack was obtained, but it was a hard, elastic cured product.
Claims
1. General formula (I): (I) (In formula (I), each X is independently a hydrogen atom, a C1-C6 alkyl group, a C1-C6 haloalkyl group, or a C1-C6 alkoxy group, and each n is independently an integer of 1 to 5.
2. The compound according to claim 1, wherein each X is independently a hydrogen atom, a methyl group, or an ethyl group, and n is an integer from 1 to 3.
3. The compound according to claim 1, wherein each X is independently a hydrogen atom or a methyl group, and n is 1.
4. The compound shown below. or 5. An epoxy resin composition comprising an epoxy resin and a compound according to any one of claims 1 to 4.
6. A curing agent for epoxy resins, comprising the compound according to any one of claims 1 to 4.
7. An epoxy resin cured product obtained by thermally curing an epoxy resin and a compound according to any one of claims 1 to 4.
Citation Information
Patent Citations
Resin composition, resin cured material, and resin molded product
JP2012153794A
Novel glycoluril having thioether linkage and mercapto group and use thereof
JP2016164134A
Resin curing agent and one-pack type epoxy resin composition
WO2014084292A1
Epoxy resin composition
JP2021031559A
Epoxy resin composition
JP2021036020A