Resin composition, molded body, and method for producing resin composition
The resin composition enhances the toughness and durability of semi-aromatic polyamide-based mechanical parts by adding carbodiimide, addressing the limitations of existing resin compositions in water absorption and mechanical performance.
Patent Information
- Application Number
- PCT/JP2024/011733
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-28
- Filing Date
- 2024-03-25
- Publication Date
- 2024-10-03
AI Technical Summary
Resin compositions containing semi-aromatic polyamides used in mechanical parts, such as gears, face challenges with toughness and durability due to high water absorption and limited improvements in these properties.
A resin composition is developed by adding a predetermined amount of carbodiimide to semi-aromatic polyamide, specifically within the range of 0.05 to 0.5 parts by mass per 100 parts of semi-aromatic polyamide, which enhances the toughness and durability of the molded articles through improved molecular weight and reaction with terminal groups.
The addition of carbodiimide significantly improves the tensile fracture energy and fatigue resistance of the molded articles, making them more suitable for mechanical parts like gears, while maintaining low water absorption and heat resistance.
Smart Images

Figure JP2024011733_03102024_PF_FP_ABST
Abstract
Description
Resin composition, molded article, and method for producing resin composition
[0001] The present invention relates to a resin composition, a molded article, and a method for producing a resin composition. This application claims priority based on Japanese Patent Application No. 2023-052088, filed on March 28, 2023, the contents of which are incorporated herein by reference.
[0002] Polyamides are known to have excellent abrasion resistance and strength, and are used as materials for machine parts, etc. Among polyamides, aliphatic polyamides, which have excellent abrasion resistance and strength, have traditionally been widely used.
[0003] However, aliphatic polyamides have the problem of poor dimensional stability due to their high water absorption, and in recent years, semi-aromatic polyamides with low water absorption have been developed and their application has been studied. For example, in the examples of Patent Document 1, a polyamide resin composition is disclosed in which more than approximately 0.5 parts by mass of a specific aliphatic carbodiimide is added to 100 parts by mass of a specific semi-aromatic polyamide resin, and the composition is evaluated for its resistance to LLC (long life coolant, automotive cooling water) as a type of water resistance.
[0004] Japanese Patent Application Laid-Open No. 2006-176597
[0005] However, when applied to applications such as machine parts such as gears, there is still room for improvement in the toughness and durability of resin compositions containing semi-aromatic polyamides.
[0006] The present invention has been made to solve the above-mentioned problems, and aims to provide a resin composition containing a semi-aromatic polyamide that can be used to produce a molded article with improved toughness and durability, and a molded article of the resin composition.
[0007] The present inventors have conducted extensive research to solve the above problems and have found that molded articles made from resin compositions containing a resin in which a predetermined amount of carbodiimide is added to a semi-aromatic polyamide have improved toughness and durability, leading to the completion of the present invention.
[0008] <1> A resin composition comprising a resin in which a carbodiimide is added to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the carbodiimide is added in an amount of 0.05 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the semi-aromatic polyamide in the resin composition. [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p is an integer of 4 to 12.] <2> The resin composition according to <1>, wherein the carbodiimide is an aliphatic polycarbodiimide. <3> In the formula (1), the Ar 1 represents a 1,4-phenylene group, and p is 10. <4> The resin composition according to any one of <1> to <3>, wherein the semi-aromatic polyamide has a melt mass-flow rate (MFR) of 150 g / 10 min or less, as measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160 g. <5> The resin composition according to any one of <1> to <4>, wherein the carbodiimide group equivalent is 100 g / mol or more and 1000 g / mol or less. <6> The resin composition according to any one of <1> to <5>, which is a gear molding resin composition used as a gear molding material. <7> A molded product comprising the resin composition according to any one of <1> to <6>. <8> A method for producing a resin composition according to any one of <1> to <6>, comprising mixing a semi-aromatic polyamide with a carbodiimide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the amount of the carbodiimide blended in the resin composition is 0.05 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the semi-aromatic polyamide: [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1may be the same or different, and p is an integer of 4 to 12.] <9> Use of the resin composition according to any one of <1> to <5> above for molding a gear. <10> Use of the resin composition according to any one of <1> to <5> above for producing a molding material for a gear.
[0009] According to the present invention, there can be provided a resin composition containing a semi-aromatic polyamide and capable of producing a molded article having improved toughness and durability, and a molded article of the resin composition.
[0010] Hereinafter, embodiments of the resin composition, molded article, and method for producing the resin composition of the present invention will be described.
[0011] <Resin Composition> A resin composition of an embodiment is a resin composition containing a resin in which a carbodiimide is added to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the carbodiimide is added in an amount of 0.05 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the semi-aromatic polyamide in the resin composition.
[0012]
[0013] [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p is an integer of 4 to 12.
[0014] Molded articles of a resin composition according to an embodiment, which contains a resin in which the above-mentioned predetermined amount of carbodiimide is added to a semi-aromatic polyamide, have improved toughness, as measured by tensile fracture energy, and durability, as evaluated by fatigue testing, compared to molded articles of a resin composition in which no carbodiimide is added.
[0015] As will be shown in the examples below, such improvements in toughness and durability are not observed when an aliphatic polyamide is contained in place of a semi-aromatic polyamide.
[0016] Furthermore, as shown in the examples described below, by adding carbodiimide in a range of 0.05 parts by mass or more and 0.5 parts by mass or less to 100 parts by mass of semi-aromatic polyamide, the toughness and durability of the molded body are improved to a good extent.
[0017] Therefore, by adding a specific amount of carbodiimide to a specific combination of carbodiimide and semi-aromatic polyamide, the toughness and durability of the molded article are improved satisfactorily.
[0018] In the resin composition of the embodiment, the carbodiimide is added in an amount of 0.05 parts by mass or more, preferably 0.1 parts by mass or more, more preferably 0.15 parts by mass or more, more preferably 0.2 parts by mass or more, and even more preferably 0.3 parts by mass or more, per 100 parts by mass of semi-aromatic polyamide. In the resin composition of the embodiment, the carbodiimide is added in an amount of 0.5 parts by mass or less, preferably less than 0.5 parts by mass, more preferably 0.45 parts by mass or less, and even more preferably 0.4 parts by mass or less, per 100 parts by mass of semi-aromatic polyamide.
[0019] The upper and lower limits of the amount of carbodiimide added can be freely combined. In the resin composition of the embodiment, the amount of carbodiimide added relative to 100 parts by mass of semi-aromatic polyamide is 0.05 parts by mass or more and 0.5 parts by mass or less, may be 0.1 parts by mass or more and less than 0.5 parts by mass, may be 0.15 parts by mass or more and 0.45 parts by mass or less, may be 0.2 parts by mass or more and 0.4 parts by mass or less, may be 0.3 parts by mass or more and 0.4 parts by mass or less.
[0020] The resin composition of the embodiment can be obtained by blending a semi-aromatic polyamide, a carbodiimide, and the other optional components used as needed such that the total content (mass %) of these components in the resin composition does not exceed 100 mass % relative to the total mass of the resin composition.
[0021] The semi-aromatic polyamide and carbodiimide blended in the resin composition of the embodiment will be described below.
[0022] The resin composition of the embodiment may contain a semi-aromatic polyamide and a carbodiimide in the form of a reaction product thereof.
[0023] <Semi-aromatic Polyamide> The semi-aromatic polyamide contained in the resin composition of the present embodiment is a semi-aromatic polyamide having a structural unit represented by the following general formula (1).
[0024]
[0025] [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p is an integer of 4 to 12.
[0026] The semi-aromatic polyamide contained in the resin composition of the embodiment can be obtained as a polymer of an aliphatic diamine and an aromatic dicarboxylic acid. The aliphatic diamine may be an aliphatic diamine having 4 to 12 carbon atoms. Examples of aliphatic diamines having 4 to 12 carbon atoms include 1,4-butanediamine, 1,5-pentanediamine, 1,6-hexanediamine, 1,7-heptanediamine, 1,8-octanediamine, 1,9-nonanediamine, 1,10-decanediamine, 1,11-undecanediamine, and 1,12-dodecanediamine. These may be used alone or in combination of two or more.
[0027] Examples of aromatic dicarboxylic acids include terephthalic acid, phthalic acid, isophthalic acid, naphthalenedicarboxylic acid, etc. These may be used alone or in combination of two or more.
[0028] From the viewpoint of excellent heat resistance of the resulting molded article, it is more preferable that Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1may be the same or different, and p may be 9 or 10 from the viewpoint of achieving superior low water absorption.
[0029] From the viewpoint of obtaining a molded article with even better heat resistance, it is more preferable that, in the general formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p may be 10 from the viewpoint of achieving a more excellent effect of improving toughness and durability by adding carbodiimide and a more excellent low water absorption.
[0030] The Ar 1 The phenylene group in Ar may be a 1,4-phenylene group or a 1,3-phenylene group. 1 The naphthylene group includes a 2,6-naphthylene group and a 2,7-naphthylene group.
[0031] Preferably, in the general formula (1), Ar 1 represents a 1,4-phenylene group, and p may be an integer of 4 to 12.
[0032] More preferably, in the general formula (1), Ar 1 represents a 1,4-phenylene group, and p may be 9 or 10.
[0033] Particularly preferably, in the general formula (1), Ar 1 represents a 1,4-phenylene group, and p may be 10.
[0034] In the polyamide, the content of the structural unit represented by the general formula (1) is preferably 40% or more, more preferably 80% or more, and even more preferably 90% or more, relative to the total number of all structural units in the polyamide (100%).
[0035] In the polyamide, the structural unit represented by the general formula (1) is Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1may be the same or different, and the content of structural units in which p is 9 or 10 is preferably 40% or more, more preferably 80% or more, and even more preferably 90% or more, relative to the total number of all structural units in the polyamide (100%), and may be 100%.
[0036] In the polyamide, the structural unit represented by the general formula (1) is Ar 1 represents a 1,4-phenylene group, and p is 9 or 10, the content of which is preferably 40% or more, more preferably 80% or more, and even more preferably 90% or more, relative to the total number of all structural units in the polyamide (100%), and may be 100%.
[0037] In the polyamide, the structural unit represented by the general formula (1) is Ar 1 represents a 1,4-phenylene group, and p is 10, the content of which is preferably 40% or more, more preferably 80% or more, and even more preferably 90% or more, relative to the total number of all structural units in the polyamide (100%), and may be 100%.
[0038] The melt mass-flow rate (MFR) of the semi-aromatic polyamide, measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160g, is preferably 150g / 10min or less, more preferably 125g / 10min or less, and even more preferably 100g / 10min or less. In another aspect, the melt mass-flow rate (MFR) of the semi-aromatic polyamide, measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160g, is preferably 80g / 10min or less, more preferably 50g / 10min or less, and even more preferably 30g / 10min or less. A resin composition containing a semi-aromatic polyamide having an MFR equal to or less than the above upper limit can exhibit even better toughness.
[0039] The melt mass-flow rate (MFR) of the semi-aromatic polyamide, measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160 g, may be 5 g / 10 min or more, 10 g / 10 min or more, or 15 g / 10 min or more.
[0040] The upper and lower limits of the melt mass-flow rate (MFR) of the semi-aromatic polyamides exemplified above can be freely combined.
[0041] The melt mass-flow rate (MFR) of the semi-aromatic polyamide measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160g may be, for example, 5g / 10min to 150g / 10min, 10g / 10min to 125g / 10min, or 15g / 10min to 100g / 10min. In another aspect, the melt mass-flow rate (MFR) of the semi-aromatic polyamide measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160g may be, for example, 5g / 10min to 80g / 10min, 10g / 10min to 50g / 10min, or 15g / 10min to 30g / 10min.
[0042] The MFR of the semi-aromatic polyamide can be controlled by appropriately adjusting the conditions related to the reaction efficiency of the polymerization reaction, such as the raw material monomer, catalyst, or reaction time.
[0043] An example of a resin composition of the embodiment is a resin composition containing a resin in which a carbodiimide is added to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the general formula (1), the proportion of the semi-aromatic polyamide relative to the total mass (100 mass%) of the resin composition may be 50 mass% or more, and the carbodiimide is added in an amount of 0.05 part by mass or more and 0.5 part by mass or less relative to 100 parts by mass of the semi-aromatic polyamide in the resin composition.
[0044] In the resin composition of the embodiment, the proportion of the semi-aromatic polyamide relative to the total mass (100 mass%) of the resin composition may be 50 mass% or more, 50 mass% or more and 99.99 mass% or less, 70 mass% or more and 99.90 mass% or less, 80 mass% or more and 99.90 mass% or less, or 90 mass% or more and 99.90 mass% or less.
[0045] <Carbodiimide> The carbodiimide used in the resin composition of the present embodiment is not particularly limited as long as it has a carbodiimide group (represented by —N═C═N—) in the molecule, and may be a monocarbodiimide having one carbodiimide group in the molecule, or a polycarbodiimide having two or more carbodiimide groups in the molecule.
[0046] The carbodiimide may be an aromatic carbodiimide or an aliphatic carbodiimide. Furthermore, the carbodiimide may be an aromatic monocarbodiimide or an aliphatic monocarbodiimide, or may be an aromatic polycarbodiimide or an aliphatic polycarbodiimide. From the viewpoint of high reactivity with polyamide, the carbodiimide is preferably an aliphatic polycarbodiimide.
[0047] The aromatic polycarbodiimide may be a polymer having a repeating unit composed of a carbodiimide group and an aromatic hydrocarbon in the main chain, and the aliphatic polycarbodiimide may be a polymer having a repeating unit composed of a carbodiimide group and a non-aromatic hydrocarbon in the main chain.
[0048] The repeating structure composed of carbodiimide groups and aromatic hydrocarbons can contain a divalent aromatic hydrocarbon group. Examples of the divalent aromatic hydrocarbon group include divalent aryl groups such as phenylene, naphthylene, and biphenylene, and divalent aromatic hydrocarbon groups having 6 to 14 carbon atoms are preferred. One or more hydrogen atoms in the aromatic hydrocarbon group may be substituted, independently of one another, with a halogen atom, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms.
[0049] The repeating structure composed of carbodiimide groups and non-aromatic hydrocarbons can contain a divalent aliphatic hydrocarbon group. The divalent aliphatic hydrocarbon group may be linear, branched, or cyclic. Examples of the divalent aliphatic hydrocarbon group include divalent saturated aliphatic hydrocarbon groups such as alkylene groups and divalent alicyclic hydrocarbon groups such as cycloalkylene groups, and the compound may contain a combination of these structures. The divalent saturated aliphatic hydrocarbon group is preferably a divalent saturated aliphatic hydrocarbon group having 1 to 20 carbon atoms. The divalent alicyclic hydrocarbon group is preferably a divalent alicyclic hydrocarbon group having 3 to 20 carbon atoms. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, and a hexylene group. Examples of the cycloalkylene group include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, and a cyclohexylene group.
[0050] The aliphatic polycarbodiimide may be linear, branched, or cyclic (also referred to as an alicyclic polycarbodiimide or an alicyclic polycarbodiimide). From the viewpoint of a superior effect of improving durability due to the addition of carbodiimide, the aliphatic polycarbodiimide is preferably linear or branched.
[0051] Commercially available aliphatic polycarbodiimides include Carbodilite (registered trademark) HMV-15CA (manufactured by Nisshinbo Chemical Inc.), Carbodilite HMV-8CA (manufactured by Nisshinbo Chemical Inc.), Carbodilite LA-1 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-02B (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-03 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-04K (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-07 (manufactured by Nisshinbo Chemical Inc.), Carbodilite V-09 (manufactured by Nisshinbo Chemical Inc.), Carbodilite 10M-SP (manufactured by Nisshinbo Chemical Inc.), and Carbodista (registered trademark) TCC-NP (manufactured by Teijin Limited).
[0052] Commercially available aromatic polycarbodiimides include Stavaxol (registered trademark) P (manufactured by Lanxess), Stavaxol P100 (manufactured by Lanxess), Stavaxol P400 (manufactured by Lanxess), Stavaxol I (manufactured by Lanxess), and Carbodilite V-05 (manufactured by Nisshinbo Chemical Inc.).
[0053] The carbodiimide can be obtained by decarboxylation of an isocyanate having a structure corresponding to the carbodiimide used in the resin composition of the embodiment, such as an aromatic diisocyanate, an aliphatic diisocyanate, etc. Examples of the isocyanate include hexamethylene diisocyanate, cyclohexane-1,4-diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylbutane-4,4'-diisocyanate, and methylcyclohexane diisocyanate.
[0054] The molar mass of the carbodiimide used in the resin composition of this embodiment may be 300 g / mol or more and 10,000 g / mol or less, 500 g / mol or more and 9,000 g / mol or less, 500 g / mol or more and 6,500 g / mol or less, or 1,000 g / mol or more and 8,000 g / mol or less.
[0055] The carbodiimide group equivalent of the carbodiimide used in the resin composition of this embodiment may be 100 g / mol or more and 1000 g / mol or less, 150 g / mol or more and 600 g / mol or less, or 230 g / mol or more and 280 g / mol or less.
[0056] The resin composition of the present embodiment is a resin composition containing a resin in which a carbodiimide is added to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the general formula (1) [in formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1may be the same or different, and p is an integer of 4 to 12.], and the carbodiimide is added in an amount of 0.05 parts by mass or more and 0.5 parts by mass or less relative to 100 parts by mass of the semi-aromatic polyamide in the resin composition, and the melt mass-flow rate (MFR) of the semi-aromatic polyamide measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160 g is 100 g / 10 min or less, and the carbodiimide group equivalent of the carbodiimide is 100 g / mol or more and 1000 g / mol or less. Another embodiment of the resin composition is a resin composition containing a resin obtained by adding a carbodiimide to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the general formula (1), and in the formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p is 9 or 10, preferably 10; the carbodiimide is added in an amount of 0.15 parts by mass or more and 0.45 parts by mass or less, preferably 0.2 parts by mass or more and 0.4 parts by mass or less, per 100 parts by mass of the semi-aromatic polyamide in the resin composition; the melt mass-flow rate (MFR) of the semi-aromatic polyamide, measured in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160 g, is 15 g / 10 min or more and 30 g / 10 min or less; and the carbodiimide group equivalent of the carbodiimide is 230 g / mol or more and 280 g / mol or less.
[0057] (Optional Components) The resin composition of the present embodiment may contain optional components that do not fall under any of the semi-aromatic polyamides, carbodiimides, and reaction products thereof, as long as the effects of the present invention are not impaired.
[0058] Examples of optional components include fillers, additives, and resins other than the semi-aromatic polyamides (hereinafter sometimes referred to as "other resins"). These optional components may be used alone or in combination of two or more.
[0059] The filler may be a fibrous filler or a granular filler, and may be an inorganic filler or an organic filler.
[0060] Examples of the additives include stabilizers, release agents, antioxidants, heat stabilizers, ultraviolet absorbers, antistatic agents, surfactants, flame retardants, and colorants.
[0061] Examples of other resins include thermoplastic resins such as polyester, polyphenylene sulfide, polyether ketone, polycarbonate, polyphenylene ether, polyetherimide, and fluororesin; and thermosetting resins such as phenolic resin, epoxy resin, polyimide resin, and cyanate resin.
[0062] According to the resin composition of the embodiment described above, the addition of carbodiimide in the above-mentioned predetermined amount improves the toughness and durability of the article molded from the resin composition.
[0063] The details of why the addition of carbodiimide in the resin composition of this embodiment improves the toughness and durability of the molded article of the resin composition are not clear, but it is thought that, for example, the carboxyl groups or amino groups present at the terminals of the semi-aromatic polyamide react with the carbodiimide groups of the carbodiimide, resulting in a high molecular weight of the semi-aromatic polyamide, thereby improving the toughness and durability.
[0064] The toughness of a resin composition can be evaluated, for example, using the tensile breaking energy measured on a test piece in the below-described "Tensile Test" as an index. The higher the tensile breaking energy, the better the toughness can be determined to be.
[0065] [Tensile Test] Using an injection molding machine (for example, an electric high-performance injection molding machine NEX50IV-5EG manufactured by Nissei Plastic Industrial Co., Ltd.) with a resin composition to be measured as a molding material, cylinder temperatures are 335 ° C. nozzle, 330 ° C. front, 320 ° C. middle, 315 ° C. rear, 120 ° C. mold temperature, 8 MPa back pressure, 100 rpm screw rotation speed, 26 mm / sec injection speed, 90 MPa injection pressure, 2 seconds injection time, 80 MPa dwell pressure, and 30 seconds cooling time. Obtain a test piece A1 type specified in ISO 3167. For this test piece, in accordance with ISO 527, at a test speed of 5 mm / min, under an atmosphere of 23 ° C. and 50% relative humidity, the tensile stress at break (MPa), tensile strain at break (%), and tensile energy at break (J) are measured. The measurement is carried out using a Tensilon universal testing machine (for example, RTG-1310 manufactured by A&D Co., Ltd.) Measurement is carried out for five samples, and the average value is used.
[0066] In the resin composition of the embodiment, the tensile fracture energy measured on the test piece may be, for example, 20 J or more, 30 J or more, 30 J or more to 200 J or less, or 40 J or more to 150 J or less.
[0067] The durability of the resin composition can be evaluated, for example, using the number of times that a test piece can be pulled until it breaks, as an index, in the fatigue test described below. The higher the number of times, the better the durability can be determined to be.
[0068] [Fatigue Test] Using pellets of the resin composition to be measured as the molding material, an injection molding machine (for example, injection molding machine SE100EV-A type, manufactured by Sumitomo Heavy Industries, Ltd.) is used to obtain a test piece (thickness: 2.5 mm) in accordance with JIS K 7118 under the injection conditions of a nozzle temperature of 340°C, a front temperature of 330°C, a middle temperature of 330°C, and a rear temperature of 320°C, a mold temperature of 120°C, a back pressure of 6 MPa, a screw rotation speed of 100 rpm, an injection speed of 50 mm / sec, an injection pressure of 130 MPa, an injection time of 0.86 seconds, a dwell pressure of 90 MPa, and a cooling time of 60 seconds. This test piece is subjected to a tensile fatigue test in accordance with JIS K 7118 using a hydraulic servo strength tester (for example, manufactured by Shimadzu Corporation, product name: Hydraulic Tabletop Servo Pulser, EHF-LV010K1A-010-0) under conditions of a stress ratio of 0.2, a frequency of 10 Hz, a chuck distance of 50 mm, and a waveform of sine wave, in an atmosphere of a test temperature of 23°C and a relative humidity of 50%. Measurements are made on 10 samples, and the average value is used.
[0069] In the resin composition of the embodiment, the test piece is subjected to a tensile stress of 40 MPa, and the number of tensile cycles measured is, for example, 2.0 × 10 6 times or more, and 6 5.0 x 10 times or more 7 times or less, and 6 1.0 x 10 times or more 7 times or less, and 6 7.0 x 10 times or more 6 times or less, and 6 More than 6.0 x 10 6 It may be less than once.
[0070] The resin composition has the above-mentioned improved toughness and durability, and is suitable as a resin composition to be used as a molding material for mechanical parts such as gears, and is particularly suitable as a gear molding resin composition to be used as a molding material for gears.
[0071] <<Method for Producing Resin Composition>> A method for producing a resin composition according to an embodiment includes mixing a semi-aromatic polyamide and a carbodiimide.
[0072] According to the method for producing a resin composition of this embodiment, it is possible to produce the resin composition of the above-described embodiment.
[0073] The resin composition of the embodiment can be obtained by mixing the above-mentioned semi-aromatic polyamide, carbodiimide, and other optional components used as needed all at once or in an appropriate order.
[0074] The resin composition of the present embodiment can be provided as a pelletized product obtained by melt-kneading the semi-aromatic polyamide, the carbodiimide, and other optional components used as needed, for example, using an extruder.
[0075] Examples of the semi-aromatic polyamide, carbodiimide, and other components include those described above in the section "Resin composition."
[0076] The mixing ratio of the above components can be exemplified by the component amounts explained above in the section "Resin Composition."
[0077] For example, an example of a method for producing a resin composition of an embodiment includes mixing a semi-aromatic polyamide with a carbodiimide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the amount of the carbodiimide in the resin composition is 0.05 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the semi-aromatic polyamide:
[0078]
[0079] [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar groups contained in the semi-aromatic polyamide 1 may be the same or different, and p is an integer of 4 to 12.
[0080] The resin composition thus obtained, particularly pellets of the resin composition, can be suitably used as a molding material for the molded article described below.
[0081] The resin composition of the embodiment includes both a pre-solidified state and a post-solidified state. The resin composition after solidification (solidified resin composition) can be used to form the molded article of the embodiment.
[0082] <<Molded Article>> A molded article according to one embodiment of the present invention includes the resin composition according to the above embodiment. An example of the molded article according to the embodiment is a molded article made of the resin composition according to the embodiment. An example of the molded article according to the embodiment is a molded article molded from the resin composition according to the above embodiment.
[0083] The method for molding the resin composition into a molded article is not particularly limited, but melt molding is preferred, and examples of such methods include extrusion molding, T-die molding, blow molding, and injection molding. The resin composition can be molded into the shape of a desired molded article by selecting a molding method depending on the shape of the molded article, etc.
[0084] The molded article of this embodiment can be applied to any application to which a resin composition can generally be applied. Examples of the molded article of this embodiment include electrical and electronic components such as connectors, sockets, relay parts, coil bobbins, optical pickups, oscillators, printed wiring boards, circuit boards, semiconductor packages, and computer-related parts; semiconductor manufacturing process-related parts such as IC trays and wafer carriers; home electrical appliance parts such as VTRs, televisions, irons, air conditioners, stereos, vacuum cleaners, refrigerators, rice cookers, and lighting fixtures; lighting fixture parts such as lamp reflectors and lamp holders; audio product parts such as compact discs, laser discs (registered trademark), and speakers; communication equipment parts such as ferrules for optical cables, telephone parts, facsimile parts, and modems; and copier parts such as separation claws and heater holders. or printing press-related parts; machine parts such as impellers, fan gears, gears, bearings, motor parts and cases; automotive parts such as automotive mechanism parts, engine parts, engine room parts, electrical parts, and interior parts; cooking utensils such as microwave cooking pots and heat-resistant tableware; heat-insulating or sound-proofing materials such as flooring and wall materials, supporting materials such as beams and pillars, and building materials such as roofing materials, or civil engineering and construction materials; parts for aircraft, spacecraft, or space equipment; radiation facility components such as nuclear reactors, marine facility components, cleaning jigs, optical equipment parts, valves, pipes, nozzles, filters, membranes, medical equipment parts and materials, sensor parts, sanitary fixtures, sporting goods, leisure goods, and cable ties.
[0085] The molded article of the embodiment has improved toughness and durability, and is therefore suitable for use as a mechanical part such as a gear, and can be particularly suitable for use as a gear.
[0086] The type of gear is not particularly limited, and examples thereof include spur gears, helical gears, racks, internal gears, worm gears, worm wheel gears, bevel gears, and hypoid gears.
[0087] Resin compositions containing resins in which carbodiimide is added to polyamide have been known. However, it was not known that a resin composition in which a smaller amount of carbodiimide than conventional semi-aromatic polyamide is added (0.05 parts by mass or more and 0.5 parts by mass or less of carbodiimide per 100 parts by mass of semi-aromatic polyamide) can significantly improve the toughness and durability of molded articles. According to the present embodiment described above, it is possible to provide a resin composition containing semi-aromatic polyamide that can produce molded articles with improved toughness and durability, and a molded article of the resin composition.
[0088] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples.
[0089] <<Measurement>> [Melt Mass-Flow Rate (MFR) of Polyamide] The melt mass-flow rate (MFR) of polyamide was measured using an MFR measuring device (Melt Indexer G-01, manufactured by Toyo Seiki Seisaku-sho, Ltd.) in accordance with JIS K 7210 at a test temperature of 330°C and a load of 2160 g.
[0090] [Tensile Test] Using pellets of each resin composition obtained in the Examples and Comparative Examples as molding materials, an injection molding machine (electric high-performance injection molding machine NEX50IV-5EG, manufactured by Nissei Plastic Industrial Co., Ltd.) was used, and the cylinder temperature was set to a nozzle temperature of 335 ° C., front temperature of 330 ° C., middle temperature of 320 ° C., rear temperature of 315 ° C., mold temperature of 120 ° C., back pressure of 8 MPa, screw rotation speed of 100 rpm, injection speed of 26 mm / sec, injection pressure of 90 MPa, injection time of 2 seconds, dwell pressure of 80 MPa, and cooling time of 30 seconds. Test pieces of type A specified in ISO 3167 were obtained under the injection conditions. For these test pieces, the tensile stress at break (MPa), tensile strain at break (%), and tensile energy at break (J) were measured in accordance with ISO 527 at a test speed of 5 mm / min under an atmosphere of 23 ° C. and relative humidity of 50%. The measurement was carried out using a Tensilon universal testing machine (RTG-1310, manufactured by A&D Co., Ltd.) The measurement was carried out for five samples, and the average value was calculated.
[0091] [Fatigue Test] Using pellets of each resin composition obtained in the Examples and Comparative Examples as molding materials, an injection molding machine (SE100EV-A injection molding machine, manufactured by Sumitomo Heavy Industries, Ltd.) was used to obtain test pieces (thickness: 2.5 mm) in accordance with JIS K 7118 under the injection conditions of a nozzle temperature of 340°C, a front temperature of 330°C, a middle temperature of 330°C, and a rear temperature of 320°C, a mold temperature of 120°C, a back pressure of 6 MPa, a screw rotation speed of 100 rpm, an injection speed of 50 mm / sec, an injection pressure of 130 MPa, an injection time of 0.86 sec, a dwell pressure of 90 MPa, and a cooling time of 60 sec. A tensile fatigue test was carried out on this test piece in accordance with JIS K 7118 at the tensile stress (40 MPa or 75 MPa) shown in each table using a hydraulic servo strength tester (manufactured by Shimadzu Corporation, product name: Hydraulic Tabletop Servo Pulser, EHF-LV010K1A-010-0) under the conditions of a test temperature of 23°C and a relative humidity of 50%, a stress ratio of 0.2, a frequency of 10 Hz, a chuck distance of 50 mm, and a waveform of sine wave. Measurements were carried out on 10 samples, and the average value was calculated.
[0092] <Production of Resin Composition> <Raw Materials> Base resin: Polyamide PA10T (Ar 1 represents a 1,4-phenylene group, and p is 10, a semi-aromatic polyamide having a structural unit represented by the general formula (1), MFR: 24 g / 10 min) PA46 (aliphatic polyamide, MFR: not measurable due to high value) PA9T (Ar 1 represents a 1,4-phenylene group, and p is 9. A semi-aromatic polyamide having a structural unit represented by the general formula (1), MFR: 20 g / 10 min.
[0093] Carbodiimides Aliphatic polycarbodiimide (manufactured by Nisshinbo Chemical Inc., Carbodilite HMV-15CA, polydicyclohexylbutane carbodiimide, molar mass: 5327 g / mol, carbodiimide group equivalent: 262 g / mol) Aliphatic polycarbodiimide (manufactured by Nisshinbo Chemical Inc., Carbodilite LA-1, polydicyclohexylmethane carbodiimide, molar mass: 6000 g / mol, carbodiimide group equivalent: 247 g / mol) Alicyclic polycarbodiimide (manufactured by Teijin Limited, Carbodistar TCC-NP, molar mass: 516 g / mol, carbodiimide group equivalent: 256 g / mol)
[0094] [Examples 1 to 7, Comparative Examples 1 to 8] The polyamides and carbodiimides of the types shown in Tables 1 to 5 were charged into a twin-screw extruder in the blending ratios (parts by mass) shown in each table, and melt-kneaded while degassing at a cylinder temperature of 330°C and a screw rotation speed of 150 rpm. The resulting kneaded mixture was extruded in the form of strands through a circular nozzle (exhaust port), and then pelletized with a strand cutter to obtain pellet-shaped resin compositions of the Examples and Comparative Examples.
[0095] The results of the above measurements are shown in Tables 1 to 5.
[0096]
[0097]
[0098]
[0099]
[0100]
[0101] Referring to Table 1, in Examples 1 and 2 in which 0.05 parts by mass or more and 0.5 parts by mass or less of aliphatic polycarbodiimide (Carbodilite HMV-15CA) was added to 100 parts by mass of semi-aromatic polyamide (PA10T), the toughness, measured by the tensile fracture energy as an index, was improved, and the durability confirmed by a fatigue test was also improved, compared to Comparative Example 1 in which no aliphatic polycarbodiimide was added.
[0102] On the other hand, in Comparative Examples 2 and 3, in which more than 0.5 parts by mass of aliphatic polycarbodiimide (Carbodilite HMV-15CA) was added to 100 parts by mass of semi-aromatic polyamide (PA10T), it was confirmed that the degree of improvement in toughness and durability was inferior to that of Examples 1 and 2.
[0103] Furthermore, as shown in Tables 2 and 3, similar results were observed when an alicyclic polycarbodiimide (Carbodistar TCC-NP) or an aliphatic polycarbodiimide (Carbodilite LA-1) was used instead of the aliphatic polycarbodiimide (Carbodilite HMV-15CA).
[0104] As shown in Table 4, similar results were confirmed when semi-aromatic polyamide (PA9T) was used instead of semi-aromatic polyamide (PA10T).
[0105] However, referring to Table 5, in Comparative Examples 6 to 8 in which aliphatic polyamide (PA46) was used instead of semi-aromatic polyamide (PA10T), no significant improvement in toughness and durability was confirmed.
[0106] The above results show that the toughness and durability of the resin composition can be effectively improved by adding carbodiimide in a range of 0.05 parts by mass or more and 0.5 parts by mass or less to 100 parts by mass of semi-aromatic polyamide.
[0107] The configurations and combinations thereof in each embodiment are merely examples, and additions, omissions, substitutions, and other modifications of the configurations are possible without departing from the spirit of the present invention. Furthermore, the present invention is not limited to each embodiment, but is limited only by the scope of the claims.
Claims
1. A resin composition comprising a resin in which a carbodiimide is added to a semi-aromatic polyamide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the carbodiimide is added in an amount of 0.05 part by mass or more and 0.5 part by mass or less per 100 parts by mass of the semi-aromatic polyamide in the resin composition. [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar in the semi-aromatic polyamide 1 may be the same or different, and p is an integer of 4 to 12.
2. The resin composition according to claim 1, wherein the carbodiimide is an aliphatic polycarbodiimide.
3. In the formula (1), the Ar 1 The resin composition according to claim 1 or 2, wherein: represents a 1,4-phenylene group; and p is 10.
4. The resin composition according to claim 1 or 2, wherein the semi-aromatic polyamide has a melt mass-flow rate (MFR) of 150 g / 10 min or less, measured in accordance with JIS K 7210 at a test temperature of 330° C. and a load of 2,160 g.
5. The resin composition according to claim 1 or 2, wherein the carbodiimide group equivalent of the carbodiimide is 100 g / mol or more and 1000 g / mol or less.
6. The resin composition according to claim 1 or 2, which is a resin composition for molding gears, used as a molding material for gears.
7. A molded article comprising the resin composition according to claim 1 or 2.
8. A method for producing a resin composition according to claim 1 or 2, comprising mixing a semi-aromatic polyamide with a carbodiimide, wherein the semi-aromatic polyamide is a semi-aromatic polyamide having a structural unit represented by the following general formula (1), and the amount of the carbodiimide in the resin composition is 0.05 parts by mass or more and 0.5 parts by mass or less per 100 parts by mass of the semi-aromatic polyamide. [In formula (1), Ar 1 represents a phenylene group or a naphthylene group, and the plurality of Ar in the semi-aromatic polyamide1 may be the same or different, and p is an integer of 4 to 12.
Citation Information
Patent Citations
Stabilized antibody protein solution
JP2023052088A
Polyamide resin composition
JP2006176597A
Electrically conductive endless belt
JP2019003139A
Resin composition for extrusion molding, molding material for extrusion molding, and extrusion molded body
JP2023010587A