Adhesive composition and method for producing same, and adhesive sheet

The adhesive composition, featuring a graft-modified ethylene/α-olefin copolymer and a (meth)acrylic resin, addresses the limitations of conventional adhesives by enhancing adhesiveness and moisture resistance, ensuring performance in low-temperature and high-humidity environments.

WO2024204149A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011865
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional adhesive compositions used in electronic devices and touch panels face challenges with insufficient low-temperature flexibility and moisture resistance, particularly in high-humidity and high-temperature automotive applications.

Method used

A graft-modified ethylene/α-olefin copolymer-based adhesive composition is developed, incorporating a (meth)acrylic resin, a graft-modified ethylene/α-olefin copolymer, and a crosslinking agent, which includes a main chain derived from ethylene/α-olefin copolymer and a graft moiety from unsaturated monomers with heteroatoms, enhancing adhesiveness and moisture resistance while maintaining low-temperature flexibility.

Benefits of technology

The adhesive composition exhibits improved adhesiveness, moisture resistance, and low-temperature flexibility, making it suitable for diverse electronic and automotive applications, including those with high-humidity and high-temperature conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The purpose of the present invention is to provide an adhesive composition having sufficient adhesiveness and excellent moisture resistance and low-temperature flexibility. This adhesive composition comprises: a (meth)acrylic resin (A); a graft-modified ethylene / α-olefin copolymer (B) containing (b-1) a main chain part derived from an ethylene / α-olefin copolymer (B0) and (b-2) a graft part derived from an unsaturated monomer including at least one heteroatom; and a crosslinking agent (C).
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive composition, method for producing the same, and adhesive sheet

[0001] The present invention relates to an adhesive composition having sufficient adhesiveness and excellent moisture resistance and low-temperature flexibility, a method for producing the same, and an adhesive sheet having an adhesive layer formed from the adhesive composition.

[0002] In recent years, adhesives have become widely used for sealing electronic devices such as organic EL devices, solar cells, and sensor devices, as well as image display devices such as liquid crystal displays, and input / output devices such as touch panels used in combination with image display devices. In the production of these devices, adhesive compositions and adhesive sheets having an adhesive layer formed from the adhesive composition are often used.

[0003] The use of touch panels in automobiles is also expanding, and automotive applications require higher high-temperature, high-humidity durability than general applications due to factors such as high temperatures in summer. For example, Patent Document 1 discloses an adhesive composition that has excellent performance even under high-temperature, high-humidity conditions, the adhesive composition containing a specific (meth)acrylic copolymer, an olefin polymer having a specific viscosity, and a crosslinking agent, and also discloses an adhesive sheet having an adhesive layer formed from such an adhesive composition.

[0004]

[0003] In addition, in recent years, electronic components constituting image display devices and input / output devices have sometimes been provided with printed portions on their peripheries to impart design features. When bonding such printed surfaces with adhesive sheets, flexibility is required to conform to uneven surfaces. For example, Patent Document 2 discloses an adhesive composition having excellent flexibility, which includes two types of methacrylic acid alkyl ester monomers having different numbers of carbon atoms in the alkyl groups, a crosslinker, and a plasticizer.

[0005] International Publication No. 2019 / 013130 ​​Pamphlet Japanese Patent Application Laid-Open No. 2015-105329

[0006] However, conventional pressure-sensitive adhesive compositions have room for improvement in terms of flexibility in low-temperature environments and compatibility between adhesive strength and moisture resistance. For example, pressure-sensitive adhesive compositions containing a (meth)acrylic copolymer, an unmodified olefin polymer, and a crosslinking agent tend to have insufficient moisture resistance, and therefore have room for improvement in terms of compatibility between adhesive strength and moisture resistance.

[0007] An object of the present invention is to provide an adhesive composition that has sufficient adhesiveness, and is excellent in moisture resistance and low-temperature flexibility.

[0008] As a result of intensive research to solve the above-mentioned problems, the present inventors have found that the above-mentioned problems can be solved by employing a specific graft-modified olefin polymer as the olefin polymer in an adhesive composition containing a (meth)acrylic copolymer, an olefin polymer, and a crosslinking agent, and have thus completed the present invention.

[0009] The present invention provides the following:

[0010] [1] A pressure-sensitive adhesive composition comprising: a (meth)acrylic resin (A); a graft-modified ethylene / α-olefin copolymer (B) satisfying the following requirements (b-1) to (b-2); and a crosslinking agent (C); (b-1) comprising a main chain portion derived from the ethylene / α-olefin copolymer (B0); and (b-2) comprising a graft portion derived from at least one unsaturated monomer containing a hetero atom.

[0011] [2] The pressure-sensitive adhesive composition according to [1], wherein the (meth)acrylic resin (A) satisfies the following (a-1) to (a-2): (a-1) it contains a structural unit derived from a (meth)acrylate having an alkyl group having 1 to 12 carbon atoms and a structural unit derived from a (meth)acrylate containing a hydroxyl group; (a-2) it has a peak temperature of loss tangent (tan δ) attributable to the glass transition temperature of less than 0°C, as determined by measuring the temperature dependence of dynamic viscoelasticity (frequency 1 Hz, -100 to 200°C).

[0012] [3] The pressure-sensitive adhesive composition according to [1] or [2], wherein the unsaturated monomer in (b-2) is at least one unsaturated monomer selected from the group consisting of at least one unsaturated carboxylic acid monomer selected from the group consisting of unsaturated carboxylic acids having 3 to 10 carbon atoms, and their acid anhydrides and esters, and at least one unsaturated monomer selected from the group consisting of ethylenically unsaturated monomers having a hydroxyl group.

[0013] [4] The pressure-sensitive adhesive composition according to any one of [1] to [3], wherein in (b-2), the unsaturated monomer is an unsaturated alcohol.

[0014] [5] The pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the ethylene / α-olefin copolymer (B0) satisfies the following (b-1-1) to (b-1-5): (b-1-1) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (b-1-2) the molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less; (b-1-3) the kinematic viscosity at 100°C is 10 to 5,000 mm 2 (b-1-4) the content of ethylene units is 10 to 85 mol %; (b-1-5) no melting point is observed as measured by differential scanning calorimetry (DSC).

[0015] [6] The pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the graft-modified ethylene / α-olefin copolymer (B) further satisfies one or more of the following (b-3) to (b-7):

[0016] (b-3) the proportion of grafted portions is 0.1% by mass or more and less than 70% by mass (where the total amount of the main chain portion and the grafted portion is 100% by mass); (b-4) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (b-5) the molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less; (b-6) the kinematic viscosity at 100°C is 10 to 5,000 mm 2(b-7) No melting point is observed as measured by differential scanning calorimetry (DSC).

[0017] [7] The pressure-sensitive adhesive composition according to any one of [1] to [6], wherein, when the total of the content of the (meth)acrylic resin (A), the content of the graft-modified ethylene-α-olefin copolymer (B), and the content of the crosslinking agent (C) is taken as 100% by mass, the amount of the (meth)acrylic resin (A) is 47% by mass or more and 99% by mass, the amount of the graft-modified ethylene-α-olefin copolymer (B) is 0.5% by mass or more and 50% by mass or less, and the amount of the crosslinking agent (C) is 0.5% by mass or more and 5% by mass or less.

[0018] [8] A pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed from the pressure-sensitive adhesive composition according to any one of [1] to [7].

[0019] [9] A method for producing a pressure-sensitive adhesive composition, comprising the step of mixing a (meth)acrylic resin (A), a graft-modified ethylene / α-olefin copolymer (B) produced by the following method (α) or method (β) and satisfying the following requirements (b-1) to (b-2), and a crosslinking agent (C); (b-1) comprising a main chain portion derived from the ethylene / α-olefin copolymer; (b-2) comprising a graft portion derived from at least one unsaturated monomer containing a hetero atom; Method (α): A step (S1) of solution-polymerizing ethylene and an α-olefin in the presence of a catalyst system comprising a bridged metallocene compound (P) represented by the following (Formula 1), and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair, to obtain an ethylene / α-olefin copolymer (B0); a step (S2) of adding the unsaturated monomer to the ethylene / α-olefin copolymer (B0) and graft-copolymerizing the unsaturated monomer.

[0020] [In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R8 , R 9 and R 12 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group; R 7 and R 10 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group; R 6 and R 7 may bond with a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, and R 10 and R 11 may bond with a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, and R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time, 13 and R 14 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure; Y is a carbon atom or a silicon atom; M is Ti, Zr, or Hf; Q is independently a halogen atom, a hydrocarbon group, an anionic ligand, or a neutral ligand capable of coordinating to a lone electron pair; and j is an integer of 1 to 4.

[0021] Method (β): A method comprising: a step (S1′) of solution polymerizing ethylene and an α-olefin in the presence of a vanadium catalyst comprising a soluble vanadium compound (V) and an organoaluminum compound (Q′) to obtain an ethylene / α-olefin copolymer (B0); and a step (S2) of adding the unsaturated monomer to the ethylene / α-olefin copolymer (B0) to graft copolymerize it.

[0022]

[10] The substituent R of the bridged metallocene compound (P) represented by the formula (1) 13 and R 14 The method according to [9], wherein either one or both of the above is an aryl group.

[0023]

[11] The substituent R of the bridged metallocene compound (P) represented by the formula (1) 13 and R 14 are both aryl groups, and the substituent R 2 and R 3 wherein either one of the above is a saturated hydrocarbon group having 4 carbon atoms.

[0024] According to the present invention, it is possible to provide an adhesive composition having sufficient adhesiveness and excellent moisture resistance and low-temperature flexibility, and an adhesive sheet having an adhesive layer formed from the adhesive composition.

[0025] The present invention will now be described in further detail.

[0026] [Adhesive Composition] The adhesive composition according to the present invention contains a (meth)acrylic resin (A), a graft-modified ethylene / α-olefin copolymer (B) that satisfies specific requirements, and a crosslinking agent (C).

[0027] In this specification, "(meth)acrylic" means acrylic or methacrylic, "(meth)acrylate" means acrylate or methacrylate, and "(co)polymer" means a homopolymer or a copolymer.

[0028] [(Meth)acrylic Resin (A)] The (meth)acrylic resin (A) is a (co)polymer of an acrylic monomer or a methacrylic monomer. The acrylic monomer or methacrylic monomer constituting the (meth)acrylic resin (A) may be, for example, a monomer derived from a fossil fuel or a monomer derived from biomass.

[0029] The acrylic or methacrylic monomers constituting the (meth)acrylic resin (A) may be one type alone or two or more types in combination.

[0030] Here, the (meth)acrylic resin (A) preferably satisfies the following requirements (a-1) and (a-2).

[0031] Requirement (a-1): The (meth)acrylic resin (A) preferably contains a structural unit derived from a (meth)acrylate having an alkyl group having 1 to 12 carbon atoms and a structural unit derived from a (meth)acrylate containing a hydroxyl group.

[0032] Specifically, when the (meth)acrylic resin (A) contains a structural unit derived from a (meth)acrylate having an alkyl group with a small number of carbon atoms, for example, a structural unit derived from a (meth)acrylate having an alkyl group having from 1 to 12 carbon atoms, the glass transition temperature (Tg) of the (meth)acrylic resin (A) increases, and the adhesiveness of the pressure-sensitive adhesive composition is further enhanced. Here, the "structural unit derived from a (meth)acrylate having an alkyl group with from 1 to 12 carbon atoms" refers to a structural unit corresponding to a (meth)acrylate having an alkyl group with from 1 to 12 carbon atoms, and specifically, a structural unit represented by -[-CH2-CR'(-C(=O)-OR)-]- ... [A1] (R is an alkyl group having from 1 to 12 carbon atoms, and R' is a hydrogen atom or a methyl group).

[0033] From the above viewpoint, the (meth)acrylate having an alkyl group having from 1 to 12 carbon atoms is more preferably a (meth)acrylate having an alkyl group having from 1 to 10 carbon atoms, and even more preferably a (meth)acrylate having an alkyl group having from 2 to 8 carbon atoms. The alkyl group may be linear or branched.

[0034] Examples of the (meth)acrylate having an alkyl group having 1 to 12 carbon atoms include methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate.

[0035] The content of the structural units derived from the (meth)acrylate having an alkyl group having 1 to 12 carbon atoms in the (meth)acrylic resin (A) relative to the total amount of its structural units is preferably 50 mol % or more, more preferably 55 mol % or more, and even more preferably 60 mol % or more. The content is preferably 99 mol % or less, more preferably 95 mol % or less, and even more preferably 90 mol % or less.

[0036] Furthermore, when the (meth)acrylic resin (A) contains a structural unit derived from a (meth)acrylate containing a hydroxyl group, the number of crosslinking points by the crosslinking agent (C) increases, thereby increasing the crosslinking density of the pressure-sensitive adhesive composition and facilitating the formation of a high molecular weight. Such a pressure-sensitive adhesive composition has excellent mechanical strength of the pressure-sensitive adhesive layer and is less susceptible to deterioration in adhesiveness. Here, the "structural unit derived from a (meth)acrylate containing a hydroxyl group" refers to a structural unit corresponding to a (meth)acrylate containing a hydroxyl group.

[0037] Examples of the hydroxyl group-containing (meth)acrylate include hydroxyalkyl (meth)acrylates such as hydroxyethyl (meth)acrylate and hydroxypropyl (meth)acrylate, as well as hydroxyalkyl (meth)acrylamides such as N-methylol (meth)acrylamide, etc. Among these, from the above viewpoint, the hydroxyl group-containing (meth)acrylate is preferably hydroxyethyl (meth)acrylate.

[0038] That is, examples of "structural units derived from (meth)acrylates containing a hydroxyl group" include structural units derived from hydroxyalkyl (meth)acrylates and structural units derived from hydroxyalkyl (meth)acrylamides, and specific examples include a structural unit represented by: -[-CH2-CR'(-C(=O)-O-R-OH)-]- ... [A2a] (R is an alkanediyl group, preferably an ethane-1,2-diyl group or a propane-1,3-diyl group, more preferably an ethane-1,2-diyl group; R' is a hydrogen atom or a methyl group), as well as a structural unit represented by: -[-CH2-CR'(-C(=O)-NH-R-OH)-]- ... [A2b] (R is an alkanediyl group (for example, a methanediyl group); R' is a hydrogen atom or a methyl group). In one exemplary and preferred embodiment of the present invention, the "structural unit derived from a (meth)acrylate containing a hydroxyl group" is a structural unit represented by the above formula [A2a].

[0039] The content of the structural units derived from the hydroxyl group-containing (meth)acrylate in the (meth)acrylic resin (A) relative to the total amount of structural units is preferably 0.1 mol % or more, more preferably 0.2 mol % or more, and even more preferably 0.3 mol % or more, and is preferably 10 mol % or less, more preferably 5 mol % or less, and even more preferably 3 mol % or less.

[0040] The (meth)acrylic resin (A) may also be a copolymer having structural units derived from a monomer (or oligomer) having a functional group capable of forming crosslinks, which is different from the (meth)acrylate having an alkyl group with 1 to 12 carbon atoms or the (meth)acrylate containing a hydroxyl group. Examples of the monomer having a functional group capable of forming crosslinks include (meth)acrylic acid and (meth)acrylamide.

[0041] Furthermore, the (meth)acrylic resin (A) may be a copolymer having structural units derived from vinyl monomers other than those mentioned above, if necessary. Examples of such vinyl monomers include styrene and vinyl acetate.

[0042] The content of each structural unit in the (meth)acrylic resin (A) can be determined using an appropriate method, for example, by pyrolysis gas chromatography mass spectrometry (pyrolysis GC-MS) as shown in the following examples.

[0043] Requirement (a-2): The (meth)acrylic resin (A) preferably has a peak temperature of loss tangent (tan δ) attributable to the glass transition temperature, measured by measuring the temperature dependence of dynamic viscoelasticity (frequency 1 Hz, −100 to 200° C.), of less than 0° C.

[0044] Specifically, when the peak temperature of the loss tangent (tan δ) attributable to the glass transition temperature of the (meth)acrylic resin (A) determined by measuring the temperature dependency of dynamic viscoelasticity (at a frequency of 1 Hz, at −100 to 200° C.) is within a specific range, for example, less than 0° C., the pressure-sensitive adhesive composition formed into a thin film pressure-sensitive adhesive layer can exhibit adhesiveness over a wide temperature range.

[0045] From the above viewpoints, the (meth)acrylic resin (A) has a loss tangent (tan δ) peak temperature of more preferably −80° C. or higher, and even more preferably −70° C. or higher. The peak temperature is more preferably lower than 0° C., and even more preferably −5° C. or lower.

[0046] The peak temperature of the loss tangent (tan δ) of the (meth)acrylic resin (A) can be adjusted to fall within the above range by changing the monomers to be polymerized and their ratio.

[0047]

[0033] Method for Producing (Meth)acrylic Resin (A)

[0034] The (meth)acrylic resin (A) can be synthesized by a known polymerization method using monomers (or oligomers) that serve as materials for each of the structural units. The polymerization method is not particularly limited as long as it is a radical polymerization method, including bulk polymerization, solution polymerization, suspension polymerization, and the like. Among these, solution polymerization is preferred because it is easy to control the glass transition temperature (Tg) and other properties of the (meth)acrylic resin (A), and it is easy to synthesize a (meth)acrylic resin (A) with desired properties.

[0048] A polymerization initiator may be used during the polymerization. Examples of the polymerization initiator include dicumyl peroxide, benzoyl peroxide, tert-butylperoxy-2-ethylhexanoate, 1,1-bis(tert-butylperoxy)cyclohexane, α,α'-azobisisobutyronitrile, acetyl peroxide, tert-butyl peroxypivalate, tert-butyl hydroperoxide, cumene hydroperoxide, tert-hexyl peroxypivalate, 2,2'-azobis-(2,4-dimethylvaleronitrile), lauryl peroxide, tert-butyl peroxyneohexanoate, di-tert-butyl peroxide, azodicyclohexylcarbonitrile, dimethyl α,α-azodiisobutyrate, succinic acid peroxide, dicumene peroxide, and dichlorobenzoyl peroxide.

[0049] Examples of the solvent used in the solution polymerization include ethyl acetate, butyl acetate, benzene, toluene, xylene, cyclohexane, and methyl ethyl ketone.

[0050] [Graft-modified ethylene / α-olefin copolymer (B)] The graft-modified ethylene / α-olefin copolymer (B) satisfies the following requirements (b-1) and (b-2).

[0051] (b-1) Contains a main chain portion derived from the ethylene / α-olefin copolymer (B0).

[0052] (b-2) Contains a graft portion derived from at least one unsaturated monomer containing a hetero atom.

[0053] Here, the graft-modified ethylene / α-olefin copolymer (B) preferably satisfies one or more of the following requirements (b-3) to (b-7) in addition to the following requirements (b-1) and (b-2), more preferably satisfies two or more of them, and even more preferably satisfies all of them:

[0054] Requirement (b-1): The graft-modified ethylene / α-olefin copolymer (B) contains a main chain portion derived from the ethylene / α-olefin copolymer (B0).

[0055] Examples of the α-olefin constituting the ethylene / α-olefin copolymer (B0) include α-olefins other than ethylene. Typical examples include linear α-olefins having 3 to 20 carbon atoms, such as propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene; and branched α-olefins having 3 to 20 carbon atoms, such as 3-methyl-1-pentene, 4-methyl-1-pentene, 8-methyl-1-nonene, 7-methyl-1-decene, 6-methyl-1-undecene, and 6,8-dimethyl-1-decene. The ethylene / α-olefin copolymer (B0) may contain one or more of these α-olefins. Among these α-olefins, α-olefins having 3 to 10 carbon atoms are preferred, and propylene is particularly preferred, from the viewpoints of the effect of effectively reducing crystallinity to become liquid, improving flowability and flexibility, and the effect of improving compatibility between the ethylene / α-olefin copolymer and the (meth)acrylic resin (A).

[0056] Here, the ethylene / α-olefin copolymer (B0) preferably satisfies the following (b-1-1) to (b-1-5):

[0057] Requirement (b-1-1) From the viewpoint of reducing bleed-out, the ethylene / α-olefin copolymer (B0) used in the present invention preferably has a weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) of 1,500 to 30,000, more preferably 1,500 to 15,000, and even more preferably 1,500 to 8,500.

[0058] If the weight-average molecular weight (Mw) is less than the lower limit, particularly 1,500, the polymer contains low-molecular-weight components, which may cause bleeding out. On the other hand, if the weight-average molecular weight (Mw) is greater than the upper limit, particularly 30,000, the polymer may have poor compatibility with the (meth)acrylic resin (A), which may cause bleeding out.

[0059] Requirement (b-1-2) In order to reduce bleed-out, the ethylene / α-olefin copolymer (B0) used in the present invention preferably has a molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) of 2.5 or less, more preferably 2.2 or less, and even more preferably 2.0 or less.

[0060] If the molecular weight distribution (Mw / Mn) exceeds the upper limit, particularly 2.5, low molecular weight components and high molecular weight components with low compatibility may cause bleeding out.

[0061] Requirement (b-1-3): The ethylene / α-olefin copolymer (B0) used in the present invention has a kinematic viscosity at 100° C. of 10 to 5,000 mm 2 / s, and 15 to 3,500 mm 2 / s, and more preferably 20 to 2,500 mm 2 It is more preferable that the ratio is / s.

[0062] The kinematic viscosity at 100°C is the above-mentioned lower limit, particularly 10 mm 2 If the kinematic viscosity at 100°C is less than the upper limit, particularly 5,000 mm / s, the composition may contain high-flow components, which may cause bleeding out. 2 If the viscosity is greater than / s, the high viscosity component may reduce dispersibility in the (meth)acrylic resin (A), causing bleeding out.

[0063] Requirement (b-1-4) The ethylene / α-olefin copolymer (B0) used in the present invention preferably has an ethylene unit content of 10 to 85 mol %, more preferably 30 to 70 mol %, and even more preferably 40 to 60 mol %.

[0064] If the content of ethylene units is greater than the above upper limit or less than the above lower limit, particularly less than 10 mol% or more than 85 mol%, the crystallinity will be high and the compatibility with the (meth)acrylic resin (A) will be poor, which may cause bleed-out or deterioration of mechanical properties.

[0065] Requirement (b-1-5) The ethylene / α-olefin copolymer (B0) used in the present invention preferably does not exhibit a melting point as measured by differential scanning calorimetry (DSC). Here, "no melting point (Tm) is observed" means that the heat of fusion (ΔH) (unit: J / g) as measured by differential scanning calorimetry (DSC) is not substantially measured. "no heat of fusion (ΔH) is substantially not measured" means that no peak is observed in differential scanning calorimetry (DSC) measurement, or the observed heat of fusion is 1 J / g or less.

[0066] If no melting point is observed, this is preferred because it has the effect of improving flowability and improving the compatibility between the graft-modified ethylene / α-olefin copolymer (B) obtained from the ethylene / α-olefin copolymer (B0) and the (meth)acrylic resin (A), thereby imparting flexibility at low temperatures.

[0067] Method for Producing Ethylene / α-Olefin Copolymer (B0) The ethylene / α-olefin copolymer (B0) can be produced by using any known method without any restrictions.

[0068] For example, a method of copolymerizing ethylene and an α-olefin in the presence of a catalyst composed of a transition metal compound such as vanadium, zirconium, titanium, or hafnium, and an organoaluminum compound (organoaluminum oxy-compound) and / or an ionizing ionic compound can be mentioned. Metallocene catalysts using transition metal compounds such as zirconium, titanium, or hafnium are preferred because they reduce the amount of 2,1-bonds (inversion) between two or more consecutive propylene monomers, thereby improving the low-temperature properties of the curable resin composition. Such methods are described, for example, in WO 2000 / 34420, JP 62-121710 A, WO 2004 / 29062 A, JP 2004-175707 A, WO 2001 / 27124 A, and the like.

[0069] The ethylene and α-olefin, which are monomers constituting the ethylene-α-olefin copolymer (B0), may be, for example, fossil fuel-derived monomers or biomass-derived monomers, and these monomers may be used alone or in combination of two or more. In other words, the ethylene-α-olefin copolymer may be composed solely of fossil fuel-derived monomers, or may be composed solely of biomass-derived monomers, or may use a combination of fossil fuel-derived monomers and biomass-derived monomers.

[0070] Fossil fuels are oil, coal, natural gas, shale gas, or combinations thereof. Biomass is any renewable natural raw material and its residues, such as from plants or animals, including fungi, yeasts, algae, and bacteria.

[0071] The ethylene / α-olefin copolymer (B0) can be produced by copolymerizing ethylene and an α-olefin (for example, an α-olefin having 3 to 20 carbon atoms) in the presence of an olefin polymerization catalyst (hereinafter referred to as a "metallocene catalyst") containing a bridged metallocene compound (P) represented by the following formula (1), and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair:

[0072] The ethylene / α-olefin copolymer (B0) can also be produced by copolymerizing ethylene and an α-olefin (for example, an α-olefin having 3 to 20 carbon atoms) in the presence of a vanadium catalyst comprising a soluble vanadium compound (V) and an organoaluminum compound (Q').

[0073] [Metallocene Catalyst] In the present invention, a metallocene catalyst can be used as an olefin polymerization catalyst for obtaining the ethylene / α-olefin copolymer (B0). The metallocene catalyst that can be used to produce the ethylene / α-olefin copolymer (B0) contains a bridged metallocene compound (P) represented by the following formula (1), and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.

[0074] <Bridged Metallocene Compound (P)>

[0075] Y, M, and R in Formula 1 1 ~R 14 , Q and j are explained below.

[0076] <<Y>> Y is a carbon atom or a silicon atom, preferably a carbon atom.

[0077] <<M>> M is a titanium atom, a zirconium atom, or a hafnium atom (Ti, Zr, or Hf), and is preferably a zirconium atom (Zr).

[0078] 《R 1 ~R 14 》R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 are each independently an atom or a substituent selected from the group consisting of a hydrogen atom, a hydrocarbon group, and a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure.

[0079] Examples of the hydrocarbon group include an alkyl group having 1 to 20 carbon atoms, a cyclic saturated hydrocarbon group having 3 to 20 carbon atoms, a chain unsaturated hydrocarbon group having 2 to 20 carbon atoms, a cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms, an alkylene group having 1 to 20 carbon atoms, and an arylene group having 6 to 20 carbon atoms.

[0080] Examples of alkyl groups having 1 to 20 carbon atoms include linear saturated hydrocarbon groups such as methyl, ethyl, n-propyl, n-butyl, n-pentyl, n-hexyl, n-heptyl, n-octyl, n-nonyl, and n-decanyl, and branched saturated hydrocarbon groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, tert-amyl, neopentyl, 3-methylpentyl, 1,1-diethylpropyl, 1,1-dimethylbutyl, 1-methyl-1-propylbutyl, 1,1-dipropylbutyl, 1,1-dimethyl-2-methylpropyl, 1-methyl-1-isopropyl-2-methylpropyl, and cyclopropylmethyl. The number of carbon atoms in the alkyl group is preferably 1 to 6.

[0081] Examples of cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic saturated hydrocarbon groups such as cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, norbornyl, 1-adamantyl, and 2-adamantyl, and groups in which a hydrogen atom of a cyclic saturated hydrocarbon group is replaced with a hydrocarbon group having 1 to 17 carbon atoms such as 3-methylcyclopentyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 4-cyclohexylcyclohexyl, and 4-phenylcyclohexyl. The number of carbon atoms in the cyclic saturated hydrocarbon group is preferably 5 to 11.

[0082] Examples of linear unsaturated hydrocarbon groups having 2 to 20 carbon atoms include alkenyl groups such as ethenyl (vinyl), 1-propenyl, 2-propenyl (allyl), and 1-methylethenyl (isopropenyl), and alkynyl groups such as ethynyl, 1-propynyl, and 2-propynyl (propargyl). The linear unsaturated hydrocarbon group preferably has 2 to 4 carbon atoms.

[0083] Examples of cyclic unsaturated hydrocarbon groups having 3 to 20 carbon atoms include cyclic unsaturated hydrocarbon groups such as cyclopentadienyl, norbornenyl, phenyl, naphthyl, indenyl, azulenyl, phenanthryl, and anthracenyl; groups in which hydrogen atoms of cyclic unsaturated hydrocarbon groups are replaced with hydrocarbon groups having 1 to 15 carbon atoms, such as 3-methylphenyl (m-tolyl), 4-methylphenyl (p-tolyl), 4-ethylphenyl, 4-tert-butylphenyl, 4-cyclohexylphenyl, biphenylyl, 3,4-dimethylphenyl, 3,5-dimethylphenyl, and 2,4,6-trimethylphenyl (mesityl); and groups in which hydrogen atoms of linear or branched saturated hydrocarbon groups are replaced with cyclic saturated or unsaturated hydrocarbon groups having 3 to 19 carbon atoms, such as benzyl and cumyl. The number of carbon atoms in the cyclic unsaturated hydrocarbon group is preferably 6 to 10.

[0084] Examples of alkylene groups having 1 to 20 carbon atoms include methylene, ethylene, dimethylmethylene (isopropylidene), ethylmethylene, methylethylene, n-propylene, etc. The alkylene group preferably has 1 to 6 carbon atoms.

[0085] Examples of the arylene group having 6 to 20 carbon atoms include an o-phenylene group, an m-phenylene group, a p-phenylene group, a 4,4'-biphenylylene group, etc. The arylene group preferably has 6 to 12 carbon atoms.

[0086] Examples of silicon-containing hydrocarbon groups include alkylsilyl groups such as trimethylsilyl, triethylsilyl, tert-butyldimethylsilyl, and triisopropylsilyl, which are groups in which carbon atoms in the above-mentioned hydrocarbon groups are replaced with silicon atoms, arylsilyl groups such as dimethylphenylsilyl, methyldiphenylsilyl, and tert-butyldiphenylsilyl, pentamethyldisilanyl, and trimethylsilylmethyl. The alkylsilyl group preferably has 1 to 10 carbon atoms, and the arylsilyl group preferably has 6 to 18 carbon atoms.

[0087] In the present invention, R 2 and R 3 In this case, it is preferable that either one of R is a saturated hydrocarbon group having 4 carbon atoms. 1 ~R 4 All of the carbon atoms other than the saturated hydrocarbon group may be hydrogen atoms, or R 1 ~R 4 In the formula (I), the two groups adjacent to the saturated hydrocarbon group having 4 carbon atoms may be hydrogen atoms, and the group not adjacent to the saturated hydrocarbon group may be a methyl group. 2 and R 3 This does not preclude embodiments in which none of the above groups is a saturated hydrocarbon group having 4 carbon atoms, and for example, R 1 ~R 4 may all be hydrogen atoms.

[0088] R 6 and R 11are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and the details of the hydrocarbon group and the silicon-containing hydrocarbon group are as described above.

[0089] R 7 and R 10 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and the details of the hydrocarbon group and the silicon-containing hydrocarbon group are as described above.

[0090] R 6 and R 7 may bond with a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, and R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure.

[0091] R 6 , R 7 , R 10 and R 11 is not a hydrogen atom at the same time.

[0092] R 13 and R 14 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and may be linked together to form a ring structure.

[0093] The hydrocarbon group and silicon-containing hydrocarbon group are as described above in detail, and the hydrocarbon group further includes an aryl group and a substituted aryl group.

[0094] Examples of aryl groups partially overlap with the examples of the cyclic unsaturated hydrocarbon groups having 3 to 20 carbon atoms described above, but include substituents derived from aromatic compounds, such as phenyl, 1-naphthyl, 2-naphthyl, anthracenyl, phenanthrenyl, tetracenyl, chrysenyl, pyrenyl, indenyl, azulenyl, pyrrolyl, pyridyl, furanyl, and thiophenyl groups. As the aryl group, a phenyl or 2-naphthyl group is preferred.

[0095] Examples of the aromatic compounds include aromatic hydrocarbons and heterocyclic aromatic compounds such as benzene, naphthalene, anthracene, phenanthrene, tetracene, chrysene, pyrene, indene, azulene, pyrrole, pyridine, furan, and thiophene.

[0096] The substituted aryl group partially overlaps with the examples of the cyclic unsaturated hydrocarbon group having 3 to 20 carbon atoms described above, but includes groups in which one or more hydrogen atoms of the aryl group are substituted with at least one substituent selected from the group consisting of hydrocarbon groups having 1 to 20 carbon atoms, aryl groups, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms, and halogen-containing groups. Specific examples include 3-methylphenyl group (m-tolyl group), 4-methylphenyl group (p-tolyl group), 3-ethylphenyl group, 4-ethylphenyl group, 3,4-dimethylphenyl group, 3,5-dimethylphenyl group, biphenylyl group, 4-(trimethylsilyl)phenyl group, 4-a-tolyl ... Examples of the aryl group include an aminophenyl group, a 4-(dimethylamino)phenyl group, a 4-(diethylamino)phenyl group, a 4-morpholinylphenyl group, a 4-methoxyphenyl group, a 4-ethoxyphenyl group, a 4-phenoxyphenyl group, a 3,4-dimethoxyphenyl group, a 3,5-dimethoxyphenyl group, a 3-methyl-4-methoxyphenyl group, a 3,5-dimethyl-4-methoxyphenyl group, a 3-(trifluoromethyl)phenyl group, a 4-(trifluoromethyl)phenyl group, a 3-chlorophenyl group, a 4-chlorophenyl group, a 3-fluorophenyl group, a 4-fluorophenyl group, a 5-methylnaphthyl group, and a 2-(6-methyl)pyridyl group.

[0097] In the present invention, R 13 and R 14 In one preferred embodiment of the present invention, it is preferable that either one or both of R 13 and R 14 are both aryl groups. 13 and R 14 It is not prohibited that one of R 13 is an aryl group, and R 14may be an alkyl group having 1 to 20 carbon atoms.

[0098] Q may be the same or different and may be selected from a halogen atom, a hydrocarbon group, an anionic ligand, and a neutral ligand capable of coordinating with a lone electron pair.

[0099] Examples of halogen atoms include fluorine, chlorine, bromine and iodine atoms, with chlorine being preferred.

[0100] The hydrocarbon group may, for example, be a hydrocarbon group having 1 to 20 carbon atoms. Details of the hydrocarbon group are as described above, and the hydrocarbon group preferably has 1 to 7 carbon atoms.

[0101] Examples of the anionic ligand include alkoxy groups such as methoxy, tert-butoxy, and phenoxy groups, carboxylate groups such as acetate and benzoate, and sulfonate groups such as mesylate and tosylate.

[0102] Examples of neutral ligands capable of coordinating with lone electron pairs include organic phosphorus compounds such as trimethylphosphine, triethylphosphine, triphenylphosphine, and diphenylmethylphosphine, and ether compounds such as tetrahydrofuran, diethyl ether, dioxane, and 1,2-dimethoxyethane.

[0103] <<j>> j is an integer of 1 to 4, preferably 2.

[0104] (Examples of Bridged Metallocene Compound (P)) The bridged metallocene compound (P) is a compound represented by the formula (1) above, where R 13 and R 14 and wherein either or both of the following are aryl groups:

[0105] Preferable examples of the bridged metallocene compound (P1) include those represented by the formula (1) above, where R 13 and R 14 are both aryl groups, and R 2 and R 3and R are each a saturated hydrocarbon group having 4 carbon atoms. 1 ~R 4 a bridged metallocene compound in which all atoms other than the saturated hydrocarbon group having 4 carbon atoms are hydrogen atoms, and R 1 ~R 4 Among these, a bridged metallocene compound in which two groups adjacent to the saturated hydrocarbon group having 4 carbon atoms are hydrogen atoms and the group not adjacent to the saturated hydrocarbon group is a methyl group can be mentioned.

[0106] Another preferred example of the bridged metallocene compound (P1) is, for example, R 13 and R 14 and only one of R is an aryl group, and 1 ~R 4 and a bridged metallocene compound (P3) in which all of the

[0107] Specific examples of the bridged metallocene compound (P) include [dimethylmethylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [dimethylmethylene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [dimethylmethylene (η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dimethylmethylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [cyclohexylidene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [cyclohexylidene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [cyclohexylidene (η5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [cyclohexylidene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -2-methyl-4-tert-butylcyclopentadienyl)(η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene{η 5 -(2-methyl-4-i-propylcyclopentadienyl)}(η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylmethylene (η 5 -3-n-butylcyclopentadienyl)(η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene (η 5 -cyclopentadienyl) (η 5-3,6-di-tert-butylfluorenyl)]zirconium dichloride, [methylphenylmethylene (η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methylphenylmethylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(3-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [methyl(4-methylphenyl)methylene(η 5 -cyclopentadienyl) (η 5-tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylsilylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [diphenylsilylene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [diphenylsilylene (η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [diphenylsilylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [bis(3-methylphenyl)silylene(η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dicyclohexylsilylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [dicyclohexylsilylene (η 5 -cyclopentadienyl) (η5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [dicyclohexylsilylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, [ethylene (η 5 -cyclopentadienyl) (η 5 -2,7-di-tert-butylfluorenyl)]zirconium dichloride, [ethylene (η 5 -cyclopentadienyl) (η 5 -3,6-di-tert-butylfluorenyl)]zirconium dichloride, [ethylene (η 5 -cyclopentadienyl) (η 5 -octamethyloctahydrodibenzofluorenyl)]zirconium dichloride, [ethylene (η 5 -cyclopentadienyl) (η 5 -tetramethyloctahydrodibenzofluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, ethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5-(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, diphenylmethylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5-(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butyl-5-methylcyclopentadienyl)][η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-tert-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η5 -(3-tert-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-diphenyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-tert-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(3,6-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)] [η 5 -(2,7-di-tert-butylfluorenyl)]zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octamethyloctahydrodibenzfluorenyl)zirconium dichloride, di(p-tolyl)methylene[η 5 -(3-n-butylcyclopentadienyl)](benzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](dibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](octahydrodibenzofluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5 -(3-n-butylcyclopentadienyl)](2,7-diphenyl-3,6-di-tert-butylfluorenyl)zirconium dichloride, di(p-tolyl)methylene [η 5-(3-n-butylcyclopentadienyl)] [η 5 -(2,7-dimethyl-3,6-di-tert-butylfluorenyl)]zirconium dichloride.

[0108] Further examples of the bridged metallocene compound (P) include compounds in which the zirconium atom of the above-mentioned compound is replaced with a hafnium atom or a titanium atom, and compounds in which the chloro ligand is replaced with a methyl group. 5 -Tetramethyloctahydrodibenzofluorenyl is 4,4,7,7-tetramethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, η 5 -Octamethyloctahydrodibenzofluorenyl is 1,1,4,4,7,7,10,10-octamethyl-(5a,5b,11a,12,12a-η 5 )-1,2,3,4,7,8,9,10-octahydrodibenzo[b,H]fluorenyl group, respectively.

[0109] The bridged metallocene compounds (P) may be used singly or in combination of two or more.

[0110] <Compound (Q)> The compound (Q) is at least one compound selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair.

[0111] Specific examples of the organometallic compound (Q-1) include the following organometallic compounds (Q-1a), (Q-1b), and (Q-1c) of Group 1, 2, 12, and 13 of the periodic table.

[0112] (Q-1a) Formula R a m Al (OR b ) n H p X q An organoaluminum compound represented by the formula: a and R bmay be the same or different and represent a hydrocarbon group having 1 to 15, preferably 1 to 4, carbon atoms; X represents a halogen atom; m is a number that satisfies 0<m≦3, n is a number that satisfies 0≦n<3, p is a number that satisfies 0≦p<3, and q is a number that satisfies 0≦q<3, and m+n+p+q=3.) Examples of such compounds include: tri-n-alkylaluminums such as trimethylaluminum, triethylaluminum, tri-n-butylaluminum, tri-n-hexylaluminum, and tri-n-octylaluminum; tri-branched alkylaluminums such as triisopropylaluminum, triisobutylaluminum, tri-sec-butylaluminum, tri-tert-butylaluminum, tri-2-methylbutylaluminum, tri-3-methylhexylaluminum, and tri-2-ethylhexylaluminum; tricycloalkylaluminums such as tricyclohexylaluminum and tricyclooctylaluminum; triarylaluminums such as triphenylaluminum and tri(4-methylphenyl)aluminum; x Al y (C5H 10 ) z (wherein x, y, and z are positive numbers, and z≦2x), alkylaluminum alkoxides such as isobutylaluminum methoxide and isobutylaluminum ethoxide, dialkylaluminum alkoxides such as dimethylaluminum methoxide, diethylaluminum ethoxide and dibutylaluminum butoxide, alkylaluminum sesquialkoxides such as ethylaluminum sesquiethoxide and butylaluminum sesquibut ... represented by the formula R a 2.5 Al (OR b ) 0.5partially alkoxylated alkylaluminums having an average composition represented by the formula (I) or (II), alkylaluminum aryloxides such as diethylaluminum phenoxide and diethylaluminum (2,6-di-tert-butyl-4-methylphenoxide), dialkylaluminum halides such as dimethylaluminum chloride, diethylaluminum chloride, dibutylaluminum chloride, diethylaluminum bromide and diisobutylaluminum chloride, alkylaluminum sesquihalides such as ethylaluminum sesquichloride, butylaluminum sesquichloride and ethylaluminum sesquibromide, partially halogenated alkylaluminums such as alkylaluminum dihalides such as ethylaluminum dichloride, dialkylaluminum hydrides such as diethylaluminum hydride, diisopropylaluminum hydride, dibutylaluminum hydride and diisobutylaluminum hydride, alkylaluminum dihydrides such as ethylaluminum dihydride and propylaluminum dihydride and other partially hydrogenated alkylaluminums, Examples include partially alkoxylated and halogenated alkylaluminums such as ethylaluminum ethoxychloride, butylaluminum butoxychloride, and ethylaluminum ethoxybromide. a m Al (OR b ) n H p X q Compounds similar to the compound represented by the formula (1) can also be used, such as organoaluminum compounds in which two or more aluminum compounds are bonded via nitrogen atoms, such as (C2H5)2AlN(C2H5)Al(C2H5)2.

[0113] (Q-1b) Formula M 2 AlR a 4 (wherein M 2 represents Li, Na or K, and R arepresents a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms.) Examples of such compounds include LiAl(C2H5)4, LiAl(C7H 15 ) 4 can be given as an example.

[0114] (Q-1c) Formula R a R b M 3 A dialkyl compound of a metal of Group 2 or 12 of the periodic table, represented by the formula: a and R b may be the same or different and represent a hydrocarbon group having 1 to 15 carbon atoms, preferably 1 to 4 carbon atoms; M 3 is Mg, Zn, or Cd.) As the organoaluminum oxy compound (Q-2), a conventionally known aluminoxane can be used as it is. Specific examples include compounds represented by the following formula [III] and compounds represented by the following formula [IV]:

[0115] In formulas [III] and [IV], R represents a hydrocarbon group having 1 to 10 carbon atoms, and n represents an integer of 2 or more.

[0116] In particular, methylaluminoxanes in which R is a methyl group and n is 3 or more, preferably 10 or more, are used. There is no problem if these aluminoxanes contain a small amount of an organoaluminum compound.

[0117] In the present invention, when copolymerization of ethylene with an α-olefin having 3 or more carbon atoms is carried out at a high temperature, benzene-insoluble organoaluminum oxy compounds such as those exemplified in JP-A No. 2-78687 can also be used. Also suitable are the organoaluminum oxy compounds described in JP-A No. 2-167305 and the aluminoxanes having two or more alkyl groups described in JP-A Nos. 2-24701 and 3-103407. The "benzene-insoluble organoaluminum oxy compounds" that may be used in the present invention are compounds that are insoluble or poorly soluble in benzene, and in which the Al component dissolved in benzene at 60°C is typically 10% or less, preferably 5% or less, and particularly preferably 2% or less, calculated as Al atoms.

[0118] Further, examples of the organoaluminum oxy compound (Q-2) include modified methylaluminoxanes represented by the following formula [V].

[0119] In formula [V], Rx represents a hydrocarbon group having 1 to 10 carbon atoms, and m and n each independently represent an integer of 2 or more.

[0120] Methylaluminoxane, an example of organoaluminum oxy compound (Q-2), is commonly used as an activator in polyolefin polymerization because it is readily available and has high polymerization activity. However, methylaluminoxane is difficult to dissolve in saturated hydrocarbons, and therefore has been used as a solution in environmentally undesirable aromatic hydrocarbons such as toluene or benzene. For this reason, flexible bodies of methylaluminoxane represented by formula [V] have been developed and used in recent years as aluminoxanes dissolved in saturated hydrocarbons. This modified methylaluminoxane represented by formula [V] can be prepared using trimethylaluminum and alkylaluminums other than trimethylaluminum, such as trimethylaluminum and triisobutylaluminum, as shown, for example, in U.S. Pat. Nos. 4,960,878 and 5,041,584. Aluminoxanes in which Rx is an isobutyl group are commercially available in the form of saturated hydrocarbon solutions under the trade names MMAO and TMAO (see Tosoh Finechem Corporation, Tosoh Research & Technology Review, Vol. 47, 55 (2003)).

[0121] Further, the organoaluminum oxy compound (Q-2) may also include a boron-containing organoaluminum oxy compound represented by the following formula [VI]:

[0122] In formula [VI], R c represents a hydrocarbon group having 1 to 10 carbon atoms. d may be the same or different and represent a hydrogen atom, a halogen atom or a hydrocarbon group having 1 to 10 carbon atoms.

[0123] Examples of the compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair (hereinafter, sometimes abbreviated as "ionized ionic compound" or simply "ionic compound") include Lewis acids, ionic compounds, borane compounds, and carborane compounds described in JP-A-1-501950, JP-A-1-502036, JP-A-3-179005, JP-A-3-179006, JP-A-3-207703, JP-A-3-207704, U.S. Pat. No. 5,321,106, and the like. Further examples include heteropoly compounds and isopoly compounds.

[0124] The ionizing ionic compound preferably used in the present invention is a boron compound represented by the following formula [VII]:

[0125] In formula [VII], R e+ As for H + , carbenium cation, oxonium cation, ammonium cation, phosphonium cation, cycloheptyltrienyl cation, ferrocenium cation having a transition metal, etc. f ~R i may be the same or different and are substituents selected from the group consisting of hydrocarbon groups having 1 to 20 carbon atoms, silicon-containing groups, nitrogen-containing groups, oxygen-containing groups, halogen atoms and halogen-containing groups, and are preferably substituted aryl groups.

[0126] Specific examples of the carbenium cation include trisubstituted carbenium cations such as triphenylcarbenium cation, tris(4-methylphenyl)carbenium cation, and tris(3,5-dimethylphenyl)carbenium cation.

[0127] Specific examples of the ammonium cation include trialkyl-substituted ammonium cations such as trimethylammonium cation, triethylammonium cation, tri(n-propyl)ammonium cation, triisopropylammonium cation, tri(n-butyl)ammonium cation, and triisobutylammonium cation; N,N-dialkylanilinium cations such as N,N-dimethylanilinium cation, N,N-diethylanilinium cation, and N,N-2,4,6-pentamethylanilinium cation; and dialkylammonium cations such as diisopropylammonium cation and dicyclohexylammonium cation.

[0128] Specific examples of the phosphonium cation include triarylphosphonium cations such as triphenylphosphonium cation, tris(4-methylphenyl)phosphonium cation, and tris(3,5-dimethylphenyl)phosphonium cation.

[0129] R e+ Of the above specific examples, carbenium cations and ammonium cations are preferred, with triphenylcarbenium cation, N,N-dimethylanilinium cation and N,N-diethylanilinium cation being particularly preferred.

[0130] Among the ionizable ionic compounds preferably used in the present invention, examples of compounds containing a carbenium cation include triphenylcarbenium tetraphenylborate, triphenylcarbenium tetrakis(pentafluorophenyl)borate, triphenylcarbenium tetrakis{3,5-di-(trifluoromethyl)phenyl}borate, tris(4-methylphenyl)carbenium tetrakis(pentafluorophenyl)borate, and tris(3,5-dimethylphenyl)carbenium tetrakis(pentafluorophenyl)borate.

[0131] Among the ionizing ionic compounds preferably used in the present invention, compounds containing a trialkyl-substituted ammonium cation include triethylammonium tetraphenylborate, tripropylammonium tetraphenylborate, tri(n-butyl)ammonium tetraphenylborate, trimethylammonium tetrakis(4-methylphenyl)borate, trimethylammonium tetrakis(2-methylphenyl)borate, tri(n-butyl)ammonium tetrakis(pentafluorophenyl)borate, triethylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(pentafluorophenyl)borate, tripropylammonium tetrakis(2,4-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis(3,5-dimethylphenyl)borate, tri(n-butyl)ammonium tetrakis{4-(trifluorophenyl)borate}. Examples of the tetrakis include dioctadecylmethylammonium tetrakis(4-methylphenyl)borate, dioctadecylmethylammonium tetrakis(pentafluorophenyl)borate, dioctadecylmethylammonium tetrakis(2,4-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(3,5-dimethylphenyl)borate, dioctadecylmethylammonium tetrakis(4-(trifluoromethyl)phenyl)borate, dioctadecylmethylammonium tetrakis(3,5-di(trifluoromethyl)phenyl)borate, and dioctadecylmethylammonium.

[0132] Among the ionizable ionic compounds preferably used in the present invention, examples of compounds containing an N,N-dialkylanilinium cation include N,N-dimethylanilinium tetraphenylborate, N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate, N,N-dimethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-diethylanilinium tetraphenylborate, N,N-diethylanilinium tetrakis(pentafluorophenyl)borate, N,N-diethylanilinium tetrakis{3,5-di(trifluoromethyl)phenyl}borate, N,N-2,4,6-pentamethylanilinium tetraphenylborate, and N,N-2,4,6-pentamethylanilinium tetrakis(pentafluorophenyl)borate.

[0133] Among the ionizable ionic compounds preferably used in the present invention, examples of compounds containing a dialkylammonium cation include di-n-propylammonium tetrakis(pentafluorophenyl)borate and dicyclohexylammonium tetraphenylborate.

[0134] In addition, the ionic compounds exemplified in JP-A-2004-51676 can also be used without any restrictions.

[0135] The ionic compound (Q-3) may be used alone or in combination of two or more.

[0136] <Configuration Examples of Metallocene Catalyst> Examples of the configuration of the metallocene catalyst system include the following [1] to [4].

[0137] [1] Comprising a bridged metallocene compound (P) and a compound (Q-2). [2] Comprising a bridged metallocene compound (P), a compound (Q-1), and a compound (Q-2). [3] Comprising a bridged metallocene compound (P), a compound (Q-1), and a compound (Q-3). [4] Comprising a bridged metallocene compound (P), a compound (Q-2), and a compound (Q-3). The bridged metallocene compound (P) and the compounds (Q-1) to (Q-3) may be introduced into the reaction system in any order.

[0138] <Support (R)> The olefin polymerization catalyst containing the bridged metallocene compound (P) and the compound (Q) may further contain a support (R).

[0139] The carrier (R) that may be used in the present invention is an inorganic or organic compound, and is a granular or fine particle solid. Among these, the inorganic compound is preferably a porous oxide, an inorganic chloride, a clay, a clay mineral, or an ion-exchangeable layered compound.

[0140] Specific examples of porous oxides that can be used include SiO2, Al2O3, MgO, ZrO, TiO2, BO3, CaO, ZnO, BaO, and ThO2, as well as composites or mixtures containing these, such as natural or synthetic zeolites, SiO2-MgO, SiO2-Al2O3, SiO2-TiO2, SiO2-VO5, SiO2-Cr2O3, and SiO2-TiO2-MgO. Of these, those containing SiO2 and / or Al2O3 as the main component are preferred. While the properties of such porous oxides vary depending on the type and production method, the carriers preferably used in the present invention have a particle size of 0.5 to 300 μm, preferably 1.0 to 200 μm, and a specific surface area of ​​50 to 1,000 m. 2 / g, preferably 100 to 700 m 2 / g, and the pore volume is in the range of 0.3 to 3.0 cm 3 Such a support is calcined at 100 to 1000°C, preferably 150 to 700°C, if necessary, before use.

[0141] Examples of inorganic chlorides that can be used include MgCl, MgBr, MnCl, and MnBr. The inorganic chlorides may be used as they are or may be pulverized using a ball mill or a vibration mill. Alternatively, the inorganic chlorides may be dissolved in a solvent such as alcohol and then precipitated into fine particles using a precipitating agent.

[0142] Clay is usually composed mainly of clay minerals. Ion-exchangeable layered compounds are compounds with a crystalline structure in which the constituent planes are stacked parallel to each other with weak bonding forces due to ionic bonds or the like, and the ions contained therein are exchangeable. Most clay minerals are ion-exchangeable layered compounds. These clays, clay minerals, and ion-exchangeable layered compounds are not limited to natural products, and artificial synthetic products can also be used. Examples of clays, clay minerals, and ion-exchangeable layered compounds include clays, clay minerals, and ionic crystalline compounds having layered crystalline structures such as hexagonal close packing type, antimony type, CdCl type, and CdI type. Examples of such clays and clay minerals include kaolin, bentonite, kibushi clay, gairome clay, allophane, hisingerite, pyrophyllite, ummo group, montmorillonite group, vermiculite, ryokudeite group, palygorskite, kaolinite, nacrite, dickite, and halloysite. Examples of ion-exchange layered compounds include crystalline acid salts of polyvalent metals such as α-Zr(HAsO)H0, α-Zr(HPO), α-Zr(KPO3H0, α-Ti(HPO), α-Ti(HAsO)H0, α-Sn(HPO), H0, γ-Zr(HPO), γ-Ti(HPO), and γ-Ti(NHPO). It is also preferable to subject the clay and clay minerals used in the present invention to chemical treatment. Examples of chemical treatment include surface treatment to remove impurities adhering to the surface and treatment to affect the crystalline structure of the clay. Specific examples of chemical treatment include acid treatment, alkali treatment, salt treatment, and organic treatment.

[0143] The ion-exchangeable layered compound may be a layered compound in which the interlayer spacing is expanded by utilizing the ion exchange property and exchanging the exchangeable ions between the layers with other large, bulky ions. Such bulky ions act as supports supporting the layered structure and are usually called pillars. The introduction of another substance (guest compound) between the layers of a layered compound is called intercalation. Examples of guest compounds include cationic inorganic compounds such as TiCl4 and ZrCl4, metal alkoxides such as Ti(OR)4, Zr(OR)4, PO(OR)3, and B(OR)3 (where R is a hydrocarbon group, etc.), and [Al 13 O4 (OH) 24 ] 7+ , [Zr(OH) 14 ] 2+ , [Fe3O(OCOCH3)6] + Examples of the metal hydroxide ions include those mentioned above. These compounds can be used singly or in combination of two or more. When intercalating these compounds, polymers obtained by hydrolysis and polycondensation of metal alkoxides (R is a hydrocarbon group, for example) such as Si(OR)4, Al(OR)3, and Ge(OR)4, colloidal inorganic compounds such as SiO2, and the like can also be present. Examples of the pillars include oxides produced by intercalating the metal hydroxide ions between layers and then dehydrating them with heat.

[0144] Of these, clay or clay minerals are preferred, and montmorillonite, vermiculite, pectolite, taeniolite and synthetic mica are particularly preferred.

[0145] Examples of organic compounds usable as the carrier (R) include granular or particulate solids having a particle size in the range of 0.5 to 300 μm. Specific examples include (co)polymers produced mainly from an α-olefin having 2 to 14 carbon atoms, such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, or (co)polymers produced mainly from vinylcyclohexane and styrene, and modified products thereof.

[0146] <Conditions for polymerization using metallocene catalyst> The method of use and order of addition of each component of the polymerization catalyst (the metallocene catalyst) may be selected arbitrarily. At least two or more of the components in the catalyst may be contacted in advance.

[0147] The bridged metallocene compound (P) (hereinafter also referred to as "component (P)") is usually used in an amount of 1 x 10 per liter of reaction volume. -9 ~1 x 10 -1 mol, preferably 1×10 -8 ~1 x 10 -2 It is used in an amount that will give a mol.

[0148] The organometallic compound (Q-1) (hereinafter also referred to as "component (Q-1)") is used in an amount such that the molar ratio of component (Q-1) to the transition metal atom (M) in component (P) [(Q-1) / M] is generally 0.01 to 50,000, preferably 0.05 to 10,000.

[0149] The organoaluminum oxy compound (Q-2) (hereinafter also referred to as "component (Q-2)") is used in an amount such that the molar ratio of aluminum atoms in component (Q-2) to transition metal atoms (M) in component (P) [(Q-2) / M] is generally 10 to 5,000, preferably 20 to 2,000.

[0150] The ionic compound (Q-3) (hereinafter also referred to as "component (Q-3)") is used in an amount such that the molar ratio of component (Q-3) to the transition metal atom (M) in component (P) [(Q-3) / M] is generally 1 to 10,000, preferably 1 to 5,000.

[0151] The polymerization temperature is usually -50°C to 300°C, preferably 30 to 250°C, more preferably 100°C to 250°C, and even more preferably 130°C to 200°C. Within this polymerization temperature range, as the temperature increases, the solution viscosity during polymerization decreases and the heat of polymerization is easily removed. The polymerization pressure is usually atmospheric pressure to 10 MPa gauge pressure (MPa-G), preferably atmospheric pressure to 8 MPa-G.

[0152] The polymerization reaction can be carried out batchwise, semi-continuously or continuously. Furthermore, the polymerization can be carried out continuously in two or more polymerization vessels with different reaction conditions.

[0153] The molecular weight of the resulting copolymer can be adjusted by changing the hydrogen concentration in the polymerization system or the polymerization temperature. Furthermore, it can also be adjusted by the amount of compound (Q) used. When hydrogen is added, the amount is suitably about 0.001 to 5,000 NL per kg of the resulting copolymer.

[0154] The polymerization solvent used in the liquid-phase polymerization method is usually an inert hydrocarbon solvent, preferably a saturated hydrocarbon having a boiling point of 50°C to 200°C under normal pressure. Specific examples of the polymerization solvent include aliphatic hydrocarbons such as propane, butane, pentane, hexane, heptane, octane, decane, dodecane, and kerosene, and alicyclic hydrocarbons such as cyclopentane, cyclohexane, and methylcyclopentane, with hexane, heptane, octane, decane, and cyclohexane being particularly preferred. The α-olefin to be polymerized itself can also be used as the polymerization solvent. Aromatic hydrocarbons such as benzene, toluene, and xylene, and halogenated hydrocarbons such as ethylene chloride, chlorobenzene, and dichloromethane can also be used as the polymerization solvent, but their use is not preferred from the standpoints of reducing the burden on the environment and minimizing the impact on human health.

[0155] [Vanadium-Based Catalyst] In the present invention, a vanadium-based catalyst can also be used as an olefin polymerization catalyst for obtaining the ethylene / α-olefin copolymer (B0). The vanadium-based catalyst that can be used to produce the ethylene / α-olefin copolymer (B0) comprises a soluble vanadium compound (V) and an organoaluminum compound (Q').

[0156] <Soluble Vanadium Compound (V)> The soluble vanadium compound (V) constituting the vanadium catalyst that can be used in the present invention is specifically represented by the following general formula.

[0157] VO(OR) a Xb or V(OR) c X d In the formula, R represents a hydrocarbon group such as an alkyl group, a cycloalkyl group, or an aryl group, X represents a halogen atom, and a, b, c, and d respectively satisfy the following conditions: 0≦a≦3, 0≦b≦3, 2≦a+b≦3, 0≦c≦4, 0≦d≦4, and 3≦c+d≦4.

[0158] Specific examples of the soluble vanadium compound (V) represented by the above general formula include VOCl3, VO(OCH3)Cl2, VO(OC2H5)Cl2, and VO(OC2H5). 1.5 C1 1.5 , VO(OC2H5)2Cl, VO(O n-C3H7)Cl2, VO(O iso-C3H7)Cl2, VO(O n-C4H9)Cl2, VO(O iso-C4H9)Cl2, VO(O sec-C4H9)Cl2, VO(O t-C4H9)Cl2, VO(OC2H5)3, VOBr2, VCl4, VOCl2, VO(O n-C4H9)3, VOCl3・2OC8H 17 OH, etc.

[0159] <Organoaluminum Compound (Q')> The organoaluminum compound (Q') constituting the vanadium catalyst is the same as the organoaluminum compound (Q-1a) described above in the "metallocene catalyst" section, and its example compounds are also the same as the examples given for the organoaluminum compound (Q-1a). The organoaluminum compound (Q') may be, for example, ethylaluminum sesquichloride.

[0160] <Conditions for polymerization using vanadium catalyst> The method of use and order of addition of the components constituting the vanadium catalyst can be selected arbitrarily.

[0161] The soluble vanadium compound (V) is usually 1 x 10 per liter of reaction volume. -5 ~5 x 10 -3 mol, preferably 5 × 10 -5 ~3 x 10 -3 It is used in an amount that will give a mol.

[0162] The organoaluminum compound (Q') is used in an amount such that the molar ratio [(Q') / M] of the organoaluminum compound (Q') to the vanadium atoms (M) in the soluble vanadium compound (V) is usually 2 to 50, preferably 3 to 20.

[0163] The polymerization temperature is usually −50° C. to 100° C., preferably −30 to 80° C., and more preferably −20 to 60° C. The polymerization pressure is usually atmospheric pressure to 5 MPa gauge pressure (MPa-G), and preferably atmospheric pressure to 2 MPa-G.

[0164] The polymerization reaction can be carried out batchwise, semi-continuously or continuously. Furthermore, the polymerization can be carried out continuously in two or more polymerization vessels with different reaction conditions.

[0165] The molecular weight of the resulting copolymer can be adjusted by changing the hydrogen concentration in the polymerization system and the polymerization temperature, and can also be adjusted by the amount of organoaluminum compound (Q') used.

[0166] The polymerization solvent used in the liquid phase polymerization method is usually an inert hydrocarbon solvent, preferably a saturated hydrocarbon having a boiling point at normal pressure of 50° C. to 200° C. The polymerization solvent may be, for example, the solvents exemplified above in the section "Conditions for polymerization using a metallocene catalyst."

[0167] Requirement (b-2): The graft-modified ethylene / α-olefin copolymer (B) contains a graft moiety derived from at least one unsaturated monomer containing a hetero atom (hereinafter, sometimes simply referred to as "unsaturated monomer").

[0168] Here, the "graft moiety derived from an unsaturated monomer containing at least one heteroatom" refers to a graft moiety containing one or more structural units corresponding to the "unsaturated monomer containing at least one heteroatom". For example, when the unsaturated monomer containing at least one heteroatom is H1 R H2 C=CR H3 R H4 (R H1 , R H2 , R H3 and R H4are each independently a hydrogen atom, a hydrocarbon group, a heteroatom, or a functional group containing a heteroatom, and R H1 , R H2 , R H3 and R H4 At least one selected from the group consisting of R H1 Or R H2 And, R H3 Or R H4 may be bonded to each other to form a ring, the "graft portion derived from an unsaturated monomer containing at least one hetero atom" is represented by -[R H1 R H2 C-CR H3 R H4 ]n H - (n H is an integer of 1 or more). Examples of the "functional group containing a hetero atom" include a hydroxyl group, a functional group containing a hydroxyl group, and a functional group containing a carbonyl group.

[0169] Specific preferred embodiments of the unsaturated monomer containing at least one heteroatom include an unsaturated carboxylic acid monomer composed of an unsaturated carboxylic acid having 3 to 10 carbon atoms, an acid anhydride or an ester thereof, and an ethylenically unsaturated monomer having a hydroxyl group. In particular, if the unsaturated monomer containing at least one heteroatom is an ethylenically unsaturated monomer having a hydroxyl group, it is preferred because it improves compatibility with the (meth)acrylic resin (A) and allows for the production of a pressure-sensitive adhesive composition that is less colored and has excellent transparency.

[0170] Unsaturated Carboxylic Acid Monomer The unsaturated carboxylic acid monomer according to the present invention is an unsaturated carboxylic acid having 3 to 10 carbon atoms, an acid anhydride thereof, or an ester thereof. More specifically, the unsaturated carboxylic acid includes acrylic acid, methacrylic acid, maleic acid, fumaric acid, tetrahydrophthalic acid, itaconic acid, citraconic acid, crotonic acid, isocrotonic acid, and nadic acid. TM (endo-cis-bicyclo[2,2,1]hept-5-ene-2,3-dicarboxylic acid) and the like.

[0171] Examples of the derivatives of unsaturated carboxylic acids include acid halide compounds, amide compounds, imide compounds, acid anhydrides, and ester compounds of the above unsaturated carboxylic acids. Specific examples include maleyl chloride, maleimide, maleic anhydride, itaconic anhydride, citraconic anhydride, tetrahydrophthalic anhydride, methyl acrylate, methyl methacrylate, monomethyl maleate, dimethyl maleate, diethyl fumarate, dimethyl itaconate, diethyl citraconic acid, dimethyl tetrahydrophthalic anhydride, 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, and glycidyl maleate.

[0172] Among these, unsaturated dicarboxylic acids and their acid anhydrides are more preferred, and particularly maleic acid and nadic acid. TM and acid anhydrides thereof are particularly preferred.

[0173] The unsaturated carboxylic acid monomers can be used either individually or in combination of two or more.

[0174] The ethylenically unsaturated monomer having a hydroxyl group according to the present invention is a compound having a hydroxyl group and an ethylenically unsaturated bond in the molecule, and examples thereof include (meth)acrylic acid esters having a hydroxyl group in the ester moiety, unsaturated alcohols, hydroxyl group-containing styrene derivatives, and hydroxyvinyl ethers. Among these, unsaturated alcohols are preferred from the viewpoints of compatibility with the (meth)acrylic resin (A) and transparency.

[0175] Examples of the (meth)acrylic acid ester having a hydroxyl group in the ester moiety include mono(meth)acrylate compounds of polyhydric alcohols, and specific examples thereof include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, and polyethylene glycol mono(meth)acrylate.

[0176] Specific examples of the unsaturated alcohol include allyl alcohol, 2-allyloxyethanol, 2-methyl-3-buten-1-ol, 2-methyl-3-buten-2-ol, 3-methyl-3-buten-1-ol, 10-undecen-1-ol, 1-octen-3-ol, 2-methanolnorbornene, 2-butene-1,4-diol, etc. Among these, 2-allyloxyethanol, 2-methyl-3-buten-1-ol, and 2-methyl-3-buten-2-ol are preferred.

[0177] Specific examples of the hydroxyl group-containing styrene derivatives include hydroxystyrene.

[0178] Specific examples of the hydroxy vinyl ether include hydroxymethyl vinyl ether, hydroxyethyl vinyl ether, hydroxypropyl vinyl ether, hydroxybutyl vinyl ether, hydroxymethyl propenyl ether, hydroxyethyl propenyl ether, hydroxypropyl propenyl ether, hydroxybutyl propenyl ether, hydroxymethyl butenyl ether, hydroxyethyl butenyl ether, hydroxypropyl butenyl ether, and hydroxybutyl butenyl ether.

[0179] Other ethylenically unsaturated monomers having a hydroxyl group that can be used include N-methylolacrylamide, 2-(meth)acryloyloxyethyl acetylphosphate, glycerin monoallyl ether, and allyloxyethanol.

[0180] The ethylenically unsaturated monomers having a hydroxyl group can be used either individually or in combination of two or more.

[0181] Requirement (b-3): The graft-modified ethylene / α-olefin copolymer (B) of the present invention is a graft-modified ethylene / α-olefin copolymer comprising a main chain derived from the ethylene / α-olefin copolymer and a graft portion derived from the at least one unsaturated monomer containing a hetero atom. From the viewpoint of reducing bleed-out while also achieving a sufficient flexibility-imparting effect, the graft portion of the graft-modified ethylene / α-olefin copolymer (B) preferably has a proportion of 0.1% by mass or more and less than 70% by mass, more preferably 0.5% by mass or more and less than 50% by mass, and even more preferably 1.0% by mass or more and less than 30% by mass (where the total amount of the main chain portion and the graft portion is taken as 100% by mass).

[0182] If the proportion of the grafted portion is less than the above lower limit, particularly 0.1% by mass, the compatibility with the acrylic resin (A) decreases, which may cause bleeding out. On the other hand, if the proportion of the grafted portion is greater than the above upper limit, particularly 70% by mass, the effect of improving flowability decreases, and a sufficient flexibility-imparting effect may not be obtained.

[0183] Requirement (b-4) From the viewpoint of reducing bleed-out, the graft-modified ethylene / α-olefin copolymer (B) according to the present invention preferably has a weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) of 1,500 to 30,000, more preferably 1,500 to 20,000, and even more preferably 1,500 to 15,000.

[0184] If the weight-average molecular weight (Mw) is less than the above lower limit, particularly 1,500, the copolymer may contain low-molecular-weight components, which may cause bleed-out. On the other hand, if the weight-average molecular weight (Mw) is greater than the above upper limit, particularly 30,000, the copolymer may become less compatible with the (meth)acrylic resin (A), which may cause bleed-out. To ensure that the resulting pressure-sensitive adhesive composition has both sufficiently high low-temperature flexibility and sufficiently high adhesiveness, it may be preferable to reduce the weight-average molecular weight (Mw) of the graft-modified ethylene / α-olefin copolymer (B) to a certain extent (for example, 10,000 or less, or in some cases, 6,000 or less).

[0185] Requirement (b-5) From the viewpoint of reducing bleed-out, the graft-modified ethylene / α-olefin copolymer (B) according to the present invention preferably has a molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) of 3.5 or less, more preferably 3.0 or less, and even more preferably 2.5 or less.

[0186] If the molecular weight distribution (Mw / Mn) exceeds the upper limit, particularly 3.5, low molecular weight components and high molecular weight components with low compatibility may cause bleeding out.

[0187] Requirement (b-6): The graft-modified ethylene / α-olefin copolymer (B) according to the present invention has a kinematic viscosity at 100° C. of 10 to 5,000 mm 2 / s, and 15 to 4,000 mm 2 / s, and more preferably 20 to 3,000 mm 2 It is more preferable that the ratio is / s.

[0188] The kinematic viscosity at 100°C is the above-mentioned lower limit, particularly 10 mm 2 If the kinematic viscosity at 100°C is less than the upper limit, particularly 5,000 mm / s, the composition may contain high-flow components, which may cause bleeding out. 2If the kinematic viscosity is greater than 1 / s, the high-viscosity component may reduce dispersibility in the (meth)acrylic resin (A), which may cause bleeding out. In order to reliably obtain both sufficiently high low-temperature flexibility and sufficiently high adhesiveness when the adhesive composition is prepared, the kinematic viscosity of the graft-modified ethylene-α-olefin copolymer (B) at 100°C should be set to a certain value (for example, 1,000 mm 2 / s or less, in some cases, 500 mm 2 It may be preferable to reduce the frequency (to 1 / s or less).

[0189] Requirement (b-7) The graft-modified ethylene / α-olefin copolymer (B) according to the present invention preferably does not exhibit a melting point as measured by differential scanning calorimetry (DSC). Here, "no melting point (Tm) is observed" means that the heat of fusion (ΔH) (unit: J / g) as measured by differential scanning calorimetry (DSC) is not substantially measured. "no heat of fusion (ΔH) is substantially not measured" means that no peak is observed in the differential scanning calorimetry (DSC) measurement, or the observed heat of fusion is 1 J / g or less.

[0190] If no melting point is observed, this is preferable because it has the effect of improving the flowability, improving the compatibility with the (meth)acrylic resin (A), and imparting flexibility at low temperatures.

[0191]

[0033] The graft-modified ethylene / α-olefin copolymer (B) according to the present invention can be prepared by various conventionally known methods, for example, by adding the at least one unsaturated monomer containing a hetero atom (hereinafter simply referred to as "unsaturated monomer" in this section) to the ethylene / α-olefin copolymer (B0) and graft-copolymerizing the resulting mixture. The ethylene / α-olefin copolymer (B0) can be obtained by the method described above in the section "Method for producing ethylene / α-olefin copolymer (B0)," and can be produced by, for example, the following method (α) or method (β).

[0192] Method (α): A method comprising: a step (S1) of solution polymerizing ethylene and an α-olefin in the presence of a catalyst system containing a bridged metallocene compound (P) represented by the following formula (1) and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2), and a compound (Q-3) that reacts with the bridged metallocene compound (P) to form an ion pair, to obtain an ethylene / α-olefin copolymer (B0); and a step (S2) of adding the unsaturated monomer described above in the requirement (b-2) to the ethylene / α-olefin copolymer (B0) to graft copolymerize it.

[0193] Y, M, and R in Formula 1 1 ~R 14 , Q and j are the same as Y, M, R described above in the section "Method for producing ethylene / α-olefin copolymer (B0)." 1 ~R 14 , Q, and j are the same as those described above in the section "Method for producing ethylene / α-olefin copolymer (B0)." The organometallic compound (Q-1), organoaluminum oxy compound (Q-2), and compound (Q-3) are the same as those described above in the section "Method for producing ethylene / α-olefin copolymer (B0)."

[0194] Method (β): A method comprising: a step (S1′) of solution polymerizing ethylene and an α-olefin in the presence of a vanadium catalyst comprising a soluble vanadium compound (V) and an organoaluminum compound (Q′) to obtain an ethylene / α-olefin copolymer (B0); and a step (S2) of adding the unsaturated monomer described above in the requirement (b-2) to the ethylene / α-olefin copolymer (B0) to graft copolymerize it.

[0195] Here, the soluble vanadium compound (V) and the organoaluminum compound (Q′) are the same as the soluble vanadium compound (V) and the organoaluminum compound (Q′) described above in the section “Method for producing ethylene / α-olefin copolymer (B0)”, respectively.

[0196] Here, the graft copolymerization of the ethylene / α-olefin copolymer (B0) with the unsaturated monomer can be carried out, for example, by the following method (1) or (2).

[0197] (1) A method in which the ethylene / α-olefin copolymer (B0) is mixed in an extruder, a batch reactor, or the like, and the unsaturated monomer is added thereto to carry out graft copolymerization.

[0198] (2) A method in which the ethylene / α-olefin copolymer (B0) is dissolved in a solvent, and the unsaturated monomer is added thereto to carry out graft copolymerization.

[0199] In either method, in order to efficiently graft copolymerize the unsaturated monomer onto the ethylene / α-olefin copolymer (B0), it is preferable to carry out the graft reaction in the presence of a radical initiator, such as an organic peroxide or an azo compound.

[0200] Examples of the organic peroxides include benzoyl peroxide, dichlorobenzoyl peroxide, dicumyl peroxide, and di-tert-butyl peroxide, and examples of the azo compounds include azobisisobutylnitrile and dimethylazoisobutyrate.

[0201] Specific examples of such radical initiators that are preferably used include dialkyl peroxides such as dicumyl peroxide, di-tert-butyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and 1,4-bis(tert-butylperoxyisopropyl)benzene.

[0202] These radical initiators are typically used in an amount of at least 0.001 parts by mass, preferably at least 0.003 parts by mass, and more preferably at least 0.05 parts by mass, per 100 parts by mass of the ethylene-α-olefin copolymer (B0), so that the radical reaction occurs sufficiently. The upper limit of the amount of radical initiator is not particularly limited as long as the effects of the present invention are not impaired. For example, the amount is 5 parts by mass or less per 100 parts by mass of the ethylene-α-olefin copolymer (B0). In one embodiment of the present invention, the radical initiator is typically used in an amount of 0.001 to 1 part by mass, preferably 0.003 to 0.5 parts by mass, and more preferably 0.05 to 0.3 parts by mass, per 100 parts by mass of the ethylene-α-olefin copolymer (B0). However, depending on the type of ethylene-α-olefin copolymer (B0), the amount of radical initiator may exceed 1 part by mass per 100 parts by mass of the ethylene-α-olefin copolymer (B0); for example, an amount of 1 to 3 parts by mass may be preferred.

[0203] The reaction temperature in the graft reaction using the above-mentioned radical initiator or in the graft reaction carried out without using a radical initiator is usually set in the range of 60 to 350°C, preferably 120 to 300°C.

[0204] [Crosslinking Agent (C)] The crosslinking agent (C) crosslinks the (meth)acrylic resin (A) to further increase the adhesiveness of the adhesive composition according to this embodiment.

[0205] Examples of the crosslinking agent (C) include epoxy compounds such as sorbitol polyglycidyl ether, polyglycerol polyglycidyl ether, pentaerythritol polyglycidyl ether, diglycerol polyglycidyl ether, glycerol polyglycidyl ether, neopentyl glycol diglycidyl ether, and resorcinol diglycidyl ether; isocyanate compounds such as tetramethylene diisocyanate, hexamethylene diisocyanate, a toluene diisocyanate triadduct of trimethylolpropane, and polyisocyanates; Examples of the crosslinking agent (C) include aziridine compounds such as trimethylolpropane-tri-β-aziridinylpropionate, tetramethylolmethane-tri-β-aziridinylpropionate, N,N'-diphenylmethane-4,4'-bis(1-aziridinecarboxamide), N,N'-hexamethylene-1,6-bis(1-aziridinecarboxamide), N,N'-toluene-2,4-bis(1-aziridinecarboxamide), and trimethylolpropane-tri-β-(2-methylaziridine)propionate, as well as melamine compounds such as hexamethoxymethylolmelamine. One type of crosslinking agent (C) may be used alone, or multiple types may be used in combination.

[0206] The crosslinking agent (C) is preferably blended in such an amount that the number of functional groups in the crosslinking agent (C) that can bond to the (meth)acrylic resin (A) (when the crosslinking agent (C) contains a blocked isocyanate, this number includes the number of functional groups generated by dissociation of the blocking agent) is not greater than the number of functional groups possessed by the (meth)acrylic resin (A). However, a larger amount may be blended in when new functional groups are generated by the crosslinking reaction or when the crosslinking reaction proceeds slowly.

[0207] [Content of each component] In the pressure-sensitive adhesive composition according to the present embodiment, when the total of the content of the (meth)acrylic resin (A), the content of the graft-modified ethylene-α-olefin copolymer (B), and the content of the crosslinking agent (C) is taken as 100% by mass, it is preferable that the amount of the (meth)acrylic resin (A) is 47% by mass or more and 99% by mass or less, the amount of the graft-modified ethylene-α-olefin copolymer (B) is 0.5% by mass or more and 50% by mass or less, and the amount of the crosslinking agent (C) is 0.5% by mass or more and 5% by mass or less.

[0208] When the content of the (meth)acrylic resin (A) is a certain amount or more, for example, 47% by mass or more, a larger amount of the (meth)acrylic resin (A) is contained in the pressure-sensitive adhesive composition, and the crosslinking density of the pressure-sensitive adhesive composition becomes higher and the molecular weight becomes higher, so that the mechanical strength is excellent and the adhesiveness is less likely to decrease. From this point of view, the content of the (meth)acrylic resin (A) is more preferably 55% by mass or more, and even more preferably 60% by mass or more.

[0209] When the content of the (meth)acrylic resin (A) is a certain amount or less, for example, 99% by mass or less, the adhesive composition contains a larger amount of the graft-modified ethylene-α-olefin copolymer (B) and the crosslinking agent (C), thereby further improving the low-temperature flexibility, moisture resistance, and adhesiveness of the adhesive composition. From this perspective, the content of the (meth)acrylic resin (A) is more preferably 97% by mass or less, and even more preferably 95% by mass or less. However, in order to reliably obtain both sufficiently high low-temperature flexibility and sufficiently high adhesiveness, it may be preferable that the content of the (meth)acrylic resin (A) be, for example, 85% by mass or less or 80% by mass or less.

[0210] From the above viewpoint, the content of the (meth)acrylic resin (A) is more preferably 55% by mass or more and 97% by mass or less, and even more preferably 60% by mass or more and 95% by mass or less.

[0211] When the content of the graft-modified ethylene / α-olefin copolymer (B) is 0.5% by mass or more, the low-temperature flexibility and moisture impermeability of the pressure-sensitive adhesive composition can be further improved. From this viewpoint, the content of the graft-modified ethylene / α-olefin copolymer (B) is more preferably 1% by mass or more, and even more preferably 3% by mass or more. However, in order to reliably obtain both sufficiently high low-temperature flexibility and sufficiently high pressure-sensitive adhesiveness, it may be preferable that the content of the graft-modified ethylene / α-olefin copolymer (B) is, for example, 15% by mass or more or 20% by mass or more.

[0212] When the content of the graft-modified ethylene / α-olefin copolymer (B) is 50% by mass or less, the adhesiveness of the adhesive composition can be further improved. From this point of view, the content of the graft-modified ethylene / α-olefin copolymer (B) is more preferably 40% by mass or less, and even more preferably 35% by mass or less.

[0213] From the above viewpoint, the content of the graft-modified ethylene / α-olefin copolymer (B) is more preferably 1% by mass or more and 40% by mass or less, and even more preferably 3% by mass or more and 35% by mass or less.

[0214] When the content of the crosslinking agent (C) is 0.5% by mass or more, the pressure-sensitive adhesive composition is likely to aggregate, and the pressure-sensitive adhesive composition is less likely to remain on the surface of the adherend after pressure-bonding, i.e., so-called adhesive residue. From this point of view, the content of the crosslinking agent (C) is more preferably 0.7% by mass or more, and even more preferably 1% by mass or more.

[0215] When the content of the crosslinking agent (C) is 5% by mass or less, a larger amount of the (meth)acrylic resin (A) is contained in the pressure-sensitive adhesive composition, and the crosslinking density of the pressure-sensitive adhesive composition becomes higher and the molecular weight becomes higher, so that the mechanical strength is excellent and the adhesiveness is less likely to decrease. From this point of view, the content of the crosslinking agent (C) is more preferably 3% by mass or less, and even more preferably 2.5% by mass or less.

[0216] From the above viewpoint, the content of the crosslinking agent (C) is more preferably 0.7% by mass or more and 3% by mass or less, and even more preferably 1% by mass or more and 2.5% by mass or less.

[0217] [Additives] In addition to the (meth)acrylic resin (A), the graft-modified ethylene-α-olefin copolymer (B), and the crosslinking agent (C), the pressure-sensitive adhesive composition of the present invention may contain, as an additive, at least one selected from an organic solvent, an antistatic agent, a silane coupling agent, an ultraviolet absorber, an antioxidant, a tackifying resin, a plasticizer, an antifoaming agent, a filler, a stabilizer, a softener, and a wettability adjuster, within a range that does not impair the effects of the present invention.

[0218] [Method for producing pressure-sensitive adhesive composition] The pressure-sensitive adhesive composition according to this embodiment can be prepared by mixing the above-described (meth)acrylic resin (A), graft-modified ethylene-α-olefin copolymer (B), and crosslinking agent (C) in amounts corresponding to the above-described contents, together with an optionally used solvent. That is, the production method according to the present invention includes a step of mixing the above-described (meth)acrylic resin (A), the above-described graft-modified ethylene-α-olefin copolymer (B), and the above-described crosslinking agent (C). Here, during the mixing, the mixture containing the above-described (meth)acrylic resin (A), the above-described graft-modified ethylene-α-olefin copolymer (B), and the above-described crosslinking agent (C) may also contain a solvent. The mixture may also contain the above-described additives.

[0219] Examples of such solvents include ethyl acetate, butyl acetate, benzene, toluene, xylene, cyclohexane, and methyl ethyl ketone.

[0220] In a preferred and exemplary embodiment of the present invention, the graft-modified ethylene / α-olefin copolymer (B) is produced by the method (α) described above in the section "Production method of graft-modified ethylene / α-olefin copolymer (B)." Accordingly, the production method may further include a step of obtaining the graft-modified ethylene / α-olefin copolymer (B) by the method (α) described above in the section "Production method of graft-modified ethylene / α-olefin copolymer (B)."

[0221] [Adhesive Sheet (Adhesive Layer)] The above-described adhesive composition can be suitably used as an adhesive, and one of the suitable uses thereof is an adhesive sheet.

[0222] The pressure-sensitive adhesive sheet of the present invention has a pressure-sensitive adhesive layer formed from the above-mentioned pressure-sensitive adhesive composition.

[0223] The pressure-sensitive adhesive layer can be produced, for example, by forming it into a film and removing the solvent. More specifically, the pressure-sensitive adhesive sheet according to this embodiment can be obtained, for example, by applying the pressure-sensitive adhesive composition according to this embodiment to a separator or a substrate to form a film, and then heating the film. More specifically, the pressure-sensitive adhesive composition according to this embodiment can be applied to a separator or a substrate by a known method such as a roll coater method, a reverse roll coater method, a gravure roll method, a bar coater method, a comma coater method, or a die coater method, and the applied pressure-sensitive adhesive composition can be dried to produce the pressure-sensitive adhesive sheet according to this embodiment.

[0224] Examples of the pressure-sensitive adhesive sheet include a double-sided pressure-sensitive adhesive sheet having only the pressure-sensitive adhesive layer, a double-sided pressure-sensitive adhesive sheet having a substrate and the pressure-sensitive adhesive layers formed on both sides of the substrate, a single-sided pressure-sensitive adhesive sheet having a substrate and the pressure-sensitive adhesive layer formed on one side of the substrate, and pressure-sensitive adhesive sheets in which a release-treated separator is attached to the side of the pressure-sensitive adhesive layer that is not in contact with other layers in these pressure-sensitive adhesive sheets.

[0225] The conditions for forming the pressure-sensitive adhesive layer are, for example, as follows. The composition is applied to a separator or a substrate and dried, usually at 60 to 120°C, preferably 70 to 110°C, usually for 1 to 15 minutes, preferably 2 to 10 minutes, to form a coating film. Subsequently, when applied to a separator, the substrate or separator is laminated to the coating film on the side without the separator. When applied to a substrate, the separator is laminated to the coating film. Subsequently, the composition is cured (aged) for usually one day or more, preferably 3 to 10 days, usually in an environment of 5 to 60°C, preferably 15 to 50°C, and usually 30 to 70% RH, preferably 40 to 70% RH. Crosslinking under the aging conditions described above enables efficient formation of a crosslinked body (network polymer). In the case of a coating film sandwiched between separators, one separator is peeled off after aging, and a substrate is laminated to the exposed pressure-sensitive adhesive layer.

[0226] Examples of the substrate and separator include plastic films such as polyester (e.g., polyethylene terephthalate, polyethylene naphthalate, etc.), polyethylene, polypropylene, polycarbonate, polymethyl methacrylate, acrylonitrile-butadiene-styrene copolymer, ethylene-vinyl acetate copolymer, polyamide, polyurethane, polyvinyl chloride, etc.; woven fabric, nonwoven fabric; paper, glass, etc. The surfaces of the substrate and separator may each be subjected to a release treatment.

[0227] The thickness of the pressure-sensitive adhesive layer is usually 3 to 1000 μm, preferably 5 to 500 μm. The thickness of the substrate and separator is usually 10 to 1000 μm. From the viewpoint of improving cohesive strength, adhesive strength, and removability, the pressure-sensitive adhesive layer preferably has a gel fraction of 40 to 90 mass %, more preferably 50 to 70 mass %.

[0228] [Uses] The pressure-sensitive adhesive composition according to this embodiment can be used in various applications requiring adhesiveness, such as adhesive processed products such as sheets, tapes, labels, and double-sided tapes, and sealing materials.

[0229] The pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet of the present invention have good adhesion to adherends such as polyolefins such as polypropylene and polyethylene, resins other than polyolefins, and glass, and can be used for a variety of components such as various display components, touch panel components, automobile components, aircraft components, ship components, electrical appliance components, building materials, electronic devices, and conductive substrates.

[0230] Touch panels are mounted on, for example, smartphones, tablet computers, and in-vehicle devices such as car navigation systems.

[0231] Examples of electronic devices include organic EL devices, solar cells, and sensor devices.

[0232] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In the following examples and comparative examples, the various physical properties were measured or evaluated by the following methods.

[0233] [Loss Tangent (tan δ) Peak Temperature] The loss tangent (tan δ) was measured using a rheometer (ARES-G2 manufactured by TA Instruments). Specifically, a sample molded into a disk shape with a diameter of 8 mm and a thickness of 0.4 mm was used, and the sample was sandwiched between two parallel plates (8 mmφ) attached to the rheometer (the gap between the parallel plates was 0.4 mm). The temperature dependence of the dynamic viscoelasticity (specifically, the loss modulus G" and the storage modulus G') from -100 to 200°C was measured at a frequency of 1 Hz and a heating rate of 3°C / min, and the peak temperature of the loss tangent (tan δ) due to the glass transition temperature was measured. Here, the loss tangent (tan δ) is the ratio of the loss modulus G" to the storage modulus G'.

[0234] [Weight-average molecular weight (Mw) and molecular weight distribution (Mw / Mn)] These were determined using the following high-speed GPC measuring device.

[0235] Measurement apparatus: HLC8320GPC manufactured by Tosoh Corporation Mobile phase: THF (manufactured by Wako Pure Chemical Industries, Ltd., stabilizer-free, liquid chromatography grade) Column: Two TSKgel Super Multipore HZ-M columns manufactured by Tosoh Corporation connected in series Sample concentration: 5 mg / mL Mobile phase flow rate: 0.35 mL / min Measurement temperature: 40°C Standard sample for calibration curve: PStQuick MP-M manufactured by Tosoh Corporation

[0236] [Kinematic Viscosity] Measurement was carried out using a fully automatic viscometer CAV-4 manufactured by Cannon Instrument Company in accordance with ASTM D 445. The measurement was carried out at 100°C unless otherwise specified.

[0237] [Composition] The content of each structural unit (ethylene and α-olefin) in the ethylene-α-olefin copolymer is 13 The NMR measurement was carried out using a nuclear magnetic resonance apparatus of the ECP500 type manufactured by JEOL Ltd., with a mixed solvent of ortho-dichlorobenzene / heavy benzene (80 / 20% by volume) as the solvent, a sample concentration of 55 mg / 0.6 mL, a measurement temperature of 120°C, and an observation nucleus of 13 The measurement was performed using C (125 MHz), a sequence of single pulse proton decoupling, a pulse width of 4.7 μs (45° pulse), a repetition time of 5.5 seconds, an accumulation count of 10,000 or more, and a chemical shift reference value of 27.50 ppm. 13 The values ​​were determined from C-NMR spectra based on the reports of "Polymer Analysis Handbook" (published by Asakura Publishing, pp. 163-170), G. J. Ray (Macromolecules, 10, 773 (1977)), J. C. Randall (Macromolecules, 15, 353 (1982)), K. Kimura (Polymer, 25, 4418 (1984)), and others.

[0238] [Melting Point] Measurement was performed using a Seiko Instruments X-DSC-7000. Approximately 8 mg of sample was placed in a sealable aluminum sample pan and placed in a DSC cell. The DSC cell was heated from room temperature to 150°C at 10°C / min under a nitrogen atmosphere, then held at 150°C for 5 minutes, and then cooled at 10°C / min to -100°C (cooling down process). The DSC cell was then held at -100°C for 5 minutes and then heated to 150°C at 10°C / min. The melting point was determined as the temperature at which the enthalpy curve (DSC curve) obtained during the heating process showed a maximum value (however, a minimum value when the heat flow (heat flow) associated with endotherm is taken in the negative direction), and the sum of the endotherms associated with melting was determined as the heat of fusion. If no peak was observed in this enthalpy curve (DSC curve) or the observed heat of fusion value was 1 J / g or less, the melting point (Tm) was considered not to be observed. The melting point and heat of fusion were determined in accordance with JIS K7121.

[0239] [(Meth)acrylic Resin (A)] [Production Example A1] Synthesis of (meth)acrylic Resin (A-1) A temperature-controllable reactor equipped with a stirrer was charged with 350 parts by mass of ethyl acetate as a polymerization solvent and 40 parts by mass of toluene, purged with nitrogen, and heated to 75°C. Thereafter, to the resulting mixture of ethyl acetate and toluene, a mixture of 316 parts by mass of n-butyl acrylate, 43 parts by mass of ethyl acrylate, 50 parts by mass of vinyl acetate, 9 parts by mass of acrylic acid, 2 parts by mass of hydroxyethyl acrylate, and 2 parts by mass of benzoyl peroxide as a polymerization initiator was continuously added, followed by a reaction for 5 hours. Five hours after the addition was completed, the resulting reaction mixture was diluted with 120 parts by mass of toluene to obtain an ethyl acetate / toluene solution containing a (meth)acrylic resin with a solids content of 45%.

[0240] Here, the (meth)acrylic resin obtained in this production example is referred to as (meth)acrylic resin (A-1).

[0241] The (meth)acrylic resin (A-1) obtained by volatilizing the solvent from the resulting ethyl acetate / toluene solution had a peak temperature of loss tangent (tan δ) attributable to the glass transition temperature, as determined by measuring the temperature dependence of dynamic viscoelasticity (frequency 1 Hz, −100 to 200° C.), of −47° C.

[0242] The composition of the (meth)acrylic resin (A-1) was quantified by pyrolysis gas chromatography mass spectrometry (pyrolysis GC-MS), and it was found that the content of structural units derived from (meth)acrylates having an alkyl group having from 1 to 12 carbon atoms was 80 mol %, and the content of structural units derived from (meth)acrylates containing a hydroxyl group was 0.5 mol %. The quantification by pyrolysis GC-MS was carried out under the following conditions.

[0243] Pyrolysis apparatus: JAIJHP-5 manufactured by Japan Analytical Industry Co., Ltd. Pyrolysis temperature: 590°C GC apparatus: 6890N manufactured by Agilent Column: DB-5MS manufactured by Agilent Column temperature: 40°C Column flow rate: 0.9 mL / min (Mobile phase: Helium) MS apparatus: JMS-Q1000GC manufactured by JEOL

[0244] [Ethylene / α-olefin copolymer (X)] [Production Example X1] Synthesis of ethylene / α-olefin copolymer (X-1) 760 mL of heptane and 120 g of propylene were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 150°C. After that, 0.85 MPa of hydrogen and 0.19 MPa of ethylene were fed to adjust the total pressure to 3 MPa-G. Next, 0.4 mmol of triisobutylaluminum, [methylphenylmethylene (η 5 -cyclopentadienyl) (η 50.0002 mmol of [N,N-2,7-di-tert-butylfluorenyl]zirconium dichloride and 0.002 mmol of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate were injected with nitrogen, and polymerization was initiated by adjusting the stirring speed to 400 rpm. Subsequently, the total pressure was maintained at 3 MPa-G by continuously supplying only ethylene, and polymerization was carried out for 5 minutes at 150°C. After terminating the polymerization by adding a small amount of ethanol to the system, unreacted ethylene, propylene, and hydrogen were purged. The resulting polymerization solution was washed three times with 1000 mL of 0.2 mol / L hydrochloric acid, followed by three times with 1000 mL of distilled water. After drying over magnesium sulfate, the solvent was removed by distillation under reduced pressure to obtain a crude ethylene-propylene copolymer.

[0245] A 1 L stainless steel autoclave was charged with 100 mL of a 0.5 wt% Pd / alumina catalyst hexane solution and 500 mL of a 30 wt% hexane solution of the resulting crude ethylene-α-olefin copolymer. The autoclave was then sealed and purged with nitrogen. The temperature was then raised to 140°C with stirring, and the system was purged with hydrogen. The pressure was then increased to 1.5 MPa with hydrogen, and a hydrogenation reaction was carried out for 15 minutes. The reaction solution was filtered to remove the hydrogenation catalyst, and the solvent was removed from the resulting filtrate by distillation under reduced pressure. The filtrate was then dried under reduced pressure at 80°C for 24 hours to obtain an ethylene-propylene copolymer.

[0246] Here, the ethylene-propylene copolymer obtained in this production example is referred to as ethylene-α-olefin copolymer (X-1).

[0247] The resulting ethylene / α-olefin copolymer (X-1) had a weight average molecular weight (Mw): 5,100, a molecular weight distribution (Mw / Mn): 1.7, and a kinematic viscosity at 100° C.: 150 mm 2 / s, ethylene content: 48 mol %, and no melting point was observed.

[0248] [Production Example X2] Synthesis of ethylene / α-olefin copolymer (X-2) 760 mL of heptane and 120 g of propylene were charged into a 2 L stainless steel autoclave that had been thoroughly purged with nitrogen, and the temperature inside the system was raised to 150°C. After that, 0.85 MPa of hydrogen and 0.19 MPa of ethylene were fed to adjust the total pressure to 3 MPa-G. Next, 0.4 mmol of triisobutylaluminum, [diphenylmethylene (η 5 -3-n-butylcyclopentadienyl)(η 5 0.0002 mmol of [N,N-2,7-di-tert-butylfluorenyl]zirconium dichloride and 0.002 mmol of N,N-dimethylanilinium tetrakis(pentafluorophenyl)borate were injected with nitrogen, and polymerization was initiated by adjusting the stirring speed to 400 rpm. Subsequently, the total pressure was maintained at 3 MPa-G by continuously supplying only ethylene, and polymerization was carried out for 5 minutes at 150°C. After terminating the polymerization by adding a small amount of ethanol to the system, unreacted ethylene, propylene, and hydrogen were purged. The resulting polymerization solution was washed three times with 1000 mL of 0.2 mol / L hydrochloric acid, followed by three times with 1000 mL of distilled water. After drying over magnesium sulfate, the solvent was removed by distillation under reduced pressure to obtain a crude ethylene-propylene copolymer.

[0249] A 1 L stainless steel autoclave was charged with 100 mL of a 0.5 wt% Pd / alumina catalyst hexane solution and 500 mL of a 30 wt% hexane solution of the resulting crude ethylene-α-olefin copolymer. The autoclave was then sealed and purged with nitrogen. The temperature was then raised to 140°C with stirring, and the system was purged with hydrogen. The pressure was then increased to 1.5 MPa with hydrogen, and a hydrogenation reaction was carried out for 15 minutes. The reaction solution was filtered to remove the hydrogenation catalyst, and the solvent was removed from the resulting filtrate by distillation under reduced pressure. The filtrate was then dried under reduced pressure at 80°C for 24 hours to obtain an ethylene-propylene copolymer.

[0250] Here, the ethylene-propylene copolymer obtained in this production example is referred to as ethylene-α-olefin copolymer (X-2).

[0251] The resulting ethylene / α-olefin copolymer (X-2) had a weight average molecular weight (Mw): 4,800, a molecular weight distribution (Mw / Mn): 1.7, and a kinematic viscosity at 100° C.: 150 mm 2 / s, ethylene content: 49 mol %, and no melting point was observed.

[0252] [Production Example X3] Synthesis of Ethylene-α-Olefin Copolymer (X-3) 1 L of dehydrated and purified hexane was placed in a 2 L continuous polymerization reactor equipped with an agitator and thoroughly purged with nitrogen. 96 mmol / L of ethylaluminum sesquichloride (Al(CH) 1.5 ・Cl 1.5 A hexane solution of VO(OCH)Cl adjusted to 16 mmol / L was continuously fed at 500 mL / h as a catalyst, and hexane was continuously fed at 500 mL / h. Meanwhile, the polymerization liquid was continuously withdrawn from the top of the reactor so that the volume of the polymerization liquid in the reactor was always 1 L.

[0253] Next, ethylene gas was supplied at a rate of 47 L / h, propylene gas at a rate of 47 L / h, and hydrogen gas at a rate of 20 L / h using a bubbling tube. The copolymerization reaction was carried out at 35°C by circulating a coolant through a jacket attached to the outside of the reactor. As a result, a polymerization solution containing an ethylene-propylene copolymer was obtained.

[0254] The resulting polymerization solution was washed three times with 500 mL of 0.2 mol / L hydrochloric acid per 1 L of the polymerization solution, and then three times with 500 mL of distilled water per 1 L of the polymerization solution, dried over magnesium sulfate, and the solvent was distilled off under reduced pressure. The resulting viscous liquid was dried under reduced pressure at 130°C for 24 hours to obtain an ethylene-propylene copolymer.

[0255] Here, the ethylene-propylene copolymer obtained in this production example is referred to as ethylene-α-olefin copolymer (X-3).

[0256] The resulting ethylene / α-olefin copolymer (X-3) had a weight average molecular weight (Mw): 12,400, a molecular weight distribution (Mw / Mn): 1.9, and a kinematic viscosity at 100°C: 2,000 mm 2 / s, ethylene content: 53 mol %, and no melting point was observed.

[0257] The data of the obtained ethylene / α-olefin copolymers (X-1) to (X-3) are shown below. In the following Production Examples B1, B4, and B5, the ethylene / α-olefin copolymer (X-1) was used as the ethylene / α-olefin copolymer (B0), in the following Production Example B2, the ethylene / α-olefin copolymer (X-2), and in the following Production Example B3, the ethylene / α-olefin copolymer (X-3) were used as the ethylene / α-olefin copolymer (B0).

[0258]

[0259] [Graft-modified ethylene / α-olefin copolymer (B)] [Production Example B1] Synthesis of graft-modified ethylene / α-olefin copolymer (B-1) Using the ethylene / α-olefin copolymer (X-1) as a raw material ethylene / α-olefin copolymer (ethylene / α-olefin copolymer (B0)), a graft-modified ethylene / α-olefin copolymer was prepared as follows.

[0260] A 500 mL glass reactor equipped with a stirrer, a nitrogen inlet tube, a water-cooled condenser, and a thermometer, was charged with 120 g of ethylene / α-olefin copolymer (X-1), 15 g of 2-methyl-3-buten-2-ol, and 3 g of di-tert-butyl peroxide, and the atmosphere was replaced with nitrogen for 1 hour to remove dissolved oxygen. The temperature inside the reactor was then raised to 160°C, and the reaction was carried out for 3 hours. The temperature inside the reactor was then raised to 180°C, and unreacted 2-methyl-3-buten-2-ol and decomposition products of di-tert-butyl peroxide were removed under reduced pressure (10 Torr), thereby obtaining a graft-modified ethylene / α-olefin copolymer.

[0261] Here, the graft-modified ethylene / α-olefin copolymer obtained in this Production Example is referred to as graft-modified ethylene / α-olefin copolymer (B-1).

[0262] The graft ratio of the resulting graft-modified ethylene / α-olefin copolymer (B-1) was 9% by mass, which was determined by quantifying the hydroxyl group content in a sample by measuring the hydroxyl value by the acetylation method and calculating the content of the hydroxyl group-containing graft monomer component from the value.

[0263] Weight average molecular weight (Mw): 5,300, molecular weight distribution (Mw / Mn): 1.8, kinematic viscosity at 100°C: 200 mm 2 / s and no melting point was observed.

[0264] [Production Example B2] Synthesis of Graft-Modified Ethylene / α-olefin Copolymer (B-2) Using the ethylene / α-olefin copolymer (X-2) as a raw material ethylene / α-olefin copolymer (ethylene / α-olefin copolymer (B0)), a graft-modified ethylene / α-olefin copolymer was prepared as follows.

[0265] A 500 mL glass reactor equipped with a stirrer, a nitrogen inlet tube, a water-cooled condenser, and a thermometer, was charged with 120 g of ethylene / α-olefin copolymer (X-2), 15 g of 2-methyl-3-buten-2-ol, and 3 g of di-tert-butyl peroxide, and the atmosphere was replaced with nitrogen for 1 hour to remove dissolved oxygen. The temperature inside the reactor was then raised to 160°C, and the reaction was carried out for 3 hours. The temperature inside the reactor was then raised to 180°C, and unreacted 2-methyl-3-buten-2-ol and decomposition products of di-tert-butyl peroxide were removed under reduced pressure (10 Torr), thereby obtaining a graft-modified ethylene / α-olefin copolymer.

[0266] Here, the graft-modified ethylene / α-olefin copolymer obtained in this Production Example is referred to as graft-modified ethylene / α-olefin copolymer (B-2).

[0267] The graft ratio of the resulting graft-modified ethylene / α-olefin copolymer (B-2) was 8% by mass, which was determined by quantifying the hydroxyl group content in a sample by measuring the hydroxyl value by the acetylation method and calculating the content of the hydroxyl group-containing graft monomer component from the value.

[0268] Weight average molecular weight (Mw): 5000, molecular weight distribution (Mw / Mn): 1.8, kinematic viscosity at 100°C: 190 mm 2 / s and no melting point was observed.

[0269] [Production Example B3] Synthesis of Graft-Modified Ethylene / α-olefin Copolymer (B-3) Using the ethylene / α-olefin copolymer (X-3) as a raw material ethylene / α-olefin copolymer (ethylene / α-olefin copolymer (B0)), a graft-modified ethylene / α-olefin copolymer was prepared as follows.

[0270] A 500 mL glass reactor equipped with a stirrer, a nitrogen inlet tube, a water-cooled condenser, and a thermometer, was charged with 120 g of ethylene / α-olefin copolymer (X-3), 15 g of 2-methyl-3-buten-2-ol, and 3 g of di-tert-butyl peroxide, and the atmosphere was replaced with nitrogen for 1 hour to remove dissolved oxygen. The temperature inside the reactor was then raised to 160°C, and the reaction was carried out for 3 hours. The temperature inside the reactor was then raised to 180°C, and unreacted 2-methyl-3-buten-2-ol and decomposition products of di-tert-butyl peroxide were removed under reduced pressure (10 Torr), thereby obtaining a graft-modified ethylene / α-olefin copolymer.

[0271] Here, the graft-modified ethylene / α-olefin copolymer obtained in this Production Example is referred to as graft-modified ethylene / α-olefin copolymer (B-3).

[0272] The graft ratio of the obtained graft-modified ethylene / α-olefin copolymer (B-3) was 8% by mass. The graft ratio was determined by quantifying the hydroxyl group content in the sample by measuring the hydroxyl value by the acetylation method and calculating the content of the hydroxyl group-containing graft monomer component from the value. The copolymer also had a weight average molecular weight (Mw): 14,300, a molecular weight distribution (Mw / Mn): 2.4, and a kinematic viscosity at 100°C: 2,020 mm 2 / s and no melting point was observed.

[0273] [Production Example B4] Synthesis of Graft-Modified Ethylene / α-olefin Copolymer (B-4) Using the ethylene / α-olefin copolymer (X-1) as a raw material ethylene / α-olefin copolymer (ethylene / α-olefin copolymer (B0)), a graft-modified ethylene / α-olefin copolymer was prepared as follows.

[0274] A 500 mL glass reactor equipped with a stirrer, a nitrogen inlet tube, a water-cooled condenser, and a thermometer, was charged with 120 g of ethylene / α-olefin copolymer (X-1), 10 g of 2-allyloxyethanol, and 2 g of di-tert-butyl peroxide, and the atmosphere was replaced with nitrogen for 1 hour to remove dissolved oxygen. The temperature inside the reactor was then raised to 160°C, and the reaction was carried out for 3 hours. The temperature inside the reactor was then raised to 180°C, and unreacted 2-allyloxyethanol and decomposition products of di-tert-butyl peroxide were removed under reduced pressure (10 Torr), thereby obtaining a graft-modified ethylene / α-olefin copolymer.

[0275] Here, the graft-modified ethylene / α-olefin copolymer obtained in this Production Example is referred to as graft-modified ethylene / α-olefin copolymer (B-4).

[0276] The graft ratio of the obtained graft-modified ethylene / α-olefin copolymer (B-4) was 7% by mass. The graft ratio was determined by quantifying the hydroxyl group content in the sample by measuring the hydroxyl value by the acetylation method and calculating the content of the hydroxyl group-containing graft monomer component from the value. The copolymer also had a weight average molecular weight (Mw): 4,800, a molecular weight distribution (Mw / Mn): 1.7, and a kinematic viscosity at 100°C: 190 mm 2 / s and no melting point was observed.

[0277] [Production Example B5] Synthesis of Graft-Modified Ethylene / α-olefin Copolymer (B-5) Using the ethylene / α-olefin copolymer (X-1) as a raw material ethylene / α-olefin copolymer (ethylene / α-olefin copolymer (B0)), a graft-modified ethylene / α-olefin copolymer was prepared as follows.

[0278] A 200 mL glass reactor equipped with a stirrer and equipped with a nitrogen inlet tube, a water-cooled condenser, a thermometer, and two dropping funnels was charged with 100 g of ethylene-α-olefin copolymer (X-1). After heating, nitrogen bubbling was initiated at 120°C and the system was maintained at 160°C. Subsequently, 6.6 g of maleic anhydride (which had been heated to about 70°C to make it liquid) and 1.3 g of di-tert-butyl peroxide, which had been previously charged into each of the two dropping funnels, were fed to the reactor over 5 hours, and the reaction was allowed to proceed for 1 hour after the completion of the feed. The temperature was then raised to 175°C, and the system was depressurized. Then, the pressure was reduced for 1 hour while gradually introducing nitrogen using a vacuum pump to remove impurities (decomposition products of unreacted maleic anhydride and di-tert-butyl peroxide), thereby obtaining a graft-modified ethylene-α-olefin copolymer.

[0279] Here, the graft-modified ethylene / α-olefin copolymer obtained in this Production Example is referred to as graft-modified ethylene / α-olefin copolymer (B-5).

[0280] The graft ratio of the resulting graft-modified ethylene / α-olefin copolymer (B-5) was 5% by mass. The graft ratio was determined by quantifying the oxygen content by elemental analysis and calculating the succinic anhydride skeleton component from the value.

[0281] Weight average molecular weight (Mw): 5600, molecular weight distribution (Mw / Mn): 1.8, kinematic viscosity at 100°C: 420 mm 2 / s and no melting point was observed.

[0282] The data of the resulting graft-modified ethylene / α-olefin copolymers (B-1) to (B-5) are shown below.

[0283]

[0284] [Crosslinking Agent (C)] Takenate D-101E (an isocyanate compound, "Takenate" is a registered trademark of Mitsui Chemicals, Inc.) was used as the crosslinking agent (C-1).

[0285] [Examples 1 to 6, Comparative Examples 1 to 5] In each of Examples 1 to 6 and Comparative Examples 1 to 5, an ethyl acetate / toluene solution containing the (meth)acrylic resin (A-1), any one of the graft-modified ethylene-α-olefin copolymers (B-1) to (B-5) or the ethylene-α-olefin copolymers (X-1) to (X-3), and a crosslinking agent (C) were mixed and stirred at room temperature to obtain an ethyl acetate / toluene solution of an adhesive composition. Here, the ratio of the mass of the (meth)acrylic resin (A-1), the mass of any one of the graft-modified ethylene-α-olefin copolymers (B-1) to (B-5) or the ethylene-α-olefin copolymers (X-1) to (X-3), and the mass of the crosslinking agent (C) contained in the ethyl acetate / toluene solution in the adhesive composition was as shown in Table 3.

[0286] In addition, in the evaluation of each physical property described below, an ethyl acetate / toluene solution obtained by adding toluene to the mixture obtained by stirring and mixing so that the mass ratio of ethyl acetate to toluene was adjusted to 40 / 60 (hereinafter referred to as "ethyl acetate / toluene (40 / 60 mass %) solution of adhesive composition") was used.

[0287] [Evaluation of Adhesion] The adhesion of each of the ethyl acetate / toluene (40 / 60 mass %) solutions of the adhesive compositions obtained in the Examples and Comparative Examples was evaluated as follows.

[0288] An ethyl acetate / toluene (40 / 60 mass%) solution of the obtained adhesive composition was applied to a release paper so that the film thickness after drying was 25 μm, and after drying at 100° C. for 10 minutes, a 50 μm thick PET film was pressed onto the coated surface to prepare an adhesive sheet having a base layer made of PET film and an adhesive layer made of the adhesive composition. The sheet was left at 50° C. for 3 days to allow the adhesive composition to be sufficiently crosslinked.

[0289] The pressure-sensitive adhesive sheet was cut into a width of 25 mm and a length of 150 mm to prepare a test specimen. The release paper was peeled off from the test specimen to expose the pressure-sensitive adhesive layer, and the exposed pressure-sensitive adhesive layer was brought into contact with a PP plate in an atmosphere of 23°C, and the test specimen was pressure-bonded by moving a 2 kg rubber roll back and forth twice. After leaving the test specimen for 20 minutes, the 180° peel strength was measured at a speed of 300 mm / min in accordance with JIS Z0237.

[0290] The adhesiveness was evaluated based on the obtained peel strength. The evaluation results are shown in Table 3. The symbols in the table have the following meanings.

[0291] ◯: Peel strength is 3 N / 25 mm or more △: Peel strength is less than 3 N / 25 mm, 1 N / 25 mm or more ×: Peel strength is less than 1 N / 25 mm Here, the symbol "◯" indicates that the adhesive sheet and the PP plate are bonded with sufficient strength.

[0292] The symbol "Δ" indicates that the adhesive sheet and the PP plate are bonded with a certain degree of strength.

[0293] The symbol "x" indicates that there is poor adhesion between the adhesive sheet and the PP plate (unbonded state).

[0294] When the pressure-sensitive adhesive composition of the present invention is used as a pressure-sensitive adhesive for pressure-sensitive adhesive sheets and the like, a higher adhesive strength is preferable because it can prevent peeling between substrates.

[0295] [Evaluation of Low-Temperature Flexibility] Evaluation of low-temperature flexibility was carried out as follows for each of the ethyl acetate / toluene (40 / 60 mass %) solutions of the pressure-sensitive adhesive compositions obtained in the Examples and Comparative Examples.

[0296] An ethyl acetate / toluene (40 / 60 mass %) solution of the obtained adhesive composition was applied to a release paper so that the film thickness after drying would be 25 μm, and the applied film was dried at 100° C. for 10 minutes. The release paper was then peeled off from the obtained laminate to obtain a sheet made of the adhesive composition.

[0297] The dynamic viscoelasticity of the obtained sheet of the pressure-sensitive adhesive composition was measured at a frequency of 1 Hz at -20°C using a rheometer (ARES-G2 manufactured by TA Instruments) with a measuring jig of parallel plates (8 mmφ). Specifically, a sheet of the pressure-sensitive adhesive composition was molded into a disk shape of 8 mm in diameter x 0.4 mm in thickness, and the sample was sandwiched between two parallel plates (8 mmφ) attached to the rheometer (the gap between the parallel plates was 0.4 mm), and the loss modulus G" and storage modulus G' were measured at a frequency of 1 Hz at -20°C. Low-temperature flexibility was evaluated from the obtained storage modulus G'. The evaluation results are shown in Table 3. The meanings of the symbols in the table are as follows:

[0298] ◯: Storage modulus G' is 0.1 MPa or more and less than 0.5 MPa △: Storage modulus G' is 0.5 MPa or more and less than 1.0 MPa ×: Storage modulus G' is 1.0 MPa or more Here, the symbol "◯" indicates that the adhesive is sufficiently soft, and when the adhesive sheet obtained by combining with a substrate is bent, the adhesive can sufficiently follow the movement of the substrate, and peeling of the adhesive from the substrate is extremely unlikely to occur (i.e., peeling of the adhesive due to insufficient following when the substrate is bent is extremely unlikely to occur).

[0299] The symbol "△" indicates that the adhesive is relatively soft, and when the adhesive sheet obtained by combining it with a substrate is folded, the adhesive can follow the movement of the substrate to some extent, and peeling of the adhesive from the substrate is somewhat unlikely to occur (i.e., peeling of the adhesive due to insufficient following when the substrate is folded is somewhat unlikely to occur).

[0300] The symbol "x" indicates that the adhesive is hard and cannot follow the movement of the substrate when the adhesive sheet obtained by combining it with a substrate is folded, making the adhesive prone to peeling from the substrate (i.e., the adhesive is prone to peeling due to insufficient following when the substrate is folded).

[0301] When the pressure-sensitive adhesive composition of the present invention is used for a pressure-sensitive adhesive such as a pressure-sensitive adhesive sheet, the lower the storage modulus G' at -20°C, the better the low-temperature flexibility. This is preferable because when the pressure-sensitive adhesive composition of the present invention is combined with a substrate to form a pressure-sensitive adhesive sheet, the pressure-sensitive adhesive can follow the substrate even when the substrate is bent, and peeling of the pressure-sensitive adhesive can be suppressed.

[0302] [Evaluation of Moisture Permeability Resistance] The moisture permeability resistance was evaluated as follows for each of the ethyl acetate / toluene (40 / 60 mass %) solutions of the pressure-sensitive adhesive compositions obtained in the Examples and Comparative Examples.

[0303] An ethyl acetate / toluene (40 / 60 mass%) solution of the obtained pressure-sensitive adhesive composition was applied to a 50 μm thick cellulose triacetate film (TAC film) so that the film thickness after drying would be 50 μm. After drying at 100° C. for 10 minutes, a 50 μm thick TAC film was pressed onto the coated surface to prepare a pressure-sensitive adhesive sheet. The pressure-sensitive adhesive composition was left to stand at 50° C. for 3 days to fully crosslink the composition.

[0304] The pressure-sensitive adhesive sheet was cut into a length of 50 mm and a width of 50 mm to prepare a test piece.

[0305] The obtained test piece was subjected to the moisture permeability test (g / m) under the conditions of 40°C, 90% RH, and 24 hours in accordance with the MOCON method. 2 ・24h) was measured.

[0306] The moisture permeability resistance was evaluated based on the moisture permeability obtained. The evaluation results are shown in Table 3. The symbols in the table have the following meanings.

[0307] ◯: The moisture permeability of the PSA sheet to be evaluated is less than 0.50 times the moisture permeability of the PSA sheet obtained in Comparative Example 4 (i.e., the rate of reduction relative to the moisture permeability of the PSA sheet obtained in Comparative Example 4 is 50% or more and less than 100%). △: The moisture permeability of the PSA sheet to be evaluated is more than 0.50 times and not more than 0.90 times the moisture permeability of the PSA sheet obtained in Comparative Example 4 (i.e., the rate of reduction relative to the moisture permeability of the PSA sheet obtained in Comparative Example 4 is 10% or more and less than 50%). ×: The moisture permeability of the PSA sheet to be evaluated is more than 0.90 times the moisture permeability of the PSA sheet obtained in Comparative Example 4 (i.e., the moisture permeability is not reduced at all compared to the PSA sheet obtained in Comparative Example 4, or the rate of reduction relative to the moisture permeability of the PSA sheet obtained in Comparative Example 4 is less than 10%).

[0308] The symbol "○" or "△" indicates that the moisture permeability of the PSA sheet to be evaluated is somewhat lower than the moisture permeability of the PSA sheet obtained in Comparative Example 4, and means that the PSA composition constituting the PSA sheet exhibits moisture permeability resistance that is somewhat superior to that of a PSA composition (Comparative Example 4) that does not contain the graft-modified ethylene-α-olefin copolymers (B-1) to (B-5) or the ethylene-α-olefin copolymers (X-1) to (X-3). Here, PSA compositions scored as "○" have high moisture permeability resistance and tend to be less likely to cause whitening, foaming, or lifting of the PSA under high durability conditions when used in PSAs such as PSA sheets. Furthermore, PSA compositions scored as "△" have a certain degree of moisture permeability resistance and tend to be less likely to cause whitening, foaming, or lifting of the PSA under high durability conditions when used in PSAs such as PSA sheets.

[0309] On the other hand, the symbol "x" indicates that the moisture permeability of the PSA sheet to be evaluated is equivalent to that of the PSA sheet obtained in Comparative Example 4, and means that the PSA composition constituting the PSA sheet does not exhibit sufficient moisture permeability resistance, similar to the PSA composition not containing the graft-modified ethylene-α-olefin copolymers (B-1) to (B-5) or the ethylene-α-olefin copolymers (X-1) to (X-3) (Comparative Example 4). In other words, PSA compositions scored with "x" have insufficient moisture permeability resistance, and when used in PSAs such as PSA sheets, tend to easily cause PSA whitening, foaming, or lifting under high durability conditions.

[0310] When the adhesive composition of the present invention is used as an adhesive for an adhesive sheet or the like, the lower the rate of decrease in moisture permeability, the better the moisture permeability resistance is, and therefore, it is preferable because the occurrence of whitening, foaming, or lifting of the adhesive can be suppressed even under high durability conditions.

[0311]

[0312]

Claims

1. An adhesive composition comprising: a (meth)acrylic resin (A); a graft-modified ethylene / α-olefin copolymer (B) satisfying the following requirements (b-1) to (b-2); and a crosslinking agent (C); (b-1) comprising a main chain portion derived from an ethylene / α-olefin copolymer (B0); (b-2) comprising a graft portion derived from at least one unsaturated monomer containing a hetero atom.

2. The adhesive composition according to claim 1, wherein the (meth)acrylic resin (A) satisfies the following (a-1) to (a-2); (a-1) it contains a structural unit derived from a (meth)acrylate having an alkyl group having 1 to 12 carbon atoms, and a structural unit derived from a (meth)acrylate containing a hydroxyl group; (a-2) it has a peak temperature of loss tangent (tan δ) due to the glass transition temperature measured by temperature dependence of dynamic viscoelasticity (frequency 1 Hz, -100 to 200°C) of less than 0°C.

3. The adhesive composition according to claim 1, wherein in (b-2), the unsaturated monomer is at least one unsaturated monomer selected from the group consisting of at least one unsaturated carboxylic acid monomer selected from the group consisting of unsaturated carboxylic acids having 3 to 10 carbon atoms, their acid anhydrides and esters, and at least one unsaturated monomer selected from the group consisting of ethylenically unsaturated monomers having a hydroxyl group.

4. The pressure-sensitive adhesive composition according to claim 1, wherein the unsaturated monomer in (b-2) is an unsaturated alcohol.

5. The pressure-sensitive adhesive composition according to claim 1, wherein the ethylene / α-olefin copolymer (B0) satisfies the following (b-1-1) to (b-1-5): (b-1-1) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (b-1-2) the molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less; (b-1-3) the kinetic viscosity at 100°C is 10 to 5,000 mm 2 (b-1-4) the content of ethylene units is 10 to 85 mol %; (b-1-5) no melting point is observed as measured by differential scanning calorimetry (DSC).

6. The adhesive composition according to claim 1, wherein the graft-modified ethylene / α-olefin copolymer (B) further satisfies one or more of the following (b-3) to (b-7): (b-3) the proportion of the graft portion is 0.1% by mass or more and less than 70% by mass (wherein the total amount of the main chain portion and the graft portion is 100% by mass); (b-4) the weight average molecular weight (Mw) determined by gel permeation chromatography (GPC) is 1,500 to 30,000; (b-5) the molecular weight distribution (Mw / Mn) determined by gel permeation chromatography (GPC) is 2.5 or less; (b-6) the kinetic viscosity at 100°C is 10 to 5,000 mm 2 / s; (b-7) No melting point is observed as measured by differential scanning calorimetry (DSC).

7. An adhesive composition as described in claim 1, wherein, when the sum of the content of the (meth)acrylic resin (A), the content of the graft-modified ethylene-α-olefin copolymer (B), and the content of the crosslinking agent (C) is 100% by mass, the amount of the (meth)acrylic resin (A) is 47% by mass or more and 99% by mass, the amount of the graft-modified ethylene-α-olefin copolymer (B) is 0.5% by mass or more and 50% by mass or less, and the amount of the crosslinking agent (C) is 0.5% by mass or more and 5% by mass or less.

8. An adhesive sheet having an adhesive layer formed from the adhesive composition according to any one of claims 1 to 7.

9. A method for producing an adhesive composition, comprising the steps of mixing a (meth)acrylic resin (A), a graft-modified ethylene / α-olefin copolymer (B) produced by the following method (α) or method (β) and satisfying the following requirements (b-1) to (b-2), and a crosslinking agent (C); (b-1) comprising a main chain portion derived from an ethylene / α-olefin copolymer; (b-2) comprising a graft portion derived from an unsaturated monomer containing at least one hetero atom; Method (α): A step (S1) of solution-polymerizing ethylene and an α-olefin in the presence of a catalyst system comprising a bridged metallocene compound (P) represented by the following formula (1) and at least one compound (Q) selected from the group consisting of an organometallic compound (Q-1), an organoaluminum oxy compound (Q-2) and a compound (Q-3) which reacts with the bridged metallocene compound (P) to form an ion pair, to obtain an ethylene / α-olefin copolymer (B0); a step (S2) of adding the unsaturated monomer to the ethylene / α-olefin copolymer (B0) to graft copolymerize it. [In formula 1, R 1 , R 2 , R 3 , R 4 , R 5 , R 8 , R 9 and R 12 are each independently a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group, and adjacent groups may be linked to each other to form a ring structure; R 6 and R 11 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group; R 7 and R 10 are the same group and are a hydrogen atom, a hydrocarbon group, or a silicon-containing hydrocarbon group; R 6 and R 7 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 10 and R 11 may be bonded to a hydrocarbon having 2 to 3 carbon atoms to form a ring structure, R 6 , R 7 , R 10and R 11 is not a hydrogen atom at the same time, 13 and R 14 are each independently a hydrogen atom, a hydrocarbon group or a silicon-containing hydrocarbon group, which may be linked together to form a ring structure, Y is a carbon atom or a silicon atom, M is Ti, Zr or Hf, Q is independently a halogen atom, a hydrocarbon group, an anionic ligand or a neutral ligand capable of coordinating to a lone electron pair, and j is an integer of 1 to 4.]. Method (β): A method comprising: a step (S1') of solution polymerizing ethylene and an α-olefin in the presence of a vanadium catalyst comprising a soluble vanadium compound (V) and an organoaluminum compound (Q') to obtain an ethylene / α-olefin copolymer (B0), and a step (S2) of adding the unsaturated monomer to the ethylene / α-olefin copolymer (B0) to graft copolymerize it.

10. The substituent R of the bridged metallocene compound (P) represented by the above formula (1) 13 and R 14 The method according to claim 9 , wherein either or both of the above is an aryl group.

11. The substituent R of the bridged metallocene compound (P) represented by the above formula (1) 13 and R 14 are both aryl groups, and the substituent R 2 and R 3 The method according to claim 9, wherein either one of the above is a saturated hydrocarbon group having 4 carbon atoms.

Citation Information

Patent Citations

  • Double-sided adhesive tape or sheet and method for producing the same

    JP2018048266A

  • Method for producing laminated polyester film

    JP2018184003A

  • Adhesive sheet

    JP2020007545A