Polyphenylene ether-based resin extruded foam particles, method for producing same, and foam molded body

WO2024204201A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/011954
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-03

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
  • Figure JPOXMLDOC01-APPB-T000003
    Figure JPOXMLDOC01-APPB-T000003
Patent Text Reader

Abstract

Provided are: a polyphenylene ether-based resin extruded foam particles having excellent heat resistance and low open cell ratio; a method for producing the same; and a foamed molded body obtained by molding said extruded foam particles. As polyphenylene ether-based extruded foam particles containing, as a base resin, a resin composition that contains a polyphenylene ether-based resin and a polystyrene-based resin, extruded foam particles, which have a glass transition temperature Tg of 130 °C to 165 °C and in which the MFR of the polystyrene-based resin, as measured under conditions of 200 °C and 5 kgf, is at least 15 g / 10 min, are used.
Need to check novelty before this filing date? Find Prior Art

Description

Extruded polyphenylene ether resin foam particles, their production method, and foamed molded articles

[0001] The present invention relates to extruded polyphenylene ether resin beads, a method for producing the same, and a foamed molded article obtained by molding the extruded foamed beads.

[0002] Foamed molded articles obtained by molding expanded resin beads are characterized by their flexibility in shape, excellent shock-absorbing properties, light weight, and thermal insulation properties, and polystyrene-based resin foamed bead molded articles, polypropylene-based resin foamed bead molded articles, etc., are already widely used in the market. Meanwhile, the market continues to demand foamed resin beads with higher performance, necessitating the development of new technologies. For example, there is a demand for foamed resin beads with high heat resistance for use in harsher environments, such as in automotive parts and electrical and electronic products. More specifically, there is a demand for foamed resin beads that exhibit long-term dimensional stability at temperatures even higher than 100°C. It is difficult to meet such demands with resin foams based on the aforementioned polystyrene-based resin or polypropylene-based resin. In other words, there is a need for foamed resin beads using a novel substrate.

[0003] In response to this, many attempts have been made to obtain extruded foams using polyphenylene ether-based resins as a base material. For example, Patent Document 1 discloses an extruded foam sheet containing 10 to 50 mass % of a polyphenylene ether-based resin in a base material. Patent Document 1 describes that the inclusion of a polyphenylene ether-based resin improves the heat resistance of the extruded foam sheet.

[0004] Japanese Patent Application Laid-Open No. 2012-077165

[0005] However, the technology disclosed in Patent Document 1 cannot be directly applied to obtain extruded foamed particles. Polyphenylene ether resins are generally known to have poor fluidity in the molten state. Therefore, as the proportion of polyphenylene ether resin in the substrate increases during extrusion processing, the pressure at the die tends to increase. In extrusion foaming, sufficient cooling to a temperature appropriate for foaming is required to achieve a good foaming state. However, when a resin containing a high proportion of polyphenylene ether resin is used as the substrate, the pressure may increase to a range that is not acceptable for the equipment before sufficient cooling, making it impossible to obtain a foam. This problem can be particularly fatal in the case of extruded foamed particles, which require the use of a die with a fixed cross-sectional opening and therefore cannot adjust the pressure, unlike extruded foamed sheets produced using a circular die, which allows the pressure to be adjusted (reduced) by adjusting the opening of the die. Furthermore, Patent Document 1 produces foamed sheets with a relatively low expansion ratio of approximately 9 times or less, whereas foamed particles are often required to be expanded to a higher expansion ratio of 10 times or more. In this case, since a larger amount of blowing agent is used, the temperature required to obtain a good foaming state tends to be lower, and the pressure problem becomes more serious. Furthermore, when producing a foamed molded article using extruded foamed beads, the extruded foamed beads are also required to have a low open cell ratio in order to ensure excellent moldability.

[0006] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide extruded polyphenylene ether-based resin foamed beads which have excellent heat resistance and a low open cell rate, a method for producing the same, and a foamed molded article obtained by molding the extruded foamed beads.

[0007] The present inventors have found that the above-mentioned problems can be solved by using a polystyrene-based resin having a predetermined or higher MFR and containing a predetermined amount or more of polyphenylene ether-based resin in extruded polyphenylene ether-based resin beads containing a resin composition containing a polyphenylene ether-based resin and a polystyrene-based resin, and have completed the present invention.

[0008] Aspects of the present disclosure relate to the following extruded polyphenylene ether resin foam beads, a production method thereof, and a foam molded article.

[0009] [1] Extruded polyphenylene ether-based resin beads containing a resin composition containing a polyphenylene ether-based resin and a polystyrene-based resin as a base resin, wherein the extruded polyphenylene ether-based resin has a glass transition temperature Tg of 130°C or higher and 165°C or lower, and the polystyrene-based resin has an MFR of 15 g / 10 min or higher, measured at 200°C and 5 kgf. [2] The extruded polyphenylene ether-based resin beads according to [1], wherein the extruded polyphenylene ether-based resin has a glass transition temperature Tg of 135°C or higher and 165°C or lower. [3] The extruded polyphenylene ether-based resin beads according to [1], wherein the extruded polyphenylene ether-based resin has a glass transition temperature Tg of 140°C or higher and 165°C or lower. [4] The extruded foam beads according to any one of [1] to [3], wherein the polyphenylene ether resin is one or more selected from the group consisting of poly(2,6-dimethylphenylene-1,4-ether), poly(2,6-diethylphenylene-1,4-ether), and poly(2,6-dichlorophenylene-1,4-ether). [5] The extruded foam beads according to any one of [1] to [4], wherein the polyphenylene ether resin has a glass transition temperature of 200 to 225°C. [6] The extruded foam beads according to any one of [1] to [5], wherein the polystyrene resin has an MFR of 15 g / 10 min or more and 50 g / 10 min or less, measured at 200°C and 5 kgf. [7] The extruded foam beads according to any one of [1] to [5], wherein the polystyrene resin has an MFR of 20 g / 10 min or more and 50 g / 10 min or less, measured at 200°C and 5 kgf. [8] The extruded foam beads according to any one of [1] to [7], wherein the polystyrene resin is polystyrene. [9] The extruded foam beads according to any one of [1] to [8], wherein the polystyrene resin has a glass transition temperature of 90 to 110°C.

[10] The extruded foam beads according to any one of [1] to [9], wherein the polystyrene resin has a weight average molecular weight of 1,000 to 10,000,000.

[11] The extruded foam beads according to any one of [1] to

[10] , wherein the polystyrene resin has a number average molecular weight of 800 to 10,000,000.

[12] The extruded foam beads according to any one of [1] to

[11] , wherein the content of the polyphenylene ether resin is 30% by weight or more and 70% by weight or less, based on the total amount of the resin composition.

[13] The extruded foam beads according to any one of [1] to

[11] , wherein the content of the polyphenylene ether resin is 40% by weight or more and 70% by weight or less, based on the total amount of the resin composition.

[14] The extruded foam beads according to any one of [1] to

[11] , wherein the content of the polyphenylene ether resin is 50% by weight or more and 70% by weight or less, based on the total amount of the resin composition.

[15] The extruded foam beads according to any one of [1] to

[14] , wherein the content of the polystyrene resin is 30% by weight or more and 70% by weight or less, based on the total amount of the resin composition.

[16] The extruded foam beads according to any one of [1] to

[14] , wherein the content of the polystyrene resin is 30% by weight or more and 60% by weight or less, based on the total amount of the resin composition.

[17] The extruded foam beads according to any one of [1] to

[14] , wherein the content of the polystyrene resin is 30% by weight or more and 50% by weight or less, based on the total amount of the resin composition.

[18] The extruded foam beads according to any one of [1] to

[17] , having an expansion ratio of 10 to 40 times.

[19] The extruded foam beads according to any one of [1] to

[18] , having an open cell ratio of 20% or less.

[20] The extruded foam beads according to any one of [1] to

[18] , having an open cell ratio of 15% or less.

[21] The extruded foam beads according to any one of [1] to

[18] , having an open cell ratio of 10% or less.

[22] The extruded foam beads according to any one of [1] to

[18] , having an open cell ratio of 7% or less.

[23] The extruded foam beads according to any one of [1] to

[22] , having an average cell diameter of 100 μm or more.

[24] The extruded foam beads according to any one of [1] to

[22] , having an average cell diameter of 100 μm or more and 600 μm or less.

[25] A foam-molded article obtained by molding the extruded foam beads according to any one of [1] to

[24] .

[26] A method for producing extruded polyphenylene ether resin beads according to any one of [1] to

[24] , comprising at least the following steps: a melt-kneading step of melt-kneading a resin composition as the base resin and a blowing agent in an extruder to obtain a blowing-agent-containing resin composition; a cooling step of cooling the blowing-agent-containing resin composition; an extrusion-foaming step of extruding the cooled blowing-agent-containing resin composition into an atmosphere having a lower pressure than that inside the extruder to foam it; and a granulation step of cutting the extruded foam to produce extruded foam beads.

[27] The method according to

[26] , wherein the blowing agent is at least one selected from the group consisting of normal butane, isobutane, and carbon dioxide gas.

[28] The method according to

[26] or

[27] , wherein the amount of the blowing agent used is 0.5 to 7.0 parts by weight per 100.0 parts by weight of the resin composition.

[29] The method according to any one of

[26] to

[28] , wherein the low-pressure atmosphere is in a gas phase or a liquid phase.

[0010] According to the present invention, it is possible to provide extruded polyphenylene ether resin beads having excellent heat resistance and a low open cell content, a method for producing the same, and a foamed molded article obtained by molding the extruded foamed beads.

[0011] Extruded Polyphenylene Ether-Based Resin Beads The extruded polyphenylene ether-based resin beads of this embodiment contain a resin composition containing a polyphenylene ether-based resin and a polystyrene-based resin as a base resin. The extruded polyphenylene ether-based resin beads have a glass transition temperature Tg of 130°C or higher and 165°C or lower, and the polystyrene-based resin has an MFR of 20 g / 10 min or higher, measured at 200°C and 5 kgf.

[0012] According to the extruded polyphenylene ether resin beads of this embodiment, it is possible to provide extruded polyphenylene ether resin beads that are excellent in heat resistance and have a low open cell ratio.

[0013] <Base Resin> The base resin contains a resin composition containing a polyphenylene ether-based resin and a polystyrene-based resin, which will be described later, and preferably contains these components as main components. In this embodiment, in an aspect in which these components are the main components, the total amount of the polyphenylene ether-based resin and the polystyrene-based resin relative to the total amount of the resin composition is preferably 80 wt % or more, more preferably 90 wt % or more, and even more preferably 95 wt % or more.

[0014] (Polyphenylene Ether Resin) Polyphenylene ether resins are generally represented by the following general formula.

[0015] In the formula, R 1 and R 2 represents an alkyl group having 1 to 4 carbon atoms or a halogen atom, and n is a positive integer representing the degree of polymerization. The degree of polymerization n is usually 10 to 5000. Examples of polyphenylene ether resins include poly(2,6-dimethylphenylene-1,4-ether), poly(2,6-diethylphenylene-1,4-ether), and poly(2,6-dichlorophenylene-1,4-ether).

[0016] From the viewpoint of achieving excellent heat resistance in the extruded foamed beads, the content of the polyphenylene ether resin is preferably 30% by weight or more and 70% by weight or less, more preferably 40% by weight or more and 70% by weight or less, and even more preferably 50% by weight or more and 70% by weight or less, relative to the total amount of the resin composition.

[0017] The glass transition point of the polyphenylene ether resin is preferably 200 to 225°C, more preferably 205 to 220°C.

[0018] (Polystyrene-based Resin) Examples of polystyrene-based resins include homopolymers of styrene or styrene-based monomers, copolymers containing styrene and / or styrene-based monomers as the main component, etc. Examples of styrene-based monomers include, but are not limited to, o-methylstyrene, m-methylstyrene, p-methylstyrene, t-butylstyrene, α-methylstyrene, β-methylstyrene, diphenylethylene, chlorostyrene, bromostyrene, etc.

[0019] Examples of the homopolymer of styrene or a styrene-based monomer include polystyrene, poly-α-methylstyrene, polychlorostyrene, etc. Examples of the copolymer containing styrene and / or a styrene-based monomer as the main component include styrene-butadiene copolymer, styrene-acrylonitrile copolymer, styrene-maleic acid copolymer, styrene-maleic anhydride copolymer, styrene-maleimide copolymer, styrene-N-phenylmaleimide copolymer, styrene-N-alkylmaleimide copolymer, styrene-N-alkyl-substituted phenylmaleimide copolymer, styrene-acrylic acid copolymer, styrene-methacrylic acid copolymer, styrene-methyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-n-alkyl acrylate copolymer, styrene-n-alkyl methacrylate copolymer, ethylvinylbenzene-divinylbenzene copolymer, terpolymers such as ABS and butadiene-acrylonitrile-α-methylbenzene copolymer, and graft copolymers such as styrene-grafted polyethylene, styrene-grafted ethylene-vinyl acetate copolymer, (styrene-acrylic acid)-grafted polyethylene, and styrene-grafted polyamide. Furthermore, polystyrene resins containing a rubber component such as butadiene may be used as needed. These may be used alone or in combination of two or more.

[0020] The lower limit of the MFR of the polystyrene resin measured under conditions of 200°C and 5 kgf is 15 g / 10 min or more, preferably 20 g / 10 min or more, from the viewpoint of obtaining extruded foamed beads with a low open cell ratio. The upper limit of the MFR of the polystyrene resin measured under conditions of 200°C and 5 kgf is not particularly limited, and is preferably, for example, 50 g / 10 min or less.

[0021] The glass transition point of the polystyrene resin is preferably 90 to 110°C, more preferably 95 to 105°C.

[0022] The weight average molecular weight of the polystyrene resin is preferably 1,000 to 10,000,000, and more preferably 10,000 to 1,000,000.

[0023] The number average molecular weight of the polystyrene resin is preferably 800 to 10,000,000, and more preferably 8,000 to 1,000,000.

[0024] From the viewpoint of providing the extruded foamed beads with excellent heat resistance, the content of the polystyrene-based resin is preferably 30% by weight or more and 70% by weight or less, more preferably 30% by weight or more and 60% by weight or less, and even more preferably 30% by weight or more and 50% by weight or less, relative to the total amount of the resin composition.

[0025] (Other Components) The resin composition of this embodiment may contain components other than the polyphenylene ether-based resin and polystyrene-based resin described above (hereinafter also referred to as "other components"), as long as the effects of the present invention are not impaired. Examples of other components include bubble nucleating agents, (a) stabilizers such as antioxidants, metal deactivators, phosphorus-based processing stabilizers, UV absorbers, UV stabilizers, fluorescent brighteners, metal soaps, and antacid adsorbents, and / or (b) additives such as crosslinkers, chain transfer agents, lubricants, plasticizers, fillers, reinforcing agents, flame retardants, colorants, and antistatic agents. These other components may be used alone or in combination of two or more. The total content of the other components in the resin composition of this embodiment is not particularly limited. The total content of the other components in the resin composition is preferably, for example, 0.01 to 20 parts by weight per 100 parts by weight of the resin composition.

[0026] (Gas nucleating agent) Examples of the gas nucleating agent include a sodium bicarbonate-citric acid mixture, monosodium citrate, talc, calcium carbonate, etc. One type of gas nucleating agent may be used alone, or two or more types may be used in combination.

[0027] The total content of the other components in the resin composition is not particularly limited, and is, for example, preferably 20 parts by weight or less, more preferably 10 parts by weight or less, and even more preferably 5 parts by weight or less, relative to 100 parts by weight of the resin composition.

[0028] <Physical Properties of Extruded Foamed Beads> (Glass Transition Point) From the viewpoint of excellent moldability and heat resistance, the glass transition point Tg of the extruded foamed beads is 130°C or higher and 165°C or lower, preferably 135°C or higher and 165°C or lower, and more preferably 140°C or higher and 165°C or lower.

[0029] (Expansion Ratio) The expansion ratio of the extruded foamed beads is not particularly limited, but is preferably 10 times or more and 40 times or less, and more preferably 12 times or more and 40 times or less.

[0030] (Bulk Density) The bulk density of the extruded foam particles is not particularly limited, but is preferably 15 g / L or more and 100 g / L or less, and more preferably 30 g / L or more and 90 g / L or less. This configuration has the advantage that the foamed molded article obtained using the extruded foam particles can better exhibit characteristics such as shape flexibility, cushioning properties, light weight, and heat insulation properties.

[0031] In this specification, the bulk density of extruded foam beads is calculated by carrying out the following steps (1) to (3) in order: (1) pouring the extruded foam beads into a container with a known volume Vk (L), such as a measuring cylinder, beaker, or bucket, until the container overflows; (2) scraping off the powder surface (top end) of the container, and measuring the weight Wb (g) of the extruded foam beads in the container; (3) calculating the bulk density of the extruded foam beads using the following formula: bulk density (g / L) = weight Wb (g) of foam beads / volume Vk (L) of container

[0032] (Open Cell Ratio) The lower the open cell ratio of the extruded foam beads, the better. The open cell ratio of the extruded foam beads is preferably 20% or less, more preferably 15% or less, even more preferably 10% or less, and even more preferably 7% or less. The lower limit of the open cell ratio of the extruded foam beads is not particularly limited, and is, for example, 0.0% or more. The above configuration has the advantages of (a) the extruded foam beads having excellent moldability because the cells are hardly broken and shrink during molding, and (b) foam molded articles obtained using the extruded foam beads exhibit characteristics such as flexibility in shape, cushioning properties, light weight, compressive strength, and heat insulation.

[0033] In this specification, the open cell ratio of extruded foamed beads is a value determined by measurement using an air-comparison type hydrometer [Tokyo Science Co., Ltd., Model 1000] in accordance with the method described in Procedure C of ASTM D2856-87. Specifically, the open cell ratio of extruded foamed beads is calculated by carrying out the following steps (1) to (3) in order: (1) The volume Vc (cm) of the extruded foamed beads is measured using an air-comparison type hydrometer. 3 (2) Next, the entire amount of the extruded foamed particles after measuring Vc is submerged in ethanol contained in a measuring cylinder; (3) After that, the apparent volume Va (cm 3 ) of the extruded foamed particles is calculated from the amount of rise in the position of the ethanol in the measuring cylinder. 3 (4) The open cell ratio of the extruded foamed beads is calculated using the following formula: Open cell ratio (%) = ((Va - Vc) x 100) / Va. The method for measuring the volume Va is also called the submersion method.

[0034] (Average Cell Diameter) The average cell diameter (also referred to as average cell diameter) of the extruded foamed beads is not particularly limited, but is preferably 100 μm or more, more preferably 100 μm to 600 μm, and more preferably 100 μm to 550 μm. If the average cell diameter of the extruded foamed beads is 100 μm or more, shrinkage of the extruded foamed bead molding tends to be small, and if it is 600 μm or less, the molding cycle during in-mold foam molding tends to be shortened.

[0035] <<Method for Producing Extruded Polyphenylene Ether Resin Foamed Beads>> The method for producing extruded polyphenylene ether resin foamed beads of this embodiment is the same as the method for producing extruded polyphenylene ether resin foamed beads described above, and includes at least the following steps: a melt-kneading step of melt-kneading a resin composition as the base resin with a foaming agent in an extruder to obtain a foaming-agent-containing resin composition; a cooling step of cooling the foaming-agent-containing resin composition; an extrusion-foaming step of extruding the cooled foaming-agent-containing resin composition into an atmosphere having a lower pressure than that inside the extruder to foam it; and a granulation step of cutting the extruded foam to produce extruded foamed beads.

[0036] According to the method for producing extruded polyphenylene ether resin beads of this embodiment, it is possible to obtain extruded polyphenylene ether resin beads that are excellent in heat resistance and have a low open cell rate.

[0037] <Melt-Kneading Step> (Resin Composition) The resin composition used in this step is the same as the embodiment explained in the section <<Extruded Polyphenylene Ether Resin Beads>> above.

[0038] (Blowing Agent) The blowing agent used in the production method of this embodiment is not particularly limited as long as it is a blowing agent commonly used in extrusion foaming. Examples of blowing agents include: (a) (a-1) aliphatic hydrocarbons such as propane, normal butane, isobutane, normal pentane, isopentane, and hexane; (a-2) alicyclic hydrocarbons such as cyclopentane and cyclobutane; (a-3) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether; (a-4) alcohols such as methanol and ethanol; (a-5) inorganic gases such as air, nitrogen, and carbon dioxide; and (a-6) physical blowing agents such as water, and (b) chemical blowing agents including thermal decomposition blowing agents such as sodium bicarbonate, azodicarbonamide, and dinitrosopentamethylenetetramine. Among these, inorganic gases and physical blowing agents are preferred from the standpoint of environmental impact.

[0039] The amount of the foaming agent used is preferably 0.5 parts by weight to 7.0 parts by weight, more preferably 0.5 parts by weight to 6.0 parts by weight, even more preferably 0.5 parts by weight to 5.0 parts by weight, still more preferably 0.5 parts by weight to 4.0 parts by weight, and particularly preferably 0.5 parts by weight to 3.0 parts by weight, relative to 100.0 parts by weight of the resin composition.

[0040] Examples of extruders used for melt-kneading include single-screw extruders and twin-screw extruders, among which twin-screw extruders are preferred because of their excellent melt-kneading properties.

[0041] The cylinder temperature of the extruder is not particularly limited and can be appropriately set depending on the glass transition point of the resin composition used, the type and amount of the blowing agent used, etc., from the viewpoint of sufficiently melt-kneading the resin composition and the blowing agent. For example, the cylinder temperature of the extruder is preferably 200°C or higher and 300°C or lower, and more preferably 220°C or higher and 280°C or lower.

[0042] <Cooling Step> Examples of cooling devices used for cooling include single-screw extruders, static mixers, and melt coolers. A die for extruding the cooled melt-kneaded product is provided at the tip of the cooling device in the extrusion direction of the melt-kneaded product. The temperature of the cooling device is not particularly limited as long as it is a temperature suitable for foaming the resulting melt-kneaded product. For example, the temperature of the cooling device is preferably 150°C or higher and 250°C or lower, and more preferably 160°C or higher and 240°C or lower. The die temperature is not particularly limited as long as it is a temperature suitable for foaming the resulting melt-kneaded product. For example, the die temperature is preferably 150°C or higher and 250°C or lower, and more preferably 160°C or higher and 240°C or lower.

[0043] <Extrusion-Foaming Step> The cooled molten kneaded material is extruded through holes in the die into an atmosphere of lower pressure than that inside the extruder to foam it. The molten kneaded material may be extruded into a gas phase or a liquid phase. The pressure of the low-pressure atmosphere is not particularly limited, but is preferably 5 MPa or less, and more preferably 1 MPa or less. The extruded molten kneaded material immediately begins to foam, and when foaming is completed, an extruded polyphenylene ether resin foam is obtained.

[0044] The low-pressure atmosphere may be a gas phase or a liquid phase, but a gas phase is preferred because expanded beads having a relatively high expansion ratio can be easily obtained. Water or the like may be sprayed onto the expanded beads cut in the gas phase to cool the surface.

[0045] In the manufacturing method of this embodiment, the extruder is connected to the cooling device provided with a die at the tip in the extrusion direction, and the cooled molten mixture is extruded from the die and expanded in a low-pressure region. This device configuration makes it possible to manufacture extruded polyphenylene ether resin foam particles that have excellent moldability when producing foamed molded articles through a simple process.

[0046] <Granulation step> The method for cutting the extruded foam to granulate extruded foam particles is not particularly limited. For example, the extruded foam may be cut along the extrusion direction using a cutter or the like provided next to the die. Through the above steps, extruded polyphenylene ether resin foam particles are obtained.

[0047] <<Foamed Molded Article>> The foamed molded article of this embodiment is obtained by molding the extruded polyphenylene ether-based resin beads described above. The manufacturing method of the foamed molded article includes molding the extruded polyphenylene ether-based resin beads described above. The method for molding the extruded polyphenylene ether-based resin beads is not particularly limited, and for example, a method of molding the expanded beads in a mold is preferred. Specifically, the foamed molded article can be obtained by filling the expanded beads into a mold that can be closed but cannot be sealed, and heating it with steam or the like to mold it. Examples of methods for producing the foamed molded article include (a) a method in which foamed beads are pressurized with an inorganic gas to impregnate the particles with the inorganic gas and apply a predetermined internal particle pressure, followed by filling a mold and heat-fusing with steam or the like (e.g., JP-B-51-22951); (b) a method in which foamed beads are compressed with gas pressure, filled into a mold, and heat-fusing with steam or the like by utilizing the particle's recovery force (e.g., JP-B-53-33996); and (c) a method in which foamed beads are filled into a mold with an expanded gap, the mold is closed to a predetermined gap, the filled foamed beads are compressed, and heat-fusing with steam or the like. In this embodiment, when foamed molded articles are produced using the above methods (a) and (c), the pressure range using steam or the like to obtain a good foamed molded article is widened. In other words, the molding width of the foamed beads is widened.

[0048] The foam molded article of this embodiment is used for automobile parts, electric and electronic products, heat insulating materials for heat pumps, and the like.

[0049] The present invention will be described in more detail below based on examples and comparative examples, but the present invention is not limited to the following examples.

[0050] <Evaluation> The MFR of the polystyrene resins B-1 to B-4 described below was measured according to the following method. The glass transition temperature, expansion ratio, bulk density, and open cell ratio of the extruded foamed particles described below were measured according to the following methods.

[0051] (MFR) In accordance with the provisions of Method B described in ISO 1133 (1997), using a melt indexer S-01 (manufactured by Toyo Seiki Seisakusho) under conditions of 200 ° C. and 5.0 kg, the amount of resin extruded from the die in a certain time was converted to the amount extruded in 10 minutes. Note that the certain time is 120 seconds when the melt flow rate is greater than 0.5 g / 10 min and 1.0 g / 10 min or less; 60 seconds when it is greater than 1.0 g / 10 min and 3.5 g / 10 min or less; and 30 seconds when it is greater than 3.5 g / 10 min and 10 g / 10 min or less.

[0052] (Glass Transition Point) Using a Seiko Instruments Inc. DSC6200 differential scanning calorimeter, the following steps (1) to (3) were carried out. (1) Approximately 10 mg of a measurement sample was heated from 40°C to 230°C at a heating rate of 10°C / min to melt the sample. (2) The temperature of the melted sample was then lowered from 230°C to 40°C at a heating rate of 10°C / min to cool the sample. (3) The sample was then further heated from 40°C to 230°C at a heating rate of 10°C / min. In the DSC curve obtained during the second heating (i.e., at the time of (3)), a tangent was drawn at the inflection point of the DSC curve where endotherm occurred, and the point where the tangent line reached the baseline of the DSC curve before heat generation was determined to be the glass transition point Tg of the resin.

[0053] (Expansion Ratio) The expansion ratio of the expanded beads was determined by measuring the mass w1 (g) of the expanded beads, then submerging them in a measuring cylinder containing ethanol, and measuring the volume v1 (cm) by the amount of rise in the water level in the measuring cylinder (submersion method). 3 ) is measured, and the true specific gravity ρb = w1 / v1 of the expanded beads is calculated, and further, the ratio (ρr / ρb) to the resin density ρr before expansion can be calculated. The resin density ρr before expansion is measured using a resin obtained by melt-kneading a resin with the same composition as the expanded beads in the absence of a blowing agent. After measuring the mass w2 (g) of the resin, it is submerged in a measuring cylinder containing ethanol, and the volume v2 (cm) is calculated by the amount of rise in the water level in the measuring cylinder. 3 ) is measured and calculated as ρr = w2 / v2.

[0054] (Bulk Density) The bulk density of the extruded foamed beads was calculated by carrying out the following steps (1) to (3) in order. (1) The extruded foamed beads were poured into a measuring cup whose internal volume Vk (L) had been accurately measured in advance, until the measuring cup overflowed. (2) The powder surface (top end) of the container was scraped off, and the weight Wb (g) of the extruded foamed beads in the container was measured. (3) The bulk density of the extruded foamed beads was calculated using the following formula: Bulk density (g / L) = Weight of foamed beads Wb (g) / Volume of container Vk (L)

[0055] (Open Cell Ratio) This was calculated according to the method described in Procedure C of ASTM D2856-87 by carrying out the following steps (1) to (3) in order: (1) The volume Vc (cm) of the extruded foam particles was measured using an air comparison type hydrometer. 3 (2) Next, the entire amount of the extruded foamed particles after measuring Vc was submerged in ethanol contained in a measuring cylinder. (3) After that, the apparent volume Va (cm) of the extruded foamed particles was calculated from the amount of rise in the position of the ethanol in the measuring cylinder. 3 (4) The open cell ratio of the extruded foamed beads was calculated using the following formula: Open cell ratio (%) = ((Va - Vc) x 100) / Va

[0056] (Average Cell Diameter) Ten samples were randomly selected from the extruded foamed beads and cut carefully so as not to destroy the cell membrane. The cut surface of each sample was observed under a microscope (Keyence: VHX Digital Microscope), and a line segment equivalent to a length of 1 mm was drawn on the part excluding the surface layer portion. The number of cells through which the line segment passed was counted, and the average cell diameter was then measured in accordance with ASTM D3576.

[0057] [Examples 1 to 7, Comparative Examples 1 to 4] (Materials) In the examples and comparative examples, the following resins A-1 and A-2 were used as polyphenylene ether resins. Resin A-1: ​​EFN4230 (manufactured by Sabic, 70% by weight of polyphenylene ether, 30% by weight of polystyrene resin) Resin A-2: 6390C (manufactured by Sabic, 90% by weight of polyphenylene ether, 10% by weight of polystyrene resin)

[0058] In the examples and comparative examples, the following resins B-1 to B-4 were used as polystyrene resins: Resin B-1: G120 (manufactured by Toyo Styrene Co., Ltd., MFR: 22 g / 10 min) Resin B-2: G100C (manufactured by Toyo Styrene Co., Ltd., MFR: 28 g / 10 min) Resin B-3: G9305 (manufactured by PS Japan Co., Ltd., MFR: 1.5 g / 10 min) Resin B-4: HF77 (manufactured by PS Japan Co., Ltd., MFR: 7.5 g / 10 min)

[0059] (Extruded Foam Beads Production Examples 1-7, Production Comparative Examples 1-4) The extruded foam beads were produced using a twin-screw extruder with a shaft diameter of 15 mm, a melt cooler, a diverter valve, and a die connected in series. The resins shown in Tables 1 and 2 were fed into the twin-screw extruder at 0.5 kg / h and melted at a cylinder temperature of 265°C and a screw rotation speed of 100 rpm. Furthermore, 3.2 parts by weight of carbon dioxide gas (a blowing agent) was fed per 100 parts by weight of the resin composition using a metering pump through an injection port installed midway through the extruder, and the resulting composition was further melt-kneaded. The resulting melt-kneaded mixture was cooled by passing it through a melt cooler connected to the tip of the twin-screw extruder and set to the temperature shown in Tables 1 and 2. The melt-kneaded mixture was then extruded into the atmosphere through a die (φ1.2 mm x 1 hole) attached to the tip of the melt cooler to foam. The extruded foam was cut immediately after extrusion using four cutter blades rotating at 500 rpm (hot-cut method) to obtain expanded beads. The resulting extruded expanded beads were dried in a drying chamber at 75°C for at least 4 hours and then allowed to stand at room temperature for at least 24 hours, after which the bulk density, expansion ratio, and open cell ratio were measured. The results are shown in Tables 1 and 2.

[0060] (Second-Stage Expansion of Expanded Beads) The extruded expanded beads obtained in Production Example 1 were placed in a pressure-resistant vessel and pressurized with air at room temperature at a rate of 0.01 MPa / 10 min until the pressure reached 0.55 MPa (gauge pressure) and maintained at that pressure for a total of 24 hours. After adjusting the internal pressure (absolute pressure) to the value shown in Table 1, the pressurized expanded beads were placed in a pressure-resistant vessel and heated for 30 seconds at the steam pressure shown in Table 1 to obtain second-stage expanded beads. The obtained second-stage expanded beads were dried in a 75°C drying chamber for 1 hour and then allowed to stand at 23°C for at least 24 hours, and the bulk density, expansion ratio, and open cell ratio were measured. The results are shown in Table 1.

[0061]

[0062]

[0063] From Tables 1 and 2, it is clear that when a polystyrene-based resin containing a predetermined amount or more of a polyphenylene ether-based resin and having a predetermined or higher MFR is used, extruded foamed beads having a glass transition temperature Tg of 135°C or higher, excellent heat resistance, and an open cell ratio of 20% or less can be obtained.

Claims

1. Extruded polyphenylene ether resin foam particles containing a resin composition containing a polyphenylene ether resin and a polystyrene resin as a base resin, wherein the glass transition point Tg of the extruded polyphenylene ether resin is 130°C or higher and 165°C or lower, and the MFR of the polystyrene resin measured under conditions of 200°C and 5 kgf is 15 g / 10 min or higher.

2. The extruded foam beads according to claim 1, wherein the glass transition point Tg of the extruded foam beads is 135°C or higher and 165°C or lower.

3. The extruded foam beads according to claim 1, wherein the glass transition point Tg of the extruded foam beads is 140°C or higher and 165°C or lower.

4. The extruded foam beads according to claim 1 or 2, wherein the polystyrene resin has an MFR of 15 g / 10 min or more and 50 g / 10 min or less, measured under conditions of 200° C. and 5 kgf.

5. The extruded foam beads according to claim 1 or 2, wherein the MFR of the polystyrene resin measured under conditions of 200° C. and 5 kgf is 20 g / 10 min or more and 50 g / 10 min or less.

6. The extruded foam beads according to claim 1 or 2, wherein the content of the polyphenylene ether resin is 30% by weight or more and 70% by weight or less based on the total amount of the resin composition.

7. The extruded foam beads according to claim 1 or 2, wherein the content of the polyphenylene ether resin is 40% by weight or more and 70% by weight or less based on the total amount of the resin composition.

8. The extruded foam beads according to claim 1 or 2, wherein the content of the polyphenylene ether resin is 50% by weight or more and 70% by weight or less based on the total amount of the resin composition.

9. The extruded foam particles according to claim 1 or 2, having an expansion ratio of 10 to 40 times.

10. The extruded foam particles according to claim 1 or 2, having an open cell ratio of 20% or less.

11. The extruded foam particles according to claim 1 or 2, having an open cell ratio of 15% or less.

12. The extruded foam particles according to claim 1 or 2, having an open cell ratio of 10% or less.

13. The extruded foam particles according to claim 1 or 2, having an average cell diameter of 100 μm or more.

14. A foamed molded article obtained by molding the extruded foam particles according to claim 1 or 2.

15. A method for producing the extruded polyphenylene ether resin foam particles according to claim 1 or 2, comprising at least the steps of: a melt-kneading step of melt-kneading the resin composition as the base resin with a foaming agent in an extruder to obtain a foaming agent-containing resin composition; a cooling step of cooling the foaming agent-containing resin composition; an extrusion-foaming step of extruding the cooled foaming agent-containing resin composition into an atmosphere having a lower pressure than that inside the extruder to cause foaming; and a granulation step of cutting the extruded foam to produce extruded foam particles.

Citation Information

Patent Citations

  • Preparation method of polyphenyl ether foamable particles

    CN115181319A

  • Low density particle of polyphenylene ether resin

    JP1988150337A

  • Highly expandable and heat- resistance-shaped, stable foaming styrol polymer and its manufacture

    JP1991170537A

  • Polyphenylene ether foam obtained from low-i.v. expandable polyphenylene ether particle

    JP1992122741A