Laminate and packaging bag

The laminate structure with a direct application of polyolefin and polyvinyl alcohol-based gas barrier resin layers on paper, combined with an inorganic vapor-deposited layer and overcoat, addresses the issue of cracking and barrier property deterioration in folded paper-based packaging, ensuring effective water vapor barrier performance and reduced plastic usage.

WO2024204251A1PCT designated stage expired Publication Date: 2024-10-03TOPPAN HOLDINGS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012049
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-30
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Packaging materials made from paper-based laminates with clay coat layers tend to develop cracks when folded, leading to a deterioration in gas barrier properties, particularly in acute fold packaging applications such as pillow, three-sided seal, and gusset packaging, which compromises the water vapor barrier performance.

Method used

A laminate structure comprising a base paper with a gas barrier resin layer made from polyolefin and polyvinyl alcohol-based resins, where the gas barrier resin layer is directly applied to the base paper without a clay coat layer, and includes an inorganic pigment concentrated in one region to enhance flexibility and prevent cracking, along with an inorganic vapor-deposited layer and an overcoat layer for improved barrier properties.

Benefits of technology

The laminate maintains sufficient water vapor barrier properties both initially and after folding, while reducing plastic usage and maintaining excellent recyclability, with improved adhesion and uniformity of the vapor-deposited layer, effectively preventing cracks and ensuring stable barrier performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012049_03102024_PF_FP_ABST
    Figure JP2024012049_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is a laminate comprising base paper and a gas-barrier resin layer disposed on the base paper so as to come into direct contact with the base paper, wherein: a binder resin constituting the gas-barrier resin layer contains at least one component selected from the group consisting of a polyolefin resin and a polyvinyl alcohol-based resin; an inorganic pigment is contained in a first region of the gas-barrier resin layer, the first region lying between the base-paper-side surface of the gas-barrier resin layer and a thickness of 50% of the whole thickness of the gas-barrier resin layer; and 80% by volume or more of the whole amount of the inorganic pigment contained in the gas-barrier resin layer is present in the first region.
Need to check novelty before this filing date? Find Prior Art

Description

Laminate and packaging bag

[0001] The present disclosure relates to a laminate and a packaging bag.

[0002] Packaging materials are used in many fields, including food, beverages, pharmaceuticals, and chemicals, depending on the contents. Packaging materials are required to have gas barrier properties that prevent the permeation of water vapor, which can cause deterioration of the contents.

[0003] In recent years, growing environmental awareness stemming from the problem of marine plastic waste and other issues has led to a growing trend toward a plastic-free society. From the perspective of reducing the amount of plastic used, the use of paper instead of plastic materials has been considered in various fields. For example, Patent Document 1 below discloses a laminate in which a clay coating layer, a resin layer, and a vapor deposition layer are laminated on paper to impart barrier properties. Here, the clay coating layer is provided to seal and smooth the paper.

[0004] Japanese Patent Application Laid-Open No. 2022-104487

[0005] Paper has the characteristic of being easy to process due to its crease-retaining property (also called dead-hold property). However, according to the study by the present inventors, when paper is used to make packaging bags with sharper creases (pillow packaging, three-side seal packaging, and gusset packaging), cracks tend to occur in the clay coat layer and the laminate, which reduces the barrier properties.

[0006] Therefore, an object of the present disclosure is to provide a laminate using paper that has sufficient water vapor barrier properties not only initially but also after being folded, and a packaging bag including the laminate.

[0007] To solve the above problems, the present disclosure provides the following laminates and packaging bags. [1] A laminate comprising base paper and a gas barrier resin layer disposed on the base paper so as to be in direct contact with the base paper, wherein the binder resin constituting the gas barrier resin layer comprises at least one selected from the group consisting of polyolefin resins and polyvinyl alcohol-based resins, and the gas barrier resin layer comprises an inorganic pigment in a first region extending from the surface facing the base paper to 50% of the total thickness of the gas barrier resin layer, with 80% by volume or more of the total amount of the inorganic pigment contained in the gas barrier resin layer being present in the first region. [2] The laminate according to [1] above, which comprises an inorganic vapor deposition layer on the surface of the gas barrier resin layer opposite the base paper. [3] The laminate according to [2] above, which comprises an overcoat layer on the surface of the inorganic vapor deposition layer opposite the gas barrier resin layer. [4] The laminate according to [3] above, wherein the overcoat layer comprises a polyolefin resin. [5] The laminate according to any one of [1] to [4] above, wherein the content of the inorganic pigment in the gas barrier resin layer is 50 parts by volume or less relative to 100 parts by volume of the binder resin. [6] The laminate according to any one of [1] to [5] above, wherein the content of the inorganic pigment in the first region is 2 to 200 parts by volume relative to 100 parts by volume of the binder resin in the first region. [7] The laminate according to any one of [1] to [6] above, wherein the aspect ratio of the inorganic pigment is 1 to 200. [8] The laminate according to any one of [1] to [7] above, wherein 100% by volume of the total amount of the inorganic pigment contained in the gas barrier resin layer is present in the first region. [9] The laminate according to any one of [1] to [8] above, wherein the surface roughness Ra of the surface of the gas barrier resin layer opposite to the base paper is 1.0 μm or less.

[10] The laminate according to any one of [1] to [9] above, wherein the gas barrier resin layer has a thickness of 1 to 20 μm.

[11] The laminate according to any one of [1] to

[10] above, wherein the gas barrier resin layer has a thickness of 3 to 5 μm.

[12] A packaging bag comprising the laminate according to any one of [1] to

[11] above.

[0008] According to the present disclosure, it is possible to provide a laminate using paper that has sufficient water vapor barrier properties not only initially but also after being folded, and a packaging bag including the laminate. Because the laminate uses paper, it has the fold retention characteristic of paper and contributes to reducing the amount of plastic material used.

[0009] 1 is a schematic cross-sectional view showing a laminate according to an embodiment of the present disclosure; 2 is a perspective view showing a packaging bag according to an embodiment of the present disclosure;

[0010] Hereinafter, embodiments of the present disclosure will be described in detail, with reference to the drawings as needed. However, the present disclosure is not limited to the following embodiments.

[0011]

[0023] <Laminate> The laminate according to this embodiment comprises a base paper and a gas barrier resin layer disposed on the base paper so as to be in direct contact with the base paper, wherein the binder resin constituting the gas barrier resin layer comprises at least one selected from the group consisting of polyolefin resins and polyvinyl alcohol-based resins, and the gas barrier resin layer comprises an inorganic pigment in a first region extending from the surface facing the base paper to 50% of the total thickness of the gas barrier resin layer, and 80% by volume or more of the total amount of the inorganic pigment contained in the gas barrier resin layer is present in the first region. The laminate according to this embodiment may comprise an inorganic vapor-deposited layer on the surface of the gas barrier resin layer opposite the base paper, and may further comprise an overcoat layer on the surface of the inorganic vapor-deposited layer opposite the gas barrier resin layer.

[0012] According to the above laminate, the gas barrier resin layer is provided directly on the base paper without a clay coat layer, and the binder resin constituting the gas barrier resin layer contains the above-mentioned specific resin, thereby achieving high flexibility and preventing cracks from occurring in the gas barrier resin layer when folded, thereby maintaining sufficient water vapor barrier properties not only initially but also after folding. Furthermore, by distributing the inorganic pigment unevenly in the first region of the gas barrier resin layer on the base paper side, excessive penetration of the binder resin into the base paper can be prevented, and the inorganic pigment can fulfill the role of filling in unevenness in the paper, thereby forming a smooth gas barrier resin layer with few defects and unevenness. This results in stable water vapor barrier properties. Furthermore, when an inorganic vapor deposition layer is formed on a smooth gas barrier resin layer, a uniform inorganic vapor deposition layer can be formed, further improving water vapor barrier properties.

[0013] 1 is a schematic cross-sectional view showing a laminate according to one embodiment. The laminate 10 according to one embodiment comprises, in this order, a base paper 1, a gas barrier resin layer 2, an inorganic vapor deposition layer 3, and an overcoat layer 4. Each layer will be described below.

[0014] [Base Paper 1] Base paper is paper without a coating layer such as a clay coating layer. The base paper may be paper whose main component is plant-derived pulp. Specific examples of base paper include fine paper, special fine paper, construction paper, kraft paper, and glassine paper.

[0015] The basis weight of the base paper is 20 to 500 g / m 2 , or 30 to 100 g / m 2 The thickness of the base paper may be 20 to 100 μm, 30 to 80 μm, or 40 to 60 μm. When the basis weight or thickness of the base paper is within the above range, the laminate can obtain better water vapor barrier properties not only initially but also after being folded.

[0016] The mass of the base paper is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, based on the mass of the entire laminate. If the mass of the base paper is 50% by mass or more, the amount of plastic material used can be sufficiently reduced, the entire laminate can be said to be made of paper, and the laminate has excellent recyclability.

[0017] [Gas barrier resin layer 2] The gas barrier resin layer is provided on the surface of the base paper so as to be in direct contact with the base paper. The gas barrier resin layer is provided to improve the gas barrier properties of the laminate. The gas barrier resin layer also plays a role in improving the adhesion between the base paper and the inorganic vapor deposition layer described below.

[0018] The binder resin constituting the gas barrier resin layer contains at least one selected from the group consisting of polyolefin resins and polyvinyl alcohol-based resins. By using these binder resins, the gas barrier resin layer can obtain good water vapor barrier properties, as well as high flexibility, and can suppress the occurrence of cracks in the gas barrier resin layer when bent, thereby maintaining sufficient water vapor barrier properties not only initially but also after bending. Furthermore, when a polyvinyl alcohol-based resin is used as the binder resin, good oxygen barrier properties can also be obtained both initially and after bending.

[0019] Examples of polyolefin resins include low density polyethylene, medium density polyethylene, high density polyethylene, ethylene-α-olefin copolymer, homopolypropylene, block polypropylene, random polypropylene, and propylene-α-olefin copolymer.

[0020] The polyolefin resin may be a polyolefin resin having a polar group. When a polyolefin resin having a polar group is used, the presence of the polar group can further improve the adhesion between the gas barrier resin layer and the inorganic vapor deposition layer.

[0021] The polyolefin having a polar group may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic acid ester.

[0022] As the polyolefin having a polar group, a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group such as acrylic acid, methacrylic acid, or maleic anhydride) or an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound may be used, or a copolymer of ethylene or propylene with vinyl acetate, an epoxy compound, a chlorine compound, a urethane compound, a polyamide compound, or the like may also be used.

[0023] Specific examples of polyolefins having a polar group include copolymers of acrylic ester and maleic anhydride, ethylene-vinyl acetate copolymers, and ethylene-glycidyl methacrylate copolymers.

[0024] The polyvinyl alcohol-based resin is a resin containing vinyl alcohol as a constituent unit. The polyvinyl alcohol-based resin may be any resin having vinyl alcohol units formed by saponifying vinyl ester units, and examples thereof include polyvinyl alcohol resin (PVA) and ethylene-vinyl alcohol copolymer (EVOH).

[0025] When the gas barrier resin layer contains a polyvinyl alcohol-based resin, the polyvinyl alcohol-based resin has polar groups (hydroxyl groups), which easily bond with the inorganic vapor deposition layer, thereby improving the adhesion between the gas barrier resin layer and the inorganic vapor deposition layer. Furthermore, a gas barrier resin layer containing a polyvinyl alcohol-based resin has excellent flexibility, can prevent cracks from occurring in the gas barrier resin layer when bent, and can maintain sufficient water vapor barrier properties not only initially but also after bending. Furthermore, when the gas barrier resin layer contains a polyvinyl alcohol-based resin, the oxygen barrier properties of the laminate can be improved.

[0026] Examples of PVA include resins obtained by homopolymerizing vinyl esters such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, and vinyl versatate, followed by saponification. The PVA may also be a modified PVA that has been copolymerized or post-modified. The modified PVA can be obtained, for example, by copolymerizing a vinyl ester with an unsaturated monomer copolymerizable with the vinyl ester, followed by saponification. Examples of unsaturated monomers copolymerizable with vinyl esters include olefins such as ethylene, propylene, isobutylene, α-octene, α-dodecene, and α-octadecene; hydroxy group-containing α-olefins such as 3-buten-1-ol, 4-pentyn-1-ol, and 5-hexen-1-ol; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, maleic anhydride, itaconic acid, and undecylenic acid; nitriles such as acrylonitrile and methacrylonitrile; diacetone acrylamide, acrylic acid, and the like. olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid; vinyl compounds such as alkyl vinyl ethers, dimethyl allyl vinyl ketone, N-vinyl pyrrolidone, vinyl chloride, vinyl ethylene carbonate, 2,2-dialkyl-4-vinyl-1,3-dioxane, glycerin monoallyl ether, and 3,4-diacetoxy-1-butene; vinylidene chloride, 1,4-diacetoxy-2-butene, and vinylene carbonate.

[0027] The degree of polymerization of the PVA may be 300 to 3000. When the degree of polymerization is 300 or more, the barrier property is likely to be improved, and when it is 3000 or less, a decrease in coatability due to an increase in viscosity is likely to be suppressed. From the viewpoint of barrier property, the saponification degree of the PVA may be 50 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. Furthermore, the saponification degree of the PVA may be 100 mol% or less, or 99.9 mol% or less. The polymerization degree and saponification degree of the PVA can be measured in accordance with the method described in JIS K 6726 (1994).

[0028] EVOH is generally obtained by saponifying a copolymer of ethylene and an acid vinyl ester such as vinyl acetate, vinyl formate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl pivalate, or vinyl versatate.

[0029] The degree of polymerization of EVOH is preferably 300 to 3000. If the degree of polymerization is less than 300, the barrier property is likely to decrease, and if it exceeds 3000, the viscosity is too high and the coatability is likely to decrease. From the viewpoint of barrier property, the saponification degree of the vinyl ester component of EVOH may be 50 mol% or more, 80 mol% or more, 90 mol% or more, 95 mol% or more, or 99 mol% or more. The saponification degree of EVOH may be 100 mol% or less. The saponification degree of EVOH can be measured by nuclear magnetic resonance ( 1 H-NMR measurement is performed, and the peak area of ​​the hydrogen atoms contained in the vinyl ester structure and the peak area of ​​the hydrogen atoms contained in the vinyl alcohol structure are used to determine the peak area.

[0030] The ethylene unit content of EVOH may be 10 mol% or more, 15 mol% or more, 20 mol% or more, or 25 mol% or more. The ethylene unit content of EVOH may be 65 mol% or less, 55 mol% or less, or 50 mol% or less. When the ethylene unit content is 10 mol% or more, the gas barrier property or dimensional stability can be maintained well under high humidity. On the other hand, when the ethylene unit content is 65 mol% or less, the gas barrier property can be improved. The ethylene unit content of EVOH can be determined by NMR.

[0031] The binder resin constituting the gas barrier resin layer may contain a resin other than polyolefin resin and polyvinyl alcohol-based resin, such as polyacrylic resin, polyester resin, polyurethane resin, polycarbonate resin, polyurea resin, polyamide resin, polyimide resin, melamine resin, and phenol resin.

[0032] The resin composition constituting the binder resin may be the same throughout the gas barrier resin layer, which provides high flexibility throughout the gas barrier resin layer, prevents cracks caused by differences in resin composition within the gas barrier resin layer, and more sufficiently suppresses deterioration of the water vapor barrier property after bending.

[0033] In the gas barrier resin layer, the total content of the polyolefin resin and the polyvinyl alcohol-based resin based on the total amount of the binder resin may be 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass. When the total content of the polyolefin resin and the polyvinyl alcohol-based resin is within the above range, the gas barrier resin layer can have high water vapor barrier properties and high flexibility, and can have excellent water vapor barrier properties both initially and after bending.

[0034] The gas barrier resin layer contains an inorganic pigment 5. As shown in Figure 1, the inorganic pigment 5 is contained in a first region A1 that extends from the surface of the gas barrier resin layer 2 on the base paper 1 side to a thickness (D / 2) that is 50% of the total thickness D of the gas barrier resin layer. 80% by volume or more of the total amount of the inorganic pigment 5 in the gas barrier resin layer 2 is present in the first region A1.

[0035]

[0003] By incorporating an inorganic pigment into the gas barrier resin layer so as to satisfy the above conditions, it is possible to prevent the binder resin from excessively penetrating into the base paper, and the inorganic pigment can fulfill the role of filling in irregularities in the paper, thereby forming a smooth gas barrier resin layer with few defects and irregularities. This allows for stable water vapor barrier properties to be obtained. Furthermore, when an inorganic vapor deposition layer is formed on a smooth gas barrier resin layer, a uniform inorganic vapor deposition layer can be formed, making it possible to further improve the water vapor barrier properties.

[0036] Examples of inorganic pigments include clay, kaolin, calcium carbonate, talc, mica, etc. These may be used alone or in combination of two or more.

[0037] The average particle size of the inorganic pigment may be 0.1 to 10 μm, or 0.1 to 5 μm, from the viewpoints of coating suitability, more sufficiently suppressing the occurrence of cracks in the gas barrier resin layer originating from the inorganic pigment when the layer is bent, and further smoothing the surface of the gas barrier resin layer. The average particle size is the volume-based median diameter (d50) measured by laser diffraction / scattering particle size distribution measurement.

[0038] From the viewpoints of coating suitability, more sufficiently suppressing the occurrence of cracks in the gas barrier resin layer originating from the inorganic pigment when folded, and further smoothing the surface of the gas barrier resin layer, the aspect ratio of the inorganic pigment may be 1 to 200, or may be 5 to 200. The aspect ratio can be measured by electron microscope observation, X-ray diffraction measurement, or the like.

[0039] The content of the inorganic pigment in the gas barrier resin layer may be 50 parts by volume or less, 1 to 45 parts by volume, 3 to 40 parts by volume, or 5 to 35 parts by volume relative to 100 parts by volume of the binder resin. When the content is 50 parts by volume or less, there is a tendency that the occurrence of cracks in the gas barrier resin layer when folded can be more sufficiently prevented, and when the content is 1 part by volume or more, there is a tendency that the binder resin can be more effectively prevented from penetrating excessively into the base paper, and the inorganic pigment can more effectively fulfill its role of filling in irregularities in the paper, resulting in the formation of a smooth gas barrier resin layer with fewer defects and irregularities.

[0040] The content of the inorganic pigment in the first region of the gas barrier resin layer may be 2 to 200 parts by volume, 5 to 150 parts by volume, or 10 to 125 parts by volume, relative to 100 parts by volume of the binder resin in the first region. If the content is 200 parts by volume or less, there is a tendency that the occurrence of cracks in the gas barrier resin layer when folded can be more sufficiently prevented, and if the content is 2 parts by volume or more, there is a tendency that the binder resin can be more sufficiently prevented from penetrating excessively into the base paper, and the inorganic pigment can more sufficiently fulfill its role of filling in unevenness in the paper, and a smooth gas barrier resin layer with fewer defects and unevenness can be formed.

[0041] In the gas barrier resin layer, 80 volume % or more of the total amount of inorganic pigment is present in the first region, but 90 volume % or more of the total amount of inorganic pigment may be present in the first region, 95 volume % or more may be present in the first region, 99 volume % or more may be present in the first region, or 100 volume % may be present in the first region. Having all or most of the inorganic pigment present in the first region as described above prevents excessive penetration of the binder resin into the base paper, and allows the inorganic pigment to fulfill its role of filling in irregularities in the paper, resulting in the formation of a smooth gas barrier resin layer with few defects and irregularities. Furthermore, the region other than the first region, i.e., the region on the inorganic vapor deposition layer side of the gas barrier resin layer, has a low inorganic pigment content or is absent, which more satisfactorily achieves the effects of further enhancing the smoothness of the surface on the inorganic vapor deposition layer side of the gas barrier resin layer, further enhancing the adhesion between the gas barrier resin layer and the inorganic vapor deposition layer, and more fully suppressing the occurrence of cracks in the gas barrier resin layer or the inorganic vapor deposition layer, which would otherwise cause a decrease in barrier properties, when the gas barrier resin layer is bent. Whether or not 80% by volume or more of the total amount of inorganic pigment in the gas barrier resin layer is present in the first region can be determined, for example, by observing a cross section of the gas barrier resin layer with an electron microscope, or from the method for forming the gas barrier resin layer and the composition of the coating liquid used.

[0042] When the inorganic pigment is present only in a partial region of the gas barrier resin layer, the thickness of the region where the inorganic pigment is present may be 0.1 to 50%, 1 to 40%, or 10 to 40% of the total thickness of the gas barrier resin layer. When this thickness ratio is equal to or greater than the lower limit, the sealing effect tends to be enhanced.

[0043] The thickness of the gas barrier resin layer may be, for example, 1 to 20 μm, 2 to 10 μm, 3 to 8 μm, 3 to 5 μm, or 3 to 4 μm. If the thickness of the gas barrier resin layer is 1 μm or more, irregularities on the base paper surface can be more efficiently filled, allowing the inorganic vapor deposition layer described below to be laminated more smoothly and uniformly, resulting in better barrier properties. Furthermore, if the thickness of the gas barrier resin layer is 20 μm or less, it is suitable for coating and the resin ratio can be reduced, making it suitable from the perspective of recycling.

[0044] The gas barrier resin layer may contain components other than the above-mentioned binder resin and inorganic pigment, such as a silane coupling agent and an organic titanate.

[0045] One method for providing a gas barrier resin layer is to coat a base paper with a coating liquid containing a binder resin and an inorganic pigment, and then coat a coating liquid containing the binder resin but not the inorganic pigment. By coating two types of coating liquids, one with an inorganic pigment and the other with an inorganic pigment, it is possible to form a gas barrier resin layer in which the base paper side contains the inorganic pigment and the inorganic vapor deposition layer side does not contain the inorganic pigment. By forming the gas barrier resin layer by the above method, the gas barrier resin layer may have a two-layer structure consisting of a layer containing an inorganic pigment and a layer not containing an inorganic pigment.

[0046] Examples of solvents used in the coating liquid include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination of two or more. Among these, from the viewpoint of properties, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.

[0047] The coating method is not particularly limited, but examples thereof include direct gravure coating, reverse coating, air knife coating, and blade coating.

[0048] After the two types of coating liquids are applied, a smoothing treatment such as calendaring may be carried out to smooth the surface of the gas barrier resin layer.

[0049] The surface roughness Ra of the gas barrier resin layer on the side opposite the base paper (the inorganic vapor deposition layer side) may be 1.0 μm or less. A surface roughness Ra of 1.0 μm or less allows the inorganic vapor deposition layer to be formed more uniformly on the gas barrier resin layer, and provides better water vapor barrier properties both initially and after folding. The surface roughness Ra of the gas barrier resin layer can be measured using a surface roughness measuring device.

[0050] [Inorganic vapor deposition layer 3] Examples of materials constituting the inorganic vapor deposition layer include metals such as aluminum, and inorganic oxides such as aluminum oxide, silicon oxide, magnesium oxide, and tin oxide. From the viewpoints of transparency and barrier properties, the inorganic oxide may be selected from the group consisting of aluminum oxide, silicon oxide, and magnesium oxide. Furthermore, from the viewpoint of excellent tensile stretchability during processing, the inorganic vapor deposition layer may be a layer using aluminum or silicon oxide. By using an inorganic vapor deposition layer, high barrier properties can be obtained with a very thin layer that does not affect the recyclability of the laminate.

[0051] The thickness of the inorganic vapor deposition layer may be appropriately set depending on the intended use, but is preferably 10 to 300 nm, more preferably 20 to 100 nm, and even more preferably 30 to 100 nm. By setting the thickness of the inorganic vapor deposition layer to 10 nm or more, sufficient continuity of the inorganic vapor deposition layer is easily ensured, and by setting the thickness to 300 nm or less, the occurrence of curling and cracking can be sufficiently suppressed, making it easy to achieve sufficient gas barrier performance and flexibility. Furthermore, by setting the thickness of the inorganic vapor deposition layer to 20 nm or more and 100 nm or less, the inorganic vapor deposition layer becomes less likely to crack, and sufficient water vapor barrier properties can be obtained even after bending.

[0052] From the viewpoint of water vapor barrier properties and film uniformity, it is preferable to form the inorganic vapor deposition layer by a vacuum film formation method. There are known film formation methods such as vacuum deposition, sputtering, and chemical vapor deposition (CVD), but vacuum deposition is preferred because of its high film formation rate and high productivity. Among vacuum deposition methods, electron beam heating is particularly effective because it allows for easy control of the film formation rate by the irradiation area and electron beam current, and allows for rapid heating and cooling of the deposition material.

[0053] [Overcoat Layer 4] The overcoat layer is provided on the surface of the inorganic vapor deposition layer so as to be in contact with the inorganic vapor deposition layer. The overcoat layer may contain a polyolefin having a polar group.

[0054] The polyolefin having a polar group may have at least one selected from a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic acid ester.

[0055] As the polyolefin having a polar group, a copolymer of ethylene or propylene with an unsaturated carboxylic acid (an unsaturated compound having a carboxyl group such as acrylic acid or methacrylic acid) or an unsaturated carboxylic acid ester, or a salt of a carboxylic acid neutralized with a basic compound may be used, or a copolymer of ethylene or propylene with vinyl acetate, an epoxy compound, a chlorine compound, a urethane compound, a polyamide compound, or the like may also be used.

[0056] Specific examples of polyolefins having a polar group include copolymers of acrylic ester and maleic anhydride, ethylene-vinyl acetate copolymers, and ethylene-glycidyl methacrylate copolymers.

[0057] By including a polyolefin having a polar group, the overcoat layer has excellent flexibility, can suppress cracking of the inorganic vapor deposition layer after bending (folding), and has excellent adhesion to the inorganic vapor deposition layer. Furthermore, by including the polyolefin having the above-mentioned polar group, it is possible to form a dense film due to the crystallinity of the polyolefin, and water vapor barrier properties are exhibited. Furthermore, the presence of a polar group enables adhesion to the inorganic vapor deposition layer to be exhibited. Furthermore, by including the polyolefin having the above-mentioned polar group, the overcoat layer can also function as a heat seal layer, so a separate heat seal layer is not necessary.

[0058] The overcoat layer may contain other components in addition to the polyolefin having a polar group, such as a silane coupling agent, organic titanate, polyacrylic, polyester, polyurethane, polycarbonate, polyurea, polyamide, polyolefin emulsion, polyimide, melamine, and phenol.

[0059] The content of the polyolefin having a polar group in the overcoat layer may be, for example, 50% by mass or more, 70% by mass or more, 90% by mass or more, or 100% by mass.

[0060] The thickness of the overcoat layer may be, for example, 0.05 μm or more, 0.5 μm or more, 1 μm or more, 2 μm or more, 20 μm or less, 10 μm or less, or 5 μm or less. When the thickness of the overcoat layer is 0.05 μm or more, it can fully fulfill its role as the heat seal layer described above. Furthermore, when the thickness of the overcoat layer is 20 μm or less, it can fully exert adhesion to the inorganic vapor deposition layer and barrier properties while suppressing costs. Furthermore, by setting the thickness of the overcoat layer to 2 μm or more and 10 μm or less, the inorganic vapor deposition layer becomes less likely to crack, and sufficient water vapor barrier properties can be obtained even after bending.

[0061] In the laminate, when the overcoat layer contains a polyolefin having a polar group, the thickness of the overcoat layer is set to 2 μm or more and 10 μm or less, and the thickness of the inorganic vapor deposition layer is set to 20 nm or more and 100 nm or less, the inorganic vapor deposition layer is less likely to crack, and the effect of being able to obtain sufficient water vapor barrier properties even after bending is particularly remarkable.

[0062] Examples of solvents contained in the coating liquid for the overcoat layer include water, methyl alcohol, ethyl alcohol, isopropyl alcohol, n-propyl alcohol, n-butyl alcohol, n-pentyl alcohol, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, toluene, hexane, heptane, cyclohexane, acetone, methyl ethyl ketone, diethyl ether, dioxane, tetrahydrofuran, ethyl acetate, and butyl acetate. These solvents may be used alone or in combination. Among these, from the viewpoint of properties, methyl alcohol, ethyl alcohol, isopropyl alcohol, toluene, ethyl acetate, methyl ethyl ketone, and water are preferred. Furthermore, from the viewpoint of the environment, methyl alcohol, ethyl alcohol, isopropyl alcohol, and water are preferred.

[0063] The overcoat layer can be provided by applying a coating liquid containing the above-mentioned polar group-containing polyolefin and a solvent, etc., onto the inorganic vapor deposition layer and drying it. The melting point of the polar group-containing polyolefin in the coating liquid is preferably 70 to 160°C, more preferably 80 to 120°C. A low melting point of the polar group-containing polyolefin has the advantage of lowering the heat-sealing start-up temperature. A high melting point of the polar group-containing polyolefin increases the risk of blocking in high-temperature environments. To prevent blocking, a larger particle size is preferable so as to reduce the contact area. While not particularly limited, the particle size may be 1 nm or more, 0.1 μm or more, or 1 μm or less, 0.7 μm or less, or 0.5 μm or less.

[0064] The thickness of the laminate including the above layers may be 20 to 150 μm, 30 to 100 μm, or 40 to 90 μm. When the thickness of the laminate is within the above range, the laminate can achieve better water vapor barrier properties not only initially but also after being folded.

[0065] <Packaging Bag> Figure 2 is a perspective view showing a gusset bag 20 made of the laminate 10. A packaging bag is produced by sealing the opening at the top of the gusset bag 20. The gusset bag 20 has portions where the laminate 10 is folded (folded portions B1, B2). The folded portion B1 is a portion where the laminate 10 is folded in a valley direction when viewed from the innermost layer side, while the folded portion B2 is a portion where the laminate 10 is folded in a mountain direction when viewed from the innermost layer side.

[0066] The packaging bag may be formed into a bag shape by folding one laminate in half so that the overcoat layers face each other, then folding it appropriately into the desired shape and heat sealing it, or may be formed into a bag shape by stacking two laminates so that the overcoat layers face each other and then heat sealing it.

[0067] In the packaging bag according to the present embodiment, the heat seal strength may be 2 N or more, or may be 4 N or more. The upper limit of the heat seal strength is not particularly limited, but may be, for example, 10 N or less.

[0068] The packaging bag can contain contents such as food, medicine, etc. It is particularly suitable for containing food such as sweets. The packaging bag according to this embodiment can maintain high gas barrier properties even when it has a shape with a folded portion.

[0069] In this embodiment, a gusset bag is given as an example of a packaging bag, but the laminate according to this embodiment may be used to produce, for example, a pillow bag, a three-side sealed bag, or a standing pouch.

[0070] The present disclosure will be described in more detail below with reference to examples, but the present disclosure is not limited to these examples.

[0071] [Example 1] <Preparation of first coating liquid> 50 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of a fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content concentration: 10 mass %, solvent: water) to prepare a first coating liquid.

[0072] <Preparation of Second Coating Liquid> A fully saponified polyvinyl alcohol resin with a degree of polymerization of 500 (solid content: 10% by mass, solvent: water) was prepared as a second coating liquid.

[0073] <Preparation of laminate> Base paper with a basis weight of 50 g / m 2The first coating liquid was applied to a piece of kraft paper using a bar coater so that the thickness after calendering (described below) would be 1 μm, and the paper was then dried in an oven to form a first layer. Next, the second coating liquid was applied to the first layer using a bar coater so that the thickness after calendering (described below) would be 3 μm, and the paper was then dried in an oven to form a second layer. The first and second layers were then compressed and the surface of the second layer was smoothed by calendering, resulting in a gas barrier resin layer consisting of the first and second layers and having a total thickness of 4 μm. The content of the inorganic pigment in the entire gas barrier resin layer was 9.1 parts by volume per 100 parts by volume of resin. Furthermore, the proportion of the inorganic pigment present in the first region of the total amount of inorganic pigment in the gas barrier resin layer was 100% by volume.

[0074] Next, aluminum was vapor-deposited on the gas barrier resin layer by vacuum deposition to form a 50 nm thick aluminum vapor-deposited layer. Next, an aqueous dispersion of a polyolefin resin containing a carboxyl group salt (manufactured by Mitsui Chemicals, Inc., product name: Chemipearl S500, solid content: 20 mass %, solvent: a mixed solvent of water / IPA = 8 / 2 (mass ratio)) was applied to the aluminum vapor-deposited layer using a bar coater and dried in an oven to form a 3 μm thick overcoat layer. This resulted in a laminate.

[0075] [Example 2] <Preparation of first coating liquid> 200 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of a fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content concentration: 10 mass%, solvent: water) to prepare a first coating liquid.

[0076] <Preparation of Second Coating Liquid> A fully saponified polyvinyl alcohol resin with a degree of polymerization of 500 (solid content: 10% by mass, solvent: water) was prepared as a second coating liquid.

[0077] <Preparation of laminate> Base paper with a basis weight of 50 g / m 2The first coating liquid was applied to a piece of kraft paper using a bar coater so that the thickness after calendering (described below) would be 1.5 μm, and the resulting coating was dried in an oven to form a first layer. Next, the second coating liquid was applied to the first layer using a bar coater so that the thickness after calendering (described below) would be 2.5 μm, and the resulting coating was dried in an oven to form a second layer. The first and second layers were then compressed and the surface of the second layer was smoothed by calendering, resulting in a gas barrier resin layer consisting of the first and second layers and having a total thickness of 4 μm. The content of the inorganic pigment in the entire gas barrier resin layer was 33.3 parts by volume relative to 100 parts by volume of resin. Furthermore, the proportion of the inorganic pigment present in the first region of the total amount of inorganic pigment in the gas barrier resin layer was 100% by volume. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0078] Example 3 Preparation of First Coating Fluid A first coating fluid was prepared by adding and mixing 50 parts by volume of kaolin to 100 parts by volume (volume of solid content) of an ethylene-vinyl alcohol copolymer resin having an ethylene content of 29 mol% (solid content concentration: 10% by mass, solvent: a mixed solvent of water / IPA=1 / 1 (mass ratio)).

[0079] <Preparation of Second Coating Fluid> An ethylene-vinyl alcohol copolymer resin having an ethylene content of 29 mol% (solid content concentration: 10% by mass, solvent: mixed solvent of water / IPA=1 / 1 (mass ratio)) was prepared as a second coating fluid.

[0080] <Preparation of Laminate> A laminate was prepared in the same manner as in Example 1, except that the first coating liquid and second coating liquid were used.

[0081] [Example 4] <Preparation of first coating liquid> 50 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of a polyvinyl alcohol resin (solid content concentration: 10 mass %, solvent: water) having a degree of polymerization of 500 and a degree of saponification of 85 mol % to prepare a first coating liquid.

[0082] <Preparation of Second Coating Fluid> A polyvinyl alcohol resin (solid content: 10% by mass, solvent: water) having a degree of polymerization of 500 and a degree of saponification of 85 mol% was prepared as a second coating fluid.

[0083] <Preparation of Laminate> A laminate was prepared in the same manner as in Example 1, except that the first coating liquid and second coating liquid were used.

[0084] Example 5 Preparation of First Coating Liquid A first coating liquid was prepared by adding 50 parts by volume of kaolin to 100 parts by volume (volume of solid content) of an aqueous dispersion of a polyolefin resin containing a salt of a carboxyl group (manufactured by Mitsui Chemicals, Inc., product name: Chemipearl S500, solid content concentration: 20 mass %, solvent: mixed solvent of water / IPA = 8 / 2 (mass ratio)).

[0085] <Preparation of second coating liquid> An aqueous dispersion of a polyolefin resin containing a salt of a carboxyl group (manufactured by Mitsui Chemicals, Inc., product name: Chemipearl S500, solid content concentration: 20 mass %, solvent: mixed solvent of water / IPA = 8 / 2 (mass ratio)) was prepared as a second coating liquid.

[0086] <Preparation of Laminate> A laminate was prepared in the same manner as in Example 1, except that the first coating liquid and second coating liquid were used.

[0087] [Example 6] <Preparation of first coating liquid> 50 parts by volume of talc was added to and mixed with 100 parts by volume (volume of solid content) of a fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content concentration: 10% by mass, solvent: water) to prepare a first coating liquid.

[0088] <Preparation of Second Coating Liquid> A fully saponified polyvinyl alcohol resin with a degree of polymerization of 500 (solid content: 10% by mass, solvent: water) was prepared as a second coating liquid.

[0089] <Preparation of Laminate> A laminate was prepared in the same manner as in Example 1, except that the first coating liquid and second coating liquid were used.

[0090] [Comparative Example 1] <Preparation of Laminate> A clay-coated sheet (thickness: 5 μm) having a basis weight of 60 g / m 2A water dispersion of polyurethane resin (manufactured by Mitsui Chemicals, Inc., product name: Takelac XWPB-LJ4, solids concentration: 20 mass%, solvent: mixed solvent of IPA = 8 / 2 (mass ratio)) was applied using a bar coater onto the clay coat layer of the clay-coated paper in such a way that the thickness after drying would be 3 μm, and the coating was dried in an oven to form a gas barrier resin layer. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0091] [Comparative Example 2] <Preparation of first coating liquid> 200 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of a fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content concentration: 10 mass%, solvent: water) to prepare a first coating liquid.

[0092] <Preparation of Second Coating Liquid> A fully saponified polyvinyl alcohol resin with a degree of polymerization of 500 (solid content: 10% by mass, solvent: water) was prepared as a second coating liquid.

[0093] <Preparation of laminate> Base paper with a basis weight of 50 g / m 2 The first coating liquid was applied to a piece of kraft paper using a bar coater so that the thickness after calendering (described below) would be 3 μm, and the resulting coating was dried in an oven to form a first layer. Next, the second coating liquid was applied to the first layer using a bar coater so that the thickness after calendering (described below) would be 1 μm, and the resulting coating was dried in an oven to form a second layer. The first and second layers were then compressed and the surface of the second layer was smoothed by calendering, resulting in a gas barrier resin layer consisting of the first and second layers and having a total thickness of 4 μm. The content of the inorganic pigment in the entire gas barrier resin layer was 100 parts by volume relative to 100 parts by volume of the resin. Furthermore, the proportion of the inorganic pigment present in the first region of the total amount of inorganic pigment in the gas barrier resin layer was 67% by volume. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0094] [Comparative Example 3] <Preparation of laminate> Base paper with a basis weight of 60 g / m 2A fully saponified polyvinyl alcohol resin (solid content: 10% by mass, solvent: water) having a degree of polymerization of 500 was applied to a sheet of glassine paper using a bar coater so that the thickness after drying would be 3 μm, and the coated sheet was then dried in an oven to form a gas barrier resin layer. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0095] Comparative Example 4 Preparation of First Coating Liquid 50 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of a fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content concentration: 10% by mass, solvent: water) to prepare a first coating liquid.

[0096] <Preparation of laminate> Base paper with a basis weight of 50 g / m 2 The first coating liquid was applied to a sheet of kraft paper using a bar coater to a dry thickness of 4 μm, and then dried in an oven to form a gas barrier resin layer. The content of the inorganic pigment in the entire gas barrier resin layer was 50 parts by volume per 100 parts by volume of resin. The proportion of the inorganic pigment present in the first region of the total amount of inorganic pigment in the gas barrier resin layer was 50% by volume. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0097] [Comparative Example 5] <Preparation of Laminate> Base paper with a basis weight of 50 g / m 2 A fully saponified polyvinyl alcohol resin having a degree of polymerization of 500 (solid content: 10% by mass, solvent: water) was applied to a sheet of kraft paper using a bar coater so that the thickness after drying would be 4 μm, and the coated sheet was then dried in an oven to form a gas barrier resin layer. Next, an aluminum vapor deposition layer and an overcoat layer were formed on the gas barrier resin layer in the same manner as in Example 1, to obtain a laminate.

[0098] Comparative Example 6 Preparation of First Coating Liquid 50 parts by volume of kaolin were added to and mixed with 100 parts by volume (volume of solid content) of an aqueous dispersion of a polyurethane resin (manufactured by Mitsui Chemicals, Inc., product name: Takelac XWPB-LJ4, solid content concentration: 20 mass %, solvent: a mixed solvent of IPA=8 / 2 (mass ratio)) to prepare a first coating liquid.

[0099] <Preparation of Second Coating Liquid> An aqueous dispersion of polyurethane resin (manufactured by Mitsui Chemicals, Inc., product name: Takelac XWPB-LJ4, solid content concentration: 20 mass %, solvent: a mixed solvent of IPA = 8 / 2 (mass ratio)) was prepared as a second coating liquid.

[0100] <Preparation of Laminate> A laminate was prepared in the same manner as in Example 1, except that the first coating liquid and second coating liquid were used.

[0101] [Measurement of surface roughness Ra] The surface roughness (Ra) of the gas barrier resin layer obtained in the examples and comparative examples on the side opposite to the paper substrate was measured using a surface roughness measuring instrument (manufactured by Tokyo Seimitsu Co., Ltd., product name: Surfcom 130A). The measurement conditions were as follows. The results are shown in Tables 1 and 2. (Measurement conditions) Evaluation length: 40 mm Measurement range: ±400 μm Measurement speed: 0.3 mm / s Tilt correction: linear Cutoff value: 0.8 mm Cutoff ratio: 300 Filter type: Gaussian

[0102] [Measurement of Water Vapor Transmission Rate (WVTR)] The laminates obtained in the examples and comparative examples were measured for water vapor transmission rate (unit: g / m) under conditions of 40°C and 90% RH by the Mocon method in accordance with JIS K7129-2. 2 The measurement was carried out three times and the average value was calculated. The results are shown in Tables 1 and 2.

[0103] [Measurement of oxygen transmission rate (OTR)] The oxygen transmission rate (unit: cc / m) of the laminates obtained in the examples and comparative examples was measured by the Mocon method under the conditions of 30°C and 70% RH. 2 The measurement was carried out three times and the average value was calculated. The results are shown in Tables 1 and 2.

[0104] [Barrier properties after bending] The laminates obtained in the examples and comparative examples were folded 180 degrees with the overcoat layer side facing outward without creating a crease, and then a 1 kg roller was rolled over them once in each direction to create a crease. The laminates were then unfolded, and the water vapor permeability and oxygen permeability in the area centered on the crease were measured using the same method as above. The results are shown in Tables 1 and 2.

[0105]

[0106]

[0107] 1... base paper, 2... gas barrier resin layer, 3... inorganic vapor deposition layer, 4... overcoat layer, 5... inorganic pigment, 10... laminate, 20... gusset bag, B1, B2... folded portions

Claims

1. A laminate comprising a base paper and a gas barrier resin layer disposed on the base paper so as to be in direct contact with the base paper, wherein the binder resin constituting the gas barrier resin layer comprises at least one type selected from the group consisting of polyolefin resins and polyvinyl alcohol-based resins, the gas barrier resin layer comprises an inorganic pigment within a first region extending from the surface on the base paper side to a thickness that is 50% of the total thickness of the gas barrier resin layer, and 80 volume % or more of the inorganic pigment contained in the gas barrier resin layer is present within the first region.

2. The laminate according to claim 1, further comprising an inorganic vapor deposition layer on the surface of the gas barrier resin layer opposite to the base paper.

3. The laminate according to claim 2, further comprising an overcoat layer on the surface of said inorganic vapor deposition layer opposite to said gas barrier resin layer.

4. The laminate of claim 3, wherein the overcoat layer comprises a polyolefin resin.

5. The laminate according to claim 1, wherein the content of the inorganic pigment in the gas barrier resin layer is 50 parts by volume or less per 100 parts by volume of the binder resin.

6. The laminate according to claim 1, wherein the content of the inorganic pigment in the first region is 2 to 200 parts by volume per 100 parts by volume of the binder resin in the first region.

7. The laminate according to claim 1, wherein the inorganic pigment has an aspect ratio of 1 to 200.

8. The laminate according to claim 1, wherein 100% by volume of the total amount of the inorganic pigment contained in the gas barrier resin layer is present in the first region.

9. The laminate according to claim 1, wherein the surface roughness Ra of the surface of the gas barrier resin layer opposite to the base paper is 1.0 μm or less.

10. The laminate according to claim 1, wherein the gas barrier resin layer has a thickness of 1 to 20 μm.

11. The laminate according to claim 1, wherein the gas barrier resin layer has a thickness of 3 to 5 μm.

12. A packaging bag comprising the laminate according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Paper container having barrier properties

    JP2001253035A

  • Gas barrier laminate and package using the same

    JP2022128849A

  • Paper-made packaging material

    JP2022143096A

  • Coating composition, a method for coating a substrate, a coated substrate, a packaging material and a liquid package

    US20140251856A1

  • Paper barrier material

    WO2018062466A1