Curable composition, sealant, frame sealant, display panel and method for producing same

The curable composition for organic EL display panels, using a cationic photopolymerization initiator and tertiary amine, addresses the issues of high temperature curing and viscosity increase, ensuring suitable bonding and shape retention with improved sealing properties.

WO2024204252A1PCT designated stage expired Publication Date: 2024-10-03MITSUI CHEMICALS INC
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012051
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional sealants for organic electroluminescent (EL) display panels face challenges with high temperature curing, leading to damage of the elements, and excessive viscosity increase after light irradiation, which impairs bonding suitability and shape retention.

Method used

A curable composition comprising a cationic photopolymerization initiator, a tertiary amine, and a curable compound such as an epoxy or (meth)acrylic modified epoxy, which controls viscosity and adhesion by trapping acid generated during light irradiation, allowing for low-temperature curing and maintaining fluidity and tack during bonding.

Benefits of technology

The solution achieves balanced low-temperature curability, maintaining shape retention and adhesive strength, while preventing excessive viscosity increase, thus enhancing the sealing properties and leak resistance of the cured product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-C000001
    Figure JPOXMLDOC01-APPB-C000001
  • Figure JPOXMLDOC01-APPB-C000002
    Figure JPOXMLDOC01-APPB-C000002
  • Figure JPOXMLDOC01-APPB-C000003
    Figure JPOXMLDOC01-APPB-C000003
Patent Text Reader

Abstract

The curable composition contains a curable compound, a curing agent containing a photocationic polymerization initiator, and a tertiary amine. The content of the tertiary amine is 20 parts by mass or more relative to 100 parts by mass of the curing agent. After light having a wavelength of 365 nm is emitted with a total light intensity of 3000 mj / cm2 at an illuminance of 100 mW / cm2, the complex viscosity at 25°C and a time lapse of 600 seconds is 1.0 × 103 Pa·s to 5.0 × 104 Pa·s.
Need to check novelty before this filing date? Find Prior Art

Description

Curable composition, sealant, frame sealant, display panel, and method for producing the same

[0001] The present invention relates to a curable composition, a sealant, a frame sealant, a display panel, and a method for producing the same.

[0002] In recent years, display devices using display elements such as organic electroluminescence elements (hereinafter referred to as organic EL elements) have been developed, but display elements are generally susceptible to deterioration due to moisture and oxygen in the atmosphere. Therefore, in various display devices, the display elements are generally sealed with a sealing layer.

[0003] For example, an organic EL display panel includes an element substrate having organic EL elements, an opposing substrate, and a sealing layer disposed between them to seal the organic EL elements. Such organic EL display panels are manufactured by various methods. One such manufacturing method is known as the dam-fill method.

[0004] In the dam-fill method, an organic EL display panel is manufactured through, for example, 1) a step of applying a first sealant in a frame shape onto an opposing substrate, 2) a step of filling a second sealant into the area surrounded by the first sealant to form a sealant layer, 3) a step of irradiating the sealant layer with light, 4) a step of bonding a substrate on which an organic EL element is disposed to the opposing substrate having the sealant layer after light irradiation, and 5) a step of heating and curing the sealant layer (see, for example, Patent Document 1).

[0005] Further, as a frame sealant used in the above-mentioned method, for example, a sealant containing a polyolefin, an epoxy compound (curable resin A), a thermosetting agent, and a water-absorbing filler is known (see, for example, Patent Document 2). In this document, a thermal cationic initiator is used as the thermosetting agent.

[0006] Further, as a sealant for an organic EL element, a sealant containing a photocurable compound containing a (meth)acrylic-modified epoxy resin and a photocationic polymerization initiator is also known (see, for example, Patent Document 3).

[0007] International Publication No. 2013 / 157059 International Publication No. 2020 / 149359 Japanese Patent Application Laid-Open No. 2012-151109

[0008] However, the sealant disclosed in Patent Document 2 has a drawback in that the element is easily damaged by heat because it is cured by heating at 100° C. In order to prevent such damage, the sealant is required to have low-temperature curing properties.

[0009] Furthermore, the above-mentioned sealant is required to have a predetermined usable time or more after light irradiation, i.e., to maintain a moderately low viscosity after light irradiation. For example, as described above, the sealant applied to one substrate is irradiated with light to temporarily cure, and then the other substrate is bonded to the substrate and heated to fully cure. However, the sealants shown in Patent Documents 2 and 3 tend to undergo an excessive increase in viscosity after light irradiation because the curing reaction proceeds too much before the other substrate is bonded. As a result, the fluidity and tack of the sealant are easily impaired during bonding, resulting in poor bonding suitability and difficulty in obtaining sufficient adhesive strength. Generally, the higher the low-temperature curing property, the more likely the viscosity is to increase after light irradiation, so it is desirable to achieve a good balance between these properties.

[0010] Furthermore, from the viewpoint of improving the sealing property and leak resistance of the cured product, it is desirable that the curable composition after light irradiation can maintain its shape well when cured by heating. In this way, it is desirable to be able to achieve both lamination suitability and shape retention while maintaining handleability during application.

[0011] The present invention has been made in view of the above circumstances, and provides a curable composition, a sealant, a frame sealant, a display panel, and a method for manufacturing the same that have low-temperature curing properties and are compatible with lamination suitability and shape retention.

[0012] [1] A curable composition comprising a curable compound, a photocationic polymerization initiator, and a tertiary amine, wherein the content of the tertiary amine is 20 parts by mass or more relative to 100 parts by mass of the photocationic polymerization initiator, and wherein the composition is irradiated with light having a wavelength of 365 nm at an illuminance of 100 mW / cm 2 The cumulative light intensity is 3000 mJ / cm 2 After 600 seconds of irradiation, the complex viscosity at 25°C was 1.0 x 10 3 Pa・s or more 5.0×10 4A curable composition having a viscosity of Pa·s or less. [2] The curable composition according to [1], wherein the curable compound comprises an epoxy compound and at least one of a (meth)acrylic-modified epoxy compound and a (meth)acrylic compound. [3] The curable composition according to [1] or [2], wherein the content of the tertiary amine is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the curable compound. [4] The curable composition according to any one of [1] to [3], wherein the tertiary amine is a bifunctional tertiary amine. [5] The curable composition according to any one of [1] to [4], wherein the tertiary amine has an N—O bond. [6] The curable composition according to any one of [1] to [5], wherein the tertiary amine has a hindered structure. [7] A sealant comprising the curable composition according to any one of [1] to [6]. [8] A frame sealant comprising the curable composition according to any one of [1] to [6]. [9] A display panel having an element substrate on which elements are arranged, a counter substrate arranged opposite the element substrate with the elements sandwiched therebetween, and a sealing portion arranged between the element substrate and the counter substrate for sealing the elements, wherein the sealing portion contains a cured product of the sealant described in [7].

[10] A method for manufacturing a display panel, comprising the steps of: applying a first sealant in a frame shape along the periphery of a display area on one surface of the element substrate or the counter substrate; filling a second sealant in the area surrounded by the first sealant to form a sealant layer; irradiating the sealant layer with light; bonding one substrate to the other substrate via the sealant layer irradiated with light; and heating and curing the sealant layer, wherein at least one of the first sealant and the second sealant is the sealant described in [7].

[0013] The present invention has been made in view of the above circumstances, and provides a curable composition that has low-temperature curing properties and is capable of achieving both lamination suitability and shape retention, a sealant, a frame sealant, a display panel, and a method for manufacturing the same.

[0014] As described above, conventional curable compositions have low suitability for lamination because their viscosity becomes too high after light irradiation.

[0015] In contrast, the curable composition of the present invention contains a curable compound, a photocationic polymerization initiator, and a tertiary amine, and is irradiated with light having a wavelength of 365 nm at an illuminance of 100 mW / cm. 2 The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the complex viscosity at 25°C after 600 seconds was 1.0 x 10 3 Pa・s or more 5.0×10 4 The viscosity is adjusted to a range of Pa·s or less, thereby making it possible to maintain the applied shape well while maintaining the fluidity and tackiness during lamination.

[0016] Specifically, the complex viscosity after light irradiation is 1.0 × 10 3 When the complex viscosity after light irradiation is 5.0×10 or more, the applied shape is easily maintained even when heated thereafter. This can improve the sealing properties of the cured product. 4 When the viscosity is Pa s or less, the fluidity and tackiness during lamination are unlikely to be impaired, and the lamination suitability can be maintained at a good level. The complex viscosity of the curable composition can be adjusted by the amount of the tertiary amine, the composition of the curable compound, etc.

[0017] That is, the curable composition of the present invention contains a predetermined amount or more of a tertiary amine relative to the photocationic polymerization initiator. When such a curable composition is irradiated with light, an acid is first generated from the photocationic polymerization initiator. This acid is captured by a sufficient amount of tertiary amine, so that after light irradiation, the curable compound is less likely to be cured by the acid, and an increase in viscosity can be reduced. When the curable composition is then heated, the acid captured by the tertiary amine is released, and the curable compound polymerizes (cures).

[0018] The curable compound preferably contains an epoxy compound and at least one of a (meth)acrylic-modified epoxy compound and a (meth)acrylic compound. The photocationic polymerization initiator may also instantaneously generate radicals when generating an acid upon light irradiation. The radicals cause the (meth)acrylic-modified epoxy compound or the (meth)acrylic compound to cure. This appropriately increases the viscosity of the curable composition upon light irradiation, making it easier to maintain its shape. Hereinafter, a curable composition according to one embodiment of the present invention will be specifically described.

[0019] 1. Curable Composition The curable composition according to this embodiment contains a curable compound, a photocationic polymerization initiator, and a tertiary amine.

[0020] 1-1. Curable Compound The curable compound includes a curable compound that reacts with a cationic photopolymerization initiator. The curable compound that reacts with a cationic photopolymerization initiator is a compound that polymerizes and hardens using, as a medium, active species such as acids or radicals generated when the cationic photopolymerization initiator receives light or heat energy. Such a curable compound preferably includes a compound that includes a cationic polymerizable group, and from the viewpoint of enhancing thermosetting properties, preferably includes an epoxy compound.

[0021] That is, the curable compound preferably contains an epoxy compound. Furthermore, from the viewpoint of easily adjusting the viscosity after light irradiation to a predetermined level or higher, the curable compound preferably further contains at least one of a (meth)acrylic compound and a (meth)acrylic-modified epoxy compound together with the epoxy compound.

[0022] 1-1-1. Epoxy Compound The curable compound may contain only one type of epoxy compound, or may contain two or more types of epoxy compounds.

[0023] In this specification, an epoxy compound refers to a compound having one or more epoxy groups in the molecule. However, the epoxy compound does not include a compound having both an epoxy group and a (meth)acryloyl group. The number of epoxy groups contained in one molecule of the epoxy compound may be one or two or more. From the viewpoint of increasing the curing reactivity, the number of epoxy groups contained in one molecule of the epoxy compound is preferably two or more.

[0024] Examples of the epoxy compound include known epoxy compounds, such as aromatic epoxy compounds, aliphatic epoxy compounds, and alicyclic epoxy compounds. Among these, from the viewpoint of further reducing the moisture permeability of the cured product, it is preferable that at least one of the epoxy compounds includes an aromatic epoxy compound.

[0025] Examples of aromatic epoxy compounds include glycidyl ethers of alcohols (including polyhydric alcohols) containing an aromatic ring. Specific examples include bisphenol-type glycidyl ether compounds obtained by reacting epichlorohydrin with bisphenols such as bisphenol A, bisphenol S, bisphenol F, and bisphenol AD, or diols obtained by modifying these aromatic diols with ethylene glycol, propylene glycol, and alkylene glycol; trisphenol-type glycidyl ether compounds obtained by reacting epichlorohydrin with trisphenol compounds (e.g., 1,1,1-tris(hydroxyphenyl)methane, 1-[α-methyl-α-(4-hydroxyphenyl)ethyl]-3-[α,α-bis(4-hydroxyphenyl)ethyl]benzene (or 4-[4-[1,1-bis(4-hydroxyphenyl)ethyl]-α,α-dimethylbenzyl]phenol); These include novolak resins derived from phenol or cresol and formaldehyde, novolak-type glycidyl ether compounds obtained by reacting polyphenols, such as polyalkenylphenols or their copolymers, with epichlorohydrin, and glycidyl ether compounds of xylylene phenol resins.

[0026] Among these, bisphenol-type epoxy compounds such as bisphenol A-type epoxy compounds and bisphenol F-type epoxy compounds, cresol novolac-type epoxy compounds, phenol novolac-type epoxy compounds, triphenolmethane-type epoxy compounds, triphenolethane-type epoxy compounds, trisphenol-type epoxy compounds, dicyclopentadiene-type epoxy compounds, diphenyl ether-type epoxy compounds, and biphenyl-type epoxy compounds are preferred.

[0027] The epoxy compound may be liquid or solid. From the viewpoint of improving the coatability of the curable composition, a liquid epoxy compound is preferred. Furthermore, from the viewpoint of further reducing the moisture permeability of the cured product, a solid epoxy compound is preferred. The softening point of the solid epoxy compound is preferably 40°C or higher and 150°C or lower. The softening point can be measured by the ring and ball method specified in JIS K7234.

[0028] The weight average molecular weight of the epoxy compound is preferably from 200 to 10,000, and more preferably from 300 to 5,000. The weight average molecular weight of the epoxy compound is measured by gel permeation chromatography (GPC) in terms of polystyrene.

[0029] As described above, the curable compound may contain only one type of epoxy compound, or may contain two or more types. For example, from the viewpoint of achieving both viscosity stability and permeability of the cured product at a higher level, a liquid epoxy compound and a solid epoxy compound may be combined. Furthermore, from the viewpoint of easily achieving both viscosity stability and permeability of the cured product, a bifunctional aromatic epoxy compound and a trifunctional or higher aromatic epoxy compound may be combined.

[0030] For example, when a difunctional aromatic epoxy compound is combined with a trifunctional or higher aromatic epoxy compound, the trifunctional or higher aromatic epoxy compound can be, for example, 10% by mass or more, preferably 30% by mass or more and 70% by mass or less, based on the total amount of epoxy compounds. When the content of the trifunctional or higher aromatic epoxy compound is 10% by mass or more, the moisture permeability of the cured product can be further improved. On the other hand, although the viscosity of the curable composition after light irradiation tends to increase, the tertiary amine traps the acid generated from the photocationic polymerization initiator, thereby suppressing excessive viscosity increase.

[0031] The total amount of epoxy compounds is preferably 50% by mass or more, more preferably 50% by mass or more and 95% by mass or less, and even more preferably 70% by mass or more and 95% by mass or less, based on the curable compounds. When the amount of epoxy compounds is 50% by mass or more, the curing reactivity by heating is more likely to be enhanced. In addition, the viscosity of the curable composition after light irradiation can be further reduced, thereby further enhancing the fluidity and tackiness during lamination. On the other hand, when the amount of epoxy compounds is 95% by mass or less, the amount of, for example, (meth)acrylic-modified epoxy compound or (meth)acrylic compound becomes relatively large, making it easier to moderately increase the viscosity of the curable composition after light irradiation and more likely to improve shape retention.

[0032] 1-1-2. (Meth)acrylic-modified epoxy compound In this specification, a (meth)acrylic-modified epoxy compound refers to a compound having one or more epoxy groups and one or more (meth)acryloyl groups in the molecule. The curable compound may contain only one type of (meth)acrylic-modified epoxy compound, or may contain two or more types.

[0033] The number of epoxy groups and (meth)acryloyl groups in the (meth)acrylic-modified epoxy compound is not particularly limited, and each may be only one, or may be two or more. The (meth)acrylic-modified epoxy compound has good compatibility with epoxy compounds.

[0034] The (meth)acrylic-modified epoxy compound can be obtained by modifying at least one epoxy group of a difunctional or higher functional epoxy compound with a (meth)acryloyl group, for example, by reacting the difunctional or higher functional epoxy compound with (meth)acrylic acid in the presence of a basic catalyst.

[0035] The epoxy compound to be modified with a (meth)acryloyl group may be a polyfunctional epoxy compound having two or more epoxy groups in the molecule, and from the viewpoints of improving coatability and suppressing a decrease in adhesive strength due to excessive crosslinking density, a bifunctional epoxy compound is preferred. Examples of bifunctional epoxy compounds include bisphenol-type epoxy compounds (bisphenol A type, bisphenol F type, 2,2'-diallyl bisphenol A type, bisphenol AD ​​type, hydrogenated bisphenol type, etc.), biphenyl-type epoxy compounds, and naphthalene-type epoxy compounds. Among these, bisphenol-type epoxy compounds of bisphenol A type and bisphenol F type are preferred from the viewpoint of easily improving coatability. (Meth)acrylic-modified epoxy compounds derived from bisphenol-type epoxy compounds have advantages such as superior coatability compared to (meth)acrylic-modified epoxy compounds derived from biphenyl ether-type epoxy compounds.

[0036] In the (meth)acrylic-modified epoxy compound, the ratio of the number of moles of (meth)acryloyl groups to the number of moles of epoxy groups is preferably 1 or more, and more preferably 2 or more. By increasing the ratio of the number of moles of (meth)acryloyl groups, the viscosity of the curable composition after light irradiation can be more easily increased.

[0037] The weight average molecular weight of the (meth)acrylic-modified epoxy compound measured by gel permeation chromatography (GPC) is preferably 300 to 500.

[0038] 1-1-3. (Meth)acrylic Compound In this specification, a (meth)acrylic compound is a compound having one or more (meth)acryloyl groups in the molecule. However, the (meth)acrylic compound does not include a compound having both a (meth)acryloyl group and an epoxy group. The curable compound may contain only one type of (meth)acrylic compound, or may contain two or more types.

[0039] The number of (meth)acryloyl groups contained in one molecule of a (meth)acrylic compound may be 1 or 2 or more. Examples of (meth)acrylic compounds containing one (meth)acryloyl group in one molecule include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate.

[0040] Examples of (meth)acrylic compounds having two or more (meth)acryloyl groups in one molecule include di(meth)acrylates derived from polyethylene glycol, propylene glycol, polypropylene glycol, etc.; di(meth)acrylates derived from tris(2-hydroxyethyl)isocyanurate; di(meth)acrylates derived from a diol obtained by adding 4 or more moles of ethylene oxide or propylene oxide to 1 mole of neopentyl glycol; di(meth)acrylates (bisphenol A or F type epoxy(meth)acrylates) derived from a diol obtained by adding 2 moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A or bisphenol F; di- or tri(meth)acrylates derived from a polyol obtained by adding 2 or 3 moles of ethylene oxide or propylene oxide to 1 mole of trimethylolpropane; di(meth)acrylates derived from a diol obtained by adding 4 or more moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A; tris( 2-hydroxyethyl) isocyanurate tri(meth)acrylate; trimethylolpropane tri(meth)acrylate or its oligomer; pentaerythritol tri(meth)acrylate or its oligomer; poly(meth)acrylate of dipentaerythritol; tris(acryloxyethyl) isocyanurate; caprolactone-modified tris(acryloxyethyl) isocyanurate; caprolactone-modified tris(methacryloxyethyl) isocyanurate; poly(meth)acrylate of alkyl-modified dipentaerythritol caprolactone-modified dipentaerythritol poly(meth)acrylate; hydroxypivalic acid neopentyl glycol di(meth)acrylate; caprolactone-modified hydroxypivalic acid neopentyl glycol di(meth)acrylate; ethylene oxide-modified phosphate (meth)acrylate; ethylene oxide-modified alkylated phosphate (meth)acrylate; and oligo(meth)acrylate of neopentyl glycol, trimethylolpropane, and pentaerythritol.Among these, di(meth)acrylates derived from diols obtained by adding 2 moles of ethylene oxide or propylene oxide to 1 mole of bisphenol A or bisphenol F (bisphenol A or F type epoxy(meth)acrylates) are preferred.

[0041] The weight average molecular weight of the (meth)acrylic compound measured by gel permeation chromatography (GPC) is preferably 200 to 10,000, more preferably 200 to 5,000.

[0042] The weight average molecular weight of the (meth)acrylic compound is preferably about 310 to 1000. The weight average molecular weight is a value measured, for example, by gel permeation chromatography (GPC) in terms of polystyrene.

[0043] The total amount of the (meth)acrylic-modified epoxy compound and the (meth)acrylic compound may be 50% by mass or less, preferably 5% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 30% by mass or less, relative to the total amount of the curable compounds. When the total amount is 5% by mass or more, it is easy to appropriately increase the viscosity of the curable composition after light irradiation, and it is easy to further improve shape retention. On the other hand, when the total amount is 50% by mass or less, the relative amount of the epoxy compound increases, making it easy to maintain a low viscosity of the curable composition after light irradiation, and fluidity and tackiness are less likely to be impaired. The total amount of the curable compounds may be the same as the total amount of the epoxy compound, the (meth)acrylic-modified epoxy compound, and the (meth)acrylic compound.

[0044] 1-1-4. Other Compounds The curable compound may further contain an oxetane compound in addition to the above.

[0045] 1-1-5. Common Features The total amount of curable compounds is preferably 20% by mass or more and 90% by mass or less, and more preferably 30% by mass or more and 70% by mass or less, relative to the total amount of the curable composition. When the total amount is 20% by mass or more, the curability of the curable composition tends to be higher. On the other hand, when the total amount is 90% by mass or less, for example, if an inorganic filler is included, the relative amount of the filler increases, making it easier to improve shape retention and low moisture permeability.

[0046] 1-2. Photocationic Polymerization Initiator The photocationic polymerization initiator has the function of curing the curable compound. The photocationic polymerization initiator is, for example, a photoacid generator that generates an acid upon light irradiation. Note that the photocationic polymerization initiator may also instantaneously generate radicals when generating an acid upon light irradiation.

[0047] The absorption wavelength of the cationic photopolymerization initiator is not particularly limited, and it is preferable that the initiator absorbs light having a wavelength of 360 nm or more, and more preferably absorbs light having a wavelength of 360 nm or more and 430 nm or less. When the absorption wavelength of the cationic photopolymerization initiator is within the above range, it is possible to reduce the influence on optical elements, for example.

[0048] The cationic photopolymerization initiator is not particularly limited, and known cationic photopolymerization initiators can be used.

[0049] Examples of photocationic polymerization initiators include those in which the anion moiety is BF 4 - , (Rf) n PF 6-n - (Rf is an organic group, n is an integer of 1 to 5), PF 6 - , SbF 6 - , or BX 4 - (X is a phenyl group substituted with at least two fluorine or trifluoromethyl groups), aromatic sulfonium salts, aromatic iodonium salts, aromatic diazonium salts, aromatic ammonium salts, etc. are included.

[0050] Examples of the aromatic sulfonium salt include bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide bistetrafluoroborate, bis[4-(diphenylsulfonio)phenyl]sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate, and the like.

[0051] Examples of aromatic iodonium salts include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, and the like.

[0052] Examples of aromatic diazonium salts include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, phenyldiazonium tetrakis(pentafluorophenyl)borate, and the like.

[0053] Examples of aromatic ammonium salts include 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, and the like.

[0054] Examples of commercially available photocationic polymerization initiators include Irgacure 250, Irgacure 270, and Irgacure 290 (manufactured by BASF), CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, and CPI-400PG (manufactured by San-Apro Co., Ltd.), and SP-150, SP-170, SP-171, SP-056, SP-066, SP-130, SP-140, SP-601, SP-606, and SP-701 (manufactured by ADEKA Corporation). Of these, sulfonium salts such as Irgacure 270, Irgacure 290, CPI-100P, CPI-101A, CPI-200K, CPI-210S, CPI-310B, CPI-400PG, SP-150, SP-170, SP-171, SP-056, SP-066, SP-601, SP-606, and SP-701 are preferred.

[0055] The cationic photopolymerization initiator may be used alone or in combination of two or more kinds.

[0056] The content of the cationic photopolymerization initiator is preferably 0.1 parts by mass or more and 20 parts by mass or less, more preferably 0.5 parts by mass or more and 15 parts by mass or less, and even more preferably 0.8 parts by mass or more and 8 parts by mass or less, per 100 parts by mass of the curable compound. When the content of the cationic photopolymerization initiator is 0.1 parts by mass or more, a larger amount of acid is more likely to be generated by light irradiation, which can make the curing reaction more likely to occur when curing by heating. Furthermore, when the curable composition contains a (meth)acrylic-modified epoxy compound or the like, a larger amount of radicals are instantaneously generated when acid is generated, which makes it easier for curing by light irradiation to occur appropriately. When the content of the cationic photopolymerization initiator is 20 parts by mass or less, bleed-out can be reduced, which can make the contamination of optical elements and the like less likely.

[0057] Tertiary amines capture the acid generated from the cationic photopolymerization initiator upon light irradiation, thereby making it difficult for the curing reaction of the curable compound to occur upon light irradiation and suppressing an excessive increase in viscosity of the curable composition after light irradiation.

[0058] Tertiary amines include monofunctional tertiary amines having one amino group in the molecule, bifunctional tertiary amines having two amino groups, and trifunctional or higher tertiary amines having three or more amino groups. Among these, from the viewpoint of further increasing the acid trapping efficiency, bifunctional tertiary amines and trifunctional or higher tertiary amines are preferred, and from the viewpoint of more easily maintaining compatibility with the epoxy compound, bifunctional tertiary amines are more preferred.

[0059] The tertiary amine preferably has an N—O bond, from the viewpoint of making it easier to release the trapped acid upon heating and further improving low-temperature curing properties. In other words, a bifunctional tertiary amine having an N—O bond is preferred.

[0060] Furthermore, the tertiary amine preferably has a hindered structure, which makes it easier to release the trapped acid upon heating and further enhances low-temperature curing properties. Examples of the hindered structure include a structure having a steric hindrance, such as 2,2,6,6-tetramethylpiperidine.

[0061] Therefore, the tertiary amine is preferably a bifunctional tertiary amine having an N—O bond, more preferably a bifunctional tertiary amine having an N—O bond and a hindered structure, and even more preferably a tertiary amine having an N—O bond and two 2,2,6,6-tetramethylpiperidine structures in the molecule.

[0062] Such tertiary amines include compounds represented by formula (1) or (2).

[0063] In formula (1), R 3 represents an alkyl group having 1 to 20 carbon atoms. Examples of the linear or branched alkyl group having 1 to 20 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and an eicosyl group. 3 may be the same as or different from each other.

[0064]

[0065] In formula (2), R4 represents a linear or branched alkyl group having 1 to 20 carbon atoms. Examples of linear or branched alkyl groups having 4 to 20 carbon atoms include a butyl group, a pentyl group, a hexyl group, a heptyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, and an eicosyl group. 4 may be the same as or different from each other.

[0066] R 5 represents an alkylene group having 1 to 8 carbon atoms. Examples of the alkylene group having 1 to 8 carbon atoms include a methylene group, an ethylene group, a propylene group, a butylene group, a pentylene group, a hexylene group, a heptylene group, and an octylene group.

[0067] Examples of the compound represented by formula (1) include a compound represented by formula (1-1); examples of the compound represented by formula (2) include a compound represented by formula (2-1).

[0068] Commercially available tertiary amines may also be used, such as ADK STAB LA-81 (manufactured by ADEKA Corporation) and Tinuvin 123 (manufactured by BASF Japan).

[0069] The tertiary amine may be contained in one kind or in two or more kinds.

[0070] The content of the tertiary amine is preferably 20 parts by mass or more per 100 parts by mass of the cationic photopolymerization initiator from the viewpoint of capturing the acid generated from the cationic photopolymerization initiator. When the content of the tertiary amine is 20 parts by mass or more, a larger amount of acid can be trapped, which makes it easier to suppress an increase in viscosity after light irradiation and further enhances tackiness. From the same viewpoint, the content of the tertiary amine is preferably 60 parts by mass or more, and more preferably 65 parts by mass or more, per 100 parts by mass of the cationic photopolymerization initiator. The upper limit of the content of the tertiary amine is not particularly limited, but may be, for example, 100 parts by mass or less from the viewpoint of further reducing the amount of tertiary amine remaining as an unreacted component after curing, further minimizing deterioration in the adhesion and moisture permeability of the cured product, and improving the physical properties of the cured product.

[0071] Furthermore, the content of the tertiary amine is, for example, preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the curable compound. When the content of the tertiary amine is 0.5 parts by mass or more, a larger amount of acid can be trapped, making it easier to suppress an increase in viscosity after light irradiation and further increasing tack. When the content of the tertiary amine is 20 parts by mass or less, the amount of tertiary amine remaining unreacted after heat curing can be further reduced, making it possible to further suppress deterioration in the physical properties of the cured product.

[0072] 1-4. Other Components The curable composition may further contain other components in addition to the above-described components. Examples of the other components include an inorganic filler, a photosensitizer, a silane coupling agent, a curing agent other than a photocationic polymerization initiator, a tackifier, organic fine particles, a plasticizer, an antioxidant, and an antifoaming agent.

[0073] 1-4-1 Inorganic Filler The inorganic filler can have the function of improving the shape retention of the cured product and reducing the moisture permeability of the cured product.

[0074] Examples of inorganic fillers include calcium carbonate, magnesium carbonate, barium sulfate, magnesium sulfate, aluminum silicate, zirconium silicate, iron oxide, titanium oxide, titanium nitride, alumina other than those mentioned above, zinc oxide, silicon dioxide (silica), potassium titanate, kaolin, talc, glass beads, sericite activated clay, bentonite, aluminum nitride, silicon nitride, etc. Of these, silicon dioxide and talc are preferred.

[0075] The inorganic filler may have a regular shape, such as a spherical, plate-like, or needle-like shape, or may have an irregular shape. When the inorganic filler is spherical, the average primary particle diameter of the inorganic filler is preferably 0.1 μm or more and 5 μm or less, and more preferably 0.5 μm or more and 3 μm or less, from the viewpoint of, for example, the shape retention and thickness adjustment of the cured product after lamination. When the average primary particle diameter of the inorganic filler is 5 μm or less, it is easier to reduce unevenness in the thickness of the cured product after lamination, and when it is 0.1 μm or more, it is possible to further suppress an increase in viscosity. Furthermore, from the viewpoint of adjusting the viscosity (thixotropy) of the curable composition, it is preferably in the range of less than 0.1 μm, for example, 7 nm or more and less than 100 nm. The average primary particle diameter of the inorganic filler can be measured by the laser diffraction method described in JIS Z8825 (2013).

[0076] The specific surface area of ​​the inorganic filler is 0.5 m 2 / g or more 20m 2 The specific surface area of ​​the inorganic filler is measured by the BET method described in JIS Z8830 (2013).

[0077] The curable composition may contain only one type of inorganic filler, or may contain two or more types. From the viewpoint of adjusting the viscosity (thixotropy) and the shape retention and thickness of the cured product, for example, the curable composition may contain an inorganic filler having a relatively small average primary particle size (e.g., less than 0.1 μm) and an inorganic filler having a relatively large average primary particle size (e.g., 0.1 μm or more). The content of the inorganic filler having a relatively small average particle size is preferably less than the content of the inorganic filler having a relatively large average particle size.

[0078] The content of the inorganic filler is preferably 10 parts by mass or more and 350 parts by mass or less relative to 100 parts by mass of the curable compound. When the content of the inorganic filler is 10 parts by mass or more, the shape retention of the cured product is more likely to be improved and moisture permeability can be further reduced. When the content of the inorganic filler is 350 parts by mass or less, not only is the coatability of the curable composition less likely to be impaired, but also a decrease in adhesive strength due to a decrease in the relative amount of the curable compound or a loss in flexibility of the cured product can be more suppressed. From the same viewpoint, the content of the inorganic filler is more preferably 150 parts by mass or more and 300 parts by mass or less.

[0079] 1-4-2. Photosensitizer The photosensitizer has the function of further improving the polymerization initiation efficiency of the above-mentioned cationic photopolymerization initiator and further accelerating the curing reaction of the curable compound.

[0080] Examples of the photosensitizer include thioxanthone compounds such as 2,4-diethylthioxanthone, 2,2-dimethoxy-1,2-diphenylethan-1-one, benzophenone, 2,4-dichlorobenzophenone, methyl o-benzoylbenzoate, 4,4'-bis(dimethylamino)benzophenone, 4-benzoyl-4'-methyldiphenyl sulfide, 9,10-dibutoxyanthracene, etc. The curable composition may contain only one type of photosensitizer, or may contain two or more types.

[0081] The content of the photosensitizer is, for example, preferably 0.1 parts by mass or more and 5 parts by mass or less, and more preferably 0.5 parts by mass or more and 2 parts by mass or less, relative to 100 parts by mass of the curable compound. The curable composition may contain only one type of photosensitizer, or may contain two or more types of photosensitizers.

[0082] 1-4-3. Silane Coupling Agent Examples of the silane coupling agent include vinyltrimethoxysilane, γ-(meth)acryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and γ-glycidoxypropyltriethoxysilane.

[0083] The content of the silane coupling agent is preferably 0.1 to 10 parts by mass, more preferably 1.0 to 5.0 parts by mass, relative to 100 parts by mass of the curable compound. When the content of the silane coupling agent is 0.1 part by mass or more, the adhesive strength of the cured product is more likely to be increased, and when it is 10 parts by mass or less, the decrease in moisture permeation resistance of the cured product can be further reduced.

[0084] 1-4-4. Other Curing Agents The curable composition may further contain a curing agent other than the cationic photopolymerization initiator, as long as the object and effect of the present invention are not impaired. Examples of such a curing agent include a radical photopolymerization initiator.

[0085] 1-4-5. Common Features The total amount of the other components is preferably 0.1% by mass or more and 50% by mass or less, based on the total amount of the curable composition. When the total amount is 50% by mass or less, the viscosity of the curable composition is unlikely to increase excessively, and the coatability is unlikely to be impaired.

[0086] 1-5. Physical Properties The viscosity of the curable composition, measured using an E-type viscometer at 25°C and 2.5 revolutions per minute, is preferably, for example, 20 Pa·s or more and 500 Pa·s or less, and more preferably 30 Pa·s or more and 300 Pa·s or less. When the viscosity of the curable composition is 20 Pa·s or more, the composition has a moderately high viscosity, which makes it easier to improve shape retention during application. When the viscosity of the curable composition is 500 Pa·s or less, the application properties are less likely to be impaired when the composition is applied, for example, by a dispenser or screen printing.

[0087] The curable composition was irradiated with light of wavelength 365 nm at a UV irradiance of 100 mW / cm 2 The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the complex viscosity at 25°C after 600 seconds was 1.0 x 10 3 Pa・s or more 5.0×10 4 It is preferable that the viscosity is 2.0×10 Pa·s or less. 3 Pa・s or more 3.0×10 4 It is more preferable that the complex viscosity of the curable composition is 5.0×10 Pa s or less. 4When the complex viscosity of the curable composition is 1.0×10 Pa s or less, the curable composition has tack even after light irradiation, and the flowability during lamination is not easily impaired, and the lamination suitability is not easily impaired. 3 When the viscosity is Pa·s or more, the applied shape can be well maintained, so that the shape retention of the cured product is high and leak resistance is easily improved.

[0088] The complex viscosity of the curable composition is measured using a dynamic viscoelasticity measuring device (e.g., a rheometer MARSIII manufactured by Haake Co., Ltd.) at a measurement frequency of 1 Hz, a cell gap of 30 μm, and a temperature of 25° C., while using a metal halide lamp with a UV irradiance of 100 mW / cm 2 The cumulative light intensity is 3000 mJ / cm 2 After irradiation, the complex viscosity can be measured after 600 seconds.

[0089] As described above, the viscosity of the curable composition after light irradiation can be adjusted by the content of the tertiary amine and the composition of the curable compound. For example, if the amount of the tertiary amine is large relative to the amount of the cationic photopolymerization initiator, a larger amount of acid generated from the cationic photopolymerization initiator upon light irradiation can be trapped, which makes it easier to suppress an increase in the viscosity of the curable composition after light irradiation. On the other hand, if the amount of the (meth)acrylic-modified epoxy compound or the (meth)acrylic compound is large, the viscosity after light irradiation tends to increase.

[0090] As described above, the curable composition according to this embodiment can be used as a sealant because its viscosity can be adjusted to a level suitable for bonding after light irradiation. That is, the sealant contains the curable composition.

[0091] As described below, the sealant can be used as a sealant or adhesive for various elements such as organic EL elements, LED elements, liquid crystal elements, semiconductor elements, and solar cell elements. For example, the sealant may be a sealant for sealing light-emitting elements such as organic EL elements and micro LED elements. The sealant may be a surface sealant or a frame sealant. Since the frame sealant is required to have a cured product with high shape retention, the curable composition is particularly suitable as a frame sealant.

[0092] Hereinafter, an example in which the curable composition is used as a sealant for a display panel will be described.

[0093] 2. Display Panel and Manufacturing Method Thereof A display panel according to one embodiment of the present invention has an element substrate, an opposing substrate, and a sealing portion disposed between them to seal the elements.

[0094] The element substrate includes a substrate and an element. The substrate is a transparent substrate. The material of the transparent substrate may be an inorganic material such as glass, or may be a plastic such as polycarbonate, polyethylene terephthalate, polyethersulfone, or PMMA. The element may be any of various elements such as an organic EL element, an LED element (including a micro LED), a liquid crystal element, a semiconductor element, or a solar cell element. For example, when the element is an organic EL element, the organic EL element is disposed on a substrate and has a laminated structure of an anode / light-emitting layer / negative electrode.

[0095] The counter substrate is disposed opposite the element substrate with the elements interposed therebetween. The counter substrate may be a transparent substrate similar to the above. The counter substrate may have, for example, a color filter layer.

[0096] The sealing portion includes a frame-shaped first sealing portion arranged to surround the outer periphery of the element, and a second sealing portion filled in the area surrounded by the first sealing portion. The first sealing portion is a cured product of a first sealant (dam material). The second sealing portion is a cured product of a second sealant (fill material). At least one of the first sealant and the second sealant, preferably the first sealant, is the curable composition.

[0097] The display panel can be manufactured by any method. For example, the display panel can be obtained by a manufacturing method including the steps of: 1) applying a first sealant in a frame shape on one of the counter substrate and the element substrate so as to surround a display region; 2) filling the region surrounded by the frame-shaped applied first sealant with a second sealant to form a sealant layer; 3) irradiating the sealant layer with light; 4) bonding the one substrate and the other substrate together via the sealant layer irradiated with light; and 5) heating and curing the sealant layer.

[0098] In step 1), the first sealant is applied to one of the opposing substrate and the element substrate, for example, the opposing substrate, in a frame shape so as to surround the display area. The application method is not particularly limited, but application can be performed using a dispenser, for example.

[0099] In step 2), a second sealant is filled into the area surrounded by the first sealant applied in a frame shape, thereby forming a sealant layer.

[0100] In step 3), the sealant layer is irradiated with light. The type of light to be irradiated is appropriately selected depending on the type of cationic photopolymerization initiator in the curable composition serving as the first sealant, but light in the visible light range is preferred, for example, light with a wavelength of 370 nm or more and 450 nm or less. This is because light in this wavelength range causes relatively little damage to the drive electrode. For the light irradiation, a known light source emitting ultraviolet or visible light can be used, such as a metal halide lamp.

[0101] The light irradiation amount is preferably such that the curable composition after irradiation remains adequately tacky. For example, 10 mW / cm 2 More than 1000mW / cm 2 At an intensity of 1000 mJ / cm 2 More than 10000mJ / cm 2 It can be as follows:

[0102] The light irradiation initiates curing of the first sealant and the second sealant. After the light irradiation is completed, the temperature of the substrate may rise to about 35°C, and the substrate may be left in this state. By waiting for a predetermined time after the light irradiation rather than immediately bonding the substrates, the curing of the first sealant and the second sealant progresses appropriately and the viscosity of the first sealant and the second sealant increases.

[0103] In step 4), in a state in which the viscosities of the first sealant and the second sealant have been appropriately increased, the opposing substrate and the element substrate are bonded together via the sealant layer.

[0104] The bonding is performed by pressing the element substrate and the opposing substrate with a press or the like in a vacuum chamber so as to crush the sealant layer. At this time, the first sealant, which has a relatively high viscosity, is present in a frame shape around the second sealant, preventing the second sealant from leaking out.

[0105] In step 5), the laminated body is heated to heat and harden the first sealant and the second sealant.

[0106] The heating temperature may be any temperature at which the sealant layer is cured, and from the viewpoint of reducing thermal damage to the element, a low temperature is preferable, for example, a temperature lower than 100° C., preferably 40° C. or higher and 90° C. or lower, more preferably 60° C. or higher and 85° C. or lower. The heating time varies depending on the heating temperature, but is, for example, 60 minutes or longer and 120 minutes or shorter.

[0107] In the above embodiment, in step 3), the viscosity of the curable composition when irradiated with light is adjusted to fall within a predetermined range.

[0108] Specifically, upon irradiation with light, an acid is generated from the photocationic polymerization initiator, and at the same time, a small amount of radicals is instantaneously generated. For example, when the curable compound contains an epoxy compound and a (meth)acrylic-modified epoxy compound, much of the acid generated by light irradiation is captured by a tertiary amine. Therefore, even when irradiated with light, the epoxy compound hardly cures, allowing the viscosity after light irradiation to be maintained low. On the other hand, the (meth)acrylic-modified epoxy compound can be cured by the small amount of radicals instantaneously generated by light irradiation. This moderately increases the viscosity of the curable composition, making it easier to maintain the applied shape. In this way, the irradiated curable composition can maintain its fluidity and tackiness during lamination and can well maintain the applied shape. As a result, in step 4), the sealing properties of the cured product can be improved while maintaining lamination suitability.

[0109] In step 5), the acid captured by the tertiary amine is released by heating, and the epoxy groups of the epoxy compound or (meth)acrylic-modified epoxy compound react and harden, resulting in sufficient adhesive strength.

[0110] In the above embodiment, the curable composition is mainly used as a sealant for organic EL elements, but the present invention is not limited thereto and the curable composition can also be used as a sealant or adhesive for various elements such as LED elements (including micro LEDs), liquid crystal elements, semiconductor elements, solar cell elements, etc., or as an interlayer filler for touch panels. The curable composition can also be used as a sealant or adhesive applied to a substrate that does not have optical transparency, such as a printed circuit board used in a smart antenna for an electric vehicle or a substrate having a light-shielding portion under wiring used in a dye-sensitized solar cell.

[0111] The present invention will be further described below with reference to examples and comparative examples, but the technical scope of the present invention is not limited thereto.

[0112] 1. Preparation of Materials 1-1. Curable Compounds (A) (1) Epoxy Compound (A1) Epoxy Compound (A1-1): Aromatic trifunctional epoxy compound (VG3101L, manufactured by Printec Co., Ltd., 2-(glycidyloxyphenyl)propylphenyl)-1,1-di(glycidyloxyphenyl)ethane, solid) Epoxy Compound (A1-2): Bisphenol F type epoxy resin (YL983U, manufactured by Mitsubishi Chemical Corporation, bifunctional, liquid)

[0113] (2) (Meth)acrylic-modified epoxy compound (A2) (Meth)acrylic-modified epoxy compound (A2-1): Acrylic-modified bisphenol A-type epoxy resin (manufactured by Shin-Nakamura Chemical Co., Ltd., EA-1010N, molecular weight 400) (Meth)acrylic-modified epoxy compound (A2-2): Acrylic-modified bisphenol A-type epoxy resin (manufactured by Kyoeisha Chemical Co., Ltd., Epoxy Ester 3000A)

[0114] 1-2. Photocationic polymerization initiator (B) CPI-210S (manufactured by San-Apro Co., Ltd.)

[0115] 1-3. Tertiary amine (C) A compound represented by the following formula (Tinuvin 123, manufactured by BASF Japan Ltd.):

[0116] 1-4. Inorganic filler (D) Inorganic filler (D-1): spherical silica (manufactured by Tokuyama Corporation, Sign Seal SP07M, average particle size 0.7 μm) Inorganic filler (D-2): finely divided silica (manufactured by Tokuyama Corporation, HM-30S, average particle size 7 nm) Inorganic filler (D-3): spherical silica (manufactured by Admatechs Co., Ltd., YA-010C, average particle size 10 nm)

[0117] 1-5. Photosensitizer (E) UVS-1331 (manufactured by Airwater Corporation)

[0118] 1-6. Silane coupling agent (F) KBM403 (manufactured by Shin-Etsu Chemical Co., Ltd.)

[0119] 2. Preparation of Curable Composition Example 1 170 parts by mass of epoxy compound (A1-1), 170 parts by mass of epoxy compound (A1-2), 60 parts by mass of (meth)acrylic-modified epoxy compound (A2), 15 parts by mass of photocationic polymerization initiator (B), 5 parts by mass of tertiary amine (C), 500 parts by mass of inorganic filler (D-1), 20 parts by mass of inorganic filler (D-2), 15 parts by mass of inorganic filler (D-3), 5 parts by mass of photosensitizer (E), and 30 parts by mass of silane coupling agent (F) were mixed in a roll kneader to obtain a curable composition.

[0120] Examples 2 to 9, Comparative Examples 1 to 7 Curable compositions were obtained in the same manner as in Example 1, except that the blending amounts of each component were changed as shown in Table 1 or Table 2.

[0121] 3. Evaluation The curable compositions obtained in Examples 1 to 9 and Comparative Examples 1 to 7 were evaluated for (1) viscosity, (2) tackiness after light irradiation, (3) lamination suitability, (4) adhesion test, and (5) shape retention by the following methods.

[0122] (1-1) Viscosity (before light irradiation) The viscosity of the obtained curable composition was measured at 25°C using an E-type viscometer (TVE-35L type viscometer, manufactured by Toki Sangyo Co., Ltd., rotor name: 3° × R9.7) in accordance with the cone and plate viscometer method of JIS K5600-2-3 (2014). The rotation speed of the cone and plate during measurement was 2.5 rotations / minute.

[0123] (1-2) Complex Viscosity (After Light Irradiation) The curable composition was measured using a rheometer (MARSIII) manufactured by Haake Co., Ltd. at a measurement frequency of 1 Hz, a cell gap (thickness of the curable composition at the time of measurement) of 30 μm, and a temperature of 25° C., while being irradiated with UV light from a metal halide lamp at an intensity of 100 mW / cm. 2 The cumulative light intensity is 3000 mJ / cm 2 The complex viscosity was measured after 600 seconds of irradiation.

[0124] (2) Tack after light irradiation Using the obtained curable composition, a coating film having a thickness of 10 μm was formed on a 0.7 mm thick non-alkali glass plate using a bar coater No. 6. The coating film was left at room temperature (25° C.) for 3 minutes while purging with nitrogen. Thereafter, the coating film was irradiated with ultraviolet light (a metal halide lamp with a wavelength of 395 nm, UV irradiance 100 mW / cm). 2 The cumulative light intensity is 3000 mJ / cm 2 ) was irradiated. Next, the coating film was touched with a hand wearing a protective device to check its tackiness. The tackiness after light irradiation was evaluated based on the following criteria: 4: Sufficient tackiness remains 3: Tackiness remains 2: Tackiness remains, although somewhat less 1: No tackiness A rating of 2 or higher was considered to be good.

[0125] (3) Bonding Suitability A first sealant (dam material) was prepared by mixing the above-prepared curable composition with 2% by mass of 5 μm spherical silica spacers. This was applied to a 0.7 mm thick non-alkali glass sheet in a 40 mm × 40 mm shape using a dispenser. The cross-sectional area of ​​the applied curable composition was 5000 μm. 3Next, a second sealant (fill material) was dropped into the area surrounded by the first sealant in an amount equivalent to the volume of the area, and lamination was performed under vacuum. A thermosetting epoxy-based fill material was used as the fill material. The laminated product was removed and heated at 80°C for 60 minutes to obtain a simple panel. The lamination suitability of the obtained simple panel was evaluated based on the following criteria: ○: Lamination was sufficient and the fill material was filled. △: Lamination was successful, but the viscosity of the dam material was too high to close the gap to 5 μm, so the volume of the space surrounded by the dam material remained large, resulting in insufficient filling of the fill material. ×: Lamination was not possible and the upper and lower substrates were not in close contact. A score of ○ was considered good.

[0126] (4) Adhesion Strength The obtained curable composition was applied in a circular pattern using a screen on a non-alkali glass sheet measuring 25 mm x 45 mm x 0.7 mm. The seal pattern was a circle with a diameter of 1 mm. Next, the coating of the curable composition was irradiated with light having a wavelength of 365 nm at an irradiation intensity of 100 mW / cm. 2 After irradiating one of the alkali-free glass sheets with a 0.7 mm thickness for 30 seconds, a pair of alkali-free glass sheets was bonded together and heated in an oven at 80°C for 60 minutes to obtain a laminate sample. The obtained sample was then aged for 24 hours in a thermostatic chamber at 23°C, and then pulled in a tensile testing machine (Intesco Model 210 tensile testing machine) in a direction parallel to the surface at a rate of 2 mm / min, and the stress at this time was measured.

[0127] (5) Shape Retention The shape of the first sealing portion (dam) of the simple panel prepared for the evaluation of the lamination suitability in (3) above was observed using an electron microscope. The shape retention was evaluated according to the following criteria: ○: The shape of the dam was maintained △: The shape of the dam was deformed ×: The dam was broken and the fill material was leaked A rating of ○ was considered good.

[0128] The evaluation results of Examples 1 to 3 and Comparative Examples 1 to 4 are shown in Table 1, and the evaluation results of Examples 4 to 9 and Comparative Examples 5 to 7 are shown in Table 2.

[0129]

[0130]

[0131] As shown in Table 1, the curable compositions of Examples 1 to 3 have lower complex viscosities after light irradiation than the curable compositions of Comparative Examples 1 and 2, and are found to retain tack. This indicates high lamination suitability and good adhesive strength. Furthermore, the curable compositions of Examples 1 to 3 have moderately higher complex viscosities after light irradiation than the curable compositions of Comparative Examples 3 and 4, and are found to have high shape retention when heat-cured.

[0132] Furthermore, as shown in Table 2, the curable compositions of Examples 4 to 9 have a complex viscosity after light irradiation that is appropriately lower than that of the curable compositions of Comparative Examples 6 and 7, and are found to retain sufficient tack. This indicates high lamination suitability and good adhesive strength. Furthermore, the curable compositions of Examples 4 to 9 have a complex viscosity after light irradiation that is appropriately higher than that of the curable composition of Comparative Example 5, and are found to have better shape retention when heat-cured.

[0133] From these findings, it is possible to determine that the tertiary amine is contained in a predetermined amount or more, and that the complex viscosity after light irradiation is 1.0 × 10 3 Pa・s or more 5.0×10 4 The curable compositions of Examples 2 to 6, which were adjusted to a viscosity in the range of Pa s or less, maintained a predetermined tack even after light irradiation and moderately increased in viscosity, and it was found that they were excellent in both lamination suitability and shape retention.

[0134] This application claims priority based on Japanese Patent Application No. 2023-54123, filed March 29, 2023, the entire contents of which are incorporated herein by reference.

[0135] According to the present invention, it is possible to provide a curable composition that has low-temperature curing properties and is capable of achieving both lamination suitability and shape retention.

Claims

1. A composition comprising a curable compound, a photocationic polymerization initiator, and a tertiary amine, the content of the tertiary amine being 20 parts by mass or more per 100 parts by mass of the photocationic polymerization initiator, and irradiating light of a wavelength of 365 nm at an illuminance of 100 mW / cm 2 With an integrated light intensity of 3000 mJ / cm 2 After irradiation, the complex viscosity at 25°C after 600 seconds was 1.0 x 10 3 Pa・s or more 5.0×10 4 The curable composition has a viscosity of 0.1 Pa·s or less.

2. The curable composition according to claim 1, wherein the curable compound comprises an epoxy compound, and at least one of a (meth)acrylic-modified epoxy compound and a (meth)acrylic compound.

3. The curable composition according to claim 1, wherein the content of the tertiary amine is 0.5 parts by mass or more and 20 parts by mass or less per 100 parts by mass of the curable compound.

4. The curable composition according to claim 1, wherein the tertiary amine is a difunctional tertiary amine.

5. The curable composition according to claim 1, wherein the tertiary amine has an N--O bond.

6. The curable composition according to claim 1, wherein the tertiary amine has a hindered structure.

7. A sealant comprising the curable composition according to any one of claims 1 to 6.

8. A frame sealant comprising the curable composition according to any one of claims 1 to 6.

9. A display panel comprising: an element substrate on which elements are arranged; a counter substrate arranged opposite the element substrate with the elements interposed therebetween; and a sealing portion arranged between the element substrate and the counter substrate for sealing the elements, the sealing portion including a cured product of the sealant according to claim 7.

10. A method for manufacturing a display panel, comprising the steps of: applying a first sealant in a frame shape along the periphery of a display area on one surface of either an element substrate or an opposing substrate; filling a second sealant into the area surrounded by the first sealant to form a sealant layer; irradiating the sealant layer with light; bonding one substrate to the other substrate via the sealant layer irradiated with light; and heating and hardening the sealant layer, wherein at least one of the first sealant and the second sealant is the sealant described in claim 7.

Citation Information

Patent Citations

  • Irradiation-cured anti-fouling coiled material coating and preparation method thereof

    CN110885619A

  • Cellulose acylate film, optical film using the film, liquid crystal display device and silver halide photosensitive material

    JP2004099775A

  • Stain resistance-imparting agent, cured product and article

    JP2006160802A

  • Optical sheet

    JP2024052308A

  • Sealing agent for organic el display element, and organic el display device

    WO2021006070A1