Adhesive multilayer sheet

The adhesive laminate sheet, featuring a fluororesin-based adhesive and nonwoven fabric structure with an air layer, addresses the lack of heat insulation and resistance in existing sheets by providing enhanced thermal insulation and maintaining strength at high temperatures, making it suitable for heat-insulating applications.

WO2024204285A1PCT designated stage expired Publication Date: 2024-10-03TOMOEGAWA CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012123
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-26
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Existing adhesive laminate sheets lack both heat insulation properties and heat resistance, despite advancements in heat-resistant tapes, as they do not consider thermal insulation.

Method used

An adhesive laminate sheet with a specific structure, comprising a nonwoven fabric sheet made of fluororesin fibers, an adhesive layer, and a mixed layer impregnated with the adhesive component, along with an air layer, providing porosity of 25% or more and thermal conductivity of 0.15 W/(K·m) or less, ensuring excellent heat insulation and resistance.

Benefits of technology

The adhesive laminate sheet achieves superior heat insulation and heat resistance, maintaining adhesive strength even after exposure to high temperatures, making it suitable for various heat-insulating applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012123_03102024_PF_FP_ABST
    Figure JP2024012123_03102024_PF_FP_ABST
Patent Text Reader

Abstract

Provided is an adhesive multilayer sheet which has excellent thermal insulation properties and excellent heat resistance. One embodiment of the present invention provides an adhesive multilayer sheet in which an adhesive layer and a base material layer are stacked in this order, wherein: the adhesive layer is composed of an adhesive component; and the base material layer comprises a nonwoven fabric sheet that is composed of fluororesin fibers. The base material layer comprises: a mixed layer which is impregnated with the adhesive component, and is provided in the range of 2% to 50% of the thickness of the base material layer from the adhesive layer-side main surface of the base material layer toward the other main surface; and an air layer which contains air and is provided in the range of 50% to 98% of the thickness of the base material layer from the mixed layer toward the other main surface. The porosity of the entire adhesive multilayer sheet is 25% or more. The adhesive component in the adhesive layer and the adhesive component in the mixed layer are integrated with each other. The change ratio (A2 / A1) of the adhesive force A2 of the adhesive layer after heating at 200°C for 300 hours to the adhesive force A1 of the adhesive layer at 23°C and the humidity of 50% is 0.40 or more.
Need to check novelty before this filing date? Find Prior Art

Description

Adhesive laminated sheet

[0001] The present invention relates to an adhesive laminate sheet.

[0002] Adhesive sheets have been developed that are intended to be exposed to a hot environment.

[0003] For example, Patent Document 1 discloses a heat-resistant tape that includes a substrate layer and a pressure-sensitive adhesive layer, in which the substrate layer is a glass fiber fabric impregnated with a fluorine-containing resin, and in which a silicon-containing agent is present between the glass fiber fabric and the fluorine-containing resin.

[0004] Patent No. 7132919

[0005] The adhesive tape disclosed in Patent Document 1 is said to provide a heat-resistant tape with high productivity, but does not take into consideration heat insulation properties.

[0006] Therefore, an object of the present invention is to provide an adhesive laminated sheet having excellent heat insulation and heat resistance.

[0007] As a result of extensive research, the present inventors have found that the above-mentioned problems can be solved by an adhesive laminated sheet having a predetermined structure.

[0008] A first aspect of the present invention is an adhesive laminated sheet comprising an adhesive layer and a base layer laminated in this order, wherein the adhesive layer is made of an adhesive component, the base layer comprises a nonwoven fabric sheet made of fluororesin fibers, the base layer comprises: a mixed layer impregnated with the adhesive component, the mixed layer being provided from the adhesive layer side main surface of the base layer toward the other main surface thereof in a range of 2% to 50% of the thickness of the base layer, and an air layer containing air, the mixed layer being provided from the mixed layer toward the other main surface thereof in a range of 50% to 98% of the thickness of the base layer, the porosity of the adhesive laminated sheet being 25% or more, the adhesive component of the adhesive layer and the adhesive component of the mixed layer being integral, and the adhesive strength A of the adhesive layer at 23°C and a humidity of 50% 1 Adhesion strength A of the adhesive layer after heating at 200°C for 300 hours 2 The rate of change of (A 2 / A 1 ) is 0.40 or more.

[0009] The adhesive component is preferably a fluororesin adhesive component.

[0010] a mixed layer impregnated with the adhesive component, the mixed layer being provided from the adhesive layer side main surface of the base layer toward the other main surface thereof, and covering a range of 2% to 50% of the thickness of the base layer; and an air layer containing air, the mixed layer being provided from the adhesive layer side main surface of the base layer toward the other main surface thereof, and covering a range of 50% to 98% of the thickness of the base layer; the porosity of the adhesive laminated sheet being 25% or more; and the adhesive component of the adhesive layer and the adhesive component of the mixed layer being integral with each other.

[0011] The double-sided pressure-sensitive adhesive laminate sheet of the first embodiment and the double-sided pressure-sensitive adhesive laminate sheet of the second embodiment preferably have the following configuration: The thermal conductivity is preferably 0.15 W / (K·m) or less. The adhesive strength A of the pressure-sensitive adhesive layer at 23°C and a humidity of 50% 1 Adhesion strength A of the adhesive layer after heating at 200°C for 300 hours 2 The rate of change of (A 2 / A 1 ) is preferably 0.40 or more. The fluororesin fiber is preferably at least PTFE, PFA, or FEP. The thickness of the adhesive layer is preferably equal to or less than the thickness of the base layer. The thickness of the base layer is preferably 20 μm to 1000 μm. The thickness of the adhesive layer is preferably 5 μm to 1000 μm.

[0012] According to the present invention, there is provided an adhesive laminated sheet having excellent heat insulation and heat resistance.

[0013] Fig. 1 is a schematic diagram of an adhesive laminate sheet, and Fig. 2 is a diagram summarizing the relationship between porosity and thermal conductivity in each example and each comparative example.

[0014] Hereinafter, when an upper limit value and a lower limit value are separately described, it is considered that a numerical range combining any upper limit value and any lower limit value is substantially disclosed.

[0015] In the following, unless otherwise specified, various measurements are carried out at room temperature (23° C.).

[0016] Hereinafter, an adhesive laminated sheet 10 according to the present invention will be described mainly with reference to FIG. 1, but the present invention is not limited thereto in any way.

[0017] <<<Structure of Adhesive Laminated Sheet 10 >>> The adhesive laminated sheet 10 according to the present invention is an adhesive laminated sheet in which an adhesive layer 1 and a base layer A are laminated in this order.

[0018] On the surface of the adhesive laminated sheet 10, another layer (for example, a protective film, etc.) may be laminated.

[0019] <<Adhesive Layer 1>> The adhesive layer 1 is made of an adhesive component. In other words, the adhesive layer 1 is configured of an adhesive component.

[0020] The adhesive component is preferably a heat-resistant adhesive component, in other words, the adhesive layer 1 is preferably made of a heat-resistant adhesive component.

[0021] In the present invention, the adhesive component constituting the adhesive laminate sheet 10 "has heat resistance" means that in the adhesive laminate sheet, the adhesive strength A of the adhesive layer 1 at 23°C and humidity 50% is 1 Adhesion strength A of adhesive layer 1 after heating at 200°C for 300 hours 2 The rate of change of (A 2 / A 1 ) is 0.40 or more.

[0022] The resin that is the main component of the adhesive component is not particularly limited. Examples of the adhesive component include a fluororesin-based adhesive component and a silicone resin-based adhesive component. The adhesive component is preferably a fluororesin-based adhesive component because it is compatible with the nonwoven fabric sheet made of fluororesin fibers. Examples of fluororesins that constitute the fluororesin-based adhesive component include copolymers containing fluorine-based monomers such as vinylidene fluoride, hexafluoropropylene, and tetrafluoroethylene.

[0023] Furthermore, if the adhesive component according to the present invention is a fluororesin-based adhesive component, it can be an adhesive component that does not contain a silicone resin-based adhesive component (silicone-free), which is preferable because it can reduce environmental pollution and product defects due to decomposition products.

[0024] The adhesive component may contain other additives to the extent that the effects of the present invention are not impaired. Examples of other additives include fillers, antioxidants, heat stabilizers, light stabilizers, antistatic agents, flame retardants, plasticizers, tackifiers, pigments, etc. The content of other additives in the adhesive component is, for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, etc., when the entire adhesive component is taken as 100% by mass.

[0025] Thickness T of adhesive layer 1 1 is not particularly limited, and is preferably 5 μm to 1000 μm, 7 μm to 500 μm, or 10 μm to 200 μm.

[0026] Total thickness T of the adhesive laminated sheet 10 10 The thickness T of the adhesive layer 1 1 The ratio (T 1 / T 10 ) is preferably 0.01 or more, 0.02 or more, or 0.05 or more, and is preferably 0.50 or less, 0.45 or less, or 0.40 or less.

[0027] Here, the thickness T of the adhesive layer 1 1 is the thickness T of the base material layer A A Specifically, the thickness T of the base material layer A is preferably A The thickness T of the adhesive layer 1 1 The thickness ratio (T 1 / TA ) is preferably 1.00 or less, 0.80 or less, or 0.60 or less. 1 / T A The lower limit of ) is not particularly limited, but is, for example, 0.01, 0.03, or 0.05.

[0028] <<Base Material Layer A>> The base material layer A includes a nonwoven fabric sheet (not shown) made of fluororesin fibers, and has an area where the nonwoven fabric sheet is impregnated with an adhesive component and an area where the nonwoven fabric sheet is not impregnated with an adhesive component.

[0029] More specifically, in the thickness direction, the base material layer A has a main surface S on the adhesive layer 1 side. A1 (the main surface in contact with the adhesive layer 1) to the other main surface S A2 A mixed layer A1 is formed toward the other main surface S, and is an area impregnated with an adhesive component. A2 and an air layer A0 containing air formed toward the

[0030] Here, the nonwoven fabric sheet constituting the substrate layer A is porous. When the porous nonwoven fabric sheet comes into contact with the paint or coating film, the adhesive component penetrates into the pores of the nonwoven fabric sheet, forming a mixed layer containing fibers and the adhesive component. Furthermore, the areas of the nonwoven fabric sheet that have not been penetrated by the adhesive component maintain the porous state inherent to the nonwoven fabric sheet, forming an air layer containing air. In this way, the substrate layer A includes a mixed layer and an air layer.

[0031] In the base layer A of the present invention, the adhesive component constituting the adhesive layer 1 and the adhesive component constituting the mixed layer A1 are integrated (continuous). By adopting such a structure in which the adhesive component of the adhesive layer 1 and the adhesive component of the mixed layer A1 are integrated, it is possible to increase the adhesive strength between the adhesive layer and the base layer.

[0032] As the nonwoven fabric sheet constituting the base material layer A, a conventionally known one can be used.

[0033] The fluororesin fibers constituting the nonwoven fabric sheet are not particularly limited, and examples include fibers made from polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), etc. From the viewpoint of improving heat resistance, the fluororesin constituting the fluororesin fibers is preferably PTFE, PFA or FEP.

[0034] The fiber diameter and fiber length of the fluororesin fibers and the density of the nonwoven fabric sheet may be appropriately adjusted taking into consideration the porosity of the base layer A (or the porosity of the air layer A0), strength, ease of impregnation with the adhesive component, etc.

[0035] Thickness T of base material layer A A is not particularly limited, and is preferably 20 μm to 1000 μm, 50 μm to 800 μm, or 100 μm to 500 μm.

[0036] <Air Layer A0> The air layer A0 is a layer formed by a nonwoven fabric sheet, and air is held by the nonwoven fabric sheet. In other words, the air layer A0 usually contains air and a nonwoven fabric fiber sheet.

[0037] The air layer A0 is provided in a range of 50% to 98% of the thickness of the base material layer A. In other words, the thickness T A The thickness T of the air layer A0 A0 The proportion of ([T A0 / T A ] × 100) is 50% to 98%. A0 / T A ]×100 is preferably 60% or more, 70% or more, or 80% or more, and is preferably 96% or less, 95% or less, or 94% or less.

[0038] Thickness T of air layer A0 A0 is not particularly limited, but is preferably 10 μm to 500 μm, 50 μm to 500 μm, or 100 μm to 500 μm.

[0039] <Mixed Layer A1> The nonwoven fabric sheet constituting the mixed layer A1 is the same as the nonwoven fabric sheet constituting the air layer A0, and therefore a description thereof will be omitted.

[0040] The adhesive component constituting the mixed layer A1 is the same as the adhesive component constituting the adhesive layer 1, and therefore a description thereof will be omitted.

[0041] The mixed layer A1 is provided to have a thickness in the range of 2% to 50% of the thickness of the base layer A. The upper limit is preferably 45% or less, 35% or less, 25% or less, 15% or less, or 10% or less. By setting the impregnation ratio of the mixed layer A1 in such a range, it is easy to obtain an adhesive laminate sheet with an excellent balance of adhesive strength, heat insulation, etc.

[0042] Thickness T of mixed layer A1 A1 is not particularly limited, but is preferably 1 μm to 100 μm, 2 μm to 50 μm, or 5 μm to 30 μm.

[0043] <<<Physical properties / characteristics of adhesive laminate sheet 10>>> <<Porosity>> The porosity of the adhesive laminate sheet 10 is 25% or more. The porosity of the adhesive laminate sheet 10 is preferably 30% or more. The upper limit of the porosity of the adhesive laminate sheet 10 is not particularly limited, and is preferably, for example, 60.0%, 70.0%, or 80.0%. By setting the porosity of the adhesive laminate sheet 10 within this range, it is easy to obtain an adhesive laminate sheet with excellent heat insulation properties.

[0044] The porosity of the adhesive laminate sheet 10 is calculated as ([Volume of air layer A0] / [Volume of adhesive laminate sheet 10]) x [Volume % of air in air layer A0], or ([Volume of air layer A0] x [Volume % of air in air layer A0]) / [Volume of adhesive laminate sheet 10].

[0045] The porosity of the adhesive laminated sheet 10 can be adjusted by the thickness of each layer, etc.

[0046] <<Thermal Conductivity>> The adhesive laminate sheet 10 preferably has a thermal conductivity of 0.15 W / (K·m) or less, 0.12 W / (K·m) or less, or 0.10 W / (K·m) or less. When the adhesive laminate sheet 10 satisfies such a thermal conductivity, it is likely to exhibit sufficient functionality as a heat-insulating adhesive sheet.

[0047] The thermal conductivity (k) of the adhesive laminate sheet 10 is calculated by the transient method from the "thermal diffusivity," "density," and "specific heat" using the following formula. The thermal diffusivity is measured on a double-sided adhesive laminate sheet 10 cut into a 5 cm square using an ultra-high sensitivity thermal diffusivity measuring device for thin films (ai-Phase Mobile M3 Type 1, manufactured by Ai-Phase Corporation) in accordance with ISO 22007-3. The specific heat is measured on a double-sided adhesive laminate sheet 10 cut into a 5 cm square using a differential scanning calorimeter (DSC) (DSC6200, manufactured by Hitachi, Ltd.) in accordance with JIS K 7123. The density is calculated from the weight of the double-sided adhesive laminate sheet 10 cut into a 5 cm square measured using a balance and the volume value of the double-sided adhesive laminate sheet 10 calculated in the "porosity calculation" section above. k = αρC P (k: thermal conductivity [W / (m・K)], α: thermal diffusivity [m 2 / s], ρ: density [kg / m 3 ], C P : specific heat (constant pressure specific heat) [J / (Kg K)])

[0048] <<Adhesive Strength>> The adhesive laminate sheet 10 has an adhesive strength A of the adhesive layer 1 at 23°C and a humidity (relative humidity) of 50%. 1 Adhesion strength A of adhesive layer 1 after heating at 200°C for 300 hours 2 The rate of change of (A 2 / A 1 ) is preferably 0.40 or more, 0.60 or more, or 1.00 or more.

[0049] When the adhesive laminate sheet 10 satisfies such adhesive strength, it is likely to exhibit sufficient functionality as a heat-resistant adhesive sheet.

[0050] The adhesive strength of the adhesive laminate sheet 10 was evaluated by polishing the surface of an aluminum alloy (A5052) aluminum plate with sandpaper in advance, and then laminating the adhesive layer surface of the adhesive laminate sheet 10, cut to a size of 5 cm x 5 mm, to the polished surface using a hand roller. The evaluation objects were divided into two conditions: (1) immediately after lamination, and (2) after lamination, heated in an oven at 200°C for 300 hours, and then cooled at room temperature for 1 hour. Measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. Measurements were performed five times under each of the above conditions (1) and (2), and the average value was used to determine the adhesive strength.

[0051] Adhesion strength A of adhesive layer 1 1 is not particularly limited, and is preferably 0.05 [N / 5 mm] or more, 0.1 [N / 5 mm] or more, or 0.2 [N / 5 mm] or more. 2 is not particularly limited, and is preferably 0.05 [N / 5mm] or more, 0.1 [N / 5mm] or more, 0.2 [N / 5mm] or more, 0.3 [N / 5mm] or more, or 0.5 [N / 5mm] or more.

[0052] <<<Method for Manufacturing the Adhesive Laminated Sheet 10 >>> The adhesive laminated sheet 10 can be manufactured according to a conventionally known method as long as the method is capable of maintaining the air layer A0 within the layer.

[0053] A predetermined adhesive paint (a composition containing an adhesive and a solvent) is applied to a predetermined nonwoven fabric sheet and dried, or a previously prepared adhesive paint film is placed adjacent to the sheet and pressed, and the adhesive laminate sheet 10 including the substrate layer A can be obtained by controlling the air layer derived from the nonwoven fabric sheet and the mixed layer, which is the region impregnated with the adhesive component, to have an appropriate shape. The adhesive laminate sheet 10 can be produced, for example, by the following method. An adhesive paint containing an adhesive that serves as the adhesive component and an appropriate solvent is applied onto a release film (such as a PET film), and then the adhesive paint is dried to form a film provided with an adhesive layer consisting of the adhesive component. The adhesive layer consisting of the adhesive component provided on the release film and one main surface of the nonwoven fabric sheet (main surface S on the adhesive layer 1 side) are then applied to the release film. A1) are brought into contact with the nonwoven fabric sheet, and while applying pressure (and heat as needed), a pressure-sensitive adhesive layer made of a pressure-sensitive adhesive component is pressed into the nonwoven fabric sheet, thereby impregnating a part of the pressure-sensitive adhesive component into the nonwoven fabric sheet, thereby forming a mixed layer A1. The part of the pressure-sensitive adhesive layer that has not been impregnated into the nonwoven fabric sheet becomes the pressure-sensitive adhesive layer 1. At this time, the pressure-sensitive adhesive layer is pressed to a depth, etc., so that the pressure-sensitive adhesive layer is pressed into the other main surface S of the nonwoven fabric sheet. A2 An air layer A0, which is an area where no adhesive component is present, is formed from the side toward the mixed layer A1. The release film is removed as needed to obtain the adhesive laminate sheet 10. In this manufacturing method, since the nonwoven fabric sheet is pressurized, the thickness of the nonwoven fabric sheet at the raw material stage may differ from that of the nonwoven fabric sheet at the stage of the adhesive laminate sheet 10. In order to set the thickness of the base material layer A within the desired range, the nonwoven fabric sheet may be compressed in advance, or a nonwoven fabric sheet with a thickness that takes into account deformation of the nonwoven fabric sheet may be used.

[0054] It should be noted that the manufacturing method of the adhesive laminated sheet 10 is not limited to this. For example, the manufacturing method of the adhesive laminated sheet 10 may be a method in which an adhesive coating before drying is directly applied to a nonwoven fabric sheet, and the adhesive coating is dried while adjusting the impregnation of the adhesive coating into the nonwoven fabric sheet so that an air layer remains in the layer of the adhesive laminated sheet 10, thereby forming a mixed layer and an adhesive layer.

[0055] <<<<Uses of Adhesive Laminate Sheet 10 >>> The double-sided adhesive laminate sheet 10 according to the present invention has a predetermined air layer, and therefore has excellent heat insulating properties and conformability, and can therefore be suitably used for various heat insulating or heat resistant applications.

[0056] Next, the present invention will be explained in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples in any way.

[0057] <<Preparation of Adhesive Laminated Sheet>> An adhesive laminated sheet was prepared as follows: The measurement methods used in this preparation are as follows.

[0058] <Measurement of Adhesive Layer Thickness> The thickness of the adhesive layer was measured using a micrometer (MDH-25MC, manufactured by Mitutoyo Corporation) and the average value was calculated by measuring five points at each of the four corners of the main surface of a 5 cm square cut adhesive layer.

[0059] <Adhesive Strength Measurement of Adhesive Layer> The adhesive strength of the adhesive layer was measured by polishing the surface of an aluminum alloy (A5052) aluminum plate with sandpaper in advance, and then peeling off one PET film from a double-sided PET film-attached adhesive layer cut to a size of 5 cm x 5 mm, and laminating the exposed adhesive layer surface to the polished surface with a hand roller. Measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. The measurement was performed a total of five times, and the average value was taken as the adhesive strength.

[0060] Example 1 A copolymer resin composed of TFE and propylene was dispersed in tetrahydrofuran (THF) to a concentration of 20 wt %, to prepare Coating 1. Subsequently, Coating 1 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain Single-Sided PET Film Composition 1. Furthermore, the treated surface of Release PET Film 2, which has a lighter release property than Release PET Film 1, was laminated to the Composition 1 side of Single-Sided PET Film Composition 1 using a laminator at room temperature and 0.1 MPa to obtain Double-Sided PET Film-Attached Adhesive Layer 1. The Adhesive Layer 1 had a thickness of 25 μm and an adhesive strength of 0.1 N / 5 mm. Then, the release PET film 2 of the adhesive layer 1 with double-sided PET film was peeled off to expose the adhesive layer 1 side, and then a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 1 side using a laminator under conditions of 120°C and 0.3 MPa, thereby obtaining an adhesive laminate sheet 1 with a single-sided PET film, in which the nonwoven fabric sheet was partially impregnated with the adhesive of the adhesive layer 1.

[0061] Example 2 Two double-sided PET film-attached adhesive layers 1 were prepared as in Example 1. Subsequently, the release PET films 2 were peeled off from each of the two double-sided PET film-attached adhesive layers 1 to expose the adhesive layer 1 surfaces. The two exposed adhesive layer 1 surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 2. The thickness of the adhesive layer 2 was 50 μm. One of the release PET films 1 from the double-sided PET film-attached adhesive layer 2 was then peeled off to expose the adhesive layer 2 surface. A nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) composed of fluororesin fibers was then thermally laminated to the exposed adhesive layer 2 surface using a laminator at 120°C and 0.3 MPa to obtain a single-sided PET film-attached adhesive laminate sheet 2 in which the adhesive from the adhesive layer 2 was partially impregnated into the nonwoven fabric sheet.

[0062] Example 3 Two double-sided PET film-attached adhesive layers 2 were prepared as in Example 2. Subsequently, the release PET film 1 was peeled off from each of the two double-sided PET film-attached adhesive layers 2 to expose the adhesive layer 2 surface. The two exposed adhesive layer 2 surfaces were then laminated together using a laminator at room temperature and 0.1 MPa to obtain a double-sided PET film-attached adhesive layer 3. The thickness of the adhesive layer 3 was 100 μm. One of the release PET films 1 from the double-sided PET film-attached adhesive layer 3 was then peeled off to expose the adhesive layer 3 surface. A nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) composed of fluororesin fibers was then thermally laminated to the exposed adhesive layer 3 surface using a laminator at 120°C and 0.3 MPa to obtain a single-sided PET film-attached adhesive laminate sheet 3 in which the adhesive of the adhesive layer 3 was partially impregnated into the nonwoven fabric sheet.

[0063] Example 4 An adhesive layer 2 with double-sided PET films prepared in Example 2 and an adhesive layer 3 with double-sided PET films prepared in Example 3 were prepared. Next, the release PET films 1 were peeled off from the two prepared adhesive layers 2 with double-sided PET films and adhesive layer 3 with double-sided PET films to expose the surfaces of adhesive layer 2 and adhesive layer 3, and then the two exposed adhesive layer surfaces were laminated together using a laminator at room temperature and 0.1 MPa to obtain an adhesive layer 4 with double-sided PET films. The thickness of adhesive layer 4 was 150 μm. Then, one of the release PET films 1 of the double-sided PET film-attached adhesive layer 4 was peeled off to expose the adhesive layer 4 side, and then a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber was thermally laminated to the exposed adhesive layer 4 side as a substrate using a laminator at 120°C and 0.3 MPa, thereby obtaining an adhesive laminate sheet 4 with a single PET film on one side, in which the nonwoven fabric sheet was partially impregnated with the adhesive of the adhesive layer 4.

[0064] Comparative Example 1 The double-sided PET film-attached adhesive layer 3 produced in Example 3 and the double-sided PET film-attached adhesive layer 4 produced in Example 4 were produced. Next, the release PET film 1 was peeled off from the double-sided PET film-attached adhesive layer 3 and the double-sided PET film-attached adhesive layer 4 produced to expose the adhesive layer 2 and adhesive layer 4 surfaces, and then the two exposed adhesive layer surfaces were laminated together using a laminator at room temperature and 0.1 MPa to produce the double-sided PET film-attached adhesive layer 5. The thickness of the adhesive layer 5 was 250 μm. Then, one of the release PET films 1 of the double-sided PET film-attached adhesive layer 5 was peeled off to expose the adhesive layer 5 surface, and then a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber was thermally laminated to the exposed adhesive layer 5 surface as a substrate using a laminator at 120°C and 0.3 MPa, thereby obtaining an adhesive laminate sheet 5 with a single PET film surface, in which the nonwoven fabric sheet was partially impregnated with the adhesive of the adhesive layer 5.

[0065] Comparative Example 2 A copolymer resin composed of EA, 2EHA, and 2HEA was dispersed in ethyl acetate to a concentration of 30 wt %, to prepare Coating 2. Subsequently, Coating 2 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain Single-sided PET film-attached Composition 2. Furthermore, the treated surface of Release PET film 2, which has a lighter release property than Release PET film 1, was laminated to the Composition 2 side of Single-sided PET film-attached Composition 2 using a laminator at room temperature and 0.1 MPa to obtain Double-sided PET film-attached Adhesive Layer 6. The Adhesive Layer 6 had a thickness of 25 μm and an adhesive strength of 2.0 N / 5 mm. Then, the release PET film 2 of the adhesive layer 6 with double-sided PET film was peeled off to expose the adhesive layer 6 side, and then a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber as a substrate was thermally laminated to the exposed adhesive layer 6 side using a laminator under conditions of 120°C and 0.3 MPa, thereby obtaining an adhesive laminate sheet 6 with a single-sided PET film, in which the nonwoven fabric sheet was partially impregnated with the adhesive of the adhesive layer 6.

[0066] Comparative Example 3 A resin composed of a styrene copolymer, an aromatic hydrocarbon resin, and a polyolefin resin was dispersed in toluene to a concentration of 30 wt %, to prepare Coating 3. Subsequently, Coating 3 was applied to the treated surface of a 38 μm-thick release PET film 1 using an applicator, and then dried at 90°C for 3 minutes to obtain Single-Sided PET Film Composition 3. Furthermore, the treated surface of Release PET Film 2, which has a lighter release property than Release PET Film 1, was laminated to the Composition 3 surface of Single-Sided PET Film Composition 3 using a laminator at room temperature and 0.1 MPa to obtain Double-Sided PET Film-Attached Adhesive Layer 7. The thickness of Adhesive Layer 7 was 27 μm, and the adhesive strength was 0.9 N / 5 mm. Then, the release PET film 2 of the adhesive layer 7 with double-sided PET film was peeled off to expose the adhesive layer 7 surface, and then a nonwoven fabric sheet (Tomyfirec F, manufactured by Tomoegawa Paper Co., Ltd.) made of fluororesin fiber was thermally laminated to the exposed adhesive layer 7 surface as a substrate using a laminator at 120°C and 0.3 MPa, thereby obtaining an adhesive laminate sheet 7 with a single-sided PET film, in which the nonwoven fabric sheet was partially impregnated with the adhesive of the adhesive layer 7.

[0067] <Examples 5-8, Comparative Examples 4 and 5> Single-sided PET film-attached adhesive laminate sheets according to Examples 5-8 and Comparative Examples 4 and 5 were obtained in the same manner as in Example 1, except that the thickness of the air layer, the thickness of the adhesive layer, the volume ratio of the mixed layer, the total thickness, and the porosity were changed as shown in Table 1.

[0068] <<Measurements and Calculations of Adhesive Laminate Sheets>> The following measurements and calculations were carried out on each of the single-sided PET film-attached adhesive laminate sheets obtained above in Examples 1 to 4 and Comparative Examples 1 to 3. The results obtained are shown in Table 1. A graph of thermal conductivity versus porosity is shown in Figure 2.

[0069] <Thickness Measurement> Each single-sided PET film-attached adhesive laminate sheet cut into a 5 cm square was cut perpendicular to the main surface to expose the cross section of each single-sided PET film-attached adhesive laminate sheet. The exposed cross section was subjected to image analysis using a microscope (VHX-8000, manufactured by Keyence Corporation) to measure the thickness of each adhesive laminate sheet and the thicknesses of the "adhesive layer," "air layer," and "mixed layer" therein. Each thickness was measured at 20 random locations in the width direction (direction perpendicular to the perpendicular direction) of the exposed cross section of the single-sided PET film-attached adhesive laminate sheet, and the average value was calculated.

[0070] <Calculation of void ratio> The void ratio was calculated as the ratio of the volume of air in the air layer to the volume of the adhesive laminate sheet. To calculate the volume of the air layer, first, the void ratio of the substrate (nonwoven fabric sheet) was calculated using the following formula. The apparent density of the substrate was measured by a geometric measurement method in accordance with JIS Z 8807, and a value measured using the geometric measurement method was used. Substrate void ratio (%) = (1 - (apparent density of substrate / true density of substrate fiber material)) x 100 The substrate void ratio was calculated using the above formula, and the volume of air in the air layer was calculated by multiplying this substrate void ratio by the apparent volume of the air layer calculated using the thickness of the air layer in the above "thickness measurement". Subsequently, the volume of the adhesive laminate sheet was calculated using the thickness of the adhesive laminate sheet in the above "thickness measurement". The ratio of the volume of air in the air layer to the volume of the adhesive laminate sheet obtained from the above was calculated as the void ratio.

[0071] <Calculation of Thermal Conductivity> The thermal conductivity (k) was calculated by the unsteady method from "thermal diffusivity," "density," and "specific heat" using the following formula. The "thermal diffusivity" and "specific heat" were values ​​measured by the methods described below. The "density" was calculated from the weight of the adhesive laminate sheet cut into 5 cm squares measured on a balance and the volume value of the adhesive laminate sheet calculated in the "void ratio calculation" above. k = αρC P (k: thermal conductivity [W / (m・K)], α: thermal diffusivity [m 2 / s], ρ: density [kg / m 3 ], C P : specific heat (constant pressure specific heat) [J / (Kg K)])

[0072] <Thermal Diffusivity Measurement> The thermal diffusivity measurement was carried out on an adhesive laminated sheet cut into a 5 cm square using an ultra-high sensitivity thermal diffusivity measuring device for thin films (ai-Phase Mobile M3 Type 1, manufactured by ai-Phase Corporation) in accordance with ISO 22007-3.

[0073] <Specific Heat Measurement> Specific heat measurement was carried out on an adhesive laminate sheet cut into a 5 cm square using a differential scanning calorimeter (DSC) (DSC6200, manufactured by Hitachi, Ltd.) in accordance with JIS K 7123.

[0074] <Adhesive Strength Measurement> The adhesive strength of the adhesive laminate sheet was measured by polishing the surface of an aluminum alloy (A5052) aluminum plate with sandpaper in advance, and then peeling off the PET film from a single-sided adhesive laminate sheet cut to a size of 5 cm x 5 mm. The PET film was then peeled off to expose the adhesive layer, which was then bonded to the polished surface with a hand roller. The evaluation samples were divided into two conditions: (1) immediately after lamination, and (2) after lamination, heated in an oven at 200°C for 300 hours, and then cooled at room temperature for 1 hour. Measurements were performed using a Tensilon universal testing machine (RTC-1210, manufactured by A&D Manufacturing) at a peel angle of 90° and a peel speed of 50 mm / min. Measurements were performed five times under each of the above conditions (1) and (2), and the average value was used as the adhesive strength.

[0075]

[0076] As described above, from this example, an adhesive laminated sheet having excellent heat insulation properties (for example, thermal conductivity of 0.15 W / (K·m) or less) and heat resistance could be obtained.

[0077] 10: adhesive laminated sheet 1: adhesive layer A: substrate layer A0: air layer A1: mixed layer

Claims

1. An adhesive laminated sheet having an adhesive layer and a base layer laminated in this order, wherein the adhesive layer is made of an adhesive component, the base layer includes a nonwoven fabric sheet made of fluororesin fibers, the base layer includes: a mixed layer impregnated with the adhesive component, the mixed layer being provided from the adhesive layer side main surface of the base layer toward the other main surface in a range of 2% to 50% of the thickness of the base layer, and an air layer including air, the mixed layer being provided from the mixed layer toward the other main surface in a range of 50% to 98% of the thickness of the base layer, the porosity of the adhesive laminated sheet being 25% or more, the adhesive component of the adhesive layer and the adhesive component of the mixed layer being integral, and the adhesive strength A of the adhesive layer at 23°C and humidity of 50% 1 Adhesive strength A of the adhesive layer after heating at 200° C. for 300 hours 2 The rate of change of (A 2 / A 1 ) is 0.40 or more.

2. The adhesive laminate sheet according to claim 1, wherein the adhesive component is a fluororesin-based adhesive component.

3. An adhesive laminated sheet having an adhesive layer and a base layer laminated in this order, wherein the adhesive layer is made of an adhesive component which is a fluororesin-based adhesive component, the base layer comprises a nonwoven fabric sheet made of fluororesin fibers, the base layer comprises: a mixed layer impregnated with the adhesive component, which is provided from the adhesive layer side main surface of the base layer toward the other main surface and is in a range of 2% to 50% of the thickness of the base layer, and an air layer containing air, which is provided from the mixed layer toward the other main surface and is in a range of 50% to 98% of the thickness of the base layer, the porosity of the adhesive laminated sheet being 25% or more, and the adhesive component of the adhesive layer and the adhesive component of the mixed layer being integral.

4. The adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the thermal conductivity is 0.15 W / (K·m) or less.

5. The adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the fluororesin fibers are at least PTFE, PFA or FEP.

6. The adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the thickness of the adhesive layer is equal to or less than the thickness of the base layer.

7. The adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the thickness of the base layer is 20 µm to 1000 µm.

8. The adhesive laminate sheet according to any one of claims 1 to 3, characterized in that the adhesive layer has a thickness of 5 µm to 1000 µm.

Citation Information

Patent Citations

  • Tape or sheet for sticking nonwoven fluororesin fabric

    JP2003138231A

  • Heat insulating structure and heat insulating tool kit for pipe arrangement

    JP2005106145A

  • Double-sided pressure-sensitive adhesive tape

    JP2005187539A

  • Polyimide resin composition and adhesive sheet

    JP2016132736A

  • Heat insulation fabric

    JP2017047551A