Recycled styrene-based resin composition and molded article comprising same

The recycled styrenic resin composition, with a balanced blend of recycled and virgin styrenic materials, addresses the challenges of extrudability and appearance in conventional compositions, achieving high performance and reduced environmental impact.

WO2024204320A1PCT designated stage expired Publication Date: 2024-10-03TOYO STYRENE CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012207
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-31
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional recycled styrenic resin compositions face challenges in maintaining high extrudability and impact resistance, especially with high recycled material content, and often suffer from poor appearance due to foreign matter and variable waste composition.

Method used

A recycled styrenic resin composition comprising a blend of recycled styrenic material and virgin styrenic material, with specific ratios and properties such as ash content, molecular weight, and magnetic attraction rate, optimized to enhance extrudability and impact resistance while reducing the environmental impact of virgin material usage.

Benefits of technology

The composition achieves high extrudability and impact resistance, along with excellent molded product appearance, suitable for applications in office automation, home appliances, and miscellaneous goods, while minimizing the environmental load by increasing recycled material content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
  • Figure JPOXMLDOC01-APPB-T000002
    Figure JPOXMLDOC01-APPB-T000002
Patent Text Reader

Abstract

Provided are a recycled styrene-based resin composition that has high extrudability and impact resistance even when the styrene-based recycled material content is high, and a molded article that is obtained by molding the recycled styrene-based resin composition and has an excellent molded article appearance. The recycled styrene-based resin composition includes a styrene-based recycled material (A) and a styrene-based virgin material (B), and is characterized in that the ash content of the recycled styrene-based resin composition after firing at 550°C is 2.5 mass% or less, and the mass average molecular weight (Mw) of the recycled styrene-based resin composition is 170,000 or greater.
Need to check novelty before this filing date? Find Prior Art

Description

Recycled styrene resin composition and molded article made thereof

[0001] The present invention relates to a recycled styrene-based resin composition that has high extrudability and impact resistance even when the content of recycled styrene-based material is high, and to a molded article obtained by molding the recycled styrene-based resin composition, which has excellent appearance.

[0002] In recent years, growing awareness of environmental issues has led to a growing trend toward using recycled materials in plastic parts for home appliances and office equipment. However, recycled materials often have poor physical properties due to deterioration or the presence of foreign matter, and the types and amounts of discarded equipment collected are not consistent. This has made it difficult to consistently manufacture recycled materials, ensure they have the impact strength required for plastic parts, or achieve a good appearance.

[0003] JP 2009-149768 A JP 2020-7424 A

[0004] An object of the present invention is to provide a recycled styrene-based resin composition that has high extrudability and impact resistance even when it has a high content of recycled styrene material, and a molded article obtained by molding the recycled styrene-based resin composition that has excellent appearance.

[0005] (1). A recycled styrene-based resin composition comprising a styrene-based recycled material (A) and a styrene-based virgin material (B), wherein the recycled styrene-based resin composition has an ash content of 2.5% by mass or less after baking at 550°C, and the recycled styrene-based resin composition has a mass average molecular weight (Mw) of 170,000 or more. (2). The recycled styrene-based resin composition according to (1), wherein the ash content includes at least one element selected from the group consisting of Si and Al. (3). The recycled styrene-based resin composition according to (1) or (2), wherein the ratio of the mass of the styrene-based recycled material (A) to the mass of the styrene-based virgin material (B) in the recycled styrene-based resin composition is 10 / 90 to 90 / 10. (4). The recycled styrene-based resin composition according to any one of (1) to (3), wherein the magnetic attraction rate of the recycled styrene-based resin composition is 0.2% by mass or less. (5). A molded article obtained by molding the recycled styrene-based resin composition according to any one of claims 1 to 4.

[0006] The recycled styrene-based resin composition of the present invention has high extrudability and impact resistance even when it has a high recycled material content, and the molded product has excellent appearance, so that molded articles of the recycled styrene-based resin composition of the present invention can be advantageously used in applications such as office equipment, home appliance parts, miscellaneous goods, etc. The higher the proportion of styrene-based recycled material (A) in the recycled styrene-based resin composition, the more the amount of styrene-based virgin material (B) used can be reduced, and as a result, the environmental load caused by the production of styrene-based virgin material (B) can be reduced.

[0007] Furthermore, conventional recycled styrene-based resin compositions have sometimes suffered from reduced extrudability and poor appearance quality of molded articles. However, since the cause of the reduced extrudability and poor appearance quality of molded articles was the presence of metal materials in the recycled styrene-based resin composition, by specifying the magnetic attraction rate of the recycled styrene-based resin composition, it is possible to improve the extrudability of the recycled styrene-based resin composition and the appearance of the molded articles.

[0008] The following describes embodiments of the present invention. The features of the embodiments described below can be combined with each other. Each feature can also be an invention independently.

[0009] [Recycled styrene-based resin composition] A recycled styrene-based resin composition according to one embodiment of the present invention contains a styrene-based recycled material (A) and a styrene-based virgin material (B), and the recycled styrene-based resin composition has an ash content of 2.5 mass% or less after baking at 500°C, and the recycled styrene-based resin composition has a mass average molecular weight (Mw) of 170,000 or more.

[0010] The ratio of the mass of the styrene-based recycled material (A) to the mass of the styrene-based virgin material (B) in the recycled styrene-based resin composition (styrene-based recycled material (A) / styrene-based virgin material (B)) may be 10 / 90 to 90 / 10, such as 10 / 90, 20 / 80, 25 / 75, 30 / 70, 35 / 65, 40 / 60, 45 / 55, 50 / 50, 55 / 45, 60 / 40, 65 / 35, 70 / 30, 75 / 25, 80 / 20, or 90 / 10, and may be within a range between any two of the ratios exemplified here. Within this range, a recycled styrene-based resin composition having high extrudability and impact resistance, and a molded article having excellent molded article appearance can be obtained by molding the recycled styrene-based resin composition. Furthermore, by increasing the proportion of styrene-based recycled material (A) in the recycled styrene-based resin composition within this range, the amount of styrene-based virgin material (B) used can be reduced, and as a result, the environmental impact caused by the production of styrene-based virgin material (B) can be reduced.

[0011] <Styrenic recycled material (A)> In the present invention, the styrene-based recycled material (A) refers to a recycled material containing a styrene-based resin, and either pre-consumer material or post-consumer material may be used. Pre-consumer material refers to a material obtained by collecting and reusing offcuts and defective products generated in the production process of styrene-based resin products, as well as styrene-based resin products that are unsold or have exceeded their quality guarantee period and are discarded before shipping. Post-consumer material refers to a material that has been shipped to the market and then collected and reused after consumer use. The amount of styrene-based recycled material (A) used refers to the total amount of styrene-based recycled material (A) used in combination.

[0012] In the present invention, from the viewpoint of producing products with a small environmental impact and promoting green purchasing and improving the recycling rate, the styrene-based recycled material is preferably a post-consumer material. Specific examples of styrene-based resins suitable as post-consumer materials include polystyrene foam, extruded sheets, containers, packaging materials, cases for recording media such as CDs and MDs, miscellaneous goods such as bobbins and hangers, plastic parts for electrical appliances and office equipment, plastic parts for home appliances such as televisions and air conditioners, and plastic parts for office equipment such as copiers.

[0013] <Styrenic virgin material (B)> The styrene-based virgin material (B) in the present invention refers to an unused styrene-based resin that has not undergone the production process of a styrene-based resin product. The styrene-based resins described below may be used alone or in combination of two or more. When a styrene-based virgin material (B) is used in combination, the amount of the styrene-based virgin material (B) used refers to the total amount of the styrene-based virgin material (B) used in combination.

[0014] <Styrene-based Resin> Styrene-based resins will be described in detail below. Styrene-based resins are obtained by radical polymerization of aromatic vinyl compound-based monomers, and may be rubber-modified by adding a conjugated diene-based rubbery polymer as needed. The polymerization method can be known, for example, bulk polymerization, two-stage bulk / suspension polymerization, or solution polymerization. The aromatic vinyl compound-based monomer is a monocyclic or polycyclic aromatic vinyl-based monomer, for example, styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, p-tert-butylstyrene, 1-vinylnaphthalene, 2-vinylnaphthalene, 1,1-diphenylethylene, isopropenylbenzene (α-methylstyrene), isopropenyltoluene, isopropenylethylbenzene, and the like. Examples of the aromatic vinyl monomer include styrene, isopropenylpropylbenzene, isopropenylbutylbenzene, isopropenylpentylbenzene, isopropenylhexylbenzene, and isopropenyloctylbenzene, either alone or in a mixture of two or more thereof. Preferred examples include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, 2,4-dimethylstyrene, 2,5-dimethylstyrene, 3,4-dimethylstyrene, 3,5-dimethylstyrene, p-ethylstyrene, m-ethylstyrene, o-ethylstyrene, and p-tert-butylstyrene, either alone or in a mixture of two or more thereof. The aromatic vinyl monomer may be used alone or in combination of two or more thereof. The homopolymer of a styrene-based monomer is obtained by polymerizing a styrene-based monomer, which is an aromatic vinyl-based monomer. The homopolymer of a styrene-based monomer refers to a polymer of only a styrene-based monomer, and may also be a copolymer of two or more styrene-based monomers.

[0015] Examples of conjugated diene rubbery polymers used for rubber modification of styrene resins include polybutadiene, styrene-butadiene random or block copolymers, polyisoprene, polychloroprene, styrene-isoprene random, block or graft copolymers, ethylene-propylene rubber, and ethylene-propylene-diene rubber, with polybutadiene and styrene-butadiene random, block or graft copolymers being particularly preferred. These may also be partially hydrogenated.

[0016] Examples of styrene-based resins include polystyrene (GPPS), rubber-modified polystyrene (HIPS), ABS resin (acrylonitrile-butadiene-styrene copolymer), AS resin (acrylonitrile-styrene copolymer), MS resin (methyl methacrylate-styrene copolymer), AAS resin (acrylonitrile-acrylic rubber-styrene copolymer), and AES resin (acrylonitrile-ethylene propylene-styrene copolymer).

[0017] Examples of polymerization methods for styrene-based resins include known styrene polymerization methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization. From the viewpoints of quality and productivity, bulk polymerization and solution polymerization are preferred, and continuous polymerization is preferable. Examples of solvents that can be used include alkylbenzenes such as benzene, toluene, ethylbenzene, and xylene, ketones such as acetone and methyl ethyl ketone, and aliphatic hydrocarbons such as hexane and cyclohexane.

[0018] In the case of continuous polymerization, first, in the polymerization step, a known complete mixing tank type agitator tank or tower reactor is used, and the polymerization reaction is controlled by adjusting the polymerization temperature, etc., so as to achieve the target molecular weight, molecular weight distribution, and reaction conversion rate. The polymerization solution containing the polymer that has left the polymerization step is transferred to the devolatilization step, where unreacted monomers and polymerization solvent are removed. The devolatilization step is composed of a vacuum devolatilization tank equipped with a heater or a devolatilization extruder equipped with a vent. The molten polymer that has left the devolatilization step is transferred to the granulation step. In the granulation step, the molten resin is extruded in the form of strands through a multi-hole die and processed into pellets using the cold cut method, the in-air hot cut method, or the underwater hot cut method.

[0019] During polymerization of the styrene-based resin, a polymerization initiator and a chain transfer agent can be used as necessary. As the polymerization initiator, a radical polymerization initiator is preferred, and known and commonly used examples thereof include peroxyketals such as 1,1-di(t-butylperoxy)cyclohexane, 2,2-di(t-butylperoxy)butane, 2,2-di(4,4-di-t-butylperoxycyclohexyl)propane, and 1,1-di(t-amylperoxy)cyclohexane, hydroperoxides such as cumene hydroperoxide and t-butyl hydroperoxide, alkyl peroxides such as t-butyl peroxyacetate and t-amylperoxyisononanoate, t-butylcumyl peroxide, di-t-butyl peroxide, dicumyl peroxide, and di-t-hexyl peroxide. Examples of suitable chain transfer agents include dialkyl peroxides such as t-butyl peroxyacetate, t-butyl peroxybenzoate, and t-butylperoxyisopropyl monocarbonate; peroxyesters such as t-butylperoxyisopropyl carbonate and polyether tetrakis(t-butylperoxycarbonate); and peroxycarbonates such as N,N'-azobis(cyclohexane-1-carbonitrile), N,N'-azobis(2-methylbutyronitrile), N,N'-azobis(2,4-dimethylvaleronitrile), and N,N'-azobis[2-(hydroxymethyl)propionitrile]. These may be used alone or in combination of two or more. Examples of suitable chain transfer agents include aliphatic mercaptans, aromatic mercaptans, pentaphenylethane, α-methylstyrene dimer, and terpinolene.

[0020] <Mass Average Molecular Weight (Mw)> From the viewpoint of strength and moldability, the recycled styrene-based resin composition preferably has a mass average molecular weight (Mw) of 170,000 to 700,000, more preferably 170,000 to 400,000. Specifically, for example, 17, 18, 19, 20, 25, 30, 35, 40, 45, 50, 55, 60, 65, or 700,000, and may be within a range between any two of the values ​​exemplified here. By setting the Mw within this range, a styrene-based resin composition with high impact resistance and an excellent balance of fluidity and heat resistance can be obtained. The mass average molecular weight (Mw) of the styrene-based monomer homopolymer can be controlled by the reaction temperature and residence time of the polymerization process, the type and amount of polymerization initiator, the type and amount of chain transfer agent, the type and amount of solvent used during polymerization, and the like.

[0021] The mass average molecular weight (Mw) of the recycled styrene-based resin composition can be measured, for example, using gel permeation chromatography (GPC) under the following conditions: GPC model: Alliance System 2695 (manufactured by WATERS) Column: TSKgel GMHXL (manufactured by Tosoh) Mobile phase: tetrahydrofuran Sample concentration: 0.2% by mass Temperature: oven 40°C, detector 40°C Detector: differential refractometer Alliance System 2414 (manufactured by WATERS)

[0022] The molecular weight is calculated at each elution time from the elution curve of monodisperse polystyrene, and is calculated as a polystyrene-equivalent molecular weight.

[0023] <Ash content> The ash content of the recycled styrene-based resin composition after baking at 550 ° C is 2.5% by mass or less, preferably 1.9% by mass or less. The ash content is derived from the styrene-based recycled material (A). Furthermore, the ash content of the recycled styrene-based resin composition after baking at 550 ° C may be 0.001% by mass or more, preferably 0.01% by mass or more. Specifically, for example, it may be within the range of any two values ​​of 0.001, 0.005, 0.01, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1, 2.2, 2.3, 2.4, and 2.5% by mass. If it is within this range, a recycled styrene-based resin composition with excellent extrudability can be produced. Specifically, the extrudability can extend the life (screen life) of the screen (for example, #60 plain weave (280 μm mesh)) used when extruding the recycled styrene resin composition. The ash content of the recycled styrene resin composition after baking at 550°C can be adjusted by changing the proportion of the styrene recycled material (A) in the recycled styrene resin composition.

[0024] The ash content of the recycled styrene-based resin composition after baking at 550°C can be calculated using the following formula: Ash content (mass%) = (A / C) x 100, where C: mass of recycled styrene-based resin composition before baking, A: mass of residue (ash) after baking. The baking time can be changed depending on the mass of the recycled styrene-based resin composition, and ash can be obtained by heating 10 to 11 g of recycled styrene-based resin composition pellets for 1 hour.

[0025] The baking process includes a temperature increase step and a baking step. In the temperature increase step, the recycled styrene-based resin composition is heated to a temperature at which it turns to ash, and in the baking step, the recycled styrene-based resin composition turns to ash. The temperature increase step may include one or more temperature stabilization steps. The presence of one or more temperature stabilization steps can prevent sudden bumping of the molten recycled styrene-based resin composition. The temperature in the temperature stabilization step is, for example, 300°C to 500°C, and may be within any two of the following ranges: 300, 350, 400, 450, and 500°C. The duration of the temperature stabilization step is, for example, 0.5 to 5 hours, and may be within any two of the following ranges: 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, and 5 hours. The temperature stabilization step may, for example, include a 3-hour step at 350°C, a 2-hour step at 400°C, a 1-hour step at 450°C, and a 1-hour step at 500°C, in that order. The temperature in the baking step is 505 to 600°C and may be within the range of any two of 505, 510, 520, 530, 540, 550, 560, 570, 580, 590, and 600°C. The duration of the baking step is 0.5 to 5 hours and may be within the range of any two of 0.5, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, and 5 hours. The temperature and duration in the temperature stabilization step and the temperature and duration in the baking step can be changed depending on the amount of recycled styrene-based resin composition and the ratio of the mass of the styrene-based recycled material (A) to the mass of the styrene-based virgin material (B) in the recycled styrene-based resin composition.

[0026] <Si and Al> The ash may contain at least one of Si and Al. Since the styrene-based virgin material (B) does not contain metal elements such as Si and Al, the Si and Al are derived from the styrene-based recycled material (A).

[0027] The content of Si element in inorganic elements present in the ash may be 0.1 to 9.0 mass %, and preferably 0.3 to 8.2 mass %. Specifically, for example, the content is 0.1, 0.2, 0.3, 0.4, 0.5, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 3.0, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4.0, 4.1, 4.2, 4.3, 4.4, 4.5, 4.6, 4.7, 4.8, 4.9, 5.0, 6.0, 7.0, 8.0, 8.1, 8.2, 8.3, 8.4, 8.5, 8.6, 8.7, 8.8, 8.9, or 9.0% by mass, and may be within a range between any two of the values ​​exemplified here.

[0028] The content of Al element in inorganic elements present in the ash may be 0.05 to 2.0% by mass, preferably 0.1 to 1.8%, specifically, for example, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1.0, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or 2.0% by mass, and may be within a range between any two of the values ​​exemplified here.

[0029] When the Si element content and Al element content among the inorganic elements present in the ash are within the above ranges, a recycled styrene-based resin composition having excellent extrudability can be produced.

[0030] The Si and Al contents in the ash can be detected and analyzed using SEM-EDX. The content of each element in the ash is determined using SEM-EDX, and the proportion of each of the Si and Al elements is expressed as a percentage when the total of the inorganic elements is taken as 100%.

[0031] <Magnetic attraction rate> When the styrene-based recycled material (A) contained in the recycled styrene-based resin composition is a post-consumer material, the recycled styrene-based resin composition may contain a metal material. The metal material may be a ferromagnetic material. The metal material may be iron or an iron-group transition metal (Co, Ni, Mn, Cr, etc.), as well as alloys, compounds, and oxides thereof. The metal material may have a size that allows it to be removed by a magnet.

[0032] In conventional recycled styrene-based resin compositions, metal materials that can be removed manually by workers are removed, but metal materials that are difficult or impossible to remove manually remain. As a result, it has become clear that the amount of metal materials remaining in the recycled styrene-based resin composition affects the extrudability of the recycled styrene-based resin composition and the appearance of the molded product. Therefore, it is preferable that the amount of metal materials in the recycled styrene-based resin composition is as small as possible. The amount of metal materials in the recycled styrene-based resin composition may be determined by the magnetic attraction rate of the recycled styrene-based resin composition.

[0033] The magnetic attraction rate of the recycled styrene-based resin composition may be 0.2% by mass or less, and may be 0.2, 0.1, 0.09, 0.08, 0.07, 0.06, 0.05, 0.04, 0.03, 0.02, 0.01, 0.009, 0.008, 0.007, 0.006, 0.005, 0.004, 0.003, 0.002, or 0.001% by mass or less. By reducing the magnetic attraction rate to the above values, a recycled styrene-based resin composition having excellent molded article appearance can be produced, and a molded article can be obtained by molding the recycled styrene-based resin composition.

[0034] The magnetic attraction rate of the recycled styrene-based resin composition can be calculated from the following formula: Magnetic attraction rate (mass%) = (M / C) x 100, where C is the mass of the recycled styrene-based resin composition before recovery with a magnet, and M is the mass of the recycled styrene-based resin composition recovered with a magnet.

[0035] <Method for evaluating impact resistance> The impact resistance of the recycled styrene-based resin composition was evaluated by Charpy impact strength (in accordance with JIS K7111). The Charpy impact strength of the recycled styrene-based resin composition was 8 kJ / m 2or more. <Other Components> Other additives, such as known additives such as reinforcing materials, flame retardants, dyes and pigments, coloring inhibitors, lubricants, antioxidants, antiaging agents, light stabilizers, antistatic agents, fillers, crystallization nucleating agents, and compatibilizers, as well as modifiers such as colorants such as titanium oxide and carbon black, can be added to the recycled styrene-based resin composition of the present invention within the scope of the present invention. The method for adding these additives is not particularly limited, and they may be added by known methods. For example, they can be added during the raw material charging process, polymerization process, or finishing process during the production of the recycled styrene-based resin composition, or during the process of mixing the resin composition using an extruder or molding machine.

[0036] <Method for producing recycled styrene resin composition> The method for mixing the recycled styrene resin composition of the present invention is not particularly limited, and known mixing techniques can be applied. For example, various raw materials (e.g., styrene-based recycled material (A) and styrene-based virgin material (B)) are premixed using a mixing device such as a mixer-type mixer, a V-type blender, or a tumbler-type mixer, and the mixture is melt-kneaded to produce a homogeneous resin composition. The melt-kneading device is also not particularly limited, and examples include a Banbury mixer, a kneader, a roll, a single-screw extruder, a special single-screw extruder, and a twin-screw extruder. Furthermore, there is also a method in which additives such as a flame retardant are separately added midway through the melt-kneading device such as an extruder.

[0037] <Molded Article> A molded article obtained by molding a recycled styrene-based resin composition can be produced by molding the recycled styrene-based resin composition. There are no particular limitations on the molding method for obtaining a molded article, film, sheet, or foam from the recycled styrene-based resin composition of the present invention, and known molding methods such as extrusion molding methods such as calendar molding, blow molding, extrusion foam molding, profile extrusion molding, lamination molding, inflation molding, T-die film molding, sheet molding, vacuum forming, and pressure forming, and injection molding methods such as injection molding, RIM molding, and injection foam molding can be suitably used.

[0038] Examples of thermoforming methods include conventionally known general forming methods such as vacuum forming, compressed air forming, and applications thereof such as free drawing forming, plug and ridge forming, ridge forming, matched mold forming, straight forming, drape forming, reverse draw forming, air slip forming, plug assist forming, and plug assist reverse load forming.

[0039] The present invention will be described in detail below with reference to examples and comparative examples, but the present invention is not limited to these.

[0040] The materials used in the examples and comparative examples are as follows.

[0041] [Styrene-based recycled materials (A)] (A-1) Post-consumer material, polystyrene resin, ash content 0.3% by mass, magnetic attraction rate 0.02% by mass (A-2) Post-consumer material, polystyrene resin, ash content 0.7% by mass, magnetic attraction rate 0.3% by mass (A-3) Post-consumer material, polystyrene resin, ash content 4.0% by mass, magnetic attraction rate 0.1% by mass (A-4) Post-consumer material, polystyrene resin, ash content 4.0% by mass, magnetic attraction rate 0.5% by mass (A-5) Post-consumer material, polystyrene resin, ash content 6.0% by mass, magnetic attraction rate 0.7% by mass

[0042] [Styrene-based virgin material (B)] (B-1) HIPS (rubber-modified polystyrene resin, rubber-like polymer content in 100% by mass of resin: 9% by mass, molecular weight Mw: 200,000) (B-2) HIPS (rubber-modified polystyrene resin, rubber-like polymer content in 100% by mass of resin: 10% by mass, molecular weight Mw: 160,000

[0043] (Examples 1 to 8, Comparative Examples 1 to 3) Each component was extruded in the amounts shown in Tables 1 and 2 using a twin-screw extruder (Toshiba Corporation, TEM26SX) under extrusion conditions of a total feed rate of 30 kg / hour and a screw rotation speed of 300 rpm while melt-kneading. The resin temperature at this time was 235 to 240°C. The extruded strand was water-cooled and then introduced into a pelletizer to obtain pellets of the recycled styrene-based resin composition.

[0044] Evaluation of extrudability (screen life) A plate with a 1 cm square opening and a #60 plain weave mesh (opening 280 μm) were installed just before the die exit of the extruder. During extrusion molding, the extrusion amount (kg) was recorded when the resin pressure (resin pressure increasing as the mesh gradually becomes clogged) reached 8.5 MPa. If the resin pressure did not reach 8.5 MPa even after extruding 70 kg, it was rated as >70. A value of 40 kg or more was considered pass, and a value of less than 40 kg was considered fail.

[0045] Ash content (unit: mass%): 10-11 g of pellets were placed in a porcelain crucible. The porcelain crucible was placed in an electric furnace (Yamato Scientific, FP102) and heated at 350°C for 3 hours, then at 400°C for 2 hours, then at 450°C for 1 hour, at 500°C for 1 hour, and finally at 550°C for 1 hour. The weight of the ash residue was then measured.

[0046] Elemental Analysis of Ash Content (Unit: Mass %) The obtained ash content was detected and analyzed by SEM-EDX (manufactured by JEOL Ltd., JSM-6510A) to determine the content of each element.

[0047] Magnetic attraction rate (unit: mass %) 900 to 1,100 g of pellets were scattered on an aluminum tray, and the magnetically attracted pellets were collected while scanning with a 12,000 gauss magnet. The mass of the collected pellets was measured.

[0048] Preparation of molded articles The pellets were dried by heating at 80°C for 3 hours, and then 10 plates were prepared using an injection molding machine (manufactured by The Japan Steel Works, Ltd., J100E-P) at a cylinder temperature of 220°C and a mold temperature of 45°C.

[0049] The evaluation criteria for the appearance of the molded product were as follows: ◎: As a result of visual observation, no irregularities were found on the surface of any of the 10 plates. ○: As a result of visual observation, irregularities were found on the surface of 1 to 5 of the 10 plates. ×: As a result of visual observation, irregularities were found on the surface of 6 or more of the 10 plates. ◎ and ○ were considered to be acceptable, and × was considered to be unacceptable.

[0050] Charpy Impact Strength Test pieces were prepared using an injection molding machine and the Charpy impact strength was determined in accordance with JIS K7111.

[0051]

[0052]

[0053] It was found from the Examples in Table 1 that the resin compositions of the present invention were excellent in the appearance, impact resistance, and extrudability of the molded products. On the other hand, it was found from the Comparative Examples in Table 2 that the resin compositions that did not satisfy the requirements of the present invention were inferior in the appearance and extrudability of the molded products, or in the impact resistance.

[0054] The resin composition of the present invention has high extrudability and impact resistance even when it has a high recycled material content, and the molded product has excellent appearance. Therefore, molded articles of the resin composition of the present invention can be advantageously used in applications such as office automation equipment, home appliance parts, and miscellaneous goods, and have industrial applicability.

Claims

1. A recycled styrene-based resin composition comprising a styrene-based recycled material (A) and a styrene-based virgin material (B), characterized in that the ash content of the recycled styrene-based resin composition after baking at 550°C is 2.5 mass% or less, and the mass average molecular weight (Mw) of the recycled styrene-based resin composition is 170,000 or more.

2. The recycled styrene-based resin composition according to claim 1, wherein the ash contains at least one of the elements Si and Al.

3. A recycled styrene-based resin composition according to claim 1 or 2, wherein the ratio of the mass of the styrene-based recycled material (A) to the mass of the styrene-based virgin material (B) in the recycled styrene-based resin composition is 10 / 90 to 90 / 10.

4. A recycled styrene-based resin composition described in any one of claims 1 to 3, characterized in that the magnetic attraction rate of the recycled styrene-based resin composition is 0.2 mass% or less.

5. A molded article obtained by molding the recycled styrene-based resin composition according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Regenerated polystyrene resin composition

    JP2009149768A

  • Regenerated styrene resin composition

    JP2020007424A

  • Packaging material and packaged body

    JP2002086636A

  • Styrenic flame-retardant resin composition and method for producing the same

    JP2004137388A

  • Reclaimed styrenic resin particle for extrusion foam molding and extrusion foam molded product using the same

    JP2006063200A