Production method and production apparatus for thermoplastic resin foam particles

The method of dispersing thermoplastic resin particles in an aqueous medium, heating with carbon dioxide, and discharging into a low-pressure container with a specific area ratio addresses blocking and expansion ratio limitations, resulting in improved thermoplastic resin particle production with reduced blocking and increased expansion ratio.

WO2024204327A1PCT designated stage expired Publication Date: 2024-10-03KANEKA CORP

Patent Information

Application Number
PCT/JP2024/012226
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional methods for producing expanded thermoplastic resin particles face challenges with blocking between foamed particles and limited expansion ratio, as seen in the technique disclosed by Patent Document 1.

Method used

A method and apparatus that involve dispersing thermoplastic resin particles in an aqueous dispersion medium, heating and pressurizing with carbon dioxide gas, and then discharging into a cylindrical low-pressure container with a specific cross-sectional area ratio between the low-pressure container and the discharge port, ranging from 300 to 3030, to reduce blocking and increase the expansion ratio.

Benefits of technology

The method effectively reduces blocking between foamed particles and enhances the expansion ratio of thermoplastic resin particles, achieving a high expansion ratio while maintaining product quality and mechanical strength.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JP2024012226_03102024_PF_FP_ABST
    Figure JP2024012226_03102024_PF_FP_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to reduce blocking between foam particles and to increase the expansion ratio of the foam particles. In a production method for thermoplastic resin foam particles according to the present invention, in a step in which a carbon dioxide gas is used as a foaming agent, after heating and pressurizing a dispersion liquid of resin particles (9), the dispersion liquid is discharged through an orifice (5) into a low-pressure container (13) in an atmosphere at a pressure lower than the internal pressure of a pressure-resistant container (7) so as to obtain foam particles (11), wherein the ratio (B) / (A) of a cross-sectional area (B) of the low-pressure container (13) to a cross-sectional area (A) of the orifice (5) is set to 300 to 3,030.
Need to check novelty before this filing date? Find Prior Art

Description

Method and apparatus for producing expanded thermoplastic resin particles

[0001] The present invention relates to a method and an apparatus for producing expanded thermoplastic resin beads.

[0002] A known prior art method for producing expanded beads is to disperse thermoplastic resin particles in an aqueous dispersion medium in a pressure vessel, heat the thermoplastic resin particles to a temperature equal to or higher than the softening temperature of the thermoplastic resin, apply pressure, and then release the thermoplastic resin particles into an atmosphere of lower pressure than that in the pressure vessel to expand them. Another known prior art method involves dispersing a blowing agent in the pressure vessel as needed.

[0003] For example, Patent Document 1 discloses a technique in which, when polyolefin resin particles are released into an atmosphere having a lower pressure than that inside the container to be expanded, the expanded particles are caused to collide with a curved collision plate from the release portion of the pressure-resistant container, which at least improves the variation in expansion ratio at low expansion ratios, and at least realizes expanded particles with a uniform cell structure at high expansion ratios.

[0004] International Publication No. 2020 / 170694

[0005] However, the technology of Patent Document 1 leaves room for improvement in terms of blocking between expanded polyolefin resin particles and expansion ratio.

[0006] An object of one aspect of the present invention is to provide a method and an apparatus for producing expanded thermoplastic resin beads that minimizes blocking between expanded beads and allows for a high expansion ratio.

[0007] In order to solve the above-mentioned problems, a method for producing expanded thermoplastic resin beads according to one embodiment of the present invention includes a dispersion preparation step of preparing a dispersion by dispersing thermoplastic resin particles in an aqueous dispersion medium in a pressure-resistant vessel, and a foaming step of heating and pressurizing the dispersion to a temperature equal to or higher than the softening temperature of the thermoplastic resin particles using carbon dioxide gas as a foaming agent, and then foaming the dispersion by releasing it from a discharge port into a cylindrical low-pressure vessel under a pressure atmosphere lower than the internal pressure of the pressure-resistant vessel, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3030.

[0008] In addition, in order to solve the above-mentioned problems, an apparatus for manufacturing expanded thermoplastic resin beads according to one embodiment of the present invention comprises a pressure-resistant vessel for containing a dispersion liquid in which thermoplastic resin particles are dispersed in an aqueous dispersion medium and for impregnating the thermoplastic resin particles with carbon dioxide gas as a blowing agent, a cylindrical low-pressure vessel having a pressure lower than the internal pressure of the pressure-resistant vessel, and a discharge port for discharging the mixture in the pressure-resistant vessel into the low-pressure vessel, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3030.

[0009] According to one aspect of the present invention, a method for producing expanded thermoplastic resin beads can be realized which reduces blocking between expanded beads and allows for a high expansion ratio.

[0010] Fig. 1 is a schematic diagram showing the general configuration of an example of an expansion device for expanded thermoplastic resin beads used in a manufacturing method according to an embodiment of the present invention. Fig. 2 is a front view showing the configuration of a squeezing plate used in a manufacturing method according to an embodiment of the present invention. Fig. 3 is a cross-sectional view showing the configuration of a squeezing plate used in a manufacturing method according to an embodiment of the present invention. Fig. 4 is a cross-sectional view showing the configuration of a low-pressure vessel used in a manufacturing method according to an embodiment of the present invention. Fig. 5 is a schematic diagram for explaining a collision step in a manufacturing method according to an embodiment of the present invention.

[0011] An embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments and examples obtained by appropriately combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, new technical features can be formed by combining the technical means disclosed in each embodiment. Furthermore, all academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, the term "A to B" representing a numerical range means "greater than or equal to A (including and greater than A) and less than or equal to B (including and less than B)."

[0012] 1. Method for producing expanded thermoplastic resin beads according to the present embodiment As a result of extensive research into the above-mentioned problems, the present inventors independently discovered that when discharging the contents of a pressure-resistant container from a discharge port into a cylindrical low-pressure container, by setting the ratio (B) / (A) of the cross-sectional area (B) of the cylindrical low-pressure container to the cross-sectional area (A) of the discharge port within a specific numerical range, blocking between the expanded beads can be reduced and the expansion ratio of the expanded beads can be increased. Based on this discovery, the present embodiment was achieved.

[0013] That is, the method for producing expanded thermoplastic resin beads according to this embodiment (hereinafter simply referred to as this method) includes a dispersion preparation step of dispersing thermoplastic resin particles in an aqueous dispersion medium in a pressure-resistant vessel to prepare a dispersion, and a foaming step of heating and pressurizing the dispersion to a temperature equal to or higher than the softening temperature of the thermoplastic resin particles using carbon dioxide gas as a foaming agent, and then releasing the dispersion through a discharge port into a cylindrical low-pressure vessel under a pressure lower than the internal pressure of the pressure-resistant vessel, thereby foaming the dispersion. In this method, the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3030.

[0014] 2. Materials for Expanded Thermoplastic Resin Beads 2-1. Thermoplastic Resin Examples of the thermoplastic resin that serves as the base resin for the expanded thermoplastic resin beads include polyolefin-based resins, polyester-based resins, polystyrene-based resins, polyphenylene ether-based resins, polyamide-based resins, and mixtures thereof. The thermoplastic resin is preferably a polyolefin-based resin. Below, we will explain this method using a polyolefin-based resin as the base resin for the expanded thermoplastic resin beads.

[0015] The polyolefin resin refers to a resin containing 50% by weight or more, preferably 80% by weight or more, and more preferably 90% by weight or more of olefin units. Specific examples of polyolefin resins include polyethylenes such as high-density polyethylene, medium-density polyethylene, low-density polyethylene, linear low-density polyethylene, and low-molecular-weight polyethylene; propylene homopolymers; α-olefin-propylene random copolymers such as ethylene-propylene random copolymers, ethylene-propylene-1-butene random copolymers, and propylene-1-butene random copolymers, as well as α-olefin-propylene block copolymers; and other polyolefin homopolymers such as polybutene. These may be used alone or in combination of two or more types.

[0016] Among these, ethylene-propylene random copolymer, ethylene-propylene-1-butene random copolymer, and propylene-1-butene random copolymer are preferably used because they exhibit good expandability when made into expanded beads.

[0017] In addition, the base resin of the expanded polyolefin resin beads may contain, in addition to the polyolefin resin, other thermoplastic resins such as polystyrene, polybutene, ionomers, etc., mixed therein, as long as the properties of the polyolefin resin are not lost.

[0018] In order to facilitate the production of expanded beads, the polyolefin resin is preferably melted using an extruder, kneader, Banbury mixer, roll, or the like and processed in advance into resin particles having a cylindrical, elliptical, spherical, cubic, rectangular parallelepiped, or other shape. Resin particles are also called pellets.

[0019] The weight of each polyolefin resin particle is preferably 0.1 to 30 mg, and more preferably 0.3 to 10 mg.

[0020] 2-2. Additives to Polyolefin Resin When adding additives to a polyolefin resin, it is preferable to mix the polyolefin resin and additives using a blender or the like before producing the polyolefin resin particles. Specific examples of additives include cell nucleating agents (also simply referred to as nucleating agents). Furthermore, when using hydrocarbon blowing agents such as propane, butane, pentane, and hexane, inorganic nucleating agents such as talc, silica, calcium carbonate, kaolin, titanium oxide, bentonite, and barium sulfate are commonly used. The amount of cell nucleating agent added varies depending on the type of polyolefin resin and the type of cell nucleating agent used, so it cannot be generally defined, but it is preferably approximately 0.001 parts by weight or more and 2 parts by weight or less per 100 parts by weight of polyolefin resin.

[0021] In the present method, in which carbon dioxide gas is used as a blowing agent, it is preferable to use the inorganic nucleating agent and / or hydrophilic substance. When water is used as a dispersion medium for the aqueous dispersion, the polyolefin resin is impregnated with water, and the impregnated water acts as a blowing agent together with other blowing agents or alone.

[0022] The hydrophilic substance acts to increase the amount of water impregnated into the polyolefin resin. Specific examples of hydrophilic substances include inorganic substances such as sodium chloride, calcium chloride, magnesium chloride, borax, and zinc borate; or organic substances such as glycerin, melamine, isocyanuric acid, melamine-isocyanuric acid condensates, polyethers such as polyethylene glycol or polyethylene oxide, polyether adducts to polypropylene, and polymer alloys thereof; and polymers such as alkali metal salts of ethylene-(meth)acrylic acid copolymers, alkali metal salts of butadiene-(meth)acrylic acid copolymers, alkali metal salts of carboxylated nitrile rubber, alkali metal salts of isobutylene-maleic anhydride copolymers, and alkali metal salts of poly(meth)acrylic acid. These hydrophilic substances may be used alone or in combination of two or more.

[0023] The amount of the hydrophilic substance added is preferably 0.005 to 2 parts by weight, more preferably 0.005 to 1 part by weight, per 100 parts by weight of the polyolefin resin. By adjusting the type and amount of the hydrophilic substance, the average cell diameter of the expanded polyolefin resin beads can be adjusted.

[0024] Furthermore, during the production of polyolefin-based resin particles, additives such as colorants, antistatic agents, antioxidants, phosphorus-based processing stabilizers, lactone-based processing stabilizers, metal deactivators, benzotriazole-based ultraviolet absorbers, benzoate-based light stabilizers, hindered amine-based light stabilizers, flame retardants, flame retardant assistants, acid neutralizers, crystal nucleating agents, and amide-based additives may be added as needed within a range that does not impair the properties of the polyolefin-based resin.

[0025] 2-3. Blowing Agent In this method, the blowing agent used in the foaming step is carbon dioxide gas. This method may be any method that uses carbon dioxide gas as the blowing agent, and methods that use carbon dioxide gas in combination with a conventionally known blowing agent are also included in the scope of this method. Examples of conventionally known blowing agents that can be used include volatile hydrocarbon blowing agents such as propane, isobutane, butane, pentane, and hexane, as well as inorganic gases such as air, nitrogen, and water.

[0026] 1-4. Dispersants and Dispersion Aids It is preferable to use water as the aqueous dispersion medium. Dispersions in which methanol, ethanol, ethylene glycol, glycerin, etc. are added to water can also be used as aqueous dispersants.

[0027] In the aqueous dispersion medium, it is preferable to use a dispersant to prevent the polyolefin resin particles from fusing together.Specific examples of the dispersant include inorganic dispersants such as tricalcium phosphate, trimagnesium phosphate, titanium oxide, basic magnesium carbonate, calcium carbonate, barium sulfate, kaolin, talc, and clay.Among these, tricalcium phosphate, barium sulfate, and kaolin are more preferable because they can stably disperse the aqueous dispersion containing the polyolefin resin particles in the pressure-resistant container even when used in small amounts.

[0028] It is also preferable to use a dispersing aid together with the dispersant. Specific examples of dispersing aids include anionic surfactants such as carboxylate-type surfactants such as N-acylamino acid salts, alkyl ether carboxylates, and acylated peptides; sulfonate-type surfactants such as alkyl sulfonates, alkylbenzene sulfonates, alkylnaphthalene sulfonates, and sulfosuccinates; sulfate-type surfactants such as sulfated oils, alkyl sulfates, alkyl ether sulfates, and alkylamide sulfates; and phosphate-type surfactants such as alkyl phosphates, polyoxyethylene phosphates, and alkyl allyl ether sulfates. Furthermore, polyvalent anionic polymer surfactants such as maleic acid copolymer salts, polycarboxylic acid-type polymer surfactants such as polyacrylates, and polystyrene sulfonates and naphthalsulfonic acid formalin condensate salts can also be used as dispersing aids.

[0029] As the dispersing aid, it is preferable to use a sulfonate-type anionic surfactant, and more preferably to use one or a mixture of two or more selected from alkyl sulfonates and alkyl benzene sulfonates. It is more preferable to use an alkyl sulfonate, and it is particularly preferable to use an alkyl sulfonate having a linear carbon chain with 10 to 18 carbon atoms as the hydrophobic group, because this can reduce the amount of dispersant adhering to the expanded polyolefin resin particles.

[0030] In an embodiment of the present invention, it is particularly preferable to use one or more dispersants selected from tricalcium phosphate, trimagnesium phosphate, barium sulfate, and kaolin in combination with sodium n-paraffinsulfonate as a dispersing aid.

[0031] 3. Steps of the Present Method 3-1. Dispersion Preparation Step In the dispersion preparation step, for example, the polyolefin resin particles are dispersed in the aqueous dispersion medium in a pressure vessel to prepare a dispersion.

[0032] The amounts of dispersant and dispersion aid used vary depending on their type or the type and amount of polyolefin resin used. Usually, the dispersant is preferably blended in an amount of 0.1 parts by weight or more and 5 parts by weight or less, more preferably 0.2 parts by weight or more and 3 parts by weight or less, per 100 parts by weight of the aqueous dispersion medium. The dispersion aid is preferably blended in an amount of 0.001 parts by weight or more and 0.3 parts by weight or less, more preferably 0.001 parts by weight or more and 0.1 parts by weight or less, per 100 parts by weight of the aqueous dispersion medium. In addition, in order to improve dispersibility in the aqueous dispersion medium, it is usually preferable to use polyolefin resin particles in an amount of 20 parts by weight or more and 100 parts by weight or less, per 100 parts by weight of the aqueous dispersion medium. With the above-mentioned configuration, the polyolefin resin particles can be stably dispersed in the aqueous dispersion medium in a pressure-resistant container.

[0033] 3-2. Foaming Process In the foaming process, the dispersion is heated and pressurized to a temperature equal to or higher than the softening temperature of the thermoplastic resin particles using carbon dioxide gas as a foaming agent, and then released through a discharge port into a cylindrical low-pressure container under a pressure lower than the internal pressure of the pressure-resistant container, thereby foaming the dispersion. More specifically, in the foaming process, the dispersion is heated to a temperature equal to or higher than the softening temperature of the polyolefin resin particles, and the polyolefin resin particles are impregnated with carbon dioxide gas as a foaming agent. Thereafter, an inorganic gas is introduced into the pressure-resistant container to bring the pressure inside the pressure-resistant container to 0.6 to 5.0 MPa, and while maintaining this pressure, the inorganic gas is released into an atmosphere lower in pressure than the internal pressure of the pressure-resistant container, thereby foaming the dispersion.

[0034] The temperature to which the dispersion is heated is not particularly limited as long as it is equal to or higher than the softening temperature of the polyolefin resin particles, but is preferably equal to or higher than the melting point of the polyolefin resin particles, more preferably equal to or higher than the melting point + 5°C. The temperature to which the dispersion is heated is preferably equal to or lower than the melting point + 20°C, more preferably equal to or lower than the melting point + 15°C. For example, in the case of an ethylene-propylene copolymer having a melting point of 145°C, the heating temperature is preferably 145 to 165°C, more preferably 150 to 160°C. If the heating temperature is lower than 145°C, the polyolefin resin particles are less likely to expand. If the heating temperature exceeds 165°C, the mechanical strength and heat resistance of the resulting expanded beads are insufficient, and the polyolefin resin particles tend to fuse together in a pressure-resistant container.

[0035] The melting point of the polyolefin resin is the temperature at the top of the melting peak that appears when the resin is heated from 40°C to 220°C at a rate of 10°C / min using a DSC (differential scanning calorimeter), cooled to 40°C at a rate of 10°C / min, and then heated again to 220°C at a rate of 10°C / min.

[0036] The inorganic gas is not particularly limited, but examples thereof include carbon dioxide gas, nitrogen gas, air, and inorganic gases that are mainly composed of these gases (usually 50% by volume or more, preferably 70% by volume or more) and contain small amounts (50% by volume or less, preferably 30% by volume or less) of inert gases such as argon, helium, and xenon, and water vapor, oxygen, hydrogen, ozone, etc., but carbon dioxide gas and nitrogen are preferred from the standpoints of economy, productivity, and environmental compatibility, and carbon dioxide gas and air are more preferred from the standpoints of safety and economy.

[0037] The holding pressure of the inorganic gas is not particularly limited, but is preferably 0.6 to 5.0 MPa, more preferably 1.0 to 3.5 MPa, as described above, from the viewpoint of improving the expansion ratio and reducing the expansion ratio variation. If the holding pressure is less than 0.6 MPa, the effect of introducing the blowing agent is reduced, and the expanded beads tend not to expand sufficiently, making it difficult to obtain expanded beads with the desired expansion ratio. Furthermore, if the holding pressure exceeds 5.0 MPa, the cells in the resulting expanded beads tend to become finer, the closed cell ratio decreases, and the molded product tends to shrink and lose its shape stability, mechanical strength, and heat resistance. The timing of introducing the inorganic gas does not significantly affect the quality of the expanded beads, such as their expansion ratio and expansion ratio variation, so it may be before, during, or after heating in the pressure-resistant vessel.

[0038] The time required for releasing the polyolefin resin particles together with the aqueous dispersion medium into a low-pressure atmosphere after the pressure has reached a predetermined value by pressurizing with the inorganic gas is not particularly limited, but is preferably within 60 minutes or as short as possible from the viewpoint of improving productivity. It is also preferable that the pressure inside the container during the release is maintained at the pressure reached.

[0039] The low-pressure atmosphere into which the dispersion is released may be any atmosphere lower than the internal pressure of the pressure vessel, but is usually an atmosphere with a pressure close to atmospheric pressure. The atmosphere refers to the space that encompasses the scattering trajectory of the released aqueous dispersion (expanded particles and aqueous dispersion medium), and generally refers to the inside of an apparatus that is isolated from the outside air by a pipe or duct.

[0040] Here, in the method for producing expanded polyolefin resin beads, the dispersion (polyolefin resin particles and aqueous dispersion medium) is preferably released from the pressure-resistant vessel through a discharge port while maintaining the internal pressure of the pressure-resistant vessel, into a cylindrical low-pressure vessel under a pressure atmosphere lower than the internal pressure of the pressure-resistant vessel.

[0041] The expansion step in this method will be described below with reference to Fig. 1. Fig. 1 is a schematic diagram showing the outline of an example of an expansion apparatus (manufacturing apparatus) for the expanded thermoplastic resin beads used in this method.

[0042] As shown in FIG. 1, the foaming apparatus used in this method includes a cylindrical throttle plate 1 (discharge section), a discharge pipe 6, a pressure-resistant vessel 7, a valve 8, and a cylindrical low-pressure vessel 13.

[0043] The discharge pipe 6 is a pipe that connects the pressure vessel 7 and the low-pressure vessel 13. A valve 8 is provided on this discharge pipe 6. The valve 8 switches the pressure vessel 7 between open and closed states. A throttle disk 1 is also disposed at the outlet of the discharge pipe 6. The discharge pipe 6 and the low-pressure vessel 13 are in communication with each other via the throttle disk 1. Here, in this specification, in the direction of the axis R of the cylindrical low-pressure vessel 13, the direction away from the throttle disk 1 is referred to as the front, and the direction approaching the throttle disk 1 is referred to as the rear.

[0044] The pressure vessel 7 contains a dispersion in which resin particles 9 made of polyolefin resin are dispersed in an aqueous dispersion medium 10. In the foaming process, the dispersion heated and pressurized inside the pressure vessel 7 passes through the discharge pipe 6 by opening the valve 8, and is discharged from the throttle plate 1 into the low-pressure vessel 13 to become foamed beads 11.

[0045] The squeezing plate 1 and the low-pressure vessel 13 used in this method will now be described in more detail.

[0046] <Squeezing disk 1> The squeezing disk 1 is generally used to adjust the release time and make the expansion ratio uniform. Figure 2 is a front view showing the configuration of the squeezing disk 1 used in this method. Figure 3 is a cross-sectional view showing the configuration of the squeezing disk 1.

[0047] As shown in Figures 2 and 3, the diaphragm 1 includes a cylindrical body 2 and an orifice plate 3. The cylindrical body 2 is cylindrical and is provided on the side of the orifice plate 3 where the dispersion liquid is discharged, i.e., on the front side. The orifice plate 3 is an orifice type, and is configured to have an orifice 5 formed therein as the discharge port through which the dispersion liquid passes. The cylindrical body 2 is disposed such that its inner surface 2a surrounds the orifice 5. More specifically, the center of the orifice 5 and the center of the cylindrical body 2 are in a positional relationship such that they are substantially aligned.

[0048] In this way, the squeezing plate 1 is a squeezing plate with a cylinder 2 attached to the orifice plate 3. The cylinder 2 can reduce the scattering angle of the dispersion liquid released from the orifice 5. As a result, it is possible to expand the expanded particles into uniform sizes and reduce the variation in expansion ratio.

[0049] The orifice plate 3 is not limited to the orifice type described above, and may be any type that allows the dispersion to pass through. As the orifice plate 3, an orifice type, a nozzle type, a venturi type, or the like may be used, and a combination of these may also be used. That is, the discharge port is not limited to the orifice 5, and may be a nozzle type or a venturi type as long as it is capable of discharging the dispersion into the low-pressure container 13. Preferably, the discharge port is the orifice 5. By using the orifice 5 as the discharge port, it is possible to maintain a constant outflow rate with a simple structure, and to obtain expanded beads with a high expansion ratio and little expansion ratio variation.

[0050] In the configuration shown in Fig. 2, three orifices 5 are provided in the orifice plate 3. However, the number of orifices 5 is not limited to three and can be set as appropriate. The number of orifices 5 may be one. When two or more orifices 5 are provided in the orifice plate 3, the multiple orifices 5 may all have the same shape or may all have different shapes. Also, some of the orifices may have the same shape and some may have different shapes.

[0051] Diameter h of orifice 5 a For example, when only one orifice 5 is formed, the diameter h a is preferably 6.0 mm or more, more preferably 7.0 mm or more, and even more preferably 8.0 mm or more. a In addition, when a plurality of orifices 5 are formed, the diameter h a is preferably 2.0 mm or more, more preferably 3.0 mm or more, and even more preferably 4.0 mm or more. ais, for example, 3.6 mm. a However, the upper limit of the diameter h a The larger the size, the greater the capacity required to transport the expanded particles, resulting in higher equipment costs.

[0052] The thickness of the orifice plate 3 is preferably 0.2 to 10 mm, more preferably 0.5 to 5 mm. If the thickness is less than 0.2 mm, the orifice plate 3 may be damaged by the pressure at the time of release. On the other hand, if the thickness exceeds 10 mm, the expansion ratio of the resulting expanded beads decreases, making it difficult to obtain expanded beads having a desired expansion ratio, and there is a risk that the openings may be blocked by the resin.

[0053] The cylindrical body 2 is attached integrally with the orifice plate 3 on the side of the orifice 5 from which the dispersion liquid is discharged. The material of the cylindrical body 2 is not particularly limited, but metal is generally used. The method of integrating the cylindrical body 2 and the orifice plate 3 is not particularly limited, and welding, fitting, screwing, adhesive bonding, etc. may be used. If necessary, the orifice plate 3 and the cylindrical body 2 may be manufactured as a single unit.

[0054] The opening area of ​​the cylindrical body 2 at the end opposite the orifice plate 3 can be set appropriately depending on the size and length of the cylindrical body 2, and is generally 1.3 times or more the opening area of ​​the orifice 5 (hereinafter sometimes referred to as the cross-sectional area of ​​the orifice 5). If the opening area of ​​the cylindrical body 2 is less than 1.3 times the opening area of ​​the orifice 5, aggregation and clogging of the released foamed particles are likely to occur. Note that if the length of the cylindrical body 2 is short, the above problems do not occur, but the effect of the cylindrical body 2 is less likely to be achieved.

[0055] The shape of the cylindrical body 2 is not limited to the cylinder shown in Fig. 2, but may be a circular hole including a part of a circle or an ellipse. The circular hole here refers to a through hole having an inner wall shaped like a circle, an ellipse, or a rectangle or square with two opposing sides to which semicircles having the diameter as the sides are added.

[0056] The cylindrical body 2 is not limited to a circular hole. The cylindrical body 2 may have a slit shape. The slit-shaped cylindrical body 2 here refers to a through hole having a polygonal shape such as a rectangle, square, rhombus, trapezoid, parallelogram, other quadrangle, triangle, pentagon, hexagon, or the like.

[0057] In addition, when the cylindrical body 2 has a cylindrical shape as shown in FIG. 2, the inner diameter H a is, for example, 0.6 mm or more, preferably 1.2 to 25 mm, and the length M of the cylindrical body 2 in the discharging direction is, for example, 5 mm or more, preferably 5 to 300 mm. If the length M of the cylindrical body 2 is less than 5 mm, the scattering trajectory of the discharged dispersion is no different from that when a squeezing disk 1 without the cylindrical body 2 is used. This weakens the effect of reducing the variation in magnification. Furthermore, if the length M is longer than 300 mm, the expanded beads may collide and fuse together inside the cylindrical body 2, making it impossible to obtain expanded beads. The length M is defined as the distance from the point on the cylindrical body 2 closest to the orifice plate 3 to the point farthest from the orifice plate 3 in the discharging direction of the dispersion.

[0058] Furthermore, the shape of the cylinder 2 may be a shape that forms part of a pyramid or a cone. In this case, the cross-sectional area of ​​the portion of the cylinder 2 that contacts the orifice plate 3 is close to the opening area of ​​the orifice 5. The cross-sectional area of ​​the cylinder 2 at the outlet from which the dispersion liquid is released is wider. In other words, the shape of the cylinder 2 is such that the area of ​​the region surrounded by the side wall of the cylinder 2 increases in the direction in which the dispersion liquid is released.

[0059] The drawing plate 1 may be provided with a number of cylindrical bodies 2 equal to or less than the number of openings of the orifices 5 of the orifice plate 3. When the drawing plate 1 has a plurality of orifices 5, this is advantageous as it increases the production speed.

[0060] In the configuration shown in Figure 2, three cylindrical bodies 2 are provided on the drawing plate 1. However, the number of cylindrical bodies 2 on the drawing plate 1 is not limited to three and can be set as appropriate. The number of cylindrical bodies 2 may be one. When two or more cylindrical bodies 2 are provided on the drawing plate 1, the multiple cylindrical bodies 2 may all have the same shape, or may all have different shapes. Furthermore, some may have the same shape and some may have different shapes.

[0061] <Low-pressure vessel 13> The space inside the low-pressure vessel 13 is a space under low pressure and in a saturated steam atmosphere. Therefore, the expanded beads 11 released from the squeezing disk 1 come into contact with saturated steam. The low-pressure vessel 13 can be any conventionally known container as long as it is cylindrical and can realize the above-mentioned low-pressure atmosphere and saturated steam atmosphere. The cross-sectional shape of the low-pressure vessel 13 is not particularly limited, and examples include a circle, an ellipse, a rectangle, a pentagon, and a hexagon. From the viewpoint of ease of installation in a production facility, the low-pressure vessel 13 is preferably in the form of a pipe. Furthermore, the low-pressure vessel 13 may be configured so that steam is introduced through a steam inlet.

[0062] <Relationship between the Cross-Sectional Area (A) of the Cylindrical Body 2 and the Cross-Sectional Area (B) of the Low-Pressure Container 13> The inventors focused on the cross-sectional area (A) of the orifice 5 serving as a discharge port and the cross-sectional area (B) of the low-pressure container 13 in order to reduce blocking between the expanded beads and increase the expansion ratio of the expanded beads. Generally, the cross-sectional area (A) of the orifice 5 serving as a discharge port is considered to determine the amount of mixture released into the pressure-resistant container 7. However, it has been unclear whether there is a correlation between the cross-sectional area (A) and the cross-sectional area (B) of the low-pressure container 13 with respect to blocking between the expanded beads and the expansion ratio. If the cross-sectional area (B) of the low-pressure container 13 is reduced, the low-pressure container 13 becomes a long, thin cylinder, and the internal temperature tends to rise to nearly 100°C. Therefore, if the cross-sectional area (B) of the low-pressure container 13 is reduced, the expanded beads released from the cylindrical body 2 tend to stick together, which makes blocking more likely to occur. On the other hand, if the cross-sectional area (B) of the low-pressure vessel 13 is increased, blocking is less likely to occur, but the expansion ratio of the expanded beads tends to decrease. As a result of extensive research, the present inventors independently discovered that the ratio of the cross-sectional area (A) of the orifice 5 to the cross-sectional area (B) of the low-pressure vessel 13 affects blocking between the expanded beads and the expansion ratio of the expanded beads.

[0063] In this method, the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel 13 to the cross-sectional area (A) of the orifice 5 is 300 to 3030, and preferably 400 to 3000. When (B) / (A) is within the above range, there are effects that the blocking between the expanded beads is reduced and the expansion ratio of the expanded beads can be increased (i.e., the decrease in the expansion ratio can be suppressed).

[0064] Next, the definition of the cross-sectional area (A) of the orifice 5 and the cross-sectional area (B) of the low-pressure vessel 13 will be explained with reference to Figures 2 and 4, respectively. Figure 4 is a cross-sectional view showing the configuration of the low-pressure vessel 13. Figure 4 is a cross-sectional view perpendicular to the axis R.

[0065] First, the cross-sectional area (A) of the orifice 5 is the area of ​​the shaded region shown in Figure 2. That is, the cross-sectional area (A) is defined as the area of ​​the region surrounded by the inner wall surface 5a of the orifice 5 in a cross section perpendicular to the axial direction of the orifice plate 3. It can be said that the cross-sectional area (A) defines the discharge amount of the dispersion liquid discharged from the orifice 5. When there are multiple orifices 5 as shown in Figure 2, the cross-sectional area (A) is the sum of the areas surrounded by the inner wall surface 5a of each orifice 5. When there is one orifice 5, it goes without saying that the cross-sectional area (A) is the area of ​​the region surrounded by the inner wall surface 5a of one orifice 5. It can also be said that the cross-sectional area (A) is the opening area of ​​the orifice 5.

[0066] The cross-sectional area (B) of the low-pressure vessel 13 is the area of ​​the shaded region shown in Figure 4. That is, the cross-sectional area (B) is defined as the area of ​​the region surrounded by the inner surface 13a in a cross section perpendicular to the axial direction of the low-pressure vessel 13. It can be said that the cross-sectional area (B) defines the area of ​​the region in which the expanded particles can move in a cross section perpendicular to the axial direction of the low-pressure vessel 13.

[0067] The cross-sectional area (A) and the cross-sectional area (B) can be set arbitrarily as long as the ratio (B) / (A) is within the above-mentioned range. From the viewpoint of stabilizing the quality of the expanded beads, the cross-sectional area (A) is set to 30 mm 2 ~60mm 2 It is preferable that the 2 ~55mm 2 It is more preferable that the cross-sectional area (A) is 60 mm 2 If the cross-sectional area (A) exceeds 40 mm, the equipment capacity required to maintain a constant pressure inside the pressure vessel 7 will increase, resulting in higher costs. 2 If it is less than 9000 mm, productivity will decrease. 2 ~125,000 mm 2 It is preferable that the 2 ~100,000 mm 2 By setting the cross-sectional area (B) within the above range, it is possible to achieve the effect of making the equipment compact.

[0068] Furthermore, the axial length of the low-pressure vessel 13 is not particularly limited, but is preferably 500 mm to 3000 mm, and more preferably 500 mm to 2000 mm. By setting the axial length of the low-pressure vessel 13 within the above numerical range, the effect of collision can be properly exerted and the equipment can be made compact.

[0069] In the present method, the foaming step preferably includes a collision step. In the collision step, the mixture in the pressure-resistant container is collided with the inner surface 13a of the low-pressure container 13 when the mixture is released from the release port (e.g., orifice 5). The term "mixture" used here refers to a mixture of polyolefin resin particles impregnated with carbon dioxide gas as a foaming agent and the dispersion.

[0070] Figure 5 is a schematic diagram illustrating the collision step in this method. In this method, as shown in Figure 4, the expanded beads 11 released from the squeezing disk 1 collide with the inner surface 13a, changing the scattering direction of the expanded beads 11. Normally, during foaming, the resin hardens and the foaming process ends when the temperature drops below the softening point of the resin beads. However, when the mixture in the pressure-resistant container is collided with the inner surface 13a as in this method, the temperature and humidity of the foaming atmosphere become more uniform, which is thought to result in the individual expanded beads expanding uniformly and reducing the variation in the expansion ratio. Therefore, according to this method, the above collision step can reduce the variation in the expansion ratio of the expanded beads.

[0071] Furthermore, the collision angle θ of the mixture with the inner surface 13a of the low-pressure vessel 13 can be set to any angle as long as the above-mentioned effect of reducing the variation in the expansion ratio is achieved. The collision angle θ is preferably 13° to 20°, and more preferably 14° to 16°. When the collision angle θ is within the above numerical range, the effect of collision is strong, and the effect of reducing the variation in the expansion ratio is likely to be large.

[0072] 5, when the mixture is caused to collide with the inner surface 13a of the low-pressure vessel 13, the axis of the cylindrical body 2 of the throttle plate 1 does not coincide with the axis R of the low-pressure vessel 13, but is tilted at a predetermined angle. When the axis of the cylindrical body 2 is tilted in this manner, most of the mixture discharged from the orifice 5 collides with the inner surface 13a of the low-pressure vessel 13 at a predetermined collision angle θ.

[0073] Here, the low-pressure vessel 13 is not limited to a configuration in which the cross-sectional area (B) is constant in the front-to-rear direction (direction of axis R). The low-pressure vessel 13 may be configured so that the cross-sectional area (B) varies in the front-to-rear direction. In this case, the cross-sectional area (B) is defined as the average cross-sectional area of ​​the mixture in the collision region D on the inner surface 13a. In other words, as long as the above (B) / (A) is within the above numerical range for at least the average cross-sectional area (cross-sectional area (B)) in the collision region D, it falls within the scope of this embodiment. When the axial length of the low-pressure vessel 13 is 1000 mm and the collision angle θ is 15°, the collision region D is a region of 400 mm to 600 mm from the end on the rear side (the squeezing disc 1 side) on the inner surface 13a.

[0074] The collision region D varies depending on the collision angle θ. For example, if the cross-sectional area (B) varies in the front-rear direction but the inner surface 13a is considered to be approximately parallel to the axis R, the collision region D can be calculated as follows. First, as shown in FIG. 5 , the position of the orifice 5 in the front-rear direction is defined as the origin O. The distance between the origin O and the orifice 5 is defined as C. The inclination angle with respect to the inner surface 13a is the collision angle θ, and the intersection of a straight line passing through the base end 2b with the inner surface 13a is defined as P. In this case, the collision region D is defined as the region of the intersection P ±350 mm. Furthermore, applying trigonometric ratios, the collision region D can be said to be the region of the inner surface 13a from the origin O to (C / tan θ) ±350 mm.

[0075] 4. Expanded Thermoplastic Resin Beads Produced by the Present Method The expansion ratio of the expanded beads produced by the present method can be set as appropriate as long as the above-mentioned effects are achieved, but is preferably 10 to 25, and more preferably 15 to 25. According to the present method, even when producing expanded beads with a high expansion ratio such as within the above numerical range, a decrease in the expansion ratio is suppressed (a high expansion ratio is maintained) and blocking between the expanded beads is reduced.

[0076] The closed cell ratio of the expanded beads produced by this method is preferably 80% to 100%, and more preferably 90% to 100%. If the closed cell ratio is less than 80%, the secondary expansion force will be insufficient, causing poor fusion during molding and reducing the mechanical strength, etc., of the resulting molded article.

[0077] The average cell diameter of the expanded beads produced by this method is preferably 20 μm to 500 μm, more preferably 100 μm to 400 μm. If the average cell diameter is less than 20 μm, problems such as distortion of the shape of the resulting molded article may occur. If the average cell diameter is more than 500 μm, the mechanical strength of the resulting molded article may decrease.

[0078] The expanded beads have a closed cell content of 80% or more. Therefore, if necessary, the expanded beads may be air-impregnated by treating them in a pressure-resistant container under heat and pressure for a certain period of time, and then filled into a molding die and heated with steam to perform in-mold expansion molding to produce a molded article conforming to the mold.

[0079] The rate of occurrence of blocking in the expanded beads produced by this method is low, preferably 1% or less, and particularly preferably 0%.

[0080] The foamed molded article thus obtained is excellent in flexibility and cushioning properties, and is also small in dimensional shrinkage and shape deformation, making it highly valuable commercially.

[0081] 5. Method for producing a molded article from expanded thermoplastic resin beads produced by this method The method for producing a molded article from expanded thermoplastic resin beads according to this embodiment is a method for molding the expanded thermoplastic resin beads obtained by the above-mentioned production method. A known method can be used to mold the expanded thermoplastic resin beads to produce a molded article from expanded thermoplastic resin beads.

[0082] 6. Apparatus for Producing Molded Thermoplastic Resin Expanded Beads The apparatus for producing expanded thermoplastic resin beads according to this embodiment is an apparatus capable of carrying out the method for producing expanded thermoplastic resin beads according to this embodiment, and examples thereof include those shown in Figures 1 to 5. Hereinafter, the apparatus for producing expanded thermoplastic resin beads according to this embodiment will be described with reference to Figures 1 to 5.

[0083] The thermoplastic resin expanded bead manufacturing apparatus according to this embodiment (hereinafter sometimes referred to as the present apparatus) includes a cylindrical throttling disk 1 (discharge section), a discharge pipe 6, a pressure-resistant container 7, a valve 8, and a cylindrical low-pressure container 13. The pressure-resistant container 7 contains a dispersion of polyolefin resin resin particles 9 dispersed in an aqueous dispersion medium 10, and is used to impregnate the resin particles 9 with carbon dioxide gas as a blowing agent. The low-pressure container 13 has a pressure lower than the internal pressure of the pressure-resistant container 7. The throttling disk 1 has an orifice 5 (discharge port) (see FIG. 2). The orifice 5 is an opening for discharging the mixture containing the carbon dioxide-impregnated resin particles 9 from the pressure-resistant container 7 into the low-pressure container 13. As described above, in the present apparatus, the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure container 13 to the cross-sectional area (A) of the orifice 5 is 300 to 3030.

[0084] Thus, according to this device, by setting the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel 13 to the cross-sectional area (A) of the orifice 5 within a specific numerical range, blocking between the expanded beads 11 is reduced and the expansion ratio of the expanded beads 11 can be increased.

[0085] The orifice plate 1 is configured so that the mixture in the pressure vessel 7 is discharged from the orifice 5 and collides with the inner surface 13a of the low-pressure vessel 13. The orifice plate 1 includes a tubular body 2 and an orifice plate 3. The tubular body 2 has a cylindrical shape and is provided on the side of the orifice plate 3 from which the dispersion is discharged, i.e., on the front surface. The orifice plate 3 is configured so that an orifice 5 through which the dispersion passes is formed. The tubular body 2 is arranged so that its inner surface 2a surrounds the orifice 5.

[0086] The axis of the cylindrical body 2 of the squeezing plate 1 does not coincide with the axis R of the low-pressure vessel 13, but is tilted at a predetermined angle. As a result, most of the mixture discharged from the orifice 5 collides with the inner surface 13a of the low-pressure vessel 13 at a predetermined collision angle θ. By causing the resin particles 9 impregnated with carbon dioxide gas to collide with the inner surface 13a in this manner, it is possible to reduce variation in the expansion ratio of the expanded beads 11.

[0087] Other specifications for the cross-sectional area (A), cross-sectional area (B), collision angle θ, etc. in this device are as explained above in "3. Each step of this method," so explanation will be omitted.

[0088] [Summary] As described above, one embodiment of the present invention is as follows.

[0089] [1] A method for producing expanded thermoplastic resin beads, comprising: a dispersion preparation step of dispersing thermoplastic resin particles in an aqueous dispersion medium in a pressure-resistant vessel to prepare a dispersion; and an expansion step of heating and pressurizing the dispersion to a temperature equal to or higher than the softening temperature of the thermoplastic resin particles using carbon dioxide gas as a blowing agent, and then releasing the dispersion from a discharge port into a cylindrical low-pressure vessel under a pressure atmosphere lower than the internal pressure of the pressure-resistant vessel, thereby causing foaming, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3,030.

[0090] [2] The method for producing expanded thermoplastic resin beads according to [1], wherein the expansion step includes a collision step of colliding the mixture in the pressure-resistant container with the inner surface of the low-pressure container when the mixture is released from the release port.

[0091] [3] The method for producing expanded thermoplastic resin beads according to [2], wherein the collision angle of the mixture with the inner surface of the low-pressure vessel is 13° to 20°.

[0092] [4] The method for producing expanded thermoplastic resin beads according to any one of [1] to [3], wherein the discharge port is an orifice.

[0093] [5] The cross-sectional area (A) is 30 mm 2 ~60mm 2 The method for producing expanded thermoplastic resin beads according to any one of [1] to [4],

[0094] [6] The cross-sectional area (B) is 9000 mm 2 ~125,000 mm 2 The method for producing expanded thermoplastic resin beads according to any one of [1] to [5],

[0095] [7] The method for producing expanded thermoplastic resin beads according to any one of [1] to [6], wherein the expanded thermoplastic resin beads to be produced have an expansion ratio of 10 to 25 times.

[0096] [8] The method for producing expanded thermoplastic resin particles according to any one of [1] to [7], wherein the thermoplastic resin particles are polyolefin-based resin particles.

[0097] [9] A method for producing an expanded thermoplastic resin bead molding, which comprises molding the expanded thermoplastic resin beads produced by the method according to any one of [1] to [7].

[0098]

[10] An apparatus for producing expanded thermoplastic resin beads, comprising: a pressure vessel for accommodating a dispersion of thermoplastic resin particles dispersed in an aqueous dispersion medium and for impregnating the thermoplastic resin particles with carbon dioxide gas as a blowing agent; a cylindrical low-pressure vessel having a pressure lower than the internal pressure of the pressure vessel; and a discharge port for discharging the mixture in the pressure vessel into the low-pressure vessel, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3030.

[0099]

[11] The thermoplastic resin foam particle manufacturing apparatus of

[10] , further comprising a discharge section having the discharge outlet, the discharge section being configured so that the mixture in the pressure-resistant container is discharged from the discharge outlet and collides with the inner surface of the low-pressure container.

[0100]

[12] The apparatus for producing expanded thermoplastic resin beads according to

[11] , wherein the collision angle of the mixture with the inner surface of the low-pressure vessel is 13° to 20°.

[0101]

[13] The device for producing expanded thermoplastic resin beads according to any one of

[10] to

[12] , wherein the discharge port is an orifice.

[0102]

[14] The cross-sectional area (A) is 30 mm 2 ~60mm 2 The apparatus for producing expanded thermoplastic resin beads according to any one of

[10] to

[13] ,

[0103]

[15] The cross-sectional area (B) is 9000 mm 2 ~125,000 mm 2 The apparatus for producing expanded thermoplastic resin beads according to any one of

[10] to

[14] ,

[0104]

[16] The method for producing expanded thermoplastic resin beads according to any one of [1] to [8], wherein the axial length of the low-pressure vessel is 500 mm to 3000 mm.

[0105]

[17] The apparatus for producing expanded thermoplastic resin beads according to any one of

[10] to

[15] , wherein the axial length of the low-pressure vessel is 500 mm to 3000 mm.

[0106]

[18] Expanded thermoplastic resin beads produced by the method for producing expanded thermoplastic resin beads according to any one of [1] to [8] and

[16] , wherein the rate of occurrence of blocking is 0%.

[0107]

[19] Expanded thermoplastic resin particles having a blocking incidence rate of 0%.

[0108] <Expansion Ratio> The weight Gi of the obtained expanded beads was accurately measured to 0.001 g (rounded off to the fourth decimal point). Then, the weighed expanded polyolefin resin beads of known weight were submerged in a measuring cylinder containing 100 ml of ethanol at 23°C, and the volume yi (cm) of the expanded polyolefin resin beads was determined from the rise in the scale. 3 The weight Gi (g) of the expanded polyolefin resin beads was then calculated based on the volume yi (cm 3The apparent density di of the expanded polyolefin resin particles of each sieve was calculated by dividing the density by the density of the expanded polyolefin resin particles (= 900 g / L) and converting the result into g / L. Finally, the expansion ratio Ki = ds / di was calculated from the ratio to the density ds (= 900 g / L) of the base resin.

[0109] <Blocking incidence rate> The obtained expanded particles were treated with a vibrating sieve to separate out coarse particles including blocked expanded particles. The weight of the separated coarse particles including blocked expanded particles was measured, and the ratio to the total weight of the expanded particles was calculated, and the obtained value was taken as the blocking incidence rate.

[0110] (Example 1) (Production of polyolefin-based resin particles) An ethylene-propylene random copolymer (density 0.90 g / cm) was used as a polyolefin-based resin. 3 7.5 parts by weight of carbon black masterbatch, 0.05 parts by weight of talc as a cell nucleating agent, and 0.1 parts by weight of glycerin were weighed out relative to 100 parts by weight of a polyolefin resin (melting point 148°C, MI = 7.5 g / 10 min), and the mixture was fed into a 26 mmφ twin-screw extruder [TEM26-SX, manufactured by Toshiba Machine Co., Ltd.] and melt-kneaded at a resin temperature of 200°C. The mixture was then extruded through a cylindrical die with a diameter of 1.2 mmφ, cooled with water, and cut with a cutter to obtain cylindrical polyolefin resin particles (pellets) (1.2 mg / particle) containing the polyolefin resin.

[0111] (Production of Expanded Polyolefin Resin Beads) 100 parts by weight of the obtained polyolefin resin particles, 0.3 parts by weight of kaolin (ASP-170, manufactured by BASF) as a dispersant, 0.05 parts by weight of sodium dodecylbenzenesulfonate (Neopelex G-15, manufactured by Kao Corporation) as a dispersing aid, and 200 parts by weight of water were charged into a pressure vessel. Then, 3.6 parts by weight of carbon dioxide gas as a blowing agent was added, and the aqueous dispersion was heated to 151°C in the pressure vessel while stirring. The pressure inside the pressure vessel at this time was approximately 2.2 MPa. Additional carbon dioxide gas was then injected to increase the pressure inside the pressure vessel to a foaming pressure of 2.6 MPa. After maintaining the predetermined foaming temperature of 151°C and foaming pressure of 2.6 MPa for 20 minutes, the aqueous dispersion in the pressure vessel was released into a low-pressure vessel 13 (foaming cylinder) shown in FIG. 5 via a squeezing plate 1 shown in FIG. 5 to obtain expanded beads. At this time, the collision angle θ was set to 15°. The cross-sectional area (A) of the cylindrical body 2 of the drawing disk 1 was 40 mm 2 The cross-sectional area (B) of the low-pressure vessel 13 is 50,000 mm 2 It was decided.

[0112] (Example 2) The cross-sectional area (B) of the low-pressure vessel 13 is set to 120,000 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0113] (Example 3) The cross-sectional area (A) of the cylindrical body 2 of the drawing plate 1 is set to 55 mm 2 , the cross-sectional area (B) of the low-pressure vessel 13 is 120,000 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0114] (Example 4) The cross-sectional area (A) of the cylindrical body 2 of the drawing plate 1 is set to 55 mm 2 The cross-sectional area (B) of the low-pressure vessel 13 is 64242 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0115] (Example 5) The cross-sectional area (B) of the low-pressure vessel 13 is 17671 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0116] (Comparative Example 1) The cross-sectional area (A) of the cylindrical body 2 of the drawing plate 1 was set to 41 mm 2The cross-sectional area (B) of the low-pressure vessel 13 is 7854 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0117] (Comparative Example 2) The cross-sectional area (A) of the cylindrical body 2 of the drawing plate 1 was set to 41 mm 2 The cross-sectional area (B) of the low-pressure vessel 13 is 125664 mm 2 The expanded beads were obtained in the same manner as in Example 1, except that:

[0118] (Results) In Examples 1 to 5 and Comparative Examples 1 and 2, the expansion ratios and blocking incidence rates of the expanded beads obtained are shown in Table 1.

[0119] As shown in Table 1, the expansion ratio of the resulting expanded beads was 14 times and the incidence of blocking was 0% in Examples 1 to 5. In Comparative Example 1, the expansion ratio of the resulting expanded beads was 14 times and the incidence of blocking was 1%. In Comparative Example 2, the expansion ratio of the resulting expanded beads was 12 times and the incidence of blocking was 0%.

[0120] The results in Table 1 show that in Examples 1 to 5, where (B) / (A) was in the range of 300 to 3030, the expansion ratio was maintained at 14 times and blocking between the expanded beads was reduced. On the other hand, in Comparative Example 1, where (B) / (A) was less than 300, the expansion ratio was maintained at 14 times, but blocking between the expanded beads was observed. In Comparative Example 1, where (B) / (A) was more than 3030, the expansion ratio was not maintained at 14 times, although blocking between the expanded beads was reduced.

[0121] The present invention can be suitably used for the expanded particles used in the production of, for example, cushioning packaging materials, logistics materials, heat insulating materials, civil engineering and construction materials, automobile parts, and the like.

[0122] REFERENCE SIGNS LIST 1 throttle plate 2 cylindrical body 2a inner surface 3 orifice plate 5 orifice (discharge port) 6 discharge pipe 7 pressure-resistant vessel 8 valve 9 resin particles 10 aqueous dispersion medium 11 expanded particles 13 low-pressure vessel 13a inner surface

Claims

1. A method for producing expanded thermoplastic resin particles, comprising: a dispersion preparation step of preparing a dispersion by dispersing thermoplastic resin particles in an aqueous dispersion medium in a pressure vessel; and an expansion step of heating and pressurizing the dispersion to a temperature equal to or higher than the softening temperature of the thermoplastic resin particles using carbon dioxide gas as a blowing agent, and then releasing the dispersion from an outlet into a cylindrical low-pressure vessel having a lower pressure atmosphere than the internal pressure of the pressure vessel, thereby causing foaming, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the outlet is 300 to 3,030.

2. The method for producing expanded thermoplastic resin particles described in claim 1, wherein the expansion process includes a collision process in which the mixture in the pressure-resistant container is collided with the inner surface of the low-pressure container when the mixture is discharged from the discharge port.

3. The method for producing expanded thermoplastic resin beads according to claim 2, wherein the collision angle of the mixture with the inner surface of the low-pressure vessel is 13° to 20°.

4. A method for producing expanded thermoplastic resin beads according to any one of claims 1 to 3, wherein the discharge port is an orifice.

5. The cross-sectional area (A) is 30 mm 2 ~60mm 2 The method for producing expanded thermoplastic resin beads according to any one of claims 1 to 3, 6. The cross-sectional area (B) is 9000 mm 2 ~125000mm 2 The method for producing expanded thermoplastic resin beads according to any one of claims 1 to 3, 7. The method for producing expanded thermoplastic resin beads according to any one of claims 1 to 3, wherein the expanded thermoplastic resin beads produced have an expansion ratio of 10 to 25 times.

8. A method for producing expanded thermoplastic resin particles according to any one of claims 1 to 3, wherein the thermoplastic resin particles are polyolefin-based resin particles.

9. A method for producing a molded article from expanded thermoplastic resin beads, which comprises molding the expanded thermoplastic resin beads produced by the method according to any one of claims 1 to 3.

10. An apparatus for producing expanded thermoplastic resin beads, comprising: a pressure vessel for containing a dispersion of thermoplastic resin particles dispersed in an aqueous dispersion medium and for impregnating the thermoplastic resin particles with carbon dioxide gas as a blowing agent; a cylindrical low-pressure vessel having a pressure lower than the internal pressure of the pressure vessel; and a discharge port for discharging the mixture in the pressure vessel into the low-pressure vessel, wherein the ratio (B) / (A) of the cross-sectional area (B) of the low-pressure vessel to the cross-sectional area (A) of the discharge port is 300 to 3,030.

11. The apparatus for producing thermoplastic resin foamed particles described in claim 10, further comprising a discharge section having the discharge outlet, the discharge section being configured so that the mixture in the pressure-resistant container is discharged from the discharge outlet and collides with the inner surface of the low-pressure container.

12. The apparatus for producing expanded thermoplastic resin beads according to claim 11, wherein the collision angle of the mixture with the inner surface of the low-pressure vessel is 13° to 20°.

13. The apparatus for producing expanded thermoplastic resin beads according to any one of claims 10 to 12, wherein the discharge port is an orifice.

14. The cross-sectional area (A) is 30 mm 2 ~60mm 2 The apparatus for producing expanded thermoplastic resin beads according to any one of claims 10 to 12, 15. The cross-sectional area (B) is 9000 mm 2 ~125000mm 2 The apparatus for producing expanded thermoplastic resin beads according to any one of claims 10 to 12,

Citation Information

Patent Citations

  • Method for producing thermoplastic resin foaming particles, and thermoplastic resin foaming particles

    WO2020170694A1

  • Expanded particle of polyolefinic resin and its preparation

    JP1984207942A

  • Method for producing pre-foamed granule of polyolefin- based resin composition

    JP2000290420A

  • Method for producing pre-expanded particles of polyolefinic resin

    WO2005085337A1

Cited By

  • Apparatus for producing thermoplastic resin foam particles, and method for producing thermoplastic resin foam particles

    WO2026203717A1