Spun-bond non-woven fabric, cable press-wrapping tape, printing base material, and method for producing spun-bond non-woven fabric

The spunbond nonwoven fabric, produced with specific polyethylene terephthalate resin fibers and thermocompression bonding, addresses the challenge of achieving mechanical strength and surface smoothness, enabling effective use in wire wrapping and printing applications.

WO2024204334A1PCT designated stage expired Publication Date: 2024-10-03TORAY INDUSTRIES INC

Patent Information

Application Number
PCT/JP2024/012233
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-29
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

Conventional spunbond nonwoven fabrics fail to achieve both mechanical strength and surface smoothness simultaneously through heat and pressure bonding alone, necessitating additional resin processing, and previous methods to enhance strength and smoothness are insufficient.

Method used

A spunbond nonwoven fabric composed of polyethylene terephthalate resin fibers with a specific crystallization peak range, intrinsic viscosity, and fiber structure, produced using high and low viscosity polyethylene terephthalate resin core-sheath composite fibers and thermocompression bonding, achieving enhanced mechanical strength and surface smoothness.

Benefits of technology

The resulting nonwoven fabric exhibits excellent mechanical strength, high surface smoothness, and suitable properties for applications such as electric wire wrapping tape and printing base materials, with improved tensile strength and print clarity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

The present invention addresses the problem of providing a non-woven fabric having excellent mechanical strength and surface smoothness. The present invention relates to a spun-bond non-woven fabric composed of fibers containing a polyethylene terephthalate resin as a main component, wherein: the crystallization peak is within a range from 100°C to 150°C inclusive, and the single melting peak is within a range from 250°C and 270°C inclusive according to differential scanning calorimetry; and the maximum height roughness Rz is 40.0 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Spunbond nonwoven fabric, electric wire pressure winding tape, printing substrate, and method for manufacturing spunbond nonwoven fabric

[0001] The present invention relates to a spunbond nonwoven fabric, an electric wire pressure winding tape, and a printing substrate.

[0002] The properties required for nonwoven fabrics used in electric wire pressure wrapping tapes include tensile strength, surface smoothness to facilitate peeling from the sheath material, thinness, etc. In addition to mechanical strength, the surface smoothness of nonwoven fabrics is also an important property for printing substrates in terms of print clarity and uniform ink adhesion.

[0003] Conventionally, in order to obtain a spunbonded nonwoven fabric having both excellent mechanical strength and excellent surface smoothness, bonding by heat and pressure alone has been insufficient because the strength and smoothness are insufficient, and it has been necessary to use a resin treatment in combination (Patent Document 1, Patent Document 2). Meanwhile, various studies have been conducted to obtain a nonwoven fabric having both excellent mechanical strength and excellent surface smoothness by bonding by heat and pressure alone.

[0004] Patent Document 3 proposes a method for obtaining a polyethylene terephthalate spunbond nonwoven fabric suitable for use as an electric wire pressure wrapping tape or a printing substrate, in which the reduced viscosity of polyethylene terephthalate is increased to increase the strength of the fiber itself, and the fiber has a specific flatness and fineness, thereby producing a spunbond nonwoven fabric that is high in strength and excellent in smoothness.

[0005] Patent Document 4 proposes a spunbond nonwoven fabric having an intrinsic viscosity within a specific range and a ratio of flatness between the surface layer and the inner layer of the fiber within a specific range.

[0006] Japanese Patent Laid-Open No. 55-32342 Japanese Patent Laid-Open No. 57-56564 Japanese Patent Laid-Open No. 2001-140157 Japanese Patent Laid-Open No. 2007-197891

[0007] In Patent Document 3, by using flat yarns, the gaps between the fibers are reduced and surface smoothness can be improved, but bonding by heat and pressure alone is not sufficient in terms of strength and smoothness.

[0008] In Patent Document 4, it is possible to increase the strength of a nonwoven fabric by adjusting the intrinsic viscosity to a specific range, and also to improve the surface smoothness by flattening only the fibers in the surface layer of the nonwoven fabric; however, bonding by heat and pressure alone is not sufficient in terms of strength and smoothness.

[0009] SUMMARY OF THE INVENTION It is therefore an object of the present invention to provide a spunbonded nonwoven fabric which is bonded only by thermocompression bonding and which has excellent mechanical strength and surface smoothness.

[0010] As a result of extensive research aimed at achieving the above object, the present inventors have discovered that by adjusting the crystallization peak and melting peak of a spunbonded nonwoven fabric in a specific temperature range as measured by differential scanning calorimetry, a spunbonded nonwoven fabric having excellent mechanical strength and excellent surface smoothness can be obtained. The present invention was completed based on these findings.

[0011] The present invention and its preferred embodiments have the following configurations: [1] A spunbond nonwoven fabric composed of fibers containing polyethylene terephthalate resin as a main component, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C, as measured by differential scanning calorimetry, and has a maximum height roughness Rz of 40.0 μm or less. [2] An apparent density of 0.40 g / cm 3 1.00g / cm or more 3The spunbond nonwoven fabric according to [1] above, which is the following: [3] An electric wire pressure winding tape comprising the spunbond nonwoven fabric according to [1] or [2] above. [4] A printing substrate comprising the spunbond nonwoven fabric according to [1] or [2] above. [5] A method for producing the spunbond nonwoven fabric according to [1] or [2] above, comprising the following steps (a) to (c) in this order: Step (a): A step of spinning out a core-sheath type composite fiber comprising a high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less, and a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less, the low-viscosity polyethylene terephthalate resin having an intrinsic viscosity (IV) that is 0.05 to 0.25 lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin. Step (b): A step of pulling and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermocompressing the fiber web with a flat roll.

[0012] According to the present invention, a nonwoven fabric having excellent mechanical strength and high surface smoothness is provided.

[0013] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of fibers containing polyethylene terephthalate resin as a main component, and has a crystallization peak in the range of 100°C to 150°C, a single melting peak in the range of 250°C to 270°C, and a maximum height roughness Rz of 40.0 μm or less, as measured by differential scanning calorimetry. The components of the fabric are described in detail below, but the present invention is not limited to the scope described below as long as the gist of the invention is not exceeded, and various modifications are possible within the scope of the invention.

[0014] [Polyethylene terephthalate resin] First, the spunbond nonwoven fabric of the present invention is composed of fibers containing polyethylene terephthalate resin as a main component.

[0015] The melting point of the polyethylene terephthalate resin is preferably 250°C or higher and 270°C or lower. By setting the melting point of the polyethylene terephthalate resin to 250°C or higher, heat resistance sufficient for practical use is easily obtained. Furthermore, by setting the melting point of the polyethylene terephthalate resin to 270°C or lower, it becomes easier to cool the yarn discharged from the spinneret, suppressing fusion of fibers and facilitating stable spinning even with a fine fiber diameter. Here, the melting point of the polyethylene terephthalate resin refers to the maximum melting peak temperature obtained by measuring the polyethylene terephthalate resin by differential scanning calorimetry (DSC).

[0016] The intrinsic viscosity (IV) of the polyethylene terephthalate resin is preferably 0.40 or more and 0.70 or less. By making the intrinsic viscosity of the polyethylene terephthalate resin 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more, it is possible to suppress a decrease in the strength of the fibers constituting the nonwoven fabric. On the other hand, by making the intrinsic viscosity of the polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0017] To the polyethylene terephthalate resin, additives such as a crystal nucleating agent, a matting agent, a lubricant, a pigment, an antifungal agent, an antibacterial agent, a flame retardant, a metal oxide, an aliphatic bisamide and / or an alkyl-substituted aliphatic monoamide, and a hydrophilic agent can be added within a range that does not impair the effects of the present invention. Among these, metal oxides such as titanium oxide have the effect of reducing the surface friction of the fibers and preventing fusion of the fibers to improve spinnability, and also improving the fusion properties of the nonwoven fabric by increasing thermal conductivity during fusion molding of the nonwoven fabric with a heated roll, thereby making it possible to obtain a spunbond nonwoven fabric with superior mechanical strength.

[0018] [Fibers] The fibers constituting the nonwoven fabric are preferably core-sheath type composite fibers.

[0019] Furthermore, the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the sheath component is preferably lower than the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the core component by a range of 0.05 to 0.25. Hereinafter, the polyethylene terephthalate resin of the sheath component in this embodiment will also be referred to as the "low-viscosity polyethylene terephthalate resin," and the polyethylene terephthalate resin of the core component will also be referred to as the "high-viscosity polyethylene terephthalate resin." When the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.05 or more, more preferably 0.08 or more, and even more preferably 0.10 or more, spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. As a result, a fiber with high single fiber strength and excellent thermal adhesiveness can be obtained, making it easier to obtain a nonwoven fabric with excellent mechanical strength. On the other hand, when the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is smaller than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by 0.25 or less, preferably 0.20 or less, the single fiber strength of the sheath-core composite fiber can be improved.

[0020] The intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is preferably 0.55 or more and 0.70 or less. By making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.55 or more, a decrease in single fiber strength can be prevented. Furthermore, by making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.

[0021] The mass ratio of the sheath component in the sheath-core composite fiber is preferably 10% by mass or more and 80% by mass or less. When the mass ratio of the sheath component is 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the sheath components are firmly fused together during thermocompression bonding, resulting in a spunbonded nonwoven fabric having sufficient strength for practical use. On the other hand, when the mass ratio of the sheath component is 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, the proportion of the highly oriented core component is increased, improving the single fiber strength of the sheath-core composite fiber, resulting in a spunbonded nonwoven fabric having sufficient strength for practical use.

[0022] The composite form of the sheath-core composite fiber may be, for example, a concentric sheath-core type, an eccentric sheath-core type, an islands-in-sea type, etc. Among these, the sheath-core type composite form is preferred, and the concentric sheath-core type composite form is more preferred, because it has excellent spinnability, allows the fibers to be uniformly bonded together by thermocompression bonding, and allows the formation of a spunbonded nonwoven fabric with excellent mechanical strength.

[0023] The fibers preferably have an average fiber diameter of 6.0 μm or more and 20.0 μm or less. By setting the average fiber diameter to 6.0 μm or more, more preferably 7.0 μm or more, and even more preferably 8.0 μm or more, it is possible to prevent a decrease in spinnability, improve production stability, and obtain a spunbond nonwoven fabric with excellent mechanical strength. On the other hand, by setting the average fiber diameter to 20.0 μm or less, more preferably 18.0 μm or less, and even more preferably 16.0 μm or less, it is possible to obtain a spunbond nonwoven fabric with uniform texture and sufficient strength for practical use.

[0024] In the present invention, the average fiber diameter (μm) is determined by the following method. (i) Ten small sample pieces measuring 10 mm x 10 mm are randomly collected from a spunbond nonwoven fabric. (ii) The surfaces of the collected small sample pieces are photographed using a scanning electron microscope or the like at a magnification of 500 to 2000 times, allowing the fiber thickness to be measured. (iii) Ten fibers are randomly selected from the photographs of each small sample piece, for a total of 100 fibers, and their thicknesses are measured. The fibers are assumed to have a circular cross section, and the thickness is taken as the fiber diameter. (iv) The arithmetic mean of these fiber diameters is rounded to one decimal place, and the calculated value is taken as the average fiber diameter.

[0025] [Spunbonded Nonwoven Fabric] The spunbonded nonwoven fabric of the present invention has a crystallization peak in the range of 100°C or higher and 150°C or lower, as measured by differential scanning calorimetry. When the spunbonded nonwoven fabric has a crystallization peak temperature within this range, fusion between fibers during flat roll bonding is promoted, resulting in a spunbonded nonwoven fabric with excellent surface smoothness and mechanical strength. On the other hand, in the case of a spunbonded nonwoven fabric that does not have a crystallization peak, fusion between fibers is difficult to occur, resulting in a spunbonded nonwoven fabric with reduced surface smoothness and low mechanical strength.

[0026] Furthermore, the spunbond nonwoven fabric has a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry. Having a single melting peak in this range makes it possible to firmly thermocompress the fibers together at a sufficient temperature without causing operational problems such as the low-melting point component melting and sticking to the heated roll during thermocompression bonding, thereby producing a spunbond nonwoven fabric having sufficient strength for practical use.

[0027] Here, the crystallization peak temperature Tc (°C) and melting peak temperature Tm (°C) of the spunbond nonwoven fabric are obtained by differential scanning calorimetry (DSC), and values ​​calculated by the following procedure are adopted: (i) A small piece of spunbond nonwoven fabric is sampled in an amount of 0.5 mg to 5 mg. (ii) Using differential scanning calorimetry (DSC), the temperature is raised from room temperature to 280°C at a heating rate of 16°C / min to obtain a DSC curve. (iii) From the DSC curve, the peak-top temperature of the crystallization exothermic peak is read and designated as the crystallization peak temperature Tc (°C) of the spunbond nonwoven fabric, and the peak-top temperature of the melting endothermic peak is read and designated as the melting peak temperature Tm (°C) of the spunbond nonwoven fabric.

[0028] The spunbond nonwoven fabric has a maximum height roughness Rz of 40.0 μm or less. By setting the maximum height roughness Rz to 40.0 μm or less, preferably 35.0 μm or less, and more preferably 33.0 μm or less, it is possible to eliminate localized irregularities from the surface of the nonwoven fabric, resulting in a nonwoven fabric with excellent surface smoothness.

[0029] In the present invention, the maximum height roughness Rz refers to a value measured and calculated by the following method: (i) Ten randomly selected locations on a 10 cm x 10 cm long-fiber nonwoven fabric are sampled. (ii) The randomly selected nonwoven fabric is measured across a 21 mm range in the width direction of the long-fiber nonwoven fabric sheet using a surface roughness meter (for example, the "Surftest SJ-210" manufactured by Mitutoyo Corporation) in accordance with JIS B0610:2001 "Geometrical Product Specifications (GPS) - Surface Profile: Profile Curve Method - Definition and Display of Rolling Circular Waviness" under conditions of λc = 2.5 mm, λs = 8 μm, and a measurement speed of 0.5 mm / s. The maximum height roughness Rz is measured in 0.1 μm increments on each side of the 10 sampled locations. (iii) The values ​​measured above are arithmetically averaged for each surface, and the average is rounded off to one decimal place. The value of the surface with the highest average value is taken as the maximum height roughness Rz.

[0030] The spunbond nonwoven fabric of the present invention preferably has an arithmetic mean roughness Ra of 4.5 μm or less. By having an arithmetic mean roughness Ra of 4.5 μm or less, more preferably 4.0 μm or less, and even more preferably 3.5 μm or less, the entire surface of the nonwoven fabric becomes smooth, resulting in a nonwoven fabric with excellent smoothness.

[0031] In the present invention, the arithmetic mean roughness Ra refers to a value measured and calculated by the following method: (i) Ten randomly selected locations on a 10 cm x 10 cm long-fiber nonwoven fabric are sampled. (ii) The randomly selected nonwoven fabric is measured across a 21 mm range in the width direction of the long-fiber nonwoven fabric sheet using a surface roughness meter (for example, the "Surftest SJ-210" manufactured by Mitutoyo Corporation) in accordance with JIS B0610:2001 "Geometric Product Specifications (GPS) - Surface Profile: Profile Curve Method - Definition and Description of Rolling Circular Waviness" under conditions of λc = 2.5 mm, λs = 8 μm, and a measurement speed of 0.5 mm / s. The arithmetic mean roughness Ra is measured on each side of the 10 sampled locations to the nearest 0.1 μm. (iii) The values ​​measured on both surfaces (20 points in total) are calculated as an arithmetic average, and the value is rounded off to one decimal place to obtain the arithmetic average roughness Ra.

[0032] The spunbond nonwoven fabric of the present invention has a tensile strength per unit area of ​​5.00 (N / 5cm) / (g / m 2 It is preferable that the tensile strength is 5.00 (N / 5cm) / (g / m 2 ) or more, more preferably 5.50 (N / 5cm) / (g / m 2 ) or more, more preferably 5.80 (N / 5cm) / (g / m 2 ) or more, it is possible to have a minimum tensile strength, which is preferable.

[0033] In the present invention, the tensile strength per unit area of ​​the spunbonded nonwoven fabric ((N / 5 cm) / (g / m 2)) shall be values ​​determined by the following method in accordance with 6.3 "Tensile Strength and Elongation" of JIS L1913:2010 "Test Methods for General Long-Fiber Nonwoven Fabrics." (i) Three 30 cm x 5.0 cm wide samples are taken from the nonwoven fabric at equal intervals in both the machine direction (MD) and the cross direction (CD). (ii) A load is applied until the sample breaks under conditions of a gripping distance of 20 cm and a pulling speed of 100±10 mm / min. (iii) The strength of the sample at the maximum load is defined as the tensile strength (N / 5 cm), and the average values ​​of three points in each of the MD and CD are calculated. The sum of these average values ​​shall be the tensile strength of the spunbond nonwoven fabric. (iv) The tensile strength per unit area of ​​the spunbond nonwoven fabric ((N / 5 cm) / (g / m)) is calculated based on the following formula: 2 )) and round off to the third decimal place.

[0034] Tensile strength per unit area of ​​spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) = [tensile strength of spunbond nonwoven fabric (N / 5 cm)] / basis weight (g / m 2 ).

[0035] The apparent density of the spunbond nonwoven fabric of the present invention is 0.40 g / cm 3 1.00g / cm or more 3 It is preferable that the apparent density is 0.40 g / cm or less. 3 or more, preferably 0.42 g / cm 3 More preferably, 0.45 g / cm 3 By adjusting the apparent density to 1.00 g / cm or more, a spunbond nonwoven fabric having both thinness and mechanical strength can be obtained. 3 or less, preferably 0.95 g / cm 3 or less, more preferably 0.90 g / cm 3 By setting the thickness below this, it is possible to provide a certain level of breathability, and when used as a printing substrate, for example, this is preferred because it allows ink to easily penetrate deep into the nonwoven fabric.

[0036] The apparent density (g / cm) of the spunbond nonwoven fabric 3 ) is the basis weight (g / m) of the spunbond nonwoven fabric described later. 2) is converted into units by the thickness (mm) of the spunbond nonwoven fabric described later, and the result (g / cm 3 The value calculated by rounding the measurement value (mm) to two decimal places is used. The thickness (mm) of the spunbond nonwoven fabric is calculated using the following procedure: (i) Three pieces of spunbond nonwoven fabric each 10 cm wide in the longitudinal direction are taken. (ii) Using a pressure tool with a diameter of 10 mm and a load of 10 kPa, the thickness is measured at 10 points per meter of the spunbond nonwoven fabric at equal intervals in the width direction to the nearest 0.01 mm. (iii) The arithmetic mean of the measurements obtained above is calculated for each of the three taken spunbond nonwoven fabrics, and the arithmetic mean for the three spunbond nonwoven fabrics is also calculated by rounding the arithmetic mean to two decimal places.

[0037] The basis weight (g / m) of the spunbond nonwoven fabric 2 The mass per unit area (g / m) is calculated by the following procedure: (i) Three pieces of spunbond nonwoven fabric measuring 30 cm x 50 cm are taken. (ii) The mass of each sample is measured, and the average of the obtained values ​​is calculated as the mass per unit area (g / m). 2 ) and rounded to one decimal place to calculate the basis weight. [Method for producing spunbonded nonwoven fabric] The spunbonded nonwoven fabric of the present invention can be preferably produced by the method for producing spunbonded nonwoven fabric of the present invention. That is, the method for producing spunbonded nonwoven fabric of the present invention is a method for producing the spunbonded nonwoven fabric of the present invention, and includes the following steps (a) to (c) in this order:

[0038] [Step (a): Step of Spinning Fibers] In step (a), a core-sheath type composite fiber is spun, in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower, and having an intrinsic viscosity (IV) that is 0.05 or higher and 0.25 or lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin, is disposed around the high-viscosity polyethylene terephthalate resin having a melting point of 250°C or higher and 270°C or lower.

[0039] That is, in the sheath-core composite fiber, it is preferable that the high-viscosity polyethylene terephthalate resin be the core component and the low-viscosity polyethylene terephthalate resin be the sheath component. By making the difference between the intrinsic viscosities of the core component and the sheath component 0.05 or more, more preferably 0.10 or more, spinning stress can be concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. On the other hand, by making the difference between the intrinsic viscosities of the core component and the sheath component 0.25 or less, preferably 0.20 or less, the single fiber strength of the sheath-core composite fiber can be improved, and rapid softening during thermocompression bonding can be suppressed, thereby suppressing sticking to heated rolls during production.

[0040] The core-sheath type composite fiber is preferably melted at a temperature of not less than its melting point but not more than 70°C above the melting point, and melt-extruded from a spinneret at a temperature of not less than its melting point but not more than 70°C above the melting point.

[0041] The shape of the outlet hole of the spinneret through which the core-sheath type composite fiber is extruded can be circular, elliptical, polygonal, multi-lobal, or a combination thereof, depending on the cross-sectional shape of the fiber. Among these, a circular shape is more preferred from the viewpoint of efficiently obtaining bonding points between the fibers and firmly bonding the fibers together by thermocompression bonding.

[0042] [Step (b): Step of forming a fiber web] In step (b), the spun core-sheath type composite fibers are pulled and stretched by an ejector and deposited on a moving net conveyor to form a fiber web.

[0043] In step (b), the spun fibers are preferably drawn and stretched by an ejector, and the fibers are deposited on a moving net conveyor to form a fiber web. In this case, the spinning speed for drawing the fibers is preferably 3000 m / min or more and 6000 m / min or less.

[0044] [Step (c): Step of thermocompression bonding the fiber web] In step (c), the fiber web is thermocompression bonded with a flat roll.

[0045] The fiber web can be heat-pressed to obtain the intended spunbonded nonwoven fabric.

[0046] The fiber web is thermocompressed using a pair of flat rolls. Unlike bonding using an embossing roll, thermocompression using flat rolls eliminates localized irregularities and reduces the maximum height roughness of the surface, resulting in a nonwoven fabric with excellent surface smoothness.

[0047] As for the surface material of the flat roll, a pair of metal rolls is preferred in order to obtain a sufficient thermocompression effect.

[0048] The surface temperature of the flat roll during thermocompression bonding is preferably set to a temperature 10°C to 100°C lower than the melting point (hereinafter sometimes referred to as Tm (°C)) of the polyethylene terephthalate resin being used (i.e., (Tm-100)°C to (Tm-10)°C). By setting the surface temperature of the thermoroll to (Tm-100)°C or higher, more preferably (Tm-90)°C or higher, it is possible to obtain a spunbonded nonwoven fabric that is strong enough for practical use by performing appropriate thermocompression bonding. Furthermore, by setting the surface temperature of the flat roll to (Tm-10)°C or lower, more preferably (Tm-15)°C or lower, excessive thermocompression bonding can be prevented, and the spunbonded nonwoven fabric can be prevented from partially becoming a film-like sheet.

[0049] The linear pressure of the flat roll during thermocompression bonding is preferably 90 N / cm or more and 1000 N / cm or less. By setting the linear pressure for thermocompression bonding to 90 N / cm or more, a spunbond nonwoven fabric with excellent mechanical strength can be obtained. By setting the linear pressure for thermocompression bonding to 1000 N / cm or less, excessive fusion of the fibers can be prevented.

[0050] [Wire Wrapping Tape] The wire wrapping tape of the present invention includes the nonwoven fabric. This allows for a wire wrapping tape that is thin, has good mechanical strength, and also has excellent surface smoothness. The wire wrapping tape of the present invention refers to a tape that is placed between an electric cable and the sheath that covers the cable to wrap the electric cable. The wire wrapping tape of the present invention can also be post-processed to impart properties such as semiconductivity and water absorption to the nonwoven fabric.

[0051] The applications for which the electric wire pressure winding tape of the present invention is used are not particularly limited, and it can be used in a variety of fields, such as power cables for electric power transmission and communication cables.

[0052] [Printing substrate] The printing substrate of the present invention comprises the nonwoven fabric described above. This makes it possible to obtain a printing substrate with excellent mechanical strength, good surface smoothness, and excellent printability. The printing substrate is preferably a substrate for commercial printing such as inkjet printing, laser printing, flexographic printing, letterpress printing, gravure printing, offset printing, and thermal transfer printing. The printing substrate of the present invention can also be subjected to post-processing to improve functions such as flame retardancy and hiding power.

[0053] The applications for which the printing substrate of the present invention is used are not particularly limited, and the printing substrate of the present invention can be used in a variety of fields. Specific examples of applications for which the printing substrate of the present invention is used include wallpaper, posters, labels, etc.

[0054] Next, the nonwoven fabric of the present invention will be specifically described based on examples, although the present invention is not limited to these examples.

[0055] [Measurement Methods] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were carried out according to the above-mentioned methods.

[0056] (1) Melting Point (°C) of Polyethylene Terephthalate Resin Using a differential scanning calorimeter ("DSC-2" manufactured by PerkinElmer Co., Ltd.), measurement was performed at a temperature rise rate of 16°C / min, and the temperature at which the extreme value was obtained in the obtained melting endothermic curve was taken as the melting point.

[0057] (2) Intrinsic Viscosity (IV) of Polyethylene Terephthalate Resin The intrinsic viscosity (IV) of the polyethylene terephthalate resin was measured by the following method.

[0058] 8 g of sample was dissolved in 100 mL of orthochlorophenol, and the relative viscosity η was measured at 25°C using an Ostwald viscometer. r was calculated using the following formula: η r = η / η 0 = (t × d) / (t 0 ×d 0 ) where η is the viscosity of the polymer solution, η 0 is the viscosity of orthochlorophenol, t is the solution drop time (seconds), and d is the solution density (g / cm 3 ), t 0 is the fall time of orthochlorophenol (seconds), d 0 is the density of orthochlorophenol (g / cm 3 ) respectively. Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV) = 0.0242η r +0.2634.

[0059] (3) Average Fiber Diameter (μm) of Fibers The average fiber diameter of the fibers was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0060] (4) Crystallization Peak Temperature (Tc) of Spunbond Nonwoven Fabric The crystallization peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter, "DSC-2 Model" manufactured by PerkinElmer Co., Ltd.

[0061] (5) Melting Peak Temperature (Tm) of Spunbond Nonwoven Fabric The melting peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter "DSC-2 Model" manufactured by PerkinElmer Co., Ltd.

[0062] (6) Surface Roughness in Maximum Height Rz (μm) of Spunbond Nonwoven Fabric The surface roughness in maximum height of a spunbond nonwoven fabric was calculated by the method described above using a surface roughness meter, "Surftest SJ-210" manufactured by Mitutoyo Corporation.

[0063] (7) Basis weight of spunbond nonwoven fabric (g / m 2 The basis weight of the spunbond nonwoven fabric was calculated using the method described above.

[0064] (8) Thickness (mm) of Spunbond Nonwoven Fabric The thickness of the spunbond nonwoven fabric was calculated by the method described above.

[0065] (9) Apparent density of spunbond nonwoven fabric (g / cm 3 The apparent density of the spunbond nonwoven fabric was calculated using the method described above.

[0066] (10) Tensile strength per unit area of ​​spunbond nonwoven fabric ((N / 5cm) / (g / m 2 ) The tensile strength per unit area of ​​the spunbond nonwoven fabric was measured by the above-mentioned method using Baldwin's RTG-1250.

[0067] (11) Arithmetic mean surface roughness Ra (μm) of spunbond nonwoven fabric The arithmetic mean surface roughness Ra of a spunbond nonwoven fabric was measured by the above-mentioned method using a surface roughness meter "Surftest SJ-210" manufactured by Mitutoyo Corporation.

[0068] [Resins Used] Details of the resins used in the Examples and Comparative Examples are described below. Polyethylene terephthalate resin A (PET_A): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.65 and a melting point of 255°C. Polyethylene terephthalate resin B (PET_B): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.51 and a melting point of 255°C. Polyethylene terephthalate resin C (PET_C): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.70 and a melting point of 255°C. Polyethylene terephthalate resin D (PET_D): polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.56 and a melting point of 255°C. Polyethylene terephthalate resin E (PET_E): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.45 and a melting point of 255°C. Polyethylene terephthalate resin F (PET_F): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.62 and a melting point of 255°C. Polyethylene terephthalate resin G (CO-PET): Copolymerized polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, having an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.

[0069] [Example 1] (Step of spinning fibers) Polyethylene terephthalate resin A and polyethylene terephthalate resin B were each melted at a temperature of 295° C. Next, concentric sheath-core composite fibers were spun from a circular nozzle using polyethylene terephthalate resin A as a core component and polyethylene terephthalate resin B as a sheath component at a spinneret temperature of 295° C. and a core:sheath weight ratio of 80:20.

[0070] (Step of forming a fiber web) The fibers spun in the above step were drawn at a spinning speed of 5000 m / min, and the basis weight of the resulting nonwoven fabric was 35.0 g / m 2The mixture was deposited on a net conveyor whose moving speed was adjusted so that the average fiber diameter was 10.1 μm, thereby forming a fiber web made of fibers having an average fiber diameter of 10.1 μm.

[0071] (Step of thermocompression bonding of fiber web) Subsequently, the formed fiber web was thermocompression bonded using a pair of upper and lower hot flat rolls consisting of an upper roll and a lower roll under the conditions of a surface temperature of the hot flat roll of 180°C and a linear pressure of 686 N / cm to obtain a spunbonded nonwoven fabric. Upper roll: metal flat roll Lower roll: metal flat roll

[0072] The spunbonded nonwoven fabric obtained was evaluated, and the results are shown in Table 1.

[0073] [Example 2] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0074] [Example 3] In the fiber spinning process, polyethylene terephthalate resin A was changed to polyethylene terephthalate resin D. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0075] [Example 4] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin E. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 2. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0076] Comparative Example 1 In the fiber spinning step, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin A to form monocomponent fibers. In addition, in the step of thermocompression bonding the fiber web, the surface temperature of the hot flat roll was set to 250°C. Except for these, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0077] Comparative Example 2 In the fiber spinning step, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin G. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0078] Comparative Example 3 In the fiber spinning step, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin F. Otherwise, a spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0079] Comparative Example 4 In the step of thermocompression bonding the fiber web, the upper roll was changed from a metal flat roll to a metal circular pattern embossing roll (compression rate 16%). Except for this, a spunbonded nonwoven fabric was obtained using the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.

[0080]

[0081] The spunbonded nonwoven fabrics of Examples 1 to 4 had high tensile strength and excellent mechanical strength, and also had a low arithmetic mean roughness Ra and excellent surface smoothness.

[0082] On the other hand, the spunbonded nonwoven fabrics of Comparative Examples 1 to 4 had a high arithmetic mean roughness Ra and were not excellent in surface smoothness (Comparative Examples 1 to 4), or had low tensile strength and insufficient mechanical strength (Comparative Example 1).

Claims

1. A spunbond nonwoven fabric composed of fibers whose main component is polyethylene terephthalate resin, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C when measured by differential scanning calorimetry, and has a maximum height roughness Rz of 40.0 μm or less.

2. Apparent density is 0.40 g / cm 3 1.00g / cm or more 3 2. The spunbond nonwoven fabric of claim 1, wherein:

3. A wire pressure winding tape comprising the spunbond nonwoven fabric according to claim 1 or 2.

4. A printing substrate comprising the spunbond nonwoven fabric according to claim 1 or 2.

5. A method for producing the spunbonded nonwoven fabric according to claim 1 or 2, comprising the following steps (a) to (c) in this order: Step (a): A step of spinning out a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less and having an intrinsic viscosity (IV) lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is disposed around a high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 0.05 to 0.25 lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermocompressing the fiber web by a flat roll.

Citation Information

Patent Citations

  • Spun-bond nonwoven fabric

    JP2001140157A

  • Composite nonwoven fabric for patch

    JP2008163538A

  • Area-bonded nonwoven fabric manufactured from a single polymer system

    JP2010537068A

  • Short-cut fiber for wet-laid nonwoven fabric

    JP2014037644A

Cited By

  • Spunbond nonwoven fabric, method for manufacturing the same, and packaging material

    JP2026165683A