Resin composition, molded body, sheet, film, bottle, tube, container, multilayer structure, and method for producing resin composition

The combination of EVOH, carbon-14 polypropylene, and a boron compound in specific ratios addresses the thermal stability issue of EVOH resin compositions, resulting in a resin with enhanced thermal stability for use in molded bodies and multilayer structures.

WO2024204379A1PCT designated stage expired Publication Date: 2024-10-03MITSUBISHI CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
PCT/JP2024/012298
Authority / Receiving Office
WO · WO
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-28
Filing Date
2024-03-27
Publication Date
2024-10-03

AI Technical Summary

Technical Problem

EVOH resin compositions containing polypropylene for modification tend to have inferior thermal stability compared to those consisting only of EVOH, necessitating an improvement in thermal stability.

Method used

A resin composition comprising EVOH, a polypropylene resin containing carbon-14, and a boron compound, with specific mass ratios and content ranges, which enhances thermal stability through a synergistic effect between the increased bond energy of carbon-14 polypropylene and the thermal deterioration inhibiting properties of boron.

Benefits of technology

The resulting resin composition exhibits superior thermal stability, making it suitable for use in molded bodies and multilayer structures, with the carbon-14 polypropylene providing stronger bond energy and the boron compound further enhancing thermal resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure JPOXMLDOC01-APPB-T000001
    Figure JPOXMLDOC01-APPB-T000001
Patent Text Reader

Abstract

Provided is the following resin composition that contains an ethylene-vinyl alcohol copolymer and a polypropylene resin and has excellent thermal stability. The resin composition contains (A) an ethylene-vinyl alcohol copolymer, (B) a polypropylene resin containing carbon 14, and (C) a boron compound.
Need to check novelty before this filing date? Find Prior Art

Description

Resin composition, molded article, sheet, film, bottle, tube, container, multilayer structure, and method for producing resin composition

[0001] The present invention relates to a resin composition containing an ethylene-vinyl alcohol copolymer and a polypropylene resin containing 14 carbon atoms. The present invention also relates to a molded article, sheet, film, bottle, tube, or container containing the resin composition, a multilayer structure having a layer containing the resin composition, and a method for producing the resin composition.

[0002] Conventionally, ethylene-vinyl alcohol copolymer (hereinafter referred to as "EVOH") has been mainly used as a food packaging material due to its excellent gas barrier properties and transparency. Sheets, films, etc. used as the food packaging material can be produced using the above-mentioned EVOH alone, but they are also used as multilayer structures in which other thermoplastic resins are blended to improve physical properties, etc., or layers made of polyolefin resins, etc. are laminated to impart other functions.

[0003] For example, it has been proposed to incorporate two types of polypropylene with different physical properties in specific proportions into an EVOH resin composition in order to enhance the flexibility of a film or the like made of EVOH (see Patent Document 1 below).It has also been proposed to incorporate EVOH as a layer of a specific shape dispersed in polypropylene in order to enhance the gas barrier properties of a film or the like made of EVOH (see Patent Document 2 below).

[0004] JP 2022-34771 A JP 2016-150949 A

[0005] However, such EVOH resin compositions containing polypropylene for modification tend to have inferior thermal stability compared to resin compositions consisting of EVOH alone, and further improvements are therefore required.

[0006] Therefore, the present invention provides a polypropylene-containing EVOH resin composition that has excellent thermal stability.

[0007] In view of the above circumstances, the present inventors have found that the above problems can be solved by using a polypropylene resin containing 14 carbon atoms instead of polypropylene and further containing a boron compound.

[0008] That is, the present invention has the following aspects. [1] A resin composition containing EVOH (A), a carbon-14 containing polypropylene resin (B), and a boron compound (C). [2] The resin composition according to [1], wherein the mass ratio [(A) / (B)] of the EVOH (A) to the carbon-14 containing polypropylene resin (B) is 10 to 90 to 99 / 1. [3] The resin composition according to [1] or [2], wherein the content of the EVOH (A) relative to the entire resin composition is 10 to 99 mass%. [4] The resin composition according to any one of [1] to [3], wherein the content of the carbon-14 containing polypropylene resin (B) relative to the entire resin composition is 1 to 90 mass%. [5] The resin composition according to any one of [1] to [4], wherein the content of the boron compound (C) relative to the entire resin composition is 1 to 10,000 ppm by mass. [6] A molded article comprising the resin composition according to any one of [1] to [5]. [7] A sheet comprising the resin composition according to any one of [1] to [5]. [8] A film comprising the resin composition according to any one of [1] to [5]. [9] A bottle comprising the resin composition according to any one of [1] to [5].

[10] A tube comprising the resin composition according to any one of [1] to [5].

[11] A container comprising the resin composition according to any one of [1] to [5].

[12] A multilayer structure having a layer comprising the resin composition according to any one of [1] to [5].

[13] A method for producing a resin composition, comprising the step of mixing EVOH (A), a carbon-14 containing polypropylene resin (B), and a boron compound (C).

[0009] The resin composition of the present invention has excellent thermal stability. Therefore, the resin composition of the present invention can be suitably used as a raw material for molded articles and multilayer structures. The excellent thermal stability of the resin composition of the present invention is thought to be due to the fact that the carbon-14-containing polypropylene resin has stronger bond energy due to the primary isotope effect compared to petroleum-derived polypropylene resins that do not contain carbon-14, which slows decomposition and increases thermal stability, and also due to a synergistic effect with the boron compound (C) that has a thermal degradation suppressing effect.

[0010] The present invention will be described in more detail below based on examples of the present invention, but the present invention is not limited to these examples.

[0011] In this specification, when "X to Y" (X and Y are any numbers) is used, it means "X or more and Y or less," unless otherwise specified, and also includes the meaning of "preferably greater than X" or "preferably smaller than Y." Furthermore, when "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also includes the meaning of "preferably greater than X" or "preferably less than Y." Furthermore, "X and / or Y (X and Y are any configurations)" means at least one of X and Y, and can mean three possibilities: X only, Y only, or X and Y. For numerical ranges described in stages in this specification, the upper or lower limit of a numerical range in one stage can be arbitrarily combined with the upper or lower limit of a numerical range in another stage. Furthermore, in the numerical ranges described in this specification, the upper or lower limit of the numerical range can also be replaced with the values ​​shown in the examples.

[0012] In this specification, the term "film" also includes "tape" and "sheet." In this specification, the term "main component" refers to a component that has a significant effect on the properties of the target object, and the content of the component is usually 50% by mass or more, preferably 55% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, and may be 100% by mass.

[0013] A resin composition according to an embodiment of the present invention (hereinafter referred to as "the resin composition") contains EVOH (A), a polypropylene resin containing 14 carbon atoms (B), and a boron compound (C). Each component will be described below.

[0014] <EVOH (A)> The EVOH (A) is a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.

[0015] The polymerization of ethylene and vinyl ester monomers can be carried out by any known polymerization method, such as solution polymerization, suspension polymerization, or emulsion polymerization, and solution polymerization using methanol as a solvent is generally used. The resulting ethylene-vinyl ester copolymer can also be saponified by a known method.

[0016] The EVOH (A) produced in this manner is mainly composed of structural units derived from ethylene and vinyl alcohol structural units, and usually contains a small amount of vinyl ester structural units that remain unsaponified.

[0017] Vinyl acetate is typically used as the vinyl ester monomer because of its commercial availability and the efficiency of impurity removal during production. Examples of vinyl ester monomers other than vinyl acetate include aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate. Aliphatic vinyl esters having typically 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms can be used. These can be used alone or in combination of two or more types.

[0018] The ethylene content in the EVOH (A) can be controlled by the ethylene pressure when copolymerizing the vinyl ester monomer with ethylene, and is 20 to 60 mol %, preferably 25 to 50 mol %, and particularly preferably 25 to 35 mol %. If the content is too low, the gas barrier properties and melt moldability under high humidity conditions tend to decrease, while if the content is too high, the gas barrier properties tend to decrease. The ethylene content can be measured in accordance with ISO 14663.

[0019] The degree of saponification of the vinyl ester component in EVOH (A) can be controlled by the amount, temperature, time, etc. of the saponification catalyst (usually an alkaline catalyst such as sodium hydroxide is used) used when saponifying the ethylene-vinyl ester copolymer, and is usually 90 to 100 mol%, preferably 95 to 100 mol%, and particularly preferably 99 to 100 mol%. If the saponification degree is too low, the gas barrier properties, thermal stability, moisture resistance, etc. tend to decrease. The saponification degree of EVOH (A) can be measured in accordance with JIS K6726 (however, EVOH is used as a solution uniformly dissolved in a water / methanol solvent).

[0020] The melt flow rate (MFR) (210°C, 2160 g load) of the EVOH (A) is usually 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and particularly preferably 3 to 35 g / 10 min. If the MFR is too high, film-forming properties tend to become unstable, while if it is too low, the viscosity tends to become too high, making melt extrusion difficult. The MFR is an index of the degree of polymerization of the EVOH, and can be adjusted by the amount of polymerization initiator and the amount of solvent used when copolymerizing ethylene and a vinyl ester monomer.

[0021] EVOH (A) may further contain structural units derived from the comonomers shown below within a range that does not impair the effects of the present invention (for example, 10 mol % or less of the EVOH).Examples of the comonomer include olefins such as propylene, 1-butene, and isobutene; hydroxyl group-containing α-olefins such as 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol, and 5-hexene-1,2-diol, and derivatives thereof such as esters and acylation products; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyryloxy-2-methylenepropane. -hydroxyalkylvinylidene diacetates such as 2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid, or their salts or mono- or di-alkyl esters in which the alkyl group has 1 to 18 carbon atoms; acrylamide, N-alkylacrylamide in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salt, acrylamidopropyldimethylamine or its acid salt or its quaternary salt, etc. Acrylamides; methacrylamide, N-alkylmethacrylamides in which the alkyl group has 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidopropanesulfonic acid or a salt thereof, methacrylamidepropyldimethylamine or an acid salt or a quaternary salt thereof, and other methacrylamido groups; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, and N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; alkyl vinyl ethers in which the alkyl group has 1 to 18 carbon atoms, hydroxybenzoates, and the like; vinyl ethers such as alkoxyalkyl vinyl ether and alkoxyalkyl vinyl ether; halogenated vinyl compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; halogenated allyl compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; and comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamido-2-methylpropanesulfonic acid.These may be used alone or in combination of two or more.

[0022] In particular, EVOH copolymerized with a hydroxy group-containing α-olefin, i.e., EVOH having a primary hydroxy group in the side chain, is preferred because it exhibits good secondary moldability while maintaining gas barrier properties, and among these, EVOH having a 1,2-diol structure in the side chain is preferred. In the case of EVOH having a primary hydroxy group in the side chain, the content of structural units derived from the monomer having the primary hydroxy group is usually 0.1 to 20 mol %, preferably 0.5 to 15 mol %, and particularly preferably 1 to 10 mol %.

[0023] The EVOH (A) used in this embodiment may be "post-modified" such as urethanized, acetalized, cyanoethylated, or oxyalkylened.

[0024] Furthermore, the EVOH (A) used in the present embodiment may be a mixture of two or more types of EVOH (A), for example, EVOHs having different ethylene contents, different degrees of saponification, different degrees of polymerization, or different copolymerization components.

[0025] The content of EVOH (A) in the resin composition is typically 1% by mass or more, preferably 10 to 99% by mass, more preferably 30 to 95% by mass, and even more preferably 50 to 90% by mass, based on the total resin composition. When the value is within the above range, the effects of the present invention tend to be more effectively achieved. Note that the "resin composition" in the "total resin composition" that serves as the basis for the content of EVOH (A) refers to the EVOH resin composition as a final product, which contains EVOH resin (A), polypropylene resin (B) containing 14 carbon atoms, boron compound (C), various additives that are blended as necessary, and the like. The same applies to the following explanation.

[0026] <Carbon-14-containing polypropylene resin (B)> The carbon-14-containing polypropylene resin (B) used in the present resin composition refers to a polypropylene resin obtained by chemical or biological synthesis using renewable biomass resources as raw materials. Carbon-14-containing polypropylene resin (B) has the characteristic that, even when incinerated, it does not increase the carbon dioxide concentration in the atmosphere due to the carbon-neutrality of biomass.

[0027] The carbon-14-containing polypropylene resin (B) is preferably biopropylene derived from biopropanol obtained from plant raw materials. That is, the carbon-14-containing polypropylene resin (B) is preferably a plant-derived polypropylene resin.

[0028] In addition, plant (biomass resource) derived polypropylene resin and petroleum derived polypropylene resin do not differ in physical properties such as molecular weight and mechanical properties. Therefore, to distinguish between them, the bio-based content is generally used. The bio-based content is defined as the carbon content of petroleum derived polypropylene resin. 14 Since it does not contain radioactive carbon 14 (half-life 5730 years), 14 The concentration of carbon-14 in the polypropylene resin (B) is measured by accelerator mass spectrometry and used as an index of the content of plant-derived bio-polypropylene resin. Therefore, if a film is made using plant-derived polypropylene resin, measuring the bio-based content of the film will give a bio-based content that corresponds to the content of plant-derived polypropylene resin. That is, polypropylene resin (B) containing carbon-14 can be used to measure the radioactive carbon ( 14 C).

[0029] The biobased content can be determined, for example, by heating and stirring the resin composition in a water / methanol mixed solvent to dissolve the EVOH (A), and then measuring the carbon content of the remaining polypropylene resin ( 14 C) content can be determined by measuring it as follows: The sample to be measured is burned to generate carbon dioxide, which is purified in a vacuum line and reduced with hydrogen using iron as a catalyst to generate graphite. Then, this graphite is analyzed using a tandem accelerator-based14 Attach it to a dedicated C-AMS device (manufactured by NEC) 14 Counting C, 13 The concentration of C ( 13 C / 12 C), 14 The concentration of C ( 14 C / 12 C) is measured, and the carbon content of the sample is compared to that of the standard modern carbon. 14 The C concentration ratio is calculated, and the biobased content is determined in accordance with ASTM D 6866. The biobased content described above is used to distinguish between polypropylene resins derived from plants (biomass resources) and petroleum-derived polypropylene resins, and the measurement method is also as described above.

[0030] The carbon-14 content of the carbon-14-containing polypropylene resin (B) is not particularly limited, but the ratio of carbon-14 to total carbon in the carbon-14-containing polypropylene resin (B) is usually 1.0 × 10 -14 or more, 1.0 × 10 -13 The upper limit is usually 1.2 × 10 -12 is.

[0031] The resin composition contains polypropylene resin (B) containing carbon-14, and therefore has superior thermal stability compared to resin compositions containing conventional petroleum-derived polypropylene resins. The reason for this is presumably that polypropylene resins containing carbon-14 have stronger bond energy due to the primary isotope effect, which slows decomposition and enhances thermal stability.

[0032] The carbon-14-containing polypropylene resin (B) used in the resin composition typically has a biobased content of 1 to 99%, preferably 5 to 95%, and particularly preferably 10 to 90%. By setting the biobased content of the carbon-14-containing polypropylene resin (B) within this range, a resin composition with even better thermal stability can be obtained.

[0033] The type of "polypropylene" in the carbon-14 containing polypropylene resin (B) is not particularly limited, and may be a homopolypropylene or a copolymer of propylene and a small amount of a comonomer. The copolymer may be in the form of a block copolymer or a random copolymer. For example, a copolymer consisting of propylene and less than 50% by mass of another α-olefin monomer, or a copolymer consisting of 3% or less by mass of a non-olefin monomer having a functional group may be used.

[0034] Examples of the other α-olefins include ethylene, α-olefins having 4 to 20 carbon atoms, such as 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, 1-eicosene, 3-methyl- Examples include 1-butene, 4-methyl-1-butene, 3-methyl-1-pentene, 3-ethyl-1-pentene, 4-methyl-1-pentene, 4-methyl-1-hexene, 4,4-dimethyl-1-hexene, 4,4-dimethyl-1-pentene, 4-ethyl-1-hexene, 3-ethyl-1-hexene, 9-methyl-1-decene, 11-methyl-1-dodecene, 12-ethyl-1-tetradecene, etc. These may be used alone or in combination of two or more.

[0035] Examples of the non-olefin monomer include styrene monomers, diene monomers, cyclic monomers, oxygen atom-containing monomers, etc. These may be used alone or in combination of two or more.

[0036] Examples of the styrene monomer include styrene, 4-methylstyrene, and 4-dimethylaminostyrene.

[0037] Examples of the diene monomer include 1,3-butadiene, 1,4-pentadiene, 1,4-hexadiene, 1,5-hexadiene, 1,4-octadiene, 1,5-octadiene, 1,6-octadiene, 1,7-octadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 4-ethylidene-8-methyl-1,7-nonadiene, 4,8-dimethyl-1,4,8-decatriene (DMDT), dicyclopentadiene, cyclohexadiene, and dicyclooctadiene.

[0038] Examples of the cyclic monomer include methylenenorbornene, 5-vinylnorbornene, 5-ethylidene-2-norbornene, 5-isopropylidene-2-norbornene, 6-chloromethyl-5-isopropenyl-2-norbornene, 2,3-diisopropylidene-5-norbornene, 2-ethylidene-3-isopropylidene-5-norbornene, 2-propenyl-2,2-norbornadiene, and cyclopentene.

[0039] Examples of the oxygen atom-containing monomer include hexenol, hexenoic acid, and methyl octenoate.

[0040] The other α-olefins and non-olefin monomers may be derived from renewable biomass resources or petroleum. When using those derived from renewable biomass resources, the bio-based content of the final product can be further increased. When using those derived from petroleum, a wide variety of petroleum-based materials are available, and by using these materials in production, the physical properties of the carbon-14-containing polypropylene resin (B) can be easily adjusted.

[0041] As described above, the polypropylene resin (B) containing 14 carbon atoms is obtained by homopolymerization of propylene or copolymerization of propylene with a comonomer, and the polymerization or copolymerization can be carried out in accordance with a conventional method using a metallocene catalyst or a Ziegler-Natta catalyst. Among these, the use of a metallocene catalyst is preferred.

[0042] The polypropylene resin (B) containing 14 carbon atoms may be used alone or in combination of two or more kinds. Among them, homopolypropylene derived from biopropylene, or ethylene-propylene block copolymer, ethylene-propylene random copolymer, or impact copolymer derived from biopropylene are preferred in terms of moldability, handleability, and thermal stability.

[0043] The melt flow rate (MFR) (230°C, 2160 g load) of the polypropylene resin (B) containing carbon 14 is usually 0.1 to 100 g / 10 min, preferably 0.5 to 90 g / 10 min, and particularly preferably 2 to 80 g / 10 min. If the MFR is too high, film formability tends to be unstable, whereas if it is too low, the viscosity tends to be high, making melt extrusion difficult.

[0044] Commercially available polypropylene resin (B) containing carbon 14 that is preferably used in this embodiment includes HP640J manufactured by LyondellBasell.

[0045] The content of the carbon-14 containing polypropylene resin (B) in the resin composition is usually 0.5% by mass or more, preferably 1 to 90% by mass, more preferably 5 to 70% by mass, and particularly preferably 10 to 50% by mass, based on the total mass of the resin composition. By setting the content of the carbon-14 containing polypropylene resin (B) within this range, a resin composition with better thermal stability can be obtained.

[0046] In the resin composition, the mass ratio [(A) / (B)] of the EVOH (A) to the polypropylene resin (B) containing 14 carbon atoms is usually 10 / 99 to 99 / 1, preferably 30 / 70 to 95 / 5, and more preferably 50 / 50 to 90 / 10. When the mass ratio of the EVOH (A) to the polypropylene resin (B) containing 14 carbon atoms is within the above range, a resin composition having better thermal stability can be obtained.

[0047] In the present resin composition, the proportion of the total content of the EVOH (A) and the polypropylene resin (B) containing 14 carbon atoms in the entire resin composition is not particularly limited, but is usually 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more.

[0048] <Boron Compound (C)> Examples of the boron compound (C) used in the present resin composition include boric acid or a metal salt thereof, such as sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, and sodium octaborate), potassium borate (potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, and potassium octaborate), lithium borates (lithium metaborate, lithium tetraborate, and lithium pentaborate), calcium borate, barium borate (barium orthoborate, barium metaborate, barium diborate, and barium tetraborate), magnesium borates (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, and pentamagnesium tetraborate), and manganese borates (boric acid). manganese (II), manganese metaborate, manganese tetraborate, etc.), cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.), cadmium borate (cadmium orthoborate, cadmium tetraborate, etc.), silver borate (silver metaborate, silver tetraborate, etc.), copper borate (cupric borate, copper metaborate, copper tetraborate, etc.), nickel borate (nickel orthoborate, nickel diborate, nickel tetraborate, Examples of suitable boron borate include lead borate (e.g., lead octaborate, nickel octaborate, etc.), aluminum potassium borate, ammonium borate (e.g., ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate, etc.), lead borate (e.g., lead metaborate, lead hexaborate, etc.), bismuth borate, and boron itself, as well as borate minerals such as borax, kernite, inyoite, cottite, suianite, and seiberite. Of these, borax and boric acid are preferred. These may be used alone or in combination of two or more.

[0049] The boron compound (C) may be in any form, such as a solid (powder, fine powder, flakes, etc.), a semi-solid, a liquid, a paste, a solution, or an emulsion (aqueous dispersion), but a powder form is preferred.

[0050] The content of the boron compound (C) is usually 1 to 10,000 ppm, preferably 10 to 5,000 ppm, more preferably 50 to 2,500 ppm, and even more preferably 100 to 1,500 ppm by mass based on the total mass of the resin composition. If the content of the boron compound (C) is too high, the thermal stability tends to be impaired, whereas if it is too low, the moldability of the resin composition tends to be impaired.

[0051] The content of the boron compound (C) in the present resin composition can be measured, for example, by the following method. First, 0.1 g of the present resin composition is treated with concentrated nitric acid by microwave decomposition to obtain a solution, and the solution is diluted to a constant volume (0.75 mg / mL) with pure water to obtain a test solution. The test solution is then measured using an inductively coupled plasma atomic emission spectrometer (ICP-AES) (Model 720-ES, manufactured by Agilent Technologies). The boron content measured in this manner corresponds to the amount of boron derived from the boron compound.

[0052] Furthermore, when the present resin composition is combined with other thermoplastic resins or the like to form a molded product, for example, in the case of a multilayer structure, the layer made of the present resin composition to be measured can be removed from the multilayer structure by any method, and the boron content can then be quantified by the same method as above.

[0053] <Other Components> The resin composition may contain other resins (e.g., petroleum-derived polypropylene resins, other types of resins) other than the EVOH (A) and the carbon-14-containing polypropylene resin (B), and any additives other than the boron compound (C) (hereinafter, these are referred to as "other components") according to various purposes, within the scope of not significantly impairing the effects of the present invention. Only one type of other component may be used, or two or more types may be used in any combination and ratio.

[0054] Examples of the additives include antioxidants, ultraviolet absorbers, plasticizers, lubricants, fillers, and antistatic agents.

[0055] When the present resin composition contains the above-mentioned "other components," the total content thereof is usually 30% by mass or less, preferably 20% by mass or less, and more preferably 10% by mass or less, based on the present resin composition.

[0056] [Method for Producing Resin Composition] The resin composition can be produced by mixing the essential components EVOH (A), the carbon-14-containing polypropylene resin (B), and the boron compound (C), as well as the other components as needed. Examples of the mixing method include known methods such as a dry blending method, a melt mixing method in which a compound is obtained using a single-screw extruder or a twin-screw extruder, a solution mixing method, and an impregnation method, and these methods can be used in any combination.

[0057] [Resin Composition] The resin composition thus obtained is less likely to decompose under high temperature heating and has excellent thermal stability compared to conventional resin compositions obtained by combining EVOH and petroleum-derived polypropylene.

[0058] The biobased content of the resin composition can be determined by, for example, the carbon-14 ( 14 C) content can be determined by measuring it as follows: The sample to be measured is burned to generate carbon dioxide, which is purified in a vacuum line and reduced with hydrogen using iron as a catalyst to generate graphite. Then, this graphite is analyzed using a tandem accelerator-based 14 Attach it to a dedicated C-AMS device (manufactured by NEC) 14 Counting C, 13 The concentration of C ( 13 C / 12 C), 14 The concentration of C ( 14 C / 12 C) is measured, and the carbon content of the sample is compared to that of the standard modern carbon. 14 The C concentration is calculated, and the biobased content is determined in accordance with ASTM D6866.

[0059] The content of carbon-14 contained in the resin composition is not particularly limited, but the ratio of carbon-14 to the total carbon in the resin composition is usually 1.0 × 10 -16 or more, 1.0 × 10 -14 The upper limit is usually 1.2 × 10 -12 is.

[0060] The biobased content of the resin composition is usually 0.01 to 99.99%, preferably 0.1 to 99.9%, more preferably 1 to 99%, even more preferably 1 to 90%, and particularly preferably 10 to 90%, 2 to 70%, or 4 to 50%. By setting the biobased content of the resin composition within the above range, a resin composition with even better thermal stability can be obtained.

[0061] The melt flow rate (MFR) (210° C., 2160 g load) of the present resin composition is usually 0.1 to 100 g / 10 min, preferably 0.5 to 90 g / 10 min, and particularly preferably 2 to 80 g / 10 min.

[0062] The water content of the present resin composition is usually 0.01 to 0.5% by mass, preferably 0.02 to 0.35% by mass, and particularly preferably 0.05 to 0.3% by mass.

[0063] The water content of the resin composition is measured and calculated by the following method: The mass (W1) of the resin composition before drying is weighed on an electronic balance, dried in a hot air dryer at 150°C for 5 hours, and then cooled in a desiccator for 30 minutes, after which the mass (W2) is weighed and calculated using the following formula: Water content (mass%) = [(W1 - W2) / W1] x 100

[0064] The temperature difference due to mass reduction of the resin composition is usually 10°C or higher, preferably 11°C or higher, more preferably 12°C or higher, and even more preferably 13°C or higher. This temperature difference due to mass reduction can be calculated by measuring the mass reduction rate when the temperature is increased at 10°C / min under a nitrogen atmosphere using a thermogravimetric analyzer (Perkin Elmer, Pyris 1 TGA), and then subtracting the temperature at which the resin composition loses 10% of its mass from the temperature at which it loses 5% of its mass (temperature difference due to mass reduction). A higher value indicates slower decomposition of the resin composition, and therefore superior thermal stability of the resin composition.

[0065] The present resin composition is prepared as a resin composition in various forms, such as pellets or powder, and is provided as a material for various molded articles and multilayer structures. As described above, the present resin composition has excellent thermal stability, so molded articles using the present resin composition or multilayer structures having layers using the present resin composition are of excellent quality. In particular, in this embodiment, when the present resin composition is provided as a material for melt molding, the effects of the present invention tend to be more efficiently obtained, which is preferable.

[0066] [Molded Article] A molded article according to one embodiment of the present invention (hereinafter referred to as the "present molded article") is obtained by molding the present resin composition.

[0067] Examples of the shape of the molded article include films, sheets, tapes, cups, trays, tubes, bottles, containers, pipes, filaments, irregular cross-section extrusions, and various irregularly shaped articles.

[0068] The resin composition may be molded by any method that is generally applicable to resin compositions, such as extrusion molding, blow molding, injection molding, and thermoforming.

[0069] [Multilayer structure] A multilayer structure according to an embodiment of the present invention (hereinafter referred to as "the multilayer structure") has at least one layer containing the resin composition of the present invention. The multilayer structure can be further strengthened or imparted with other functions by being laminated with another substrate (hereinafter referred to as "substrate resin") whose main component is a thermoplastic resin other than the resin composition of the present invention.

[0070] Examples of the base resin include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and the side chain); and polyolefins containing unsaturated carboxylic acid. Examples of the polyolefin resin include polyolefin resins in the broad sense, including modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins graft-modified with an acid or an ester thereof, ionomers, ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, and aromatic or aliphatic polyketones.

[0071] Of these, polyamide resins, polyolefin resins, polyester resins, and polystyrene resins are preferred from the viewpoint of economy and productivity, and more preferred are polyolefin resins such as polyethylene resins, polypropylene resins, polycyclic olefin resins, and unsaturated carboxylic acid-modified polyolefin resins thereof.

[0072] The layer structure of the present multilayer structure can be any combination, such as a / b, b / a / b, a / b / a, a1 / a2 / b, a / b1 / b2, b2 / b1 / a / b1 / b2, or b2 / b1 / a / b1 / a / b1 / b2, where a represents the resin composition layer and b represents the base resin layer (b1, b2, ...). It is also possible to provide a recycled layer containing a mixture of the present resin composition and the base resin, obtained by remelting and molding end portions or defective products generated during the manufacturing process of the multilayer structure. The total number of layers in the multilayer structure is typically 2 to 15, preferably 3 to 10. In the above layer structure, an adhesive resin layer containing an adhesive resin may be interposed between each layer, if necessary.

[0073] Known adhesive resins can be used, and may be selected appropriately depending on the type of thermoplastic resin used in the base resin layer "b." Representative examples include carboxyl-containing modified polyolefin polymers obtained by chemically bonding an unsaturated carboxylic acid or its anhydride to a polyolefin resin via addition reaction, graft reaction, or the like. Examples of the carboxyl-containing modified polyolefin polymers include maleic anhydride-grafted polyethylene, maleic anhydride-grafted polypropylene, maleic anhydride-grafted ethylene-propylene (block and random) copolymers, maleic anhydride-grafted ethylene-ethyl acrylate copolymers, maleic anhydride-grafted ethylene-vinyl acetate copolymers, maleic anhydride-grafted polycyclic olefin resins, and maleic anhydride-grafted polyolefin resins. One or a mixture of two or more selected from these can be used.

[0074] In the present multilayer structure, when an adhesive resin layer is used between the resin composition layer and the base resin layer, since the adhesive resin layers are located on both sides of the resin composition layer, it is preferable to use an adhesive resin with excellent hydrophobicity.

[0075] The base resin and adhesive resin may contain conventionally known plasticizers, fillers, clay (montmorillonite, etc.), colorants, antioxidants, antistatic agents, lubricants, core materials, antiblocking agents, waxes, etc., within a range that does not impair the spirit of the present invention (for example, 30% by mass or less, preferably 10% by mass or less, based on the total mass of the resin).

[0076] The present resin composition and the above-mentioned base resin can be laminated (including through an adhesive resin layer) by a known method. Examples include a method of melt-extrusion laminating the base resin onto a film, sheet, etc. of the present resin composition, a method of melt-extrusion laminating the present resin composition onto a base resin layer, a method of co-extruding the resin composition and the base resin, a method of dry-laminating the resin composition layer and the base resin layer using a known adhesive such as an organic titanium compound, an isocyanate compound, a polyester compound, or a polyurethane compound, and a method of applying a solution of the resin composition onto the base resin and then removing the solvent. Among these, the method of co-extruding the resin composition and the base resin is preferred from the viewpoints of cost and environment.

[0077] The multilayer structure is optionally subjected to a (heat) stretching treatment. The stretching treatment may be either uniaxial stretching or biaxial stretching, and in the case of biaxial stretching, it may be simultaneous stretching or sequential stretching. Furthermore, the stretching method may be a roll stretching method, tenter stretching method, tubular stretching method, stretch-blow method, vacuum pressure forming, or the like, whichever provides a higher stretch ratio. The stretching temperature is a temperature near the melting point of the multilayer structure, and is usually selected from the range of 40 to 170°C, preferably about 60 to 160°C. If the stretching temperature is too low, the stretchability will be poor, and if it is too high, it will be difficult to maintain a stable stretched state.

[0078] For the purpose of imparting dimensional stability, heat setting may be performed after the stretching treatment. Heat setting can be performed by known means, for example, by heat treating the stretched film while maintaining it in a tensile state, typically at 80 to 180°C, preferably 100 to 165°C, for typically 2 to 600 seconds. When the multilayer stretched film obtained from the present resin composition is used as a shrink film, heat shrinkability can be imparted by not performing the heat setting described above, but by performing a treatment such as cooling and setting the stretched film by blowing cold air on it.

[0079] In some cases, the multilayer structure can be used to produce cup- or tray-shaped multilayer containers. In this case, a drawing method is typically used, specifically vacuum forming, pressure forming, vacuum-pressure forming, plug-assisted vacuum-pressure forming, etc. Furthermore, blow molding is used to produce tube- or bottle-shaped multilayer containers (laminate structure) from a multilayer parison (a hollow tubular preform before blowing). Specific examples include extrusion blow molding (double-head, mold-moving, parison-shift, rotary, accumulator, horizontal parison, etc.), cold parison blow molding, injection blow molding, and biaxial stretch blow molding (extrusion-type cold parison biaxial stretch blow molding, injection-type cold parison biaxial stretch blow molding, injection-molding in-line biaxial stretch blow molding, etc.). The resulting laminate may be subjected to heat treatment, cooling treatment, rolling treatment, printing treatment, dry lamination treatment, solution or melt coating treatment, bag making, deep drawing, box processing, tube processing, splitting processing, etc. as required.

[0080] The thickness of the multilayer structure (including the stretched structure), and further the thickness of the resin composition layer, substrate resin layer, and adhesive resin layer constituting the multilayer structure, cannot be generally determined depending on the layer configuration, type of substrate resin, type of adhesive resin, intended use, packaging form, required physical properties, etc., but is usually 10 to 5,000 μm, preferably 30 to 3,000 μm, and particularly preferably 50 to 2,000 μm. The resin composition layer is usually 1 to 500 μm, preferably 3 to 300 μm, and particularly preferably 5 to 200 μm; the substrate resin layer is usually 5 to 3,000 μm, preferably 10 to 2,000 μm, and particularly preferably 20 to 1,000 μm; and the adhesive resin layer is usually 0.5 to 250 μm, preferably 1 to 150 μm, and particularly preferably 3 to 100 μm.

[0081] Furthermore, the thickness ratio of the resin composition layer to the base resin layer in the multilayer structure (resin composition layer / base resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 1 / 99 to 50 / 50, preferably 5 / 95 to 45 / 55, and particularly preferably 10 / 90 to 40 / 60. Furthermore, the thickness ratio of the resin composition layer to the adhesive resin layer (resin composition layer / adhesive resin layer), expressed as the ratio between the thickest layers when there are multiple layers of each type, is usually 10 / 90 to 99 / 1, preferably 20 / 80 to 95 / 5, and particularly preferably 50 / 50 to 90 / 10.

[0082] The bags made of the films, sheets, and stretched films obtained as described above, and containers made of cups, trays, tubes, bottles, etc. are useful as various packaging materials and containers for general foods as well as seasonings such as mayonnaise and dressings, fermented foods such as miso, oily foods such as salad oil, beverages, cosmetics, pharmaceuticals, etc.

[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. Unless otherwise specified, "parts" and "%" below refer to mass standards. Prior to the examples, the following components were prepared.

[0084] [EVOH] EVOH (A1): ethylene unit content 29 mol%, MFR (210°C, load 2160 g) 3.8 g / 10 min, saponification degree 99.9 mol% [Polypropylene resin] Carbon-14 containing polypropylene (B1): Carbon-14 containing polypropylene (manufactured by LyondellBasell, HP640J), MFR (230°C, load 2160 g) 3.2 g / 10 min, bio-based degree 40% Petroleum-derived polypropylene (B'1): Polypropylene (manufactured by Japan Polypropylene, FY6), MFR (230°C, load 2160 g) 2.4 g / 10 min

[0085] Example 1 90 parts of EVOH (A1), 10 parts of a carbon-14-containing polypropylene (B1), and a predetermined amount of a boron compound (C) were dry-blended all at once, and then fed to a twin-screw kneader at a rate of 8 kg / hour using a mass feeder. The resulting mixture was then strand-cut using a drum pelletizer to prepare a pelletized resin composition. The kneading conditions were as follows: Twin-screw extruder: diameter 20 mm, L / D=48 (manufactured by Toshiba Machine Co., Ltd.) Extruder temperature settings: C1 / C2 / C3 / C4 / C5 / C6 / H=170 / 200 / 210 / 210 / 210 / 210 / 210 Screw rotation speed: 250 rpm Take-up speed: 12 m / min

[0086] Examples 2 and 3, Comparative Examples 1 to 3 Resin compositions of Examples 2 and 3 and Comparative Examples 1 to 3 were prepared in the same manner as in Example 1, except that the types and amounts of each component were changed as shown in Table 1 below.

[0087] The following thermal stability evaluation was carried out using the obtained resin compositions of Examples 1 to 3 and Comparative Examples 1 to 3. The results are shown in Table 1 below.

[0088] [Evaluation of Thermal Stability] [Temperature Decrease Difference] Using 5 mg of the obtained pellet-like resin composition, the mass decrease rate was measured in a thermogravimetric analyzer (Perkin-Elmer, Pyris 1 TGA) under a nitrogen atmosphere while the temperature was increased at 10°C / min. The temperature at which the resin composition had a 10% mass decrease minus the temperature at which it had a 5% mass decrease (temperature decrease difference) was then calculated. The higher this value, the slower the decomposition of the resin composition, and the better the thermal stability of the resin composition. [Thermal Stability Improvement Rate] The thermal stability improvement rate was calculated using the following formula, where the temperature decrease difference of the comparative example corresponding to each example (for example, the comparative example corresponding to Example 1 is Comparative Example 1) is set to 100: Thermal Stability Improvement Rate (%) = (Temperature Decrease Difference of Example / Temperature Decrease Difference of the Comparative Example Corresponding to the Example × 100) - 100 (decimals below the decimal point in the thermal stability improvement rate (%) are rounded off).

[0089]

[0090] The results in Table 1 show that the resin compositions of Examples 1 and 2, which use carbon-14 polypropylene (B1) and a boron compound, have significantly improved thermal stability compared to Comparative Example 1, which uses only carbon-14 polypropylene (B1). This is thought to be due to the slower decomposition of carbon-14 polypropylene due to the stronger bond energy caused by the primary isotope effect, and the synergistic effect with the boron compound significantly enhances thermal stability. On the other hand, the resin composition of Comparative Example 2 uses petroleum-derived polypropylene (B'1), and therefore, although it contains a boron compound, it has inferior thermal stability compared to Example 1. Furthermore, Examples 1 to 3 and Comparative Examples 1 to 3 above demonstrate that the excellent thermal stability of the present invention can be achieved even when the blending ratios of the various components are changed. Molded articles, sheets, films, bottles, tubes, and containers containing the resin compositions of Examples 1 to 3, as well as multilayer structures having layers containing the resin compositions of Examples 1 to 3, also have excellent thermal stability.

[0091] Although the above examples show specific embodiments of the present invention, the examples are merely illustrative and should not be construed as limiting. Various modifications that are obvious to those skilled in the art are intended to fall within the scope of the present invention.

[0092] The resin composition has superior thermal stability to resin compositions using petroleum-derived polypropylene, and therefore molded articles made from the resin composition and multilayer structures having a layer containing the resin composition are useful as materials for various packaging containers.

Claims

1. A resin composition containing an ethylene-vinyl alcohol copolymer (A), a bio-polypropylene resin containing carbon-14 (B), and a boron compound (C).

2. The resin composition according to claim 1, wherein the mass ratio [(A) / (B)] of the ethylene-vinyl alcohol copolymer (A) to the polypropylene resin containing 14 carbon atoms (B) is 10 to 90 to 99 / 1.

3. A resin composition according to claim 1 or 2, wherein the content of the ethylene-vinyl alcohol copolymer (A) in the entire resin composition is 10 to 99 mass %.

4. A resin composition according to claim 1 or 2, wherein the content of the polypropylene resin (B) containing carbon-14 relative to the entire resin composition is 1 to 90 mass%.

5. A resin composition according to claim 1 or 2, wherein the content of the boron compound (C) in the entire resin composition is 1 to 10,000 ppm by mass.

6. A molded article comprising the resin composition according to claim 1 or 2.

7. A sheet comprising the resin composition according to claim 1 or 2.

8. A film comprising the resin composition according to claim 1 or 2.

9. A bottle comprising the resin composition according to claim 1 or 2.

10. A tube comprising the resin composition according to claim 1 or 2.

11. A container comprising the resin composition according to claim 1 or 2.

12. A multilayer structure having a layer containing the resin composition according to claim 1 or 2.

13. A method for producing a resin composition, comprising the step of mixing an ethylene-vinyl alcohol copolymer (A), a carbon-14 containing polypropylene resin (B), and a boron compound (C).

Citation Information

Patent Citations

  • Molding and method for producing the same

    JP2016150949A

  • Fresh-keeping plastic packaging bag for foods

    CN109320846A

  • Preparation of resin composition

    JP1998330533A

  • Ethylene-vinyl alcohol resin composition

    JP2022034771A

  • Resin composition, method for producing resin composition, molded article, multilayer structure and packaging body