Metal foil for current collectors, electrode, and battery
The use of a metal foil with a composite surface of Ni particles and resin on the current collector addresses the challenge of achieving high adhesion and maintaining discharge capacity by optimizing the surface structure, ensuring effective battery performance.
Patent Information
- Application Number
- PCT/JP2024/012304
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-30
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Current metal foils for current collectors in batteries face challenges in achieving high adhesion to the electrode mixture layer while maintaining the discharge capacity, as surface roughening can increase the volume of the current collector, potentially reducing battery performance.
A metal foil with a composite surface consisting of Ni particles and resin, where the Ni particles have an average size of 20 μm or less, a sintered body, and a resin volume ratio of 14.0 to 40.0%, forming peaks with a height exceeding 10 μm, as determined by line roughness analysis, to enhance adhesion without increasing the volume of the current collector excessively.
The solution provides high adhesion to the electrode mixture layer while maintaining the discharge capacity of the battery, as the composite structure allows for improved contact resistance and penetration of the active material and binder, ensuring effective battery performance.
Smart Images

Figure JP2024012304_03102024_PF_FP_ABST
Abstract
Description
Metal foil for current collector, electrode, and battery
[0001] The present disclosure relates to a metal foil for a current collector used in an electrode of a battery, an electrode using the metal foil for a current collector, and a battery using the electrode.
[0002] Batteries such as primary batteries and secondary batteries have been used as power sources for various electronic devices. Specifically, in recent years, secondary batteries, typified by lithium-ion batteries, have rapidly become popular due to the widespread use of small electronic devices such as home video cameras, laptops, and smartphones. As such small electronic devices become smaller and more powerful, batteries are being required to be further miniaturized and have improved performance. In this specification, the term "secondary battery" is a general term that includes, for example, non-aqueous electrolyte secondary batteries, aqueous electrolyte secondary batteries, and all-solid-state secondary batteries.
[0003] A battery includes electrodes and an electrolyte. The electrodes include a positive electrode and a negative electrode. Both the positive electrode and the negative electrode have an electrode mixture layer formed on a current collector. The current collector is the base material of the electrode. The electrode mixture layer is a layer containing an active material. The electrode mixture layer may contain a binder. The current collector has the function of supplying current to the active material and the function of holding the active material. Until now, metal foils have been used as current collectors. Specifically, for example, in lithium-ion batteries, copper foil is currently used as the negative electrode current collector and aluminum foil is currently used as the positive electrode current collector.
[0004] The active material means a material that can absorb and release ions contained in the electrolyte. Specifically, for example, in lithium ion batteries, graphite-based carbon materials are currently used as negative electrode active materials, and LiCoO 2 The binder has a function of binding the active materials together and between the active materials and the current collector. The binder is, for example, a resin.
[0005] When the electrolyte is dissolved in a liquid, the battery also includes a separator in addition to the electrodes and electrolyte. The separator acts as an insulator between the positive and negative electrodes, preventing electrical short circuits. Specifically, for example, liquid-based lithium-ion batteries currently use porous organic membranes as separators. The electrolyte exchanges ions with the positive and negative electrodes. In recent years, solid electrolytes have been developed in addition to liquid electrolyte solutions.
[0006] Incidentally, it is preferable that the metal foil used as the substrate of the current collector has high adhesion to the electrode mixture layer. If the adhesion to the electrode mixture layer is low, the electrode mixture layer is likely to peel off from the metal foil for the current collector. As a result, an electrode comprising the metal foil for the current collector and the electrode mixture layer will not be able to fully perform its functions. Therefore, the metal foil for the current collector is required to have excellent adhesion to the electrode mixture layer. JP 2011-009207 A (Patent Document 1) and JP 2009-026491 A (Patent Document 2) propose metal foils for current collectors that have improved adhesion to the electrode mixture layer.
[0007] The metal foil for a current collector disclosed in Patent Document 1 is a rolled copper foil for a lithium battery current collector, and has a surface roughness in the rolling direction of the top and bottom surfaces that satisfies 0.01 μm≦Ra≦0.10 μm and RSm≦20 μm. Patent Document 1 discloses that this metal foil for a current collector has high adhesion to a negative electrode active material by appropriately controlling the rolling conditions and forming finer irregularities on the surface rather than performing a roughening treatment.
[0008] The metal foil for a current collector disclosed in Patent Document 2 has a metal film formed by applying a dispersion of metal fine particles dispersed in a non-aggregated state to a base foil to form a coating film, and then heating the coating film in an inert atmosphere to aggregate and precipitate the metal fine particles. This metal film is characterized by having a roughly mountain-shaped configuration in which protruding fine particles with pointed apexes are connected together, and the protruding fine particles have a maximum particle diameter of 100 μm or less and a ten-point mean roughness Rz according to JIS B 0601-1994 of 0.4 to 10 μm. Patent Document 2 discloses that when an electrode mixture layer of Si or the like that constitutes an alloy-based negative electrode is formed on this metal foil for a current collector, even when the electrode mixture layer expands and contracts, the electrode mixture layer does not peel off and has excellent adhesion.
[0009] JP 2011-009207 A JP 2009-026491 A
[0010] As described above, metal foils for current collectors are required to have excellent adhesion to electrode mixture layers. Patent Documents 1 and 2 propose metal foils for current collectors that have excellent adhesion to electrode mixture layers. However, metal foils for current collectors that have excellent adhesion to electrode mixture layers may be obtained by techniques other than those disclosed in Patent Documents 1 and 2.
[0011] Generally, increasing the volume of components involved in power storage inside a battery (e.g., active materials and electrolytes) increases the discharge capacity of the battery. Furthermore, as mentioned above, there has been a demand in recent years for further miniaturization of batteries. In other words, in the development of batteries, strict restrictions are sometimes imposed on the volume of the battery. Meanwhile, current collectors are not involved in power storage. Therefore, if the volume occupied by the current collectors increases, the volume of the components involved in power storage will decrease due to the battery volume restrictions. In this case, there is a concern that the discharge capacity of the battery will decrease.
[0012] In the above-mentioned Patent Documents 1 and 2, an uneven shape is formed on the surface of the metal foil for a current collector to improve adhesion with the electrode mixture layer. When an uneven shape is formed on the surface of the metal foil for a current collector to improve adhesion with the electrode mixture layer, the volume of the current collector increases by the amount of the uneven shape. In this case, there is a concern that the discharge capacity of the battery will decrease due to the constraints of the battery volume. In other words, there is a demand for metal foil for a current collector to have both excellent adhesion to the electrode mixture layer and the ability to maintain the discharge capacity of the battery.
[0013] An object of the present disclosure is to provide a metal foil for a current collector that can improve adhesion to an electrode mixture layer while maintaining the discharge capacity of the battery, an electrode using the metal foil for a current collector, and a battery using the electrode.
[0014] A metal foil for a current collector according to the present disclosure comprises: a substrate; and a plurality of composites held on the surface of the substrate, wherein the plurality of composites include Ni particles having an average particle size of 20 μm or less, a sintered body formed by sintering the plurality of Ni particles, and 14.0 to 40.0 volume % of a resin, and the number of peaks on the surface of the metal foil for a current collector, which are identified by line roughness analysis and have a height from the surface of the substrate of more than 10 μm, is 20.0 to 50.0 peaks / mm.
[0015] The electrode according to the present disclosure comprises: the current collector metal foil; and an electrode mixture layer formed on the surface of the current collector metal foil.
[0016] A battery according to the present disclosure comprises the electrodes and an electrolyte.
[0017] The metal foil for a current collector according to the present disclosure can improve adhesion to an electrode mixture layer while maintaining the discharge capacity of the battery. The electrode according to the present disclosure has high adhesion between the metal foil for a current collector and the electrode mixture layer. The battery according to the present disclosure can maintain the discharge capacity of the battery to a certain extent.
[0018] Fig. 1 is a diagram showing an example of a microscopic image of a metal foil for a current collector having a composite of Ni particles and a resin formed on the surface of a substrate. Fig. 2 is a diagram showing another example of a microscopic image of a metal foil for a current collector having a composite of Ni particles and a resin formed on the surface of a substrate. Fig. 3 is a diagram showing another example of a microscopic image of a metal foil for a current collector having a composite of Ni particles and a resin formed on the surface of a substrate.
[0019] The present inventors have investigated means for obtaining a metal foil for a current collector that can improve adhesion to an electrode mixture layer while maintaining the discharge capacity of the battery, and have made the following discoveries.
[0020] The present inventors first focused on the surface of metal foil for current collector. When a metal foil with a smooth surface is used, there is a concern that adhesion to the electrode mixture layer may not be obtained. In particular, metal foils manufactured by cold rolling tend to have very smooth surfaces. Even in such cases, the present inventors thought that roughening the surface of the metal foil could potentially improve adhesion to the electrode mixture layer.
[0021] On the other hand, as mentioned above, the current collector itself does not contribute to power storage. In other words, roughening the surface of a metal foil for a current collector to form large irregularities on the metal foil surface may improve adhesion to the electrode mixture layer, but there is a concern that the proportion of the current collector in the battery volume will increase, reducing the battery's discharge capacity. Therefore, the present inventors investigated forming fine irregularities on the surface of the metal foil substrate using fine metal particles.
[0022] Specifically, the inventors focused on nickel (Ni) particles as fine metal particles. Ni particles have a larger particle diameter than fine carbon particles such as carbon black. Therefore, if Ni particles are bonded together and dispersed and held on the surface of a metal foil, it may be possible to form large irregularities. Furthermore, when Ni particles are dispersed and held on the surface of a metal foil, their high corrosion resistance allows the electrical conductivity of the metal foil surface to be maintained at a high level. Therefore, the use of Ni particles may enable the contact resistance of the electrode to be maintained at a low level.
[0023] Therefore, the present inventors have investigated binding Ni particles with a resin and holding them on the surface of a metal foil substrate. As a result of the investigations by the present inventors, it has become clear that if a composite formed by binding Ni particles with a resin is held on a part of the surface of the metal foil substrate, large irregularities can be formed on the surface of the metal foil. Hereinafter, in this specification, a composite formed by binding Ni particles with a resin will also be simply referred to as a "composite." The composite held on the surface of a metal foil substrate will be specifically described with reference to the drawings.
[0024] 1 and 2 are diagrams showing examples of microscopic images of a metal foil for a current collector in which a composite of Ni particles and a resin is formed on the surface of a substrate. Figures 1 and 2 were obtained by observing secondary electron images of the metal foil for a current collector in which a composite of Ni particles and a resin is held on the surface of a substrate using a scanning electron microscope (SEM). Note that in Figures 1 and 2, the composites were formed using Ni particles with different average particle sizes.
[0025] 1 and 2, the white region 10 in the figure indicates the region occupied by Ni particles and resin. Furthermore, the black region 20 in the figure indicates the region where Ni particles and resin are not present and the substrate surface is exposed. In other words, when a composite of Ni particles and resin is formed on the substrate surface, it can be confirmed that large irregularities can be formed on the surface of the metal foil for current collector while leaving a portion of the substrate surface exposed. In this case, it is possible to form large irregularities on the surface while keeping the volume of the metal foil for current collector to a certain extent.
[0026] As a result of detailed investigations based on the above findings, it has been revealed that in a current collector metal foil in which composites are formed on the surface of a substrate, the density of composites having a certain height or more affects the adhesion of the current collector metal foil to an electrode mixture layer. Therefore, in this embodiment, the density of composites formed on the substrate surface of the current collector metal foil is defined by line roughness analysis. Specifically, in this embodiment, the number of peaks with a height of more than 10 μm from the substrate surface, as determined by line roughness analysis of the surface of the current collector metal foil, is also referred to as the high spot count (HSC). In the current collector metal foil of this embodiment, the "peaks" determined by line roughness analysis essentially correspond to composites. Therefore, in this embodiment, the HSC essentially corresponds to the number of composites having a certain height or more formed on an imaginary 1 mm line on the surface of the current collector metal foil.
[0027] Here, if the HSC on the surface of the current collector metal foil is too small, the number of irregularities having a certain height formed on the surface of the current collector metal foil will be too small. As a result, sufficient adhesion of the current collector metal foil to the electrode mixture layer will not be obtained. On the other hand, if the HSC on the surface of the current collector metal foil is too large, the gap between the composites will be narrow, making it difficult for the active material of the electrode mixture layer and the binder to penetrate into the gap between the composites. As a result, sufficient adhesion of the current collector metal foil to the electrode mixture layer will not be obtained. In this case, there is a further concern that the volume of the composite will become too large, resulting in a decrease in the discharge capacity of the battery. Therefore, in this embodiment, the HSC on the surface of the current collector metal foil is set to 20.0 to 50.0 particles / mm.
[0028] Therefore, in this embodiment, the HSC density on the surface of the metal foil for a current collector is set to 20.0 to 50.0 particles / mm. Based on the above assumptions, the present inventors conducted further detailed studies and found that the adhesion of the metal foil for a current collector to the electrode mixture layer and the discharge capacity of the battery are affected not only by the HSC density but also by the size of the Ni particles, the proportion of the resin in the composite, and the morphology of the Ni particles.
[0029] First, the Ni particles in this embodiment have an average particle size of 20 μm or less for single particles (primary particles). If the average particle size of the primary particles is too large, it may be difficult to form a composite of the Ni particles and the resin. If the average particle size of the primary particles is too large, the volume of the composite may become too large, which may result in a decrease in the discharge capacity of the battery. Therefore, in this embodiment, the average particle size of the Ni particles (primary particles) is set to 20 μm or less.
[0030] Furthermore, the volume fraction of the resin in the composite of Ni particles and resin is 14.0 to 40.0%. If the volume fraction of the resin is too high, the resin may enter the gaps between the Ni particles, resulting in a smooth surface of the composite. In this case, the adhesion of the current collector metal foil to the electrode mixture layer decreases. On the other hand, if the volume fraction of the resin is too low, the composite of Ni particles and resin is less likely to be retained on the substrate surface. In this case, the adhesion of the current collector metal foil to the electrode mixture layer decreases. Therefore, in this embodiment, the volume fraction of the resin in the composite is set to 14.0 to 40.0%.
[0031] Furthermore, at least a portion of the Ni particles in the composite is sintered. Here, particles formed by sintering Ni particles together are also referred to as a "sintered body." A sintered body has void regions formed therein. Therefore, if the composite contains a sintered body, the active material of the electrode mixture layer and the binder enter the void regions inside the sintered body, dramatically increasing the adhesion of the current collector metal foil to the electrode mixture layer. If the composite contains a sintered body, the composite is even more likely to be formed tall. As a result, the adhesion of the current collector metal foil to the electrode mixture layer is further increased. Therefore, in this embodiment, the composite contains a sintered body formed by sintering Ni particles together.
[0032] The metal foil for a current collector, the electrode, and the battery according to the present embodiment, which have been completed based on the above findings, are summarized as follows.
[0033] [1] A metal foil for a current collector, comprising: a substrate; and a plurality of composites held on a surface of the substrate, wherein the plurality of composites include: Ni particles having an average particle size of 20 μm or less; a sintered body formed by sintering the plurality of Ni particles; and 14.0 to 40.0 volume % of a resin; and wherein, on the surface of the metal foil for a current collector, the number of peaks having a height of more than 10 μm from the surface of the substrate, as identified by line roughness analysis, is 20.0 to 50.0 peaks / mm.
[0034] [2] The metal foil for a current collector according to [1], wherein the average thickness of the substrate is 5 to 30 μm.
[0035] [3] An electrode comprising: the metal foil for a current collector according to [1] or [2]; and an electrode mixture layer formed on the surface of the metal foil for a current collector.
[0036] [4] A battery comprising the electrode according to [3] and an electrolyte.
[0037] The metal foil for a current collector according to this embodiment, the electrode according to this embodiment, and the battery according to this embodiment will be described below.
[0038] [Metal Foil for Current Collector] The metal foil for current collector according to this embodiment includes a substrate and a plurality of composites held on the surface of the substrate.
[0039] [Substrate] In this embodiment, the substrate is a metal foil. In this specification, "metal foil" refers to a metal plate having a thickness of 50 μm or less. In short, the thickness of the substrate of the metal foil for a current collector according to this embodiment is 50 μm or less. The thinner the thickness of the substrate, the smaller the volume of the metal foil for a current collector including the substrate. As a result, the volume of the current collector relative to the volume of the battery can be reduced, and the discharge capacity of the battery can be increased. However, if the thickness of the substrate is too thin, it becomes difficult to manufacture the substrate and the metal foil for a current collector using the substrate. In this specification, the thickness of the substrate refers to the average thickness of the substrate.
[0040] The substrate is not particularly limited as long as it is a metal foil, and well-known metal foils can be used. The metal foil may be, for example, a metal foil made of a single metal, a metal foil made of an alloy, or a metal foil having a plating layer on its surface. When the substrate is a metal foil made of a single metal, the single metal may be, for example, copper, aluminum, iron, nickel, zinc, silver, gold, manganese, or platinum. When the substrate is a metal foil made of an alloy, the alloy may be, for example, an iron-based alloy (steel), a nickel-based alloy (Ni-based alloy), or a copper-based alloy.
[0041] More specifically, when the substrate is an iron-based alloy foil (steel foil), the substrate may be a carbon steel foil or a stainless steel foil. When the substrate is a stainless steel foil, the type of stainless steel is not particularly limited, and may be, for example, a ferritic stainless steel foil, a martensitic stainless steel foil, an austenitic stainless steel foil, a ferritic-martensitic duplex stainless steel foil, or a ferritic-austenitic duplex stainless steel foil.
[0042] When the substrate is a metal foil having a plating layer on its surface, a known plating layer can be used as the plating layer. In this case, the plating layer may be a plating layer made of a single metal or a plating layer made of an alloy. When made of a single metal, the plating layer may be, for example, a nickel plating layer, a copper plating layer, or a zinc plating layer. Furthermore, the plating layer may be a single-layer plating or a multi-layer plating.
[0043] More preferably, the substrate is a steel foil having a nickel-plated layer (Ni-plated steel foil) or a stainless steel foil. When the substrate is a Ni-plated steel foil or a stainless steel foil, the substrate has excellent strength, heat resistance, and corrosion resistance. In this case, the Ni particles contained in the composite described below have excellent corrosion resistance and are therefore less likely to form an oxide film. Therefore, in an electrode fabricated using a current collector metal foil forming the composite, the Ni particles serve as electrical contact points, thereby reducing the electrical resistance of the electrode. In other words, when the substrate is a Ni-plated steel foil or a stainless steel foil, the synergistic effect with the Ni particles further improves the performance of the battery.
[0044] In this embodiment, the preferred upper limit of the thickness of the substrate is 45 μm, more preferably 40 μm, even more preferably 35 μm, and even more preferably 30 μm. In this embodiment, the preferred lower limit of the thickness of the substrate is 1 μm, more preferably 3 μm, and even more preferably 5 μm. In short, in this embodiment, the thickness of the substrate is preferably 5 to 30 μm. In this case, the substrate can be produced stably, and the discharge capacity of a battery using an electrode produced using the substrate is further increased.
[0045] [Composite] In the current collector metal foil according to this embodiment, multiple composites are held on the surface of a substrate. The multiple composites include Ni particles (primary particles) having an average particle size of 20 μm or less, a sintered body formed by sintering the Ni particles, and a resin. In other words, in this embodiment, it is sufficient that the multiple composites formed on the surface of the substrate as a whole include Ni particles, a sintered body, and a resin, and it is not necessary for all of the composites to include Ni particles, a sintered body, and a resin.
[0046] Specifically, in this embodiment, the composites are classified into the following three types: (Composite A) a composite containing Ni particles, a sintered body, and a resin; (Composite B) a composite containing a sintered body and a resin but not containing Ni particles; and (Composite C) a composite containing Ni particles and a resin but not containing a sintered body.
[0047] Here, composite A and composite B form large irregularities on the surface of the substrate, greatly improving the adhesion of the current collector metal foil to the electrode mixture layer. Therefore, in this embodiment, the densities of composite A and composite B are pseudo-counted using high spot count (HSC), which will be described later. On the other hand, composite C forms small irregularities on the surface of the substrate, so it does not contribute much to the adhesion of the current collector metal foil to the electrode mixture layer. However, the multiple composites held on the surface of the substrate of the current collector metal foil according to this embodiment may also include a composite (composite C) that does not contain a sintered body.
[0048] The composite according to this embodiment also contains a resin. Therefore, the Ni particles and / or the sintered body can be bound together. The resin further binds the composite to the surface of the substrate, holding the composite to the surface of the substrate. As a result, even if a certain amount of stress is applied when manufacturing the electrode, the shape of the composite is maintained, and adhesion to the electrode mixture layer is maintained.
[0049] [Ni Particles] In this embodiment, Ni particles refer to primary particles of particles containing Ni as a main component. In other words, the chemical composition of the Ni particles may be a chemical composition consisting of Ni and impurities, or a chemical composition consisting of a Ni-based alloy. In this specification, "primary particles" refers to single particles that are not sintered. In this specification, the average particle size of the Ni particles is 20 μm or less. Note that commercially available, well-known Ni particles can be used as the Ni particles.
[0050] Ni particles have a larger particle diameter than carbon particles, such as carbon black, that are applied to the substrate. Therefore, the composite according to this embodiment forms large irregularities on the surface of the substrate, thereby improving the adhesion of the current collector metal foil to the electrode mixture layer. On the other hand, if the average particle diameter of the Ni particles is too large, it may be difficult to form a composite of the Ni particles and the resin. Furthermore, if the average particle diameter of the Ni particles is too large, the volume of the composite may become too large, which may result in a decrease in the discharge capacity of the battery. Therefore, in this embodiment, the average particle diameter of the Ni particles (primary particles) is set to 20 μm or less.
[0051] The lower limit of the average particle size of the Ni particles is not particularly limited. The lower limit of the average particle size of the Ni particles may be, for example, 0.1 μm, 0.5 μm, or 1 μm. A preferred lower limit of the average particle size of the Ni particles is 2 μm. If the average particle size of the Ni particles is 2 μm or more, the void region in the composite containing the Ni particles increases, further increasing the discharge capacity. Therefore, the average particle size of the Ni particles is preferably 2 to 20 μm. A more preferred lower limit of the average particle size of the Ni particles is 3 μm, and even more preferably 5 μm. A preferred upper limit of the average particle size of the Ni particles is 15 μm, and even more preferably 10 μm. A method for determining the average particle size of the Ni particles will be described later.
[0052] [Sintered body] In this embodiment, a sintered body refers to a mass formed by sintering Ni particles (primary particles). In a sintered body, Ni particles are bonded to each other more strongly than in agglomerates. Therefore, void regions are formed inside the sintered body of the composite. As a result, the active material of the electrode mixture layer and a portion of the binder enter the void regions, dramatically increasing the adhesion of the current collector metal foil to the electrode mixture layer. If the composite contains a sintered body, the composite is more likely to be formed tall. As a result, the adhesion of the current collector metal foil to the electrode mixture layer is further increased.
[0053] The more sintered body is contained in the composite, the higher the proportion of void regions in the composite. In this case, the surface irregularities of the current collector metal foil formed by the composite become large, and the volume occupied by the current collector metal foil becomes small. As a result, the adhesion of the current collector metal foil to the electrode mixture layer becomes high, and the discharge capacity of the battery is less likely to decrease. Therefore, it is preferable that the composite contains a large amount of sintered body. However, in this embodiment, it is not necessary for all of the multiple composites to contain a sintered body. In the current collector metal foil according to this embodiment, the effect shown in this embodiment can be obtained as long as at least some of the multiple composites formed on the substrate surface contain a sintered body. A method for identifying whether a composite contains a sintered body will be described later.
[0054] In this embodiment, the measurement of the average particle size of Ni particles and the confirmation of the presence or absence of a sintered body can be performed by the following method. Specifically, a test piece for SEM observation is prepared from the metal foil for current collector according to this embodiment. The test piece is prepared by CP (cross section polisher: trademark) processing using an Ar ion beam. Specifically, first, the metal foil for current collector according to this embodiment is fixed to a Si wafer using an adhesive. CP processing is performed on the Si wafer to which the metal foil for current collector is fixed using a CP cross section specimen preparation device. Through the above steps, a test piece is prepared in which the cross section of the metal foil for current collector is used as the observation surface.
[0055] The observation surface of the prepared test piece is observed using a scanning electron microscope (SEM) with 10 fields of view as secondary electron images. The field area is, for example, 0.02 mm 2 (Magnification: 1000x). In each field of view, Ni particles can be identified from the contrast. In this case, if multiple Ni particles are not only arranged adjacent to each other but also form void regions, it can be determined that the multiple Ni particles are sintered.
[0056] This point will be explained more specifically with reference to the drawings. Fig. 3 is a diagram showing another example of a microscope image of a metal foil for a current collector in which a composite of Ni particles and a resin is formed on the substrate surface. Fig. 3 is a backscattered electron image obtained by SEM observation of a cross section of a metal foil for a current collector according to this embodiment, which was cut in the thickness direction by CP processing. Note that Fig. 3 is an image obtained by observation at a magnification of 3000 times. Referring to Fig. 3, the lower region 50 in the figure is the substrate (metal foil) of the metal foil for a current collector. Furthermore, referring to Fig. 3, the white region 30 in the figure corresponds to the cut surface of the Ni particles.
[0057] Referring to Figure 3, it can be seen that the cut surface 30 of the Ni particle in the figure has a circular outline and a complex outline. Specifically, it can be seen that the cut surface 30 of the Ni particle near the center of Figure 3 is formed by at least three or more Ni particles being integrated. In this way, when it can be seen from the cut surface that the Ni particles are integrated, rather than simply having their outer surfaces in contact, it can be determined that the plurality of Ni particles are sintered.
[0058] Furthermore, the primary particle diameter of Ni particles can be determined as follows. As described above, 100 or more random Ni particles are identified in 10 fields of view. The particle diameters of the identified Ni particles are determined by image analysis. The arithmetic mean value of the determined Ni particle diameters is defined as the average particle diameter (μm) of the Ni particles. The average particle diameter of Ni particles is determined by rounding the obtained value to one decimal place.
[0059] The measurement of the average particle size of Ni particles and the confirmation of the presence or absence of a sintered body can also be carried out by the following method. Specifically, if the average particle size of Ni particles is measured and the presence of a sintered body is confirmed in a composition used to produce a metal foil for a current collector, this can be carried out more easily than the above-mentioned method. Specifically, the particle size distribution of Ni particles in the composition is measured using a laser diffraction particle size distribution analyzer (Microtrac FRA, manufactured by Microtrac-Bell Corporation).
[0060] When Ni particles include not only primary particles but also sintered bodies, two peaks are observed in the histogram of particle size and frequency. In other words, in this case, the particle size distribution is bimodal. In this case, assuming that each of the two peaks has a normal distribution, the peak is separated into a peak with a small particle size and a peak with a large particle size. The particle size (μm) showing the mode of the peak with the small particle size thus identified is defined as the average particle size (μm) of Ni particles (primary particles). Note that even in this case, the average particle size of Ni particles is used by rounding the obtained value to one decimal place.
[0061] Furthermore, as described above, when the Ni particles include not only primary particles but also sintered bodies, the particle size distribution becomes bimodal. Therefore, in this embodiment, when the particle size distribution becomes bimodal and the frequency of the peak with a large particle size is greater than 1 / 5 of the frequency of the peak with a small particle size, it can be determined that the particles also include sintered bodies.
[0062] In the metal foil for a current collector according to this embodiment, the average particle size of Ni particles may be determined using any of the methods described above. Regardless of which method is used, the average particle size of Ni particles will be almost the same. Similarly, in the metal foil for a current collector according to this embodiment, the presence or absence of a sintered body may be confirmed using any of the methods described above. Regardless of which method is used, the presence or absence of a sintered body can be confirmed in the same way.
[0063] [Resin] In this embodiment, the resin binds the Ni particles and the sintered body to form a composite. In this embodiment, the resin is not particularly limited, and well-known resins can be used. The resin may be, for example, an aqueous resin or an organic solvent-based resin. Examples of aqueous resins include polyvinyl alcohol (PVA), carboxymethyl cellulose (CMC), polyacrylic acid (PAA), and styrene butadiene rubber (SBR). Examples of organic solvent-based resins include polymethyl methacrylate (PMMA), polytetrafluoroethylene (PTFE), polyimide (PI), polyamide (PA), and polyvinylidene fluoride (PVdF).
[0064] Preferably, the resin used in the composite of metal foil for a current collector according to this embodiment is an aqueous resin. Aqueous resins have a small environmental impact during production. For this reason, aqueous resins have been widely used as binders for the electrode mixture layers of electrodes described below. More preferably, the resin used in the composite of metal foil for a current collector according to this embodiment is styrene butadiene rubber (SBR).
[0065] In this embodiment, the volume fraction of the resin is 14.0 to 40.0%. If the volume fraction of the resin is too high, the resin may enter the gaps between the Ni particles, resulting in a smooth surface of the composite. In this case, the adhesion of the current collector metal foil to the electrode mixture layer decreases. On the other hand, if the volume fraction of the resin is too low, the composite of Ni particles and resin is less likely to be retained on the surface of the substrate. In this case, the adhesion of the current collector metal foil to the electrode mixture layer decreases. Therefore, in this embodiment, the volume fraction of the resin in the composite is 14.0 to 40.0%.
[0066] The lower limit of the volume fraction of the resin is preferably 16.0%, more preferably 18.0%, and even more preferably 20.0%, and the upper limit of the volume fraction of the resin is preferably 38.0%, more preferably 36.0%, and even more preferably 35.0%.
[0067] In this embodiment, the volume fraction of the resin can be determined by the following method. Specifically, an elemental analysis is performed on a test piece for SEM observation to measure the average particle size of the Ni particles using an electron probe microanalyzer (hereinafter also referred to as "EPMA"). Preferably, a field emission electron probe microanalyzer (FE-EPMA) is used as the EPMA. In the elemental analysis using EPMA, a wavelength dispersive X-ray spectrometer (hereinafter also referred to as "WDX") is used as the characteristic X-ray.
[0068] More specifically, in the same manner as in the case of measuring the average particle size of Ni particles described above, 10 secondary electron images are observed using an SEM. The area of the field of view is, for example, 0.02 mm. 2(Magnification: 1000x). Elemental analysis is performed using EPMA in each measurement field to generate an elemental map. In elemental analysis using EPMA with WDX, the target elements are Ni, Fe, C, and O. The region where C is detected as a result of the elemental analysis is defined as the region occupied by resin. The area fraction of the region occupied by resin in the observation field is calculated. In this embodiment, Ni particles and resin are present randomly, so the difference between the area fraction and the volume fraction is small. Therefore, in this embodiment, the area fraction occupied by resin is defined as the volume fraction (%) of resin. The volume fraction of resin is calculated by rounding the obtained value to one decimal place.
[0069] The volume fraction of the resin can also be determined by the following method. Specifically, the volume fraction of the resin can be determined from the mixing weight ratio of the compositions used in producing the current collector metal foil. For example, the specific gravity is 0.97 for styrene butadiene rubber (SBR), 1.6 for carboxymethyl cellulose (CMC), and 1.78 for polyvinylidene fluoride (PVdF). Furthermore, the volume fraction of the resin can be determined using the specific gravity of Ni particles. The specific gravity of Ni particles is, for example, 8.9. This method provides values that are almost identical to those obtained by the above-mentioned method of determining the volume fraction of the resin using SEM.
[0070] [High Spot Count (HSC)] The metal foil for current collector according to this embodiment has a surface that is subjected to line roughness analysis, and the number of peaks (HSC: high spot count) with a height of more than 10 μm from the substrate surface is determined to be 20.0 to 50.0 peaks / mm. As described above, the "peaks" determined by line roughness analysis essentially correspond to complexes. Therefore, in this embodiment, the HSC essentially corresponds to the number of complexes having a height equal to or greater than a certain level that are formed on an imaginary 1 mm line on the surface of the metal foil for current collector.
[0071] If the HSC on the surface of the current collector metal foil is too small, the number of irregularities having a certain height formed on the surface of the current collector metal foil will be too small. As a result, the current collector metal foil will not have sufficient adhesion to the electrode mixture layer. On the other hand, if the HSC on the surface of the current collector metal foil is too large, the gap between the composites will be narrow, making it difficult for the active material of the electrode mixture layer and the binder to penetrate into the gap between the composites. As a result, the current collector metal foil will not have sufficient adhesion to the electrode mixture layer. In this case, there is a further concern that the volume of the composite will become too large, resulting in a decrease in the discharge capacity of the battery. Therefore, in this embodiment, the HSC on the surface of the current collector metal foil is set to 20.0 to 50.0 particles / mm.
[0072] In this embodiment, the lower limit of the HSC on the surface of the metal foil for a current collector is preferably 21.0 counts / mm, more preferably 25.0 counts / mm, and even more preferably 30.0 counts / mm. The upper limit of the HSC on the surface of the metal foil for a current collector is preferably 48.0 counts / mm, more preferably 46.0 counts / mm, and even more preferably 42.0 counts / mm.
[0073] In this embodiment, the HSC of the surface of the metal foil for a current collector can be determined by the following method. Specifically, a line roughness analysis is performed on the surface of the metal foil for a current collector according to this embodiment to obtain a roughness curve. Note that the cross-sectional curve for obtaining the roughness curve is determined using a method in accordance with JIS B 0601 (2013). More specifically, the line roughness of the surface of the metal foil for a current collector according to this embodiment is measured using a profile measuring laser microscope. The profile measuring laser microscope is not particularly limited, but for example, a profile measuring laser microscope manufactured by Keyence Corporation (trade name: VK-X100) can be used. The magnification for the line roughness measurement is 2000 times. The evaluation length is not particularly limited, but for example, it is 100 to 150 μm.
[0074] From the results of the line roughness measurement, a profile curve is obtained in accordance with JIS B 0601 (2013). A low-pass filter with a reference length of 2.5 μm is applied to the obtained profile curve to obtain a roughness curve. Note that, depending on the average particle size of the Ni particles, it may be impossible to identify the height position of the substrate surface on the roughness curve. In this case, a portion of the surface of the metal foil for a current collector may be peeled off to define the height position of the substrate surface. Note that, in this case, it is preferable to perform line roughness analysis in multiple regions so that the total evaluation length in the unpeeled regions is 100 μm or more.
[0075] When the substrate (metal foil) is manufactured by rolling, the line roughness measurement is preferably performed in a direction perpendicular to the rolling direction of the substrate. That is, when the length direction of the substrate and the rolling direction are parallel, the line roughness measurement is preferably performed along the width direction of the substrate. The rolling direction of the substrate is determined by observing the surface of the metal foil for a current collector under a microscope. However, even those skilled in the art may not be able to determine the rolling direction of the substrate by observing the surface of the metal foil for a current collector under a microscope. In this case, the direction in which the line roughness measurement is performed does not have to be perpendicular to the rolling direction.
[0076] For the obtained roughness curve, a line is drawn 10 μm above the substrate surface (in the direction from the metal foil for current collector toward the space, in the height direction from the substrate surface) to serve as a reference line. The portion above the reference line is defined as a "peak," and the number of peaks is counted. The number of peaks is divided by the evaluation length to define the high spot count (HSC) (number / mm). The high spot count (HSC) is obtained by rounding the obtained value to one decimal place.
[0077] [Electrode] The electrode according to this embodiment includes the above-described metal foil for a current collector and an electrode mixture layer formed on the surface of the metal foil for a current collector. The electrode according to this embodiment may be a positive electrode or a negative electrode. That is, the electrode is not particularly limited as long as it includes the above-described metal foil for a current collector and an electrode mixture layer.
[0078] [Electrode Mixture Layer] In this embodiment, the electrode mixture layer is not particularly limited, and may have a well-known configuration. The electrode mixture layer contains an active material. The electrode mixture layer may further contain a binder, or may contain a composition other than the active material and the binder. In this case, for example, the electrode mixture layer contains a conductive additive. The conductive additive helps improve the electrical conductivity. In this embodiment, the binder is not particularly limited, and well-known binders can be used. The binder used in the electrode mixture layer is preferably the same type as the resin used in the above-mentioned composite.
[0079] [Active Material] In this embodiment, the active material is not particularly limited, and known active materials can be used. The active material is powder particles that do not dissolve in the electrolyte, which will be described later. When the electrode is a negative electrode, the negative electrode active material may be, for example, a carbon-based material such as graphite, an alloy material such as a CuSn alloy or a NiTiSi alloy, or a Si-based material such as SiO. When the electrode is a positive electrode, the positive electrode active material may be, for example, lithium cobalt oxide, a ternary material, lithium manganese oxide, or lithium iron phosphate. In other words, both the positive electrode active material and the negative electrode active material may have known configurations and are not particularly limited.
[0080] The electrode according to this embodiment includes the above-described metal foil for a current collector and a well-known electrode mixture layer formed on the surface of the metal foil for a current collector. As a result, the electrode according to this embodiment can maintain the discharge capacity of the battery and has high adhesion between the metal foil for a current collector and the electrode mixture layer.
[0081] [Battery] The battery according to this embodiment includes the above-described electrodes and an electrolyte. When the battery according to this embodiment is a liquid-based secondary battery, it includes a separator in addition to the electrodes and the electrolyte. The battery according to this embodiment may have any known configuration other than the electrodes including the above-described metal foil for current collector, and is not particularly limited. The shape of the battery according to this embodiment is not particularly limited, and may be cylindrical, prismatic, coin-shaped, or sheet-shaped. Furthermore, the battery according to this embodiment may be a secondary battery or a primary battery. When the battery according to this embodiment is a secondary battery, it may be, for example, a non-aqueous electrolyte secondary battery, an aqueous electrolyte secondary battery, or an all-solid-state secondary battery.
[0082] [Electrolyte] In the case of a liquid-based battery, the electrolyte exchanges ions with the positive electrode and the negative electrode through the electrolytic solution. In the case of an all-solid-state battery, the electrolyte exchanges ions directly with the positive electrode and the negative electrode. In this embodiment, the electrolyte is not particularly limited, and a well-known electrolyte can be used.
[0083] The battery according to this embodiment includes the above-described electrode and a known electrolyte, and as a result, the battery according to this embodiment can maintain its discharge capacity and has high adhesion between the current collector metal foil and the electrode mixture layer.
[0084] [Adhesion] The metal foil for a current collector according to this embodiment has high adhesion to an electrode mixture layer. In this embodiment, the adhesion of the metal foil for a current collector to an electrode mixture layer is evaluated by the following method.
[0085] A test piece is prepared from the current collector metal foil according to this embodiment. Specifically, the composition for the electrode mixture layer is applied to the current collector metal foil, dried, and then the test piece is cut out. The size of the current collector metal foil is, for example, 210 mm in length and 150 mm in width. The composition for the electrode mixture layer is not particularly limited, but for example, NiTiSi alloy powder, styrene butadiene rubber (SBR), and carboxymethyl cellulose (CMC) are mixed in a ratio of 95:4:1 and kneaded. In this case, water is used as the solvent. The composition for the electrode mixture layer is applied to the test piece using an applicator with a coating width of 80 mm and a gap of 150 μm.
[0086] The applied composition is heated at 75°C for 20 minutes to dry. A test piece is cut from the dried electrode. The test piece size is 15 mm in width and 50 mm or more in length. At this time, it is preferable to cut the test piece so that the length (50 mm or more) of the test piece includes 30 mm or more of the coated portion and 5 mm or more of the uncoated portion. Furthermore, it is preferable that the length direction of the test piece is parallel to the rolling direction of the substrate. A test piece having an electrode mixture layer formed thereon is prepared by the above method. A 90° peel test described in JIS Z 0237 (2009) is performed on the test piece. If excellent peel strength is obtained as a result of the 90° peel test, it is determined that the adhesion of the metal foil for current collector to the electrode mixture layer is excellent.
[0087] [Discharge Capacity] The metal foil for a current collector according to this embodiment can maintain its discharge capacity even when its adhesion to the electrode mixture layer is increased. In this embodiment, the discharge capacity is evaluated by the following method.
[0088] Specifically, when a composite is formed on a metal foil of the same thickness (e.g., 50 μm), the higher the volume fraction of the composite, the lower the discharge capacity when a battery is formed. Therefore, the volume fraction of the composite is calculated, and it is determined that the discharge capacity has decreased by that volume. The volume fraction of the composite can be determined from the applied weight of the composition, the specific gravities of the components of the composition (Ni particles, sintered body, and resin), and their mixing ratios. If the volume fraction of the composite is small, it is determined that the discharge capacity can be maintained when the metal foil for a current collector is used in a battery.
[0089] [Method for manufacturing metal foil for current collector] An example of a method for manufacturing metal foil for current collector according to this embodiment will be described. The manufacturing method described below is one example for manufacturing metal foil for current collector according to this embodiment, and the manufacturing method for metal foil for current collector according to this embodiment may be a manufacturing method other than the manufacturing method described below. However, the manufacturing method described below is a preferred example of a method for manufacturing metal foil for current collector according to this embodiment. The method for manufacturing metal foil for current collector according to this embodiment includes a substrate preparation step, a composition preparation step, and a composite formation step.
[0090] [Substrate Preparation Step] In the substrate preparation step, a substrate for a metal foil for a current collector is prepared. The method for preparing the substrate is not particularly limited and may be a well-known method. For example, the method for preparing the substrate may involve preparing an intermediate steel material having a desired chemical composition and cold working the intermediate steel material to prepare the substrate. This case will be specifically described below.
[0091] The intermediate steel material having a desired chemical composition can be appropriately set depending on the mechanical properties of the substrate to be obtained. Here, the intermediate steel material means a steel sheet having a thickness of several hundred μm to several mm. The intermediate steel material may be a stainless steel sheet or a plated steel sheet.
[0092] When preparing a substrate by cold working an intermediate steel material, a preferred cold working method is cold rolling. Cold rolling can be performed using a known device. For example, a multiple reversing cold rolling mill may be used. In this case, the degree of reduction in cold rolling is not particularly limited. The degree of reduction can be set appropriately depending on the thickness of the substrate to be obtained. Furthermore, the substrate after cold rolling may be subjected to an appropriate heat treatment.
[0093] As described above, in the substrate preparation step, a substrate is prepared. The substrate may be manufactured by the preferred process described above, or a substrate manufactured by a third party, or a substrate manufactured in a factory or business other than the factory where the composition preparation step described below is performed, may be prepared. In short, in this embodiment, the substrate preparation step is not particularly limited and may be a well-known method.
[0094] As described above, the substrate may have a plating layer on its surface. When forming a plating layer on the surface of the substrate, preferably, the plating layer is formed on the surface of an intermediate steel material, followed by cold rolling. In this case, the plating layer on the surface of the substrate can be formed thinly. Preferably, a Ni plating layer is formed on the surface of the intermediate steel material. In this case, for example, an intermediate steel material (thickness: several hundred μm) having a Ni plating layer is cold rolled to obtain a substrate having a thickness of 50 μm or less. The method for forming the Ni plating layer is not particularly limited, and any well-known method may be used.
[0095] [Composition Preparation Step] In the composition preparation step, a composition for forming and maintaining a composite on the surface of a substrate is prepared. The Ni particles, sintered body, and resin constituting the composition can be prepared by purchasing appropriate commercially available products.
[0096] Note that Ni particles may be heated at high temperatures during the manufacturing process. Therefore, commercially available, well-known Ni particles may be partially sintered. In other words, when well-known Ni particles are purchased, Ni particles (primary particles) may be mixed with a sintered body. In this case, the composite formed by the method described below may also contain a sintered body. On the other hand, if a certain level of stress is applied to a mixture of a sintered body and Ni particles, the sintered body will be crushed. Therefore, in the composition preparation step according to this embodiment, it is preferable to purchase Ni particles mixed with a sintered body from a third party. In this case, it is also preferable to consider the stress applied to the composition when mixing the composition so as not to crush the sintered body.
[0097] The prepared Ni particles, sintered body, and resin are mixed with a solvent as needed. Specifically, it is preferable to mix them using a planetary rotation / revolution mixer. In this case, a solvent is also used to appropriately control the viscosity. The solvent may be water or an organic solvent such as N-methyl-2-pyrrolidone (NMP).
[0098] [Complex Formation Step] In the composite formation step, a composite is formed and maintained on the surface of a substrate using the prepared composition. Specifically, the mixed composition is applied to the surface of the substrate. The application method is not particularly limited, and may be, for example, a gapped doctor blade method, a spray application method, a gravure coating method, or the like.
[0099] The substrate coated with the composition is dried to form a composite on the surface of the substrate. The drying method is not particularly limited, and any known method may be used. For example, drying may be performed by heating at 75°C for 20 minutes. For example, drying may be performed without further heating. The composition of the composite according to this embodiment contains a solvent. Therefore, even if a resin containing a solvent penetrates into the void region inside the sintered body, the void region will return after drying. It is presumed that such void region is obtained because the bonding strength of sintering is stronger than that of aggregation, etc.
[0100] The metal foil for a current collector according to this embodiment can be manufactured by the above steps. As mentioned above, the manufacturing steps described above are a preferred example for manufacturing the metal foil for a current collector according to this embodiment, and the manufacturing method of the metal foil for a current collector according to this embodiment is not limited to the above method.
[0101] [Method for Manufacturing Electrode] An example of a method for manufacturing an electrode using the metal foil for a current collector according to the present embodiment is as follows: The method for manufacturing an electrode according to the present embodiment includes an electrode mixture preparation step and an electrode mixture layer formation step.
[0102] [Electrode Mixture Preparation Step] In the electrode mixture preparation step, a composition for forming an electrode mixture layer is prepared. The composition for forming the electrode mixture layer may be prepared depending on the electrode mixture layer to be obtained. For example, the composition may be prepared by kneading an active material and a binder. For example, the composition may be prepared by further kneading an active material, a binder, and a conductive additive. For example, the composition may be prepared by further kneading an active material, a binder, and a solvent. For example, the composition may be prepared by further kneading an active material, a binder, a conductive additive, and a solvent. The kneading method is adjusted appropriately depending on the active material, binder, conductive additive, and solvent. In other words, the electrode mixture preparation step may be performed using a known method.
[0103] [Electrode Mixture Layer Forming Step] In the electrode mixture layer forming step, an electrode mixture layer is formed on the surface of the current collector metal foil. Specifically, the kneaded composition for forming the electrode mixture layer is applied to the current collector metal foil. The application method is not particularly limited, and any known method may be used. For example, the composition may be applied to the current collector metal foil using an applicator with a gap. For example, the composition may be further applied to the current collector metal foil by spraying using a sprayer.
[0104] The composition coated on the current collector metal foil is then dried to form an electrode mixture layer. The drying method is not particularly limited, and any known method may be used. For example, the composition may be dried by heating at 75°C for 20 minutes. For example, the composition may be dried without further heating.
[0105] The electrode according to this embodiment can be manufactured through the above steps. As described above, the manufacturing steps described above are a preferred example for manufacturing the electrode according to this embodiment, and the manufacturing method of the electrode according to this embodiment is not limited to the above method.
[0106] [Method for Manufacturing Battery] The method for manufacturing the battery according to this embodiment is not particularly limited. To manufacture the battery according to this embodiment, a laminate is manufactured by laminating the above-described electrode and a counter electrode by a well-known method. The laminate is placed in a case to manufacture the battery.
[0107] Substrates with the test numbers shown in Table 1 were prepared. The size of the substrate for each test number was a rectangle with a length of 210 mm and a width of 150 mm, with the longitudinal direction parallel to the rolling direction. The "Ni-plated steel foil" listed in the "Substrate" column of Table 1 refers to a Ni-plated steel foil with a thickness of 10 μm. The Ni-plated steel foil was prepared by cold-rolling a Ni-plated steel sheet with a thickness of 200 μm. The base material of the Ni-plated steel foil was ultra-low carbon steel. The "Stainless steel foil 1" listed in the "Substrate" column of Table 1 refers to a ferritic stainless steel foil with a thickness of 10 μm, which corresponds to SUS430 as specified in JIS G 4305 (2012). The "Stainless steel foil 2" listed in the "Substrate" column of Table 1 refers to a ferritic stainless steel foil with a thickness of 10 μm, which corresponds to SUS444 as specified in JIS G 4305 (2012).
[0108]
[0109] For each test number, a composition for forming a composite on the surface of the substrate was prepared. Specifically, a composition was prepared using the particles and resin listed in Table 1. Note that for test number 1, no composite was formed. "Ni-A" in the "Particles" column of Table 1 refers to Ni particles having a chemical composition consisting of Ni and impurities and an average primary particle size of 8 μm. These Ni particles were manufactured by Nilaco Corporation, product number NI-314010. "Ni-B" in the "Particles" column of Table 1 refers to Ni particles having a chemical composition consisting of Ni and impurities and an average primary particle size of 5 μm. These Ni particles were manufactured by VALE INCO, product number C-255.
[0110] The "Ni-C" in the "Particles" column of Table 1 is the same Ni particles as the "Ni-B" particles, but the particles were obtained by crushing the sintered body in advance through strong kneading. Specifically, 10 g of the "Ni-B" particles were mixed with 8.5 g of water, and crushed by processing for 2 minutes at a rotational peripheral speed of 30 m / s using a planetary kneader (product number ARE250, manufactured by Thinky Corporation).
[0111] "Ni-D" in the "Particles" column of Table 1 refers to Ni particles having a chemical composition consisting of Ni and impurities, with an average primary particle size of 53 μm or less. These Ni particles were manufactured by Kojundo Chemical Laboratory Co., Ltd., product number: NIE18PB. "C" in the "Particles" column of Table 1 refers to the use of carbon particles instead of Ni particles. The average particle size of these carbon particles was 1 μm. "Ni-E" in the "Particles" column of Table 1 refers to Ni particles having a chemical composition consisting of Ni and impurities, with an average primary particle size of 0.4 μm. These Ni particles were made by using ultrafine nickel powder (particle size 400 nm) manufactured by Toho Titanium Co., Ltd.
[0112] "SBR" in the "Resin" column of Table 1 means styrene butadiene rubber. As SBR, product number TRD2001 manufactured by JSR Corporation was used. "CMC" in the "Resin" column of Table 1 means carboxymethyl cellulose. As CMC, product number 2110 manufactured by Daicel Corporation was used. "PVdF" in the "Resin" column of Table 1 means polyvinylidene fluoride. As PVdF, product number KFP9100 manufactured by Kureha Corporation was used.
[0113] For test numbers 2 to 18, compositions mixed at the weight ratios shown in Table 1 were mixed using a planetary centrifugal mixer. Since SBR and CMC are water-based resins, water was used as the solvent. Furthermore, since PVdF is an organic solvent-based resin, N-methyl-2-pyrrolidone (NMP) was used as the solvent.
[0114] For test numbers 2 to 18, the prepared compositions were applied to the surface of the substrate. Application was performed using an automatic coating device (manufactured by Imoto Machinery Co., Ltd., model number: IMC-70F0). The substrate was fixed to the stage of the automatic coating device by vacuum suction, and the composition was applied using an applicator. At this time, the gap distance of the applicator was set to 25 to 50 μm to control the amount of application, and the application speed was set to 20 mm / sec. The amount of application of the composition to the surface of the substrate was adjusted by changing the gap distance of the applicator.
[0115] Test Nos. 2 to 18 were dried by being held for 20 minutes in a dryer set at 75° C. Metal foils for current collectors were produced in the above manner.
[0116] For the metal foil for current collector of each test number manufactured as described above, calculation of the amount of composition applied, confirmation of the presence or absence of a sintered body of the composite, calculation of the volume ratio of the resin in the composite, HSC measurement, adhesion test, and discharge capacity evaluation were performed. Note that for test number 1, no composite was formed, so only the adhesion test and discharge capacity evaluation were performed. For test number 16, the Ni particles were too large, so the Ni particles were dragged by the applicator when the composition was applied, and a composite could not be formed. Therefore, the above tests were not performed.
[0117] [Calculation of the amount of composition applied] The amount of composition applied was calculated for each test number except for test numbers 1 and 16. Specifically, a part of the metal foil for current collector of each test number except for test numbers 1 and 16 was punched out with a punch having a diameter of 13 mm. For each test number except for test numbers 1 and 16, the amount of composition applied (mg / cm) was calculated from the weight difference from test number 1 and the punched area. 2 The coating amounts obtained are shown in Table 1.
[0118] [Confirmation of the Presence or Absence of Sintered Body in Composite] For each test number of the current collector metal foil except for test numbers 1 and 16, it was confirmed whether or not a sintered body was contained in the composite. In this example, as a simple method, whether or not a sintered body was contained in the composition was confirmed using a laser diffraction particle size distribution analyzer. If the particle size distribution obtained with the laser diffraction particle size distribution analyzer was bimodal and the frequency of the peak with a large particle size was greater than 1 / 5 of the frequency of the peak with a small particle size, it was determined that the particles also contained a sintered body ("A (Acceptable)" in Table 2). If not, it was determined that the particles did not contain a sintered body ("NA (Not Acceptable)" in Table 2). The results of the determination are shown in Table 2.
[0119]
[0120] [Calculation of Volume Percentage of Resin in Composite] The volume percentage of resin in the composite was calculated for each test number of the current collector metal foil except for test numbers 1 and 16. In this example, the volume percentage of resin was calculated using the weight ratio and specific gravity of the resin in the composition as a simple method. The specific gravities used were 0.97 for SBR, 1.6 for CMC, 1.78 for PVdF, 8.9 for Ni particles, and 1.8 for carbon particles. The volume percentages of the resulting resins are shown in Table 2.
[0121] [HSC Measurement] For each of the current collector metal foils with test numbers 1 and 16, the HSC (pieces / mm) was measured using the method described above. The line roughness was measured using a shape measuring laser microscope VK-X100 manufactured by Keyence Corporation. The line roughness was measured at three random locations in the direction perpendicular to the longitudinal direction (rolling direction) of the current collector metal foil. The HSC was determined, and the arithmetic average value was used. The obtained HSC values are shown in Table 2.
[0122] [Adhesion Test] An adhesion test was carried out by the method described above for the metal foils for current collectors of each test number except for test number 16. The size of the test specimen was 15 mm in width and 74 mm in length (coated portion 40 mm). The peel strength (N / m) was determined for each test specimen. The peel strength of test number 1 was used as the reference value, and the peel strengths of the other test numbers were determined as relative values. The obtained peel strengths (relative values) are shown in the "Adhesion" column of Table 2.
[0123] [Discharge Capacity Evaluation] The discharge capacity of each current collector metal foil except for Test No. 16 was evaluated using the method described above. Specifically, the composition was applied to the substrate surface of each test number except for Test No. 16 to a thickness of 50 μm. The composition was dried at 75° C. for 20 minutes, and the volume occupied by the composite was determined. The volume occupied by the composite was calculated from the applied weight of the composition, the constituents of the composition, and the mixing ratio. Furthermore, an electrode mixture layer was formed to a thickness of 50 μm on the substrate surface to which the composition was not applied. The discharge capacity was defined as the volume of the electrode mixture layer with a thickness of 50 μm, minus the volume occupied by the composite, when the volume of the electrode mixture layer with a thickness of 50 μm was taken as 100.0. The obtained discharge capacity is shown in the "Discharge Capacity" column of Table 2.
[0124] [Evaluation Results] Referring to Tables 1 and 2, for the current collector metal foils of test numbers 2 to 10, the composites contained Ni particles with an average particle size of 20 μm or less, a sintered body, and 14.0 to 40.0 volume % of resin. These current collector metal foils also had an HSC of 20.0 to 50.0 particles / mm. As a result, the peel strength (relative value) was 1.50 or more, indicating excellent adhesion. These current collector metal foils also had a discharge capacity (relative value) of 85.0 or more, indicating that the discharge capacity was maintained despite the high adhesion.
[0125] Furthermore, the average particle size of the Ni particles in the current collector metal foils of test numbers 2 to 9 satisfied the requirement of 2 to 20 μm. As a result, the discharge capacity (relative value) of these current collector metal foils was 89.0 or more, and the discharge capacity was further maintained.
[0126] On the other hand, the current collector metal foil of test number 11 did not contain a sintered body in the composite, and as a result, the peel strength (relative value) of this current collector metal foil was less than 1.50, and it did not have excellent adhesion.
[0127] The current collector metal foil of test number 12 had an excessively high volume ratio of resin in the composite, resulting in a peel strength (relative value) of less than 1.50, indicating that the current collector metal foil did not have excellent adhesion.
[0128] The current collector metal foil of test number 13 had too high a volume ratio of resin in the composite and too much HSC, resulting in a peel strength (relative value) of less than 1.50 and thus not having excellent adhesion.
[0129] The metal foil for current collector of test number 14 had too little HSC, and as a result, the peel strength (relative value) of this metal foil for current collector was less than 1.50, and the metal foil did not have excellent adhesion.
[0130] The metal foil for current collector of test number 15 had too much HSC, and as a result, the peel strength (relative value) of this metal foil for current collector was less than 1.50, and the metal foil did not have excellent adhesion.
[0131] The current collector metal foil of test number 16 was unable to form and maintain a composite.
[0132] The current collector metal foil of test number 17 had an excessively low volume ratio of resin in the composite, resulting in a peel strength (relative value) of less than 1.50, indicating that the current collector metal foil did not have excellent adhesion.
[0133] The current collector metal foil of test number 18 did not contain Ni particles or a sintered body in the composite. Furthermore, the volume fraction of the resin in the composite was too low, resulting in a low HSC. As a result, the peel strength (relative value) of this current collector metal foil was less than 1.50, indicating that it did not have excellent adhesion.
[0134] The embodiments of the present disclosure have been described above. However, the above-described embodiments are merely examples for implementing the present disclosure. Therefore, the present disclosure is not limited to the above-described embodiments, and can be implemented by appropriately modifying the above-described embodiments within the scope of the present disclosure.
Claims
1. A metal foil for a current collector comprising: a substrate; and a plurality of composites held on a surface of the substrate, the plurality of composites including: Ni particles having an average particle size of 20 μm or less; a sintered body formed by sintering the Ni particles; and 14.0 to 40.0 volume % of resin, wherein the number of peaks on the surface of the metal foil for a current collector that are greater than 10 μm in height from the substrate surface, as determined by line roughness analysis, is 20.0 to 50.0 peaks / mm.
2. The metal foil for a current collector according to claim 1, wherein the average thickness of the substrate is 5 to 30 μm.
3. An electrode comprising: the metal foil for a current collector according to claim 1 or 2; and an electrode mixture layer formed on the surface of the metal foil for a current collector.
4. A battery comprising the electrode according to claim 3 and an electrolyte.
Citation Information
Patent Citations
Metal foil and its manufacturing method, secondary battery current collector, electrode for secondary battery, and nonaqueous secondary battery
JP2009026491A
Rolled copper foil for lithium battery collector
JP2011009207A
Collector for lithium ion cells and method for manufacturing it
JP2008171788A
Secondary battery current collector and secondary battery
JP2022175835A
Metal foil, metal foil production method, secondary battery negative electrode, and secondary battery positive electrode