Composite metal foil, metal-clad laminated board and circuit board
By using composite metal foil on the circuit board for semi-cured sheet compression process, a stable resistor layer is formed, which solves the problem of temperature control of small-volume circuit boards, realizes resistance stability and temperature monitoring accuracy, simplifies the processing technology and improves the Protection effect of components.
Patent Information
- Application Number
- CN202411177233.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-29
AI Technical Summary
The existing temperature control components and surface-mounted thermistors of existing electronic components are large in size, and the temperature control of small-volume circuit boards cannot be achieved. The embedded resistor is prone to failure during the production process, and the temperature of electronic components cannot be effectively monitored.
The composite metal foil is arranged in the circuit board through the semi-cured sheet pressing process to form a stable first resistance layer, with a resistance change rate of less than or equal to 20%, realizing the production of a temperature control circuit of a small volume circuit board for temperature monitoring of micro devices , avoid subsequent welding of the chip resistance.
It realizes the production of temperature-controlled circuits of small-volume circuit boards, has high resistance stability, can accurately monitor the temperature of components such as chips, streamlines the circuit board processing technology, extends the service life of composite metal foil, and improves working reliability.
Smart Images

Figure CN119049819A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of electronic technology, and in particular to a composite metal foil, a metal-clad laminate and a circuit board. Background Art
[0002] With the continuous advancement of the electronics industry and information technology, electronic components are developing towards high performance and miniaturization. Electronic components will generate heat during operation, and the increase in temperature will affect the normal operation of electronic components. Therefore, it is necessary to control the temperature of electronic components to keep them running normally.
[0003] At present, temperature control elements or surface mounted thermistors are usually set on the surface of electronic components. However, the temperature control elements and surface mounted thermistors are large in size and cannot realize the production of temperature control circuits of small-volume circuit boards. In addition, conventional embedded resistors are prone to failure during the circuit board production process, resulting in the inability of the resistors in the circuit to monitor the temperature of electronic components. Summary of the invention
[0004] The present invention provides a composite metal foil, a metal-clad laminate and a circuit board, so as to realize direct arrangement of the composite metal foil inside or on the surface of the circuit board, and to be used for manufacturing temperature control circuits of small-volume circuit boards, so as to realize temperature monitoring of tiny devices.
[0005] According to a first aspect of the present invention, there is provided a composite metal foil, comprising:
[0006] a first resistance layer;
[0007] After the composite metal foil is placed in the circuit board through N prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 20%; wherein N is an integer greater than or equal to 1.
[0008] Optionally, after the composite metal foil is placed in the circuit board through one prepreg lamination process, the resistance change rate of the first resistance layer is less than or equal to 10%.
[0009] Optionally, when the composite metal foil undergoes N prepreg lamination processes, after each prepreg lamination, the resistance change rate of the first resistance layer is less than or equal to 3%.
[0010] Optionally, after the composite metal foil is placed in the circuit board through N prepreg lamination processes, after the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the first resistance layer is less than or equal to 20%.
[0011] Optionally, after the composite metal foil is placed in the circuit board through N prepreg lamination processes, the temperature rises from 25° C. to 125° C. and then drops to 25° C. as one cycle, and after M cycles, the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the first resistance layer is less than or equal to 30%;
[0012] Wherein, M is an integer greater than or equal to 500.
[0013] Optionally, the first resistance layer includes at least one element of Ni, Cr, Zn, Si, Al, Fe, O, N, Cu and Mo.
[0014] Optionally, in the first resistance layer, a ratio of Fe content to Cr content is greater than or equal to 0.8 and less than or equal to 1.5.
[0015] And / or, in the first resistance layer, a ratio of Fe content to Ni content is greater than or equal to 0.8 and less than or equal to 1.8.
[0016] And / or, in the first resistance layer, a ratio of O content to Fe content is greater than or equal to 1.5 and less than or equal to 2.5.
[0017] Optionally, the Cr content in the first resistance layer is less than or equal to 20%, the Fe content is less than or equal to 30%, the Ni content is greater than or equal to 30%, and the O content is less than or equal to 60%.
[0018] Optionally, the composite metal foil further includes: a base layer stacked with the first resistance layer.
[0019] Optionally, the thickness of the base layer is greater than or equal to 2 microns and less than or equal to 100 microns.
[0020] Optionally, the thickness of the first resistance layer is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
[0021] Optionally, the composite metal foil further includes: a peeling layer and a carrier layer, wherein the peeling layer is arranged on a side of the base layer facing away from the first resistor layer, and the carrier layer is arranged on a side of the peeling layer facing away from the base layer, and the carrier layer can be peeled off from the base layer.
[0022] Optionally, the composite metal foil further comprises:
[0023] At least one of an absorption layer, a second resistance layer and an adjustment layer stacked with the base layer and the first resistance layer.
[0024] According to a second aspect of the present invention, there is provided a metal-clad laminate, the metal-clad laminate comprising the composite metal foil according to any embodiment of the present invention.
[0025] According to a third aspect of the present invention, a circuit board is provided. The circuit board comprises the composite metal foil according to any embodiment of the present invention, and the composite metal foil is arranged on the surface or inside of the circuit board.
[0026] After the composite metal foil of the present invention is placed in a circuit board through N times of prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 20%, that is, the composite metal foil of the embodiment of the present invention has a small resistance change within this change rate after the prepreg lamination process, and the resistance is stable. The composite metal foil can be directly placed inside or on the surface of the circuit board for direct circuit manufacturing. In addition, the composite metal foil of the present invention has a small volume and can be used for the manufacture of temperature control circuits of small-volume circuit boards to achieve temperature monitoring of tiny devices without the need for subsequent soldering of chip resistors, thereby streamlining the processing technology of the circuit board.
[0027] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 is a schematic diagram of a composite metal foil provided by an embodiment of the present invention;
[0030] Figure 2 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention;
[0031] Figure 3 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention;
[0032] Figure 4 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention;
[0033] Figure 5 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention;
[0034] Figure 6 is a schematic diagram of a circuit board provided by an embodiment of the present invention;
[0035] Figure 7 This is a schematic diagram of another circuit board provided by an embodiment of the present invention. DETAILED DESCRIPTION
[0036] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0037] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0038] An embodiment of the present invention provides a composite metal foil, comprising: a first resistance layer;
[0039] After the composite metal foil is placed in the circuit board through N prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 20%; wherein N is an integer greater than or equal to 1.
[0040] The resistance change rate of the first resistor layer is: the resistance change rate of the first resistor layer after N prepreg lamination processes relative to the resistance change rate of the first resistor layer before N prepreg lamination processes.
[0041] Composite metal foil can be made into thin film resistors, which are also called buried copper foil, embedded copper foil, thin film resistor copper foil, etc. In this embodiment, the first resistor layer has the properties of a thermistor. As the temperature rises, the resistance of the first resistor layer changes. As the temperature returns to the initial position, the resistance of the first resistor layer can return to near the original resistance value. The operating temperature of the components to be tested can be monitored in real time by detecting the resistance change of the first resistor layer. When the preset temperature is exceeded, other temperature control circuits can be used for timely protection, thereby protecting the components to be tested and preventing the electronic components from being burned out due to excessive temperature.
[0042] Each film layer in the circuit board needs to be pressed together by a prepreg, and the circuit board production process needs to go through one, two or more prepreg pressing processes. The maximum temperature during the prepreg pressing can reach 200°C, and the maximum pressure can reach 380PSI. Conventional embedded resistors are prone to failure after the prepreg pressing process, resulting in the inability of the resistors in the circuit to monitor the temperature of electronic components. In this embodiment, after the composite metal foil is set in the circuit board after one, two or more prepreg pressing processes, the resistance change rate of the first resistor layer is less than or equal to 20%, that is, after one, two or more prepreg pressing processes, the resistance value of the first resistor layer changes little, the resistance is stable, and the characteristics of the first resistor layer are not affected. Therefore, the composite metal foil of this embodiment can be directly set inside or on the surface of the circuit board for direct circuit production, and the temperature monitoring of components such as chips is subsequently realized. There is no need for subsequent soldering of chip resistors, which simplifies the processing technology of the circuit board, and the composite metal foil is small in size and can be used for the production of temperature control circuits of small-volume circuit boards to realize temperature monitoring of tiny devices.
[0043] On the basis of the above embodiment, further, after the composite metal foil is placed in the circuit board through a prepreg lamination process, the resistance change rate of the first resistor layer is less than or equal to 10%. After the first resistor layer is placed in the circuit board, the resistance change is smaller, the resistance is more stable, and the temperature of components such as chips can be monitored more accurately.
[0044] On the basis of the above embodiment, further, when the composite metal foil undergoes N prepreg lamination processes, after each prepreg lamination, the resistance change rate of the first resistance layer is less than or equal to 3%.
[0045] Among them, after each prepreg lamination, the resistance change rate of the first resistor layer is the change rate of the resistance of the first resistor layer after each prepreg lamination process relative to the resistance of the first resistor layer before the prepreg lamination process. After each prepreg lamination, the resistance change rate of the first resistor layer is less than or equal to 3%, indicating that each prepreg lamination process has little effect on the resistance of the first resistor layer, the resistance of the first resistor layer is more stable, and the temperature of components such as chips can be more accurately monitored.
[0046] Based on the above embodiment, optionally, after the composite metal foil is placed in the circuit board through N prepreg lamination processes, after the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the first resistance layer is less than or equal to 20%.
[0047] Wherein, after the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the first resistor layer = | the resistance value of the first resistor layer after the temperature rises from 25°C to 125°C and then drops to 25°C - the initial resistance value of the first resistor layer after being set in the circuit board through N prepreg lamination processes | / the initial resistance value of the first resistor layer after being set in the circuit board through N prepreg lamination processes. The initial resistance value after being set in the circuit board through N prepreg lamination processes is the resistance value of the first resistor layer at the initial temperature of 25°C when the temperature cycle is not performed after the first resistor layer is set in the circuit board.
[0048] After the composite metal foil is placed in the circuit board through N times of semi-cured sheet lamination process, the resistance of the first resistor layer 10 decreases linearly during the process of temperature rising from 25°C to 125°C, which can be a linear decrease or a curve decrease. During the process of temperature dropping from 125°C to 25°C, the resistance of the first resistor layer 10 increases linearly, and the resistance of the first resistor layer 10 can return to the vicinity of the initial resistance value, and the rate of change of the initial resistance value of the first resistor layer 10 is within 20%. In the state of use, after the temperature rises and then returns to room temperature, the resistance of the first resistor layer can return to the vicinity of the initial resistance value, so that the composite metal foil can be reused to achieve the temperature detection function, while also ensuring the service life of the composite metal foil, ensuring its working accuracy, and improving its working reliability.
[0049] On the basis of the above embodiment, optionally, after the composite metal foil is placed in the circuit board through N prepreg lamination processes, the temperature rises from 25° C. to 125° C. and then drops to 25° C. as one cycle, and after M cycles, the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the first resistance layer 10 is less than or equal to 30%;
[0050] Wherein, M is an integer greater than or equal to 500.
[0051] Specifically, after M cycles, when the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the first resistor layer = |resistance of the first resistor layer after M cycles - initial resistance of the first resistor layer after being set in the circuit board through N semi-cured sheet pressing processes | / initial resistance of the first resistor layer after being set in the circuit board through N semi-cured sheet pressing processes.
[0052] After more than 500 cycles, the resistance change rate of the first resistance layer 10 is within 30%, that is, after multiple cycles, the resistance value of the first resistance layer 10 can still be restored to near the initial resistance value, and the resistance value still changes steadily, thereby ensuring that the composite metal foil has a longer service life.
[0053] Based on the above embodiments, optionally, the first resistance layer includes at least one element of Ni, Cr, Zn, Si, Al, Fe, O, N, Cu and Mo.
[0054] The first resistor layer may include one element, two or more elements selected from Ni, Cr, Zn, Si, Al, Fe, O, N, Cu and Mo. Exemplarily, the material of the first resistor layer is an alloy such as nickel-chromium alloy or nickel-chromium-iron alloy. In addition, the first resistor layer may also include oxides or nitrides. By adjusting the ratio of different elements, the resistance of the first resistor layer 10 meets the performance of the above embodiment.
[0055] Optionally, the first resistance layer 10 may be formed on the first substrate layer by bonding, electroplating, chemical plating, physical vapor deposition, chemical vapor deposition or other forming methods.
[0056] Specifically, the first resistor layer 10 is formed by vacuum magnetron sputtering process. The target material element is sputtered onto the base layer, and the common electroplating method is not used, and the water washing and drying operation after electroplating is not required. The first resistor layer 10 is formed by vacuum sputtering process, so that the resistance of the first resistor layer 10 is more stable and more uniform, and the uniformity of square resistance is improved.
[0057] On the basis of the above embodiments, optionally, the first resistance layer includes Fe and O, or the first resistance layer includes Fe and Cr, or the first resistance layer includes Fe and Ni, or the first resistance layer includes Fe and N, or the first resistance layer includes Ni, Fe and O, or the first resistance layer includes Ni, Cr, Fe and O, or the first resistance layer includes Ni, Cr and N, or the first resistance layer includes Ni, Cr and O, or the first resistance layer includes Ni and O, or the first resistance layer includes Fe, Cu and O, or the first resistance layer includes Fe, Cr, Si and O, or the first resistance layer includes Fe, Mo and O, etc.
[0058] Specifically, by adjusting different elements in the first resistor layer, the basic resistance value of the first resistor layer is adjusted, the resistance change rate is adjusted after N semi-cured sheet pressing processes, and the resistance change rate is adjusted after multiple temperature cycles.
[0059] Based on the above embodiment, optionally, in the first resistor layer, the ratio of Fe content to Cr content is greater than or equal to 0.8 and less than or equal to 1.5, so as to ensure that the resistance change rate is small after N prepreg lamination processes and that the resistance change rate is small after multiple temperature cycles. Exemplarily, the ratio of Fe content to Cr content is 1 or 1.5.
[0060] Based on the above embodiment, optionally, in the first resistor layer, the ratio of Fe content to Ni content is greater than or equal to 0.8 and less than or equal to 1.8, so as to ensure that the resistance change rate is small after N prepreg lamination processes and achieve a small resistance change rate after multiple temperature cycles. Exemplarily, the ratio of Fe content to Ni content is 0.9 or 1.2, etc.
[0061] Based on the above embodiment, optionally, in the first resistor layer, the ratio of O content to Fe content is greater than or equal to 1.5 and less than or equal to 2.5, so as to ensure that the resistance change rate is small after N prepreg lamination processes and achieve a small resistance change rate after multiple temperature cycles. Exemplarily, the ratio of O content to Fe content is 2.3, 2 or 1.8, etc.
[0062] Based on the above embodiment, optionally, the Cr content in the first resistor layer is less than or equal to 20%, the Fe content is less than or equal to 30%, the Ni content is greater than or equal to 30%, and the O content is less than or equal to 60%, so as to ensure that the resistance change rate is small after N semi-cured sheet pressing processes, and to achieve a small resistance change rate after multiple temperature cycles.
[0063] Based on the above embodiment, optionally, Figure 1 is a schematic diagram of a composite metal foil provided by an embodiment of the present invention, with reference to Figure 1 , the composite metal foil also includes:
[0064] The base layer 20 is stacked on the first resistance layer 10 .
[0065] The base layer 20 supports and conducts electricity for the first resistor layer 10 , so that the first resistor layer 10 can spread on its surface and can be normally used to make circuits.
[0066] The material of the base layer 20 is a conductive material or a dielectric material, and the base layer can be a single-layer structure or a multi-layer structure. The conductive material includes but is not limited to at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold. Specifically, the base layer can be copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil or gold foil, or an alloy foil containing at least two of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold, or a composite foil composed of at least two of copper foil, aluminum foil, titanium foil, zinc foil, iron foil, nickel foil, chromium foil, cobalt foil, silver foil and gold foil. The dielectric material includes PET (Polyethylene Terephthalate), PP (Polypropylene), PS (Polystyrene), ABF (Acrylonitrile-Butadiene-Styrene Terpolymer, polyacrylamide / styrene / styrene sulfate terpolymer) film, BT resin, polyacrylic acid, polyurethane, polyimide, etc., which are not listed in detail here. Among them, BT resin is a thermosetting resin formed by adding bismaleimide (BMI) and triazine as the main resin components, and epoxy resin, polyphenylene ether resin (PPE) or allyl compounds as modified components. In the base layer 20 with a multi-layer structure, the materials of different layers can be the same or different.
[0067] Based on the above embodiment, optionally, the thickness of the base layer 20 is greater than or equal to 2 micrometers and less than or equal to 100 micrometers.
[0068] For example, the thickness of the base layer is 2.5 μm, 3 μm, 5 μm, 10 μm, 16 μm, etc. While the base layer 20 of such thickness ensures the supporting effect, when the base layer 20 is a copper layer, it can be used to directly etch the temperature measurement circuit to meet the circuit etching requirements.
[0069] Based on the above embodiment, optionally, the roughness of a side of the base layer 20 close to the first resistance layer 10 is greater than or equal to 0.5 micrometers and less than or equal to 10 micrometers.
[0070] Specifically, the roughness within the above range can further improve the bonding force between the base layer 20 and the first resistor layer 10, and because the first resistor layer 10 is relatively thin, often at the nanometer level, the roughness of the first resistor layer 10 replicates the roughness of the base layer 20, so that after the composite metal foil is set on the surface of the device to be tested, the bonding force between the first resistor layer 10 and the circuit board is relatively large, thereby improving the peeling resistance performance.
[0071] Based on the above embodiment, optionally, the thickness of the first resistance layer 10 is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
[0072] Specifically, if the thickness of the first resistor layer 10 is too large or too small, it will affect the resistance of the first resistor layer 10, thereby affecting the recovery accuracy of the resistance of the first resistor layer 10 and the accuracy of the monitoring circuit. Therefore, by setting the thickness of the first resistor layer 10 to be greater than or equal to 5 nanometers and less than or equal to 1 micron, the resistance of the first resistor layer 10 can be within a suitable range, so that the recovery accuracy of the resistance of the first resistor layer 10 and the accuracy of the monitoring circuit are both high, which can meet the requirements of monitoring the temperature of the component to be measured on the circuit board.
[0073] Figure 2 It is a schematic diagram of another composite metal foil provided by an embodiment of the present invention. On the basis of the above embodiment, optionally, the composite metal foil also includes: a peeling layer 60 and a carrier layer 70, the peeling layer 60 is arranged on the side of the base layer 20 facing away from the first resistance layer 10, and the carrier layer 70 is arranged on the side of the peeling layer 60 facing away from the base layer 20, and the carrier layer 70 can be peeled off from the base layer 20.
[0074] Specifically, the carrier layer 70 plays a supporting role, and the material used for the carrier layer 70 can be a conductive material or a dielectric material. The conductive material includes but is not limited to at least one of copper, aluminum, titanium, zinc, iron, nickel, chromium, cobalt, silver and gold. The peeling layer 60 can be made of organic material or inorganic material, and the peeling layer 60 plays the role of separating the base layer 20 and the carrier layer 70. When making the composite metal foil, the peeling layer 60 can be first made on the surface of the carrier layer 70, and then the base layer 20 can be made on the surface of the peeling layer 60, and then the first resistor layer 10 can be made on the surface of the base layer 20. When in use, after the first resistor layer 10 is pressed onto the circuit board, the carrier layer 70 is peeled off, and the first resistor layer 10 and the base layer 20 are left on the surface of the circuit board for making a temperature measurement circuit. Since the carrier layer 70 plays a supporting role, the base layer 20 can be set thinner, and the base layer 20 can be made of ultra-thin copper foil, and the first resistor layer 10 and the base layer 20 can be made into fine circuits.
[0075] Figure 3 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention, Figure 4 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention, Figure 5 FIG. 1 is a schematic diagram of another composite metal foil provided by an embodiment of the present invention. Figure 3-Figure 5 , the composite metal foil also includes:
[0076] At least one of the absorption layer 40 , the second resistance layer 50 , and the adjustment layer 30 stacked with the base layer 20 and the first resistance layer 10 .
[0077] Specifically, refer to Figure 3The absorption layer 40 can be disposed between the first resistance layer 10 and the base layer 20, or on the surface of the first resistance layer 10 away from the base layer 20, which is not limited in the embodiment of the present invention. The absorption layer 40 is used to absorb electromagnetic waves, and the material used in the absorption layer 40 includes polymer materials.
[0078] refer to Figure 4 The second resistance layer 50 can be located on the side of the first resistance layer 10 away from the base layer 20, or can be located between the first resistance layer 10 and the base layer 20. As the temperature changes, the resistance value of the second resistance layer 50 remains unchanged. The second resistance layer 50 is used to adjust the overall resistance of the composite metal foil, so that the basic resistance is larger, thereby improving the temperature measurement accuracy.
[0079] refer to Figure 5 The adjustment layer 30 can be arranged on the side of the first resistor layer 10 away from the base layer 20, and the side of the first resistor layer 10 away from the base layer 20 is pressed on the circuit board; the function of the adjustment layer 30 is to improve the bonding force between the composite metal foil and the circuit board to prevent the composite metal foil from falling off. The material of the adjustment layer 30 may include at least one of a silane coupling agent, an aluminate coupling agent, a metal composite coupling agent, a phosphate coupling agent, a borate coupling agent, polyethylene (PE), polypropylene (PP) and polyvinyl chloride (PVC).
[0080] An embodiment of the present invention further provides a metal-clad laminate, which includes the composite metal foil described in any embodiment of the present invention.
[0081] The metal-clad laminate according to the embodiment of the present invention has the same beneficial effects as the composite metal foil according to any embodiment of the present invention.
[0082] An embodiment of the present invention further provides a circuit board, Figure 6 is a schematic diagram of a circuit board provided by an embodiment of the present invention, Figure 7 is a schematic diagram of another circuit board provided by an embodiment of the present invention, with reference to Figure 7 and Figure 6 The circuit board includes the composite metal foil 100 described in any embodiment of the present invention, and the composite metal foil 100 is arranged on the surface or inside of the circuit board.
[0083] refer to Figure 6 The composite metal foil 100 is pressed into the circuit board 300 through the prepreg 200 and is arranged on the surface of the circuit board 300. Figure 7 The composite metal foil 100 is pressed into the circuit board 300 through two prepreg sheets 200 and is arranged inside the circuit board 300 .
[0084] The circuit board according to the embodiment of the present invention has the same beneficial effects as the composite metal foil according to any embodiment of the present invention.
[0085] Example 1
[0086] This embodiment provides a composite metal foil, including a base layer and a first resistor layer, the base layer is a copper layer, the first resistor layer includes nickel, chromium and iron, the Cr content in the first resistor layer is 15%, the Fe content is less than 25%, and the Ni content is 60%. The thickness of the first resistor layer is 50 nanometers, and the thickness of the base layer is 10 micrometers.
[0087] After the composite metal foil of this embodiment is pressed into the circuit board through three semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 8%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 5% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 500 cycles, the resistance change rate of the first resistor layer is 13% after the temperature rises from 25°C to 125°C and then drops to 25°C. After the composite metal foil of this embodiment is pressed through the semi-cured sheet pressing process, the resistance change is small and the resistance is stable; and during use, after the temperature rises and then returns to room temperature, the resistance of the first resistor layer can return to near the initial resistance value. The composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0088] Example 2
[0089] Different from the first embodiment, the first resistor layer in this embodiment includes nickel, chromium, iron and oxygen, and the Cr content in the first resistor layer is 15%, the Fe content is less than 25%, the Ni content is 35%, and the O content is 25%.
[0090] After the composite metal foil of this embodiment is pressed into the circuit board through three semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 7%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 4% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 800 cycles, the resistance change rate of the first resistor layer is 15% after the temperature rises from 25°C to 125°C and then drops to 25°C. After multiple semi-cured sheet pressing processes, the composite metal foil of this embodiment has a small resistance change and stable resistance; and after multiple temperature cycles during use, the resistance of the first resistor layer can return to near the initial resistance value. Therefore, the composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0091] Example 3
[0092] Different from the embodiment 2, the Cr content in the first resistor layer of the embodiment is 10%, the Fe content is less than 20%, the Ni content is 39%, and the O content is 31%.
[0093] After the composite metal foil of this embodiment is pressed into the circuit board through 5 semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 10%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 5% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 800 cycles, the resistance change rate of the first resistor layer is 14% after the temperature rises from 25°C to 125°C and then drops to 25°C. After multiple semi-cured sheet pressing processes, the composite metal foil of this embodiment has a small resistance change and stable resistance; and after multiple temperature cycles during use, the resistance of the first resistor layer can return to near the initial resistance value. Therefore, the composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0094] Example 4
[0095] Different from the embodiment 3, the Cr content in the first resistor layer of the embodiment is 18%, the Fe content is 18%, the Ni content is 31%, and the O content is 33%.
[0096] After the composite metal foil of this embodiment is pressed into the circuit board through four semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 9%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 5% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 800 cycles, the resistance change rate of the first resistor layer is 13% after the temperature rises from 25°C to 125°C and then drops to 25°C. After multiple semi-cured sheet pressing processes, the composite metal foil of this embodiment has a small resistance change and stable resistance; and after multiple temperature cycles during use, the resistance of the first resistor layer can return to near the initial resistance value. Therefore, the composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0097] Example 5
[0098] This embodiment provides a composite metal foil. Different from Embodiment 2, in this embodiment, the thickness of the first resistance layer is 100 nanometers, and the thickness of the base layer is 20 micrometers.
[0099] After the composite metal foil of this embodiment is pressed into the circuit board through three semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 8%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 6% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 800 cycles, the resistance change rate of the first resistor layer is 16% after the temperature rises from 25°C to 125°C and then drops to 25°C. After multiple semi-cured sheet pressing processes, the composite metal foil of this embodiment has a small resistance change and stable resistance; and after multiple temperature cycles during use, the resistance of the first resistor layer can return to near the initial resistance value. Therefore, the composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0100] Example 6
[0101] Different from the embodiment 2, the composite metal foil of the embodiment further includes an adjustment layer. The material of the adjustment layer is an aluminate coupling agent. The thickness of the adjustment layer is 5 micrometers.
[0102] After the composite metal foil of this embodiment is pressed into the circuit board through 5 semi-cured sheet pressing processes, the resistance change rate of the first resistor layer is 11%. After being pressed into the circuit board, the resistance change rate of the first resistor layer is 7% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 600 cycles, the resistance change rate of the first resistor layer is 13% after the temperature rises from 25°C to 125°C and then drops to 25°C. After multiple semi-cured sheet pressing processes, the composite metal foil of this embodiment has a small resistance change and a stable resistance; and after multiple temperature cycles during use, the resistance of the first resistor layer can return to near the initial resistance value. Therefore, the composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0103] Comparative Example 1
[0104] The metal foil includes a resistor layer and a base layer, wherein the base layer is made of Cu, the thickness of the base layer is 10 microns, the resistor layer is made of Ni-P alloy, and the thickness of the resistor layer is 100 nanometers. After being pressed into a circuit board through a semi-cured sheet pressing process once, the resistance change rate of the resistor layer is 50%. After being pressed into the circuit board, the resistance change rate of the resistor layer is 40% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 100 cycles, the resistance change rate of the first resistor layer is 300% after the temperature rises from 25°C to 125°C and then drops to 25°C. After the metal foil of comparative example 1 is subjected to the semi-cured sheet pressing process, the resistance change of the resistor layer is large, and after the temperature rises and returns to room temperature and after multiple temperature cycles, the resistance layer changes greatly, the resistor layer fails, and the temperature of the electronic components cannot be monitored.
[0105] Comparative Example 2
[0106] Unlike Comparative Example 1, the thickness of the resistor layer is 2.5 microns. After being pressed into the circuit board through three semi-cured sheet pressing processes, the resistance change rate of the resistor layer is 60%. After being pressed into the circuit board, the resistance change rate of the resistor layer is 70% after the temperature rises from 25°C to 125°C and then drops to 25°C. After 200 cycles, the resistance change rate of the first resistor layer is 350% after the temperature rises from 25°C to 125°C and then drops to 25°C. After the metal foil of Comparative Example 2 is subjected to the semi-cured sheet pressing process, the resistance of the resistor layer changes greatly, and after the temperature rises and returns to room temperature and after multiple temperature cycles, the resistance layer changes greatly, the resistor layer fails, and the temperature of the electronic components cannot be monitored.
[0107] Combining Examples 1 to 6 and Comparative Examples 1 and 2, it can be seen that:
[0108] In the composite metal foil of this embodiment, the first resistor layer uses Ni, Cr and Fe or Ni, Cr, Fe and O, and the Cr content in the first resistor layer is less than 20%, the Fe content is less than 30%, the Ni content is greater than 30%, and the O content is less than 60%. When the thickness of the first resistor layer is greater than or equal to 5 nanometers and less than or equal to 1 micron, after 3-5 prepreg lamination processes, the resistance change rate of the first resistor layer is less than or equal to 11%, and after the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the first resistor layer is less than or equal to 7%, and after 500-800 temperature cycles, the resistance change rate of the first resistor layer is less than or equal to 16%.
[0109] The material of the resistance layer in the comparative example is Ni-P alloy, and the thickness of the resistance layer is 100 nanometers to 2.5 micrometers. After the metal foil in the comparative example is pressed into the circuit board through 1-3 prepreg pressing processes, the resistance change rate of the resistance layer is greater than or equal to 50%. After the temperature rises from 25°C to 125°C and then drops to 25°C, the resistance change rate of the resistance layer is greater than or equal to 40%. After 100-200 temperature cycles, the resistance change rate of the first resistance layer is greater than or equal to 200%.
[0110] It can be seen that the resistance layer of the metal foil in the comparative example fails after the circuit board manufacturing process, and it cannot meet the temperature cycle requirements and cannot perform temperature monitoring. The composite metal foil of the present application is pressed into the circuit board through a limited semi-cured sheet pressing process, and the change rate of the resistance of the first resistance layer is stable, which can meet the stability of the properties of the resistance layer. And after multiple temperature cycles, the resistance of the first resistance layer can be restored to near the initial resistance value, meeting the recovery accuracy of the thermistor, thereby ensuring the temperature monitoring effect. The composite metal foil of this embodiment can be set in the circuit board for temperature monitoring, and can be reused, with a long service life, high working accuracy and reliability.
[0111] It should be understood that the various forms of processes shown above can be used to reorder, add or delete steps. For example, the steps described in the present invention can be executed in parallel, sequentially or in different orders, as long as the desired results of the technical solution of the present invention can be achieved, and this document does not limit this.
[0112] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite metal foil, characterized in that: include: a first resistance layer; After the composite metal foil is placed in the circuit board through N prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 20%; wherein N is an integer greater than or equal to 1.
2. The composite metal foil according to claim 1, characterized in that: After the composite metal foil is placed in the circuit board through one prepreg lamination process, the resistance change rate of the first resistance layer is less than or equal to 10%.
3. The composite metal foil according to claim 1, characterized in that: When the composite metal foil is subjected to N prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 3% before and after each prepreg lamination.
4. The composite metal foil according to claim 1, characterized in that: After the composite metal foil is placed in the circuit board through N prepreg lamination processes, the resistance change rate of the first resistance layer is less than or equal to 20% after the temperature rises from 25° C. to 125° C. and then drops to 25° C.
5. The composite metal foil according to claim 1, characterized in that: After the composite metal foil is placed in the circuit board through N prepreg lamination processes, the temperature rises from 25° C. to 125° C. and then drops to 25° C. for one cycle, and after M cycles, the temperature rises from 25° C. to 125° C. and then drops to 25° C., the resistance change rate of the first resistance layer is less than or equal to 30%; Wherein, M is an integer greater than or equal to 500.
6. The composite metal foil according to any one of claims 1 to 5, characterized in that: The first resistance layer includes at least one element of Ni, Cr, Zn, Si, Al, Fe, O, N, Cu and Mo.
7. The composite metal foil according to claim 6, characterized in that: In the first resistor layer, a ratio of Fe content to Cr content is greater than or equal to 0.8 and less than or equal to 1.5; And / or, in the first resistance layer, the ratio of Fe content to Ni content is greater than or equal to 0.8 and less than or equal to 1.8; And / or, in the first resistance layer, a ratio of O content to Fe content is greater than or equal to 1.5 and less than or equal to 2.
5.
8. The composite metal foil according to claim 7, characterized in that: The Cr content in the first resistance layer is less than or equal to 20%, the Fe content is less than or equal to 30%, the Ni content is greater than or equal to 30%, and the O content is less than or equal to 60%.
9. The composite metal foil according to claim 1, characterized in that: Also includes: A base layer stacked with the first resistor layer; Preferably, the thickness of the base layer is greater than or equal to 2 microns and less than or equal to 100 microns; Preferably, the thickness of the first resistance layer is greater than or equal to 5 nanometers and less than or equal to 1 micrometer.
10. The composite metal foil according to claim 9, characterized in that: Also includes: A peeling layer and a carrier layer, wherein the peeling layer is arranged on a side of the base layer facing away from the first resistor layer, and the carrier layer is arranged on a side of the peeling layer facing away from the base layer, and the carrier layer can be peeled off from the base layer.
11. The composite metal foil according to claim 9, characterized in that: Also includes: At least one of an absorption layer, a second resistance layer and an adjustment layer stacked with the base layer and the first resistance layer.
12. A metal-clad laminate, characterized in that: The metal-clad laminate comprises the composite metal foil according to any one of claims 1 to 11.
13. A circuit board, characterized in that: The circuit board comprises the composite metal foil according to any one of claims 1 to 11, and the composite metal foil is arranged on the surface or inside of the circuit board.
Citation Information
Cited By
Composite metal foil, metal-clad laminated board and circuit board
CN119724779A
Composite metal foil and circuit board
CN119889845A