Interlayer film for laminated glass, and laminated glass
The interlayer film with a nano-laminated reflective layer and filler-containing layers addresses the lack of design enhancement in conventional laminated glass by creating a significant color difference when viewed from different angles, enhancing the aesthetic appeal of laminated glass.
Patent Information
- Application Number
- PCT/JP2024/012513
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-31
- Filing Date
- 2024-03-27
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional interlayer films for laminated glass lack sufficient design enhancement capabilities, as they only color the window glass and fail to provide diverse expressions for vehicles and buildings.
An interlayer film with a reflective layer having a nano-laminated structure, comprising two resin layers with different refractive indexes and a filler-containing layer, which creates a significant color difference when viewed from different angles, enhancing the design by providing a metallic feel and unique visual effects.
The interlayer film achieves a substantial color difference (ΔE*ab) of 0.5 or more, allowing for distinct designs when viewed from different sides, thereby improving the aesthetic appeal and design quality of laminated glass.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002 
Figure 00000078_0000
Abstract
Description
Interlayer film for laminated glass, and laminated glass
[0001] The present invention relates to an interlayer film for laminated glass and laminated glass having the interlayer film for laminated glass.
[0002] Laminated glass is safe because it shatters little if it is broken by an external impact, and is therefore widely used as window glass for various vehicles such as automobiles and for windows in buildings, etc. A widely known type of laminated glass is one in which a pair of panes of glass are integrated together by sandwiching an interlayer film for laminated glass containing a resin component such as a polyvinyl acetal resin between them.
[0003] It has been known that laminated glass contains a reflective film for the purpose of imparting various functions. For example, Patent Document 1 discloses that a reflective film having a visible light selective reflection layer and an infrared light selective reflection layer is incorporated between a pair of panes of laminated glass. Here, it is disclosed that the visible light selective reflection layer has a reflection peak in the range of 380 to 850 nm and a natural light reflectance of 5 to 25% at the reflection peak wavelength, thereby reflecting a certain amount of light from a head-up display light source while maintaining high transmittance, thereby improving the projection performance of HUD images. It is also disclosed that the infrared light selective reflection layer has a reflection peak in the range of 900 to 1200 nm and a natural light reflectance of 26% or more at the reflection peak wavelength, thereby facilitating driver face and iris authentication using infrared light.
[0004] Furthermore, in recent years, interlayer films for laminated glass have often been required to have a design feature, and therefore, they are sometimes colored by incorporating a colorant. It is also known that interlayer films for laminated glass are blended with metal-based particles for coloring purposes. For example, Patent Document 2 discloses that a metal-based pigment is blended into an interlayer film for laminated glass, which comprises polyvinyl butyral and a plasticizer, for coloring purposes. Patent Document 2 also discloses that the resin composition of the interlayer film for laminated glass containing the metal-based pigment may further contain a coloring material such as a pigment or dye.
[0005] International Publication No. WO 2022 / 075184 International Publication No. WO 2016 / 028963
[0006] However, in recent years, the designs of window glass for automobiles and buildings have become increasingly diverse, and for example, various expressions are sometimes desired even in automobiles. However, conventional interlayer films for laminated glass containing pigments or dyes only color the window glass and are unable to sufficiently enhance the design.
[0007] Therefore, an object of the present invention is to provide an interlayer film for laminated glass that has excellent design properties.
[0008] As a result of extensive research, the present inventors have discovered that by setting the color difference ΔE*ab between reflected light from light incident from one direction and reflected light from the opposite direction in an interlayer film for laminated glass to a certain value or more, it is possible to make the design when viewed from one side of the laminated glass including the interlayer film different from the design when viewed from the other side. That is, the present invention provides the following [1] to
[26] . [1] An interlayer film for laminated glass, in which the color difference ΔE*ab(R) between reflected light from light incident from one direction in the L*a*b* color space and reflected light from light incident from the opposite direction in the L*a*b* color space is 0.5 or more. [2] The interlayer film for laminated glass according to [1] above, which comprises a reflective layer. [3] The interlayer film for laminated glass according to [2] above, in which the reflective layer is a nano-laminate film. [4] The interlayer film for laminated glass according to [3] above, wherein the reflective layer includes two resin layers A and B having different refractive indices, and 30 or more of these layers are laminated together. [5] The interlayer film for laminated glass according to [4] above, wherein the thickness of the resin layer A is 30 nm or more and 500 nm or less, and the thickness of the resin layer B is 30 nm or more and 500 nm or less. [6] The interlayer film for laminated glass according to [4] or [5] above, wherein the difference in refractive index between the resin layer A and the resin layer B is 0.01 or more and 0.15 or less. [7] The interlayer film for laminated glass according to any of [2] to [6] above, wherein the reflective layer has an average reflectance of 25.0% or more in a wavelength range of 380 to 780 nm. [8] The interlayer film for laminated glass according to any of [2] to [7] above, wherein the reflective layer has a non-uniform hue within its plane. [9] The interlayer film for laminated glass according to any one of [2] to [8] above, which includes one or more first resin layers disposed on one surface of the interlayer film closer to the reflective layer.
[10] The interlayer film for laminated glass according to [9] above, wherein the one or more first resin layers have at least a colored layer containing a colorant.
[11] The interlayer film for laminated glass according to
[10] above, wherein the colorant contains a pigment, and the pigment contains one or more pigments selected from the group consisting of carbon black, quinacridone pigments, copper phthalocyanine pigments, nickel complex azo pigments, isoindolinone pigments, and perylene pigments.
[12] The interlayer film for laminated glass according to any one of [2] to
[11] above, which includes one or more second resin layers arranged on the other surface side of the interlayer film relative to the reflective layer.
[13] The interlayer film for laminated glass according to
[12] above, wherein the second resin layer contains a filler (A) having at least one of a non-metallic material and a metal oxide.
[14] The interlayer film for laminated glass according to
[13] above, wherein the filler (A) contains two or more types of metal oxides.
[15] The interlayer film for laminated glass according to
[14] above, wherein the two or more types of metal oxides have mutually different refractive indices.
[16] The interlayer film for laminated glass according to any one of
[13] to
[15] above, wherein the filler (A) has a flat plate shape.
[17] The interlayer film for laminated glass according to any one of
[13] to
[16] above, wherein the filler (A) has a multilayer structure.
[18] The interlayer film for laminated glass according to any one of
[13] to
[17] above, wherein the aspect ratio of the filler (A) is 1 or more and 50 or less.
[19] The interlayer film for laminated glass according to any one of [2] to
[18] above, comprising: one or more first resin layers disposed on one side of the interlayer film closer to the reflective layer; and one or more second resin layers disposed on the other side of the interlayer film closer to the reflective layer, wherein the color difference ΔE*ab(S) between visible light transmitted through the first resin layer and visible light transmitted through the second resin layer in the L*a*b* color system is greater than 0 and less than 100.
[20] The interlayer film for laminated glass according to any one of [1] to
[19] above, wherein the color difference E*ab(R) is 2.0 or more.
[21] The interlayer film for laminated glass according to any one of [1] to
[20] above, wherein the color difference E*ab(R) is 15 or more.
[22] The interlayer film for laminated glass according to any one of [1] to
[21] above, wherein the color difference E*ab(R) is 30 or more.
[23] Laminated glass comprising: a first laminated glass member; a second laminated glass member; and the interlayer film for laminated glass according to any one of [1] to
[22] above, wherein the interlayer film for laminated glass is disposed between the first laminated glass member and the second laminated glass member.
[24] Laminated glass, wherein the color difference ΔE*ab(Rg) between the L*a*b* color space of reflected light of light incident from one direction and the L*a*b* color space of reflected light of light incident from the opposite direction is 0.5 or more.
[25] The laminated glass according to the above
[24] , comprising a first laminated glass member, a second laminated glass member, and an interlayer film for laminated glass, the interlayer film for laminated glass being disposed between the first laminated glass member and the second laminated glass member, the interlayer film for laminated glass comprising a reflective layer, and the reflective layer having an average reflectance of 25.0% or more in a wavelength range of 380 to 780 nm.
[26] The laminated glass according to any of the above
[23] to
[25] , comprising a first member, a reflective layer, and a second member, the first member comprising a first laminated glass member and one or more first resin layers, the second member comprising a second laminated glass member and one or more second resin layers, the first laminated glass member, the first resin layer, the reflective layer, the second resin layer, and the second laminated glass member being disposed in this order, and the first member and the second member having different colors.
[0009] According to the present invention, it is possible to provide an interlayer film for laminated glass that has excellent design properties by making it possible to make the design when viewed from one side of the laminated glass having the interlayer film different from the design when viewed from the other side.
[0010] FIG. 1 is a schematic cross-sectional view showing a flat-plate-shaped filler (A) having a laminated structure. FIG. 2 is a schematic cross-sectional view showing an example of laminated glass. FIG. 3 is a schematic cross-sectional view showing an example of laminated glass. FIG. 4 is a schematic cross-sectional view showing an example of laminated glass. FIG. 5 is a schematic cross-sectional view showing an example of laminated glass. FIG. 6 is a schematic cross-sectional view showing an example of laminated glass. FIG. 7 is a schematic cross-sectional view showing an example of laminated glass. FIG. 8 is a schematic cross-sectional view showing an example of laminated glass. FIG. 9 is a schematic cross-sectional view showing an example of laminated glass. FIG. 10 is a schematic cross-sectional view showing an example of laminated glass. FIG. 11 is a schematic cross-sectional view showing an example of laminated glass. FIG. 12 is a schematic cross-sectional view showing an example of laminated glass.
[0011] The present invention will be described in more detail below. <Interlayer Film for Laminated Glass> The interlayer film for laminated glass of the present invention (hereinafter sometimes simply referred to as "interlayer film") has a color difference ΔE*ab (hereinafter sometimes referred to as ΔE*ab(R)) between the L*a*b* color space of reflected light of light incident from one direction and the L*a*b* color space of reflected light of light incident from the opposite direction of 0.5 or more. In the present invention, since the color difference ΔE*ab(R) of reflected light is 0.5 or more, the design when viewed from one side of laminated glass having the interlayer film of the present invention can be made different from the design when viewed from the other side, thereby imparting high designability to the laminated glass.
[0012] From the viewpoint of enhancing designability, the color difference ΔE*ab(R) of the reflected light is preferably 2.0 or more, more preferably 15 or more, and even more preferably 30 or more. Furthermore, from the viewpoint of ease of realization and preventing the design viewed from one side from differing too greatly from the design viewed from the other side, the color difference ΔE*ab(R) of the reflected light is preferably 100 or less, more preferably 75 or less, and even more preferably 50 or less. As described below, the color difference ΔE*ab(R) of the reflected light can also be increased by providing a reflective layer in the interlayer film or by providing a colored layer as the first resin layer in addition to the reflective layer. Furthermore, the color difference ΔE*ab(R) of the reflected light can also be increased by providing a filler-containing layer containing a specific filler (A) as the second resin layer in the interlayer film. Furthermore, the color difference ΔE*ab(R) of the reflected light can also be increased by increasing the color difference ΔE*ab(S) between the visible light transmitted through the first resin layer and the visible light transmitted through the second resin layer, as described below.
[0013] In the present invention, the above-mentioned reflected light color difference ΔE*ab(R) is a value obtained by measuring a laminated glass prepared by bonding two reference clear glass sheets together via an interlayer film. Specifically, light is incident on one side (i.e., one direction) of the prepared laminated glass, and the L*a*b* color space of the reflected light of the light is determined. Light is also incident on the other side (i.e., the opposite direction) of the laminated glass, and the L*a*b* color space of the reflected light of the light is determined. The color difference is then calculated from the obtained L*, a*, and b* values, and this calculated color difference is the color difference ΔE*ab(R) of the reflected light of the interlayer film. The reference clear glass sheet has a thickness of 2.5 mm and a visible light transmittance of 90.5% measured in accordance with JIS R 3106:1998. The clear glass plate has a*=-0.6, b*=0.2, and a haze of 0.2% or less, as obtained using CIE standard illuminant D65 and a 10° visual field color matching function specified in JIS Z 8781-1 (2012), JIS Z 8781-2 (2012), and JIS Z 8781-4 (2013).
[0014] [Reflective Layer] The interlayer film in the present invention preferably includes a reflective layer. The reflective layer is preferably a layer capable of reflecting visible light. By reflecting visible light, the reflective layer can, when used in combination with the first resin layer and the second resin layer described below, make it possible to make the color difference ΔE*ab(R) of the reflected light at a certain level or more.
[0015] As described above, from the viewpoint of easily achieving a color difference ΔE*ab(R) of a certain value or more, the reflective layer preferably has an average reflectance in the visible light region of a certain value or more. Specifically, the reflective layer preferably has an average reflectance in the wavelength range of 380 to 780 nm of 25.0% or more, preferably 30.0% or more, and more preferably 35.0% or more. Furthermore, from the viewpoint of ensuring a certain level of transparency in the interlayer film, the reflective layer preferably has an average reflectance in the visible light region of a certain value or less. Specifically, the reflective layer preferably has an average reflectance in the wavelength range of 380 to 780 nm of 70.0% or less, preferably 60.0% or less, and more preferably 55.0% or less.
[0016] The reflective layer preferably reflects light in the infrared region in addition to the visible light region, but may not reflect light in the infrared region. The reflective layer can improve the heat-shielding performance of the interlayer film by reflecting light in the infrared region. The reflective layer preferably has an average reflectance in the wavelength range of 380 to 2500 nm of 15.0% or more, more preferably 17.0% or more, and even more preferably 21.0% or more, and preferably 55.0% or less, preferably 40.0% or less, and even more preferably 30.0% or less.
[0017] The reflective layer preferably has a higher average reflectance in the visible light region than in the infrared light region. Specifically, the average reflectance in the wavelength range of 380 to 780 nm is preferably higher than the average reflectance in the wavelength range of 780 to 2500 nm. Increasing the average reflectance in the visible light region in this way facilitates increasing the color difference ΔE*ab(R) of the reflected light described above without complicating the structure of the reflective layer or increasing the thickness of the reflective layer more than necessary. From the above perspectives, the average reflectance in the wavelength range of 380 to 780 nm is higher than the average reflectance in the wavelength range of 780 to 2500 nm, and the difference therebetween is preferably 5% or more, more preferably 12% or more, and even more preferably 18% or more. The upper limit of the difference in average reflectance is not particularly limited, but is, for example, 50%, preferably 45%, and more preferably 38%. Specifically, the average reflectance in the wavelength range of 780 to 2500 nm may be 0% or more, but from the viewpoint of practicality and ensuring a certain level of heat shielding properties, it is preferably 3.0% or more, more preferably 5% or more, and even more preferably 10% or more. Also, from the viewpoint of simplifying the structure of the reflective layer, it is preferably 40% or less, preferably 30% or less, and even more preferably 20% or less.
[0018] Furthermore, it is preferable that the reflective layer has a non-uniform hue within the plane. Such a characteristic of the reflective layer makes it easier to achieve a metallic appearance, further enhancing the design. The phrase "having a non-uniform hue within the plane" means that the reflection intensity varies depending on the angle at which sunlight or simulated sunlight is irradiated onto the reflective layer, making the color appear different. A reflective layer having the above characteristics can be achieved, for example, by using a nano-laminate film, as described below. Here, "appearing to be a different color" means that the color of the reflected light observed when the angle at which simulated sunlight is irradiated varies by a color difference (ΔE) of 1.2 or more.
[0019] The reflective layer is not particularly limited, and examples include known reflective films such as nano-laminate films and resin films (e.g., PET films) sputtered with thin metal films. Among these, nano-laminate films are preferred. By using a nano-laminate film, the reflectance in the desired wavelength range can be easily increased by appropriately adjusting the in-plane refractive index difference between resin layer A and resin layer B, the number of layers, and layer thickness, as described below. Therefore, by appropriately adjusting the wavelength range in which the reflectance is increased, the color difference ΔE*ab(R) of the reflected light can also be easily increased. Furthermore, the use of a nano-laminate film makes it easier to impart a metallic feel and improve the design.
[0020] The nano-laminate film preferably includes two resin layers A and B with different refractive indices, and these layers are laminated in 30 or more layers. The resin layers A and B are preferably laminated alternately, and the thickness of each resin layer A is preferably 30 nm to 500 nm, and the thickness of each resin layer B is preferably 30 nm to 500 nm. The thickness of the resin layer A is more preferably 50 nm to 500 nm, and even more preferably 100 nm to 400 nm. The thickness of the resin layer B is more preferably 50 nm to 500 nm, and even more preferably 100 nm to 400 nm.
[0021] Furthermore, the total number of layers of the nano-laminate film may be 30 or more as described above, but is preferably 50 or more, more preferably 200 or more, even more preferably 400 or more, and particularly preferably 600 or more. By increasing the total number of layers, it is possible to easily increase the reflectance in the visible light region and also to easily impart a high-brightness metallic feel. The total number of layers is not particularly limited in terms of upper limit, but is preferably 1500 or less in order to prevent the manufacturing equipment from becoming too large and to prevent a decrease in lamination accuracy and a decrease in wavelength selectivity.
[0022] In the nano-laminate film, the refractive index of the resin layer A is preferably relatively higher than the refractive index of the resin layer B, and the difference between the refractive index of the resin layer A and the refractive index of the resin layer B is preferably 0.01 or more. By making the refractive index difference 0.01 or more, sufficient reflectivity is easily obtained. Furthermore, the difference between the refractive index of the resin layer A and the refractive index of the resin layer B is preferably 0.15 or less. Note that the refractive index here refers to the in-plane average refractive index, which is the average value of the refractive index in a direction parallel to the plane direction of the film. For example, it can be determined by the average value of the refractive index in two mutually perpendicular directions (if the MD and TD of the film are known, the average value of the refractive index in the MD and TD). Furthermore, it is preferable that the difference between the in-plane average refractive index of the resin layer A and the thickness direction refractive index is 0.01 or more, and the difference between the in-plane average refractive index of the resin layer B and the thickness direction refractive index is 0.01 or less. This is more preferable because even if the angle of incidence increases, the reflectance in the reflection band is less likely to decrease.
[0023] It is preferable that resin a constituting resin layer A and resin b constituting resin layer B are resins each containing the same basic skeleton. Here, the basic skeleton refers to the repeating units constituting resin a and resin b. For example, if one resin is polyethylene terephthalate, the basic skeleton is ethylene terephthalate. As another example, if one resin is polyethylene, the basic skeleton is ethylene. Resins a and b containing the same basic skeleton are preferable because they further reduce the likelihood of peeling between the layers. A preferred combination of resin a and resin b is one in which the difference in glass transition temperature between resin a and resin b is 20°C or less. A glass transition temperature difference of 20°C or less improves thickness uniformity when forming the nano-laminate film, making it less likely to cause appearance defects such as color unevenness. In addition, overstretching and other problems can be prevented when forming the nano-laminate film.
[0024] The resin constituting the nano-laminate film is preferably a polyester resin, and therefore, it is preferable that both resin a and resin b are polyester resins. Furthermore, it is more preferable to use at least polyethylene terephthalate as the resin constituting the nano-laminate film. Therefore, it is more preferable that resin a and resin b contain ethylene terephthalate as the basic skeleton. Furthermore, it is preferable that resin a is polyethylene terephthalate, and resin b is a polyester copolymerized with at least one of spiroglycol, cyclohexanedimethanol, and cyclohexanedicarboxylic acid. It is also preferable that resin a is polyethylene terephthalate, and resin b is a polyester copolymerized with neopentyl glycol.
[0025] A preferred example of a combination of resin a and resin b is a combination in which resin a is polyethylene terephthalate or polyethylene naphthalate and resin b is a polyester containing spiroglycol. Here, polyester containing spiroglycol refers to a polyester copolymerized with spiroglycol or a polyester blended with another homopolyester. Because the polyester containing spiroglycol has a small difference in glass transition temperature from polyethylene terephthalate or polyethylene naphthalate, it is less likely to be overstretched during molding and less likely to undergo delamination.
[0026] A more preferred example of a combination of resin a and resin b is a combination in which resin a is polyethylene terephthalate or polyethylene naphthalate, and resin b is a polyester containing spiroglycol and cyclohexanedicarboxylic acid. Here, "polyester containing spiroglycol and cyclohexanedicarboxylic acid" refers to a polyester copolymerized with spiroglycol and cyclohexanedicarboxylic acid (or an ester derivative of cyclohexanedicarboxylic acid), or a polyester blended with another homopolyester. When resin b is a polyester containing spiroglycol and cyclohexanedicarboxylic acid, the difference in in-plane refractive index between resin b and polyethylene terephthalate or polyethylene naphthalate is large, making it easier to achieve high reflectance. Furthermore, the small difference in glass transition temperature between resin b and polyethylene terephthalate or polyethylene naphthalate makes it less likely to be overstretched during molding, and less likely to cause delamination.
[0027] Another preferred example of a combination of resin a and resin b is a combination in which resin a is polyethylene terephthalate or polyethylene naphthalate and resin b is a polyester containing cyclohexanedimethanol. Here, polyester containing cyclohexanedimethanol refers to a polyester copolymerized with cyclohexanedimethanol or a polyester blended with another homopolyester. Polyester containing cyclohexanedimethanol has a small difference in glass transition temperature from polyethylene terephthalate or polyethylene naphthalate, making it less susceptible to overstretching during molding and less susceptible to delamination. Another preferred example of a combination of resin a and resin b is a combination in which resin a is polyethylene terephthalate or polyethylene naphthalate and resin b is a polyester containing neopentyl glycol. Here, polyester containing neopentyl glycol refers to a polyester copolymerized with neopentyl glycol or a polyester blended with another homopolyester.
[0028] More preferably, resin b is an ethylene terephthalate polycondensate in which the copolymerization amount of cyclohexanedimethanol is 15 mol% or more and 60 mol% or less. This results in high reflectivity, minimal change in optical properties, particularly due to heating or aging, and little interlayer delamination. An ethylene terephthalate polycondensate in which the copolymerization amount of cyclohexanedimethanol is 15 mol% or more and 60 mol% or less adheres very strongly to polyethylene terephthalate. Furthermore, the cyclohexanedimethanol group has geometric isomers, either cis or trans, and conformational isomers, either chair or boat. Therefore, even when co-stretched with polyethylene terephthalate, it is less likely to undergo orientation crystallization, has high reflectivity, shows even less change in optical properties due to thermal history, and is less likely to break during film formation. Another preferred resin b is an ethylene terephthalate polycondensate in which the copolymerization amount of neopentyl glycol is 15 mol% or more and 60 mol% or less.
[0029] The nano-laminate film of the present invention has a structure in which resin layers A and B are alternately laminated in the thickness direction, and this alternating laminate structure may include a third layer (resin layer C) other than resin layers A and B. Examples include laminate structures with regular permutations such as A(BCA)n, A(BCBA)n, and A(BABCBA)n. Here, n is the number of repeating units, and for example, when n = 3 in A(BCA)n, it represents a structure laminated in the thickness direction in the permutation ABCABCABCA.
[0030] The manufacturing method of the above-mentioned nano-laminate film is described in, for example, JP 2004-249587 A, JP 2005-59332 A, JP 2007-301982 A, JP 2009-78421 A, JP 2010-184493 A, JP 2015-110276 A, etc., and can be manufactured by referring to these patent publications. In addition, the nano-laminate film used in the present invention is generally commercially available and can be obtained. For example, "PICASUS" (registered trademark) manufactured by Toray Industries, Inc. and the "MLF Film" series manufactured by Teijin DuPont Films Co., Ltd. can be mentioned.
[0031] The thickness of the reflective layer is, for example, 20 μm or more and 300 μm or less, preferably 30 μm or more and 250 μm or less, and more preferably 50 μm or more and 200 μm or less. When the reflective layer is 20 μm or more, it sufficiently reflects visible light and makes it easy to increase the color difference ΔE*ab(R) of the reflected light. Furthermore, when the thickness is 300 μm or less, it is possible to prevent the reflective layer from becoming thicker than necessary and adjust the thickness of the interlayer to an appropriate value.
[0032] [First Resin Layer] The interlayer film of the present invention preferably includes one or more first resin layers in addition to the reflective layer. The first resin layer is a resin layer that is disposed on one side of the interlayer film closer to the reflective layer. The first resin layer may be a single layer or multiple layers. In the following description, one side of the interlayer film (i.e., the side facing the first resin layer) will be the indoor side (i.e., the interior side in an automobile) when used as laminated glass. Therefore, the other side of the interlayer film (i.e., the side facing the second resin layer when a second resin layer described below is provided) will be the outdoor side (i.e., the exterior side in an automobile) when used as laminated glass.
[0033] (Colored Layer) The first resin layer preferably includes a colored layer containing a colorant. Therefore, when the first resin layer is a single layer, it is sufficient that the single resin layer is a colored layer. When the first resin layer has multiple layers, it is sufficient that at least one of the multiple first resin layers is a colored layer. In the first resin layer, it is sufficient that the colorant is dispersed in the resin constituting the first resin layer.
[0034] The first resin layer includes a colored layer, which allows the interlayer film to be colored in a desired color, thereby enhancing its design. Furthermore, the colorant can absorb a portion of sunlight, thereby improving its heat-shielding properties. Furthermore, the first resin layer includes a colored layer, which absorbs incident light and light reflected by the reflective layer. This sufficiently changes the L*, a*, and b* of light incident from one side of the interlayer film and its reflected light, thereby increasing the color difference ΔE*ab(R) of the reflected light. Therefore, the hue of the interlayer film is likely to change when viewed from one side compared to the other side. For example, the metallic effect can be enhanced when viewed from the other side, while being reduced when viewed from the one side, thereby further enhancing its design. As mentioned above, if the appearance has a strong metallic feel when viewed from the other side and a weak metallic feel when viewed from one side, the exterior can be made to have an impact when viewed from the other side (i.e., outdoors), while the interior can have a subdued impression when viewed from one side (i.e., indoors), thereby enhancing the design.
[0035] As the colorant, pigments and dyes that are conventionally incorporated into interlayer films for laminated glass can be used. Furthermore, pigments are preferred because they can effectively color the interlayer film with a small amount incorporated. Examples of pigments include phthalocyanine pigments such as copper phthalocyanine pigments, anthraquinone pigments, perylene pigments, azo pigments, carbon black, quinacridone pigments, titanium oxide pigments, diketopyrrolopyrrole pigments, thioindigo pigments, Ni complex pigments, perinone pigments, isoindoline pigments, quinophthalone pigments, threne pigments, dioxazine pigments, pyrrocholine pigments, calcium carbonate, and derivatives thereof. In the colored layer, one colorant may be used alone, or two or more colorants may be used in combination.
[0036] Among the above, from the viewpoint of durability and compatibility with the film, at least one selected from the group consisting of carbon black, quinacridone pigments, copper phthalocyanine pigments, cobalt phthalocyanine pigments, nickel complex azo pigments, isoindolinone pigments, anthraquinone (anthraquinone) pigments, thioindigo pigments, isoindoline pigments, isoindolinone pigments, quinophthalone pigments, threne pigments, titanium oxide pigments, diketopyrrolopyrrole pigments, and perylene pigments is preferred, and at least one selected from the group consisting of carbon black, quinacridone pigments, copper phthalocyanine pigments, nickel complex azo pigments, isoindolinone pigments, and perylene pigments is more preferred, and among these, it is particularly preferred that the colorant contains carbon black. The use of carbon black can achieve a subdued color tone, make it easier to impart a luxurious feel, and further enhance the design properties. Furthermore, when carbon black is used as a colorant, it is also preferable to use a colorant other than carbon black in combination with the carbon black from the viewpoint of further enhancing design properties, and the colorant other than carbon black may be appropriately selected from the colorants other than carbon black described above. More specifically, it is also preferable to use any one of azo pigments, phthalocyanine pigments, and quinacridone pigments in combination.
[0037] The colorant content in the colored layer is preferably 0.0001% by mass or more and 0.3% by mass or less. When the content is 0.0001% by mass or more, the colorant sufficiently absorbs transmitted light and light reflected by the reflective layer, allowing the design viewed from one side of the laminated glass to be sufficiently different from the design viewed from the other side, thereby enhancing the design. Appropriate colorability can also be achieved. Furthermore, when the content is 0.3% by mass or less, excessive light absorption by the colorant is prevented, making it easier to ensure the transparency of the laminated glass. From these perspectives, the colorant content in the colored layer is more preferably 0.001% by mass or more, even more preferably 0.003% by mass or more, even more preferably 0.05% by mass or more, and more preferably 0.2% by mass or less, even more preferably 0.15% by mass or less, and even more preferably 0.12% by mass or less.
[0038] The colored layer may contain a heat-shielding material in addition to the colorant described above. That is, the colored layer may have the function of a heat-shielding layer, which will be described later. The heat-shielding material used in the colored layer is as described in the heat-shielding layer, which will be described later, and the content thereof is also as described in the heat-shielding layer, so description thereof will be omitted.
[0039] (Heat-shielding layer) The first resin layer may include a heat-shielding layer containing a heat-shielding material. Having the heat-shielding layer in the first resin layer can appropriately prevent the interior of the vehicle or indoors from becoming too hot. Furthermore, since a certain amount of incident light and light reflected by the reflective layer is absorbed by the heat-shielding layer, the color difference ΔE*ab(R) of the reflected light described above tends to increase, making it possible to change the design when viewed from one side compared to the other side. The heat-shielding material may be dispersed in the resin constituting the heat-shielding layer.
[0040] The heat-shielding layer is typically a material capable of absorbing infrared rays having a wavelength of 780 nm or more, i.e., heat rays. The heat-shielding material is made of an inorganic material, and typically, heat-shielding particles are used, specific examples of which include metal oxide particles and particles other than metal oxide particles, such as lanthanum hexaboride (LaB6) particles. Examples of metal oxide particles include tin oxide particles such as aluminum-doped tin oxide particles, indium-doped tin oxide particles, and antimony-doped tin oxide particles (ATO particles); zinc oxide particles such as gallium-doped zinc oxide particles (GZO particles), indium-doped zinc oxide particles (IZO particles), aluminum-doped zinc oxide particles (AZO particles), tin-doped zinc oxide particles, and silicon-doped zinc oxide particles; titanium oxide particles such as niobium-doped titanium oxide particles; indium oxide particles such as tin-doped indium oxide particles (ITO particles); and tungsten oxide particles such as sodium-doped tungsten oxide particles, cesium-doped tungsten oxide particles (CWO particles), thallium-doped tungsten oxide particles, and rubidium-doped tungsten oxide particles. Heat-shielding materials other than these may also be used. The heat-shielding materials may be used alone or in combination of two or more. Among these, metal oxide particles are preferred because of their high heat ray shielding function, and it is more preferable to use at least one selected from ATO particles, GZO particles, ITO particles and CWO particles, and it is even more preferable to use ITO particles or CWO particles, and it is preferable to use ITO particles.
[0041] The content of the heat-shielding material in the heat-shielding layer is not particularly limited, but is, for example, 0.01% by mass or more and 3% by mass or less, preferably 0.05% by mass or more and 1% by mass or less, and more preferably 0.1% by mass or more and 0.5% by mass or less, based on the total amount of the heat-shielding layer. By making the content of the heat-shielding material equal to or greater than the above-mentioned lower limit, it is possible to appropriately prevent the interior of a vehicle or a room from becoming too hot. In addition, it is easy to increase the color difference ΔE*ab(R) of reflected light described above. In addition, by making the content equal to or less than the above-mentioned upper limit, it is possible to prevent the transparency of the interlayer film from being unnecessarily impaired by the heat-shielding layer.
[0042] (Filler-Containing Layer) The first resin layer may also have a filler-containing layer containing the filler (A) described below. When the first resin layer has a filler-containing layer, it becomes easier to impart a metallic appearance to the interlayer film. The filler (A) used in the filler-containing layer is as described in the second resin layer described below, and its content is also as described below, so description thereof will be omitted.
[0043] (Clear layer) The first resin layer may have a layer that does not substantially contain the above-mentioned colorant, heat-shielding agent, and filler (A). A layer that does not substantially contain a colorant, heat-shielding agent, or filler (A) generally has high transmittance and is also referred to as a clear layer in this specification. Note that "not substantially containing a colorant, heat-shielding agent, or filler (A)" means that the colorant, heat-shielding agent, or filler (A) is not intentionally blended into the first resin layer, and the specific content of the colorant, heat-shielding agent, and filler (A) in the first resin layer is, for example, less than 0.0001% by mass in total, preferably less than 0.00001% by mass, and most preferably 0% by mass.
[0044] The first resin layer may be composed of one layer or two or more layers. Therefore, the interlayer film may have a single resin layer disposed on one side of the reflective layer, or two or more resin layers may be disposed. As described above, each first resin layer may be any of a colored layer, a heat-shielding layer, a filler-containing layer, and a clear layer. When the first resin layer is a single layer, the single first resin layer may be any of a colored layer, a heat-shielding layer, a filler-containing layer, and a clear layer. Furthermore, when the first resin layer is composed of multiple layers, it is sufficient that at least one of the above layers is present, and two or more layers of the same type may be present. For example, two or more first resin layers may include two or more colored layers, two or more heat-shielding layers, two or more filler-containing layers, or two or more clear layers. Furthermore, when there are multiple first resin layers, two of the above-mentioned types of layers may be provided; for example, a colored layer and a clear layer may be provided, a colored layer and a heat-shielding layer may be provided, or a colored layer and a filler-containing layer may be provided.
[0045] Among the above, the first resin layer preferably has at least a clear layer, a colored layer, or a heat-shielding layer, more preferably a colored layer or a heat-shielding layer, and even more preferably a colored layer. As described above, by having a heat-shielding layer or a colored layer, and especially a colored layer, the first resin layer is likely to have a larger color difference ΔE*ab(R) of reflected light, which makes it easier for the hue and design to change when viewed from the other side and when viewed from one side, thereby facilitating improved design. Furthermore, when there are multiple first resin layers, an embodiment having a clear layer in addition to a colored layer or a heat-shielding layer is also preferred, and an embodiment having a clear layer in addition to a colored layer is more preferred.
[0046] [Second Resin Layer] The interlayer film of the present invention preferably includes one or more second resin layers in addition to the reflective layer. The second resin layer is a resin layer that is disposed on the other side of the interlayer film relative to the reflective layer. The second resin layer may be a single layer or may include multiple layers. Therefore, it is more preferable that the interlayer film has one or more first resin layers that are disposed on one side of the reflective layer, and one or more second resin layers that are disposed on the other side of the reflective layer.
[0047] (Filler-containing layer) The second resin layer preferably has a layer containing a filler (A) (sometimes referred to as a "filler-containing layer" in this specification). Therefore, when the second resin layer is a single layer, it is sufficient that the single resin layer is a filler-containing layer, and when there are multiple second resin layers, it is sufficient that at least one of the multiple second resin layers is a filler-containing layer. In the filler-containing layer, it is sufficient that the filler (A) is dispersed in the resin constituting the filler-containing layer.
[0048] The filler (A) is a filler containing any one of a metal, a metal oxide, and a non-metallic material. The filler (A) has visible light reflecting properties. The filler (A) preferably contains at least any one of a metal oxide and a non-metallic material, and more preferably contains a metal oxide. The filler (A) is formed from a specific material and has visible light reflecting properties, which makes it easier to create a metallic look.
[0049] In the present invention, the second resin layer includes a filler-containing layer, which facilitates the creation of a metallic appearance in the interlayer film, particularly when viewed from the other side (i.e., the outdoor side). Furthermore, the interlayer film is more likely to reflect light incident from the other side, thereby increasing the color difference ΔE*ab(R) of the reflected light. Therefore, the interlayer film can have a significantly different design when viewed from the other side and one side, for example, giving the interlayer film a stronger metallic appearance when viewed from the other side, while giving the interlayer film a more subdued metallic appearance when viewed from the one side. This allows the interlayer film to have an impactful exterior when viewed from the other side (i.e., the outdoor side), while providing an interior with a more subdued impression when viewed from one side (i.e., the indoor side), further enhancing its design.
[0050] Examples of metals in the filler (A) include aluminum, silver, copper, platinum, gold, titanium, nickel, tin, tin-cobalt alloy, indium, and chromium. Examples of metal oxides include titanium oxide, silicon oxide, indium oxide, niobium oxide, zinc oxide, antimony oxide, tungsten oxide, and aluminum oxide. Examples of non-metallic materials include inorganic compounds other than metals and metal oxides, such as glass and mica.
[0051] The metal oxide-containing filler (A) is preferably a filler containing two or more compounds in each particle, such as a filler containing two or more metal oxides in each particle, or a filler containing a metal oxide and a non-metallic material such as mica or glass in each particle. In this case, the non-metallic material is preferably glass. Furthermore, fillers containing two or more compounds preferably have a multilayer structure. Specific examples include fillers having a multilayer structure of two or more metal oxides, fillers having a multilayer structure of a metal oxide and mica, and fillers having a multilayer structure of a metal oxide and glass. The first resin layer is more likely to have a metallic appearance when filler (A) has the above-described multilayer structure. Furthermore, the hue of transmitted light and reflected light can be changed as the angle of incidence of light on the interlayer film changes, resulting in color travel, where the color varies depending on the viewing angle, and thus improving the design of the interlayer film.
[0052] The filler (A) has a multilayer structure of two or more metal oxides, which makes it easy to impart a metallic appearance to transmitted and reflected light. Furthermore, while it is easy to color reflected light, it is difficult to impart color to transmitted light that passes through the interlayer film, making it possible to make the light nearly achromatic. Furthermore, the filler (A) has a multilayer structure of metal oxide and glass, which makes it possible to reduce haze and ensure the transparency of the interlayer film for laminated glass. Furthermore, reflections from the filler (A) can be visually recognized as glossy granular patterns, which allows the interlayer film for laminated glass to have a unique design. Furthermore, the filler (A) has a multilayer structure of metal oxide and mica, which makes it possible to increase the whiteness of the interlayer film and also to impart a glossy appearance.
[0053] In the metal oxide multilayer structure, it is preferable that the refractive indexes of two or more metal oxides are different from each other. By forming layers with different refractive indexes using metal oxides with different refractive indexes, it is easy to ensure a moderate metallic effect by reflection between the layers. Furthermore, in a filler having a metal oxide multilayer structure, it is preferable that the layers formed by metal oxides with different refractive indexes are adjacent to each other. From the viewpoint of improving transparency and metallic effect, the refractive index difference between the metal oxides with different refractive indexes is preferably 0.1 or more and 1.2 or less. The refractive index difference is more preferably 0.3 or more and 1.1 or less, and even more preferably 0.6 or more and 1.05 or less.
[0054] In filler (A) having a multilayer structure of two or more metal oxides, the thickness ratio between layers formed by different metal oxides is preferably 1:2 to 1:15. Filler (A) having such a thickness ratio facilitates the creation of a metallic appearance. The thickness ratio is more preferably 1:3 to 1:13, and even more preferably 1:4 to 1:11. Furthermore, by controlling the thickness ratio, filler (A) can also change the color of reflected light. The thickness ratio is the average value of values measured by observing 50 random particles using a scanning electron microscope (SEM) or the like.
[0055] The two or more metal oxides may be selected from the group consisting of titanium oxide, silicon oxide, indium oxide, niobium oxide, zinc oxide, antimony oxide, tungsten oxide, aluminum oxide, and iron oxide, and among these, titanium oxide, silicon oxide, and aluminum oxide are preferred. Titanium oxide is titanium dioxide (TiO 2 ), and may be of the rutile type, the anatase type, or the brookite type. Silicon oxide is silicon dioxide (SiO 2 ) Aluminum oxide is alumina (Al 2 O 3) is preferable. The filler (A) more preferably contains both titanium oxide and silicon oxide, and further preferably has a multilayer structure of a titanium oxide layer and a silicon oxide layer. The filler (A) also preferably contains both titanium oxide and aluminum oxide, and preferably has a multilayer structure of a titanium oxide layer and an aluminum oxide layer. As described above, the filler (A) is preferably metal oxide particles having a multilayer structure formed from two or more types of metal oxides, and is preferably metal oxide particles (an intermediate layer described later) made of at least one type of metal oxide coated with at least one type of metal oxide of a different type.
[0056] The filler (A) having a multilayer structure of metal oxide and glass is preferably formed from glass and a metal oxide selected from the group consisting of titanium oxide, silicon oxide, indium oxide, niobium oxide, zinc oxide, antimony oxide, tungsten oxide, aluminum oxide, and iron oxide. Among these, the metal oxide is preferably titanium oxide, silicon oxide, or both of these. The filler (A) having a multilayer structure of metal oxide and glass more preferably has a multilayer structure of a glass layer and a metal oxide layer, and in particular, it is preferable that the middle layer constituting the glass layer is a particle coated with a metal oxide (preferably titanium oxide, silicon oxide, or both of these).
[0057] The filler (A) having a multilayer structure of a metal oxide and mica is preferably formed from mica and a metal oxide selected from the group consisting of titanium oxide, silicon oxide, indium oxide, niobium oxide, zinc oxide, antimony oxide, tungsten oxide, aluminum oxide, and iron oxide, and among these, titanium oxide is preferred as the metal oxide.The filler (A) having a multilayer structure of a metal oxide and mica more preferably has a multilayer structure of a mica layer and a metal oxide layer, and in particular, it is preferred that the middle layer constituting the mica layer is a particle coated with a metal oxide (preferably titanium oxide).
[0058] The shape of the filler (A) may be any of polygonal shapes such as spherical or quadrangular prism, polygonal pyramid shapes such as triangular or quadrangular pyramid, cylindrical, conical, amorphous, needle-like, fibrous, and flat shapes, but a flat shape is preferred. The flat shape of the filler (A) causes color travel, and the hue of transmitted light or reflected light can be changed as the angle of incidence of light on the interlayer film changes. The flat shape of the filler (A) allows it to be oriented along the surface direction of the interlayer film, as described below, which makes it easier to reflect a certain amount of incident visible light while increasing the transparency of the interlayer film. Furthermore, regular reflection makes it less likely for light scattering to occur, making it easier to reduce the haze of the laminated glass.
[0059] When the flat-plate-shaped filler (A) has the above-described multilayer structure, it is preferable that a plurality of layers are provided along the thickness direction, and preferably 2 to 5 layers, more preferably 2 to 4 layers, and even more preferably 3 layers are provided along the thickness direction.
[0060] A specific example of a flat-plate-shaped filler (A) having a three-layer structure is shown in FIG. 1. When the filler (A) has a three-layer structure, as shown in FIG. 1, it is preferable that the filler (A) has an intermediate layer 100 and coating layers 111 and 112 provided on both sides of the intermediate layer 100. The filler shown in FIG. 1 preferably has a multilayer structure of metal oxides, and the metal oxides forming the coating layers 111 and 112 are preferably different from the metal oxide forming the intermediate layer 100. The metal oxides forming the coating layers 111 and 112 are preferably the same. The refractive index of the metal oxides forming the coating layers 111 and 112 is preferably higher than the refractive index of the intermediate layer 100. By relatively increasing the refractive index of the coating layers 111 and 112, light is transmitted while being appropriately reflected, which makes it easier to improve both the transparency and metallic feel of the interlayer film. Furthermore, because the three-layer structure has a higher refractive index of the metal oxides of the coating layers 111 and 112 than that of the middle layer 100, light incident from either of the two surfaces is appropriately reflected, thereby more effectively ensuring transparency while creating a metallic appearance. The preferred value for the difference in refractive index between the coating layers 111 and 112 and the middle layer 100 is as described above. The thickness of each of the coating layers 111 and 112 is preferably smaller than that of the middle layer 100. The preferred specific thickness ratio (each coating layer:middle layer) is as shown in the thickness ratio between the layers.
[0061] In the plate-shaped filler (A) having a multilayer structure of metal oxides, the coating layers 111 and 112 are both titanium oxide layers, and the middle layer 100 is preferably a silicon oxide layer or an aluminum oxide layer, and it is particularly preferable that the middle layer 100 is a silicon oxide layer. The plate-shaped filler (A) is not limited to the above-mentioned three-layer structure, and may have a two-layer structure, in which case one of the coating layers 111 and 112 may be omitted. The plate-shaped filler (A) may also have a multilayer structure of four or more layers.
[0062] Furthermore, the filler having a multilayer structure of glass and metal oxide may be composed of a glass layer constituting a middle layer and metal oxide layers provided on both sides of the glass layer and constituting coating layers. The metal oxide in the metal oxide layer may be at least one selected from the above metal oxides, with titanium oxide and silicon oxide being preferred. Titanium oxide and silicon oxide may be used alone or in combination. Here, the metal oxide layer in each coating layer may be a single layer or a double layer. That is, the filler having a multilayer structure of glass and metal oxide may have a three-layer structure consisting of a metal oxide layer, a middle layer, and a metal oxide layer, or may have a two-layer structure consisting of a metal oxide layer, a metal oxide layer, a middle layer, a metal oxide layer, and a metal oxide. In the five-layer structure, it is preferred that the metal oxide constituting the outer metal oxide layer is titanium oxide and the metal oxide constituting the inner metal oxide layer is silicon oxide. Furthermore, in a filler having a multilayer structure in which an intermediate layer is composed of a glass layer, the metal oxide layers provided on both sides of the glass layer are not limited to a two-layer structure, but may be three or more layers. Therefore, a filler having a multilayer structure in which an intermediate layer is composed of a glass layer is not particularly limited as long as it has a structure in which a single or multiple metal oxide layers are provided on both sides of the glass layer.
[0063] The filler having a metal oxide layer may be a filler having a mica layer and a metal oxide layer. Specifically, the mica layer may constitute a middle layer, and the metal oxide layer may constitute a coating layer, and the coating layer is preferably a titanium oxide layer.
[0064] As described above, the filler (A) is preferably a filler having an intermediate layer and a coating layer formed of a metal oxide. In this case, the coating layer may cover the entire surface of the intermediate layer, or may cover only a portion of the intermediate layer surface. By coating a portion of the intermediate layer surface, reflection by the filler (A) becomes non-uniform. As a result, the reflected light or transmitted light in the laminated glass may be, for example, mottled, thereby imparting a unique design. When a portion of the intermediate layer surface is coated, the coverage rate of the intermediate layer with the coating layer is, for example, 30% to 99%, preferably 40% to 90%, and more preferably 50% to 80%. When a portion of the intermediate layer surface is coated, the portion of the intermediate layer not covered by the coating layer may be provided continuously or discontinuously, for example, in the form of spots.
[0065] The average particle size (D50) of the filler (A) is preferably 1 μm or more and 100 μm or less. By setting the average particle size within the above range, the hue of transmitted light and reflected light is more likely to change with changes in the angle of incidence of light on the interlayer film, making color travel more likely to occur. From the viewpoint of causing color travel, the average particle size of the filler (A) is more preferably 3 μm or more and 90 μm or less, and even more preferably 5 μm or more and 80 μm or less. The average particle size (D50) is a value measured using a laser diffraction / scattering particle size distribution analyzer, and the value (D50) at which the cumulative volume is 50% is defined as the average particle size.
[0066] The average particle size of the filler (A) having a multilayer structure of metal oxides is preferably 1 μm or more and 20 μm or less, preferably 3 μm or more and 18 μm or less, and more preferably 5 μm or more and 16 μm or less, from the viewpoint of easily suppressing light scattering in the interlayer film while achieving both transparency and a metallic finish. On the other hand, the average particle size of the filler (A) having a multilayer structure of metal oxides and glass is preferably a certain value or more, from the viewpoint of making a glossy granular pattern visible by light reflected from the filler and imparting a unique design to the interlayer film for laminated glass, and specifically, is preferably 5 μm or more and 100 μm or less, more preferably 10 μm or more and 90 μm or less, and even more preferably 15 μm or more and 80 μm or less.
[0067] The thickness of the filler (A) is preferably 0.01 μm or more and 4 μm or less, more preferably 0.1 μm or more and 3.5 μm or less, and even more preferably 0.2 μm or more and 3 μm or less, from the viewpoint of ensuring transparency and facilitating color travel. Furthermore, a filler (A) having a multilayer structure of metal oxides with the above thickness range is more likely to produce a metallic effect. The thickness of the filler (A) is the average value of values measured by observing 50 random particles using a scanning electron microscope (SEM) or the like. The thickness of the filler (A) may be the length in the direction perpendicular to the longitudinal direction of the filler, in which the maximum length is the shortest. The thickness of the plate-shaped filler (A) is the length in the vertical direction in FIG. 1.
[0068] The aspect ratio of the filler (A) is preferably 1 or more, more preferably 1.1 or more, even more preferably 1.2 or more, and preferably 50 or less, more preferably 30 or less, even more preferably 15 or less, and even more preferably 10 or less. The above aspect ratios facilitate color travel. Furthermore, as described below, by orienting the filler (A) along the in-plane direction of the interlayer film, it becomes easier to improve the transparency of the interlayer film while reflecting a certain amount of incident visible light. Furthermore, by setting the aspect ratio to 50 or less, it is possible to prevent the average particle size (D50) of the filler (A) from becoming unnecessarily large. The aspect ratio of the filler (A) is the ratio of the length of the major axis to the length of the minor axis of the filler (A) observed with a scanning electron microscope. The major axis and minor axis refer to the major axis and minor axis of the filler (A) when viewed in a planar view along the thickness direction. For a flat-shaped filler, these refer to the longitudinal direction and the direction perpendicular to the in-plane direction.
[0069] When the filler (A) has orientable anisotropy, such as when it has a flat plate shape, it is preferable that its longitudinal direction be oriented along the plane direction of the interlayer film. Furthermore, when it has a flat plate shape, it is preferable that the plane direction of the filler (A) be oriented along the plane direction of the interlayer film. That is, the flat-shaped filler (A) is preferably oriented so that the thickness direction of the filler (A) is oriented along the thickness direction of the interlayer film. The filler (A) having the above orientation appropriately reflects light traveling along the thickness direction of the interlayer film while partially transmitting the light, and can also suppress light scattering caused by the filler (A). This makes it easier to reduce haze and improve transparency. In the first resin layer, one type of filler (A) may be used alone, or two or more types may be used in combination.
[0070] The method for producing the filler (A) is not particularly limited, and for example, a filler (A) having a multilayer structure may be produced by coating particles formed from a metal oxide with another metal oxide, or by coating particles formed from mica or glass with a metal oxide. Alternatively, a sheet formed from a metal oxide may be coated with another metal oxide and then crushed to form a flat-plate-shaped filler (A). A commercially available product may be used as the filler (A).
[0071] The content of the filler (A) in the filler-containing layer is preferably 0.01% by mass or more and 0.5% by mass or less. A content of 0.01% by mass or more makes it easier to relatively increase the color difference ΔE*ab(R), and also makes it easier to create a metallic look and cause color travel, thereby improving the design. Furthermore, a content of 0.5% by mass or less prevents unnecessary reflection of light in the first resin layer, reduces haze, and ensures transparency of the laminated glass. From these viewpoints, the content of the filler (A) is more preferably 0.02% by mass or more, even more preferably 0.04% by mass or more, even more preferably 0.08% by mass or more, and more preferably 0.4% by mass or less, even more preferably 0.3% by mass or less, and even more preferably 0.2% by mass or less.
[0072] The filler-containing layer may further contain a colorant to function as a colored layer. The inclusion of a colorant in the filler-containing layer facilitates enhancing the design properties of the interlayer film. Details of the colorant are as described above for the first resin layer. However, it is preferable that the filler-containing layer used in the second resin layer substantially does not contain a colorant. By substantially not containing a colorant, the transmitted light through the filler-containing layer is more likely to reflect the hue of the filler (A). Furthermore, the reflection of the filler (A) is less likely to be blocked by the colorant, making color travel more likely to occur. "Substantially not containing a colorant" means that a colorant is not intentionally blended into the filler-containing layer. The specific colorant content in the filler-containing layer is, for example, less than 0.0001% by mass, preferably less than 0.00001% by mass, and most preferably 0% by mass, based on the total amount of the filler-containing layer. On the other hand, when the filler-containing layer contains a colorant, the details of the colorant are as described above for the first resin layer, and the content of the colorant is also as described above, so the description thereof will be omitted.
[0073] The second resin layer may have a colored layer containing a colorant. Having a colored layer in the second resin layer makes it easier to enhance the design of the interlayer film. Details of the colorant used in the colored layer in the second resin layer are as described above for the first resin layer. The content of the colorant in the colored layer of the second resin layer is also as described above, and a description thereof will be omitted. The second resin layer may have a heat-shielding layer containing a heat-shielding material. Having a heat-shielding layer in the second resin layer makes it possible to appropriately prevent the interior of a vehicle or a room from becoming hot. Details of the heat-shielding material used in the heat-shielding layer in the second resin layer are as described above. The content of the heat-shielding material in the second resin layer is also as described above, and a description thereof will be omitted. The second resin layer may also have a layer (clear layer) that is substantially free of the colorant, heat-shielding agent, and filler (A) described above. Details of the clear layer are as described above for the first resin layer, and a description thereof will be omitted.
[0074] The second resin layer may be composed of one layer or two or more layers. Therefore, the interlayer film may have a single resin layer disposed on the other side of the reflective layer, or two or more resin layers may be disposed. As described above, each second resin layer may be any of a colored layer, a heat-shielding layer, a filler-containing layer, and a clear layer. When the second resin layer is a single layer, the single second resin layer may be any of a colored layer, a heat-shielding layer, a filler-containing layer, and a clear layer. Furthermore, when the second resin layer is composed of multiple layers, it is sufficient that at least one of the above layers is present, and two or more layers of the same type may be present. For example, two or more second resin layers may include two or more colored layers, two or more heat-shielding layers, two or more filler-containing layers, or two or more clear layers. Furthermore, when there are multiple second resin layers, two of the above-mentioned types of layers may be provided; for example, a filler-containing layer and a clear layer may be provided, a filler-containing layer and a colored layer may be provided, or a colored layer and a heat-shielding layer may be provided.
[0075] Among the above, the second resin layer preferably has at least one of a clear layer, a heat-shielding layer, a color layer, and a filler-containing layer, and particularly preferably has at least a filler-containing layer. By having the first resin layer have a filler-containing layer, as described above, the color difference ΔE*ab(R) of reflected light tends to increase, and the design tends to be improved. Furthermore, when there are multiple first resin layers, it is also preferable to have a clear layer in addition to the filler-containing layer.
[0076] [Thermoplastic Resin] The resin constituting each of the above-mentioned first resin layers (colored layer, heat-shielding layer, clear layer, filler-containing layer, etc.) is preferably a thermoplastic resin. Furthermore, the resin constituting each of the second resin layers (colored layer, heat-shielding layer, clear layer, filler-containing layer, etc.) is also preferably a thermoplastic resin. By containing a thermoplastic resin, the first resin layer or the second resin layer can easily function as an adhesive layer, and the adhesiveness to the laminated glass member or other layers constituting the interlayer film can be improved.
[0077] The thermoplastic resin in each resin layer is not particularly limited, but examples include polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ionomer resin, polyurethane resin, thermoplastic elastomer, acrylic resin, acrylic-vinyl acetate copolymer resin, polyvinyl alcohol resin, polyolefin resin, polyvinyl acetate resin, and polystyrene resin. The use of these resins facilitates ensuring adhesion to laminated glass components. Among these, polyvinyl acetal resin, ethylene-vinyl acetate copolymer resin, ionomer resin, polyurethane resin, and thermoplastic elastomer are preferred. In the interlayer film of the present invention, the thermoplastic resin may be used alone or in combination of two or more. When two or more types are used in combination, the interlayer film may contain two or more types of thermoplastic resins in one resin layer (first or second resin layer), or different resin layers (first and second resin layers) may contain different types of thermoplastic resins. Among these, at least one selected from polyvinyl acetal resins and ethylene-vinyl acetate copolymer resins is preferred, with polyvinyl acetal resins being more preferred, particularly in terms of the excellent adhesion to inorganic glass they exhibit when used in combination with a plasticizer. Accordingly, the resin in each first resin layer is more preferably at least one selected from polyvinyl acetal resins and ethylene-vinyl acetate copolymer resins, with polyvinyl acetal resins being even more preferred. Similarly, the resin in each second resin layer is more preferably at least one selected from polyvinyl acetal resins and ethylene-vinyl acetate copolymer resins, with polyvinyl acetal resins being even more preferred.
[0078] The resin constituting each resin layer may be appropriately selected from the resins listed above. The resins constituting each resin layer may be different from each other, but are preferably the same. Therefore, the resins constituting both the first and second resin layers are preferably polyvinyl acetal resins or ethylene-vinyl acetate copolymer resins, and more preferably polyvinyl acetal resins.
[0079] (Polyvinyl Acetal Resin) The polyvinyl acetal resin is not particularly limited as long as it is a polyvinyl acetal resin obtained by acetalizing polyvinyl alcohol (PVA) with an aldehyde. The aldehyde is not particularly limited, but generally, an aldehyde having 1 to 10 carbon atoms is preferably used. The aldehyde having 1 to 10 carbon atoms is not particularly limited, and examples thereof include n-butyl aldehyde, isobutyraldehyde, n-valeraldehyde, 2-ethylbutyraldehyde, n-hexyl aldehyde, n-octyl aldehyde, n-nonyl aldehyde, n-decyl aldehyde, formaldehyde, acetaldehyde, and benzaldehyde. These aldehydes may be used alone or in combination of two or more. Among the above, n-butylaldehyde, n-hexylaldehyde, and n-valeraldehyde are preferred, and n-butylaldehyde is more preferred. Therefore, the polyvinyl acetal resin is preferably a polyvinyl butyral resin.
[0080] Polyvinyl alcohol (PVA) can be obtained, for example, by saponifying a polyvinyl ester such as polyvinyl acetate. The degree of saponification of polyvinyl alcohol is generally 70 to 99.9 mol %. Polyvinyl acetal resins may be used singly or in combination of two or more. The average degree of polymerization of PVA is preferably 200 or more, more preferably 500 or more, even more preferably 1000 or more, and even more preferably 1500 or more. Increasing the average degree of polymerization above the lower limit improves the penetration resistance of laminated glass. Furthermore, the average degree of polymerization of PVA is preferably 5000 or less, more preferably 4000 or less, even more preferably 3500 or less, and even more preferably 2500 or less. The average degree of polymerization of polyvinyl alcohol is determined according to JIS K6726 "Testing Methods for Polyvinyl Alcohol."
[0081] The amount of hydroxyl groups in the polyvinyl acetal resin is preferably 15 mol% or more and preferably 38 mol% or less. By setting the amount of hydroxyl groups to 15 mol% or more, adhesiveness is likely to be improved and the penetration resistance of the laminated glass is likely to be improved. Furthermore, by setting the amount of hydroxyl groups to 38 mol% or less, the laminated glass is prevented from becoming too hard. From the viewpoint of adhesiveness to the laminated glass member, the amount of hydroxyl groups is more preferably 20 mol% or more, and even more preferably 25 mol% or more. Furthermore, the amount of hydroxyl groups is more preferably 35% or less, and even more preferably 33 mol% or less. When a polyvinyl butyral resin is used as the polyvinyl acetal resin, from the same viewpoint, the amount of hydroxyl groups is 15 mol% or more and preferably 38 mol% or less, more preferably 20 mol% or more, even more preferably 25 mol% or more, more preferably 35% or less, and even more preferably 33 mol% or less. The amount of hydroxyl groups in the polyvinyl acetal resin is the molar fraction calculated by dividing the amount of ethylene groups having hydroxyl groups by the total amount of ethylene groups in the main chain, and is expressed as a percentage. The amount of ethylene groups having hydroxyl groups can be measured, for example, in accordance with JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0082] The degree of acetalization of the polyvinyl acetal resin is preferably 47 mol% or more and preferably 85 mol% or less. The degree of acetalization is more preferably 55 mol% or more, even more preferably 60 mol% or more, and more preferably 80 mol% or less, even more preferably 75 mol% or less. Note that the term "degree of acetalization" refers to the degree of butyralization when the acetal group is a butyral group and the polyvinyl acetal resin (A) is a polyvinyl butyral resin.
[0083] The degree of acetalization is a molar fraction obtained by subtracting the amount of ethylene groups having hydroxyl groups and the amount of ethylene groups having acetyl groups from the total amount of ethylene groups in the main chain, and dividing the result by the total amount of ethylene groups in the main chain, and the percentage is expressed as the molar fraction. The degree of acetalization (degree of butyralization) may be calculated from the results of measurements made, for example, according to JIS K6728 "Testing Methods for Polyvinyl Butyral."
[0084] The degree of acetylation of the polyvinyl acetal resin is preferably 30 mol% or less, more preferably 20 mol% or less, even more preferably 10 mol% or less, and even more preferably 2 mol% or less. When the degree of acetylation is equal to or less than the upper limit, the moisture resistance of the interlayer film and laminated glass is improved. The degree of acetylation is not particularly limited, but is preferably 0.01 mol% or more, more preferably 0.1 mol% or more. The degree of acetylation is a molar fraction calculated by dividing the amount of ethylene groups to which acetyl groups are bonded by the total amount of ethylene groups in the main chain, expressed as a percentage. The amount of ethylene groups to which acetyl groups are bonded can be measured, for example, in accordance with JIS K6728 "Test Methods for Polyvinyl Butyral."
[0085] (Ethylene-Vinyl Acetate Copolymer Resin) The ethylene-vinyl acetate copolymer resin may be a non-crosslinked ethylene-vinyl acetate copolymer resin or a high-temperature crosslinked ethylene-vinyl acetate copolymer resin. Furthermore, modified ethylene-vinyl acetate resins such as saponified ethylene-vinyl acetate copolymers and hydrolyzed ethylene-vinyl acetate can also be used as the ethylene-vinyl acetate copolymer resin. The ethylene-vinyl acetate copolymer resin preferably has a vinyl acetate content of 10 to 50 mass%, more preferably 20 to 40 mass%, as measured in accordance with JIS K 6730 "Test Methods for Ethylene-Vinyl Acetate Resins" or JIS K 6924-2:1997. By adjusting the vinyl acetate content to be equal to or greater than these lower limits, adhesion to laminated glass components is improved and the penetration resistance of the laminated glass is likely to be improved. Furthermore, by adjusting the vinyl acetate content to be equal to or less than these upper limits, the rupture strength of the interlayer film is increased, resulting in improved impact resistance of the laminated glass.
[0086] (Ionomer Resin) The ionomer resin is not particularly limited, and various ionomer resins can be used. Specific examples include ethylene-based ionomers, styrene-based ionomers, perfluorocarbon-based ionomers, telechelic ionomers, polyurethane ionomers, etc. Among these, ethylene-based ionomers are preferred because they improve the mechanical strength, durability, transparency, etc. of the laminated glass and have excellent adhesion to laminated glass members.
[0087] As the ethylene-based ionomer, an ionomer of an ethylene-unsaturated carboxylic acid copolymer is preferably used due to its excellent transparency and toughness. The ethylene-unsaturated carboxylic acid copolymer is a copolymer having at least ethylene-derived structural units and unsaturated carboxylic acid-derived structural units, and may also have structural units derived from other monomers. Examples of unsaturated carboxylic acids include acrylic acid, methacrylic acid, maleic acid, etc., with acrylic acid and methacrylic acid being preferred, and methacrylic acid being particularly preferred. Examples of other monomers include acrylic acid esters, methacrylic acid esters, and 1-butene. The ethylene-unsaturated carboxylic acid copolymer preferably contains 75 to 99 mol % of ethylene-derived structural units and 1 to 25 mol % of unsaturated carboxylic acid-derived structural units, assuming that the total structural units of the copolymer are 100 mol %. The ionomer of an ethylene-unsaturated carboxylic acid copolymer is an ionomer resin obtained by neutralizing or crosslinking at least a portion of the carboxyl groups of the ethylene-unsaturated carboxylic acid copolymer with metal ions, and the degree of neutralization of the carboxyl groups is usually 1 to 90%, preferably 5 to 85%.
[0088] Examples of ion sources for the ionomer resin include alkali metals such as lithium, sodium, potassium, rubidium, and cesium, and polyvalent metals such as magnesium, calcium, and zinc, with sodium and zinc being preferred.
[0089] The method for producing the ionomer resin is not particularly limited, and the resin can be produced by a conventionally known production method. For example, when an ionomer of an ethylene-unsaturated carboxylic acid copolymer is used as the ionomer resin, for example, ethylene and an unsaturated carboxylic acid are radically copolymerized under high temperature and high pressure to produce the ethylene-unsaturated carboxylic acid copolymer. The ionomer of the ethylene-unsaturated carboxylic acid copolymer can then be produced by reacting the ethylene-unsaturated carboxylic acid copolymer with a metal compound containing the above-mentioned ion source.
[0090] (Polyurethane Resin) Examples of polyurethane resins include polyurethanes obtained by reacting an isocyanate compound with a diol compound, and polyurethanes obtained by reacting an isocyanate compound with a diol compound and a chain extender such as a polyamine. The polyurethane resin may also contain sulfur atoms. In this case, some or all of the diols may be selected from polythiols and sulfur-containing polyols. Polyurethane resins can improve adhesion to organic glass. Therefore, they are preferably used when the laminated glass member is made of organic glass.
[0091] (Thermoplastic Elastomer) Examples of thermoplastic elastomers include styrene-based thermoplastic elastomers and aliphatic polyolefins. The styrene-based thermoplastic elastomer is not particularly limited, and known elastomers can be used. Styrenic thermoplastic elastomers generally have a styrene monomer polymer block as a hard segment and a conjugated diene compound polymer block or a hydrogenated block thereof as a soft segment. Specific examples of styrene-based thermoplastic elastomers include styrene-isoprene diblock copolymers, styrene-butadiene diblock copolymers, styrene-isoprene-styrene triblock copolymers, styrene-butadiene / isoprene-styrene triblock copolymers, styrene-butadiene-styrene triblock copolymers, and hydrogenated products thereof. The aliphatic polyolefins may be saturated aliphatic polyolefins or unsaturated aliphatic polyolefins. The aliphatic polyolefins may be polyolefins containing a chain olefin as a monomer or polyolefins containing a cyclic olefin as a monomer. From the viewpoint of effectively improving the storage stability and sound insulation of the interlayer film, the aliphatic polyolefins are preferably saturated aliphatic polyolefins.Examples of the aliphatic polyolefin material include ethylene, propylene, 1-butene, trans-2-butene, cis-2-butene, 1-pentene, trans-2-pentene, cis-2-pentene, 1-hexene, trans-2-hexene, cis-2-hexene, trans-3-hexene, cis-3-hexene, 1-heptene, trans-2-heptene, cis-2-heptene, trans-3-heptene, cis-3-heptene, 1-octene, trans-2-octene, cis-2-octene, and trans-3- octene, cis-3-octene, trans-4-octene, cis-4-octene, 1-nonene, trans-2-nonene, cis-2-nonene, trans-3-nonene, cis-3-nonene, trans-4-nonene, cis-4-nonene, 1-decene, trans-2-decene, cis-2-decene, trans-3-decene, cis-3-decene, trans-4-decene, cis-4-decene, trans-5-decene, cis-5-decene, 4-methyl-1-pentene, and vinylcyclohexane.
[0092] (Plasticizer) The interlayer film may further contain a plasticizer. As described above, the interlayer film has one or more resin layers, and each resin layer (i.e., for example, each of the first and second resin layers) may contain a plasticizer in addition to a thermoplastic resin. The inclusion of a plasticizer makes each resin layer flexible, thereby improving the flexibility and penetration resistance of the laminated glass. It also makes it possible to improve adhesion to laminated glass components. The inclusion of a plasticizer is particularly effective when a polyvinyl acetal resin is used as the thermoplastic resin. Therefore, it is more preferable that each resin layer, such as the first resin layer or the second resin layer, contain a polyvinyl acetal resin and a plasticizer. Examples of plasticizers include organic ester plasticizers such as monobasic organic acid esters and polybasic organic acid esters, and phosphorus-based plasticizers such as organic phosphate ester plasticizers and organic phosphite ester plasticizers. Among these, organic ester plasticizers are preferred.
[0093] Examples of the organic ester plasticizer include triethylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylhexanoate, triethylene glycol dicaprylate, triethylene glycol di-n-octanoate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, tetraethylene glycol di-2-ethylhexanoate, dibutyl sebacate, dioctyl azelate, dibutyl carbitol adipate, ethylene glycol di-2-ethylbutyrate, 1,3-propylene glycol di-2-ethylbutyrate, 1,4-butylene glycol di-2-ethylbutyrate, 1,2-butylene glycol di-2-ethylbutyrate, and diethylene glycol di- Examples of suitable adipates include 2-ethyl butyrate, diethylene glycol di-2-ethylhexanoate, dipropylene glycol di-2-ethylbutyrate, triethylene glycol di-2-ethylpentanoate, tetraethylene glycol di-2-ethylbutyrate, diethylene glycol dicaprylate, triethylene glycol di-n-heptanoate, tetraethylene glycol di-n-heptanoate, triethylene glycol di-2-ethylbutyrate, dihexyl adipate, dioctyl adipate, hexylcyclohexyl adipate, diisononyl adipate, heptylnonyl adipate, dibutyl sebacate, oil-modified alkyd sebacic acid, a mixture of a phosphate ester and an adipate ester, and mixed adipates. Examples of mixed adipates include adipates prepared from two or more alcohols selected from alkyl alcohols having 4 to 9 carbon atoms and cyclic alcohols having 4 to 9 carbon atoms. Among the above plasticizers, triethylene glycol-di-2-ethylhexanoate (3GO) is particularly suitable.
[0094] For example, the content of plasticizer in each resin layer, such as each first resin layer or each second resin layer, is not particularly limited, but is preferably 10 parts by mass or more and 100 parts by mass or less per 100 parts by mass of thermoplastic resin. When the plasticizer content is 10 parts by mass or more, the resin layer becomes moderately flexible, and penetration resistance, adhesion, etc. are improved. Furthermore, when the plasticizer content is 100 parts by mass or less, separation of the plasticizer from each resin layer is prevented. The content of plasticizer in each resin layer is more preferably 20 parts by mass or more, even more preferably 30 parts by mass or more, even more preferably 35 parts by mass or more, and more preferably 70 parts by mass or less, even more preferably 63 parts by mass or less.
[0095] Each resin layer is mainly composed of a resin, or a resin and a plasticizer. For example, in each first resin layer or each second resin layer, the total amount of the thermoplastic resin and the plasticizer is usually 70% by mass or more, preferably 80% by mass or more, and more preferably 90% by mass or more but less than 100% by mass, based on the total amount of each resin layer.
[0096] [Other Additives] Each resin layer of the present invention may contain additives other than those described above, such as an ultraviolet absorber, an antioxidant, a light stabilizer, an adhesion modifier, a heat-shielding agent, a fluorescent brightening agent, a crystal nucleating agent, etc. As described above, the interlayer film of the present invention has one or more resin layers, and each resin layer may contain at least one selected from these additives as appropriate.
[0097] <Laminate Structure> The laminate structure of the interlayer film of the present invention will be described below with reference to the drawings. As shown in Figures 2 to 19, for example, the interlayer film 10 preferably includes a reflective layer 15, one or more first resin layers 11 provided on one surface 10A of the interlayer film closer to the reflective layer 15, and one or more second resin layers 12 provided on the other surface 10B of the interlayer film closer to the reflective layer 15. The interlayer film 10 is preferably bonded to a first laminated glass member 21 via one or more first resin layers 11, and to a second laminated glass member 22 via one or more second resin layers 12, thereby forming a laminated glass 20. Preferably, one surface 10A of the interlayer film 10 serves as the bonding surface for the first laminated glass member 21, and the other surface 10B serves as the bonding surface for the first laminated glass member 21, but other layers may be provided between the one surface 10A and the first laminated glass member 21 and between the other surface 10B and the second laminated glass member 22. As described above, when the interlayer film 10 is applied to laminated glass, it is preferred that the second resin layer 12 side, i.e., the other surface 10B side, is disposed on the outdoor side (i.e., the exterior side of an automobile), and the one surface 10A side is disposed on the indoor side (i.e., the interior side of an automobile).
[0098] The layer structure when the interlayer film has first and second resin layers will be described in more detail below. As shown in Figures 2 to 5, the interlayer film preferably includes a colored layer 11A as the first resin layer 11. In this case, the other surface of the reflective layer may be provided with a second resin layer 12, which may include a filler-containing layer 12B (see Figure 2), a heat-shielding layer 12C (see Figure 3), a clear layer 12D (see Figure 4), or the colored layer 12A (see Figure 5).
[0099] As shown in FIG. 2 , the interlayer film 10 includes a colored layer 11A on one surface 10A and a filler-containing layer 12B on the other surface 10B. The colored layer 11A and the filler-containing layer 12B facilitate increasing the color difference ΔE*ab(R) of reflected light, allowing the design viewed from the one surface 10A to be sufficiently different from the design viewed from the other surface 10B. The filler-containing layer 12B also enables a metallic appearance and color travel, further improving the design. Furthermore, by arranging the filler-containing layer 12B on the other surface 10B and the colored layer 11A on the one surface 10A, the metallic appearance is strong when viewed from the other surface 10B (i.e., the outdoor side), while the metallic appearance is subdued when viewed from the one surface 10A (i.e., the indoor side). Therefore, when viewed from the other side 10B (i.e., outdoors), the exterior can be made to have an impactful appearance, while when viewed from the one side 10A (i.e., indoors), the interior can be made to have a calm impression, thereby improving the design.
[0100] 3, the interlayer film 10 has a colored layer 11A on one surface 10A and a heat-shielding layer 12C on the other surface 10B, which makes it easier for the color difference ΔE*ab(R) of reflected light to be at least a certain level due to the colored layer 11A, allowing the design viewed from one surface to be sufficiently different from the design viewed from the other surface. Furthermore, the provision of the heat-shielding layer can appropriately prevent the interior of the vehicle or indoors from becoming too hot.
[0101] Furthermore, as shown in FIG. 4 , the interlayer film 10 includes a colored layer 11A on one surface 10A and a clear layer 12D on the other surface 10B, thereby achieving a relatively large color difference between the visible light transmitted through the first resin layer 11 (visible light transmission light) and the visible light transmitted through the second resin layer 12 (visible light transmission light). This allows the design viewed from one surface to be sufficiently different from the design viewed from the other surface. Furthermore, providing the clear layer 12D facilitates increasing the transmittance of the entire interlayer film 10. In the configuration shown in FIG. 4 , the second resin layer 12 may have a multilayer structure, as described below. In this case, it is preferable that all of the second resin layers 12 be clear layers.
[0102] Furthermore, as shown in FIG. 5 , the interlayer film 10 includes a colored layer 11A on one side 10A and a colored layer 12A on the other side 10B, enabling various color expressions. Furthermore, the design viewed from one side can be made different from the design viewed from the other side. When the interlayer film 10 includes a colored layer 11A on one side 10A and a colored layer 12A on the other side 10B, the type and content of the colorant in each colored layer can be appropriately adjusted so that the color difference ΔE*ab(S), described below, is a certain value or greater. Furthermore, the type and content of the colorant used can be appropriately adjusted so that the L*(S1) of the first resin layer 11 in the visible light transmission light is smaller than the L*(S2) of the second resin layer 12 in the visible light transmission light, and the difference ΔL* is a certain value or greater.
[0103] Furthermore, as shown in Figure 2 and Figures 6 to 8 above, it is preferable that the intermediate film has a filler-containing layer 12B as the second resin layer 12 on the other surface 10B side. In this case, as described above, on the one surface 10A side, as the first resin layer 11, a colored layer 11A (see Figure 2) may be provided (see Figure 2), a heat-shielding layer 11C may be provided (see Figure 6), a clear layer 11D may be provided (see Figure 7), or a filler-containing layer 11B may be provided (see Figure 8).
[0104] As shown in Figure 6, the interlayer film 10 includes a heat-shielding layer 11C on one side 10A and a filler-containing layer 12B on the other side 10B. This filler-containing layer 12B facilitates achieving a certain value or greater for the color difference ΔE*ab(R) of reflected light, allowing the design viewed from one side to be sufficiently different from the design viewed from the other side. It also makes it possible to create a metallic effect and allow color travel. Additionally, the provision of the heat-shielding layer 11C can appropriately prevent the interior of a vehicle or other room from becoming too hot.
[0105] As shown in Figure 7, the interlayer film 10 has a clear layer 11D on one side 10A and a filler-containing layer 12B on the other side 10B. The filler-containing layer 12B facilitates achieving a certain level of color difference in reflected light, ΔE*ab(R), and allows the design viewed from one side to be sufficiently different from the design viewed from the other side. It also makes it possible to create a metallic effect and produce color travel. Additionally, the clear layer 11D facilitates increasing the transmittance of the entire interlayer film 10.
[0106] Furthermore, as shown in FIG. 8 , the interlayer film 10 includes a filler-containing layer 11B and a filler-containing layer 12B on each of the first and second surfaces 10A, 10B. This provides a sufficient metallic appearance when viewed from both the first and second surfaces 10A (indoor and outdoor), and also facilitates color travel. Furthermore, the design viewed from one surface can be made different from the design viewed from the other surface. When the interlayer film 10 includes filler-containing layers 12B, 11B on both surfaces, the type and content of the filler (A) used can be appropriately adjusted so that the color difference ΔE*ab(S), described below, is equal to or greater than a certain value. Furthermore, the type and content of the filler (A) used may be appropriately adjusted so that L*(S1) in the visible light transmitted through the first resin layer 11 is smaller than L*(S2) in the visible light transmitted through the second resin layer 12, and the difference ΔL* is a certain value or more.
[0107] 2 to 8, the first resin layer 11 is formed of one layer and the second resin layer 12 is formed of one layer, but in each configuration, at least one of the first resin layer 11 and the second resin layer 12 may be formed of two or more layers. Even when either the first resin layer 11 or the second resin layer 12 is formed of two or more layers, it is preferable that the first resin layer 11 includes a colored layer 11A as illustrated in FIGS. 2 to 5, or that the second resin layer 12 includes a filler-containing layer 12B as illustrated in FIGS. 2, 6 to 8.
[0108] For example, in an embodiment in which a colored layer 11A is provided as the first resin layer 11 and a filler-containing layer 12B is provided as the second resin layer 12, a clear layer 12D may be additionally provided on the second resin layer 12, so that the second resin layer 12 has the clear layer 12D and the filler-containing layer 12B, as shown in Fig. 9. Of course, in an embodiment in which a colored layer 11A is provided as the first resin layer 11 and a filler-containing layer 12B is provided as the second resin layer 12, the first resin layer 11 may have the clear layer 11D and the colored layer 11A, although this is not shown.
[0109] Furthermore, in an embodiment in which a colored layer 11A is provided as the first resin layer 11 and a clear layer 12D is provided as the second resin layer 12 as in the configuration shown in Fig. 4, a clear layer 11D may be additionally provided on the first resin layer 11, so that the first resin layer 11 has the colored layer 11A and the clear layer 11D, as shown in Fig. 10. Similarly, in an embodiment in which a clear layer 11D is provided as the first resin layer 11 and a filler-containing layer 12B is provided as the second resin layer 12, a clear layer 12D may be additionally provided on the second resin layer 12, so that the second resin layer 11 has the filler-containing layer 12B and the clear layer 12D, as shown in Fig. 11.
[0110] Furthermore, for example, in an embodiment in which a colored layer 11A is provided as the first resin layer 11 and a colored layer 12A is provided as the second resin layer 12, a clear layer 11D may be additionally provided on the first resin layer 11, so that the first resin layer 11 has the colored layer 11A and the clear layer 11D, as shown in Fig. 12. Similarly, although not shown, in an embodiment in which a colored layer 11A is provided as the first resin layer 11 and a colored layer 12B is provided as the second resin layer 12, a clear layer 12D may be additionally provided on the second resin layer 12, so that the second resin layer 12 has the colored layer 12A and the clear layer 12D.
[0111] Furthermore, for example, in an embodiment in which a filler-containing layer 11B is provided as the first resin layer 11 and a filler-containing layer 12B is provided as the second resin layer 12, a clear layer 12D may be additionally provided on the second resin layer 12, so that the second resin layer 12 has the filler-containing layer 12B and the clear layer 12D, as shown in Fig. 13. Similarly, although not shown, in an embodiment in which a filler-containing layer 11B is provided as the first resin layer 11 and a filler-containing layer 12B is provided as the second resin layer 12, a clear layer 11D may be additionally provided on the first resin layer 11, so that the first resin layer 11 has the filler-containing layer 11B and the clear layer 11D.
[0112] Furthermore, in the above, when a plurality of first resin layers 11 are provided, an embodiment has been shown in which the first resin layers 11 include a clear layer 11D and a layer other than the clear layer 11D, such as a colored layer 11A, but the clear layer 11D does not need to be provided, and two layers other than the clear layer 11 may be provided, for example, two or more identical layers other than the clear layer 11D, such as a colored layer 11A, may be provided, or two or more different layers other than the clear layer 11D may be provided, for example, as shown in Figure 14, a colored layer 11A and a filler-containing layer 11B may be provided. In this case, it is preferable that the second resin layer 12 includes a filler-containing layer 12B, but other embodiments may also be possible.
[0113] Similarly, when a plurality of second resin layers 12 are provided, an embodiment has been shown in which the second resin layers 12 include a clear layer 12D and a layer other than the clear layer 12D, such as a filler-containing layer 12B, but the clear layer 12D does not need to be provided, and two layers other than the clear layer 12 may be provided, for example, two or more identical layers other than the clear layer 12D, such as a filler-containing layer 12B, may be provided, or two or more different layers other than the clear layer 12D may be provided, for example, as shown in Figure 15, a colored layer 12A and a filler-containing layer 12B may be provided. In this case, it is preferable that the first resin layer 11 be provided with a colored layer 11A, but other embodiments may also be possible.
[0114] The above describes a configuration in which a colored layer 11A is provided as the first resin layer 11 or a filler-containing layer 12B is provided as the second resin layer 12. However, the colored layer 11A and the filler-containing layer 12B may not be provided. In such a case, for example, each of the first and second resin layers 11, 12 may be composed of at least one of a heat-shielding layer and a clear layer. In one embodiment, both the first and second resin layers 11, 12 may be clear layers 11D, 12D as shown in FIG. 16 . In such a case, the configuration of the clear layers 11D, 12D may be adjusted so that, for example, ΔE*ab(S), described below, is a certain value or more, L*(S1) is smaller than L*(S2), and the difference ΔL*(S) is a certain value or more. For example, the thickness of the first resin layer 11 may be greater than the thickness of the second resin layer 12.
[0115] When the first resin layer 11 consists of two or more layers, for example, as shown in FIG. 17 , the first resin layer 11 may have a three-layer structure with a central resin layer called a core layer 11T and skin layers 11S, 11S on either side of the core layer 11, thereby providing sound insulation performance. Here, the resins used for the skin layer 11S and the core layer 11T are as described above, but preferably a polyvinyl acetal resin, and more preferably a polyvinyl butyral resin. Furthermore, as described above, both the skin layer 11S and the core layer 11T preferably contain a plasticizer. In this case, the content of the plasticizer in the core layer 11T per 100 parts by mass of the thermoplastic resin is preferably greater than the content of the plasticizer in the skin layer 11S per 100 parts by mass of the thermoplastic resin, and the difference between the two contents is preferably 5 parts by mass or more and 60 parts by mass or less, more preferably 10 parts by mass or more and 50 parts by mass or less, and even more preferably 15 parts by mass or more and 35 parts by mass or less. Increasing the plasticizer content in the core layer 11T facilitates improving sound insulation performance. Furthermore, the hydroxyl group content of the polyvinyl acetal resin in the core layer 11T is preferably lower than the hydroxyl group content of the polyvinyl acetal resin in the skin layer 11S, with the difference in hydroxyl group content being preferably 1 mol % to 20 mol %, more preferably 2 mol % to 15 mol %, and even more preferably 2 mol % to 10 mol %. Lowering the hydroxyl group content in the core layer facilitates increasing the plasticizer content, which also facilitates improving sound insulation performance.
[0116] Even when the first resin layer has a three-layer structure, as explained above, the first resin layer preferably has a colored layer 11A, and it is preferable that either the skin layer 11S or the core layer 11T is the colored layer 11A, but as shown in Figure 17, it is preferable that either the skin layers 11S, 11S is the colored layer 11A, and it is more preferable that the outer skin layer 11S is the colored layer 11A, as shown in Figure 17. In this case, the second resin layer 12 may be provided with a filler-containing layer 12B as shown in Figure 17, or may be provided with a heat-shielding layer 12C, a clear layer 12D, or a colored layer 12A as explained with reference to Figures 3 to 5.
[0117] Of course, when the first resin layer has a three-layer structure including skin layers 11S, 11S, and a core layer 11T, the first resin layer does not need to have a colored layer, and may be provided with a heat-shielding layer 11C or a filler-containing layer 11B, as described with reference to Figures 6 and 8. The heat-shielding layer 11C or the filler-containing layer 11B may be composed of any of the skin layers 11S, 11S, and the core layer 11T, as in the case of the colored layer 11A, but is preferably composed of any of the skin layers 11S, 11S, and in particular, it is preferable that the outer skin layer 11S is the heat-shielding layer 11C or the filler-containing layer 11B. Furthermore, as described with reference to Figures 7 and 16, the first resin layer 11 does not need to be provided with the colored layer 11A, the heat-shielding layer 11C, or the filler-containing layer 11B, and the skin layers 11S, 11S, and the core layer 11T of the first resin layer 11 may all be clear layers 11D.
[0118] Similarly, when the second resin layer 11 is made up of two or more layers, for example, as shown in Fig. 18, the second resin layer may have a three-layer structure in which a central resin layer is a core layer 12T and layers on both sides thereof are skin layers 12S, 12S, thereby providing sound insulation performance. In this case, the details of the core layer 12T and the skin layer 12S are the same as those of the core layer 11T and the skin layer 11S described above, and therefore a description thereof will be omitted.
[0119] Furthermore, even when the second resin layer has a three-layer structure, as explained above, it is preferable that the second resin layer has a filler-containing layer 12B, and it is preferable that either the skin layer 12S or the core layer 12T is a filler-containing layer 12B, but it is more preferable that either the skin layer 12S, 12S is a filler-containing layer 12B, and in particular, it is preferable that the outer skin layer 12S is a filler-containing layer 12B, as shown in Figure 18.
[0120] In this case, the first resin layer 11 may be provided with a colored layer 11A as shown in Figure 18, or may be provided with a heat-shielding layer 11C, a clear layer 11D, or a filler-containing layer 11B as described with reference to Figures 6 to 8. Of course, when the second resin layer has a three-layer structure including skin layers 12S, 12S, and a core layer 12T, the second resin layer does not need to have a filler-containing layer 12B, and may be provided with a heat-shielding layer 12C or a colored layer 12A as described with reference to Figures 3 and 5. As with the filler-containing layer 12B, the heat-shielding layer 12C or the colored layer 12A may be formed of any of the skin layers 12S, 12S, and the core layer 12T, but is preferably formed of any of the skin layers 12S, 12S, and it is particularly preferable that the outer skin layer 12S is the heat-shielding layer 12C or the colored layer 12A. Furthermore, as explained with reference to Figures 4 and 16, the second resin layer does not need to be provided with the colored layer 12A, the heat-shielding layer 12C, or the filler-containing layer 12B, and the skin layers 12S, 12S, and the core layer 122T may all be clear layers 12D.
[0121] The laminated structure of the interlayer film described above is merely an example, and needless to say, is not limited to the above. The one or more first resin layers and the one or more second resin layers may each have a laminated structure other than the above. Furthermore, at least one of the first resin layer and the second resin layer may be omitted. In such a case, the reflective layer may be directly bonded to the laminated glass member, or the reflective layer may be bonded to the laminated glass member via a layer other than the first and second resin layers.
[0122] (Optical Properties of Resin Layer) As described above, the interlayer film preferably includes a reflective layer, one or more first resin layers 11, and one or more second resin layers 12. In this case, the color difference ΔE*ab (hereinafter sometimes referred to as "ΔE*ab(S)") in the L*a*b* color system between the visible light transmitted through the first resin layer 11 and the visible light transmitted through the second resin layer 12 may be, for example, greater than 0 and less than 100. When ΔE*ab(S) is greater than 0, it becomes easier to achieve the above-mentioned color difference ΔE*ab(R) at a certain value or higher, making it possible to differentiate the design when viewed from one side from the design when viewed from the other side. Furthermore, when ΔE*ab(S) is less than 100, there is no need to apply extreme coloring to the first resin layer or the second resin layer, thereby maintaining good design properties. ΔE*ab (hereinafter referred to as ΔE*ab(S)) is preferably 1 or more, more preferably 5 or more, even more preferably 20 or more, and even more preferably 35 or more, and is preferably 95 or less, more preferably 85 or less, even more preferably 75 or less, and even more preferably 65 or less.
[0123] Furthermore, it is preferable that the L* (hereinafter sometimes referred to as "L*(S1)") of the visible light transmitted through the first resin layer 11 and the L* (hereinafter sometimes referred to as "L*(S2)") of the visible light transmitted through the second resin layer 12 are such that L*(S2) is higher than L*(S1). When L*(S2) is higher than L*(S1), a design can be achieved in which the reflected light from the reflective layer 15 is more clearly reflected when viewed from the other surface 10B of the interlayer 10 (i.e., the outdoor side) than when viewed from the one surface 10A of the interlayer 10. This allows for an appearance that has a stronger impact when viewed from the outdoor side, thereby further enhancing the design. Furthermore, the difference ΔL*(S) between L*(S2) and L*(S1) is preferably 1 or more, more preferably 5 or more, even more preferably 20 or more, and even more preferably 30 or more, and is preferably 95 or less, more preferably 85 or less, even more preferably 75 or less, and even more preferably 65 or less.
[0124] The L*(S1) of the visible light transmitted through the first resin layer 11 is not particularly limited, but from the viewpoint of imparting a certain level of transparency to the interlayer film, it is preferably 5 or more, more preferably 10 or more, even more preferably 20 or more, and even more preferably 35 or more. Furthermore, L*(S1) may be less than 100, but from the viewpoints of practicality and design, it is preferably 97 or less, more preferably 80 or less, even more preferably 70 or less, and even more preferably 60 or less. Furthermore, the L*(S2) of the visible light transmitted through the second resin layer 12 is not particularly limited, but from the viewpoint of imparting a certain level of transparency to the interlayer film, it is preferably 40 or more, more preferably 50 or more, even more preferably 60 or more, and even more preferably 70 or more. Furthermore, L*(S2) may be less than 100, but from the viewpoints of practicality and design, it is preferably 98 or less, more preferably 97 or less, and even more preferably 93 or less.
[0125] ΔE*ab(S) can be determined by measuring the L*, a*, and b* of each of the first and second resin layers using the visible light transmitted through them when irradiated with light, and then calculating the color difference (ΔE*ab(S)) from the measured L*, a*, and b*. The calculated color difference (ΔE*ab(S)) is then used as the color difference ΔE*ab(S) in the L*a*b* color system between the visible light transmitted through the first resin layer and the visible light transmitted through the second resin layer. In this case, when multiple first resin layers are provided, the visible light transmitted through all of the provided first resin layers. Therefore, L*, a*, and b* can be measured using a laminate of multiple first resin layers. The same applies when a second resin layer is provided. Furthermore, the optical properties such as L*, a*, and b* of each resin layer are measured by laminating two reference clear glass plates together with each resin layer therebetween to produce a laminated glass, and then measuring the laminated glass. The obtained measured values are regarded as the optical properties of each resin layer.
[0126] For example, when the interlayer film of the present invention has a heat-shielding layer, the total solar transmittance (Tts) of a laminated glass produced by bonding two standard clear glass sheets via the interlayer film is preferably 70% or less. A total solar transmittance (Tts) of 70% or less can ensure sufficient heat-shielding properties and prevent the interior of a vehicle or room from becoming too hot. The total solar transmittance (Tts) is more preferably 60% or less, even more preferably 55% or less, even more preferably 45% or less, even more preferably 40% or less, even more preferably 35% or less, and particularly preferably 33% or less. From the viewpoint of improving heat-shielding properties, the lower the total solar transmittance (Tts), the better, and a value of 0% or more is sufficient, but in practical terms, a value of 10% or more is preferred. The total solar transmittance (Tts) may be measured by illuminating light from both surfaces, as long as either of the values falls within the above range. However, it is preferable that the value measured by illuminating light from the other surface 10B (i.e., the surface facing the outdoors) falls within the above range. The Tts used here is a value measured by transmitting light from the vehicle exterior (i.e., the second resin layer side).
[0127] When the first resin layer is multilayered (preferably three or more layers), any of the multiple first resin layers may be provided in a partial region of the interlayer film. For example, in the first resin layer, a partial region may have a laminated structure of clear layer / colored layer / clear layer, and the remaining region may have a laminated structure of clear layer / clear layer. In this case, in regions where no colored layer is provided, the two clear layers may be integrated to form a single clear layer. Similarly, when the second resin layer is multilayered (preferably three or more layers), any of the multiple second resin layers may be provided in a partial region of the interlayer film. For example, in the second resin layer, a partial region may have a laminated structure of clear layer / filler-containing layer / clear layer, and the remaining region may have a laminated structure of clear layer / clear layer. In this case, in regions where no filler-containing layer is provided, the two clear layers may be integrated to form a single clear layer. In this way, when any of the multiple first resin layers or any of the multiple second resin layers is provided in a certain region, it is sufficient that the color difference ΔE*ab(R) in any of the regions is a predetermined value, and it is sufficient that any of the regions has the above-mentioned laminated structure.
[0128] The interlayer film may have a rectangular cross section and a constant thickness, but is not limited to a rectangular cross section and may have, for example, a wedge shape. A wedge-shaped interlayer film has a cross-sectional thickness that differs from one end to the other end, and may have a trapezoidal or triangular cross section. Furthermore, a wedge-shaped interlayer film has a thickness that changes from one end to the other, but the thickness does not need to change over the entire area; it may have a constant thickness in one area, and the thickness may change only in part.
[0129] [Thickness of Each Layer] The total thickness of the first resin layers is preferably 0.1 mm to 1.8 mm, more preferably 0.16 mm to 1.6 mm, and even more preferably 0.2 mm to 1.2 mm. Note that the total thickness here refers to the thickness of the single resin layer when the first resin layer is a single layer, and the total thickness of the multiple layers when there are multiple first resin layers. The same also applies to the total thickness of the second resin layer below. Furthermore, when multiple first resin layers are provided, the thickness of each first resin layer is preferably 0.05 mm to 1.0 mm, more preferably 0.08 mm to 0.9 mm, and even more preferably 0.1 mm to 0.8 mm. When multiple first resin layers are provided, the thicknesses of the first resin layers may be the same or different from each other.
[0130] The total thickness of the second resin layers is preferably 0.1 mm to 1.8 mm, more preferably 0.16 mm to 1.6 mm, and even more preferably 0.2 mm to 1.2 mm. The total thickness of the second resin layers may be the same as or different from the total thickness of the first resin layers. When multiple second resin layers are provided, the thickness of each second resin layer is preferably 0.05 mm to 1.0 mm, more preferably 0.08 mm to 0.9 mm, and even more preferably 0.1 mm to 0.8 mm. When multiple second resin layers are provided, the thicknesses of the second resin layers may be the same as or different from each other. The total thickness of the interlayer film is not particularly limited, but is preferably 0.25 mm to 3.5 mm, more preferably 0.4 mm to 2.5 mm, and even more preferably 0.5 mm to 2 mm. The thickness of each resin layer and interlayer film may vary. In such a case, the thickness of each resin layer and the thickness of the interlayer film described above may be an average value in a region where the color difference ΔE*ab(R) satisfies a predetermined requirement.
[0131] (Method for Manufacturing Interlayer Film) The interlayer film of the present invention is not particularly limited, but may be obtained by preparing each resin composition for forming each resin layer, molding a resin layer from the resulting resin composition, appropriately laminating the molded resin layer on a reflective layer, and, if necessary, appropriately laminating the resin layers together. Each resin composition may be obtained, for example, by mixing a thermoplastic resin with a filler (A), a colorant, a heat-shielding material, a plasticizer, and other additives, which are blended as needed. Here, each colored layer, heat-shielding layer, and filler-containing layer may be blended with a thermoplastic resin, a colorant, a heat-shielding material, and a filler (A). However, in order to improve dispersibility in the resin composition, when a plasticizer is used, for example, one of the colorant, the heat-shielding material, and the filler (A) may be blended with the plasticizer and thoroughly dispersed in the plasticizer before being mixed with the thermoplastic resin. In this case, a dispersant or the like may be added to the plasticizer as appropriate.
[0132] The interlayer film may be formed by extrusion molding, press molding, or the like. For example, a resin layer obtained by extrusion molding may be laminated on a reflective layer. Alternatively, resin layers may be laminated together as appropriate by extrusion molding. Co-extrusion may be used as necessary for extrusion molding. The thickness of each resin layer may vary in a direction perpendicular to the thickness direction. In such a case, the thickness may be changed, for example, by adjusting the amount of resin supplied during extrusion molding. Alternatively, the interlayer film may be produced by preparing a resin layer and a reflective layer, disposing the resin layer and the reflective layer between a pair of laminated glass components to obtain a laminate, and then thermocompressing (press molding) the laminate, thereby producing the interlayer film while producing the laminated glass. When the filler (A) has orientable anisotropy, such as when it has a flat shape, the longitudinal direction or planar direction of the filler (A) can be oriented along the planar direction of the interlayer film (each resin layer) by the above-mentioned press molding, extrusion molding, or the like.
[0133] <Laminated Glass> The present invention also provides laminated glass. The laminated glass comprises two laminated glass members (first and second laminated glass members) and an interlayer film disposed between these laminated glass members. The two laminated glass members are bonded via the interlayer film. One surface of the interlayer film is bonded to one laminated glass member, and the other surface is bonded to the other laminated glass member. The configuration of the interlayer film is as described above. The laminated glass may be produced by disposing the above-described interlayer film between two laminated glass members and integrating them by thermocompression bonding or the like. Alternatively, the laminated glass may be produced by preparing a resin layer and a reflective layer, disposing the resin layer and the reflective layer between a pair of laminated glass members to obtain a laminate, and integrating the laminate by thermocompression bonding or the like.
[0134] (Laminated Glass Member) Examples of the laminated glass member used in the laminated glass include glass plates. The glass plates may be either inorganic or organic glass, but inorganic glass is preferred. Examples of inorganic glass include, but are not limited to, clear glass, float glass, polished glass, figured glass, wired glass, striped glass, and colored glass. Examples of organic glass generally used are what is called resin glass, and include, but are not limited to, organic glass made from resins such as polycarbonate, acrylic resin, acrylic copolymer resin, and polyester. The organic glass may also be colored glass. Colored glass is described below. The two laminated glass members may be made of the same material or different materials. For example, one may be inorganic glass and the other organic glass. However, it is preferred that both the two laminated glass members be inorganic glass or organic glass. The thickness of each laminated glass member is, but is not limited to, about 0.1 to 15 mm, preferably 0.5 to 5 mm. The thickness of each laminated glass member may be the same or different from each other, but it is preferable that they are the same.
[0135] The laminated glass of the present invention preferably has a color difference ΔE*ab (hereinafter sometimes referred to as "ΔE*ab(Rg)") between the L*a*b* color space of reflected light of light incident from one direction and the L*a*b* color space of reflected light of light incident from the opposite direction of 0.5 or more. In the present invention, when the color difference ΔE*ab(R) of reflected light is 0.5 or more, the design when viewed from one side of the laminated glass of the present invention can be made different from the design when viewed from the other side, thereby imparting high designability to the laminated glass.
[0136] From the viewpoint of enhancing design, the color difference ΔE*ab(Rg) of the reflected light is preferably 2.0 or more, more preferably 15 or more, and even more preferably 30 or more. From the viewpoint of ease of realization and preventing the design viewed from one side from differing too greatly from the design viewed from the other side, the color difference ΔE*ab(Rg) of the reflected light is preferably 100 or less, more preferably 75 or less, and even more preferably 50 or less. The color difference ΔE*ab(Rg) can be made to be a certain value or more by setting the ΔE*ab(R) of the interlayer film to a certain value or more as described above. Furthermore, as shown in a laminated glass according to another aspect described later, the color difference ΔE*ab(Rg) can be adjusted to be within a predetermined range by, for example, coloring one of the laminated glass members (e.g., the first laminated glass member) to make the color of the first member different from the color of the second member.
[0137] In the present invention, the color difference ΔE*ab(Rg) between the reflected light and the transmitted light of the laminated glass is determined by illuminating light from one side (i.e., one direction) of the laminated glass and measuring the L*a*b* color space of the reflected light of that light, and by illuminating light from the other side (i.e., the opposite direction) of the laminated glass and measuring the L*a*b* color space of the reflected light of that light. The color difference is then calculated from the determined L*, a*, and b* values, and the above-mentioned color difference ΔE*ab(Rg) of the reflected light can be determined.
[0138] (Laminated Glass According to Another Aspect) In another aspect of the present invention, as shown in Figures 2 to 19, a laminated glass can be described as comprising a first member 31 having a first laminated glass member 21 and one or more first resin layers 11, a reflective layer 15, and a second member 32 having a second laminated glass member 22 and one or more second resin layers 12. Here, the laminated glass comprises the first laminated glass member 21, one or more first resin layers 11, the reflective layer 15, one or more second resin layers 12, and the second laminated glass member 22 arranged in this order. The first member 31 and the second member 32 may preferably be different in color. The laminated glass having the above configuration is provided with the reflective layer 15, and the first member 31 and the second member 32 have different colors, so that ΔE*ab(Rg) is equal to or greater than a predetermined value, and the design when viewed from one side of the laminated glass can be made different from the design when viewed from the other side.
[0139] Here, to make the colors of the first member 31 and the second member 32 different, it is preferable to make the colors of the first resin layer 11 and the second resin layer 12 different. Specifically, as described above, the color difference ΔE*ab (ΔE*ab(S)) between the visible light transmitted through the first resin layer 11 and the visible light transmitted through the second resin layer 12 may be, for example, greater than 0 and less than 100. The preferred range of ΔE*ab(S) is as described above. Here, "different colors" means that the color difference ΔE*ab(M) between the visible light transmitted through the first member 31 and the second member 32 in the L*a*b* color system is greater than 0, and the color difference ΔE*ab(M) is preferably 2.5 or more, more preferably 5, even more preferably 15, even more preferably 20 or more, and even more preferably 30 or more. Furthermore, the color difference ΔE*ab(M) is not particularly limited, but is preferably 95 or less, more preferably 85 or less, even more preferably 75 or less, and even more preferably 65 or less. Furthermore, the L* of the visible light transmitted through the first member 31 (hereinafter sometimes referred to as "L*(M1)") and the L* of the visible light transmitted through the second member 32 (hereinafter sometimes referred to as "L*(M2)") are preferably higher than L*(M1). Having L*(M2) higher than L*(M1) allows for a design that reflects the reflected light from the reflective layer more clearly when viewed from the second resin layer side (i.e., the outdoor side) than when viewed from the first resin layer side of the laminated glass 20.
[0140] To differentiate the colors of the first member 31 and the second member 32, the colors of the first laminated glass member 21 and the second laminated glass member 22 may be differentiated. Specifically, the color difference ΔE*ab (hereinafter referred to as ΔE*ab(G)) in the L*a*b* color system between the visible light transmitted through the first laminated glass member 21 and the visible light transmitted through the first laminated glass member 22 may be, for example, greater than 0 and less than 100. Here, ΔE*ab(G) is preferably 1 or greater, more preferably 5 or greater, even more preferably 10 or greater, and even more preferably 15 or greater, and is preferably 95 or less, more preferably 70 or less, even more preferably 50 or less, and even more preferably 40 or less.
[0141] When the first and second laminated glass members 21, 22 are made to have different colors, it is preferable that the L* (hereinafter sometimes referred to as "L*(G1)") of the visible light transmitted through the first laminated glass member 21 and the L* (hereinafter sometimes referred to as "L*(G2)") of the visible light transmitted through the second laminated glass member 22 (hereinafter sometimes referred to as "L*(G2)") (G2) are higher than L*(G1). When L*(G2) is higher than L*(G1), a design can be achieved in which the reflected light from the reflective layer 15 is more reflected when viewed from the second laminated glass member 22 side (i.e., the other surface 10B side) than when viewed from the first laminated glass member 21 side (i.e., the one surface 10A side) of the laminated glass. This allows for an appearance that has a stronger impact when viewed from the outdoors, thereby further enhancing the design. Furthermore, when L*(G2) is higher than L*(G1), the difference ΔL*(G) between L*(G2) and L*(G1) is preferably 1 or more, more preferably 5 or more, even more preferably 10 or more, and even more preferably 20 or more, and is preferably 95 or less, more preferably 70 or less, even more preferably 50 or less, and even more preferably 40 or less.
[0142] When the first laminated glass member 21 and the second laminated glass member 22 are made to have different colors, the L*(G1) of visible light transmitted through the first laminated glass member 21 is not particularly limited, but from the viewpoint of imparting a certain level of transparency to the laminated glass, it is preferably 30 or more, more preferably 40 or more, even more preferably 50 or more, and even more preferably 55 or more. Furthermore, L*(G1) may be less than 100, but from the viewpoints of practicality and design, it is preferably 97 or less, more preferably 95 or less, even more preferably 90 or less, and even more preferably 80 or less. When the first laminated glass member 21 and the second laminated glass member 22 are made to have different colors, the L*(G2) of visible light transmitted through the second laminated glass member 22 is not particularly limited, but from the viewpoint of imparting a certain level of transparency to the laminated glass, it is preferably 70 or more, more preferably 80 or more, and even more preferably 90 or more. Furthermore, L*(G2) may be less than 100, but from the viewpoints of practicality and design, it is preferably 98 or less, more preferably 97 or less.
[0143] To differentiate the colors of the first and second laminated glass members 21, 22 as described above, it is preferable to color at least one of them to form colored glass, and in particular, it is preferable to color the first laminated glass member 21 to form colored glass 21C, as shown in Figure 19. The colored glass 21C is glass colored with a coloring agent.
[0144] The colored glass 21C may be formed by incorporating a colorant into the laminated glass member itself. For example, when incorporating a colorant into the glass member, a known composition may be used. In the case of inorganic glass, a known colorant such as a metal ion may be blended into the inorganic glass. In the case of organic glass, the above-mentioned pigments, dyes, or the like may be blended into the organic glass. When incorporating a colorant into the glass member itself, for example, the colorant may be incorporated into at least one of the two glass members. Alternatively, colored glass may be formed by forming a colored layer containing a colorant on the surface of the laminated glass member. Specifically, the colored layer may be formed on the surface of the laminated glass member 21 facing the interlayer film 10 (inner surface 21X), or on the surface of the laminated glass member 21 opposite the surface facing the interlayer film 10 (outer surface 21Y). The colored layer is a coating formed on the surface of the glass member and may be in any form as long as it contains a colorant. However, the coating may contain a binder component such as a thermosetting resin or a thermoplastic resin, as necessary, and may further contain appropriate additives. As the colored glass, commercially available glass such as green glass or plycy glass may be used.
[0145] In colored glass, the colored layer does not need to be provided over the entire area of the laminated glass, but may be provided over only a portion of the area. Also, even when the glass members constituting the laminated glass themselves contain a colorant to color the glass members, only a portion of the glass members may be colored.
[0146] 19, the embodiment in which the colored glass 21C is used is an embodiment in which both the first and second resin layers 11, 12 are clear layers 11D, 12D, but the embodiment is not limited to this embodiment, and any of the laminate structures shown in FIGS. 2 to 18 can be employed, as well as laminate structures other than those shown in FIGS. 2 to 18. However, when the colored glass 21C is used, among the above-mentioned embodiments, the embodiment in which both the first and second resin layers 11, 12 are clear layers 11D, 12D as shown in FIG. 19, the embodiment in which the colored layer 11A is provided on the first resin layer 11 (see, for example, FIGS. 2 to 5), and the embodiment in which the filler-containing layer 12B is provided on the second resin layer 12 (see, for example, FIGS. 2 and 6 to 8) are preferred. Furthermore, in an embodiment in which the first resin layer 11 is provided with a colored layer 11A, an embodiment in which the second resin layer 12 is a clear layer 12D (see, for example, FIG. 4 ) or an embodiment in which the second resin layer 12 is provided with a filler-containing layer 12B (see FIG. 2 ) are preferred. Furthermore, in an embodiment in which the second resin layer 12 is provided with a filler-containing layer 12B, an embodiment in which the first resin layer 11 is provided with a colored layer 11A (see FIG. 2 ) or an embodiment in which the first resin layer 11 is a clear layer 11D (see FIG. 7 ) are preferred. Note that when the first member 31 and the second member 32 are made to have different colors, the first resin layer 11 and the second resin layer 12 may have different colors, and the first laminated glass member 21 and the second laminated glass member 22 may have different colors.
[0147] The laminated glass of the present invention can be used as window glass for various vehicles such as automobiles, aircraft, ships, and other vehicles, buildings, and the like, but is preferably used as automotive laminated glass. The automotive laminated glass may be any of windshield glass (front glass), side glass, rear glass, and roof glass. In each application, window glass is generally used as a component for separating the outdoors from the indoors. As described above, the interlayer film 10 is preferably arranged such that one surface 10A, which is the surface on the first resin layer 11 side, faces the indoor side (i.e., the interior side in an automobile), and the other surface 10B, which is the surface on the second resin layer 12 side, faces the outdoor side (the exterior side in an automobile).
[0148] The present invention will be explained in more detail by way of examples, but the present invention is not limited to these examples in any way.
[0149] The measurement and evaluation methods in the present examples are as follows. [Reflected light color difference ΔE*ab(R), (Rg)] One surface of each of the laminated glasses obtained in the Examples and Comparative Examples was irradiated with light from a D65 light source at an incident angle of 90° and a measurement wavelength range of 300 nm to 2000 nm over a 10° field of view, and the reflected light was detected at wavelength intervals of 5 nm from one surface, and a*, b*, and L* were measured using a UV-Vis-Near-Infrared Spectrophotometer "V-670" (manufactured by JASCO Corporation) equipped with an absolute reflectance measurement unit (ARSN-733). Similarly, the other surface of the laminated glass was irradiated with light from the light source at an incident angle of 90°, and the reflected light was detected at wavelength intervals of 5 nm from the other surface, and a*, b*, and L* were similarly measured. The a*, b*, and L* detected on one surface were defined as a*1, b*1, and L*1, and the a*, b*, and L* detected on the other surface were defined as a*2, b*2, and L*2, and the color difference ΔE*ab was calculated using the following formula (1) to be the color difference ΔE*ab(Rg). In the case of laminated glass, if both of the two laminated glass members are standard clear glass plates, ΔE*ab(Rg) becomes the color difference ΔE*ab(R). Formula (1): ΔE*ab={(a*2-a*1) 2 +(b*2-b*1) 2 +(L*2-L*1) 2} 1/2
[0150] [L*, a*, b*, and color difference ΔE*ab(G) of laminated glass members] Using CIE standard illuminant D65 and 10° visual field color matching functions specified in JIS Z 8781-1 (2012), JIS Z 8781-2 (2012), and JIS Z 8781-4 (2013), the L*, a*, and b* of the first and second laminated glass members were measured. Note that the a*, b*, and L* of the first laminated glass member were defined as a*1, b*1, and L*1, and the a*, b*, and L* of the second laminated glass member were defined as a*2, b*2, and L*2, respectively. The color difference ΔE*ab was calculated according to the above formula (1), and the obtained value was designated as the color difference ΔE*ab(G).
[0151] [L*, a*, b*, and color difference ΔE*ab(S) of resin layer] Each resin layer was produced in the same manner as in each example and comparative example, and a laminated glass member was pressure-bonded via the obtained resin layer under the same conditions as in each example and comparative example to produce a laminated glass (laminated glass for measurement). A reference clear glass plate was used as the laminated glass member. The L*, a*, and b* of the first and second resin layers of the obtained laminated glass for measurement were measured using a UV-Visible-Near-Infrared Spectrophotometer "V-670" (manufactured by JASCO Corporation) equipped with an absolute reflectance measurement unit (ARSN-733). The a*, b*, and L* of the first resin layer were defined as a*1, b*1, and L*1, and the a*, b*, and L* of the second resin layer were defined as a*2, b*2, and L*2, respectively. The color difference ΔE*ab was calculated using the above formula (1), and the obtained value was defined as the color difference ΔE*ab(S).
[0152] [L*, a*, b*, and color difference ΔE*ab of first and second members] A first resin layer was produced using the same method as in each example and comparative example, and the first and second laminated glass members used in each example and comparative example were pressure-bonded via the obtained first resin layer under the same conditions as in each example and comparative example to obtain laminated glass. The surface of the laminated glass member on one side of the produced laminated glass (i.e., the second laminated glass member) was scraped with a cutter, and the laminated glass with the scraped surface was immersed in liquid nitrogen. After removing it from the liquid nitrogen, the laminated glass member on the scraped side was struck to break the laminated glass, thereby peeling off the laminated glass member on one side, and a first member consisting of a laminate of the first resin layer and the first laminated glass member was obtained. A laminated glass was prepared using the second resin layer, the first laminated glass member, and the second laminated glass member in the same manner as above, and the first laminated glass member was peeled from the prepared laminated glass in the same manner as above to obtain a second member consisting of a laminate of the second resin layer and the second laminated glass member. The L*, a*, and b* of the obtained first and second members were measured in the same manner as the method used for the measurement laminated glass. The a*, b*, and L* of the first member were defined as a*1, b*1, and L*1, and the a*, b*, and L* of the second member were defined as a*2, b*2, and L*2, respectively. The color difference ΔE*ab was calculated using the above formula (1), and the obtained value was designated as the color difference ΔE*ab(M).
[0153] [Reflectance of Reflective Layer] One surface of the reflective layer was irradiated with light from a D65 light source at an incident angle of 90° and a measurement wavelength range of 300 nm to 2000 nm in a 10° field of view, and reflected light was detected from one surface at wavelength intervals of 5 nm. The reflectance at each wavelength was measured using an ultraviolet-visible-near-infrared spectrophotometer "V-670" (manufactured by JASCO Corporation) equipped with an absolute reflectance measurement unit (ARSN-733), and the average reflectance from 380 to 780 nm, the average reflectance from 780 to 2500 nm, and the average reflectance from 380 to 2500 nm were measured.
[0154] [Total Solar Transmittance (Tts)] Total solar transmittance (Tts) was measured using a spectrophotometer (Hitachi High-Technologies Corporation's "U-4100") in accordance with ISO 13837. The measurement conditions were a scan speed of 300 nm / min and a slit width of 8 nm.
[0155] [Evaluation] When viewing the glass from the inside or outside of the vehicle, the difference in the apparent metallic feel perceived visually was evaluated using the following four-point scale. The smaller the number, the better the design. 1: The metallic feel was strong on the outside of the vehicle, but not on the inside. 2: The metallic feel was weak on the outside of the vehicle, but not on the inside. 3: The metallic feel was strong on both the outside and inside of the vehicle. 4: The metallic feel was completely absent on both the outside and inside of the vehicle.
[0156] The raw materials used in the examples and comparative examples are as follows: [Laminated Glass Member] CLR: Clear glass (standard clear glass sheet) Gray: Privacy glass (gray-tinted privacy glass)
[0157] [Reflective layer] GM40: Toray Industries, Inc., "Picasus", product number: GM40, nano-laminated film having non-uniform hue within the surface GL40: Toray Industries, Inc., "Picasus", product number: GL40, nano-laminated film having non-uniform hue within the surface
[0158] Films 1 to 3 were prepared as follows. (Film 1) Polyethylene terephthalate (resin a) and polyethylene terephthalate (PET) copolymerized with 20 mol% neopentyl glycol (resin b) were each melted at 280°C in separate vented twin-screw extruders and then merged in a 601-layer feedblock with four separate members each having 180 slits. In the multilayer structure, the outermost layers on both sides consisted of PET (resin a), layers of resin a and layers of resin b were alternately laminated, and the thicknesses of adjacent layers of resin a and resin b were approximately the same. The film was then introduced into a T-die and molded into a sheet. It was then rapidly solidified by adhering it to a casting drum maintained at a surface temperature of 25°C by electrostatic application, yielding a cast film. The resulting cast film was stretched 4.0 times in the machine direction while heated to 80°C, and then cooled once to obtain a uniaxially stretched film. The obtained uniaxially stretched film was stretched 4.3 times in the transverse direction at a temperature of 120°C in a tenter. The stretched film was heat-treated at 240°C and then subjected to an 8% relaxation treatment in the width direction at the same temperature to obtain Film 1. (Film 2) Film 2 was produced in the same manner as Film 1, except that Resin b was changed to a mixture of PET and polyethylene terephthalate copolymerized with 20 mol% neopentyl glycol in a mass ratio of 1:3. (Film 3) Film 3 was produced in the same manner as Film 1, except that Resin b was changed to polyethylene terephthalate copolymerized with 40 mol% neopentyl glycol and 2 mol% diethylene glycol, and the number of layers was changed to 801.
[0159] (1) Thermoplastic resin PVB: polyvinyl butyral resin, acetalization degree 69 mol%, hydroxyl group amount 30 mol%, acetylation degree 1 mol%, average polymerization degree of PVA used in synthesis 1700 (2) Plasticizer 3GO: triethylene glycol di-2-ethylhexanoate (3) Filler (A) Filler 1: middle layer is SiO with a refractive index of 1.46 2 The layer and the covering layer are TiO with a refractive index of 2.49. 2 The layer is a three-layer structure shown in FIG. 1, with a flat plate shape, thickness ratio (each coating layer: middle layer = 1:8), D50: 14 μm, thickness 0.5 μm, aspect ratio: 2.8. Filler 2: The middle layer is SiO with a refractive index of 1.46.2 The layer and the covering layer are TiO with a refractive index of 2.49. 2 The filler 3 has a three-layer structure shown in FIG. 1 in a flat plate shape, thickness ratio (each coating layer: middle layer = 1:9), D50: 14 μm, thickness 0.5 μm, aspect ratio: 2.8. Filler 3: TiO 2 / SiO 2 / glass / SiO 2 / TiO 2 Five-layer structure, D50 = 72 μm, thickness: 2.5 μm, aspect ratio: 1.5 Filler 4: middle layer is aluminum oxide layer, coating layer is TiO 2 / Tin oxide / Zirconium oxide multilayer structure Filler 5: Middle layer is mica layer, coating layer is TiO 2 / zirconium oxide / tin oxide multilayer structure (4) Heat-shielding material ITO: tin-doped indium oxide particles (5) Colorant CB: carbon black, pigment black 7 (CAS No. 1333-86-4), carbon black pigment GRN: phthalocyanine (CAS No. 147-14-8),
[0160] [Example 1] (Preparation of Interlayer Film) According to the formulation in Table 1, a plasticizer and a polyvinyl butyral resin (PVB) were fed into an extruder and kneaded in the extruder to obtain a resin composition. The obtained resin composition was molded into first and second resin layers having the thicknesses shown in Table 1, and these were laminated on both sides of a nano-reflective film (reflective layer) to prepare an interlayer film with a three-layer structure of a first resin layer / reflective layer / second resin layer.
[0161] (Preparation of Laminated Glass) Two sheets of clear glass (reference clear glass sheets), each measuring 100 mm long x 100 mm wide x 2.5 mm thick, were prepared as first and second laminated glass members. The interlayer film obtained above was sandwiched between the two sheets of clear glass and temporarily bonded using a vacuum bag method. The temporarily bonded laminate was then held in an autoclave at a temperature of 140°C and a pressure of 1.2 MPa for 20 minutes, and then the temperature was lowered to 23°C and returned to atmospheric pressure to complete the permanent bonding, yielding a laminated glass in which the two sheets of clear glass were bonded together by the interlayer film. The optical properties of the resulting laminated glass were measured, and the evaluation results for the interlayer film and the laminated glass are shown in Table 1.
[0162] [Example 2] According to the formulation in Table 1, carbon black as a colorant was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a first resin layer. The plasticizer and polyvinyl butyral resin (PVB) were also added to an extruder and kneaded in the extruder to obtain a resin composition for forming a second resin layer. First and second resin layers with the thicknesses shown in Table 1 were molded from the obtained resin composition and laminated on both sides of the reflective layer to produce an interlayer film with a three-layer structure of first resin layer / reflective layer / second resin layer. Laminated glass was then produced in the same manner as in Example 1.
[0163] [Example 3] The same procedure as in Example 2 was carried out, except that the content of the colorant in the first resin layer was changed as shown in Table 1. [Example 4] The same procedure as in Example 2 was carried out, except that the nanoreflective film used was changed as shown in Table 1.
[0164] [Example 5] According to the formulation in Table 1, carbon black as a colorant was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a first resin layer. Furthermore, filler (A) was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a second resin layer. First and second resin layers with the thicknesses shown in Table 1 were molded from the obtained resin composition and laminated on both sides of the reflective layer to produce an interlayer film with a three-layer structure of first resin layer / reflective layer / second resin layer. Thereafter, laminated glass was produced in the same manner as in Example 1. The filler (A) was oriented so that its surface direction was aligned with the surface direction of the interlayer film, and this was also the case in the following examples using filler (A).
[0165] [Examples 6 to 9] The same procedure as in Example 5 was carried out, except that the type of filler (A) used was changed as shown in Table 1. [Example 10] The same procedure as in Example 5 was carried out, except that the nanoreflective film used was changed as shown in Table 1.
[0166] [Example 11] The same procedure as in Example 1 was carried out, except that the thickness of the second resin layer was changed as shown in Table 1 and the clear glass used as the first laminated glass member to be superimposed on the first resin layer was changed to plywood glass.
[0167] [Example 12] According to the formulation in Table 1, a plasticizer and polyvinyl butyral resin (PVB) were added to an extruder and kneaded in the extruder to obtain a resin composition for forming a first resin layer. Furthermore, a filler (A) was mixed and dispersed in the plasticizer, and then added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a second resin layer. First and second resin layers having the thicknesses shown in Table 1 were molded from the obtained resin composition and laminated on both sides of the reflective layer to produce an interlayer film with a three-layer structure of first resin layer / reflective layer / second resin layer. Then, a laminated glass was produced in the same manner as in Example 1, except that the clear glass used as the first laminated glass component to be laminated on the first resin layer was replaced with plywood glass.
[0168] Examples 13 and 14 Examples 13 and 14 were carried out in the same manner as in Examples 4 and 5, respectively, except that the clear glass used as the first laminated glass member to be laminated on the first resin layer was changed to plywood glass.
[0169] [Example 15] According to the formulation in Table 1, carbon black as a colorant was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a first resin layer. Furthermore, carbon black as a colorant was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a second resin layer. First and second resin layers with the thicknesses shown in Table 1 were molded from the obtained resin composition and laminated on both sides of the reflective layer to produce an interlayer film with a three-layer structure of first resin layer / reflective layer / second resin layer. Laminated glass was then produced in the same manner as in Example 1.
[0170] [Example 16] According to the formulation in Table 1, carbon black as a colorant was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a first resin layer. Furthermore, a heat-shielding material was mixed and dispersed in a plasticizer, and then the mixture was added to an extruder together with polyvinyl butyral resin (PVB) and kneaded in the extruder to obtain a resin composition for forming a second resin layer. First and second resin layers having the thicknesses shown in Table 1 were molded from the obtained resin composition and laminated on both sides of the reflective layer to produce an interlayer film with a three-layer structure of first resin layer / reflective layer / second resin layer. Laminated glass was then produced in the same manner as in Example 1.
[0171] Examples 17 to 19 were carried out in the same manner as in Example 2, except that the reflective layer was changed as shown in Table 1.
[0172] Comparative Example 1 Comparative Example 1 was carried out in the same manner as in Example 2, except that a resin composition was obtained in the same manner as in Example 2, and first and second resin layers having the thicknesses shown in Table 1 were molded from the obtained resin composition, and these were directly laminated together to produce an interlayer film having a two-layer structure of a first resin layer / a second resin layer.
[0173]
[0174] *phr is parts by mass relative to 100 parts by mass of PVB. *wt% is the content (% by mass) in the first resin layer or the second resin layer.
[0175] As shown in Table 1, in each Example, the color difference ΔE*ab(R) of reflected light in the interlayer film or the color difference ΔE*ab(Rg) of reflected light in the laminated glass was 0.5 or greater. Therefore, the design of the laminated glass when viewed from the first laminated glass component side (i.e., one side) was different from the design when viewed from the second laminated glass component side (i.e., the other side). Furthermore, in all Examples, a metallic appearance was achieved when viewed from the second laminated glass component side (the vehicle exterior side), providing a high level of design. Furthermore, in Examples 2 to 19, the first resin layer contained a colorant, or the first laminated glass component was colored glass, so the design viewed from the first laminated glass component side had a subdued impression. Furthermore, in Examples 5 to 10, 12, and 14, in which the second resin layer contained filler (A), an impactful appearance was achieved when viewed from the second laminated glass component side. Furthermore, in Example 16 and the like in which a heat-shielding material was used, Tts was reduced and the heat-shielding performance was improved.
[0176] In contrast, in Comparative Example 1, the color difference ΔE*ab(R) of the reflected light from the interlayer film and the color difference ΔE*ab(Rg) of the reflected light from the laminated glass were both less than 0.5, so the design when viewed from the first laminated glass component side (i.e., one side) and the design when viewed from the second laminated glass component side (i.e., the other side) were not sufficiently different, and it was not possible to impart a high level of design.
[0177] DESCRIPTION OF SYMBOLS 10 Interlayer film for laminated glass 10A One side 10B Other side 11 First resin layer 12 Second resin layer 11A, 12A Colored layer 11B, 12B Filler-containing layer 11C, 12C Heat-shielding layer 11D, 12D Clear layer 11T Core layer 11S Skin layer 20 Laminated glass 21 First laminated glass member 22 Second laminated glass member 31 First member 32 Second member 100 Middle layer 111, 112 Covering layer
Claims
1. An interlayer film for laminated glass, in which the color difference ΔE*ab(R) between the L*a*b* color space of reflected light for light incident from one direction and the L*a*b* color space of reflected light for light incident from the opposite direction is 0.5 or more.
2. The interlayer film for laminated glass according to claim 1, which is provided with a reflective layer.
3. The interlayer film for laminated glass according to claim 2, wherein the reflective layer is a nano-laminate film.
4. The interlayer film for laminated glass according to claim 3, wherein the reflective layer includes two layers, a resin layer A and a resin layer B, which have different refractive indices, and these layers are laminated in a total of 30 or more layers.
5. The interlayer film for laminated glass according to claim 4, wherein the thickness of the resin layer A is 30 nm or more and 500 nm or less, and the thickness of the resin layer B is 30 nm or more and 500 nm or less.
6. The interlayer film for laminated glass according to claim 4, wherein the difference in refractive index between said resin layer A and said resin layer B is 0.01 or more and 0.15 or less.
7. The interlayer film for laminated glass according to claim 2, wherein the reflective layer has an average reflectance of 25.0% or more in a wavelength range of 380 to 780 nm.
8. The interlayer film for laminated glass according to claim 2, wherein the reflective layer has a non-uniform hue within its surface.
9. The interlayer film for laminated glass according to claim 2, further comprising one or more first resin layers disposed on one surface side of the interlayer film relative to the reflective layer.
10. The interlayer film for laminated glass according to claim 9, wherein the one or more first resin layers have at least a colored layer containing a colorant.
11. The interlayer film for laminated glass according to claim 10, wherein the colorant comprises a pigment, and the pigment comprises at least one selected from the group consisting of carbon black, quinacridone pigments, copper phthalocyanine pigments, nickel complex azo pigments, isoindolinone pigments, and perylene pigments.
12. The interlayer film for laminated glass according to claim 2, further comprising one or more second resin layers disposed on the other surface side of the interlayer film relative to the reflective layer.
13. The interlayer film for laminated glass according to claim 12, wherein the second resin layer contains a filler (A) having at least one of a nonmetallic material and a metal oxide.
14. The interlayer film for laminated glass according to claim 13, wherein the filler (A) contains two or more types of metal oxides.
15. The interlayer film for laminated glass according to claim 14, wherein the refractive indexes of the two or more metal oxides are different from each other.
16. The interlayer film for laminated glass according to claim 13, wherein the filler (A) has a flat plate shape.
17. The interlayer film for laminated glass according to claim 13, wherein the filler (A) has a multilayer structure.
18. The interlayer film for laminated glass according to any one of claims 13 to 17, wherein the aspect ratio of the filler (A) is 1 or more and 50 or less.
19. An interlayer film for laminated glass according to claim 2, comprising: one or more first resin layers arranged on one side of the interlayer film relative to the reflective layer; and one or more second resin layers arranged on the other side of the interlayer film relative to the reflective layer, wherein a color difference ΔE*ab(S) between visible light transmitted through the first resin layer and visible light transmitted through the second resin layer in the L*a*b* color system is greater than 0 and less than 100.
20. The interlayer film for laminated glass according to claim 1 or 2, wherein the color difference E*ab(R) is 2.0 or more.
21. The interlayer film for laminated glass according to claim 1 or 2, wherein the color difference E*ab(R) is 15 or more.
22. The interlayer film for laminated glass according to claim 1 or 2, wherein the color difference E*ab(R) is 30 or more.
23. A laminated glass comprising: a first laminated glass component; a second laminated glass component; and the interlayer film for laminated glass according to claim 1, wherein the interlayer film for laminated glass is disposed between the first laminated glass component and the second laminated glass component.
24. Laminated glass in which the color difference ΔE*ab(Rg) between the L*a*b* color space of reflected light for light incident from one direction and the L*a*b* color space of reflected light for light incident from the opposite direction is 0.5 or more.
25. The laminated glass according to claim 24, comprising a first laminated glass component, a second laminated glass component, and an interlayer film for laminated glass, the interlayer film for laminated glass being disposed between the first laminated glass component and the second laminated glass component, the interlayer film for laminated glass comprising the reflective layer, and the average reflectance of the reflective layer in the wavelength range of 380 to 780 nm is 25.0% or more.
26. The laminated glass according to any one of claims 23 to 25, comprising a first member, a reflective layer, and a second member, wherein the first member has a first laminated glass member and one or more first resin layers, and the second member has a second laminated glass member and one or more second resin layers, the first laminated glass member, the first resin layer, the reflective layer, the second resin layer, and the second laminated glass member are arranged in this order, and the first member and the second member are different in color.
Citation Information
Patent Citations
Biaxially oriented multi-layer polyester film
JP2004249587A
Biaxially oriented multilayer laminated film
JP2005059332A
Laminated polyester film
JP2007301982A
Resin sheet
JP2009078421A
Laminated film
JP2010184493A