Shock-absorbing composition and catch material for micro-led display element
A buffer film composition with an aliphatic urethane structure and crosslinkable functional groups addresses the precision and speed issues in micro LED displays by providing a thin, flexible, and adhesive film for micro LED elements, ensuring precise placement and efficient mass transfer in micro LED displays.
Patent Information
- Application Number
- PCT/JP2024/012605
- Authority / Receiving Office
- WO · WO
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-28
- Publication Date
- 2024-10-03
AI Technical Summary
Conventional buffer materials with thick foam layers are not suitable for the laser lift-off method in micro LED displays, as they do not provide the necessary precision and speed for arranging micro LED elements on an array substrate, and existing solutions like multilayer buffer materials with uncured thermosetting adhesive resins are not thin enough for high precision and flexibility.
A buffer film composition containing an aliphatic compound with a urethane structure and two or more crosslinkable functional groups, a crosslinking agent, and a polymerization initiator, which forms a cured film with a glass transition temperature below 0°C, providing excellent adhesion and impact absorption for micro LED elements during the laser lift-off process.
The buffer film composition ensures precise placement and high flexibility of micro LED elements by maintaining their position without displacement, achieving a low coefficient of restitution and suitable thickness for efficient mass transfer in micro LED displays.
Smart Images

Figure JPOXMLDOC01-APPB-T000001 
Figure JPOXMLDOC01-APPB-T000002
Abstract
Description
Buffer composition and catch material for micro LED display element
[0001] The present invention relates to a buffering composition, and more particularly to a buffering composition that functions as a catch material for a micro LED display element.
[0002] Currently, liquid crystal displays (LCDs) and organic light-emitting diode displays (OLEDs) are primarily used in flat panel displays used in mobile phones, monitors, and TVs. While LCDs have well-established mass production technology, they are inexpensive and can be made large. However, the need for a backlight for display results in poor form factor and flexibility. OLEDs, while offering superior flexibility, face the challenge of shortening their lifespan as the brightness of the display increases. To address these drawbacks, micro-LED display elements, which use inorganic light-emitting diodes arranged on each pixel of an array substrate, have been developed in recent years. Because micro-LED display elements use micrometer-sized inorganic light-emitting diodes as light sources, they can achieve higher brightness, higher color purity, and a longer lifespan than LCDs and OLEDs. Furthermore, because LEDs are arranged for each pixel, each pixel can be isolated and the display is highly flexible.
[0003] LED elements, which serve as light-emitting sources, are supplied as small pieces by epitaxially growing a semiconductor layer on a sapphire substrate, forming electrodes, and then dicing the substrate. Micro LED display elements require a large number of tiny LED element pieces manufactured in this way to be arranged on an array substrate with high precision. The conventional pick-and-place method for arranging LED elements on an array substrate, in which each LED element is installed one by one, requires a significant takt time. Therefore, mass-transfer methods, in which a large number of LED elements are transferred to an array substrate at once, are being actively investigated. In particular, for larger displays and other applications, high speed as well as high precision are required, and mass-transfer methods using the laser lift-off (LLO) method are considered promising.
[0004] The simplest process using the LLO method is to directly transfer the LED elements from the support substrate onto the array substrate, as proposed in Patent Document 1. To achieve this direct transfer, the LED elements that have been ejected by the laser must be positioned on the array substrate without misalignment, and to achieve this, a buffer film with excellent adhesiveness must be provided on the array substrate in advance as a catch material.
[0005] Typically, the electrode height of a micro LED element is no more than several tens of micrometers. Since the LED element transferred to the substrate is subsequently bonded to the substrate electrode by bonding, the buffer film required for the laser mass transfer process must also be no more than several tens of micrometers thick. On the other hand, many impact-absorbing sheets containing a foam layer, known as an excellent buffer material, often have a thickness of several hundred micrometers (Patent Document 2).
[0006] As such, the thickness of conventional buffer materials is not suitable as a catch material for the LLO process of micro-LEDs, and therefore Patent Document 3 proposes a multi-step process in which an uncured thermosetting adhesive resin layer is provided on the bump electrode side of the LED.
[0007] JP 2010-161221 A JP 2021-183695 A JP 2020-145243 A
[0008] The present invention has been made in consideration of the above circumstances, and relates to a transfer process for micro LED elements using the LLO method, and aims to provide a buffer film that is a thin film suitable for micro LEDs and functions as a catch material.
[0009] The present inventors have conducted extensive research to solve the above problems and have come up with the present invention.
[0010] 1. A composition comprising (A) an aliphatic compound having a urethane structure and two or more crosslinkable functional groups, (B) a crosslinking agent, and (C) a polymerization initiator, the composition having a glass transition temperature (Tg) of less than 0°C after curing. 2. The composition according to 1, further comprising a solvent. 3. The composition according to 1 or 2, further comprising a photopolymerization initiator. 4. The composition according to any one of 1 to 3, further comprising a silane coupling agent. 5. A cured film obtained by applying thermal energy or ultraviolet light energy to the composition according to any one of 1 to 4. 6. The cured film according to 5, having a film thickness of 10 μm or less. 7. The cured film according to 6, having a restitution coefficient of 0.5 or less. 8. A patterned cured film obtained by exposing and developing the composition according to any one of 1 to 4. 9. An LED display element having the cured film according to any one of 5 to 8 as a catch material.
[0011] The composition of the present invention contains the following components (A), (B), and (C), and has a glass transition temperature (Tg) of less than 0°C after curing.
[0012] Component (A): an aliphatic compound having a urethane structure and two or more crosslinkable functional groups; Component (B): a crosslinking agent; Component (C): a polymerization initiator. It is not entirely clear why the object of the present invention can be achieved by the present invention, but it is generally thought to be as follows.
[0013] The flexibility of the urethane structure contained in the compound of the present invention plays a role in absorbing the impact of the thrown micro-LED chip, and at the same time, the adhesiveness of the film resulting from the low Tg is presumed to keep the micro-LED held in the desired position without displacement.
[0014] Each component is described in detail below. <Component (A)> Component (A) is an aliphatic compound having a urethane structure and two or more crosslinkable functional groups, and is characterized in that a cured film of the polymer has a glass transition temperature (Tg) of less than 0°C.
[0015] The aliphatic compound constituting component (A) of the present invention preferably has two or more crosslinkable functional groups. Furthermore, if there are too many crosslinking moieties, the flexibility of the cured film is impaired and the catching performance is reduced, so it is more preferable that the number of functional groups at the crosslinking moieties is two.
[0016] The crosslinkable functional group refers to a functional group capable of forming a chemical bond with other molecules. Specific examples include vinyl groups, acrylic groups, methacrylic groups, cyclic ether groups, carboxyl groups, and maleimide groups. From the viewpoint of reactivity, vinyl groups, acrylic groups, methacrylic groups, and epoxy groups are preferred, and acrylic groups and methacrylic groups are more preferred.
[0017] Specific examples of compounds preferred as component (A) include aliphatic urethane acrylates such as EBECRYL230, EBECRYL270, EBECRYL4491, EBECRYL8411, and EBECRYL8413 (trade names, manufactured by Daicel Allnex Co., Ltd.), SU514, SU530, SU570, and SU5656 (trade names, manufactured by Okajima Corporation), and GENOMER4215 and GENOMER4269 / M22 (trade names, manufactured by RAHN AG); and aliphatic ester-based urethane acrylates such as KAYARAD UX-3204 (trade name, manufactured by Nippon Kayaku Co., Ltd.), UN-350, UN-1255, and UN-7700 (trade name, manufactured by Negami Chemical Industrial Co., Ltd.), and UF-3003 (trade name, manufactured by Kyoeisha Chemical Co., Ltd.). Examples of aliphatic ether urethane acrylates include KAYARAD UXF-4002 (Nippon Kayaku Co., Ltd., trade name), UN-6200, UN-6304 (Negami Chemical Industrial Co., Ltd., trade name), UA-1138P, UA-3573AB (Shin-Nakamura Chemical Co., Ltd., trade name).
[0018] <Component (B)> Component (B) is a crosslinking agent contained for the purpose of assisting the crosslinking of component (A) to form a cured film, and the type is not particularly limited. To avoid impairing the catching performance exhibited by component (A), component (B) is preferably one that contributes to promoting crosslinking in a small amount. Examples of compounds that contribute to promoting crosslinking in a small amount include polyfunctional thiols and organic peroxides such as peroxyketals that also function as cationic initiators.
[0019] The amount of component (B) is preferably 0.1 to 10 parts by mass, and more preferably 0.5 to 5 parts by mass, based on 100 parts by mass of component (A).
[0020] <Component (C)> In order to promote the crosslinking reaction between the components (A) and (B) by heat or light, a polymerization initiator can be used as the component (C) as needed.
[0021] As the polymerization initiator for the composition of the present invention, a compound that generates radical or cationic active species can be used. Radical initiators include thermal radical initiators and photoradical initiators. Thermal radical initiators include, for example, organic peroxides such as peroxyketals and azo compounds such as 2,2'-azobisbutyronitrile. Photoradical initiators generate radicals upon irradiation with ultraviolet light or electron beams, and include oxime ester compounds and benzoin compounds. Cationic initiators generate cations upon receiving heat or light energy, and include, for example, sulfonium salts and iodonium salts.
[0022] When component (C) is used, its content is usually 0.1 to 10 parts by mass, and preferably 0.5 to 5 parts by mass, based on 100 parts by mass of component (A).
[0023] <Solvent> The solvent used in the present invention dissolves the components (A) and (B) and also dissolves the components described below that are added as desired. There are no particular limitations on the type or structure of the solvent, as long as it has such dissolving ability.
[0024] Examples of such solvents include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, methyl cellosolve acetate, ethyl cellosolve acetate, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, propylene glycol propyl ether acetate, toluene, xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, 2-butanone, 3-methyl-2-pentanone, ... Examples of suitable solvents include acetone, 2-heptanone, γ-butyrolactone, ethyl 2-hydroxypropionate, ethyl 2-hydroxy-2-methylpropionate, ethyl ethoxyacetate, ethyl hydroxyacetate, methyl 2-hydroxy-3-methylbutanoate, methyl 3-methoxypropionate, ethyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 3-ethoxypropionate, methyl pyruvate, ethyl pyruvate, ethyl acetate, butyl acetate, ethyl lactate, butyl lactate, N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone. These solvents can be used alone or in combination of two or more.
[0025] Among these solvents, propylene glycol monomethyl ether, propylene glycol monomethyl ether acetate, 2-heptanone, propylene glycol propyl ether, propylene glycol propyl ether acetate, ethyl lactate, butyl lactate, etc. are preferred from the viewpoint of good film-forming properties and high safety. These solvents are generally used as solvents for photoresist materials.
[0026] <Silane Coupling Agent> The composition of the present invention may further contain a silane coupling agent for the purpose of improving adhesion to the substrate.
[0027] Examples of the silane coupling agent include vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-glycidylpropyltrimethoxysilane, 3-glycidylpropyltriethoxysilane, 2-(3,4-epoxycyclohexyl)propyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)propyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 2-(3,4-epoxycyclohexyl)methyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)methyltriethoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, and 3-phenylaminopropyltrimethoxysilane.
[0028] When a silane coupling agent is used, its content is usually 0.5 to 20 parts by mass, and preferably 2 to 10 parts by mass, based on 100 parts by mass of component (A).
[0029] <Coated Film and Cured Film> The composition of the present invention can be applied to a semiconductor substrate (e.g., a silicon / silicon dioxide-coated substrate, a silicon nitride substrate, a substrate coated with a metal such as aluminum, molybdenum, or chromium, a glass substrate, a quartz substrate, an ITO substrate, etc.) by spin coating, flow coating, roll coating, slit coating, spin coating followed by slit coating, inkjet coating, or the like, and then pre-dried on a hot plate or in an oven, etc. A cured film can then be formed by subjecting this coated film to a heat treatment or irradiation with light such as ultraviolet light.
[0030] The conditions for pre-drying are a heating temperature and a heating time appropriately selected from the ranges of 70 to 130°C and 0.3 to 10 minutes, respectively. The heating temperature and heating time are preferably 80 to 120°C and 0.5 to 5 minutes.
[0031] The thickness of the coating film formed from the composition of the present invention is, for example, 0.1 to 30 μm, or, for example, 1 to 20 μm, or, further, for example, 5 to 15 μm.
[0032] When curing is performed by heat treatment using a thermal radical generator or the like as component (B), the conditions are a heating temperature of 120 to 180°C and a heating time of 0.3 to 10 minutes, and the heating temperature and heating time are appropriately selected from the ranges of 140 to 160°C and 0.5 to 5 minutes, respectively. The heating temperature and heating time are preferably 140 to 160°C and 0.5 to 5 minutes, respectively. The atmosphere for the heat treatment may be air or an inert gas, but in order to more effectively utilize the function of the thermal radical generator, heat treatment in an inert gas such as nitrogen is preferred.
[0033] When curing by light irradiation using a photopolymerization initiator as component (B), the conditions are, for example, 100 to 5,000 mJ / cm using ultraviolet light with a wavelength of 365 nm. 2 The composition can be cured by irradiation with light of an intensity of 10 ....
[0034] <Patterning of cured film> A mask having a predetermined pattern is attached to the coating film obtained above, and the film is irradiated with light such as ultraviolet light, and developed with an alkaline developer, whereby the exposed areas are washed out and a sharp pattern with sharp edge surfaces is obtained.
[0035] Examples of alkaline developers that can be used include aqueous solutions of alkali metal hydroxides such as potassium carbonate, sodium carbonate, potassium hydroxide, and sodium hydroxide, aqueous solutions of quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and choline, and aqueous amine solutions such as ethanolamine, propylamine, and ethylenediamine. Furthermore, surfactants and the like can also be added to these developers.
[0036] Among the above, a 0.1 to 2.38 mass % aqueous solution of tetraethylammonium hydroxide is generally used as a developer for photoresists, and the photosensitive adhesive composition of the present invention can also be developed satisfactorily using this alkaline developer without causing problems such as swelling.
[0037] The developing method may be any of the puddle method, dipping method, and swing immersion method, etc. The developing time is usually 15 to 180 seconds.
[0038] After development, the positive photosensitive adhesive film is washed with running water for, for example, 20 to 120 seconds, followed by air drying with compressed air or compressed nitrogen or by spinning, thereby removing water from the substrate and obtaining a patterned film.
[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The abbreviations of the compounds used and the methods for measuring the physical properties are as follows: (Resins) R1: EBECRYL230 (difunctional aliphatic urethane acrylate, manufactured by Daicel-Allnex Corporation) R2: EBECRYL4491 (difunctional aliphatic urethane acrylate, manufactured by Daicel-Allnex Corporation) R3: EBECRYL8411 (difunctional aliphatic urethane acrylate, manufactured by Daicel-Allnex Corporation) R4: EBECRYL8413 (difunctional aliphatic urethane acrylate, manufactured by Daicel-Allnex Corporation) R5: KAYARAD UX-3204 (difunctional aliphatic urethane acrylate, manufactured by Nippon Kayaku Co., Ltd.) R6: EBECRYL8402 (difunctional aliphatic urethane acrylate, manufactured by Daicel-Allnex Corporation) R7: EBECRYL350 (silicon diacrylate, manufactured by Daicel-Allnex Co., Ltd.) R8: EBECRYL3708 (epoxy acrylate, manufactured by Daicel-Allnex Co., Ltd.) R9: UF-8001G (bifunctional urethane acrylate, manufactured by Kyoeisha Chemical Co., Ltd.) R10: AH-600 (bifunctional urethane acrylate, manufactured by Kyoeisha Chemical Co., Ltd.) R11: DAUA-167 (bifunctional carboxylic acid-containing urethane acrylate, manufactured by Kyoeisha Chemical Co., Ltd.) R12: UA-306H (hexafunctional urethane acrylate, manufactured by Kyoeisha Chemical Co., Ltd.) (crosslinking agent) C1: Karenz MT PE1 (manufactured by Showa Denko K.K.) C2: Perhexa V (manufactured by NOF Corporation) (other additives) A1: Irgacure OXE01 (photopolymerization initiator, manufactured by BASF Japan Ltd.) A2: 3-phenylaminopropyltrimethoxysilane (manufactured by Tokyo Chemical Industry Co., Ltd.) A3: Omnirad 184 (photopolymerization initiator, manufactured by IGM Resins) (solvent) PGME: propylene glycol monomethyl ether
[0040] <Measurement of Glass Transition Temperature (Tg)> The Tg of the cured film of the composition obtained in the examples was measured using a differential scanning calorimetry (DSC) DSC1 (manufactured by METTLER TOREDO) under the following conditions: Heating rate: 10°C / min, Measurement temperature: -20°C to 150°C, Number of measurements: 2. Tg was calculated from the result of the second temperature decrease.
[0041] <Preparation of Buffer Composition> (Example 1-1) To bifunctional aliphatic urethane acrylate resin R1 (5.455 g), crosslinker C1 (0.273 g), photopolymerization initiator A1 (0.273 g), and solvent PGME (4.0 g) were added, and the mixture was stirred at room temperature for 2 hours to prepare composition V1 having the composition shown in Table 1.
[0042] Examples 1-2 to 1-5 and Comparative Examples 1-1 to 1-7 Compositions V2 to V5 and RV1 to RV7 having the compositions shown in Table 1 were prepared in the same manner as in Example 1-1, except that the resin components were changed as shown in Table 1. However, composition RV7 had poor compatibility, and a homogeneous solution could not be obtained.
[0043] (Example 1-6) Resin R3 (1.0 g), crosslinking agent C1 (0.250 g), photopolymerization initiator A1 (0.250 g), silane coupling agent A2 (0.500 g), and solvent PGME (4.0 g) were added to resin R1 (4.0 g), and the mixture was stirred at room temperature for 2 hours to prepare composition V6 having the composition shown in Table 1.
[0044] Example 1-7 To resin R1 (3.636 g), crosslinking agent C2 (0.364 g) and solvent PGME (6.0 g) were added, and the mixture was stirred at room temperature for 2 hours to prepare composition V7 shown in Table 1.
[0045] (Example 1-8) To resin R1 (5.405 g), crosslinker C1 (0.541 g), photopolymerization initiator A3 (0.054 g), and solvent PGME (4.0 g) were added, and the mixture was stirred at room temperature for 2 hours to prepare composition V8 having the composition shown in Table 1.
[0046]
[0047] (Example 2-1) <Preparation and Evaluation of Cured Film> Composition V1 prepared in Example 1-1 was applied to a 3 cm × 4 cm ITO substrate using a spin coater, and then the solvent was evaporated on a hot plate at 100°C for 120 seconds to form a coating film with a thickness of 10 μm. This coating film was irradiated with ultraviolet light having a wavelength of 365 nm at 3,000 mJ / cm. 2 The cured film was then irradiated with light to produce a cured film. The Tg of the resulting cured film was below -20°C. The shock-absorbing properties of the cured film were then evaluated by the finger touch method. Specifically, the surface of the cured film was pressed with a finger at room temperature to form an indentation, and if the indentation disappeared within 30 minutes, the shock-absorbing properties were rated as "good." If the indentation remained after 30 minutes, the film had insufficient curing and did not return to its original state, and the shock-absorbing properties were rated as "poor 1." If no indentation was formed at all, the film was unlikely to undergo elastic deformation upon curing, and the shock-absorbing properties were rated as "poor 2." The results are shown in Table 2. Elastic deformation is defined as the deformation of the film such that the indentation formed by finger pressing returns to its original state.
[0048] <Evaluation of Restitution Coefficient> A 1 mm diameter SUS ball was allowed to freely fall from a height h1 of 50 mm onto the cured film produced in Example 2-1, the rebound height h2 was measured, and the restitution coefficient e was calculated using formula (1).
[0049] e = (h2 / h1) 1/2 ...(1)
[0050] (Examples 2-2 to 2-6 and Comparative Examples 2-1 to 2-6) Using the cushioning compositions V2 to V6 and RV1 to RV6 prepared in Examples 1-2 to 1-6 and Comparative Examples 1-1 to 1-6, Tg, cushioning properties, and restitution coefficient were evaluated in the same manner as in Example 2-1. The results are shown in Table 2.
[0051] Comparative Example 2-7 The restitution coefficient was evaluated on a 3 cm×4 cm ITO substrate without forming an organic film. The results are shown in Table 2.
[0052] Example 2-7 Buffering composition V7 prepared in Example 1-7 was applied to a 3 cm x 4 cm ITO substrate using a spin coater, and then the solvent was evaporated on a hot plate at 150°C for 60 seconds under a nitrogen atmosphere to form a cured film with a thickness of 10 μm. The Tg, cushioning properties, and restitution coefficient of the resulting cured film were evaluated in the same manner as in Example 2-1. The results are shown in Table 2.
[0053] (Example 2-8) Composition V8 prepared in Example 1-8 was applied to a 3 cm x 4 cm ITO substrate using a spin coater, and then the solvent was evaporated on a hot plate at 100°C for 120 seconds to form a coating film with a thickness of 10 μm. This coating film was irradiated with ultraviolet light having a wavelength of 365 nm at 1,000 mJ / cm. 2 The cured film was subjected to irradiation to produce a cured film. The Tg, shock absorption properties, and restitution coefficient of the obtained cured film were evaluated in the same manner as in Example 2-1. The results are shown in Table 2.
[0054]
[0055] As shown in Table 2, the cured films prepared from the compositions of the examples using bifunctional aliphatic urethane acrylate resins had Tg values below 0°C, exhibited excellent curability and adhesion, and exhibited low resilience coefficients of less than 0.5. In contrast, when resins with cured film Tg values of 0°C or higher were used (Comparative Example 2-1 and Comparative Examples 2-3 to 2-6), the elastic deformation of the films was insufficient, resulting in high resilience coefficients of 0.7 or higher. Furthermore, when only silicone diacrylate resin was used (Comparative Example 2-2), the curability was insufficient, and the resilience coefficient could not be evaluated.
[0056] (Example 3-1) <Patterning Evaluation> The buffer composition V6 prepared in Example 1-6 was applied to a 5 cm x 5 cm glass substrate using a spin coater, and then the solvent was evaporated on a hot plate at a temperature of 100°C for 120 seconds to form a coating film with a thickness of 1 μm. This coating film was then irradiated with light of 3,000 mJ / cm at a wavelength of 365 nm. 2The film was irradiated with ultraviolet light of 1000 kJ / cm² through a mask. The film was then developed by immersion in a 2.38% by mass aqueous solution of tetramethylammonium hydroxide (hereinafter referred to as TMAH) for 60 seconds, and then washed with running ultrapure water for 30 seconds to produce a patterned film. The resulting patterned film had no residue in the unexposed areas and maintained a thickness within ±10% of the thickness of the coating film.
Claims
1. A composition containing (A) an aliphatic compound having a urethane structure and two or more crosslinkable functional groups, (B) a crosslinking agent, and (C) a polymerization initiator, and having a glass transition temperature (Tg) of less than 0°C after curing.
2. The composition of claim 1 further comprising a solvent.
3. The composition according to claim 1 or 2, further comprising a photopolymerization initiator.
4. The composition according to any one of claims 1 to 3, further comprising a silane coupling agent.
5. A cured film obtained by applying heat energy or ultraviolet light energy to the composition according to any one of claims 1 to 4.
6. The cured film according to claim 5, having a film thickness of 10 μm or less.
7. The cured film according to claim 6, having a restitution coefficient of 0.5 or less.
8. A patterned cured film obtained by exposing and developing the buffer composition according to any one of claims 1 to 4.
9. An LED display element having the cured film according to any one of claims 5 to 8 as a catch material.
Citation Information
Patent Citations
Protective film, and molded article having the same
JP2012143936A
Adhesive sheet and production method of the same, and method for manufacturing image display device
JP2019131679A
Adhesive, curable adhesive composition, adhesive sheet, and method for producing the same
JP2019131680A
Impact absorption adhesive sheet
JP2022101804A
Resin composition
JP2023102162A